Composite positive electrode material, its manufacturing method and lithium ion battery
A composite positive electrode material with a phosphoric acid compound coating layer addresses coating uniformity and structural stability issues, enhancing conductivity and cycle stability, and reducing manufacturing costs through an atomization coating method.
Patent Information
- Application Number
- JP2022516734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-16
- Filing Date
- 2022-02-18
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2042-02-18
AI Technical Summary
Conventional lithium-ion battery positive electrode materials face issues with coating uniformity, structural stability, and high impedance due to particle cracking and uneven coating, leading to poor rate characteristics and cycle stability, with manufacturing methods like liquid and solid phase coating having limitations.
A composite positive electrode material with a phosphoric acid compound coating layer on the surface of active material particles, manufactured through an atomization coating method, ensuring high particle hardness and uniform coating distribution, thereby improving conductivity and cycle stability.
The composite material achieves low impedance, high thermal stability, and excellent cycle stability by enhancing particle hardness and conductivity, while reducing manufacturing costs through improved coating uniformity and reaction activity.
Smart Images

Figure 0007583796000002 
Figure 0007583796000003 
Figure 0007583796000004
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of cathode materials, in particular to a composite cathode material, its manufacturing method and a lithium ion battery. [Background technology]
[0002] Lithium-ion batteries have the advantages of high energy density, high power output, long cycle life, and less environmental pollution, and are therefore widely used in electric vehicles and consumer electronic products. Improving the rate characteristics, thermal stability, and cycle stability of lithium batteries has always been the research direction of developers. After long-term cycles, traditional high-nickel positive electrode materials are prone to particle cracking, directly exposing the internal structure, which often impairs the long-term cycle stability of the positive electrode material and impairs the rate characteristics of lithium batteries. In addition, as a conventional method for producing a positive electrode material, for example, a method for mixing a coating material in a liquid phase can be mentioned, but in the case of the liquid phase method, the surface structure of the positive electrode material is easily destroyed, there is a lot of Li / Ni mixing of the material, the structural stability is poor, and the coating material is easily washed away with the solution, so that it is difficult to control the coating amount. In addition, a solid phase coating method can be mentioned, but the positive electrode material obtained by the solid phase coating has a lot of residual lithium, which affects the processing performance of the positive electrode material, and the coating is also uneven.
[0003] Therefore, there is an urgent need to provide a composite positive electrode material and a manufacturing method thereof that can improve the coating uniformity, further improve the rate characteristics and cycle stability of lithium batteries, and reduce the manufacturing cost. Summary of the Invention [Problem to be solved by the invention]
[0004] In view of the above circumstances, the present invention provides a composite positive electrode material that can improve coating uniformity, accurately control the coating amount, improve the rate characteristics and cycle stability of a lithium battery, and reduce production costs, a manufacturing method thereof, and a lithium ion battery. [Means for solving the problem]
[0005] According to a first aspect of the present invention, General formula: Li a (Ni x Co y R z ) 1-b M b O2 (wherein, 0.9≦a≦1.10, x+y+z=1, 0.8≦x≦0.99, 0≦y≦0.15, 0≦z≦0.1, 0≦b≦0.1, R includes Al and / or Mn, and M includes a metal element); and a coating layer comprising a phosphate compound and distributed on the surface of the active material. The composite positive electrode material has a particle hardness Cs of 50 MPa or more, and Cs 10 / Cs 50 ≧0.7 (where Cs 10 is the hardness of a particle with a diameter of D10, and Cs 50 is the hardness of a particle with a particle size of D50.
[0006] In the above-mentioned technical solution, the coating layer distributed on the surface of the active material contains a phosphate compound, which not only provides the positive electrode material with low impedance, high rate, high thermal stability and excellent cycle stability, but also repairs the surface defects of small particles through coating modification, reduces Li / Ni mixing and greatly improves particle hardness.
[0007] In one embodiment of the first aspect, the composite positive electrode material satisfies at least one of the following conditions a to c: a. The Li a (Ni x Co y R z ) 1-b M b M in O2 includes at least one selected from Mg, Sr, Ca, Ba, Ti, Zr, Mn, Y, Gd, W, Nb, La, and Mo; b. Intensity I of the X-ray diffraction peak corresponding to the (003) crystal plane of the active material 003and the intensities of the X-ray diffraction peaks corresponding to the (104) crystal plane I 104 The ratio of is 1.25 or more; c. The Li ions contained in the active material occupy 98% or more of the Li sites of the crystal lattice.
[0008] In one embodiment of the first aspect, the composite positive electrode material satisfies at least one of the following conditions a to e: a. The phosphate compound is Li3PO4 or LiXPO4 (wherein X is Na, K, Al, Sr, Zr, B, Mg, Ba, Contains at least one selected from Ca, Co, and W; b. the content of the phosphate compound in the coating layer is 0.05 wt % to 1.5 wt % based on the mass of the active material; c. the powder conductivity of the composite positive electrode material is 0.001 S / cm to 0.1 S / cm; d. The specific surface area of the composite positive electrode material is 0.2 m 2 / g~2.0m 2 / g; e. The average particle size of the composite positive electrode material is 3 μm to 20 μm. In the present invention, the term "particle size" refers to the maximum linear length of a particle, that is, the maximum linear distance between two points on the periphery of the particle. In the present invention, "D10" refers to the particle size at which the particle size reaches 10% by number from the small particle side in the cumulative particle size distribution of the particles, that is, the number of particles having a particle size of D10 or less is 10% of the total number of particles. In the present invention, "D50" refers to the particle size at which the particle size reaches 50% by number from the small particle side in the cumulative particle size distribution of particles, that is, the number of particles having a particle size of D50 or less is 50% of the number of all particles.
[0009] According to a second aspect of the present invention, A process for obtaining a sintered product by mixing a main component, a subcomponent and a lithium compound and then sintering the mixture, the main component being Ni x Co y R z O, Ni x Coy R z (OH)2 or Ni x Co y R z OOH (wherein, in each of the above formulae, x+y+z=1, 0.8≦x≦0.99, 0≦y≦0.15, 0≦z≦0.1), the subcomponent comprises at least one selected from an oxide of M, a hydroxide of M, or a phosphate of M, where M comprises a metal element and R comprises Al and / or Mn; crushing, washing and filtering the sintered product to obtain an active material cake; a step of performing a coating treatment using a coating solution containing phosphate ions and lithium ions and the active material cake by an atomization method to obtain a composite positive electrode material, the composite positive electrode material having an active material and a coating layer distributed on a surface of the active material, the coating layer containing a phosphate compound.
[0010] In this technical proposal, the atomized coating method is adopted, which can avoid the loss of coating dissolved in the solution due to filtration in the conventional liquid phase coating method, improve the accuracy of the coating amount, and improve the coating uniformity and reaction activity compared with solid phase coating. During the atomized coating process, the phosphate coating solution forms micro- and nano-structured droplets, which have higher adsorption properties and can improve the reaction activity during the mixing process with the active material. The coating is easy to be uniformly embedded in the pores of the active material (lithium-nickel-cobalt-aluminum composite oxide or lithium-nickel-cobalt-manganese composite oxide), which repairs the surface defects of the active material, resulting in a uniform coating, improving the particle hardness, and forming a network with high lithium ion conductivity on the surface of the primary particles of the active material, which can significantly reduce the impedance of the active material and optimize the electrochemical performance of the active material. And since the specific surface area of the small particles in the composite positive electrode material is larger and more surface defects can be formed during the washing process, the particle hardness of the small particles is lower than that of the large particles, but the particle hardness of the small particles is lower than that of the large particles due to the coating with the sprayed phosphate. 10 / Cs 50The hardness of the small particles can be significantly improved to meet ≧0.7, so that during the manufacturing process of the electrode sheet, the small particles can exhibit higher pressure resistance, improve the compression density of the electrode sheet, and also improve the energy density of the battery.
