Polyester composition, its production method and its application
The polyester composition with aliphatic-aromatic copolyesters addresses issues of non-degradability and flexibility in shape memory materials and other products, offering high recovery and fixation rates, low-temperature processing, and environmental sustainability.
Patent Information
- Application Number
- JP2019520899
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-08-16
- Filing Date
- 2017-10-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2037-10-20
AI Technical Summary
Current shape memory materials, 3D printed wires, heat-shrinkable sleeves, medical limb immobilization devices, heat-shrinkable films, non-woven fabrics, and elastic fibers face issues such as non-degradability, limited flexibility, poor fit to body contours, and inadequate adjustability, leading to discomfort and environmental impact.
Development of a polyester composition comprising aliphatic-aromatic copolyesters with specific repeating units and additives, allowing for low-temperature processing, high gloss, and degradability, with applications in shape memory materials, 3D printed wires, heat-shrinkable sleeves, functional layers for sports protectors, medical limb immobilization devices, heat-shrinkable films, non-woven fabrics, and elastic fibers.
The polyester composition achieves high shape recovery and fixation rates, low-temperature printability, and degradability, enhancing comfort and adaptability, reducing environmental footprint, and expanding application possibilities.
Smart Images

Figure 0007584219000063 
Figure 0007584219000064 
Figure 0007584219000065
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of polymeric materials, in particular to polyester compositions, methods for making polyester compositions, and their use in embodiments such as shape memory materials, 3D printed wires, heat shrinkable sleeves, functional layers, medical limb braces, heat shrinkable films, nonwovens, and elastic fibers. [Background technology]
[0002] Shape memory materials are a special class of intelligent materials. After initial formation, thermally stimulated shape memory materials are deformed by external forces at a certain temperature. The stimulated shape memory materials can maintain the deformed shape after cooling; they can restore the original shape after reheating. Shape memory polymers have the advantages of easy processing, light weight, low operating temperature, low cost, etc. Therefore, shape memory polymers are often researched in many high value-added industries. Shape memory polymers are classified into two types, so-called reversible and irreversible.
[0003] CN103160948A discloses a cross-linked shape memory polymer. The deformation fixation rate is about 90-98%, the shape recovery rate is 85-95%, and the maximum deformation rate is usually 20-400%. The initial shape of such a shape memory polymer is not repeatedly reproducible.
[0004] CN105504474A discloses shape memory polymers with a shape recovery rate of 80-95%, a shape fixation rate of about 90-98%, and a maximum deformation rate of about 50%. Although the initial shape of such shape memory polymers is repeatable, their shape recovery rate and shape fixation rate are often inferior to those of irreversible shape memory polymers, and their maximum deformation rate is much worse.
[0005] Currently, there are no commercially available reversible shape-memory polymers that are capable of significant deformation and have both shape recovery and shape retention rates approaching 100%.
[0006] As an additive manufacturing technology, 3D printing offers infinite possibilities for the design and manufacturing of products with complex shapes, and has attracted much attention in recent years. At present, 3D printing technologies mainly include selective laser sintering (SLS), stereolithography (SLA), fused deposition modeling (FDM), etc. Among these, FDM is the simplest and most convenient 3D printing method, with low equipment costs. At present, the market for 3D printing wire for FDM is still relatively limited, and the most important consumables on the market are ABS and PLA. With the promotion of FDM 3D printing technology in different fields, there are also more and more requirements for the physical properties and processing of 3D printed articles.
[0007] At present, the main consumables on the market are hard materials, while soft and elastic materials are still limited. Flexible consumables on the market are mainly polyurethane (TPU) materials (such as polyurethane (TPU) materials described in CN104845353A or TPU composite materials described in CN104004377A). In the TPU materials described in CN104845353A, the printing temperatures presented in the examples are 220°C or higher. In the TPU composite materials described in CN104004377A, the printing temperatures presented are 240-260°C. In commercially available FDM polyurethane wires, the printing temperatures presented are generally above 190°C (such as 190-250°C).
[0008] Therefore, the development of flexible wires that can be printed at low temperatures is of great importance for expanding the applications of 3D printing in different occasions, improving printing safety, reducing energy consumption, etc.
[0009] In the aspect of heat shrinkable sleeves, currently on the market, heat shrinkable sleeves are mainly made of irradiation cross-linked polyolefin materials, and can be restored to their original shape by heating after expansion and molding.
[0010] CN1033402A discloses the construction of a red phosphorus-free, halogen-free heat-shrinkable pipe obtained by crosslinking with ethylene-hexene acetate copolymer, magnesium hydroxide, etc. as the main component.
[0011] In addition, there are some special heat shrink pipes to meet special needs, such as polyvinylidene fluoride (PVDF) heat shrink pipes which are highly resistant to chemical corrosion, optical fiber heat shrink pipes with high transparency, and silicone resin heat shrink pipes with good dielectric properties, etc., to meet various needs.
[0012] However, all of these commercially available products are made from crosslinked polymeric materials, which are difficult to dispose of after disposal, especially the crosslinked polymer network structure is difficult to decompose.
[0013] Currently, in view of the increasingly serious environmental problems, as a kind of disposable product with mass consumption, the thermoplastic sleeve has a potential demand for a biodegradable processing mode.
[0014] CN101049729A discloses a method for producing PET heat shrinkable pipe, the main component of which is polyethylene terephthalate (PET) mixed polyester elastomer. The method can be extruded without crosslinking, but the decomposition of PET is still difficult.
[0015] CN1580092A discloses a copolyester and a method for producing a heat-shrinkable sleeve using the copolyester. The polyester used is a material containing ethylene glycol as a comonomer, which has good shrink properties but is not biodegradable.
[0016] Therefore, there is currently an urgent need to find a heat-shrinkable sleeve that not only has good heat-shrink properties but is also degradable.
[0017] Currently, there are mainly soft and hard protectors in the sports protector market. The inner layer of the most common hard protector on the market is the same as the soft protector in terms of material, and is surrounded by cotton, spandex, and rubber fibers to provide a fixing effect, and is further combined with a middle layer made of EVA or polyurethane and other cushioning materials. The outermost layer is usually made of PP or PE or ABS to provide impact resistance and scratch resistance. The advantage of this type of sports protector is that it is relatively inexpensive, and the disadvantage is that it is not fixed firmly, is prone to falling off and slipping during movement, or has an uncomfortable fit due to a poor match between the shape of the hard outer layer and the shape of the body part to be protected.
[0018] In the development of sports protectors, Dow Corning of the United States proposed a new patented impact resistance technology-Dow Corning Active Protection System, D3O Lab of the United Kingdom developed special clothing such as sports protective helmets using D3O described in US0157083, POC of Sweden independently developed armor protection materials, and Rogers of the United States developed Poron protector materials. In addition, the above-mentioned materials are expensive, and furthermore, they do not have low-temperature plasticity, and cannot be adjusted to the shape according to individual needs after wearing on the human body. In addition, these materials do not have high-temperature memory recovery function, and after being scratched, the appearance and subsequent use will be greatly affected.
[0019] In addition, the role of dental shields in sports protectors is also very important. The materials of finished dental shields are mainly rubber, polyvinyl chloride, and polyvinyl acetate-polyethylene copolymer. Finished dental shields are cheap, cannot be modified according to individual needs, are uncomfortable when worn, easily cause discomfort, affect movement, and have been gradually abandoned. At present, semi-finished products molded in the oral cavity are divided into two categories (one is hard shell soft core dental shields, the other is thermoplastic polymer materials). For hard shell soft core dental shields, acrylic materials and EVA are injected into the hard shell (polyvinyl chloride) as a soft core and integrally attached to the teeth. The said thermoplastic polymer materials are usually polyvinyl acetate-polyethylene copolymers, which are molded by biting in the mouth after heating with hot water. These two forms of dental shields can provide a certain degree of protection performance, but due to low plasticity and too short thermoplastic time, wearing is not comfortable enough, and due to repeated heating and the influence of oral saliva, the service life of these types of products is short.
[0020] A thermoplastic dental shield is described in US005339832A, in which an elastic body is embedded in the appliance to absorb energy, but it still has the disadvantage that the plasticity is not good enough.
[0021] In addition, in the field of children's dental shields, since the shape of a child's oral cavity keeps changing during growth, a dental shield that can be precisely shaped and has a memory function is a product that is urgently needed in the market.
[0022] In the aspect of medical limb immobilization, there are currently two main categories on the market (one is plaster dressings and the other is polyurethane polymer dressings). In addition, there are relatively expensive cross-linked dressings, which are used only a little in hospitals, and which are mainly made from cross-linked polycaprolactone.
[0023] US4376438 presents a polyurethane-based bandage product, and there are also many improved patents on polymeric bandages in China, such as CN102397133B. Compared with plaster bandages, they have the advantages of high strength, X-ray transparency, and light weight. To be fixed, all polymeric bandages utilize rapid polymerization or hardening via crosslinking of isocyanate prepolymers upon contact with water. The process still requires opening the package, then immersing in water to squeeze multiple times, followed by rapid shaping and rolling of the affected area.
[0024] Furthermore, neither plaster of Paris nor polyurethane polymer dressings are recyclable or decomposable after disposal and are treated as medical waste.
[0025] Therefore, there is an urgent need to find a material suitable for medical limb fixation devices that is easy to mold, has good fixation effect, is easy to remove, and is recyclable.
[0026] Heat shrinkable films are films that can significantly reduce in size after heating. Heat shrinkable films are widely used in the packaging industry. Commonly used heat shrinkable films are polyvinyl chloride films, non-crosslinked polyethylene blown films, polypropylene films, polystyrene films, PET and PETG films. Such films can achieve large shrinkage (up to 75%) in one direction and very small shrinkage (only 1%) in the other direction. In recent years, in addition to pure material films, composite material films have also been used in large quantities as heat shrinkable films, which mainly include the following two categories: (1) POF films (generally polypropylene / polyethylene / polypropylene three-layer co-extruded and blown by double bubble treatment); (2) multilayer co-extruded crosslinked polyethylene films. Some important properties that heat shrinkable films required in the market may have include larger shrinkage, environmental protection (e.g. recyclable, not harmful when burned, etc.), high heat seal strength, good surface gloss, etc. At present, there is no film on the market that has all these properties at the same time.
[0027] Moreover, currently there is no relatively complete solution for degradable heat shrinkable film in the market. As described in CN106519400A, the type of polyolefin film with added photodegradation agent is also claimed to be in the category of degradable film, but such film cannot be completely degraded, and polyolefin can only be degraded into small fragments. Current degradable films include those based on hydroxyalkanoates as described in CN103483789A, and those based on polylactic acid as described in CN103625061B. However, the properties of these current degradable films do not reach the general properties of the general heat shrinkable films described above, so their promotion is hindered.
[0028] Disposable textile articles, especially disposable medical textile articles, are mainly made by nonwoven fabrics. Currently, the common materials of disposable surgical clothing on the market include the following types: polypropylene wood pulp composite spunlace nonwoven fabric, as described in CN20580418U; polypropylene, polyhydroxybutyrate and polylactic acid multilayer composite, as described in CN20439434U and CN105054444A; polyethylene film and SMS nonwoven composite, as described in CN204317582U; nonwoven fabric with resin reinforcement sheet, as described in CN105015128B. After one operation, disposable surgical protective clothing becomes medical waste. Disposal of medical waste causes secondary pollution. Currently, most of the materials on the market are difficult to recycle. Therefore, how to conveniently recycle disposable medical textile articles has become an urgent issue.
[0029] Elastic fiber is a general term that describes a classification of fibers with high elasticity, low modulus, and high elastic recovery. These elastic fibers are broadly divided into two categories. One is elastic fiber obtained by the elasticity of the material itself (e.g., natural rubber fiber, polyurethane fiber (spandex), polyacrylate fiber, polybutylene terephthalate (PBT) fiber, polyether ester elastomer (TPEE) fiber, polytrimethylene terephthalate (PTT) fiber, and polyolefin (XLA) fiber). The elasticity of such elastic fibers is mainly determined by the material itself. Among them, polyacrylate fiber, PBT fiber, and PTT fiber have low elasticity and slight elasticity; natural rubber fiber has high elasticity but weak strength and is easily deteriorated with age; polyurethane fiber has weak strength; polyether ester elastomer fiber has excellent comprehensive properties and can be adjusted in a wide range of properties, but the cost is too high; XLA fiber has good elasticity, good heat resistance, and good mechanical strength, but its properties are relatively fixed and its adaptability is insufficient. The other category is multifilament composite elastic fiber, which utilizes the spiral elasticity resulting from the difference in the shrinkage rate of the two materials, and is generally T400 fiber. The elasticity of such fibers can be controlled by the manufacturing process, but the value of the elastic force caused by the spiral is very low, and is usually much smaller than the elasticity brought about by the material itself.
[0030] Currently, there is no elastic fiber on the market that is low cost, has both suitable elasticity and strength, and has properties that can be adjusted over a wide range to meet the needs of various products.
[0031] In summary, there is a continuing need for improved shape memory materials, 3D printed wires, heat shrink sleeves, functional layers, medical limb fixations, heat shrink films, nonwovens, and elastic fibers that do not suffer from the above-mentioned drawbacks. [Disclosure] Summary of the Invention
[0032] In view of the above, in order to overcome the above-mentioned shortcomings of existing shape memory products, 3D printed wires, heat shrinkable sleeves, functional layers, medical limb braces, heat shrinkable films, nonwoven fabrics and elastic fibers, the object of the present invention is to provide a polyester composition and a method for producing the same, as well as the use of the polyester composition in these materials.
[0033] In particular, an object of the present invention is to provide a polyester composition having excellent low-temperature plasticity and shape memory properties.
[0034] Another object of the present invention is to provide a polyester composition, wherein the 3D printed wire produced from the polyester composition is a flexible wire, can be printed at low temperatures, and also has high gloss and degradability.
[0035] Another object of the present invention is to provide a polyester composition which allows the heat-shrinkable sleeve produced from the polyester composition to have excellent heat-shrinkable and heat insulating properties, and further, the heat-shrinkable sleeve does not require crosslinking during production and has good decomposability, thus expanding the market for heat-shrinkable sleeves.
[0036] Another object of the present invention is to provide a polyester composition which, when used in sports protectors, can be molded according to different application sites so that the protectors are more adapted to the body, more comfortable and easier to manufacture; and when said sports protectors are worn or slightly damaged, can be softened at elevated temperatures and remolded at low temperatures to restore the original appearance again.
[0037] Another object of the present invention is to provide a polyester composition whose hardness changes with time and temperature, in particular, which has a relatively low hardness at a relatively high temperature, and after cooling, the hardness increases obviously in a relatively short time, and which shows good plasticity and fixation. Therefore, the polyester composition is particularly suitable for producing medical limb braces.
