Method for producing copper selenide nanoparticles, copper selenide nanoparticle aggregates, copper selenide nanoparticles and film-coated structure
A continuous flow process for producing copper selenide nanoparticles with controlled environments and ligand encapsulation addresses the challenge of synthesizing uniform, scalable, and high-absorption near-infrared photodetectors, achieving efficient near-infrared photodetection.
Patent Information
- Application Number
- JP2020165705
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-09-30
AI Technical Summary
There is a need for low-cost, non-toxic materials that can strongly absorb near-infrared wavelengths for photodetectors, as existing materials like CuInSe2 are difficult to synthesize uniformly and are limited in scalability.
A method involving a continuous flow process to produce copper selenide nanoparticles, using a copper-selenium mixture with a ligand in a controlled environment to achieve uniform particle size and strong absorption, encapsulating the nanoparticles with a ligand to stabilize them, and forming a film structure for enhanced photodetection.
The method enables mass production of copper selenide nanoparticles with a narrow absorption peak and high peak-to-valley ratio, suitable for near-infrared photodetection applications, overcoming synthesis challenges and enabling scalable production.
Smart Images

Figure 0007584009000002 
Figure 0007584009000003 
Figure 0007584009000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing copper selenide nanoparticles, copper selenide nanoparticle aggregates, copper selenide nanoparticles, and a film-coated structure. This application claims priority to U.S. Provisional Application No. 62 / 908,476, filed September 30, 2019, the contents of which are incorporated herein by reference. [Background technology]
[0002] Quantum dots are semiconductor nanoparticles or crystallites small enough to show evidence of quantum confinement. In the quantum confinement size regime, the small dimensions of the crystallites spatially confine excitons generated within them. Various optical properties of quantum dots are size dependent and therefore tunable if quantum dots of desired sizes can be isolated. This property is exploited in technologies that exploit quantum dot photoemission, such as light emitting diodes for displays, lighting, and lasing, as well as in technologies that exploit light absorption and photoinduced charge carrier transport, such as photon detection and photovoltaics. The optical tunability of quantum dots can also be exploited in specialized electro-optical materials and components such as downshifting color conversion sheets.
[0003] In recent years, quantum dots have also attracted attention as a near-infrared photodetector material. However, there are only a limited number of materials that can absorb energy in the near-infrared wavelength range. Si is perhaps one of the best-known materials, but it can only detect wavelengths up to 900 nm. Ge can observe wavelengths from 400 nm to 1700 nm, but Ge is expensive and difficult to manufacture. InGaAs, PbS, and HgCdTe can detect a variety of IR wavelengths, but these materials contain toxic elements and have high manufacturing costs. Therefore, there is a need for low-cost IR photodetector materials that are free of RoHS restrictions.
[0004] CuInSe2 has been studied so far as a low-cost IR photodetector material. Although this material can absorb NIR wavelengths, the absorption is generally weak and is often accompanied by luminescence, which is an undesirable characteristic for photodetectors. On the other hand, copper selenide nanoparticles (including various morphologies and stoichiometries referred to here as copper selenide nanoparticles) are inexpensive, have high carrier density, and can strongly absorb light with wavelengths in the near-infrared region, making them very promising IR photodetector materials (Non-Patent Documents 1-3). However, this material has several challenges. This material is difficult to synthesize because it is very sensitive to stoichiometry. That is, it is difficult to create a uniform morphology in a single sample, and very strict control over the reaction is required. As disclosed in Non-Patent Documents 4 and 5, although copper selenide nanoparticles with a relatively strong IR absorption peak have been obtained in laboratory-scale preparation, when attempting to scale up, the synthesis of high-quality copper selenide nanoparticles is difficult due to the comprehensive challenges mentioned above, limiting their adoption in the commercial market. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Dorfs, D.; et al. J. Am. Chem. Soc. 2011, 133, 11175 [Non-Patent Document 2] Kriegel, I.; et al. J. Am. Chem. Soc. 2012, 134, 1583 [Non-Patent Document 3] Luther, J.; Alivisatos, P.; et al. Nature Materials 2011, 10, 361 [Non-Patent Document 4] Scotognella, F.; et al. Nano Lett. 2011, 11, 4711 [Non-Patent Document 5] Hessel, C.; et al. Nano Lett. 2011, 11(6), 2560 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to provide a method for producing copper selenide nanoparticles that can mass-produce copper selenide nanoparticles that strongly absorb light with wavelengths in the near-infrared region and have a small half-width at half maximum of the absorption peak, and to provide copper selenide nanoparticle aggregates, copper selenide nanoparticles, and film-coated structures obtained thereby. [Means for solving the problem]
[0007] The method for producing copper selenide nanoparticles according to an embodiment of the present invention includes: 1. A method for producing copper selenide nanoparticles by a flow process, comprising: forming a flowable copper precursor by combining a copper starting material with a ligand; forming a flowable selenium precursor by suspending a selenium starting material in a liquid; forming a flowable copper-selenium mixture by combining the flowable copper precursor and the flowable selenium precursor; passing the flowable copper-selenium mixture through at least one heating unit to form a solution containing copper selenide nanoparticles; isolating the copper selenide nanoparticles in an oxygen-depleted environment; Including, the fluid copper-selenium mixture comprises a low polarity solvent; the step of isolating the copper selenide nanoparticles comprises precipitating the copper selenide nanoparticles by combining a solution containing the copper selenide nanoparticles with a deoxygenated highly polar solvent; The high polarity solvent is more polar than the low polarity solvent. A method for producing copper selenide nanoparticles.