[0011] In one embodiment of the second aspect, the method satisfies at least one of the following conditions a to d: a. The amount of the lithium compound added is such that the ratio of the sum of the molar contents of Ni, Co, and R in the main component to the molar content of Li is 1:(0.9 to 1.10); b. The sintering conditions for obtaining the sintered product are to heat the mixture to 650°C to 850°C in an oxygen-containing atmosphere and sinter for 5 hours to 20 hours; c. the average particle size of the main component is 3 μm to 20 μm; d. The lithium compound includes at least one selected from lithium hydroxide, lithium carbonate, lithium acetate, lithium nitrate, and lithium oxalate.
[0012] In one embodiment of the second aspect, the method satisfies at least one of the following conditions a to d: a. the washing temperature is 10°C to 40°C, and the washing time is 10 min to 60 min; b. The amount of the cleaning solvent used satisfies the following: sintered product (g) / amount of cleaning solvent used (L) = 500 g / L to 2000 g / L; c. the filtration time is 30 min to 150 min, and the water content of the active material cake is 5 wt % or less; d. The filtration includes at least one selected from pressure filtration and suction filtration.
[0013] In one embodiment of the second aspect, before performing a coating process using a coating solution containing phosphate ions and lithium ions and the active material cake by a mist coating method, the method includes: The method further includes dissolving a phosphorus source and a soluble lithium compound in an aqueous solution to obtain a coating solution containing phosphate ions and lithium ions.
[0014] In one embodiment of the second aspect, the method satisfies at least one of the following conditions a to e: a. the phosphorus source is HPO3, H3PO2, H3PO4, Li3PO4, K3PO4, BPO4, NH4H2PO4, (NH4)2HPO4, Zr(HPO4)2, Na2HPO4, SrHPO4, BaHPO4, Ba3(PO4)2, MgHPO4, Ca(H2PO2)2, Al(H2PO4)3, CoHPO4, or H3P(W3O 10 )4·nH2O (wherein n ≧1); b. the soluble lithium compound includes at least one selected from lithium hydroxide, lithium carbonate, lithium nitrate, lithium chlorate, and lithium acetate; c. In the coating solution, the molar ratio of the lithium ions to the phosphate ions is (0-10):1; d. the mass of phosphate ions in the phosphorus source is 0.05 wt% to 1.5 wt% based on the active material cake; e. The total mass of the phosphorus source and the soluble lithium compound is 1.5 wt % to 45 wt % with respect to the coating solution.
[0015] In one embodiment of the second aspect, the method satisfies at least one of the following conditions a to b: a. the atomization method includes at least one selected from ultrasonic atomization and high-pressure atomization; b. During the coating process, the coating temperature is controlled to 50°C to 100°C, and the heat retention time is controlled to 5 minutes to 60 minutes.
[0016] In one embodiment of the second aspect, after the coating process, the method further comprises: The method further includes a step of drying the composite positive electrode material, controlling the drying temperature to 150° C. to 210° C. and the warming time to 10 hours to 24 hours.
[0017] According to a third aspect of the present invention, there is provided a lithium ion battery including a positive electrode sheet, a negative electrode sheet, a separator, a non-aqueous electrolyte, and an outer case, The positive electrode sheet provides a lithium ion battery including a current collector and the composite positive electrode material according to the first aspect or the composite positive electrode material produced by the method for producing a composite positive electrode material according to the second aspect, applied to the current collector. Effect of the Invention
[0018] The present invention can provide at least the following beneficial effects:
[0019] The composite positive electrode material according to the present invention has a coating layer distributed on the surface of the active material, and the active material has a high crystallinity, which can contribute to improving the conductive performance of the positive electrode material. In addition, the gap between the surface of the active material and the active material is filled or coated with a phosphate compound, which can significantly improve the conductivity of the active material, and not only can the positive electrode material have low impedance, high rate, high thermal stability, and excellent cycle stability, but the coating-modified composite positive electrode material can also repair defects on the particle surface, improve particle hardness, and contribute to improving the processing performance of the material.
[0020] The method for producing the composite positive electrode material according to the present invention adopts the atomized coating method, which can avoid the loss of the coating dissolved in the solution due to filtration in the conventional liquid phase coating method, improve the accuracy of the coating amount, and improve the coating uniformity and reaction activity compared with solid phase coating. During the atomized coating process, the phosphate coating solution forms micro- and nano-structured droplets, which have higher adsorption properties and can improve the reaction activity during the mixing process with the active material, and the coating is easily uniformly embedded in the pores of the active material (lithium-nickel-cobalt-aluminum composite oxide or lithium-nickel-cobalt-manganese composite oxide), repairing the surface defects of the active material, resulting in a uniform coating, improving the particle hardness, and forming a network with high lithium ion conductivity on the surface of the primary particles of the active material, thereby significantly reducing the impedance of the active material and optimizing the electrochemical performance of the active material. Furthermore, the manufacturing method according to the present invention is simple, mass-produced, and can reduce costs. [Brief description of the drawings]
[0021] [Figure 1] 1 is a flowchart of a method for producing a composite positive electrode material used in an embodiment of the present invention. [Diagram 2] 1 is a SEM image of the composite positive electrode material prepared in Example 1 of the present invention. [Figure 3a] 1 is a SEM image of a local area of the composite positive electrode material prepared in Example 1 of the present invention. [Figure 3b] 1 is an elemental mapping of phosphorus by energy dispersive X-ray analysis of the composite positive electrode material produced in Example 1 of the present invention. [Figure 4] 1 is a SEM image of the composite positive electrode material prepared in Comparative Example 1 of the present invention. [Figure 5a] 1 is a SEM image of a region of the composite positive electrode material prepared in Comparative Example 1 of the present invention. [Figure 5b] 1 is an elemental mapping of phosphorus by energy dispersive X-ray analysis of the composite positive electrode material produced in Comparative Example 1 of the present invention. [Figure 6] FIG. 2 is a comparative diagram of the capacity retention rates of batteries manufactured using the composite positive electrode materials manufactured in Example 1 of the present invention and Comparative Example 1. [Figure 7] FIG. 2 is a comparison diagram of the DC internal resistance of batteries manufactured using the composite positive electrode materials prepared in Example 1 and Comparative Example 1 of the present invention. [Figure 8] FIG. 2 is a comparison diagram of the impedance of batteries manufactured using the composite positive electrode materials manufactured in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The following describes preferred embodiments and examples of the present invention, and it is understood that those skilled in the art can make some improvements and modifications without departing from the principles and spirit of the present invention, and these improvements and modifications are also within the scope of protection of the present invention.
[0023] According to a first aspect of the present invention, there is provided a composite positive electrode material having an active material and a coating layer distributed on a surface of the active material, The active material has the general formula: Li a (Ni x Co y R z ) 1-b M b O2 (wherein 0.9≦a≦1.10, x+y+z=1, 0.8≦x≦0.99, 0≦y≦0.15, 0≦z≦0.1, 0≦b≦0.1, R includes Al and / or Mn, and M includes a metal element), and the coating layer includes a phosphate compound. The composite positive electrode material has a particle hardness Cs of 50 MPa or more and a Cs 10 / Cs 50 ≧0.7 (where Cs 10 is the hardness of a particle with a diameter of D10, and Cs 50 is the hardness of a particle with a particle size of D50.
