Anchor Fixing Material

The anchor fixing material with cement, Erimite, Ternesite, and high SiO2 plasticizer ensures uniform mixing and adhesion, addressing flow-out issues in non-vertical applications, enhancing fixation efficacy.

JP7583592B2Active Publication Date: 2024-11-14DENKA CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020200454
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-02
Publication Date
2024-11-14
Estimated Expiration
2040-12-02

AI Technical Summary

Technical Problem

Existing fixing materials for reinforcing bars and anchor bolts in construction fail to maintain uniform mixing and adhesion, leading to potential separation of components and flow-out during application in horizontal or upward directions, compromising fixation.

Method used

An anchor fixing material comprising cement, an expanding agent with Erimite and Ternesite, and a plasticizer with high SiO2 content, ensuring high adhesion and preventing flow-out during construction by maintaining plasticity and pumpability.

Benefits of technology

The material achieves uniform mixing and high adhesion, allowing for effective fixation without flow-out, even in non-vertical applications, through controlled expansion and plasticity enhancement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583592000001
    Figure 0007583592000001
  • Figure 0007583592000002
    Figure 0007583592000002
Patent Text Reader

Abstract

To provide an anchor fixing material that has a plasticity not flowing out from an insertion hole even when it is filled in the insertion hole in the horizontal or upward direction, has handling properties that allow its transportation under pressure by a pump or the like, and can tightly fix an anchor element inserted into the insertion hole without the leakage of the material at the time when the element is fixed.SOLUTION: An anchor fixing material that contains cement, an expander, and a plasticizer, in which the expander contains ye'elimite and ternesite, and the mass ratio of ye'elimite to ternesite (ye'elimite / ternesite) is 1 to 40.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anchoring material for fixing elements such as deformed bars, reinforcing bars, anchor bolts, rock bolts, etc., in drilled holes. [Background technology]

[0002] 2. Description of the Related Art Conventionally, fixing materials have been used in the fields of architecture and civil engineering to drill holes in hard materials such as concrete, stone, brick, block, and bedrock, and to fix elements such as reinforcing bars, anchor bolts, and rock bolts.

[0003] Methods of fixing the elements can be divided into two types: like metal anchor bolts, where the tip of the anchor bolt expands when buried and fixes the element, and adhesive materials are used to fix the elements around the element. Adhesive materials can be divided into organic and inorganic fixing materials.

[0004] A known inorganic fixing material is one in which a hydraulic substance containing cement and calcium aluminate is stored in a destructible container made of Heatlon paper, thereby reducing insertion resistance when driving the anchor (Patent Document 1).

[0005] Also, a capsule for fixing elements is known which contains cement, calcium aluminosilicate glass or calcium aluminate glass, gypsum, aggregate, colloidal silica, microfibrillated fibrous cellulose, water, and a setting retarder in an easily breakable container (Patent Document 2).

[0006] Furthermore, a rapid-hardening cement composition for use as an anchor element fixing material, which contains an alkali metal carbonate, an aluminate, an inorganic compound, calcium aluminate, and a water-retentive substance, is known (Patent Document 3).

[0007] When the inorganic fixing materials described in Patent Documents 1 to 3 are fixed in bores, the cement composition containing cement, calcium aluminate, and aggregate is allowed to absorb water. However, particularly in the case of Patent Document 2, the water and aggregate may be stored in a mixed state for a long period of time, causing the aggregate and water to separate, preventing the fixing material from being mixed uniformly, and the element may not be completely fixed in the borehole. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2011-079708 A [Patent Document 2] JP 2009-114000 A [Patent Document 3] JP 2006-335586 A Summary of the Invention [Problem to be solved by the invention]

[0009] As mentioned above, it is practically necessary for the fixing material to be mixed uniformly. However, in consideration of application to various construction sites, fixing materials that are easy to apply to holes on the top surface and in the horizontal direction, have good pumpability, and can achieve good adhesion without flowing out of the holes during construction will become more important in the future.