[0008] The copper selenide nanoparticle aggregate according to the embodiment of the present invention is It is an air-stable copper selenide nanoparticle aggregate, Copper selenide nanoparticles encapsulated by ligands and exhibiting exciton absorption with an absorbance maximum between 900 and 1200 nanometers. Copper selenide nanoparticle aggregates.
[0009] The copper selenide nanoparticles according to the embodiment of the present invention are having an absorbance maximum between 900 and 1200 nanometers, and the absorbance maximum having a peak-to-valley ratio of 10 or greater; Copper selenide nanoparticles.
[0010] The film covering structure according to an embodiment of the present invention is Including copper selenide nanoparticles according to the embodiment of the present invention described above, It is a film-coated structure. Effect of the Invention
[0011] According to the present invention, there is provided a method for producing copper selenide nanoparticles that can mass-produce copper selenide nanoparticles that strongly absorb light with wavelengths in the near-infrared region and have a small half-width at half maximum of the absorption peak, and a copper selenide nanoparticle aggregate, copper selenide nanoparticles, and a film-coated structure obtained thereby. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 shows an example of an embodiment of a continuous segmented flow reactor system. [Diagram 2] FIG. 2 illustrates an exemplary method for preparing copper selenide nanoparticles. [Diagram 3] FIG. 3 shows an exemplary UV-visible absorption spectrum of a solution of copper selenide nanoparticles prepared according to the method of FIG. [Figure 4] FIG. 4 shows an exemplary X-ray fluorescence spectrum of copper selenide nanoparticles prepared according to the method of FIG. [Figure 5A] FIG. 5A shows an example of a transmission electron microscope (TEM) micrograph of copper selenide nanoparticles prepared according to the method of FIG. [Figure 5B] FIG. 5B is a magnified photograph of the two-dimensional superlattice of copper selenide nanoparticles shown in FIG. 5A. [Figure 6] Figure 6 shows an exemplary particle size histogram of copper selenide nanoparticles prepared according to the method of Figure 2 using the reactor system of Figure 1. The histogram is based on particle size measurements using TEM micrographs such as Figures 5A and 5B. [Figure 7] FIG. 7 shows an embodiment of an exemplary film-coated structure that can be fabricated using copper selenide nanoparticles prepared according to the method of FIG. [Figure 8] FIG. 8 illustrates an exemplary process for making a film-coated structure such as that shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] An example of the preparation of copper selenide (Cu2-xSe) nanoparticles is disclosed herein. In one embodiment, a flowable copper precursor is formed by combining a copper starting material with a ligand, and a flowable selenium precursor is formed by suspending a selenium starting material in a liquid. The flowable copper precursor and the flowable selenium precursor are then combined to form a flowable copper-selenium mixture with a low polarity solvent. The flowable copper-selenium mixture is directed through at least one heating unit to form a solution containing copper selenide nanoparticles, and the copper selenide nanoparticles are isolated in an oxygen-deficient environment. The isolation includes combining the solution containing the copper selenide nanoparticles with a deoxygenated highly polar solvent to precipitate the copper selenide nanoparticles.
[0014] Another example provides an air-stable copper selenide nanoparticle assembly comprising copper selenide nanoparticles prepared by a flow process and precipitated from solution under anaerobic conditions, the copper selenide nanoparticles being encapsulated by ligands and exhibiting excitonic absorption with an absorbance maximum between 900 and 1200 nanometers.
[0015] Another example provides copper selenide nanoparticles having an absorbance maximum between 900 and 1200 nanometers, and said absorbance maximum having a peak to valley ratio of 10 or greater.
[0016] Another example provides an electronically conductive substrate and a plurality of layers of two-dimensional close-packed copper selenide nanoparticles disposed on the electronically conductive substrate, the plurality of layers including ligand bridges bridging adjacent layers of the plurality of layers and bridging at least one of the plurality of layers to the electronically conductive substrate.
[0017] The above Summary is provided to introduce a selection of concepts in a simplified form that are further described in the Detailed Description. It is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
[0018] Semiconductor nanoparticles, or "quantum dots," can be prepared by conventional batch processing. However, batch processing in heterogeneous reaction systems is difficult to scale and typically results in broad particle size distributions. Because the useful optical properties of quantum dots depend on particle size, synthesis methods that result in narrow particle size distributions are generally desirable.
[0019] Continuous flow processing offers advantages in particle size distribution as well as scalability. Continuous flow reactor systems can contain one or more reaction zones (e.g., zones of controlled temperature, controlled irradiation, controlled exposure to catalyst, etc.). For kinetically controlled processes occurring in a reaction zone, the extent of reaction is determined by the residence time of the flowing reactants in that zone. However, reactants flowing through a conduit exhibit a distribution of velocities normal to the wall, even at a constant flow rate. As a result, the residence time is not uniform for a given flow rate, but follows a distribution. Changes in the residence time of reactants can result in kinetically controlled products with altered chemical composition and / or physical properties, such as particle size and morphology, which may be undesirable.
[0020] However, improved particle size dispersity can be achieved by continuous segmented flow processing. In this approach, segments of flowing reactants are separated by intervening segments of a non-reactive fluid that is immiscible with the reactants. Confined to a series of relatively short, fixed-length flow segments, the reactants exhibit a tighter distribution of residence times in the various reaction zones, resulting in a more uniform distribution of kinetically controlled products.