[0024] Preferably, M comprises a doping element and includes at least one selected from Mg, Sr, Ca, Ba, Ti, Zr, Mn, Y, Gd, W, Nb, La and Mo.
[0025] In a preferred embodiment of the present invention, the intensity I of the X-ray diffraction peak corresponding to the (003) crystal plane of the active material is 003 and the intensities of the X-ray diffraction peaks corresponding to the (104) crystal plane I 104 The ratio of is 1.25 or more, specifically, it may be 1.25, 1.26, 1.27, 1.28, 1.29, 1.30, 1.32, 1.35, 1.4, etc., but is not limited thereto. It is understood that the larger the intensity ratio of the X-ray diffraction peak corresponding to the specific crystal plane of the active material, the higher the crystallinity of the active material, which is advantageous for improving the conductive performance of the positive electrode material.
[0026] In a preferred embodiment of the present invention, the Li ions contained in the active material have an occupancy rate of the Li sites of the crystal lattice (hereinafter, sometimes abbreviated as "Li site occupancy rate of Li ions") of 98% or more. In addition, the "Li site occupancy rate of Li ions" described in the present invention means the ratio of the number of Li ions occupying the Li sites in the Li layer of the active material crystal lattice to the total number of Li sites. It is understood that the higher the Li site occupancy rate of Li ions, the stronger the discharge capacity of the active material. When the Li site occupancy rate of Li ions in the active material is low, the number of Li ions at the Li sites decreases, Ni, Co, and Al are present at the Li sites, Li / Ni mixing is likely to occur, and defects are likely to occur in the crystal structure of the active material, which may reduce the discharge capacity and cycle characteristics of the active material. In addition, when Li ions leave the crystal structure, they may exist in the form of lithium carbonate, etc., which may cause gas generation and affect the safety of the battery.
[0027] In the present invention, the surface of the active material is coated with a phosphate compound, and the phosphate compound can increase the ionic conductivity of the active material. It is understood that the ionic conductivity of the active material can be significantly improved by filling or coating the surface of the active material and the gaps between the active materials with the phosphate compound, and the positive electrode material can have low impedance, high rate, high thermal stability, and excellent cycle stability.
[0028] Preferably, the phosphate compound is Li3PO4 or LiXPO4 (wherein X is Na, K, Al, Sr, Zr, B, Mg, Ba, It contains at least one of Ca, Co and W and is derived from the metal phosphate compound.
[0029] Preferably, the content of the phosphate compound in the coating layer is 0.05 wt% to 1.5 wt% relative to the mass of the active material, and specifically, it may be 0.05 wt%, 0.08 wt%, 0.1 wt%, 0.2 wt%, 0.5 wt%, 0.8 wt%, 1.0 wt%, 1.2 wt%, or 1.5 wt%, etc., and of course, it may be other values within the above range and is not limited thereto.
[0030] Preferably, the average particle size of the composite positive electrode material is 3 μm to 20 μm, specifically, it may be 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 10 μm, 12 μm, 15 μm, 18 μm, or 20 μm, etc., and of course, it may be other values within the above range, and is not limited here. By controlling the particle size of the composite positive electrode material within the above range, it can contribute to improving the structural stability, thermal stability, and long-term cycle stability of the positive electrode material.
[0031] In a preferred embodiment of the present invention, the composite positive electrode material has a resistance of 20 kN / cm 2 The powder conductivity under pressure is 0.001 S / cm to 0.1 S / cm, ensuring the charge / discharge capacity of the composite positive electrode material.
[0032] In a preferred embodiment of the present invention, the specific surface area of the composite positive electrode material is less than 0.2 m 2 / g~2.0m 2 / g. Specifically, 0.2m 2 / g, 0.5m 2 / g, 0.7m 2 / g, 0.9m 2 / g, 1.1m 2 / g, 1.3m 2 / g, 1.5m 2 / g, 2.0m 2 / g, etc. As a result of extensive research, the inventors have found that controlling the specific surface area of the composite positive electrode material within the above range is advantageous in improving the cycle characteristics of a lithium battery manufactured from the positive electrode material.
[0033] According to a second aspect of the present invention, there is provided a method for producing a composite positive electrode material, as shown in FIG. 1, comprising the following steps S10 to S30.
[0034] <Process S10> In step S10, the main component, the subcomponent and the lithium compound are mixed and then sintered to obtain a sintered product.
[0035] In a preferred embodiment of the present invention, the main component is Ni x Co y R z O, Ni x Co y R z (OH)2 or Ni x Co y R z OOH (wherein x+y+z=1, 0.8≦x≦0.99, 0≦y≦0.15, 0≦z≦0.1, and R includes Al and / or Mn).
[0036] Ni x Co y R z O, Ni x Co y R z (OH)2 and Ni x Co y R z The molar content of Ni in OOH is 0.8≦x≦0.99, and the value range of x may be specifically 0.8, 0.82, 0.84, 0.86, 0.88, 0.9, 0.92, 0.94, 0.96, 0.98, or 0.99, etc. Ni x Co y R z O, Ni x Co y R z (OH)2 and Ni x Co y R z The molar content of Co in OOH is 0≦y≦0.15, and the value range of y may be specifically 0, 0.01, 0.02, 0.05, 0.06, 0.08, 0.1, 0.11, 0.12, 0.14, or 0.15, etc. Ni x Co y R z O, Nix Co y R z (OH)2 and Ni x Co y R z The molar content of R in OOH is 0≦z≦0.1, and the value range of z may be specifically 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, or 0.1, etc.
[0037] Specifically, the average particle size of the main component is 3 μm to 20 μm, specifically, it may be 3 μm, 5 μm, 7 μm, 9 μm, 10 μm, 12 μm, 14 μm, 15 μm, or 20 μm, etc., and of course, it may be other values within the above range, and is not limited thereto. As a result of repeated research, the inventors have found that when the average particle size of the main component is controlled within the range of 3 μm to 20 μm, the particle size of the active material can be effectively controlled, the problem of the active material cracking during the cycle process can be avoided, and it is advantageous to improve the structural stability, thermal stability, and long-term cycle stability of the active material.
[0038] In one embodiment of the present invention, the subcomponent includes at least one selected from an oxide of M, a hydroxide of M, or a phosphate of M, where M is a metal element.
[0039] In one embodiment of the present invention, the lithium compound is at least one selected from lithium hydroxide, lithium carbonate, lithium acetate, lithium nitrate, and lithium oxalate.
[0040] In one embodiment of the present invention, the ratio of the sum of the molar contents of Ni, Co and R in the main component to the molar content of Li is 1: (0.9 to 1.10), specifically, 1:0.9, 1:0.95, 1:0.96, 1:0.97, 1:0.98, 1:0.99, 1:1.00, 1:1.01, 1:1.02, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1.10, etc., and of course, other values within the above range may also be used, and are not limited thereto. If the above ratio is too small, Li becomes excessive, which leads to the formation of a Li2MO3 phase in the surface layer of the material, and the active Li + The content of Li / Ni is reduced, which reduces the capacity and is prone to gas generation during cycling. If the above ratio is too large, Li / Ni mixing becomes serious, which leads to more Li vacancies in the crystal lattice and Ni + may enter the Li layer, causing mixing of the metal layers, resulting in reduced stability of the material structure, material degradation, and reduced cycle characteristics.