[0010] Therefore, the present invention aims to provide an anchor fixing material that has plasticity that does not flow out of holes located horizontally or upwardly when filled therein, yet has handleability that allows it to be pressurized with a pump or the like, and that fixes the anchor element inserted into the insertion hole with high adhesion without the fixing material flowing out during construction. [Means for solving the problem]

[0011] As a result of extensive research, the present inventors have discovered that the above problems can be solved by using an expanding agent, a plasticizer, and a cement containing specific components, and have thus completed the present invention.

[0012] The present invention is as follows. [1] An anchor fixing material comprising cement, an expanding agent, and a plasticizer, the expanding agent containing eelimite and ternesite, and a mass ratio of the eelimite to the ternesite (eelimite / ternesite) of 1 to 40. [2] The anchor fixing material according to [1], wherein the plasticizer contains SiO2 and the amount of the SiO2 is 85 parts by mass or more per 100 parts by mass of the plasticizer. [3] The plasticizer has a BET specific surface area of ​​5m 2 / g~70m 2 / g of the anchor fixing material described in [1] or [2]. Effect of the Invention

[0013] The anchor fixing material of the present invention, which contains the cement, expansion agent, and plasticizer, is mixed with water and has plasticity that prevents it from flowing out even when filled into holes in the horizontal or upward direction, while being easy to handle so that it can be pumped using a pump or the like.When fixing an anchor element inserted into an insertion hole, the fixing material does not flow out during construction, and the anchor element can be fixed tightly. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail, but the present invention is not limited to the embodiment. In this specification, "parts" and "%" are based on mass unless otherwise specified.

[0015] [cement] The cement used in the present invention typically includes various types of commercially available Portland cement, such as normal, early strength, medium heat, low heat, and extra early strength Portland cement, various mixed cements in which fly ash or blast furnace slag is mixed with these Portland cements, and ecocement, and these can also be used in a finely powdered form.

[0016] [Expansion material] The expanding agent used in the present invention contains eelimite and ternesite. The expanding agent can fix the anchor element with high adhesion. The details are explained below.

[0017] (Elimite) Eelimite is a mineral represented by the formula 3CaO·3Al2O3·CaSO4, which hydrates in the presence of gypsum and other substances to form ettringite (3CaO·Al2O3·3CaSO4·32H2O), which contributes to improving early strength.

[0018] From the viewpoint of reactivity, the particle size of Elimite is set to 4500 to 12000 cm in terms of Blaine specific surface area. 2 / g, and 5000 to 10000 cm 2 It is more preferable that the molecular weight is / g.

[0019] The content of Elimite is preferably 5 to 35 parts, more preferably 8 to 30 parts, based on 100 parts of the expanding agent. When the content is 5 to 35 parts, good early strength can be obtained.

[0020] (Ternesite) Ternesite is a mineral expressed as 5CaO·2SiO2·SO3, and promotes the hydraulic reaction of eelimite. Ternesite itself hardly reacts, so it is assumed to act as a filler and improve fluidity retention. Therefore, flow-down can be reduced.

[0021] The content of ternesite is preferably 0.05 to 20 parts, more preferably 0.1 to 15 parts, and even more preferably 1 to 10 parts, relative to 100 parts of the expansive material. By being 0.05 to 20 parts, both the hardening acceleration and the fluidity retention of elimit can be improved.

[0022] Here, the mass ratio of eelimite to ternesite (eelimite / ternesite) is preferably 1 to 40, more preferably 4 to 35, and even more preferably 5 to 30. If the mass ratio is less than 1, good expansion characteristics, particularly a large rate of change in length, may not be obtained when applied to an expansion agent. Also, if the mass ratio exceeds 40, it becomes difficult to obtain the effect of ternesite in promoting the hardening of eelimite.

[0023] The expanding agent containing eelimite and ternesite is prepared by, for example, blending CaO raw material, Al2O3 raw material, SiO2 raw material, and CaSO4 raw material, mixing and grinding them, and then firing them at 1100 to 1600 °C to synthesize clinker, and producing a granular material having a Blaine specific surface area of ​​2000 to 6000 cm. 2 It can be produced by crushing it to about 1000g / g. The mass ratio of erimite to ternesite can be adjusted by adjusting the ratio of the raw materials. CaO raw materials include limestone and slaked lime, Al2O3 raw materials include bauxite and aluminum ash, SiO2 raw materials include silica stone, and CaSO4 raw materials include gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum.