[0021] As described in more detail herein, continuous segmented flow processing can be used to create ligand-encapsulated copper selenide nanoparticles of high purity and monodispersity. Upon precipitation from fluid solution under anaerobic conditions, the copper selenide nanoparticles exhibit strong excitonic absorption with an absorbance maximum between 900 and 1200 nanometers (nm), depending on the desired crystallite size. In a more specific example, the absorbance maximum may be between 940 and 1100 nm. These copper selenide nanoparticles can be used in particular to create membrane-coated electrode structures that can be used as near-infrared (NIR) photodetectors.
[0022] The present disclosure is now presented by way of example and with reference to the drawings listed above. Components, process steps, and other elements that may be substantially the same in one or more figures are identified in a coordinated manner and described with minimal repetition. It should be noted, however, that coordinately identified elements may differ to some extent. It should also be noted that the figures are schematic and generally not drawn to scale. Rather, the scales, aspect ratios, and number of components of the various figures shown in the figures may be intentionally distorted to facilitate viewing of certain features or relationships.
[0023] Figure 1 illustrates an embodiment of an example continuous segmented flow reactor system 10. The reactor system is suitable for making semiconductor nanoparticles, such as copper selenide nanoparticles.
[0024] The reactor system 10 includes a precursor reservoir 12A, a precursor reservoir 12B, and a diluent reservoir 12D. In an example relating to the synthesis of copper selenide nanoparticles, the precursor reservoir 12A can include a flowable solution and / or suspension of a suitable copper starting material, and the precursor reservoir 12B can include a flowable solution and / or suspension of a suitable selenium starting material. The diluent reservoir 12D can include any suitable diluent mixture, such as a mixture of liquids used to dissolve or suspend the copper and / or selenium starting materials. In some examples, the contents of the precursor reservoirs 12A and 12B and / or the diluent reservoir 12D are maintained under a non-reactive atmosphere, such as an atmosphere of nitrogen, argon, or helium. In some examples, the reservoirs can include a gas dispersion unit configured to emit bubbles of a non-reactive gas 14 into a solution or suspension contained therein. In this manner, any, some, or all of the contents of the reservoir can be actively deoxygenated and maintained under a blanket of non-reactive atmosphere.
[0025] The reactor system 10 includes a multi-channel pump 16 configured to draw the contents of the precursor reservoirs 12A and 12B and the diluent reservoir 12D into a pre-mix vessel 18. The multi-channel pump can draw the contents of each of the reservoirs at a controlled volumetric rate based on the configuration and / or settings of the multi-channel pump. In some examples, the multi-channel pump can be a peristaltic pump with a common rotor driving each channel. Alternatively, multiple single channel pumps can be used. The pre-mix vessel 18 is a vessel in which the fluid solution and / or suspension is homogenized to form a fluid reaction mixture. The pre-mix vessel can include a mechanical or magnetic stir bar or impeller in some examples. In other examples, the fluid solution can be homogenized in-line, for example, via a T-piece and a mixing stage downstream of the T-piece.
[0026] The reactor system 10 includes a single channel or other pump 20 configured to draw the contents of the premix vessel 18 into an optional preheater 22. The single channel pump may be a gear pump in some examples. The preheater may be configured to preheat the discharge from the single channel pump to a desired temperature. To that end, the preheater may include a heating tape or heating wire wrapped around a conduit carrying the discharge from the single channel pump. In the example shown in FIG. 1, this conduit leads to a segmentation unit 24, where each controlled length segment of the discharge from the single channel pump is interrupted by bubbles of non-reactive gas 14. In this manner, a segmented stream of preheated reaction mixture is formed.
[0027] The reactor system 10 includes an optional microwave unit 26 that receives the split stream and exposes the split stream to microwave radiation. In some, but not all, embodiments, exposure to microwave radiation can nucleate the growth of nanoparticles in the fluid reaction mixture. From the microwave unit 26 (or from the segmentation unit 24 in examples where the microwave unit is omitted), the segmented stream is conducted to a flow heater 28 where the copper selenide nanoparticles are grown to a desired particle size distribution. The flow heater may be configured to provide controlled (e.g., constant temperature) heating of the flowing reactants for a predetermined period of time, which is generally a function of the flow rate and the length of the conduit disposed within the flow heater. In some examples, the flow heater may include a significant length of conduit, arranged in a serpentine or spiral configuration, etc., to reduce the total volume of space to be maintained at a controlled temperature. Thus, in some examples, the flow heater may include a conduit immersed in a controlled temperature liquid bath or routed through a controlled temperature block. In other examples, the flow heater may comprise a conduit disposed within a controlled temperature forced air oven.
[0028] In some examples, the reactor system 10 may include a temperature controller (not shown in the drawings) configured to control the heating power applied by any of the various heating units of the reactor system, such as the preheater 22 and the microwave unit 26. The temperature controller may also control the setpoint temperature of the flow heater 28. Input to the temperature controller is provided via temperature sensors 30A, 30B, 30C, which are fluidly disposed downstream of the segmentation unit 24, the microwave unit 26, and the flow heater 28, respectively. In this manner, the temperature controller can provide closed-loop control over the heating power delivered to the various stages of the reactor system. However, it should be noted that alternative temperature control strategies can also be used.
[0029] The reactor system 10 includes a cooler 32 configured to rapidly cool the split product stream emerging from the flow heater 28. Cooling stops the growth of the copper selenide nanoparticles and facilitates their subsequent collection. The cooler may include a heat exchanger in which heat from the flowing product is transferred, for example, to chilled or ambient temperature water. From the cooler, the product flows to a collection unit 34. In the collection unit, the flowing product is added to an excess of a deoxygenated liquid in which the product does not dissolve, but which is miscible with the solvent system in which the product dissolves. This action causes the nanoparticle product to precipitate in aggregate, i.e., solid form. Thus, the collection unit may include a filter or centrifuge configured to separate and thereby collect the copper selenide nanoparticle aggregates (solid product) from the deoxygenated liquid. In some examples, the filtered or centrifuged aggregates (solid product) can be rinsed with additional deoxygenated liquid before final collection. In some examples, the deoxygenated liquid can include a relatively polar solvent sparged into the solvent reservoir 12S, for example with nitrogen, argon, or helium, to remove dissolved oxygen.