[0041] In one embodiment of the present invention, the sintered product is an active material, and the conditions for obtaining the sintered product include heating to 650°C to 850°C in an oxygen-containing atmosphere and sintering for 5h to 20h. By sufficiently sintering, a lithium-nickel-cobalt-aluminum composite oxide or a lithium-nickel-cobalt-manganese composite oxide is obtained.
[0042] Specifically, the lithium content in the lithium compound on the surface of the lithium-nickel-cobalt-aluminum composite oxide or the lithium-nickel-cobalt-manganese composite oxide is 0.6wt% or less relative to the total amount of the corresponding composite oxide, that is, the lithium in the lithium compound on the surface of the lithium-nickel-cobalt-aluminum composite oxide or the lithium-nickel-cobalt-manganese composite oxide has already migrated to the inside of the composite oxide. By reducing the lithium content on the surface, the gas generation phenomenon during the cycle process of the positive electrode material can be suppressed.
[0043] Preferably, the oxygen content in the oxygen-containing atmosphere is 99% or more, so that each metal element can be sufficiently oxidized.
[0044] Preferably, the sintering temperature is specifically 650°C, 680°C, 700°C, 720°C, 750°C, 780°C, 800°C, 820°C, 850°C, etc., and may be other values within the above ranges. Preferably, the sintering temperature is 700°C to 800°C.
[0045] Preferably, the sintering time is specifically 5h, 7h, 9h, 11h, 13h, 15h, 17h, 19h, 20h, etc., or may be other values within the above range. Preferably, the sintering time is 8 to 15h.
[0046] In one embodiment of the present invention, the intensity I of the X-ray diffraction peak corresponding to the (003) crystal plane of the active material 003 and the intensities of the X-ray diffraction peaks corresponding to the (104) crystal plane I 104 The ratio of is 1.25 or more, specifically, it may be 1.25, 1.26, 1.27, 1.28, 1.29, 1.30, 1.32, 1.35, 1.40, etc., and is not limited thereto. It is understood that the larger the intensity ratio of the X-ray diffraction peak corresponding to the specific crystal plane of the active material, the higher the crystallinity of the active material, which is advantageous for improving the conductive performance of the positive electrode material.
[0047] In a preferred embodiment of the present invention, the Li ions of the active material have an occupancy rate of 98% or more of the Li sites in the crystal lattice (Li site occupancy rate of Li ions). The Li site occupancy rate of Li ions means the ratio of the number of Li ions occupying the Li sites in the Li layer of the active material crystal lattice to the total number of Li sites. It is understood that the higher the Li site occupancy rate of Li ions, the stronger the discharge capacity of the active material. When the Li site occupancy rate of Li ions of the active material is low, the number of Li ions at the Li sites is reduced, Ni, Co, and Al are present at the Li sites, and Li / Ni mixing is likely to occur, as well as the Li ions may be separated from the crystal structure and exist in the form of lithium carbonate, etc. By improving the Li site occupancy rate of Li ions, Li / Ni mixing in the material can be effectively suppressed, the structural stability of the active material can be significantly improved, and safety can be improved.
[0048] <Process S20> In step S20, the sintered product is crushed, washed and filtered to obtain an active material cake.
[0049] As a specific example, the washing solvent is water, the washing temperature is 10° C. to 40° C., and the washing time is 10 min to 60 min. Specifically, the washing time may be 10 min, 20 min, 30 min, 40 min, 50 min, or 60 min, and the washing temperature may be 10° C., 20° C., 25° C., 30° C., 35° C., or 40° C.
[0050] Preferably, the amount of the cleaning solvent used is 500g / L to 2000g / L when expressed by the mass of the sintered product contained per 1 liter of the solvent. Specifically, the amount of the cleaning solvent used may be 500g / L, 600g / L, 700g / L, 800g / L, 900g / L, 1000g / L, 1200g / L, 1400g / L, 1500g / L, 1800g / L, or 2000g / L, etc., and is not limited thereto. The filtration time is 30min to 150min, specifically, may be 30min, 50min, 60min, 80min, 100min, 120min, or 150min, etc.
[0051] Preferably, the washing temperature is 20°C to 30°C, the amount of washing solvent used is 800g / L to 1500g / L, the washing time is 20min to 40min, and the filtration time is 60min to 120min. It is understood that impurities such as lithium carbonate and lithium hydroxide attached to the surface of the sintered product can be removed by washing the sintered product thoroughly. If the washing is insufficient, the lithium content on the surface of the composite positive electrode material will be high, and the residual lithium on the surface will react with the electrolyte during the battery cycle process to generate gas, which may affect the safety of the battery.
[0052] Preferably, the water content of the active material cake obtained by filtration is 5 wt % or less. Preferably, by making the water content of the active material cake 1 wt % or less, the effect of water on the performance of the active material can be reduced.
[0053] Preferably, prior to step S20, the method further comprises: The method further includes dissolving a phosphorus source and a soluble lithium compound in an aqueous solution to obtain a coating solution containing phosphate ions and lithium ions.
[0054] Preferably, the phosphorus source comprises at least one selected from HPO3, H3PO2, H3PO4, Li3PO4 and metal phosphate compounds.
[0055] Preferably, the metal phosphate compound is K3PO4, BPO4, NH4H2PO4, (NH4)2HPO4, Zr(HPO4)2, Na2HPO4, SrHPO4, BaHPO4, Ba3(PO4)2, MgHPO4, Ca(H2PO2)2, Al(H2PO4)3, CoHPO4, or H3P(W3O 10 )4·nH2O (wherein n ≧ 1).
[0056] Preferably, the soluble lithium compound includes at least one selected from lithium hydroxide, lithium carbonate, lithium nitrate, lithium chlorate, and lithium acetate. Preferably, the soluble lithium compound is lithium hydroxide.
[0057] Preferably, in the coating solution, the molar ratio of the lithium ion to the phosphate ion is (0-10):1, specifically, it may be 0:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, etc., and of course, it may be other values within the above range, and is not limited here. If the content of lithium ion is too high, the amount of residual lithium on the surface of the material will be too much, and if the content of phosphate radical is too high, the material coating layer will be too thick, which may affect the capacity and rate characteristics of the material. Preferably, the molar ratio of the lithium ion to the phosphate ion is (0-5):1.
[0058] In one embodiment of the present invention, the mass of phosphate ions in the phosphorus source is 0.05wt%-1.5wt% based on the active material cake, specifically, 0.05wt%, 0.08wt%, 0.10wt%, 0.2wt%, 0.3wt%, 0.5wt%, 0.8wt%, 1.0wt%, 1.2wt%, 1.3wt%, 1.5wt%, etc., or other values within the above range. If the content of phosphate ions in the phosphorus source is too high, the phosphate coating on the active material surface may become excessive, which may reduce the material capacity. Preferably, the mass of phosphate ions in the phosphorus source is 0.1wt%-1wt% based on the active material cake.
[0059] In one embodiment of the present invention, the total mass of the phosphorus source and the soluble lithium compound is 1.5 wt% to 45 wt% relative to the coating solution, and specifically, may be 1.5 wt%, 5 wt%, 8 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, or 45 wt%, etc., or may be other values within the above range.