[0038] Another object of the present invention is to provide a polyester composition, the heat shrinkable film produced from which not only has a relatively high heat shrinkage rate, but also can change the heat shrinkage rate within a wider range to meet different needs.In addition, the heat shrinkable film has suitable heat seal strength, has a flat surface with good gloss, is degradable, and can be repeatedly thermoplastically processed and recycled.
[0039] Another object of the present invention is to provide a polyester composition, which is a nonwoven fabric produced from the polyester composition, which has good water absorption, gas permeability, and is easy to sterilize. In particular, the nonwoven fabric can be disinfected in hot water (e.g., 100°C) and shrinks significantly. Therefore, the nonwoven fabric can be easily compressed and reduced in volume. This is convenient for restoring and regenerating materials (especially disposable materials). Furthermore, the newly produced nonwoven fabric has similar properties to those of the nonwoven fabric that was initially used, and is suitable for continuing to function as a starting material for disposable nonwoven fabric articles (especially disposable medical textile articles).
[0040] Another object of the present invention is to provide a polyester composition which produces elastic fibers having both suitable elasticity and strength, and which allows the properties to be adjusted over a wide range.
[0041] According to the present invention, the above object is achieved by a polyester composition comprising a specific aliphatic-aromatic copolyester.
[0042] Specifically, the present invention provides the following aspects.
[0043] In a first aspect, the present invention provides a method for producing a composition comprising the steps of: (1) A plurality of aliphatic-aromatic copolyesters, which are copolymers containing a repeating unit A represented by formula (I) and a repeating unit B represented by formula (II).
[0044] [ka]
[0045] (wherein, with respect to the total molar amount of the repeating unit A and the repeating unit B in the aliphatic-aromatic copolymer, the content of the repeating unit A is 51 to 95 mol %, the content of the repeating unit B is 5 to 49 mol %, and preferably, the content of the repeating unit A is 55 to 80 mol %, and the content of the repeating unit B is 20 to 45 mol %; m is an integer of 2 to 10, preferably 2 to 6, more preferably 2 to 4; n is an integer of 2 to 8, preferably 2 to 4; p is an integer of 2 to 10, preferably 2 to 4; and m, n, and p are the same or different from each other). a first polyester which is one or more selected from the following, in an amount of 50 to 100% by weight, preferably 51 to 99% by weight, based on the total weight of the first polyester and the second polyester; (2) Optionally, a second polyester, which is one or more selected from an aliphatic polyester, an aromatic polyester, and an aliphatic-aromatic copolyester different from the first polyester, is added in an amount of 50% by weight or less, preferably 1 to 49% by weight, based on the total weight of the first polyester and the second polyester. Including, comprising at least two polyesters, A polyester composition is provided.
[0046] Preferably, the aliphatic polyester as the second polyester comprises a repeat unit D represented by formula (I'''):
[0047] [ka]
[0048] (wherein m3 is the same as defined for m above, n3 is the same as defined for n above, m3 and n3 are the same or different from each other, and the aliphatic polyester has a weight average molecular weight of 50,000 to 900,000, preferably 100,000 to 500,000, as measured by gel permeation chromatography (GPC).
[0049] Preferably, the aromatic polyester as the second polyester comprises the repeating unit B represented by formula (II).
[0050] Preferably, the aliphatic-aromatic copolyester as the second polyester, which is different from the first polyester, is a copolymer containing a repeating unit A represented by formula (I) and a repeating unit B represented by formula (II).
[0051] Preferably, the aliphatic-aromatic copolyester as the first polyester or the second polyester, comprising the repeating unit A represented by formula (I) and the repeating unit B represented by formula (II), has a weight average molecular weight of 50,000 to 900,000, preferably 100,000 to 500,000, as measured by GPC, and preferably has a molecular weight distribution of 1.2 to 3, as measured by GPC.
[0052] The aliphatic-aromatic copolyester as the first polyester may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers and graft copolymers; the aliphatic-aromatic copolyester as the second polyester may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers and graft copolymers.
[0053] The polyester composition of the present invention may further comprise one or more additives selected from the group consisting of nucleating agents, fibrous fillers, auxiliary fillers that act to promote solidification of the composition melt, adjust the mechanical strength of the composition, adjust the color and gloss of the composition, and improve the flame retardancy and oxidation resistance of the composition, and erucylamide and / or white oil.
[0054] For example, the auxiliary filler may be a small compound selected from the group consisting of carbonates, silicates, sulfates, inorganic hollow microspheres, metal powders, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylates, metal phosphates, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low density polyethylene, polyphosphate esters or salts, phosphites, hindered phenols, hindered amines, dibenzyl sorbitol and derivatives thereof, highly branched polyamides, ethylene-methacrylic acid ionomers, ethylene bisstearamide, silicone powders, and pentaerythritol stearate. At least one, preferably at least two; preferably at least one, preferably at least two selected from the group consisting of calcium carbonate, anhydrous calcium sulfate, copper powder, iron oxide, carbon black, titanium dioxide, tris(2,3-dibromopropyl)phosphate, low-density polyethylene, highly branched polyamide, ethylene bisstearamide and erucylamide, and preferably, the content of the auxiliary filler is 0.1 to 60% by weight, preferably 0.1 to 50% by weight, more preferably 1 to 25% by weight, more preferably 1 to 20% by weight, and even more preferably 2 to 10% by weight, based on the total weight of the polyester composition.
[0055] For example, the nucleating agent is one or more selected from the group consisting of talc, calcium oxide, carbon black, calcium carbonate, inorganic pigments, kaolin, metal carboxylates, metal phosphates, dibenzyl sorbitol and derivatives thereof, polyvinylcyclohexane, polyvinylcyclopentane, low-density polyethylene, highly branched polyamides, and ethylene-methacrylic acid ionomers; preferably, the nucleating agent may be one or more selected from the group consisting of calcium carbonate, low-density polyethylene, dibenzyl sorbitol and derivatives thereof, and highly branched polyamides, and preferably, the content of the nucleating agent is 0.01 to 20% by weight, preferably 0.2 to 5% by weight, based on the total weight of the polyester composition.
[0056] For example, the fibrous filler may be one or more selected from the group consisting of carbon fiber, glass fiber, basalt fiber, aramid fiber, and PET fiber, preferably the fibrous filler may be one or more selected from the group consisting of glass fiber, carbon fiber, and basalt fiber, and preferably the length of the fibrous filler is 0.1 to 10 mm, preferably 0.5 to 2 mm.
[0057] In a first preferred embodiment, the polyester composition according to the present invention comprises: (1) Polyester A is a copolymer containing a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1), (2) Polyester B, which is a copolymer containing a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1); (3) Aliphatic polyester Includes
[0058] [ka]
[0059] (wherein m1 and m2 are, independently of one another, the same as defined for m above, n1 and n2 are, independently of one another, the same as defined for n above, m1 and n1 are the same or different from one another, m2 and n2 are the same or different from one another, and n1 is less than n2); The content of the repeating unit B is 5 to 49 mol %, preferably 10 to 45 mol %, and more preferably 20 to 40 mol %, based on the total number of moles of the polyester A, the polyester B, and the aliphatic polyester.
[0060] Preferably, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A, the content of the repeating unit A is 51 to 90 mol % and the content of the repeating unit B is 10 to 49 mol %; based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B, the content of the repeating unit C is 40 to 95 mol %, preferably 50 to 90 mol %, and the content of the repeating unit B is 5 to 60 mol %, preferably 10 to 50 mol %.
[0061] The molar ratio of the polyester A, the polyester B and the aliphatic polyester is preferably 20-90:1-90:1-20, and more preferably 20-90:1-70:1-20.
[0062] In a second preferred embodiment, the polyester composition according to the invention comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I-1) and repeating unit B represented by formula (II-1)
[0063] [ka]
[0064] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, m1 and n1 are the same or different from each other, a1 is the same as defined for p above, and a1 and m1 are the same or different from each other) 51 to 98% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I') and repeating unit D represented by formula (IV')
[0065] [ka]
[0066] 1 to 48% by weight of polyester B, which is a copolymer comprising: (3) Repeating unit E represented by formula (I'') and repeating unit F represented by formula (IV'')
[0067] [ka]
[0068] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, m2 and n2 are the same or different from each other, a2 is the same as defined for p above, and a2 and m2 are the same or different from each other) 1 to 48% by weight of polyester C, which is a copolymer containing Including, the content of the repeating unit A is 56 to 80 mol %, preferably 60 to 75 mol %, and the content of the repeating unit B is 20 to 44 mol %, preferably 25 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; the content of the repeating unit C in the polyester B is 81 to 99 mol %, preferably 85 to 95 mol %, and the content of the repeating unit D is 1 to 19 mol %, preferably 5 to 15 mol %, based on the total number of moles of the repeating unit C and the repeating unit D in the polyester B; Based on the total number of moles of the repeating units E and F in the polyester C, the content of the repeating unit E is 0 to 55 mol %, preferably 15 to 50 mol %, and the content of the repeating unit F is 45 to 100 mol %, preferably 50 to 85 mol %.
[0069] Preferably, the polyester composition contains 70 to 94% by weight of the polyester A, 3 to 25% by weight of the polyester B, and 3 to 20% by weight of the polyester C.
[0070] In a third preferred embodiment, the polyester composition according to the invention comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0071] [ka]
[0072] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, and m1 and n1 are the same or different; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, preferably 2). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0073] [ka]
[0074] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, and m2 and n2 are the same or different; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, preferably 2). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 51 to 70 mol %, preferably 55 to 68 mol %, and the content of the repeating unit B is 30 to 49 mol %, preferably 32 to 45 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; Based on the total number of moles of the repeating units C and B in the polyester B, the content of the repeating unit C is 1 to 50 mol %, preferably 20 to 45 mol %, and the content of the repeating unit B is 50 to 99 mol %, preferably 55 to 80 mol %.
[0075] Preferably, the polyester composition contains the polyester A in an amount of 80 to 95% by weight and the polyester B in an amount of 5 to 20% by weight.
[0076] In a fourth preferred embodiment, the polyester composition according to the invention comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0077] [ka]
[0078] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, preferably 4). 50 to 98% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0079] [ka]
[0080] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, preferably 2). 1 to 49% by weight of polyester B, which is a copolymer comprising: (3) 1 to 49% by weight of fiber filler Including, the content of the repeating unit A is 55 to 79 mol %, preferably 60 to 77 mol %, and the content of the repeating unit B is 21 to 45 mol %, preferably 23 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; With respect to the total number of moles of the repeating unit C and the repeating unit B in the polyester B, the content of the repeating unit C is 80 to 100 mol %, preferably 85 to 95 mol %, and the content of the repeating unit B is 0 to 20 mol %, preferably 5 to 15 mol %.
[0081] Preferably, the polyester composition comprises 60 to 90% by weight of the polyester A, 5 to 30% by weight of the polyester B, and 5 to 30% by weight of the fibrous filler.
[0082] In a fifth embodiment, the polyester composition according to the invention comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0083] [ka]
[0084] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, preferably, n1 is 2). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0085] [ka]
[0086] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, and preferably, n2 is 2). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 60 to 80 mol %, preferably 62 to 78 mol %, and the content of the repeating unit B is 20 to 40 mol %, preferably 22 to 38 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; Based on the total number of moles of the repeating units C and B in the polyester B, the content of the repeating unit C is 20 to 59 mol %, preferably 30 to 55 mol %, and the content of the repeating unit B is 41 to 80 mol %, preferably 45 to 70 mol %.
[0087] Preferably, the polyester composition contains the polyester A in an amount of 70 to 90% by weight and the polyester B in an amount of 10 to 30% by weight.
[0088] In a sixth preferred embodiment, the polyester composition according to the invention comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0089] [ka]
[0090] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, and preferably, n1 is 2). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0091] [ka]
[0092] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, and preferably, n2 is 2). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 60 to 80 mol %, preferably 62 to 72 mol %, and the content of the repeating unit B is 20 to 40 mol %, preferably 28 to 38 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; Based on the total number of moles of the repeating units C and B in the polyester B, the content of the repeating unit C is 81 to 99 mol %, preferably 85 to 97 mol %, and the content of the repeating unit B is 1 to 19 mol %, preferably 3 to 15 mol %.
[0093] Preferably, the polyester composition contains the polyester A in an amount of 60 to 90% by weight and the polyester B in an amount of 10 to 40% by weight.
[0094] In a seventh preferred embodiment, the polyester composition according to the invention comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0095] [ka]
[0096] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, and preferably, n1 is 2). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0097] [ka]
[0098] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, and preferably, n2 is 2). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 75 to 95 mol %, preferably 81 to 95 mol %, and the content of the repeating unit B is 5 to 25 mol %, preferably 5 to 19 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; Based on the total number of moles of the repeating units C and B in the polyester B, the content of the repeating unit C is 20 to 74 mol %, preferably 40 to 70 mol %, and the content of the repeating unit B is 26 to 80 mol %, preferably 30 to 60 mol %.
[0099] Preferably, the polyester composition contains the polyester A in an amount of 55 to 70% by weight and the polyester B in an amount of 30 to 45% by weight.
[0100] In an eighth preferred embodiment, the polyester composition according to the invention comprises the following components, based on the total weight of the various components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0101] [ka]
[0102] (wherein m1 is the same as defined for m above, n1 is the same as defined for n above, and m1 and n1 are the same or different from each other; preferably, m1 is an integer of 2 to 8, and n1 is an integer of 2 to 6, and more preferably, m1 is an integer of 2 to 4, and n1 is an integer of 2 to 4). 30 to 98% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0103] [ka]
[0104] (wherein m2 is the same as defined for m above, n2 is the same as defined for n above, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4). 1 to 69% by weight of polyester B, which is a copolymer comprising: (3) Repeating unit D represented by formula (I''') and repeating unit B represented by formula (II-1)
[0105] [ka]
[0106] (wherein m3 is the same as defined for m above, n3 is the same as defined for n above, and m3 and n3 are the same or different from each other; preferably, m3 is an integer of 2 to 8, and n3 is an integer of 2 to 6, and more preferably, m3 is an integer of 2 to 4, and n3 is an integer of 2 to 4). 1 to 69% by weight of polyester C, which is a copolymer containing Including, the content of the repeating unit A is 51 to 80 mol %, preferably 60 to 75 mol %, and the content of the repeating unit B is 20 to 49 mol %, preferably 25 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; the content of the repeating unit C in the polyester B is 81 to 99 mol %, preferably 83 to 95 mol %, and the content of the repeating unit B is 1 to 19 mol %, preferably 5 to 17 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; Based on the total number of moles of the repeating unit D and the repeating unit B in the polyester C, the content of the repeating unit D is 0 to 49 mol %, preferably 15 to 45 mol %, and the content of the repeating unit B is 51 to 100 mol %, preferably 55 to 85 mol %.
[0107] Preferably, the polyester composition contains 60 to 93% by weight of the polyester A, 5 to 38% by weight of the polyester B, and 1 to 20% by weight of the polyester C.