[0030] 2 shows an exemplary process 36 for preparing air-stable, ligand-encapsulated copper selenide nanoparticles. In some examples, the method can be carried out using a continuous segmented flow reactor system as described above. However, it is understood that other reactor systems can also be used for this process.
[0031] In steps 36-38, a flowable copper precursor is formed as a solution or suspension of a suitable copper starting material. The flowable copper precursor can be formed by combining a copper starting material, a ligand, and optionally a solvent. The copper starting material can be a monovalent copper simple salt or complex salt. In some examples, the copper starting material can include substantially anhydrous copper(I) chloride. In other non-limiting examples, the copper starting material can include substantially anhydrous copper(I) bromide or copper(I) acetate. The ligand can be an organic compound capable of coordinating monovalent copper to form a soluble complex ion. The ligand can also be attached to the outside of the copper selenide nanoparticle product of process 36, thereby encapsulating each nanoparticle in an organized lipid layer. The encapsulation stabilizes the nanoparticles after synthesis, effectively "locking" the product particle size distribution. Nevertheless, the ligand can be exchangeably attached to the nanoparticle product such that in some examples, a ligand molecule with a greater affinity for the nanoparticle product can replace any, some, or all of the ligands incorporated during synthesis. The ligand exchange strategy can be used to prepare structures of copper selenide nanoparticles for various applications (see below).
[0032] Continuing with process 36, the ligand may include an amine having at least one relatively long chain (>10 carbon atoms) aliphatic substituent, although other types of ligands are also contemplated. The ligand may include oleylamine in some examples. The amine ligand may form a complex in the fluid copper-selenium mixture described below, which may contribute to the formation of uniform copper selenide nanoparticles. The solvent, if included, may be any relatively high boiling point solvent (bp>250° C.) capable of dissolving the lipophilic, ligand-encapsulated copper selenide nanoparticles. Examples include non-polar solvents and solvents with relatively low polarity, such as hydrocarbons. The use of solvents with relatively low polarity may be compatible with the precursor, the ligand, and contribute to the formation of more uniform copper selenide nanoparticles. The solvent may include 1-octadecene in some examples. In some examples, the fluid copper precursor may be deoxygenated by sparging with a non-reactive gas, such as nitrogen, argon, or helium. Deoxygenating the fluid copper precursor may eliminate factors that degrade the properties of the copper selenide nanoparticles during the flow process. It is noted that the incorporation of a solvent in addition to the ligand can be particularly advantageous in the flow synthesis of copper selenide nanoparticles, where dilution of the reaction system is a viable strategy to avoid clogging.
[0033] At 40, a flowable selenium precursor is formed by dissolving and / or suspending a suitable selenium starting material (e.g., elemental black selenium) in a liquid. By inference, other selenium allotropes can be used. In some examples, the liquid components of the flowable selenium precursor can be the same as the liquid components of the flowable copper precursor. More specifically, it can include amine ligands that can bind to the selenium starting material to form a soluble complex. In other examples, the liquid components of the flowable selenium precursor can be somewhat different from the liquid components of the flowable copper precursor. In some examples, the flowable selenium precursor can be deoxygenated by sparging with a non-reactive gas such as nitrogen, argon, or helium. Deoxygenating the flowable selenium precursor can eliminate factors that degrade the properties of the copper selenide nanoparticles during the flow process.
[0034] At 42, a flowable copper-selenium mixture is formed by combining a flowable copper precursor and a flowable selenium precursor. In some examples, the flowable copper-selenium mixture can include 1 molar equivalent of copper (from the flowable copper precursor) for every 1-3 molar equivalents of selenium (from the flowable selenium precursor). Furthermore, the fluid copper-selenium mixture preferably contains 0.5 moles or more of amine ligand per molar equivalent of copper. By containing 0.5 moles or more of amine ligand per molar equivalent of copper, a copper-selenium-amine complex is formed in the fluid copper-selenium mixture. The copper-selenium-amine complex is present in the fluid copper-selenium mixture as an aggregate containing copper atoms and selenium atoms at a certain ratio. In the flow process, by passing through a heating unit, adjacent copper-selenium atoms in the complex first react with each other in the fluid copper-selenium mixture, uniform nucleation occurs, and then grain growth occurs. Therefore, the composition ratio of the obtained copper selenide nanoparticles is stable, and copper selenide nanoparticles having a high peak-to-valley ratio are obtained. In the fluid copper-selenium mixture, the amount of the amine ligand is not particularly limited as long as it is 0.5 or more per 1 molar equivalent of copper. However, since the above-mentioned effects can be obtained as long as there is a sufficient amount of the amine ligand to form a complex between copper and selenium, the amount of the amine ligand is preferably 50 or less, and more preferably 30 or less, per 1 molar equivalent of copper.