[0024] (Plasticizer) The plasticizer used in the present invention contains SiO2 as a chemical component, and the content is preferably 85 parts or more, more preferably 90 parts or more, per 100 parts by mass of the plasticizer. By using 85 parts or more, high plasticity can be achieved. The term "plasticization" used here refers to the property of preventing the overflow of the fixing material during application while maintaining non-fluidity after application. This property can provide the effect of making the fixing material easier to handle (facilitating processing) when pumping or filling holes. The SiO2 content in the plasticizer can be measured by fluorescent X-ray diffraction. An example of a plasticizer containing SiO2 is silica fume.

[0025] The BET specific surface area of ​​the plasticizer is 5m 2 / g~70m 2 / g, and preferably 10m 2 / g~60m 2 / g is more preferable. 2 / g or more, it becomes easier to ensure sufficient plasticity, and 2 When the molecular weight is 1 / g or less, pumping performance can be improved.

[0026] In 100 parts by mass of the anchor fixing material consisting of cement, an expanding agent, and a plasticizer, the amount of cement is preferably 85 to 98 parts, and more preferably 90 to 95 parts. The amount of the expanding agent is preferably 0.5 to 8 parts, and more preferably 1 to 5 parts. Furthermore, the amount of the plasticizer is preferably 0.5 to 10 parts, and more preferably 2 to 8 parts. By having the above components in the specified ranges in 100 parts by mass of the anchor fixing material, adhesion, handling, and plasticity are improved.

[0027] In the anchor fixing material of the present invention, in addition to aggregates such as sand and gravel, one or more of water reducing agents, high-performance water reducing agents, AE water reducing agents, high-performance AE water reducing agents, fluidizing agents, antifoaming agents, thickening agents, rust inhibitors, antifreeze agents, shrinkage reducing agents, polymer emulsions and setting regulators, as well as cement hardening agents, clay minerals such as bentonite and zeolite, anion exchangers such as hydrotalcite, etc. can be used within a range that does not substantially impair the object of the present invention.

[0028] The anchor fixing material of the present invention can be mixed with water and filled into the bored hole into which the anchor is to be inserted for installation. However, for example, under construction conditions requiring a large amount of material, it can be installed by a method in which the anchor fixing material is mixed with water in a construction mixer or the like, pressurized by a pump or the like, and the material is filled into the hole before the anchor is inserted. EXAMPLES

[0029] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0030] (Experimental Examples 1 to 6) Of the 100 parts by mass of anchor fixing material consisting of cement, expansive agent, and plasticizer, 90 parts by mass of cement, 5 parts by mass of expansive agent, and 5 parts by mass of plasticizer were used, and a cement paste with a water / anchor fixing material ratio of 40% was prepared in a room at 20°C, and the compressive strength, length change rate, and flow were measured. The results are shown in Table 1.

[0031] (Materials used) Water: Tap water Cement: Ordinary Portland cement, commercially available Plasticizer: Silica fume with SiO2 content of 99.3%, BET specific surface area of ​​45m 2 / g Expansion agent: CaO raw material (limestone), Al2O3 raw material (bauxite), SiO2 raw material (silica stone), and CaSO4 raw material (anhydrous gypsum) are mixed and crushed, then fired at 1,200°C to synthesize clinker, which is then crushed using a ball mill to produce a material with a Blaine specific surface area of ​​3,000 cm. 2 The mixture was crushed to 100 g / g to prepare an expanding material having the composition shown in Table 1. The mineral composition was calculated based on the chemical composition determined from X-ray fluorescence and the results of powder X-ray diffraction.

