Process for preparing composite anodes for lithium-ion batteries
A composite anode process for lithium-ion batteries, using graphite and PVDF, addresses cycle life and capacity issues by forming a composite with improved peel strength and capacity retention, suitable for electric vehicles and satellites.
Patent Information
- Application Number
- JP2022511046
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-20
- Filing Date
- 2020-07-07
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-07-07
AI Technical Summary
Existing high-capacity anode materials for lithium-ion batteries face limitations in cycle life due to high volume change during cycling, which is critical for applications like satellites, and combinations of graphite with non-graphitizable carbon result in lower capacity and density issues.
A process involving mixing active materials like spherical and flaky graphite with a binder such as PVDF in a solvent, coating onto a copper foil substrate, and calendering at controlled temperatures to form a composite anode with improved peel strength, specific capacity, and capacity retention.
The composite anode achieves over 80% capacity retention after 2000 cycles and exhibits specific capacities of 345-365 mAh/g, enhancing battery performance for applications like electric vehicles and satellites.
Smart Images

Figure 0007583790000001 
Figure 0007583790000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for preparing a composite anode for a lithium ion battery, particularly to a process for preparing a composite anode for a lithium ion battery having excellent peel strength, specific capacity and capacity retention. [Background technology]
[0002] In recent years, lithium-ion batteries have attracted considerable attention as power sources for a variety of applications, namely, mobile phones, cameras, laptops, and high technology applications such as military, aviation, space and electric vehicles.
[0003] In general, the main components of a lithium-ion battery include a cathode, an anode, an electrolyte, and a separator. The performance of a lithium-ion battery is affected by the properties of the electrodes used, which depend on the type of materials used, the electrode composition, and the electrode manufacturing technology.
[0004] Lithiated transition metal oxides / phosphates are used as the cathode, graphite / carbon as the anode, and lithium salts dissolved in organic solvents as the electrolyte in lithium-ion batteries. The anode materials used in lithium-ion batteries should exhibit high specific capacity, good cycle performance, rate capability, and safety characteristics. In some cases, such as satellite applications, it is required that the battery should exhibit a sloped discharge curve rather than a flat one so that the state of charge at any point in time can be predicted by checking the battery voltage.
[0005] Electronic devices for modern applications require high energy lithium ion batteries which necessitate the use of high capacity anode materials.
[0006] A significant amount of research has been conducted to develop anode materials for use in lithium-ion batteries that have particular characteristics, electrode compositions, and the processes in which they are employed.
[0007] US Pat. No. 5,399,433 deals with a composite anode consisting of an active material such as Si, graphite and a binder.
[0008] US Pat. No. 5,399,633 deals with negative electrodes made of active materials such as tin, tin alloys, silicon, silicon alloys, and the like.
[0009] US Pat. No. 5,399,433 and US Pat. No. 5,499,443 deal with lithium-ion batteries containing Si- or Sn-based anodes.
[0010] US Pat. No. 5,399,633 deals with metal alloy / intermetallic particles as anode active materials.
[0011] Patent Document 6 discloses a negative electrode for a lithium ion battery, the active material of which is a mixture of a carbonaceous material, graphite, and nano-metal particles selected from the group consisting of Ag, Zn, Al, Ga, In, Si, Ge, Sn, and Pb.
[0012] The main problem associated with prior art high capacity anode materials is that the high volume change during cycling limits the cycle life, a key parameter especially for critical applications in satellites.
[0013] As far as cycle life is concerned, especially for satellite applications, the most suitable active material is graphite due to its excellent electrochemical characteristics. In order to improve the performance of graphite anodes, attempts have been made to composite graphite with various carbonaceous materials.
[0014] US Patent No. 5,399,633 discloses a graphite-based composite electrode containing graphite and non-graphitizable carbon: particles of said material comprise a graphite core provided with a surface layer of non-graphitizable carbonaceous material.
[0015] Patent Document 8 discloses a lithium ion battery in which the carbon material for the anode contains both graphite and non-graphitizable carbon material.
[0016] Graphite has a higher true density than non-graphitizable carbon materials and therefore exhibits high electrode packing when used in an anode. The lower true density of non-graphitizable carbon and the lower intercalation capacity of lithium ions into non-graphitizable carbon are the main drawbacks of non-graphitizable carbon anodes.
[0017] US Patent No. 5,399,633 discloses an anode composition consisting of a mixture of graphite and coke, but because coke has a lower capacity compared to graphite, the mixture provides a lower capacity.