[0035] At 44, the fluid copper-selenium mixture is conducted through at least one heating unit. In some examples, the fluid copper-selenium mixture may be conducted through two or more heating units. Further, in some examples, the fluid copper-selenium mixture may be conducted through a microwave unit. Further, in some examples, the fluid copper-selenium mixture may be conducted through a flow heater maintained at a temperature in the range of 220-300°C. The heating unit is preferably one in which the conduit is disposed in a medium of controlled temperature. In particular, when the flow heater is one in which the conduit is immersed in a bath maintained at a designated set point temperature, the resulting copper selenide nanoparticles have low variability in properties. Conventionally, in the flow process, the nucleation and growth of particles are separated by passing through two or more heating units, resulting in uniform particles. However, by using the above-mentioned copper-selenium-amine complex in the fluid copper-selenium mixture, the nucleation and growth of particles are uniform even in a single heating unit, making it possible to obtain uniform copper selenide nanoparticles in the end. The ability to obtain high-quality copper selenide nanoparticles with fewer steps is industrially advantageous.
[0036] In 46, the solution containing copper selenide nanoparticles is combined with an excess of a deoxygenated highly polar solvent to precipitate air-stable copper selenide nanoparticles. The nanoparticles are isolated in an oxygen-depleted environment, which is believed to reduce the level of impurities in the product. The inventors herein have noted that aerobic workup of copper selenide nanoparticles typically results in a color change indicative of product degradation or the formation of undesirable by-products. That is, by carrying out not only the synthesis of copper selenide nanoparticles but also the isolation step, where nanoparticle growth has already been completed, in an anaerobic atmosphere, the final copper selenide nanoparticles are more air-stable and have a higher peak-to-valley ratio. In some examples, the highly polar solvent may include absolute ethanol, which is freely miscible with 1-octadecene and other solvents that readily dissolve the ligand-encapsulated copper selenide nanoparticles. Other highly polar solvents are also contemplated.
[0037] FIG. 3 shows an exemplary UV-visible absorption spectrum of an n-hexane solution of copper selenide nanoparticles prepared according to the method of FIG. 2. The spectrum shows excitonic absorption with an absorbance maximum (λmax) at 1096 nm. The excitonic absorption has a half-width at half maximum (HWHM) of 114 millielectron volts (meV) and a peak-to-valley ratio (PVR) of 12.5. In other examples, the excitonic absorption may have an absorption maximum between 900 nm and 1200 nm. In more specific examples, the absorbance maximum may be between 940 and 1100 nm.
[0038] FIG. 4 shows an exemplary energy dispersive X-ray fluorescence (XRF) spectrum of copper selenide nanoparticles prepared according to the method of FIG. 2. A solution phase sample was prepared by dissolving copper selenide nanoparticles in n-hexane solution under helium atmosphere. The sample was irradiated and data was collected for about 200 seconds. The spectrum shows a copper Kα peak at 8.05 kiloelectron volts (keV) and a selenium Kα peak at 11.22 keV. The area ratio of the copper Kα peak to the selenium Kα peak is 1.75.
[0039] Figures 5A and 5B show example transmission electron microscope (TEM) micrographs of copper selenide nanoparticles prepared according to the method of Figure 2. The micrograph specimens were obtained by depositing the nanoparticles onto a lacy carbon TEM grid from a solution of the nanoparticles in n-hexane. Figure 5A shows a large number of individual copper selenide nanoparticles 48 with diameters of 10-11 nanometers. The size distribution among the nanoparticles is narrow enough that the nanoparticles can self-organize into a series of two-dimensional superlattices 50. Figure 5B is a close-up view of one of the superlattices.
[0040] FIG. 6 shows exemplary particle size histograms of copper selenide nanoparticles prepared according to the method of FIG. 2 using the continuous segmented flow reactor system of FIG. 1. The histograms are based on particle size measurements using TEM micrographs such as those in FIG. 5A and FIG. 5B. Histogram 52 reflects the particle size distribution of nanoparticles collected from the discharge of reactor system 10 over a 20 minute collection interval at a reactant flow rate of 6 mL / min. Histograms 54 and 56 reflect the particle size distribution of nanoparticles collected during two different subintervals of the 20 minute collection interval. In particular, histogram 54 was collected during the 6.67 to 10 minute subinterval, and histogram 56 was collected during the 16.67 to 20 minute subinterval. These results indicate that particle size distributions obtained using a continuous segmented flow reactor system can vary within a collection interval, and collection time can be a useful control parameter to obtain a desired particle size distribution.
[0041] FIG. 7 shows an embodiment of an exemplary film-coated structure 58 that can be fabricated using copper selenide nanoparticles prepared according to the method of FIG. The film coated structure includes an electronically conductive substrate 60. In some examples, the electronically conductive substrate can include a transparent optical flat, such as glass or quartz, supporting a thin coating 62 of a degenerately doped semiconductor, such as indium tin oxide (ITO). The film coated structure includes a plurality of layers 64 of two-dimensional close-packed copper selenide nanoparticles 48 disposed on the electronically conductive substrate. The plurality of layers includes a bridging ligand 66 capable of bridging adjacent layers of the plurality of layers. The term "bridging ligand" is used herein to denote any ligand having two or more donor sites arranged such that different donor sites can bind to different acceptor sites. In the film coated structure 58, the bridging ligand also bridges at least one of the plurality of layers (e.g., base layer 64B) to the electronically conductive substrate. In some examples, the bridging ligand can be α,ω-bifunctional or μ-bifunctional, as known in the art of coordination chemistry. 2More specific examples of bridging ligands include α,ω-dithiols, such as 1,2-ethaneditol and 1,3-propanedithiol.
[0042] Typically, layers 64 of two-dimensionally close-packed copper selenide nanoparticles may contain defect sites 68, or "surface states," that support charge carrier transport through the layers. In the illustrated example, the layers contain void regions 70. To enhance the performance of the film-coated structure as an infrared detector, the void regions may be filled with a dielectric 72. Suitable dielectrics include, for example, aluminum oxide and zirconium oxide.