[0032] (Test Method) Compressive strength: Test specimens measuring 4 x 4 x 16 cm were prepared in accordance with JIS R 5201, and the compressive strength after 7 days (7d) was measured. Length change: Measured and evaluated in accordance with JIS A 6202 after 7 days (7d). If shrinkage is large, the adhesion and fixation between the anchor and the existing structure after construction cannot be sufficiently secured, and conversely, if expansion is too large, there is a possibility that the existing structure will be destroyed. Therefore, the evaluation method is ○ (expansion strain is -200×10 -6 ~1000×10 -6 ), × (expansion strain is -200 × 10 -6 The evaluation was based on a standard deviation of 0.05%. Flow: In accordance with JIS R 5201-2015 "Physical Testing Methods for Cement," the flow value was measured immediately after the flow cone was removed from the mixture just after it was mixed, and after 15 hits. The same measurements were then taken using material that had been mixed for 60 minutes, and changes in flow were confirmed. The static state indicates the plasticity of the material, and a flow of 120mm or less is desirable. After 15 hits, it indicates the pumpability, and a flow of 160mm or more is desirable.

[0033] [Table 1]

[0034] Table 1 shows that by using an expansive material with a specific mineral ratio, it is possible to obtain good flow retention and sufficient expansion to fix the hole and anchor after hardening.

[0035] (Experimental Examples 7 to 13) A cement paste with a water / anchor material ratio of 40% was prepared in a room at 20°C using 90 parts by mass of cement, 5 parts by mass of expansive agent, and 5 parts by mass of plasticizer out of 100 parts by mass of anchor fixing material consisting of cement, expansion agent, and plasticizer, and the compressive strength, flow immediately after mixing (immediately after the flow cone was removed and after 15 strokes), and change in length were measured. The method of judging the change in length was the same as in Experiments 1 to 6. As a comparative example without adding a plasticizer, a cement paste with a water / anchor fixing material ratio of 40% was similarly tested using 95 parts by mass of cement and 5 parts by mass of expansive agent out of 100 parts by mass of anchor fixing material. The test results are shown in Table 2.

[0036] (Materials used) Water: Tap water Cement: Ordinary Portland cement, commercially available Expanding agent: 30 parts of Elimite, 1.5 parts of Ternesite (No. 4 used in Experiment 1) Plasticizer B: Silica fume with SiO2 content of 84.1%, specific surface area (BET) of 20m 2 / g Plasticizer B: Silica fume with SiO2 content of 90.9%, specific surface area (BET) of 33m 2 / g Plasticizer: Silica fume with SiO2 content of 95.8%, specific surface area (BET) of 18m 2 / g Plasticizer 2: Silica fume with SiO2 content of 98.5%, specific surface area (BET) of 74m 2 / g Plasticizer E: Silica fume with SiO2 content of 98.7%, specific surface area (BET) of 20m 2 / g To plasticizer: Silica fume with SiO2 content of 99.3%, specific surface area (BET) of 45m 2 / g (same as the plasticizer used in Experimental Example 1)

[0037] [Table 2]

[0038] From Table 2, it can be seen that by using a plasticizer with a specific SiO2 and a specified specific surface area, good plasticity and sufficient flow spread at 15 strokes can be obtained. In the comparative example, Test No. 13, the flow value immediately after the flow cone was removed was large, so there was a high possibility that the material would flow out during construction in the horizontal or upward direction. The evaluation based on the length change measurement was ○ (expansion strain was -200×10 -6 ~1000×10 -6 ) was. [Industrial Applicability]

[0039] The anchor fixing material of the present invention can be suitably used in the fields of civil engineering and construction.

Claims

[Claim 1] The composition comprises a cement, an expanding agent, and a plasticizer, the expanding agent containing eelimite and ternesite, and a mass ratio of the eelimite to the ternesite (eelimite / ternesite) is 1 to 40; The plasticizer contains SiO 2 , the amount of the SiO 2 being 85 parts by mass or more per 100 parts by mass of the plasticizer, and the anchor fixing material is silica fume having a BET specific surface area of ​​5 m 2 / g to 70 m 2 / g.

Citation Information

Patent Citations

  • Compound for cable bolt anchoring material

    JP1997112198A

  • Fixing-element fixing material

    JP2006161461A

  • Rapid-hardening cement composition for anchor element fixing material, anchor element fixing material, and method of fixing anchor element

    JP2006335586A

  • Mortar composition, coating material, and spray material

    JP2007084420A

  • Element fixation capsule comprising quick hardening component

    JP2009114000A