[0018] In the prior art of composite anodes, graphite is used in combination with non-graphitizable carbon, low crystalline carbon, graphitized microbead carbon particles or coke. The drawback of these materials is their low capacity compared to graphite. Therefore, this combination results in a lower capacity. Also, graphite has a higher true density than these materials, and therefore shows a higher electrode filling when used in the anode.
[0019] It would therefore be advantageous to provide an effective composite anode that has desirable anode properties such as excellent specific capacity and cycle life, loading level, thickness, moisture content and peel strength, as well as maximum packing efficiency, resulting in improved interparticle conductivity and packing density, and thus improving the overall specific capacity and rate capability of the battery. [Prior art documents] [Patent documents]
[0020] [Patent Document 1] UA2008 / 0206641A1 [Patent Document 2] US8,354,189B2 [Patent Document 3] US2013 / 0216910A1 [Patent Document 4] US2014 / 0234719A1 [Patent Document 5] US2009 / 0305131A1 [Patent Document 6] JP2004213927A [Patent Document 7] US5,908,715 [Patent Document 8] EP627,777 [Patent Document 9] US5,958,622 Summary of the Invention
[0021] An object of the present invention is to provide a process for preparing a composite anode for lithium ion batteries, for lithium ion batteries with excellent anode properties for various applications including electric vehicles, launch vehicles, satellites, submarines, aircraft, etc., comprising: (i) forming an anode slurry in a planetary mixer by mixing active material, binder and solvent; (ii) coating the slurry on a copper foil substrate in a coater at a speed of 0.3-1.0 m / min; and (iii) calendering the anode in a calendering machine at a temperature of 50-130° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] For the purposes of the following detailed description, it is to be understood that the present invention can assume various alternative variations and sequences of steps, unless expressly specified otherwise. Moreover, other than in any examples or unless otherwise indicated, all numbers expressing amounts of ingredients used herein, for example, should be understood to be modified in all cases by the term "about". It should be noted that all percentages shown in this specification and the appended claims refer to weight percentages of the total composition, unless otherwise specified.
[0023] Therefore, before describing the present invention in detail, it is to be understood that this invention is not limited to specific illustrated system or method parameters, which may, of course, vary. It is also to be understood that the terminology used herein is for the purpose of describing particular embodiments of the present invention only, and is not intended to limit the scope of the present invention in any way.
[0024] The use of examples anywhere in this specification, including examples of any term discussed herein, is illustrative only and in no way limits the scope and meaning of the invention or of any exemplified term. Similarly, the invention is not limited to the various embodiments provided herein.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. In case of conflict, the present document including definitions will control.
[0026] It should be noted that as used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the content clearly dictates otherwise. Thus, for example, reference to a "polymer" may include two or more such polymers.
[0027] The terms "preferred" and "preferably" refer to embodiments of the invention that may provide certain benefits, under particular circumstances. However, other embodiments may also be preferred, under the same or other circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.
[0028] As used herein, the terms "comprising," "including," "having," "containing," "involving," and the like, should be understood to be open-ended, i.e., meaning including but not limited to.
[0029] In one aspect, the present application provides a process for preparing a composite anode for a lithium ion battery, comprising the steps of: i. forming an anode slurry in a planetary mixer by mixing an active material, a binder, and a solvent; ii. Coating the slurry on the copper foil substrate in a coating machine at a speed of 0.3 to 1.0 m / min; and iii. Calendering the anode in a calender at a temperature between 50 and 130°C; Includes.
[0030] In one embodiment, the anode slurry is prepared in a planetary mixer by mixing the active material and binder in the presence of a solvent. The anode slurry according to the present invention is made in a planetary mixer by dry mixing the active material, followed by addition of the binder, and then addition of the solvent.
[0031] In one embodiment, the active material is selected from spherical graphite, flake graphite, non-graphitizable carbon, mesocarbon microbeads, etc. In a preferred embodiment, the active material is spherical graphite and flake graphite.
[0032] In one embodiment, the binder is selected from polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene), and the like. In a particular embodiment, the binder is polyvinylidene fluoride. The binder provides good adhesion between the components in the electrode as well as binding the components on the substrate. The binder must be compatible with the materials used in the battery and must exhibit electrochemical stability in the operating potential window of the battery.
[0033] In one embodiment, the solvent is selected from 1-methyl-2-pyrrolidinone (NMP), dimethylacetamide (DMAC), dimethylformamide (DMF), etc. In a preferred embodiment, the solvent is 1-methyl-2-pyrrolidinone. The role of the solvent is to dissolve the binder to provide better mixing of the components in the slurry.