[0043] Figure 8 illustrates an exemplary process 74 for making a film coated structure such as that shown in Figure 7. At 76 of the process 74, an electronically conductive substrate is treated to remove surface contamination. Suitable processing modes include, for example, mechanical and / or chemical etching, application of cleaning agents and / or solvents, and heat treatment. At 78, a solution of bridging ligands in a non-coordinating solvent is applied to the electronically conductive substrate. The form of application of the solution is not particularly limited. For example, dip coating, spray coating, and / or doctor blade techniques may be used. At 80, a first application of a solution of copper selenide nanoparticles in a non-coordinating solvent is applied to the electronically conductive substrate to assemble the base layer 64B (again, referring to the film-coated structure of FIG. 7). The form of application of the solution is not particularly limited. At this stage of the process 74, the bridging ligands can replace exchangeable ligands that assembled on the outside of the copper selenide nanoparticles during synthesis.
[0044] At 82, the solution of bridging ligand is reapplied to the electronically conductive substrate to support additional layers of copper selenide nanoparticles. At 84, other copper selenide nanoparticle layers are formed by reapplying the copper selenide nanoparticle solution. Steps 82-84 can now be repeated to assemble multiple layers of copper selenide nanoparticles of any desired thickness. Once the desired number of layers have been assembled, the film-coated substrate is dried and placed in an atomic layer deposition (ALD) chamber at 86 where a dielectric is deposited to fill void areas of the film-coated structure.
[0045] It will be understood that the configurations and / or approaches described herein are exemplary in nature, and that these specific embodiments or examples are not to be construed in a limiting sense, as numerous variations are possible. The particular routines or methods described herein may represent one or more of any number of processing strategies. Thus, various operations illustrated and / or described may be performed in the sequence illustrated and / or described, in other sequences, in parallel, or omitted. Similarly, the order of operations described above may be changed.
[0046] The subject matter of the present disclosure includes all novel and non-obvious combinations and subcombinations of the various structures, properties, functions, processes, operations, and other features disclosed herein, and any and all equivalents thereof.
[0047] A method for producing copper selenide nanoparticles according to an embodiment of the present invention includes the following configuration. (1) A method for producing copper selenide nanoparticles by a flow process, comprising: forming a flowable copper precursor by combining a copper starting material with a ligand; forming a flowable selenium precursor by suspending a selenium starting material in a liquid; forming a flowable copper-selenium mixture by combining the flowable copper precursor and the flowable selenium precursor; passing the flowable copper-selenium mixture through at least one heating unit to form a solution containing copper selenide nanoparticles; isolating the copper selenide nanoparticles in an oxygen-depleted environment; Including, the fluid copper-selenium mixture comprises a low polarity solvent; the step of isolating the copper selenide nanoparticles comprises precipitating the copper selenide nanoparticles by combining a solution containing the copper selenide nanoparticles with a deoxygenated highly polar solvent; The high polarity solvent is more polar than the low polarity solvent. A method for producing copper selenide nanoparticles. (2) adding segments of an immiscible, non-reactive fluid to the fluid copper-selenium mixture in a series of fixed length segments to form a segmented stream of the fluid copper-selenium mixture; passing a segmented flow of said fluid copper-selenium mixture through said at least one heating unit. A method for producing copper selenide nanoparticles according to (1) above. (3) combining the copper starting material with the ligand includes combining with the low polarity solvent; A method for producing copper selenide nanoparticles according to (1) or (2) above. (4) The liquid contains the low-polarity solvent. A method for producing copper selenide nanoparticles according to any one of (1) to (3) above. (5) The at least one heating unit includes a conduit disposed within a controlled temperature medium. A method for producing copper selenide nanoparticles according to any one of (1) to (4) above. (6) The ligand comprises an amine ligand. A method for producing copper selenide nanoparticles according to any one of (1) to (5) above. (7) The fluid copper-selenium mixture contains at least 0.5 moles of the amine ligand per mole equivalent of copper. The method for producing copper selenide nanoparticles according to (6) above. (8) sparging the deoxygenated highly polar solvent with a non-reactive gas to remove dissolved oxygen; A method for producing copper selenide nanoparticles according to any one of (1) to (7) above. (9) sparging each of the copper precursor and the selenium precursor with a non-reactive gas to remove dissolved oxygen; A method for producing copper selenide nanoparticles according to any one of (1) to (8) above. (10) The copper starting material comprises a substantially anhydrous copper(I) salt and the selenium starting material comprises elemental selenium. A method for producing copper selenide nanoparticles according to any one of (1) to (9) above. (11) The low polarity solvent comprises 1-octadecene and the high polarity solvent comprises anhydrous ethanol. The method for producing copper selenide nanoparticles according to any one of (1) to (10) above.
[0048] The copper selenide nanoparticle aggregate according to the embodiment of the present invention includes the following configuration. (12) An air-stable copper selenide nanoparticle assembly, Copper selenide nanoparticles encapsulated by ligands and exhibiting exciton absorption with an absorbance maximum between 900 and 1200 nanometers. Copper selenide nanoparticle assemblies. (13) The ligand comprises an exchangeable ligand. The copper selenide nanoparticle aggregate according to (12) above. (14) The ligand comprises an amine ligand. The copper selenide nanoparticle aggregate according to (12) or (13) above. (15) The absorbance maximum has a peak-to-valley ratio of 10 or greater. The copper selenide nanoparticle aggregate according to any one of (12) to (14) above. (16) The copper selenide nanoparticles are crystallized in a two-dimensional close-packed array. The copper selenide nanoparticle aggregate according to any one of (12) to (15) above.