[0060] Furthermore, the mass ratio of the phosphorus source in the coating solution is 1.5wt% to 30wt%, specifically, 1.5wt%, 5wt%, 8wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, etc., or may be other values within the above range. The mass ratio of the soluble lithium compound in the coating solution is 0wt% to 15wt%, specifically, 0wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 12wt%, 15wt%, etc., or may be other values within the above range.
[0061] <Process S30> In step S30, a coating solution containing phosphate ions and lithium ions is applied to the active material cake by atomization to obtain a composite positive electrode material.
[0062] In one embodiment of the present invention, the atomization method includes at least one selected from ultrasonic atomization and high-pressure atomization. It is understood that coating the active material by atomization can reduce the loss of phosphorus source and / or soluble lithium compound in the coating solution compared with the conventional liquid phase coating method, can improve the accuracy of the coating amount of the coating material, and can improve the coating uniformity and reaction activity compared with the conventional solid phase coating method.
[0063] During coating, the coating solution is atomized to form micro-nano-structured droplets, which have higher adsorption ability and higher reaction activity with the active material when mixed with the active material, and can be uniformly embedded or infiltrated into the pores of the active material, repair the surface defects of the active material, achieve a uniform coating effect, and form a network with high lithium ion conductivity on the surface of the primary particles of the active material, thereby significantly reducing the impedance of the active material and optimizing the electrochemical performance of the active material.
[0064] During the coating process, the coating temperature is controlled to 50°C to 100°C, specifically, it may be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc., but is not limited thereto. During the stepwise temperature increase process, the coating solution and the active material cake are mixed and dried, so that the coating and the active material can be fully reacted, thereby improving the reaction activity between the coating and the active material and improving the coating effect.
[0065] During the coating process, the heat retention time is controlled to 5 to 60 minutes, and specifically, it may be 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, or 60 minutes, etc., but is not limited thereto.
[0066] Preferably, after step S30, the method further comprises: The method further includes a step of drying the composite positive electrode material, controlling the drying temperature to 150° C. to 210° C. and the warming time to 10 hours to 24 hours.
[0067] In one embodiment of the present invention, the drying temperature may be, but is not limited to, 150° C., 155° C., 160° C., 165° C., 170° C., 175° C., 180° C., 185° C., 190° C., 195° C., 200° C., 210° C., etc. The incubation time may be, but is not limited to, 10 h, 12 h, 14 h, 15 h, 17 h, 18 h, 19 h, 20 h, 22 h, 24 h, etc.
[0068] In one embodiment of the present invention, the moisture content of the composite positive electrode material after drying is less than or equal to 0.04 wt%, which can reduce the moisture content in the composite positive electrode material and improve the processing performance of the composite positive electrode material.
[0069] In addition, in the present invention, a stepwise heating method is adopted during the coating-drying process, and process parameters such as the atomization liquid spray speed, the rotation speed of the mixer, and the temperature are controlled, so that the coating material and the active material can be thoroughly mixed and dried, and the reaction activity and coating uniformity can be improved.
[0070] According to the present invention, the atomization coating method can avoid the loss of coating dissolved in the solution due to filtration in the conventional liquid phase coating method, and can improve the accuracy of the coating amount, and can also improve the coating uniformity and reaction activity compared with the solid phase coating method. During the atomization coating process, the phosphate coating solution forms micro- and nano-structured droplets, which have higher adsorption properties and can improve the reaction activity during the active material mixing process, and the coating is easily uniformly embedded in the pores of the active material (lithium-nickel-cobalt-aluminum composite oxide or lithium-nickel-cobalt-manganese composite oxide), repairing the surface defects of the active material and achieving a uniform coating effect, forming a network with high lithium ion conductivity on the surface of the primary particles of the active material, which can significantly reduce the impedance of the active material and optimize the electrochemical performance of the active material.
[0071] According to a third aspect of the present invention, there is provided a lithium ion battery having a positive electrode sheet, a negative electrode sheet, a separator, a non-aqueous electrolyte, and an outer case, The present invention further provides a lithium ion battery, wherein the positive electrode sheet includes a current collector and the composite positive electrode material coated on the current collector, or the positive electrode material produced by the method for producing the composite positive electrode material. EXAMPLES
[0072] The present invention will be further described below with reference to several examples. However, the examples of the present invention are not limited to the following specific examples. The present invention can be modified appropriately without departing from the spirit of the present invention.
[0073] <Example 1> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.88 Co 0.09 Al 0.03 A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. The sintered product was washed by preparing a slurry with a concentration of 1300 g / L using 10 kg of sintered product and water (L). The washing temperature was 20°C, the washing time was 15 min, and the washed slurry was filtered under pressure. The pressure filtration time was 1 h. LiNi 0.88 Co 0.09 Al 0.03 O2 active material cake was obtained. 40.0 g of LiOH·H2O was dissolved in 300 ml of water, and 70.0 g of NH4H2PO4 was added and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C, and the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. The oil temperature of the mixer was then increased to 180°C, and the mixture was dried in a nitrogen gas atmosphere for 20 h. The lithium phosphate-coated LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained as a composite cathode material. The composite positive electrode material prepared in this example included an active material and a lithium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 11.3 μm and a specific surface area of 0.75 m. 2 / g, powder conductivity is 0.056S / cm 2 It was. Figure 2 is a SEM image of the composite cathode material prepared in this example. Figure 3a is a SEM image of a local area of the composite cathode material prepared in this example, and Figure 3b is an energy dispersive X-ray analysis (EDX) phosphorus elemental mapping of the composite cathode material prepared in this example.
[0074] <Example 2> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.88 Co 0.09 Al 0.03 A mixture of (OH)2, LiOH·H2O and Zr(OH)4 was obtained, where the molar ratio of Zr to the sum of Ni, Co and Al was 0.005:1. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product Li(Ni 0.88 Co 0.09 Al 0.03 ) 0.995 Zr 0.005 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. The sintered product (g) and water (L) were used to prepare a slurry with a concentration of 1300 g / L and washed. The washing temperature was 20°C, the washing time was 15 min, the washed slurry was pressure filtered, the pressure filtration time was 1 h, and the Li(Ni 0.88 Co 0.09 Al 0.03 ) 0.995 Zr 0.005 O2 active material cake was obtained. 40.0 g of LiOH·H2O was dissolved in 300 ml of water, and 70.0 g of NH4H2PO4 was added and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C. At the same time, the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. Next, the oil temperature of the mixer was increased to 180°C, and the mixture was dried in a nitrogen gas atmosphere for 20 h. Li(Ni 0.88 Co 0.09 Al 0.03 ) 0.995 Zr 0.005 O2 was obtained as a composite cathode material. The composite positive electrode material prepared in this example included an active material and a lithium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 11.6 μm and a specific surface area of 0.64 m. 2 / g, powder conductivity is 0.068S / cm 2 It was.