[0034] This process involves drying the ingredients before mixing in a planetary mixer. The moisture content in the electrode is an important factor affecting the efficiency, reversible capacity and cycle life of a lithium-ion battery. Therefore, the ingredients used in the anode slurry preparation are dried before mixing to remove moisture.
[0035] Dry the powdered materials except PVDF under vacuum at 150-230°C for 20-36 hours. Dry PVDF at a lower temperature. Dry PVDF under vacuum at 600-700mmHg at 50-80°C for 2-7 hours.
[0036] Formation of the anode slurry by mixing the active material and binder in the presence of a solvent is performed in a planetary mixer. The components of the anode are fed into the planetary mixer through an inlet. The planetary mixer includes a planetary blade and a high speed disperser. Mixing the components in the planetary mixer ensures uniform mixing of the components and avoids crushing of the active material, thereby helping to achieve an anode with superior performance characteristics.
[0037] In one embodiment, the planetary blade speed is in the range of 40-160 rpm and the disperser speed is in the range of 450-600 rpm.
[0038] The order adopted for mixing the components is very important in determining the electrochemical properties of the anode. According to the present disclosure, the anode slurry formation process is carried out in a planetary mixer equipped with a high-speed disperser. The first step of anode slurry preparation involves dry mixing the powdered materials at a slower speed, followed by adding the required amount of PVDF solution. Then, while continuing mixing, NMP is added at different intervals to reduce the viscosity of the anode slurry to the desired level.
[0039] The slurry processing is carried out in a humidity-controlled environment with a relative humidity in the range of 2-15%.
[0040] In a particular embodiment, the viscosity of the slurry ranges from 2000 to 15000 cps at a speed of 100 rpm (measured with a Brookfield Viscometer RVDV-1Prime using spindle S-06). The viscosity of the slurry plays an important role in determining the properties of the electrode. It determines the loading level (adhesion), the controllability of the peel strength, and thereby the performance of the electrode during cycling.
[0041] In one embodiment, the active material is present in an amount ranging from 45 to 55 weight percent based on the total weight of the anode slurry.
[0042] In one embodiment, the binder is present in an amount ranging from 1 to 10 weight percent based on the total weight of the anode slurry.
[0043] In one embodiment, the solvent is present in an amount in the range of 45 to 55 weight percent based on the total weight of the anode slurry.
[0044] The composition of the electrode is very important in determining its electrochemical properties. The concentration of active material in the electrode determines the discharge capacity by the electrode. The binder provides adhesion between the components in the electrode as well as binding the components on the substrate. High active material concentration results in high capacity. However, optimal concentrations of conductive diluents and binders are required for good cycle life and rate capability of the battery.
[0045] In a further step, the process includes coating the anode slurry onto a copper foil substrate in a coating machine. In one embodiment, the copper foil substrate is in the range of 8 to 15 μm thick.
[0046] Coating of the anode slurry onto the copper foil substrate is done in a coating machine. The anode slurry formed in the planetary mixer is transferred to the coating machine. The coating machine operates in a reverse comma mode. The gap between the reverse comma blade and the applicator is first adjusted to obtain the desired loading level of active material on the copper foil substrate. In one embodiment, the gap setting is in the range of 100-300 μm. Optimal coating speed and drying temperature are required to completely remove the solvent and obtain an electrode without defects such as cracks, peeling of active material, etc.
[0047] Coating the anode slurry according to the present disclosure includes a) feeding the slurry into a slurry dam to initiate coating, b) transferring the slurry to the foil based on thickness between the applicator and a reverse comma blade, c) passing the slurry coated foil through two heating zones, and d) completing coating on one side of the foil and then flipping to create the coating on the other side of the foil.
[0048] The coater includes multiple heating zones. The foil coated with the slurry passes through the heating zones. After completing the coating on one side of the foil, it is turned over to produce the coating on the other side of the foil. The coating speed and temperature values are determined based on the drying of the anode after passing through the two heating zones.
[0049] In one embodiment, the anode is dried in a heating zone in the coater at a temperature in the range of 50-150°C.
[0050] The dried anode is then finally wound into a roll. In one embodiment, the coating speed is in the range of 0.3-0.8 m / min.
[0051] The coating environment plays an important role in determining the properties of the electrode. The coating process is carried out at a relative humidity in the range of 2-15%. The coated anode is dried under vacuum at a temperature in the range of 60-100°C. In one embodiment, the thickness of the coated anode is in the range of 150-250 μm. In one embodiment, the anode is dried under vacuum in the range of 600 mmHg-700 mmHg for 15 hours to 25 hours.