[0049] The copper selenide nanoparticles according to an embodiment of the present invention include the following configuration. (17) Having an absorbance maximum between 900 and 1200 nanometers, and the absorbance maximum has a peak-to-valley ratio of 10 or more. Copper selenide nanoparticles. (18) Encapsulated by a ligand, The copper selenide nanoparticles according to (17) above. (19) The ligand comprises an exchangeable ligand. The copper selenide nanoparticles according to (18) above.
[0050] The film covering structure according to an embodiment of the present invention includes the following configuration. (20) An electronically conductive substrate; and a plurality of layers of two-dimensionally close-packed copper selenide nanoparticles disposed on the electronically conductive substrate; the plurality of layers includes a ligand that bridges adjacent layers of the plurality of layers and bridges at least one of the plurality of layers to the electronically conductive substrate. Film-coated structure. (21) The layers include a plurality of defect sites that support charge carrier transport through the layers. The film-covered structure described in (20) above. (22) The layers include a plurality of void regions filled with a dielectric. A film-covered structure according to (20) or (21) above. (23) The dielectric material comprises aluminum oxide. The film-covered structure described in (22) above. (24) The aluminum oxide is deposited by atomic layer deposition. The film-covered structure described in (23) above. (25) The film covering structure is configured as a near-infrared sensor. The film-covered structure according to any one of (20) to (24) above. (26) The copper selenide nanoparticles according to any one of (17) to (19) above are included. Film-coated structure. EXAMPLES
[0051] [Experimental Example 1] <Preparation of precursor solution> Anhydrous copper(I) chloride was dissolved in a dispersion medium in which oleylamine and 1-octadecene were mixed in a 1:1 ratio to obtain a fluid copper precursor. Next, selenium and 1-octadecene were mixed to obtain a fluid selenium precursor solution. The obtained fluid copper precursor and fluid selenium precursor were mixed with oleylamine to adjust the fluid copper-selenium mixture so that the molar ratio of copper:selenium:oleylamine in the fluid copper-selenium mixture was 1:1:12. <Preparation of copper selenide nanoparticles by flow process> The resulting fluid copper-selenium mixture was passed through a conduit at 6 mL / min, and N2 gas was introduced to create a segmented flow. The mixture was passed through a microwave unit with a frequency set to 2 kW, and then through an oven set to 220°C to obtain a fluid containing copper selenide nanoparticles. In an anaerobic atmosphere, an excess amount of deoxygenated anhydrous ethanol was added to the fluid containing copper selenide nanoparticles to precipitate the copper selenide nanoparticles.
[0052] [Experimental Example 2]~[Experimental Example 5] The fluid copper precursor solution prepared in Experimental Example 1 was deoxygenated by spraying N2 gas. Furthermore, the fluid selenium precursor solution prepared in Experimental Example 1 was deoxygenated by spraying N2 gas. Using both precursor solutions from which dissolved oxygen had been removed, a fluid copper-selenium mixture having the same molar ratio of copper:selenium:oleylamine as in Experimental Example 1 was obtained. The nanoparticles were produced by the flow process under the same conditions as in Experimental Example 1, and copper selenide nanoparticles were produced. This was repeated four times, and the results are shown as the values of Experimental Example 2 to Experimental Example 5, respectively. The precursor solution was also deoxygenated to obtain copper selenide nanoparticles with a higher peak-to-valley ratio.
[0053] [Experimental Example 6] The fluid copper precursor solution from which dissolved oxygen had been removed, prepared in Experimental Example 2, and the fluid selenium precursor solution from which dissolved oxygen had been removed, and oleylamine were mixed to prepare a fluid copper-selenium mixture so that the molar ratio of copper:selenium:oleylamine in the fluid copper-selenium mixture was 1:1:20. The flow process conditions were the same as in Experimental Example 1, and copper selenide nanoparticles were produced.
[0054] [Experimental Example 7]~[Experimental Example 9] The fluid copper precursor solution from which dissolved oxygen had been removed, prepared in Experimental Example 2, and the fluid selenium precursor solution from which dissolved oxygen had been removed, were mixed in the same ratio as in Experimental Example 2. Copper selenide nanoparticles were produced in the same manner as in Experimental Example 2, except that when producing nanoparticles by continuous flow, the flow heater was changed from an oven (convection heating) to an immersion heater (conduction heating). This was repeated three times, and the results are shown as the values of Experimental Examples 7 to 9, respectively. By using the immersion method flow heater, the variation in properties of the copper selenide nanoparticles obtained in Experimental Examples 7 to 9 was reduced.
[0055] [Experimental Example 10]~[Experimental Example 11] The fluid copper precursor solution from which dissolved oxygen was removed, prepared in Experimental Example 2, and the fluid selenium precursor solution from which dissolved oxygen was removed were mixed in the same ratio as in Experimental Example 6. Copper selenide nanoparticles were produced under the same conditions as in Experimental Examples 7 to 9. This was repeated twice, and the results are shown as Experimental Example 10 and Experimental Example 11, respectively.
[0056] [fruit Experience Example 12] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that the frequency of the microwave unit was set to 0.
[0057] [fruit Experience Example 13] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that the frequency of the microwave unit was set to 0 and the temperature inside the flow heater was set to 240°C.
[0058] [fruit Experience Example 14] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that the microfluidic copper-selenium mixture was flowed through the conduit at 8 mL / min and the frequency of the microwave unit was set to 0.