[0075] <Example 3> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1:1, and the Ni particles had an average particle size of 5.0 μm. 0.99 Co 0.01 A mixture of (OH)2, LiOH·H2O, Zr(OH)4, and Ti(OH)4 was obtained, where the molar ratio of the sum of Zr and Ti to the sum of Ni and Co was 0.005:1, and the molar ratio of Zr to Ti was 3:2. The mixture was sintered at 660°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 8 h. The sintered product Li(Ni 0.99 Co 0.02 ) 0.995 Zr 0.003 Al 0.002 O2 was obtained. The average particle size of the sintered product was controlled to 4.5 μm to 5.5 μm using an airflow pulverizer. The sintered product (g) and water (L) were used to prepare a slurry with a concentration of 2000 g / L and washed. The washing temperature was 10°C, the washing time was 10 min, the washed slurry was pressure filtered, the pressure filtration time was 1 h, and the Li(Ni 0.99 Co 0.02 ) 0.995 Zr 0.003 Ti 0.002 O2 active material cake was obtained. 30.0 g of LiOH·H2O was dissolved in 300 ml of water, and then 40.0 g of SrHPO4 and 10 g of NH4H2PO4 were added and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C. At the same time, the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, mixing was continued for 15 min. Next, the oil temperature of the mixer was increased to 180°C, and drying was continued in a nitrogen gas atmosphere for 20 h. Li(Ni) coated with lithium strontium phosphate was obtained. 0.99 Co 0.02 ) 0.995 Zr 0.003 Ti 0.002 O2 was obtained as a composite cathode material. The composite positive electrode material prepared in this example included an active material and a lithium strontium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 5.2 μm and a specific surface area of 0.83 m. 2 / g, powder conductivity is 0.045S / cm 2 It was.
[0076] <Example 4> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 15.0 μm. 0.80 Co 0.15 Al 0.05 A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 800°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 15 h. The sintered product was LiNi 0.80 Co 0.15 Al 0.05 O2 was obtained. The average particle size of the sintered product was controlled to 14.0 to 16.0 μm using an airflow pulverizer. The sintered product (g) and water (L) were used to prepare a slurry with a concentration of 1300 g / L and washed. The washing temperature was 30°C, the washing time was 60 min, and the washed slurry was filtered under pressure. The pressure filtration time was 1 h. LiNi 0.80 Co 0.15 Al 0.05 O2 active material cake was obtained. 30.0 g of LiOH·H2O was dissolved in 300 ml of water, and 49.0 g of Zr(HPO4)2·H2O was added and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C. At the same time, the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. The oil temperature of the mixer was then increased to 180°C. The mixture was then dried in a nitrogen gas atmosphere for 20 h. The LiNi coated with lithium zirconium phosphate was obtained. 0.80 Co 0.15 Al 0.05 O2 was obtained as a composite cathode material. The composite positive electrode material prepared in this example included an active material and a lithium zirconium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 15.3 μm and a specific surface area of 0.92 m. 2 / g, powder conductivity is 0.057S / cm 2 It was.
[0077] <Example 5> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoMnAl was 1.04:1, and the Ni0.88Co0.06MnAl with an average particle size of 11.0 μm was obtained. 0.03 Al 0.03 A mixture of (OH)2, LiOH·H2O and lithium acetate was obtained. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.88 Co 0.06 Mn 0.03 Al 0.03 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. The sintered product (g) and water (L) were used to prepare a slurry with a concentration of 1300 g / L and washed. The washing temperature was 20°C, the washing time was 15 min, and the washed slurry was pressure filtered. The pressure filtration time was 1 h. LiNi 0.88 Co 0.06 Mn 0.03 Al0.03 O2 active material cake was obtained. 450.0 g of H3PO was dissolved in 250 ml of water and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C, and the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. The oil temperature of the mixer was then increased to 180°C, and the mixture was dried in a nitrogen gas atmosphere for 20 h. The lithium phosphate-coated LiNi 0.88 Co 0.06 Mn 0.03 Al 0.03 O2 was obtained as a composite cathode material. The composite positive electrode material produced in this example included an active material and a lithium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 11.9 μm and a specific surface area of 1.01 m. 2 / g, powder conductivity is 0.082S / cm 2 It was.
[0078] <Example 6> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.91 Co 0.04 Al 0.05 A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.91 Co 0.04 Al 0.05 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. The sintered product (g) and water (L) were used to prepare a slurry with a concentration of 1300 g / L and washed. The washing temperature was 20°C, the washing time was 15 min, and the washed slurry was pressure filtered. The pressure filtration time was 1 h. LiNi 0.91 Co0.04Al 0.05 O2 active material cake was obtained. 450.0 g of H3PO was dissolved in 250 ml of water and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C, and the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. The oil temperature of the mixer was then increased to 180°C, and the mixture was dried in a nitrogen gas atmosphere for 20 h. The lithium phosphate-coated LiNi 0.91 Co 0.04 Al 0.05 O2 was obtained as a composite cathode material. The composite positive electrode material prepared in this example included an active material and a lithium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 11.6 μm and a specific surface area of 1.13 m. 2 / g, powder conductivity is 0.039S / cm 2 It was.
[0079] <Example 7> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoMn was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.83 Co 0.11 Mn 0.06 A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 760°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.83 Co 0.11 Mn 0.06 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. 10 kg of the sintered product and water (L) were used to prepare a slurry with a concentration of 1000 g / L and washed. The washing temperature was 20°C, the washing time was 20 min, and the washed slurry was filtered under pressure. The pressure filtration time was 1 h. LiNi 0.83 Co 0.11 Mn 0.06 O2 active material cake was obtained. 60.0 g of H3PO4 was dissolved in 250 ml of water and stirred to obtain a coating solution. 10 kg of active material cake was placed in a VC mixer and started at a rotation speed of 300 rpm. The oil temperature of the mixer was set to 80°C, and the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. The oil temperature of the mixer was then increased to 180°C, and the mixture was dried in a nitrogen gas atmosphere for 20 h. The lithium phosphate-coated LiNi 0.83 Co 0.11Mn0.06 O2 was obtained as a composite cathode material. The composite positive electrode material prepared in this example included an active material and a lithium phosphate coating layer on the surface of the active material. The composite positive electrode material had an average particle size of 11.5 μm and a specific surface area of 0.65 m. 2 / g, powder conductivity is 0.060S / cm 2 It was.
[0080] <Comparative Example 1> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.88 Co 0.09 Al 0.03 A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. The sintered product was washed by preparing a slurry with a concentration of 1300 g / L using 10 kg of sintered product and water (L). The washing temperature was 20°C, the washing time was 15 min, and the washed slurry was filtered under pressure. The pressure filtration time was 1 h. LiNi 0.88 Co 0.09 Al 0.03 O2 active material cake was obtained. LiNi 0.88 Co 0.09 Al 0.03 The cake of O2 active material was placed under a nitrogen gas atmosphere and dried at 180 °C for 20 h. The LiNi 0.88 Co0.09 Al 0.03 O2 was obtained as the positive electrode material. Figure 4 shows an SEM image of the composite cathode material produced in this comparative example. Figure 5a shows an SEM image of a local area of the composite cathode material produced in this comparative example, and Figure 5b shows an energy dispersive X-ray analysis (EDX) phosphorus elemental mapping of the composite cathode material produced in this comparative example.
[0081] <Comparative Example 2> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.88 Co 0.09 Al 0.03 A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. A slurry with a concentration of 1300 g / L was prepared using 10 kg of the sintered product and water (L), and 40.0 g of LiOH·H2O and 70.0 g of NH4HPO4 were added in sequence to wash the slurry. The washing temperature was 20°C, the washing time was 15 min, and the slurry after washing was filtered under pressure. The pressure filtration time was 1 h, and LiNi 0.88 Co 0.09 Al 0.03 O2 active material cake was obtained. The active material cake was taken out and dried at 180°C under a nitrogen gas atmosphere for 20 hours. LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained as the positive electrode material.