[0108] In another aspect, the present invention provides a method for preparing the polyester blend according to the present invention, comprising the steps of mixing all the components including the first polyester and the second polyester, and then extruding and pelletizing the resulting mixture to obtain a polyester composition, preferably without adding a compatibilizer during the mixing step.
[0109] Preferably, the mixing step is carried out under stirring.
[0110] Preferably, the extrusion and pelletization is carried out in a twin-screw extruder, preferably at 80 to 270° C., preferably 110 to 220° C., with a screw rotation speed of 10 to 70 rpm and a torque of 2 to 80 N·m.
[0111] In another aspect, the present invention provides the use of the polyester composition of the present invention in one or more of the following aspects: shape memory materials, 3D printed wires, heat shrinkable sleeves, functional layers (e.g., functional layers for sports protectors), sports protectors (e.g., dental protectors, limb joint protectors, large area protectors for body and head protectors), medical limb immobilizers, heat shrinkable films, nonwoven fabrics and nonwoven articles (particularly disposable nonwoven articles, more preferably disposable medical nonwoven articles).
[0112] In another aspect, the present invention provides a shape memory material comprising a polyester composition according to the first preferred embodiment described above.
[0113] In another aspect, the present invention provides a 3D printing wire comprising the polyester composition according to the second preferred embodiment described above. Preferably, the 3D printing wire has a diameter of 0.1 to 10 mm, preferably 1 to 4 mm.
[0114] In another aspect, the present invention provides a method for producing a 3D printed wire according to the present invention, comprising the steps of continuously extruding a polyester composition and cooling it to obtain a 3D printed wire; preferably, the extrusion temperature is 90 to 260°C, and the cooling temperature is 0 to 60°C.
[0115] In another aspect, the present invention provides a heat shrinkable sleeve comprising a polyester composition according to the third preferred embodiment described above.
[0116] In another aspect, the present invention provides a method for producing the heat-shrinkable sleeve according to the present invention, comprising the steps of continuously extruding, stretching, cooling and forming a polyester composition to obtain a heat-shrinkable sleeve; the extrusion temperature is preferably 90 to 240°C, preferably 120 to 180°C, and the cooling temperature is preferably 0 to 60°C, preferably 20 to 40°C.
[0117] Preferably, the method further comprises the steps of successively heating, diameter expanding, secondary cooling and forming the cooled pipe, preferably the heating temperature is 65-120°C, preferably 70-90°C; preferably the expansion ratio of the diameter expansion is 1.5-5 times, preferably 3-5 times, of the original size; preferably the secondary cooling temperature is 0-60°C, preferably 20-40°C.
[0118] In another aspect, the present invention provides a functional layer, preferably a functional layer for a sports protector, comprising the polyester composition according to the fourth preferred embodiment described above.
[0119] In another aspect, the present invention provides a method for producing a functional layer according to the present invention, comprising a step of molding a polyester composition, the molding step being preferably extrusion molding or injection molding; preferably, the injection molding temperature is 140 to 270°C, preferably 170 to 185°C.
[0120] In another aspect, the present invention provides a medical limb fixation device comprising a polyester composition according to the above-mentioned fifth preferred embodiment; preferably the thickness of the medical limb fixation device is from 0.2 to 10 mm, preferably from 1 to 3 mm, and preferably the medical limb fixation device has and / or does not have a pore structure, preferably has a pore structure, more preferably the pore size of the pore structure is from 1 to 10 mm, preferably from 1 to 5 mm.
[0121] In another aspect, the present invention provides a method for producing a medical limb fixation device according to the present invention, comprising the steps of continuously extruding and molding a polyester composition, and optionally punching holes to obtain a medical limb fixation device; preferably, the extrusion temperature is 90 to 230°C, preferably 110 to 170°C, and preferably, the molding is injection molding and / or compression molding; preferably, the molding step results in a thickness of the medical limb fixation device of 0.2 to 10 mm, preferably 1 to 3 mm; and preferably, the diameter of a puncher used in the hole punching step is 1 to 10 mm, preferably 1 to 5 mm.
[0122] In another aspect, the present invention provides a heat shrinkable film comprising a polyester composition according to the sixth preferred embodiment described above.
[0123] In another aspect, the present invention provides a method for producing a heat-shrinkable film according to the present invention, comprising a step of continuously forming the polyester composition into a film by steps of casting, leaving and stretching to obtain a heat-shrinkable film; preferably, the temperature for the film formation is 80 to 220°C, preferably 110 to 180°C; preferably, the leaving time is 30 minutes to 20 days, preferably 4 to 24 hours; preferably, the stretching step is uniaxial stretching or biaxial stretching; and preferably, the stretching temperature is 40 to 150°C, preferably 60 to 120°C.
[0124] In another aspect, the present invention provides a nonwoven fabric comprising a polyester composition according to the seventh preferred embodiment described above.
[0125] In another aspect, the present invention provides a method for producing a nonwoven fabric according to the present invention, comprising the steps of producing a nonwoven fabric from a polyester composition by a spunbonding method; preferably, the spunbonding method comprises an extrusion step, a spinning step, a reticulation step, and a consolidation step; preferably, the extrusion step has three temperature zones, wherein the temperature of the first temperature zone is 140-250°C, the temperature of the second temperature zone is 150-260°C, and the temperature of the third temperature zone is 170-260°C; preferably, the spinning temperature is 150-240°C, and the spinning speed is 10-40 r / min; preferably, the reticulation speed is 5-30 r / min; and preferably, the consolidation step employs a hot rolling method, and the hot rolling temperature is 80-170°C.
[0126] In another aspect, the present invention provides an elastic fiber comprising the polyester composition according to the above-mentioned eighth preferred embodiment; preferably, the elastic fiber has a fiber count of 5 to 500 dtex; a breaking strength of 3 to 19 cN / dtex; an elongation at break of 130 to 620%; a stress relaxation rate of 1 to 12%; and a permanent set rate of 1 to 11%.
[0127] In another aspect, the present invention provides a method for producing an elastic fiber according to the present invention, comprising the steps of continuously forming a polyester composition into a filament, low-temperature placing, and drawing, thereby obtaining the elastic fiber; preferably, the method for forming the filament is melt spinning; preferably, the temperature for the filament formation is 120 to 270°C, preferably 150 to 220°C; preferably, the low-temperature placing conditions include a temperature of 20 to 55°C, preferably 25 to 45°C, and a time of 2 to 120 minutes, preferably 15 to 60 minutes; preferably, the drawing conditions include a temperature of 56 to 110°C, preferably 60 to 90°C, and a draw ratio of 1.2 to 10 times, preferably 2 to 5 times.
[0128] In another aspect, the present invention also provides the use of an aliphatic-aromatic copolyester as the first polyester described above in one or more of the following aspects: shape memory materials, 3D printed wires, heat shrinkable sleeves, functional layers (e.g., functional layers for sports protectors), sports protectors (e.g., dental protectors, limb joint protectors, large area protectors for body and head protectors), medical limb immobilizers, heat shrinkable films, nonwovens and nonwoven articles (particularly disposable nonwoven articles, more preferably disposable medical nonwoven articles). [Brief description of the drawings]
[0129] [Figure 1] FIG. 1 is a cross-sectional view of a completed dental protector obtained in Example IV-10 according to the present invention (wherein 1 is an oral maxillary appliance and 2 is an oral mandibular appliance). [Diagram 2] FIG. 2 is a side three-dimensional view of the completed dental protector obtained in Example IV-10 according to the present invention. [Diagram 3] FIG. 3 is a side view of the completed knee pad obtained in Example IV-11 of the present invention (wherein 1 is the inner layer of the knee pad, 2 is the middle layer of the knee pad, 3 is the outer layer of the knee pad, and 4 is the protruding part on the surface of the outer layer of the knee pad). [Figure 4] FIG. 4 is a front three-dimensional view of the completed knee pad obtained in Example IV-11 of the present invention (wherein 1 is the inner layer of the knee pad, 2 is the middle layer of the knee pad, 3 is the outer layer of the knee pad, and 4 is the protruding part on the surface of the outer layer of the knee pad). [Diagram 5] FIG. 5 is a front three-dimensional view of the completed upper body protector obtained in Example IV-12 according to the present invention. [Figure 6] FIG. 6 is a cross-sectional view of the completed upper body protector obtained in Example IV-12 of the present invention (wherein 1 is the inner layer of the upper body protector, 2 is the middle layer of the upper body protector, and 3 is the outer layer of the upper body protector). [Figure 7] FIG. 7 is a side view of a completed helmet obtained in Example IV-13 according to the present invention (wherein 1 is the outer layer of the helmet, 2 is the middle layer of the helmet, 3 is the inner layer of the helmet, and 4 is the buckle). [Figure 8] 8 and 9 are diagrams showing an example of a medical limb fixation device according to the present invention. [Figure 9] 8 and 9 are diagrams showing an example of a medical limb fixation device according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0130] Detailed Description of the Invention The polyester composition of the present invention can be used in shape memory materials, 3D printing wires, heat shrinkable sleeves, functional layers, medical limb braces, heat shrinkable films, nonwoven fabrics, elastic fibers, and other embodiments. The polyester composition of the present invention is described below for different applications.
[0131] [Shape memory material] The present invention provides a polyester composition, comprising: (1) Polyester A is a copolymer containing a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1), (2) Polyester B, which is a copolymer containing a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1); (3) Aliphatic polyester Includes
[0132] [ka]
[0133] (wherein m1 is an integer from 2 to 10, n1 is an integer from 2 to 8, and m1 and n1 are the same or different; m2 is an integer from 2 to 10, n2 is an integer from 2 to 8, and m2 and n2 are the same or different); The weight average molecular weight of the polyester A is 50,000 to 900,000. The weight average molecular weight of the polyester B is 50,000 to 900,000; Further, n1 is less than n2; The content of the repeating unit B is 5 to 49 mol % based on the total number of moles of the polyester A, the polyester B, and the aliphatic polyester.
[0134] Preferably, m1 is an integer of 2 to 6, n1 is an integer of 2 to 4, m1 and n1 are the same or different, the weight average molecular weight of the polyester A is 100,000 to 500,000, m2 is an integer of 2 to 6, n2 is an integer of 2 to 4, m2 and n2 are the same or different, the weight average molecular weight of the polyester B is 100,000 to 500,000, and further, n1 is less than n2, and the content of the repeating unit B relative to the total number of moles of the polyester A, the polyester B, and the aliphatic polyester is 5 to 49 mol%, preferably 10 to 45 mol%, more preferably 20 to 40 mol%, more preferably 25 to 40 mol%, or 35 to 45 mol%.
[0135] In the present invention, the weight average molecular weight of the polymer is measured by gel permeation chromatography (GPC).
[0136] In the present invention, the polyester A may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers and graft copolymers, preferably random copolymers and / or block copolymers. The source of polyester A in the present invention is not particularly limited. Polyester A can be obtained by conventional methods in the art. For example, it can be commercially obtained or produced by the process disclosed in CN100429256C. Specifically, the method for producing polyester A includes the following steps: add 1,4-butanediol, dimethyl benzoate and a catalyst described in US11312373 to a reactor, heat and stir under nitrogen atmosphere until a clear solution is obtained; then increase the temperature to 160-220°C for reaction; add succinic acid when removing most of the distilled methanol in the system, and increase the temperature to 180-240°C; remove most of the water by distillation, then slowly create a reduced pressure environment and increase the temperature of the system to 220-280°C; complete the reaction after 3-6 hours to obtain the product.
[0137] In the present invention, the polyester B may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers and graft copolymers, preferably random copolymers and / or block copolymers. The source of polyester B in the present invention is not particularly limited. Polyester B can be obtained by conventional means in the art. For example, it can be obtained commercially or produced by the method disclosed in CN100429256C. Specifically, the method for producing polyester B includes the following steps: 1,4-butanediol, dimethyl benzoate and a catalyst described in US11312373 are added to a reactor, heated and stirred under nitrogen atmosphere until a clear solution is obtained; then, the temperature is raised to 160-220°C for reaction; adipic acid is added when removing most of the distilled methanol in the system, and the temperature is raised to 180-240°C; most of the water is removed by distillation, and then a reduced pressure environment is created slowly, and the temperature of the system is raised to 220-280°C; the reaction is completed after 3-6 hours to obtain the product.
[0138] According to the present invention, the content of the repeating unit A may be 40 to 95 mol %, preferably 45 to 90 mol %, and more preferably 45 to 70 mol %, and the content of the repeating unit B may be 5 to 60 mol %, preferably 10 to 55 mol %, and more preferably 30 to 55 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; With respect to the total number of moles of the repeating unit C and the repeating unit B in the polyester B, the content of the repeating unit C may be 40 to 95 mol %, preferably 50 to 90 mol %, and more preferably 50 to 80 mol %, and the content of the repeating unit B may be 5 to 60 mol %, preferably 10 to 50 mol %, and more preferably 20 to 50 mol %.
[0139] According to the present invention, the molar ratio of the polyester A, the polyester B and the aliphatic polyester may be 20-90:1-90:1-20, preferably 20-90:1-70:1-20.
[0140] In the present invention, the type and source of the aliphatic polyester are not particularly limited, and may be any aliphatic polyester that has been conventionally used in the technical field.
[0141] Preferably, the aliphatic polyester comprises the repeat unit D represented by formula (I'''):
[0142] [ka]
[0143] (wherein m3 is an integer of 2 to 10, n3 is an integer of 2 to 8, m3 and n3 are the same or different, and the weight average molecular weight of the aliphatic polyester is 50,000 to 900,000; more preferably, m3 is an integer of 2 to 6, n3 is an integer of 2 to 4, m3 and n3 are the same or different, and the weight average molecular weight of the aliphatic polyester is 100,000 to 500,000).
[0144] In the present invention, the aliphatic polyester can be obtained by conventional methods. For example, it can be commercially available (for example, purchased from BASF, product name "1111HTA4"), or can be produced according to the method disclosed in CN104039865B. Here, the type of starting material for the reaction can be appropriately adjusted according to the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio, respectively.
[0145] According to the present invention, the polyester composition may further comprise a nucleating agent; the content of the nucleating agent may be 0.01 to 20% by weight, preferably 0.01 to 10% by weight, more preferably 0.2 to 5% by weight, more preferably 1 to 5% by weight, based on the total weight of the polyester composition.
[0146] According to the present invention, the nucleating agent may be selected from conventional in the art. The nucleating agent may be one or more selected from the group consisting of talc, calcium oxide, carbon black, calcium carbonate, inorganic pigments (such as yellow or green pigments purchased from Guangzhou Yingyi Plastic Pigment Co., Ltd.), kaolin, metal carboxylates, metal phosphates, dibenzyl sorbitol and derivatives thereof, polyvinylcyclohexane, polyvinylcyclopentane, low density polyethylene, highly branched polyamides, and ethylene-methacrylic acid ionomers; preferably one or more selected from the group consisting of calcium carbonate, low density polyethylene, dibenzyl sorbitol and derivatives thereof, and highly branched polyamides; more preferably calcium carbonate and / or low density polyethylene.