[0059] [fruit Experience Example 15] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that the microfluidic copper-selenium mixture was flowed through the conduit at 8 mL / min, the frequency of the microwave unit was set to 0, and the temperature inside the flow heater was set to 240°C. As shown in Experimental Examples 12 to 15, copper selenide nanoparticles having a high PVR value were obtained without separating the nucleation zone from the grain growth zone.
[0060] [Experimental Example 16] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that the molar ratio of copper:selenium:oleylamine in the fluid copper-selenium mixture was 1:1:0.6.
[0061] [Experimental Example 17] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that, instead of adding an excess amount of deoxygenated absolute ethanol to the fluid containing copper selenide nanoparticles, air was purged to create an aerobic atmosphere.
[0062] [Experimental Example 18] Copper selenide nanoparticles were obtained in the same manner as in Experimental Example 7, except that the molar ratio of copper:selenium:oleylamine in the fluid copper-selenium mixture was 1:1:0.3.
[0063] -evaluation- The UV-visible absorption spectrum of the copper selenide nanoparticles prepared in Experimental Examples 1 to 18 was measured in an air environment, and the exciton absorption absorbance maximum (λmax), peak-to-valley ratio (PVR), and half-width at half maximum (HWHM) were obtained. The results are shown in Table 1.
[0064] [Table 1]
[0065] In Examples 1 to 6, the flow heater conduit was placed in an oven controlled to operate at a designated set temperature, and in Examples 7 to 18, the flow heater conduit was immersed in a bath whose temperature was controlled to maintain the designated set temperature. [Explanation of symbols]
[0066] 10. Reactor System 12A, 12B Precursor reservoir 12D Diluent Reservoir 12S Solvent Reservoir 14 Non-reactive gases 16 Multichannel Pump 18 Premix container 20 Pump 22 Preheater 24 Segmentation Unit 26 Microwave Unit 28 Flow Heater 30A, 30B, 30C Temperature Sensors 32 Cooler 34 Collection Unit 36 Process 48 Copper Selenide Nanoparticles 50 Two-dimensional superlattice 52, 54, 56 Histogram 58 Film-coated structure 60 Electronically Conductive Substrates 62 Coating 64 Multiple Layers 64B Base Layer 66 Cross-linking Ligands 68 Defective Area 70 void area 72 Dielectric 74 Process
Claims
1. 1. A method for producing copper selenide nanoparticles by a flow process, comprising: forming a flowable copper precursor by combining a copper starting material with a ligand; sparging the flowable copper precursor with a non-reactive gas to remove dissolved oxygen; forming a flowable selenium precursor by suspending a selenium starting material in a liquid; sparging the flowable selenium precursor with a non-reactive gas to remove dissolved oxygen; forming a flowable copper-selenium mixture by combining the flowable copper precursor and the flowable selenium precursor; passing the flowable copper-selenium mixture through at least one heating unit to form a solution containing copper selenide nanoparticles; isolating the copper selenide nanoparticles in an oxygen-depleted environment; Including, The ligand comprises an amine ligand; the fluid copper-selenium mixture comprises a low polarity solvent and at least 0.5 moles of the amine ligand per molar equivalent of copper; the step of isolating the copper selenide nanoparticles comprises precipitating the copper selenide nanoparticles by combining a solution containing the copper selenide nanoparticles with a deoxygenated highly polar solvent; The high polarity solvent is more polar than the low polarity solvent. A method for producing copper selenide nanoparticles.
2. adding segments of an immiscible non-reactive fluid to the fluid copper-selenium mixture in a series of fixed length segments to form a segmented stream of the fluid copper-selenium mixture; passing a segmented flow of said fluid copper-selenium mixture through said at least one heating unit. The method for producing copper selenide nanoparticles according to claim 1.
3. combining the copper starting material with the ligand includes combining with the low polarity solvent. The method for producing copper selenide nanoparticles according to claim 1 or 2.
4. The liquid comprises the low polarity solvent. The method for producing copper selenide nanoparticles according to any one of claims 1 to 3.
5. the at least one heating unit includes a conduit disposed within a controlled temperature medium; The method for producing copper selenide nanoparticles according to any one of claims 1 to 4.
6. sparging the deoxygenated highly polar solvent with a non-reactive gas to remove dissolved oxygen; The method for producing copper selenide nanoparticles according to any one of claims 1 to 5.
7. It is an air-stable copper selenide nanoparticle aggregate, copper selenide nanoparticles encapsulated by a ligand and exhibiting excitonic absorption with an absorbance maximum between 900 and 1200 nanometers; the absorbance maximum has a peak-to-valley ratio of 10 or greater; Copper selenide nanoparticle assemblies.
8. wherein the ligand comprises an exchangeable ligand; The copper selenide nanoparticle aggregate according to claim 7 .
9. the ligand comprises an amine ligand; The copper selenide nanoparticle aggregate according to claim 7 or 8.
10. The copper selenide nanoparticles are crystallized in a two-dimensional close-packed array. The copper selenide nanoparticle aggregate according to any one of claims 7 to 9.
11. having an absorbance maximum between 900 and 1200 nanometers, said absorbance maximum having a peak-to-valley ratio of 10 or greater, and being encapsulated by a ligand; Copper selenide nanoparticles.
12. wherein the ligand comprises an exchangeable ligand; The copper selenide nanoparticles according to claim 11.
13. 13. A film-coated structure comprising the copper selenide nanoparticles of claim 11 or 12.
Citation Information
Patent Citations
Method for preparing Cu2-xSe nanoparticles in different particle diameters
CN107265411A
Method for forming nanocrystals
JP2010540398A
Reactor for nanoparticle production
JP2011514242A
Ionic nanocrystalline materials with high surface charge density and composites of the same