[0052] In a next step, the process includes calendering the anode in a calender. In one embodiment, the calendering of the anode is performed at a speed of 0.5-3 m / min. In one embodiment, the calendering of the anode is performed in the calender at a temperature in the range of 50-150° C.
[0053] The calender includes a preheat zone and two heated rolls for pressing the anode. The anode thus formed in roll form according to the present disclosure passes through the preheat zone and is pressed in the rollers of the calender to a thickness of 100-200 μm at a speed of 0.5-3 m / min.
[0054] In one embodiment, the temperature of the preheat zone is in the range of 80-150° C. In one embodiment, the temperature of the calender rolls is in the range of 50-100° C.
[0055] The anode thus formed according to the present disclosure is assembled with a cathode to form a lithium ion battery. The lithium ion battery thus formed exhibited excellent battery characteristics. 0.8 Co 0.15 Al 0.05 Lithium-ion batteries with O2-based cathodes showed a capacity retention rate of over 80% at 100% depth of discharge at a C / 2-1C charge / discharge rate when tested for 2000 cycles.
[0056] In one embodiment, the peel strength of the anode is in the range of 10 to 40 gf / cm, and in a preferred embodiment, the peel strength is in the range of 10 to 20 gf / cm.
[0057] In one embodiment, the specific capacity of the anode is in the range of 345 to 365 mAh / g. In a preferred embodiment, the specific capacity is in the range of 350 to 355 mAh / g.
[0058] In one embodiment, the capacity retention of a battery having an anode according to the present invention is 0.8 Co 0.15 Al 0.05 When tested at C / 2 charge rate and 1C discharge rate against O2, it exceeds 80% at 2000 cycles.
[0059] The composite anode for lithium ion batteries according to the present disclosure includes, except for copper foil, (i) graphite (spherical): 60-80%, (ii) graphite (flake): 10-30%, PVDF: 2-10%. In some embodiments, the active material in the composite anode may also be mesocarbon microbeads, non-graphitizable carbon, Si, etc.
[0060] The following examples are provided to better illustrate the claimed invention and should not be interpreted as limiting the scope of the invention in any way. All specific materials and methods described below are within the scope of the invention. These specific compositions, materials, and methods are not intended to limit the invention, but are merely intended to illustrate specific embodiments within the scope of the invention. Those skilled in the art can develop equivalent materials and methods without exerting the capacity of the invention and without departing from the scope of the invention. It is the intention of the inventors that such variations are included within the scope of the invention. EXAMPLES
[0061] The preparation of a composite anode for lithium ion batteries having excellent battery properties is described in the following examples.
[0062] Example 1 The electrode fabrication of the mixed graphite based composite anode is described below.
[0063] The composite anode is made of a mixture of spherical and flake graphite as the active material and polyvinylidene fluoride (PVDF) as the binder. The electrode composition is graphite (spherical): 70-75%, (ii) graphite (flake): 20-25%, PVDF: 4-6%. The particle size of the spherical graphite is 15-30 μm (D 50 ), and the particle size of the flake graphite is 15 to 35 μm (D 50 ) The electrode slurry is processed using 1-methyl-2-pyrrolidinone (NMP) as a solvent. The graphite powder and PVDF are dried under vacuum before mixing. The electrode fabrication includes slurry preparation, electrode coating and calendering.
[0064] The slurry preparation is carried out in a planetary mixer equipped with a high speed disperser. The slurry preparation involves dry mixing of spherical and flake graphite powders in the mixer at a planetary blade speed of 50-70 rpm and disperser speed of 450-500 rpm, followed by addition of polyvinylidene fluoride solution and addition of NMP at different intervals while continuing mixing at a planetary blade speed of 50-150 rpm. The volume of NMP is adjusted to obtain a slurry solids content of 50-54%.
[0065] The electrode coating is carried out in a coating machine working in reverse comma mode. Copper foil with a thickness of 10-12 μm was used for coating. The gap between the reverse comma blade and the applicator is adjusted to obtain a gap of 150-200 μm. The slurry is loaded into the slurry dam and coating is carried out. Coating is carried out at a speed of 0.3-0.7 m / min. The temperature in the heating zone is kept at 80-120 °C. The electrodes after drying are recovered in roll form from the machine. The electrodes are then dried under vacuum at 70 °C for 15-20 hours. The thickness of the electrodes after double-sided coating is 200-260 μm.
[0066] Calendering of the electrode is carried out in a calendering machine equipped with a preheat zone and calender rolls. The preheat temperature is 100-120° C. and the temperature of the calendering rolls is 50-80° C. The electrode in roll form is passed through the preheat rolls and calender rolls at a speed of 1-2 m / min to obtain a final electrode thickness of 140-170 μm.