[0147] In the present invention, the polyester composition may further contain other additives (such as erucylamide and / or white oil).
[0148] The present invention further provides a method for producing a polyester composition, comprising the steps of mixing the polyester A, the polyester B and the aliphatic polyester, and then extrusion pelletizing the resulting mixture to obtain a polyester composition.
[0149] In the present invention, the method may further comprise carrying out a step of mixing the polyester A, the polyester B, the aliphatic polyester and the nucleating agent in the presence of the nucleating agent and optionally other additives, wherein the other additives may be erucylamide and / or white oil.
[0150] According to the present invention, the mixing step can be carried out under stirring, and the stirring speed can be 6 to 60 rpm, and the stirring time can be 2 to 30 minutes.
[0151] According to the present invention, the extrusion and pelletizing step can be carried out according to a conventional extrusion and pelletizing method. For example, the extrusion and pelletizing step can be carried out in a twin-screw extruder, and the extrusion and pelletizing conditions are preferably a temperature of 160-220°C, a screw rotation speed of 10-70 rpm, and a torque of 2-80 N·m; more preferably, the twin-screw extruder includes six temperature zones, and the temperatures of the respective temperature zones from the feed inlet to the extrusion outlet are successively 160-190°C, 170-200°C, 180-210°C, 180-220°C, 180-220°C, and 170-210°C.
[0152] The present invention further provides the use of said polyester composition in a shape memory material.
[0153] The present invention obtains a polyester composition suitable for use as a shape memory material by copolymerizing and mixing polybutylene terephthalate (PBT). When the polyester composition is used as a shape memory material, the deformation fixation rate and shape recovery rate of the shape memory material are both 92% or more, close to 100%, and the maximum deformation rate is high, 400% or more. In addition, both the initial molding temperature and the starting temperature of the shape memory material can be adjusted, which is more favorable for applying the shape memory material in daily life.
[0154] [3D printing materials] The present invention relates to a polyester composition comprising the following components, based on the total weight of the various components: (1) Repeating unit A represented by formula (I-1) and repeating unit B represented by formula (II-1)
[0155] [ka]
[0156] (wherein m1 is an integer of 2 to 10, preferably an integer of 2 to 4, n1 is an integer of 2 to 8, preferably an integer of 2 to 4, m1 and n1 are the same or different from each other; a1 is an integer of 2 to 10, preferably an integer of 2 to 4, a1 and m1 are the same or different from each other) 51 to 98% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I') and repeating unit D represented by formula (IV')
[0157] [ka]
[0158] 1 to 48% by weight of polyester B, which is a copolymer comprising: (3) Repeating unit E represented by formula (I'') and repeating unit F represented by formula (IV'')
[0159] [ka]
[0160] (wherein m2 is an integer of 2 to 10, preferably an integer of 2 to 4, n2 is an integer of 2 to 8, preferably an integer of 2 to 4, m2 and n2 are the same or different from each other; a2 is an integer of 2 to 10, preferably an integer of 2 to 4, a2 and m2 are the same or different from each other) 1 to 48% by weight of polyester C, which is a copolymer containing Including, the content of the repeating unit A is 56 to 80 mol %, preferably 60 to 75 mol %, and the content of the repeating unit B is 20 to 44 mol %, preferably 25 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, preferably 100,000 to 500,000; the content of the repeating unit C is 81 to 99 mol %, preferably 85 to 95 mol %, and the content of the repeating unit D is 1 to 19 mol %, preferably 5 to 15 mol %, based on the total number of moles of the repeating unit C and the repeating unit D in the polyester B; and the weight average molecular weight of the polyester B is 50,000 to 900,000, preferably 100,000 to 500,000; the content of the repeating unit E is 0 to 55 mol %, preferably 15 to 50 mol %, and the content of the repeating unit F is 45 to 100 mol %, preferably 50 to 85 mol %, based on the total number of moles of the repeating unit E and the repeating unit F in the polyester C; and the weight average molecular weight of the polyester C is 50,000 to 900,000, preferably 100,000 to 500,000. A polyester composition is provided.
[0161] In the present invention, m1 and m2 may be the same or different, and n1 and n2 may be the same or different, but when m1 and m2 are the same and n1 and n2 are also the same, the content of the repeating unit D in the polyester B is different from the content of the repeating unit F in the polyester C.
[0162] Preferably, the polyester composition contains the polyester A in an amount of 70 to 94% by weight, the polyester B in an amount of 3 to 25% by weight, and the polyester C in an amount of 3 to 20% by weight.
[0163] In the present invention, the polyester A, the polyester B and the polyester C may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers and graft copolymers, preferably random copolymers and / or block copolymers. The source of the polyester A, the polyester B and the polyester C in the present invention is not particularly limited. The polyester A, the polyester B and the polyester C can be obtained by conventional means in the art. They can be commercially obtained or can be produced by the methods disclosed in Examples B13 to B21 of CN100429256C. Specifically, the method for producing the polyester A may include the following steps: In a preferred embodiment of the present invention, when m1 is 4, the method for producing polyester A comprises the following steps: (S1) reacting butanediol with monomer A' in the presence of a first catalyst in an inert atmosphere; (S2) reacting the reaction product obtained in step (S1) with succinic acid in the presence of a second catalyst; wherein A' is terephthalic acid and / or its ester, preferably at least one selected from the group consisting of terephthalic acid, dimethyl terephthalate and diethyl terephthalate; said first catalyst and said second catalyst are as described above and will not be further described herein.
[0164] In the present invention, in step (S1), the molar ratio of monomer A' to the first catalyst is 1:0.0001-0.02:0.0001-0.02, more preferably 1:0.001-0.003:0.001-0.003.
[0165] Preferably, the molar ratio of the amount of the first catalyst to the amount of the second catalyst is 1:0.5-1.5, preferably 1:0.8-1.2.
[0166] In the present invention, the types of various reactive monomers can be appropriately adjusted depending on the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio.
[0167] In the present invention, the reaction temperature in step (S1) is preferably 160 to 220°C, and in the present invention, the reaction temperature in step (S2) is preferably 180 to 240°C.
[0168] Preferably, the process for producing polyester B comprises the following steps: (1) reacting monomer A with monomer B in the presence of a first catalyst in an inert atmosphere; (2) reacting monomer C with monomer D in the presence of a first catalyst in an inert atmosphere; (3) reacting the reaction product from step (1) with the reaction product from step (2) in the presence of a second catalyst; wherein the monomer A is a C2-C8 diol (particularly a linear saturated diol); the monomer B is terephthalic acid and / or its ester, preferably at least one selected from the group consisting of terephthalic acid, dimethyl terephthalate, and diethyl terephthalate; the monomer C is a C2-C10 diol (particularly a linear saturated diol); the monomer D is a C4-C10 dibasic acid (particularly a linear saturated dibasic acid); the first catalyst is at least one selected from the group consisting of tetrabutyl titanate, titanium dioxide, diethoxytitanium, and zinc acetate, preferably tetrabutyl titanate; and the second catalyst is at least one selected from the group consisting of lanthanum acetylacetonate, lanthanum trichloride, triphenoxylanthanum, and lanthanum propionate, preferably lanthanum acetylacetonate.
[0169] In the present invention, in step (1), the molar ratio of the monomer B to the first catalyst is 1:0.0001-0.02:0.0001-0.02, more preferably 1:0.001-0.003:0.001-0.003.
[0170] In the present invention, in step (2), the molar ratio of the monomer D to the first catalyst is 1:0.0001-0.02:0.0001-0.02, more preferably 1:0.001-0.003:0.001-0.003.
[0171] Preferably, the molar ratio of the total amount of the first catalyst (the sum of the amount of the first catalyst in step (1) and the amount of the first catalyst in step (2)) to the amount of the second catalyst is 1:0.5-1.5, preferably 1:0.8-1.2.
[0172] In the present invention, the types of various reactive monomers can be appropriately adjusted depending on the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio.
[0173] In the present invention, in step (1), the reaction temperature is preferably 160 to 220°C, in the present invention, the reaction temperature is preferably 160 to 220°C, in the present invention, the reaction temperature is preferably 160 to 220°C, and in the present invention, the reaction temperature is preferably 180 to 240°C in step (3).
[0174] According to the present invention, the polyester C can also be produced according to the method for producing the polyester B. Here, in order to obtain the polyester C, the types of various reactive monomers can be appropriately adjusted according to the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio.
[0175] According to the present invention, the polyester composition may further comprise an auxiliary filler; preferably, the content of the auxiliary filler is 0.1-50% by weight, preferably 1-25% by weight, based on the total weight of the polyester composition.
[0176] According to the present invention, the auxiliary filler has the functions of accelerating the solidification of the melt of the composition, adjusting the mechanical strength of the composition, improving the flame retardancy and oxidation resistance of the composition, and adjusting the color and gloss of the composition, and may be one that is conventionally selected in the art. For example, the auxiliary filler is at least one selected from the group consisting of calcium carbonate, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylates, metal phosphates, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low-density polyethylene, polyphosphate esters or salts, phosphites, hindered phenols, hindered amines, dibenzyl sorbitol and its derivatives, highly branched polyamides, ethylene-methacrylic acid ionomers, ethylene bisstearamide, silicone powders, and pentaerythritol stearate, and is preferably at least one selected from the group consisting of calcium carbonate, carbon black, titanium dioxide, tris(2,3-dibromopropyl)phosphate, low-density polyethylene, highly branched polyamides, ethylene bisstearamide, and erucylamide.
[0177] The present invention further provides a method for producing the above-mentioned polyester composition, comprising the steps of mixing said polyester A, said polyester B and said polyester C, and then extruding and pelletizing the resulting mixture.
[0178] The inventors unexpectedly found during the research that, in the present invention, the polyester A, the polyester B and the polyester C have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0179] According to the present invention, the mixing step can be carried out under stirring. The stirring conditions in the present invention are not particularly limited as long as the starting materials can be mixed uniformly. Preferably, the stirring speed is 20 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0180] According to the present invention, the extrusion and pelletizing step can be carried out according to conventional extrusion and pelletizing methods. For example, the extrusion and pelletizing step can be carried out in a screw extruder. Preferably, the temperature of the extrusion and pelletizing step is 90-260°C, preferably 110-180°C.
[0181] The present invention also provides a 3D printing wire comprising the above-mentioned polyester composition, i.e., the 3D printing wire is manufactured from the above-mentioned polyester composition.
[0182] According to the present invention, the diameter of the 3D printing wire may be 0.1-10 mm, preferably 1-4 mm.
[0183] The present invention also provides a method for producing a 3D printed wire, comprising the steps of continuously extruding and cooling a polyester composition to obtain a 3D printed wire, wherein the polyester composition is the polyester composition described above.
[0184] According to the present invention, the extrusion step can be carried out using conventional extrusion methods. For example, the extrusion step can be carried out in a screw extruder. Preferably, the extrusion step is carried out in an extruder with a round hole die to obtain a 3D printing wire, more preferably, the diameter of the obtained 3D printing wire is 0.1-10 mm, preferably 1-4 mm.
[0185] In the method for producing a 3D print wire of the present invention, the extrusion temperature is 90 to 260°C. Preferably, the cooling temperature is 0 to 60°C.
[0186] In the present invention, a polyester composition is obtained by blending specific polyester A, polyester B and polyester C in a specific ratio (51-98% by weight of polyester A, 1-48% by weight of polyester B, and 1-48% by weight of polyester C), and the 3D printing wire made from the polyester composition has a relatively high gloss and can be printed at a relatively low temperature (105-165°C). At the same time, the 3D printing wire can be used as a flexible wire (Shore D hardness of 35-50), is degradable, has the advantages of being environmentally friendly, and has the prospect of excellent application.
[0187] [Heat shrinkable pipe] The present invention relates to a polyester composition comprising the following components, based on the total weight of the various components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0188] [ka]
[0189] (wherein m1 is an integer of 2 to 4; n1 is an integer of 2 to 4, preferably 2; m1 and n1 are the same or different). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0190] [ka]
[0191] (wherein m2 is an integer from 2 to 4; n2 is an integer from 2 to 4, preferably 2; m2 and n2 are the same or different). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 51 to 70 mol %, and preferably 55 to 68 mol %, and the content of the repeating unit B is 30 to 49 mol %, and preferably 32 to 45 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, and preferably 100,000 to 500,000; the content of the repeating unit C is 1 to 50 mol %, preferably 20 to 45 mol %, and the content of the repeating unit B is 50 to 99 mol %, preferably 55 to 80 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; and the weight average molecular weight of the polyester B is 50,000 to 900,000, preferably 100,000 to 500,000. A polyester composition is provided.
[0192] In the present invention, m1 and m2 may be the same or different, and n1 and n2 may be the same or different, but when m1 and m2 are the same and n1 and n2 are also the same, the content of the repeating unit B in the polyester A is different from the content of the repeating unit B in the polyester B.
[0193] Preferably, the polyester composition contains the polyester A in an amount of 80 to 95% by weight and the polyester B in an amount of 5 to 20% by weight.
[0194] In the present invention, the composition of the polymer is determined by the amount of the starting materials fed.
[0195] In the present invention, the polyester A and the polyester B may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers and graft copolymers, preferably random copolymers and / or block copolymers. The source of the polyester A and the polyester B in the present invention is not particularly limited. The polyester A and the polyester B can be obtained by conventional methods in the art. They can be commercially obtained or can be produced by the methods disclosed in Examples B13 to B21 of CN100429256C. Specifically, the method for producing the polyester A may include the following steps: (1) reacting monomer A with monomer B in the presence of a first catalyst in an inert atmosphere; (2) reacting monomer C with monomer D in the presence of a first catalyst in an inert atmosphere; (3) reacting the reaction product from step (1) with the reaction product from step (2) in the presence of a second catalyst; wherein the monomer A is butanediol; the monomer B is terephthalic acid and / or its ester, preferably at least one selected from the group consisting of terephthalic acid, dimethyl terephthalate and diethyl terephthalate; the monomer C is a C2-C4 diol (particularly a linear saturated diol); the monomer D is a C4-C6 dibasic acid (particularly a linear saturated dibasic acid); the first catalyst is at least one selected from the group consisting of tetrabutyl titanate, titanium dioxide, diethoxytitanium and zinc acetate, preferably tetrabutyl titanate; and the second catalyst is at least one selected from the group consisting of lanthanum acetylacetonate, lanthanum trichloride, triphenoxylanthanum and lanthanum propionate, preferably lanthanum acetylacetonate.