[0082] <Comparative Example 3> The raw materials were mixed in a high-speed mixer so that the molar ratio of Li / NiCoAl was 1.04:1, and the Ni particles had an average particle size of 11.0 μm. 0.88 Co 0.09 Al 0.03A mixture of (OH)2 and LiOH·H2O was obtained. The mixture was sintered at 740°C in an atmosphere with an oxygen content of 99% or more, and the sintering time was 10 h. The sintered product was LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained. The average particle size of the sintered product was controlled to 10.0 to 12.0 μm using an airflow pulverizer. 40.0 g of LiOH·H2O was dissolved in 300 ml of water, and 70.0 g of NH4HPO4 was added and stirred to obtain a coating solution. Sintered product LiNi 0.88 Co 0.09 Al 0.03 10 kg of O2 was put into the VC mixer, and the mixer was started at a rotation speed of 300 rpm. The mixer's oil temperature was set to 80°C, and the coating solution was atomized and sprayed into the mixer at a spray rate of 40 mL / min. After all the coating solution was sprayed into the mixer, the mixture was mixed for 15 min. The mixer's oil temperature was then increased to 180°C, and the mixture was dried in a nitrogen gas atmosphere for 20 h. The lithium phosphate-coated LiNi 0.88 Co 0.09 Al 0.03 O2 was obtained as a composite cathode material.
[0083] (Measurement method) A Malvern Mastersizer 2000 laser diffraction particle size analyzer was used to perform particle size analysis on the positive electrode material to determine its particle size distribution and average particle size. The particle hardness of the composite cathode material was measured using a Shimadzu dynamic ultra-microhardness tester.
[0084] The specific surface area of the positive electrode material was measured using a Micromeritics TriStar II 3020 automatic specific surface area / pore distribution analyzer. Specifically, a certain mass of the positive electrode material powder was weighed, heated in a vacuum to perform a complete degassing treatment, and any adsorbed gas on the surface was removed. The specific surface area of the particles was then calculated from the amount of adsorbed nitrogen by nitrogen gas adsorption.
[0085] The powder conductivity of the positive electrode material was measured using an FT-8100 series four-probe powder resistance measuring device. Specifically, a certain mass of the positive electrode material powder was weighed and subjected to a resistance test of 20 kN / cm 2 The powder was compressed under a pressure of 0.01 g / cm2 and the powder conductivity of the material was measured using the four-probe powder resistance measuring device described above.
[0086] [Manufacturing of 2032 type coin batteries] The positive electrode, conductive carbon, and polyvinylidene fluoride produced in each Example were added to N-methylpyrrolidone in a ratio of 96:2:2, stirred to obtain a slurry, which was then applied to aluminum foil and dried to form a positive electrode sheet. A lithium sheet was used as the negative electrode to produce a 2032-type coin battery.
[0087] [Measurements of discharge capacity, cycle characteristics, and rate performance] Using a LAND battery measurement system, electrical performance tests were performed at 25°C, 2.5V to 4.3V. In the first charge / discharge cycle, the battery was charged to 4.3V at a current of 0.1C, and then discharged to 2.5V at a current of 0.1C. Thereafter, the charge / discharge cycle was repeated, and the capacity retention rate over 50 cycles was recorded. In each charge / discharge cycle, the battery was charged to 4.3V at a current of 0.5C, and then discharged to 2.5V at a current of 1C.
[0088] [DCR measurement] Electrical performance tests were performed at 25°C, 2.5V to 4.3V using an Arbin battery measurement system. In the first charge / discharge cycle, the battery was charged to 4.3V at a current of 0.5C, and then discharged to 2.5V at a current of 1C. The DCR was calculated by dividing the voltage drop 10 seconds after the start of discharge by the current value.
[0089] [EIS measurement] Using a multichannel potentiostat (Bio-Logic; VMP3), electrochemical impedance measurements were performed on a 2032-type coin battery at frequencies of 1 MHz to 1 mHz, 100% SOC, and 25°C.
[0090] [SEM Measurement] The surface morphology of the materials was measured using a Hitachi S4800 scanning electron microscope.
[0091] [EDS analysis] A Hitachi S4800 scanning electron microscope was used to study the surface of the material. Elemental mapping was performed with an energy dispersive X-ray spectrometer.
[0092] [Measurement of Li site occupancy of Li ions] The obtained positive electrode material was identified by powder X-ray diffraction measurement using CuKα radiation, and the X-ray diffraction pattern of the positive electrode material was obtained and the Li site occupancy rate of Li ions was calculated by Rietveld analysis. The following method was used for Rietveld analysis. A crystal structure model was constructed, and the X-ray diffraction pattern obtained by the crystal structure model was fitted to the actually measured X-ray diffraction pattern. The lattice constant parameters of the crystal structure model were adjusted to match the two X-ray diffraction patterns, and the Li site occupancy rate of Li ions was calculated from the lattice constant data obtained in this case.
[0093] [Intensity ratio of the X-ray diffraction peak corresponding to the (003) crystal plane to the X-ray diffraction peak corresponding to the (104) crystal plane] The obtained positive electrode material was identified by powder X-ray diffraction measurement using CuKα radiation, and the X-ray diffraction pattern of the positive electrode material was obtained and the Li site occupancy rate of Li ions was calculated by Rietveld analysis. The following method was used for Rietveld analysis. A crystal structure model was constructed, and the X-ray diffraction pattern obtained by the crystal structure model was fitted to the actually measured X-ray diffraction pattern. The two X-ray diffraction patterns were matched to each other by adjusting the lattice constant parameters of the crystal structure model. In this case, the intensity of the X-ray diffraction peaks corresponding to the (003) and (104) crystal planes was calculated.
[0094] As can be seen from Figs. 2 and 4, the surface of the sample in which the filter cake was coated with phosphate in Example 1 had a clear coating layer, whereas the sample in Comparative Example 1 was not coated and had a smoother surface.
[0095] As can be seen from Figures 3b and 5b, with the same coating amount, the sample in which the filter cake was coated with phosphate in Example 1 had a higher phosphorus content and was distributed evenly, while the sample in which no coating treatment was performed in Comparative Example 1.
[0096] As shown in FIGS. 6 to 8, the sample of Example 1 has a better surface coating effect of lithium phosphate, and therefore has higher cycle characteristics, lower direct current internal resistance, and lower impedance.
[0097] [Table 1]
[0098] Comparing the experimental data shown in Table 1 (measurement results), the sample in which the filter cake is coated with phosphate has better particle hardness, discharge capacity, cycle characteristics, and rate performance.
[0099] As can be seen from the experimental data of the Li site occupancy rate of Li ions and the intensity ratio of the X-ray diffraction peaks corresponding to the (003) and (104) crystal planes in Example 1 and Comparative Example 1, the sample obtained by coating the filter cake with phosphate has a higher Li site occupancy rate of Li ions and a higher intensity ratio of the X-ray diffraction peaks corresponding to the (003) and (104) crystal planes, and therefore the sample obtained by coating the filter cake with phosphate has lower Li / Ni mixing, higher structural stability and higher particle hardness.
[0100] In Comparative Example 2, a liquid-phase coating method was adopted, and some of the phosphorus source and soluble lithium compound were washed away with the solution, making it difficult to control the amount of coating on the material surface. As a result, the difference in specific surface area of the material before and after coating was large, which affected the stability of the material structure.