[0067] Example 2 The electrode fabrication of the mixed graphite based composite anode is described below.
[0068] The composite anode consists of a mixture of spherical and flake graphite as active material and polyvinylidene fluoride (PVDF) as binder. The electrode composition is (i) graphite (spherical): 71-73%, (ii) graphite (flake): 21-24%, PVDF: 5-7%. 1-methyl-2-pyrrolidinone (NMP) is used as a solvent for processing the electrode slurry. The graphite powder and PVDF are dried under vacuum before mixing. The electrode fabrication includes slurry preparation, electrode coating and calendering.
[0069] The slurry preparation is carried out in a planetary mixer equipped with a high speed disperser. The PVDF solution is prepared in the planetary mixer by adding 1-methyl-2-pyrrolidinone to the PVDF in the planetary mixer at different time intervals while continuing mixing. The slurry preparation involves dry mixing of spherical and flake graphite powders in the mixer at a planetary blade speed of 50-60 rpm and a disperser speed of 500-550 rpm, followed by adding the prepared polyvinylidene fluoride solution and adding NMP at different intervals while continuing mixing at a planetary blade speed of 50-150 rpm. The volume of NMP is adjusted to obtain a slurry solids content of 48-52%.
[0070] The electrode coating is carried out in a coating machine working in reverse comma mode. Copper foil with a thickness of 10-12 μm was used for coating. The gap between the reverse comma blade and the applicator is adjusted to obtain a gap of 100-150 μm. The slurry is loaded into the slurry dam and coating is carried out. Coating is carried out at a speed of 0.5-0.9 m / min. The temperature in the heating zone is kept at 80-120 °C. The electrodes after drying are recovered in rolls from the machine. The electrodes are then dried under vacuum at 70 °C for 15-20 hours. The thickness of the electrodes after double-sided coating is 120-160 μm.
[0071] Calendering of the electrode is carried out in a calendering machine equipped with a preheating zone and calender rolls. The preheating temperature is 100-120° C. and the temperature of the calendering rolls is 50-80° C. The electrode in roll form is passed through the preheating rolls and calender rolls at a speed of 1-2 m / min to obtain a final electrode thickness of 100-130 μm.
[0072] TIFF0007583790000001.tif47170
[0073] TIFF0007583790000002.tif43170
Claims
1. 1. A process for preparing a composite anode for a lithium ion battery, comprising: i. forming an anode slurry in a planetary mixer by mixing an active material, a binder, and a solvent; ii. Coating the slurry on a copper foil substrate in a coating machine at a speed of 0.3-1.0 m / min; iii. Calendering the anode in a calender at a temperature of 50-150° C.; Including, the active material is a mixture of spherical graphite and flake graphite, the binder is polyvinylidene fluoride; the solvent is 1-methyl-2-pyrrolidinone; the amount of the binder is in the range of 1 to 15 wt %, based on the total weight of the anode slurry, and the amount of the solvent is in the range of 45 to 55 wt %, based on the total weight of the anode slurry; step (i) comprises forming the anode slurry of viscosity in the range of 2000-15000 cps by dry mixing the active material, followed by adding a binder solution, and then adding the solvent at different time intervals; process.
2. 10. The process of claim 1 including drying the active material and the binder prior to mixing in the planetary mixer.
3. 2. The process of claim 1, wherein the amount of the spherical graphite ranges from 30 to 40 wt. %, based on the total weight of the anode slurry.
4. 2. The process of claim 1, wherein the amount of the flake graphite ranges from 5 to 15 weight percent based on the total weight of the anode slurry.
5. The process of claim 1, wherein the copper foil substrate is in the range of 8 to 15 μm thick.
6. The process of claim 1, wherein the thickness of the anode after coating is in the range of 200 to 300 μm.
7. The process of claim 1, wherein the final thickness of the anode after calendering is in the range of 100 to 200 μm.
8. 10. The process of claim 1, wherein the relative humidity of the process environment in which the electrode fabrication takes place is in the range of 2-15%.
9. 2. The process of claim 1, comprising drying the anode after coating in a drying zone at a temperature in the range of 50 to 150°C.
10. 2. The process of claim 1, wherein the calendering of the anode is carried out at a speed of 0.5 to 3 m / min and at a temperature in the range of 50 to 150°C.
Citation Information
Patent Citations
EP627,777
Manufacture of negative electrode mix of nonaqueous secondary battery
JP1996195201A
Nonaqueous secondary battery and manufacture thereof
JP2000011997A
Lithium secondary battery and anode
JP2002175810A
Non-aqueous secondary battery
JP2003068301A