[0196] In the present invention, in step (1), the molar ratio of the monomer B to the first catalyst is 1:0.0001-0.02:0.0001-0.02, more preferably 1:0.001-0.003:0.001-0.003.
[0197] In the present invention, in step (2), the molar ratio of the monomer D to the first catalyst is 1:0.0001-0.02:0.0001-0.02, more preferably 1:0.001-0.003:0.001-0.003.
[0198] Preferably, the molar ratio of the total amount of the first catalyst (the sum of the amount of the first catalyst in step (1) and the amount of the first catalyst in step (2)) to the amount of the second catalyst is 1:0.5-1.5, preferably 1:0.8-1.2.
[0199] In the present invention, the types of various reactive monomers can be appropriately adjusted depending on the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio.
[0200] In the present invention, in step (1), the reaction temperature is preferably 160 to 220°C, in the present invention, the reaction temperature is preferably 160 to 220°C, in the present invention, the reaction temperature is preferably 160 to 220°C, and in the present invention, the reaction temperature is preferably 180 to 240°C in step (3).
[0201] In a preferred embodiment of the present invention, when m1 is 4, the method for producing polyester A comprises the following steps: (S1) reacting butanediol with monomer A' in the presence of a first catalyst in an inert atmosphere; (S2) reacting the reaction product obtained in step (S1) with monomer B' in the presence of a second catalyst; Here, A' is terephthalic acid and / or its ester, preferably at least one selected from the group consisting of terephthalic acid, dimethyl terephthalate and diethyl terephthalate; the monomer B' is a C4-C6 dibasic acid (particularly a linear saturated dibasic acid); the first catalyst and the second catalyst are as described above and will not be further described in this specification.
[0202] In the present invention, in step (S1), the molar ratio of the monomer A' to the first catalyst is 1:0.0001-0.02:0.0001-0.02, more preferably 1:0.001-0.003:0.001-0.003.
[0203] Preferably, the molar ratio of the amount of the first catalyst to the amount of the second catalyst is 1:0.5-1.5, preferably 1:0.8-1.2.
[0204] In the present invention, the types of various reactive monomers can be appropriately adjusted depending on the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio.
[0205] In the present invention, the reaction temperature in step (S1) is preferably 160 to 220°C, and in the present invention, the reaction temperature in step (S2) is preferably 180 to 240°C.
[0206] According to the present invention, the polyester B can be produced according to the above-mentioned method for producing the polyester A. Here, in order to obtain the polyester B, the types of various reactive monomers can be appropriately adjusted according to the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeating unit in the product can be controlled by adjusting the supply amount and supply ratio.
[0207] According to the present invention, the polyester composition may further comprise an auxiliary filler; preferably, the content of the auxiliary filler is 0.1 to 60% by weight, more preferably 1 to 20% by weight, based on the total weight of the polyester composition.
[0208] According to the present invention, the auxiliary filler has the function of adjusting the mechanical strength of the composition, the function of improving the flame retardancy and oxidation resistance of the composition, the function of adjusting the color and gloss of the composition, etc., and may be one conventionally selected in the art. For example, the auxiliary filler may be at least one selected from the group consisting of calcium carbonate, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylates, metal phosphates, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low density polyethylene, polyphosphates or polyphosphate esters, phosphites, hindered amines, hindered phenols, dibenzyl sorbitol and its derivatives, highly branched polyamides, and ethylene-methacrylic acid ionomers; preferably at least one selected from the group consisting of carbon black, hindered phenols, calcium carbonate, erucylamide, titanium dioxide, polyphosphate esters, low density polyethylene, and highly branched polyamides; more preferably at least two selected from the group consisting of carbon black, hindered phenols, calcium carbonate, erucylamide, titanium dioxide, tris(2,3-dibromopropyl)phosphate (TDBPP), low density polyethylene, and highly branched polyamides.
[0209] The present invention further provides a method for producing the above-mentioned polyester composition, comprising the steps of mixing the above-mentioned polyester A and polyester B, and then extruding and pelletizing the resulting mixture.
[0210] The inventors unexpectedly found during the research that, in the present invention, the polyester A and the polyester B have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0211] According to the present invention, the mixing step is as described above. Preferably, the stirring speed is 20 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0212] According to the present invention, the extrusion and pelletizing step is as described above. Preferably, the temperature in the extrusion and pelletizing step is 160 to 220° C., the screw rotation speed of the screw extruder is 10 to 70 rpm, and the screw torque is 2 to 80 N·m.
[0213] The present invention also provides a heat-shrinkable sleeve comprising the above-mentioned polyester composition and / or the polyester composition obtained by the above-mentioned manufacturing method, i.e., said heat-shrinkable sleeve is manufactured from the above-mentioned polyester composition and / or the polyester composition obtained by the above-mentioned manufacturing process.
[0214] In the present invention, the heat-shrinkable sleeve may have a thickness of 0.3 to 10 mm, a shrinkage ratio of 5:1 to 4.5, good insulation properties, and a breaking strength of 25 kV / mm or more.
[0215] The present invention also provides a method for producing said heat shrinkable sleeve, comprising the steps of sequentially extruding, stretching, cooling and forming said polyester composition to obtain a heat shrinkable sleeve.
[0216] In the method for producing the heat-shrinkable sleeve of the present invention, the extrusion step is not particularly limited and can be carried out with a conventional screw extruder to obtain a pipe. Preferably, the extrusion step is carried out with a screw extruder equipped with a ring-shaped die. More preferably, the extrusion temperature is 90 to 240°C, and even more preferably 120 to 180°C.
[0217] In the method for producing the heat-shrinkable sleeve of the present invention, the cooling temperature may be 0 to 60°C, and preferably 20 to 40°C.
[0218] Preferably, the method further comprises the steps of successively heating, expanding the diameter, secondary cooling and forming the cooled pipe. Preferably, the heating temperature is 65-120°C, more preferably 70-90°C.
[0219] In the present invention, the expansion rate of the diameter is preferably 1.5 to 5 times, and more preferably 3 to 5 times, the original size (that is, before the diameter expansion).
[0220] In the present invention, the secondary cooling temperature may be 0 to 60°C, preferably 20 to 40°C.
[0221] [Functional layer (sports protector)] The present invention comprises the following components, based on the total weight of the various components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0222] [ka]
[0223] (wherein m1 is an integer of 2 to 4; n1 is an integer of 2 to 4, preferably 4; m1 and n1 are the same or different). 50 to 98% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0224] [ka]
[0225] (wherein m2 is an integer from 2 to 4; n2 is an integer from 2 to 4, preferably 2; m2 and n2 are the same or different). 1 to 49% by weight of polyester B, which is a copolymer comprising: (3) 1 to 49% by weight of fiber filler Including, the content of the repeating unit A is 55 to 79 mol %, preferably 60 to 77 mol %, and the content of the repeating unit B is 21 to 45 mol %, preferably 23 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, preferably 100,000 to 500,000; the content of the repeating unit C is 80 to 100 mol %, preferably 85 to 95 mol %, and the content of the repeating unit B is 0 to 20 mol %, preferably 5 to 15 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; the weight average molecular weight of the polyester B is 50,000 to 900,000, preferably 100,000 to 500,000; and the content of the repeating unit B in the polyester A is greater than the content of the repeating unit B in the polyester B. A polyester composition is provided.
[0226] In the present invention, m1 and m2 may be the same or different, and n1 and n2 may be the same or different, but when m1 and m2 are the same and n1 and n2 are also the same, the content of the repeating unit B in the polyester A is different from the content of the repeating unit B in the polyester B.
[0227] Preferably, the content of the repeating unit B in the polyester A is greater than the content of the repeating unit B in the polyester B.
[0228] Preferably, the polyester composition contains 60 to 90% by weight of the polyester A, 5 to 30% by weight of the polyester B, and 5 to 30% by weight of the fibrous filler.
[0229] In the present invention, the polyester A and the polyester B may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers, and graft copolymers, preferably random copolymers and / or block copolymers. The supply sources of the polyester A and the polyester B in the present invention are not particularly limited, and the supply sources and production methods are as described above.
[0230] The fiber filler may be one or more selected from the group consisting of carbon fiber, glass fiber, basalt fiber, aramid fiber, and polyethylene terephthalate fiber, and preferably one or more selected from the group consisting of glass fiber, carbon fiber, and basalt fiber. Preferably, the length of the fiber filler is 0.1 to 10 mm, preferably 0.5 to 2 mm.
[0231] According to the present invention, the polyester composition may further comprise an auxiliary filler; preferably, the content of the auxiliary filler is 0.1 to 25% by weight, more preferably 1 to 20% by weight, based on the total weight of the polyester composition.
[0232] According to the present invention, the auxiliary filler has a function of promoting solidification of the composition melt, a function of adjusting the mechanical strength of the composition, a function of adjusting the color and gloss of the composition, etc., and may be one that is conventionally selected in the art. For example, the auxiliary filler may be one or more selected from the group consisting of inorganic carbonate fillers, inorganic silicate fillers, inorganic sulfate fillers, inorganic hollow microspheres, and metal powders, preferably one or more selected from the group consisting of inorganic carbonate fillers, inorganic silicate fillers, inorganic sulfate fillers, and metal powders, more preferably at least one selected from the group consisting of anhydrous calcium sulfate, calcium carbonate, and copper powder.
[0233] The present invention further provides a method for producing the above-mentioned polyester composition, comprising the steps of mixing said polyester A, said polyester B and said fibrous filler, and then extruding and pelletizing the resulting mixture.
[0234] The inventors unexpectedly found during the research that, in the present invention, the polyester A, the polyester B and the fibrous filler have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0235] According to the present invention, the mixing step is as described above. Preferably, the stirring speed is 20 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0236] According to the present invention, the extrusion and pelletizing step is as described above. Preferably, the temperature of the extrusion and pelletizing step is 120-240°C, preferably 150-200°C.
[0237] The present invention further provides a functional layer comprising the above-mentioned polyester composition, i.e. said functional layer is produced from the above-mentioned polyester composition.
[0238] In the present invention, the functional layer has low-temperature plasticity and shape memory properties. Specifically, under the condition of T1 (80 to 100°C), the Shore D hardness value of the functional layer is 0 to 35, and under the condition of T2 (-20 to 50°C), the Shore D hardness value of the functional layer is 40 to 80. That is, under the condition of T1 (80 to 100°C), the functional layer can be softened, and at this time, it can be molded into a desired shape by applying an external force. After the molding is completed, the temperature is lowered to the condition of T2 (-20 to 50°C), the hardness of the functional layer is increased, and the shape is maintained.
[0239] The present invention further provides a method for producing a functional layer, comprising the step of molding the above-mentioned polyester composition.
[0240] In the present invention, functional layers of any shape and size can be produced by molding according to various applications.
[0241] According to the present invention, the molding step can be extrusion molding or injection molding, preferably injection molding. Preferably, the temperature of the injection molding is 140 to 270°C, preferably 170 to 185°C.
[0242] The present invention further provides the application of the above-mentioned polyester composition and the above-mentioned functional layer in a sports protector; preferably, the sports protector is one or more selected from the group consisting of dental protectors, limb joint protectors, large area protectors for body and head protectors.
[0243] In the present invention, the term "dental protector" refers to a protector that protects teeth during movement. The dental protector may include the functional layer, and may preferably consist of the functional layer.
[0244] In the present invention, the dental protector has low-temperature plasticity and shape memory properties. Specifically, the dental protector has a Shore D hardness of 0 to 35 under the condition of T1 (80 to 100°C), and a Shore D hardness of 40 to 80 under the condition of T2 (-20 to 50°C).
[0245] The present invention further provides a method for producing a dental protector, which includes the steps of successively softening, shaping, and cooling the functional layer provided by the present invention. Specifically, the method includes the steps of softening the functional layer under a condition of T1 (80 to 100°C), shaping the functional layer by applying an external force (such as teeth occlusion) to obtain a desired shape (such as a tooth shape), and lowering the temperature to a condition of T2 (-20 to 50°C) after the shaping is completed, thereby increasing the hardness of the dental protector and maintaining the shape.
[0246] In the present invention, the term "limb joint protector" refers to a protector that protects a limb joint (e.g., knee joint, elbow joint, shoulder joint, wrist joint, etc.) during exercise. The limb joint protector includes the functional layer.
[0247] In a preferred case, the limb joint protector includes an optional outer layer, an intermediate layer, and an optional inner layer. Here, the intermediate layer is the functional layer described above; the outer layer may be a hard material (such as at least one selected from the group consisting of metal materials, hard plastics (excluding the polyester composition of the present invention), ceramics, and wood); and the inner layer may be a soft material (such as at least one selected from the group consisting of sponge, foam, soft silica gel, and soft rubber). Furthermore, the outer layer, the intermediate layer, and the inner layer are bonded; preferably, they are bonded by bonding (such as using an adhesive), threading, or buckling. More preferably, the outer layer, the intermediate layer, and the inner layer are all removable.
[0248] The present invention further provides a method for producing a limb joint protector, which includes the steps of softening, molding and cooling the functional layer provided by the present invention in succession to obtain an intermediate layer of the limb joint protector. Specifically, the manufacturing steps include the steps of softening the functional layer under the condition of T1 (80 to 100°C) and molding the functional layer by applying an external force (e.g., placing it on the surface of the joint and applying pressure) to obtain a desired shape (e.g., a shape that fits the joint); and the step of lowering the temperature to the condition of T2 (-20 to 50°C) after the completion of molding, thereby increasing the hardness of the functional layer and maintaining the shape, thereby obtaining the limb joint protector. Optionally, the manufacturing method for the limb joint protector further includes the steps of bonding the outer layer and / or the inner layer to the outer surface and / or the inner surface of the intermediate layer, respectively. Here, the outer layer and the inner layer are as described above, and will not be described again here.
[0249] In the present invention, the term "large-area protector for the body" refers to a protector that protects a major part of the body during exercise (e.g., chest, back, waist, abdomen, front of the thigh, front of the lower leg, etc.). The large-area protector for the body includes the functional layer.
[0250] In a preferred case, the large-area protector for the body includes an outer layer, an intermediate layer, and an optional inner layer. Here, the intermediate layer is the functional layer described above; the outer layer may be a hard material (e.g., at least one selected from the group consisting of metal materials, hard plastics (excluding the polyester composition of the present invention), ceramics, and wood); the inner layer may be a soft material (e.g., at least one selected from the group consisting of sponge, foam, soft silica gel, and soft rubber). Furthermore, the outer layer, the intermediate layer, and the inner layer are bonded; preferably, the inner layer and the intermediate layer are bonded by bonding, and the intermediate layer and the outer layer are bonded by fixing using buckling, attachment, or bandage. More preferably, the outer layer, the intermediate layer, and the inner layer are all removable.