[0101] In Comparative Example 3, the sintered product was not cleaned during the preparation, resulting in high residual lithium on the surface of the final prepared positive electrode material, which increased the DC internal resistance and impedance of the battery, and affected the capacity and rate characteristics of the material.
[0102] The present invention has been disclosed above with reference to the preferred embodiments, but these are not intended to limit the scope of the claims. Those skilled in the art may make various possible modifications and variations without departing from the spirit of the present invention. Therefore, the scope of protection of the present invention should be limited only by the scope of the claims.
Claims
1. General formula: Li a (Ni x Co y R z ) 1-b M b O 2 (wherein 0.9≦a≦1.10, x+y+z=1, 0.8≦x≦0.99, 0.01≦y≦0.15, 0≦z≦0.1, 0≦b≦0.1, R contains Al and / or Mn, and M is at least one metal element selected from Mg, Sr, Ca, Ba, Ti, Zr, Y, Gd, W, Nb, La, and Mo), and a coating layer containing a phosphate compound and distributed on a surface of the active material; The composite positive electrode material has a particle hardness Cs50 of 50 MPa or more, and 10 / Cs 50 ≧0.7 (where Cs 10 is the hardness of a particle having a particle size of D10, and Cs 50 is the hardness of particles having a particle size of D50.
2. The composite positive electrode material of claim 1 , which satisfies at least one of the following conditions b to c: b. The intensity I of the X-ray diffraction peak corresponding to the (003) crystal plane of the active material 003 and the intensity of the X-ray diffraction peak corresponding to the (104) crystal plane I 104 is greater than or equal to 1.25; c) The Li ions contained in the active material occupy 98% or more of the Li sites of the crystal lattice.
3. The composite positive electrode material of claim 1 or 2, which satisfies at least one of the following conditions a to e: a. The phosphate compound is Li 3 P.O. 4 and LiXPO 4 (In the formula, X includes at least one selected from Na, K, Al, Sr, Zr, B, Mg, Ba, Ca, Co, and W); b. The content of the phosphate compound in the coating layer is 0.05 wt % to 1.5 wt % based on the mass of the active material; c. the powder conductivity of the composite cathode material is 0.001 S / cm to 0.1 S / cm; d. The specific surface area of the composite positive electrode material is 0.2 m 2 / g to 2.0 m 2 / g; e) The average particle size of said composite cathode material is between 3 μm and 20 μm.
4. A process for obtaining a sintered product by mixing a main component, a subcomponent and a lithium compound and then sintering the mixture, the main component being Ni x Co y R z O, Ni x Co y R z (OH) 2 Or Ni x Co y R z OOH (wherein, in each of the above formulae, x+y+z=1, 0.8≦x≦0.99, 0.01≦y≦0.15, 0≦z≦0.1), the auxiliary component includes at least one selected from an oxide of M, a hydroxide of M, or a phosphate of M, where M is at least one metal element selected from Mg, Sr, Ca, Ba, Ti, Zr, Y, Gd, W, Nb, La, and Mo, and R includes Al and / or Mn; crushing, washing and filtering the sintered product to obtain an active material cake; A step of performing a coating treatment using a coating solution containing phosphate ions and lithium ions and the active material cake in an atomization manner to obtain a composite positive electrode material, the composite positive electrode material has an active material and a coating layer distributed on a surface of the active material, the coating layer containing a phosphate compound, and the composite positive electrode material has a particle hardness Cs50 of 50 MPa or more and satisfies Cs10 / Cs50≧0.7 (where Cs10 is the hardness of particles having a particle size of D10, and Cs50 is the hardness of particles having a particle size of D50).
5. The method according to claim 4, which satisfies at least one of the following conditions a to d: a. The amount of the lithium compound added is set so that the ratio of the sum of the molar contents of Ni, Co, and R in the main component to the molar content of Li is 1:(0.9 to 1.10); b) The sintering conditions for obtaining the sintered product are as follows: in an oxygen-containing atmosphere, heating to 650°C to 850°C and sintering for 5h to 20h; c. The average particle size of the main component is 3 μm to 20 μm; d) The lithium compound includes at least one selected from the group consisting of lithium hydroxide, lithium carbonate, lithium acetate, lithium nitrate, and lithium oxalate.
6. The method according to claim 4, which satisfies at least one of the following conditions a to d: a. The washing temperature is 10°C to 40°C, and the washing time is 10 min to 60 min; b) The amount of the cleaning solvent used satisfies the following formula: sintered product (g) / amount of cleaning solvent used (L) = 500 g / L to 2000 g / L; c. the filtration time is 30 min to 150 min, and the moisture content of the active material cake is 5 wt % or less; d) The filtration includes at least one selected from pressure filtration and suction filtration.
7. Before the coating process is performed using a coating solution containing phosphate ions and lithium ions and the active material cake by the atomization coating method, 5. The method of claim 4, comprising dissolving a phosphorus source and a soluble lithium compound in an aqueous solution to obtain a coating solution containing phosphate ions and lithium ions.
8. The method according to claim 7, which satisfies at least one of the following conditions a to e: a. The phosphorus source is HPO 3 , H 3 P.O. 2 , H 3 P.O. 4 , Li 3 P.O. 4 , K 3 P.O. 4 , BPO 4 , N.H. 4 H 2 P.O. 4 , (NH 4 ) 2 H.P.O. 4 , Zr(HPO 4 ) 2 , Na 2 H.P.O. 4 , SrHPO 4 , BaHPO 4 , Ba 3 (P.O. 4 ) 2 , MgHPO 4 , Ca(H 2 P.O. 2 ) 2 , Al(H 2 P.O. 4 ) 3 , CoHPO 4 Or H 3 P (W 3 O 10 ) 4 ・nH 2 O (wherein n ≧1); b. The soluble lithium compound includes at least one selected from lithium hydroxide, lithium carbonate, lithium nitrate, lithium chlorate, and lithium acetate; c. In the coating solution, the molar ratio of the lithium ions to the phosphate ions is (0-10):1; d. The mass of phosphate ions in the phosphorus source is 0.05 wt % to 1.5 wt % based on the active material cake; e) The combined weight percent of the phosphorus source and the soluble lithium compound is 1.5 wt % to 45 wt % of the coating solution.
9. The method according to any one of claims 4 to 7, which satisfies at least one of the following conditions a to b: a. the atomization method includes at least one selected from ultrasonic atomization and high-pressure atomization; b) During the coating process, the coating temperature is controlled to be 50°C to 100°C, and the heat retention time is controlled to be 5min to 60min.
10. After the coating process, The method according to claim 4, further comprising the step of drying the composite positive electrode material and controlling the drying temperature to 150° C. to 210° C. and the incubation time to 10 h to 24 h.
11. A lithium ion battery including a positive electrode sheet, a negative electrode sheet, a separator, a non-aqueous electrolyte, and an outer case, The positive electrode sheet comprises a current collector and the composite positive electrode material according to any one of claims 1 to 3 applied to the current collector.
Citation Information
Patent Citations
Lithium ion battery anode material and manufacturing method thereof
CN102637877A
Positive active material and preparation method thereof, cathode material of lithium ion battery and preparation method thereof, as well as lithium ion battery
CN105470495A
Preparation method and product of lithium phosphate coated ternary ion battery positive electrode material
CN109546136A
Preparation method of high-nickel positive electrode material with improved water washing
CN111653761A
High-nickel positive electrode material, preparation method thereof and lithium ion secondary battery
CN112382741A