[0251] The present invention further provides a method for manufacturing a large-area protector for the body, which includes the steps of successively softening, shaping, and cooling the functional layer provided by the present invention to obtain an intermediate layer of the large-area protector for the body. Specifically, the manufacturing method includes the steps of softening the functional layer under conditions of T1 (80 to 100°C) and shaping the functional layer by applying an external force (e.g., placing it on the surface of the body part and applying pressure) to obtain a desired shape (e.g., a shape that fits the body part); after completion of shaping, lowering the temperature to conditions of T2 (-20 to 50°C), thereby increasing the hardness of the functional layer and maintaining the shape, thereby obtaining an intermediate layer of the large-area protector for the body; and further includes the step of bonding an outer layer to the outer surface of the intermediate layer. Optionally, the manufacturing process of the large-area protector for the body further includes the step of bonding an inner layer to the inner surface of the intermediate layer. Here, the outer layer and the inner layer are as described above and will not be described again here.
[0252] In the present invention, the term "head protector" refers to a protector that protects the head during exercise. Preferably, the head protector is a helmet.
[0253] In the present invention, the head protector includes the functional layer.
[0254] Preferably, the head protector includes an optional outer layer, an intermediate layer, and an optional inner layer. Here, the intermediate layer is the functional layer described above; the outer layer may be a hard material (e.g., at least one selected from the group consisting of metal materials, hard plastics (excluding the polyester composition of the present invention), ceramics, and wood); the inner layer may be a soft material (e.g., at least one selected from the group consisting of sponge, foam, soft silica gel, and soft rubber). Furthermore, the outer layer, the intermediate layer, and the inner layer are bonded; preferably, the inner layer and the intermediate layer are bonded by bonding, and the intermediate layer and the outer layer are bonded by fixing using a buckling, attachment, or bandage. More preferably, the outer layer, the intermediate layer, and the inner layer are all removable.
[0255] The present invention further provides a method for producing a head protector, which includes the steps of successively softening, forming, and cooling the functional layer provided by the present invention to obtain an intermediate layer of the head protector. Specifically, the method includes the steps of softening the functional layer under conditions of T1 (80 to 100°C) and forming the functional layer by applying an external force (e.g., placing it on the surface of the head and pressing it) to obtain a desired shape (e.g., a shape that fits the head); and the step of lowering the temperature to conditions of T2 (-20 to 50°C) after the completion of forming, thereby increasing the hardness of the functional layer and maintaining the shape, thereby obtaining the intermediate layer of the head protector. Optionally, the method for producing a head protector further includes the step of bonding the inner layer and / or the outer layer to the inner surface and / or the outer surface of the intermediate layer, respectively. Here, the outer layer and the inner layer are as described above, and will not be described again here.
[0256] In the present invention, a polyester composition can be obtained by combining polyester A and polyester B having a specific structure, and a fiber filler in a specific ratio (50 to 98% by weight of the polyester A, 1 to 49% by weight of the polyester B, and 1 to 49% by weight of the fiber filler). The polyester composition can be sufficiently softened (hardness is reduced) under high temperature conditions (e.g., 80 to 100°C), and the softened polyester composition can be made into a functional layer of any shape through molding according to the target part. In this way, the polyester composition can be well adapted to the target part. Then, the hardness can be significantly increased at a relatively low temperature (e.g., -20 to 50°C). This allows the desired molding to be performed. Furthermore, the polyester composition provided by the present invention further has good shape memory properties, and its deformation fixation rate is 90% or more, its deformation recovery rate is 90% or more, and its maximum deformation rate is as high as 280% or more. In addition, the above-mentioned softening and molding process of the polyester composition provided by the present invention is reversible. When the sports protector is manufactured from the polyester composition, after the sports protector is worn or slightly damaged, it can be softened again by raising the temperature and reformed at a low temperature, so that the original appearance of the protector can be restored. Therefore, the sports protector manufactured by the functional layer provided by the present invention is expected to have excellent applicability.
[0257] The polyester composition of the present invention has good low-temperature plasticity and shape memory properties.Therefore, when the polyester composition provided by the present invention is used in sports protectors, it can be molded according to different application parts so that the protectors can better fit the body, so that the protectors are more comfortable and convenient to manufacture.
[0258] [Medical limb immobilizer] The present invention relates to a polyester composition comprising, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0259] [ka]
[0260] (wherein m1 is an integer of 2 to 4; n1 is an integer of 2 to 4, preferably 2; m1 and n1 are the same or different). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0261] [ka]
[0262] (wherein m2 is an integer from 2 to 4; n2 is an integer from 2 to 4, preferably 2; m2 and n2 are the same or different). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 60 to 80 mol %, preferably 62 to 78 mol %, and the content of the repeating unit B is 20 to 40 mol %, preferably 22 to 38 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, preferably 100,000 to 500,000; the content of the repeating unit C is 20 to 59 mol %, preferably 30 to 55 mol %, and the content of the repeating unit B is 41 to 80 mol %, preferably 45 to 70 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; and the weight average molecular weight of the polyester B is 50,000 to 900,000, preferably 100,000 to 500,000. The present invention provides a polyester composition comprising:
[0263] In the present invention, m1 and m2 may be the same or different, and n1 and n2 may be the same or different, but when m1 and m2 are the same and n1 and n2 are also the same, the content of the repeating unit B in the polyester A is different from the content of the repeating unit B in the polyester B.
[0264] Preferably, the polyester composition contains 70 to 90% by weight of the polyester A and 10 to 30% by weight of the polyester B; more preferably, the polyester composition contains 70 to 80% by weight of the polyester A and 20 to 30% by weight of the polyester B.
[0265] In the present invention, the polyester A and the polyester B may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers, and graft copolymers, preferably random copolymers and / or block copolymers. The source of the polyester A and the polyester B in the present invention is not particularly limited, and the source and the production process are as described above.
[0266] According to the present invention, the polyester composition may further comprise an auxiliary filler; preferably, the content of the auxiliary filler is 0.1-60% by weight, more preferably 1-20% by weight, based on the total weight of the polyester composition.
[0267] According to the present invention, the auxiliary filler has the function of adjusting the solidification of the composition, adjusting the mechanical strength of the composition, improving the flame retardancy and oxidation resistance of the composition, adjusting the color and gloss of the composition, etc., and may be one conventionally selected in the art. For example, the auxiliary filler may be at least one selected from the group consisting of calcium carbonate, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylates, metal phosphates, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low density polyethylene, polyphosphates or polyphosphate esters, phosphites, hindered phenols, hindered amines, dibenzyl sorbitol and its derivatives, highly branched polyamides, and ethylene-methacrylic acid ionomers; preferably at least one selected from the group consisting of calcium carbonate, carbon black, erucylamide, titanium dioxide, polyphosphates or polyphosphate esters, low density polyethylene, and highly branched polyamides; more preferably at least one selected from the group consisting of iron oxide, titanium dioxide, calcium carbonate, carbon black, erucylamide, tris(2,3-dibromopropyl)phosphate (TDBPP), low density polyethylene, and highly branched polyamides.
[0268] The present invention further provides a method for producing the above-mentioned polyester composition, characterized in that it comprises a step of mixing the above-mentioned polyester A with polyester B, followed by extruding and pelletizing the resulting mixture.
[0269] The inventors unexpectedly found during the research that, in the present invention, the polyester A and the polyester B have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0270] According to the present invention, the mixing step is as described above. Preferably, the stirring speed is 20 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0271] According to the present invention, the extrusion and pelletizing step is as described above. Preferably, the temperature in the extrusion and pelletizing step is 110-260°C, preferably 160-220°C.
[0272] The present invention further provides a medical limb fixation device comprising the above-mentioned polyester composition, i.e., the medical limb fixation device is produced from the above-mentioned polyester composition.
[0273] According to the present invention, the medical limb fixation device may have a thickness of 0.2 to 10 mm, preferably 1 to 3 mm.
[0274] According to the present invention, the medical limb fixation device may or may not have a porous structure, and preferably has a porous structure.
[0275] In the present invention, the pore structure is distributed throughout the medical limb fixation device to improve the gas permeability of the medical limb fixation device. Preferably, the pore size of the pore structure is 1-10 mm, preferably 1-5 mm.
[0276] In the present invention, the medical limb fixation device can be used to fix any limb part, for example, it can be used on various body parts such as fingers, four limbs, neck, and back.
[0277] The present invention further provides a method for producing a medical limb fixation device, comprising the steps of continuously extruding the polyester composition, molding, and optionally punching, to obtain a medical limb fixation device, wherein the polyester composition is the polyester composition described above.
[0278] In the method for producing a medical limb fixation device of the present invention, the extrusion step is preferably melt extrusion, and more preferably the extrusion temperature is 90 to 230°C, preferably 110 to 170°C.
[0279] In the method for producing a medical limb fixation device of the present invention, the molding step may be injection molding and / or compression molding. Preferably, the molding step is a step in which the thickness of the medical limb fixation device is 0.2 to 10 mm, preferably 1 to 3 mm.
[0280] In the method for producing a medical limb fixation device of the present invention, the hole punching step may be performed using a puncher, and the diameter of the puncher used is preferably 1 to 10 mm, and more preferably 1 to 5 mm.
[0281] In the method for manufacturing a medical limb fixation device of the present invention, the manufacturing method may further include a step of cutting the molded material to obtain a medical limb fixation device of an appropriate size and shape.
[0282] In the present invention, a polyester composition whose hardness can be changed by temperature and time is obtained by mixing specific copolymers (polyester A and polyester B) in a specific ratio (the content of polyester A is 51 to 99% by weight, and the content of polyester B is 1 to 49% by weight). The medical limb fixation device produced by using the polyester composition provided by the present invention can be sufficiently softened under high temperature conditions (for example, in hot water, especially in boiling water), and the softened material is easy to cut when cut into an appropriate size and shape, and can harden and adhere by itself when wrapped around the limb part that needs to be fixed. This allows the medical limb fixation device to be well molded and achieve the purpose of fixation. Furthermore, the above-mentioned manufacturing method is reversible and can be reshaped according to the limb part, and further, the medical limb fixation device can be easily removed and cleaned, and has good decomposability. The manufacturing process adopts a thermoplastic treatment (without using a crosslinking agent), so that the remaining material can be recycled and reused.
[0283] In addition, the medical limb fixation device of the present invention has the following further advantages: it does not require special packaging such as waterproof packaging during storage and transportation, and even after the package is opened, no deterioration occurs for at least two years; its weight is close to that of a polymer bandage and is only about 1 / 5 of the weight of a plaster bandage; it has excellent X-ray transparency; and it is completely water-repellent as it does not react with water, so there is no need to worry about humidity during storage before use.
[0284] The hardness of the polyester composition provided by the present invention changes with time and temperature. Specifically, the hardness is low at high temperatures and increases significantly in a short time after cooling, thus exhibiting good plasticity and fixability. Therefore, the polyester composition provided by the present invention is particularly suitable for the manufacture of medical limb braces.
[0285] [Heat shrinkable film] The present invention comprises the following components, based on the total weight of the various components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0286] [ka]
[0287] (wherein m1 is an integer of 2 to 4; n1 is an integer of 2 to 4, preferably 2; m1 and n1 are the same or different). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0288] [ka]
[0289] (wherein m2 is an integer of 2 to 4; n2 is an integer of 2 to 4, preferably 2; m2 and n2 are the same or different). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 60 to 80 mol %, and preferably 62 to 72 mol %, and the content of the repeating unit B is 20 to 40 mol %, and preferably 28 to 38 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, and preferably 100,000 to 500,000; the content of the repeating unit C is 81 to 99 mol %, preferably 85 to 97 mol %, and the content of the repeating unit B is 1 to 19 mol %, preferably 3 to 15 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; and the weight average molecular weight of the polyester B is 50,000 to 900,000, preferably 100,000 to 500,000. A polyester composition is provided.
[0290] In the present invention, m1 and m2 may be the same or different, and n1 and n2 may be the same or different, but when m1 and m2 are the same and n1 and n2 are also the same, the content of the repeating unit B in the polyester A is different from the content of the repeating unit B in the polyester B.
[0291] Preferably, the content of the repeating unit B in the polyester A is greater than the content of the repeating unit B in the polyester B.
[0292] Preferably, the polyester composition contains the polyester A in an amount of 60 to 90% by weight and the polyester B in an amount of 10 to 40% by weight.
[0293] In the present invention, the polyester A and the polyester B may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers, and graft copolymers, preferably random copolymers and / or block copolymers. The supply sources of the polyester A and the polyester B in the present invention are not particularly limited, and the supply sources and production methods are as described above.
[0294] According to the present invention, the polyester composition may further contain an auxiliary filler; preferably, the content of the auxiliary filler is 0.1 to 20% by weight, more preferably 10 to 20% by weight, based on the total weight of the polyester composition.
[0295] According to the present invention, the auxiliary filler has the functions of accelerating solidification of the composition melt, adjusting the mechanical strength of the composition, improving the flame retardancy and oxidation resistance of the composition, adjusting the color and gloss of the composition, etc., and may be one conventionally selected in the art. For example, the auxiliary filler may be at least one selected from the group consisting of calcium carbonate, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylates, metal phosphates, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low density polyethylene, polyphosphates or esters of polyphosphates, phosphites, hindered phenols, hindered amines, dibenzyl sorbitol and its derivatives, highly branched polyamides, and ethylene-methacrylic acid ionomers; preferably at least one selected from the group consisting of calcium carbonate, carbon black, erucylamide, titanium dioxide, polyphosphates, low density polyethylene, and highly branched polyamides; more preferably at least two selected from the group consisting of calcium carbonate, carbon black, erucylamide, titanium dioxide, tris(2,3-dibromopropyl)phosphate, low density polyethylene, and highly branched polyamides.
[0296] The present invention further provides a method for producing the above-mentioned polyester composition, comprising the steps of mixing the above-mentioned polyester A and polyester B, and then extruding and pelletizing the resulting mixture.
[0297] The inventors unexpectedly found during the research that, in the present invention, the polyester A and the polyester B have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0298] According to the present invention, the mixing step is as described above. Preferably, the stirring speed is 10 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0299] According to the present invention, the extrusion and pelletizing step is as described above. Preferably, the temperature in the extrusion and pelletizing step is 80-220°C, preferably 110-180°C.
[0300] The present invention further provides a heat shrinkable film comprising the above-mentioned polyester composition, i.e., the heat shrinkable film is produced from the above-mentioned polyester composition.
[0301] In the present invention, the thickness of the heat shrinkable film may be 5-1000 μm, and the heat shrinkage rate can be changed in a wide range by adjusting the composition and polyester structure. For example, the heat shrinkage rate of the heat shrinkable film is 10-80%, and the heat shrinkable film can meet different needs. Furthermore, the heat seal strength of the heat shrinkable film is 11-19 N / 15 mm, and the heat shrinkable film has good decomposability.
[0302] The present invention further provides a method for producing a heat-shrinkable film, comprising the steps of continuously forming the polyester composition into a film by casting, leaving and stretching, to obtain a heat-shrinkable film, wherein the polyester composition is the polyester composition described above.
[0303] According to the present invention, the method of forming a film by casting is not particularly limited, and can be performed, for example, by a casting machine. The temperature of the step of forming a film by casting is preferably 80 to 220°C, and more preferably 110 to 180°C.
[0304] In the present invention, the method of the leaving step is not particularly limited, and for example, the step can be left in a room temperature (25° C.) environment. The leaving time is preferably 30 minutes to 20 days, and more preferably 4 to 24 hours.
[0305] In the present invention, the stretching step may be uniaxial stretching or biaxial stretching. The stretching temperature is preferably 40 to 150°C, more preferably 60 to 120°C.
[0306] In the present invention, by blending a specific copolymer (polyester A and polyester B) in a specific ratio (the content of the polyester A is 51 to 99% by weight, and the content of the polyester B is 1 to 49% by weight), a heat shrinkable film having a heat shrinkage rate of 70% or more can be obtained, and a film having a heat shrinkage rate of 10% can be obtained, which shows that in the present invention, the heat shrinkage rate of the film can be changed in a wide range by adjusting the blending and polyester structure. Furthermore, the heat shrinkable film obtained by the present invention has a suitable heat seal strength (up to 11 to 19 N / 15 mm), the film has a flat surface, has good gloss, is decomposable, can be repeatedly processed thermoplastically, and can be recycled. Therefore, it is obvious that the heat shrinkable film has the advantage of being environmentally friendly, and has the prospect of industrial use.
[0307] [Nonwoven fabric] The present invention provides a polyester composition, which comprises, relative to the total weight of the various components, the following components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0308] [ka]
[0309] (wherein m1 is an integer of 2 to 4; n1 is an integer of 2 to 4, preferably 2; m1 and n1 are the same or different). 51 to 99% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0310] [ka]
[0311] (wherein m2 is an integer from 2 to 4; n2 is an integer from 2 to 4, preferably 2; m2 and n2 are the same or different). 1 to 49% by weight of polyester B, which is a copolymer containing Including, the content of the repeating unit A is 75 to 95 mol %, and preferably 81 to 95 mol %, and the content of the repeating unit B is 5 to 25 mol %, and preferably 5 to 19 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, and preferably 100,000 to 500,000; Based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B, the content of the repeating unit C is 20 to 74 mol %, and preferably 40 to 70 mol %, the content of the repeating unit B is 26 to 80 mol %, and preferably 30 to 60 mol %, and the weight average molecular weight of the polyester B is 50,000 to 900,000, and preferably 100,000 to 500,000.
[0312] In the present invention, m1 and m2 may be the same or different, and n1 and n2 may be the same or different, but when m1 and m2 are the same and n1 and n2 are also the same, the content of the repeating unit B in the polyester A is different from the content of the repeating unit B in the polyester B.
[0313] Preferably, the polyester composition contains the polyester A in an amount of 55 to 70% by weight and the polyester B in an amount of 30 to 45% by weight.
[0314] In the present invention, the polyester A and the polyester B may be at least one selected from the group consisting of random copolymers, alternating copolymers, block copolymers, and graft copolymers, preferably random copolymers and / or block copolymers. The supply sources of the polyester A and the polyester B in the present invention are not particularly limited, and the supply sources and the production methods are as described above.
[0315] According to the present invention, the polyester composition may further comprise an auxiliary filler; preferably, the content of the auxiliary filler is 0.1-25% by weight, more preferably 1-20% by weight, based on the total weight of the polyester composition.
[0316] According to the present invention, the auxiliary filler may be selected from the group consisting of calcium carbonate, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylate, metal phosphate, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low density polyethylene, polyphosphate or polyphosphate ester, phosphite ester, hindered phenol, hindered amine, dibenzyl sorbitol and its derivatives, hyperbranched polyamide and ethylene-methacrylic acid ionomer; preferably, hindered phenol, calcium carbonate, carbon black, erucylamide, titanium dioxide, tris(2,3-dibromopropyl)phosphate (TDBPP), low density polyethylene and hyperbranched polyamide.
[0317] The present invention further provides a method for producing the above-mentioned polyester composition, comprising the steps of mixing the above-mentioned polyester A and polyester B, and then extruding and pelletizing the resulting mixture.
[0318] The inventors unexpectedly found during the research that, in the present invention, the polyester A and the polyester B have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0319] According to the present invention, the mixing step is as described above. Preferably, the stirring speed is 20 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0320] According to the present invention, the extrusion and pelletizing step is as described above. Preferably, the temperature in the extrusion and pelletizing step is 140-220°C, preferably 160-200°C.
[0321] The present invention further provides a nonwoven fabric comprising the above-mentioned polyester composition, i.e., the nonwoven fabric is made from the above-mentioned polyester composition.
[0322] In the present invention, the filament diameter of the nonwoven fabric may be 5 to 100 μm, preferably 20 to 50 μm.
[0323] The present invention further provides a method for producing a nonwoven fabric, comprising producing a nonwoven fabric from the above-mentioned polyester composition by a spunbonding method. The machine used in the spunbonding method of the present invention is not particularly limited, and for example, a spunbonding machine conventionally used in the technical field can be used.
[0324] Preferably, the spunbonding method includes an extrusion step, a spinning step, a network forming step, and a reinforcing step. More preferably, the extrusion step includes three temperature zones. Here, the temperature of the first temperature zone is 140 to 250°C, preferably 160 to 210°C, the temperature of the second temperature zone is 150 to 260°C, preferably 165 to 220°C, and the temperature of the third temperature zone is 170 to 260°C, preferably 180 to 230°C.
[0325] In the present invention, the conditions for the spinning step are not particularly limited. For example, the spinning temperature is 150 to 240° C., preferably 170 to 220° C., and the spinning speed is 10 to 40 r / min, preferably 15 to 30 r / min.
[0326] In the present invention, the conditions for the network-forming step are not particularly limited, and for example, the network-forming speed can be 5 to 30 r / min, preferably 10 to 20 r / min.
[0327] In the present invention, the reinforcing step is preferably carried out by hot rolling, and the hot rolling temperature is 80 to 170°C, preferably 90 to 120°C.
[0328] The present invention further provides the use of the above-mentioned polyester composition and the above-mentioned nonwoven in a nonwoven article, preferably a disposable nonwoven article, more preferably a disposable medical nonwoven article.
[0329] Preferably, the disposable medical nonwoven article is at least one selected from the group consisting of disposable surgical gowns, disposable medical masks, disposable medical caps, disposable medical bed sheets, and disposable surgical drapes.
[0330] [Elastic fiber] The present invention comprises the following components based on the total weight of the various components: (1) Repeating unit A represented by formula (I') and repeating unit B represented by formula (II-1)
[0331] [ka]
[0332] (wherein m1 is an integer of 2 to 8, preferably an integer of 2 to 4; n1 is an integer of 2 to 6, preferably an integer of 2 to 4; m1 and n1 are the same or different). 30 to 98% by weight of polyester A, which is a copolymer comprising: (2) Repeating unit C represented by formula (I″) and repeating unit B represented by formula (II-1)
[0333] [ka]
[0334] (wherein, m2 is an integer of 2 to 8, preferably an integer of 2 to 4; n2 is an integer of 2 to 6, preferably an integer of 2 to 4; m2 and n2 are the same or different). 1 to 69% by weight of polyester B, which is a copolymer comprising: (3) Repeating unit D represented by formula (I''') and repeating unit B represented by formula (II-1)
[0335] [ka]
[0336] (wherein m3 is an integer of 2 to 8, preferably an integer of 2 to 4; n3 is an integer of 2 to 6, preferably an integer of 2 to 4; m2 and n3 are the same or different). 1 to 69% by weight of polyester C, which is a copolymer containing Including, the content of the repeating unit A is 51 to 80 mol %, preferably 60 to 75 mol %, and the content of the repeating unit B is 20 to 49 mol %, preferably 25 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; and the weight average molecular weight of the polyester A is 50,000 to 900,000, preferably 100,000 to 500,000; the content of the repeating unit C is 81 to 99 mol %, preferably 83 to 95 mol %, and the content of the repeating unit B is 1 to 19 mol %, preferably 5 to 17 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; and the weight average molecular weight of the polyester B is 50,000 to 900,000, preferably 100,000 to 500,000; the content of the repeating unit D is 0 to 49 mol %, preferably 15 to 45 mol %, and the content of the repeating unit B is 51 to 100 mol %, preferably 55 to 85 mol %, based on the total number of moles of the repeating unit D and the repeating unit B in the polyester C; and the weight average molecular weight of the polyester C is 50,000 to 900,000, preferably 100,000 to 500,000. A polyester composition is provided.
[0337] In the present invention, m1, m2, and m3 may be the same or different, and n1, n2, and n3 may be the same or different, provided that when m1, m2, and m3 are the same and n1, n2, and n3 are also the same, the contents of the repeating unit B in the polyester A, polyester B, and polyester C are different from each other.
[0338] Preferably, the polyester composition contains the polyester A in an amount of 60 to 93% by weight, the polyester B in an amount of 5 to 38% by weight, and the polyester C in an amount of 1 to 20% by weight.
[0339] In the present invention, the polyester A, the polyester B, and the polyester C may each be at least one selected from the group consisting of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer, preferably a random copolymer and / or a block copolymer. The supply sources of the polyester A, the polyester B, and the polyester C in the present invention are not particularly limited, and the supply sources and the production methods are as described above.
[0340] According to the present invention, the polyester composition may further comprise an auxiliary filler; preferably, the content of the auxiliary filler is 1 to 20% by weight, more preferably 2 to 10% by weight, based on the total weight of the polyester composition.
[0341] In the present invention, the auxiliary filler may have the function of accelerating the solidification of the melt of the composition, the function of adjusting the mechanical strength of the composition, the function of improving the flame retardancy and oxidation resistance of the composition, the function of adjusting the color and gloss of the composition, etc., and may be one that is conventionally selected in the art. For example, the auxiliary filler is at least one selected from the group consisting of calcium carbonate, carbon black, talc, erucylamide, titanium dioxide, low-density polyethylene, polyphosphates or polyphosphate esters, phosphites, hindered phenols, hindered amines, dibenzyl sorbitol and its derivatives, highly branched polyamides, and ethylene-methacrylic acid ionomers; preferably, at least one selected from the group consisting of calcium carbonate, carbon black, erucylamide, titanium dioxide, tris(2,3-dibromopropyl)phosphate (TDBPP), and low-density polyethylene.
[0342] The present invention further provides a method for producing the above-mentioned polyester composition, comprising the steps of mixing the above-mentioned polyester A, polyester B and polyester C, and then extruding and pelletizing the resulting mixture.
[0343] The inventors unexpectedly found during the research that, in the present invention, the polyester A, the polyester B and the polyester C have good compatibility, so that it is possible not to add a compatibilizer during mixing. The compatibilizer is a substance that is conventionally used in the art to improve the compatibility of mixed starting materials. The compatibilizer may be, for example, at least one selected from the group consisting of PE-g-ST, PP-g-ST, ABS-g-MAH, PE-g-MAH and PP-g-MAH.
[0344] According to the present invention, the mixing step is as described above. Preferably, the stirring speed is 10 to 150 r / min, and the stirring time is 5 to 15 minutes.
[0345] According to the present invention, the extrusion and pelletizing step is as described above. Preferably, the temperature in the extrusion and pelletizing step is 110-270°C, preferably 130-230°C.
[0346] The present invention further provides an elastic fiber comprising the above-mentioned polyester composition and / or the polyester composition obtained by the above-mentioned production method, i.e., the elastic fiber is produced from the above-mentioned polyester composition and / or the polyester composition obtained by the above-mentioned production method.
[0347] According to the present invention, the number of fibers of the elastic fibers may be 5 to 500 dtex. The breaking strength is 1 cN / dtex or more, preferably 3 to 19 cN / dtex; the elongation at break is 100% or more, preferably 130 to 620%; the stress relaxation rate is 12% or more, preferably 1 to 12%; and the permanent set rate is 12% or more, preferably 1 to 11%. In the present invention, the number of fibers can be detected using a conventional denier meter.
[0348] The present invention further provides a method for producing an elastic fiber, comprising the steps of sequentially filament-forming, cold-placing and drawing a polyester composition to obtain an elastic fiber, wherein the polyester composition is the polyester composition described above.
[0349] According to the present invention, the method of filament formation can be any conventional method selected in the art, preferably melt spinning. Preferably, the temperature of filament formation is between 120 and 270°C, preferably between 150 and 220°C.
[0350] According to the present invention, the conditions of low temperature placement include a temperature of 20-55° C., preferably 25-45° C., and a time of 2-120 minutes, preferably 15-60 minutes.
[0351] According to the present invention, the conditions for the stretching step include a temperature of 56-110° C., preferably 60-90° C., and a stretch ratio of 1.2-10 times, preferably 2-5 times.
[0352] In the present invention, a polyester composition is obtained by mixing specific polyester A, polyester B, and polyester C in a specific ratio (30-98% by weight of polyester A, 1-69% by weight of polyester B, and 1-69% by weight of polyester C). The breaking strength of the elastic fiber produced by using the polyester composition is 1 cN / dtex or more, and can be changed in a wide range by adjusting the composition and molecular structure, and the maximum breaking strength is close to 20 cN / dtex. Furthermore, the breaking elongation of the elastic fiber provided by the present invention is as high as 130% or more, and both the stress relaxation rate and the permanent set rate can be 12% or more. This means that the elastic fiber provided by the present invention has both elasticity and strength appropriately, and the properties can be adjusted in a wide range, and therefore it is expected to have excellent applicability.
[0353] In addition, the present invention specifically uses a method and conditions of high temperature filamentation-low temperature placement-high temperature drawing to produce elastic fibers, which can further improve the breaking strength of elastic fibers, extend the tailorable range of properties, and reduce the stress relaxation and permanent set rate of elastic fibers.
[0354] The measurement criteria for some parameters in the present invention are as follows: Fiber count: The fiber count was measured directly with a propeller micrometer, and the corresponding value was calculated according to the method of JIS L0104-2000.
[0355] Fiber breaking strength: GB / T 14337-2008 Fiber elongation at break: GB / T 14337-2008 Stress relaxation rate: GB / T 14337-2008 Permanent distortion rate: GB / T 14337-2008 Strength of plastic test specimens: GB / T 1040.2-2006 / ISO 527-2:1993 Elongation at break for plastic specimens: GB / T 1040.2-2006 / ISO 527-2:1993 Shore hardness: GB / T 2411-2008 / ISO 868:2003.
[0356] [Embodiment] The present invention will be described in detail below with reference to examples. It should be understood that the examples are merely used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0357] [Example] In the following examples and comparative examples, the weight average molecular weight of the polymers was measured by gel permeation chromatography (GPC) on a Waters-208 (Waters 2410 RI detector, 1.5 mL / min flow rate, 30° C.) instrument using tetrahydrofuran (THF) as the solvent and calibrated against polystyrene standards; The microstructures of the polyester A, the polyester B, the polyester C, the aliphatic polyester and the aromatic polyester were measured by an AVANCE DRX 400MHz NMR spectrometer from Bruker, Switzerland, using deuterated chloroform as a solvent; The composition of the polyester composition was determined by the supply of starting materials; The deformation memory properties of the polyester compositions were measured using an Instron 5965 tensile tester (with incubator) as follows: The initial length of the polyester composition sample at room temperature was "a". When the temperature of the incubator was raised to 80°C, it was sufficiently softened and stretched to a length "b" at a stretching speed of 50 mm / min. An external force was maintained so that the stretched length did not change. After the temperature was lowered and the sample was solidified, the external force was removed, at which point the length of the sample was "c". The temperature of the sample was raised again to 80°C, and the sample was sufficiently shrunk to a length "d"; Deformation fixation rate (%) = (cA) / (bA) × 100%; Shape recovery rate (%)=(cd) / (ca)×100%; Maximum deformation rate (%) = b max / a×100% (where b max was the maximum b value that the specimen could reach before it was damaged); Unless otherwise specified, the aliphatic-aromatic copolyester used in the present invention is self-prepared according to the method disclosed in Example B13 to B21 of CN100429256C, where the type of starting material for reaction can be appropriately adjusted according to the composition and molecular weight of the target product, and the molecular weight of the product and the content of each repeat unit in the product can be controlled by adjusting the supply amount and supply ratio, respectively.
[0358] <Shape memory material> (Example I-1) Under stirring conditions (stirring speed 30 rpm, 10 minutes), butylene terephthalate (BT)-butylene succinate (BS) copolyester (weight average molecular weight 100,000, the content of BT repeat units was 30 mol% relative to the total number of moles of BT repeat units and BS repeat units), butylene terephthalate (BT)-butylene adipate (BA) copolyester (purchased from BASF, trade name "ecoflex", the content of BT repeat units was 50 mol% relative to the total number of moles of BT repeat units and BA repeat units), and polybutylene succinate (PBS) (purchased from BASF, trade name "1111HTA4") were mixed in a molar ratio of 40:40:20, and 1 wt% calcium carbonate (relative to the total weight of the mixture) was added. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were successively 190°C, 200°C, 210°C, 220°C, 220°C, and 210°C) and pelletized to obtain polyester composition I-A1.
[0359] (Comparative example I-1) A polyester composition I-D1 was produced in accordance with the steps of Example I-1, except that the BT-BS copolyester used in Example I-1 was replaced with the same molar amount of polybutylene terephthalic acid (PBT) (purchased from DuPont under the trade name "Crastin SC164 NC010").
[0360] (Comparative example I-2) A polyester composition I-D2 was produced in accordance with the steps of Example I-1, except that the BT-BA copolyester used in Example I-1 was replaced with the same molar amount of PBT (purchased from Dupont, product name "Crastin SC164 NC010").
[0361] (Comparative example I-3) A polyester composition I-D3 was obtained by producing a polyester composition according to the method of Example I-1, except that the PBS used in Example I-1 was not added.
[0362] (Comparative example I-4) A polyester composition I-D4 was obtained by producing a polyester composition according to the process of Example I-1, except that the BT-BS copolyester, the BT-BA copolyester and the PBS were mixed in a molar ratio of 2:2:96.
[0363] (Example I-2) Under stirring conditions (stirring speed 30 rpm, 10 min), BT-BS copolyester (weight average molecular weight 100,000, the content of BT repeat units was 55 mol% relative to the total number of moles of BT repeat units and BS repeat units), BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeat units was 20 mol% relative to the total number of moles of BT repeat units and BA repeat units) and PBS were mixed in a molar ratio of 20:70:10, and 1 wt% (relative to the total weight of the mixture) of calcium carbonate was added. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously 190°C, 200°C, 210°C, 220°C, 220°C, 210°C) and pelletized to obtain polyester composition I-A2.
[0364] (Example I-3) Under stirring conditions (stirring speed 30 rpm, 10 min), BT-BS copolyester (weight average molecular weight 100,000, the content of BT repeat units was 30 mol% relative to the total number of moles of BT repeat units and BS repeat units), BT-BA copolyester (purchased from BASF, trade name "ecoflex", weight average molecular weight 100,000, the content of BT repeat units was 50 mol% relative to the total number of moles of BT repeat units and BA repeat units) and PBS were mixed in a molar ratio of 50:49:1, and 1 wt% (relative to the total weight of the mixture) of calcium carbonate was added. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 190°C, 200°C, 210°C, 220°C, 220°C, 210°C) and pelletized to obtain polyester composition I-A3.
[0365] (Example I-4) Under stirring conditions (stirring speed 30 rpm, 10 min), BT-BS copolyester (weight average molecular weight 100,000, the content of BT repeat units was 40 mol% relative to the total number of moles of BT repeat units and BS repeat units), BT-BA copolyester (purchased from BASF, trade name "ecoflex", weight average molecular weight 100,000, the content of BT repeat units was 50 mol% relative to the total number of moles of BT repeat units and BA repeat units) and PBS were mixed in a molar ratio of 90:1:9, and 1 wt% (relative to the total weight of the mixture) of calcium carbonate was added. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 160°C, 170°C, 180°C, 180°C, 180°C, 170°C) and pelletized to obtain polyester composition I-A4.
[0366] (Example I-5) Under stirring conditions (stirring speed 30 rpm, 10 min), BT-BS copolyester (weight average molecular weight 100,000, the content of BT repeat units was 40 mol% relative to the total number of moles of BT repeat units and BS repeat units), BT-BA copolyester (purchased from BASF, trade name "ecoflex", weight average molecular weight 100,000, the content of BT repeat units was 50 mol% relative to the total number of moles of BT repeat units and BA repeat units) and PBS were mixed in a molar ratio of 90:1:9, and 5 wt% (relative to the total weight of the mixture) of calcium carbonate was added. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 160°C, 170°C, 180°C, 180°C, 170°C) and pelletized to obtain polyester composition I-A5.
[0367] (Example I-6) Under stirring conditions (stirring speed 30 rpm, 10 min), BT-BS copolyester (weight average molecular weight 100,000, the content of BT repeat units was 40 mol% relative to the total number of moles of BT repeat units and BS repeat units), BT-BA copolyester (purchased from BASF, trade name "ecoflex", weight average molecular weight 100,000, the content of BT repeat units was 50 mol% relative to the total number of moles of BT repeat units and BA repeat units) and PBS were mixed in a molar ratio of 90:1:9, and 5 wt% (relative to the total weight of the mixture) of low density polyethylene (SINOPEC Yanshan Petrochemical Co., Ltd., trade name "LD607") was added. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were successively 160°C, 170°C, 180°C, 180°C, 170°C) and pelletized to obtain polyester composition I-A4.
[0368] (Example I-7) A polyester composition was produced in accordance with the steps of Example I-1, except that the calcium carbonate used in Example I-1 was not added, to obtain polyester composition I-A7.
[0369] (Example I-8) A polyester composition was produced in accordance with the steps of Example I-1, except that the BT-BS copolyester used in Example I-1 was replaced with the same molar amount of ethylene terephthalate (ET)-ethylene succinate (ES) copolyester (weight average molecular weight: 100,000, in which the content of ET repeating units was 50 mol % relative to the total number of moles of ET repeating units and ES repeating units), to obtain polyester composition I-A8.
[0370] (Example I-9) A polyester composition was produced in the same manner as in Example I-1, except that the PBS used in Example I-1 was replaced with the same molar amount of polyhexylene succinate (PHS) (produced in accordance with the method disclosed in CN104039865B, weight average molecular weight 100,000), to obtain polyester composition I-A9.
[0371] (Shape memory property test example) Samples were prepared from the polyester compositions produced in Examples I-1 to I-9 and Comparative Examples I-1 to I-4, and a shape memory property test was carried out. The results are shown in Table 1 below.
[0372] [Table 1]
[0373] When the polyester compositions prepared in the above Examples I-1 to I-9 are used as shape-memory materials, the deformation fixation rate and shape recovery rate of the shape-memory materials are both 92% or more, and the maximum deformation rate is 400% or more. In addition, both the initial molding temperature and the starting temperature of the shape-memory materials can be adjusted. This is more favorable for applying the shape-memory materials in daily life.
[0374] <3D printing materials> (Example II-1) Under stirring conditions (stirring speed 50r / min, 10 min), 1 kg of BT-BS copolyester A (weight average molecular weight 300,000, the content of BT repeat units is 30 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 50 g of BT-BS copolyester B (weight average molecular weight 200,000, the content of BT repeat units is 10 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 50 g of BT-BS copolyester C (weight average molecular weight 200,000, the content of BT repeat units is 80 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 100 g of titanium dioxide were mixed and then charged into a twin-screw extruder. The mixture was melt extruded at 180°C and pelletized to obtain polyester composition II-A1.
[0375] The polyester composition II-A1 was put into an extruder, extruded from a round hole die at 180° C., and cooled through an air or water tank at 0° C. In this manner, a 3D printing wire II-B1 having a diameter of 1.75 mm was obtained.
[0376] (Example II-2) Under stirring conditions (stirring speed 50r / min, 10 min), 880g of BT-BS copolyester A (weight average molecular weight 300,000, BT repeat unit content is 40 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 110g of BT-BS copolyester B (weight average molecular weight 200,000, BT repeat unit content is 15 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 110g of BT-BS copolyester C (weight average molecular weight 200,000, BT repeat unit content is 85 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 100g of titanium dioxide were mixed and then charged into a twin-screw extruder. The mixture was melt extruded at 180°C and pelletized to obtain polyester composition II-A2.
[0377] The polyester composition II-A2 was put into an extruder, extruded from a round hole die at 180° C., and cooled through an air or water tank at 0° C. In this way, a 3D printing wire II-B2 having a diameter of 1.75 mm was obtained.
[0378] (Example II-3) Under stirring conditions (stirring speed 50r / min, 10 min), 770g of BT-BS copolyester A (weight average molecular weight 300,000, the content of BT repeating units is 25 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 165g of BT-BS copolyester B (weight average molecular weight 200,000, the content of BT repeating units is 5 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 165g of BT-BS copolyester C (weight average molecular weight 200,000, the content of BT repeating units is 50 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, and 100g of titanium dioxide were mixed and then charged into a twin-screw extruder. The mixture was melt extruded at 180°C and pelletized to obtain polyester composition II-A3.
[0379] The polyester composition II-A3 was put into an extruder, extruded from a round hole die at 180° C., and cooled through an air or water tank at 0° C. In this way, a 3D printing wire II-B3 having a diameter of 1.75 mm was obtained.
[0380] (Example II-4) Under stirring conditions (stirring speed 50r / min, 10 min), 605g of BT-BS copolyester A (weight average molecular weight 300,000, the content of BT repeating units is 44 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 275g of BT-BS copolyester B (weight average molecular weight 200,000, the content of BT repeating units is 19 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 220g of PBT (polyester C, purchased from DuPont, trade name "Crastin SC164 NC010") particles, and 100g of titanium dioxide were mixed, and then the mixture was put into a twin-screw extruder. The mixture was melt extruded at 180°C and pelletized to obtain polyester composition II-A4.
[0381] The polyester composition II-A4 was put into an extruder, extruded from a round hole die at 180° C., and cooled through an air or water tank at 0° C. In this way, a 3D printing wire II-B4 having a diameter of 1.75 mm was obtained.
[0382] (Example II-5) Under stirring conditions (stirring speed 50r / min, 10 min), 1078g of BT-BS copolyester A (weight average molecular weight 300,000, BT repeat unit content is 20 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 11g of BT-BS copolyester B (weight average molecular weight 200,000, BT repeat unit content is 1 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 11g of BT-BS copolyester C (weight average molecular weight 200,000, BT repeat unit content is 45 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 100g of titanium dioxide were mixed and fed into a twin-screw extruder. The mixture was melt extruded at 180°C and pelletized to obtain polyester composition II-A5.
[0383] The polyester composition II-A5 was put into an extruder, extruded from a round hole die at 180° C., and cooled through an air or water tank at 0° C. In this way, a 3D printing wire II-B5 having a diameter of 1.75 mm was obtained.
[0384] (Example II-6) Polyester B was changed to BT-BA copolyester (weight average molecular weight 200,000, the content of BT repeating units was 10 mol% relative to the total number of moles of BT repeating units and BA repeating units), and polyester was changed to BT-BA copolyester (weight average molecular weight 200,000, the content of BT repeating units was 80 mol% relative to the total number of moles of BT repeating units and BA repeating units).Other than that, polyester composition II-A6 and 3D print wire II-B6 were obtained according to the process of Example II-1.
[0385] (Example II-7) Polyester B was changed to ET-EA (ethylene adipate) copolyester (weight average molecular weight 200,000, ET repeat unit content was 10 mol% relative to the total number of moles of ET repeat units and EA repeat units), and polyester C was changed to ET-EA copolyester (weight average molecular weight 200,000, ET repeat unit content was 80 mol% relative to the total number of moles of ET repeat units and EA repeat units).Other than that, polyester composition II-A7 and 3D print wire II-B7 were obtained according to the process of Example II-1.
[0386] (Example II-8) Polyester B was changed to ET-BS copolyester (weight average molecular weight 200,000, ET repeat unit content was 10 mol% relative to the total number of moles of ET repeat units and BS repeat units), and polyester C was changed to BT-EA copolyester (weight average molecular weight 200,000, BT repeat unit content was 80 mol% relative to the total number of moles of BT repeat units and EA repeat units).Other than that, polyester composition II-A8 and 3D print wire II-B8 were obtained according to the process of Example II-1.
[0387] (Example II-9) Polyester composition II-A9 and 3D print wire II-B9 were obtained in accordance with the process of Example II-1, except that the same weight of calcium carbonate was used instead of titanium dioxide in Example II-1.
[0388] (Example II-10) Polyester composition II-A10 and 3D print wire II-B10 were obtained according to the process of Example II-1, except that 100 g of titanium dioxide was not added.
[0389] (Comparative Example II-1) Wire II-D1 was obtained in accordance with the process of Example II-1, except that 1 kg of polyester A used in Example II-1, 100 g of polyester B used in Example II-1, and 100 g of titanium dioxide were mixed and polyester C used in Example II-1 was not added.
[0390] (Comparative Example II-2) Wire II-D2 was obtained in accordance with the process of Example II-1, except that 1 kg of Polyester A used in Example II-1, 100 g of Polyester C used in Example II-1, and 100 g of titanium dioxide were mixed and Polyester B used in Example II-1 was not added.
[0391] (Comparative Example II-3) Wire II-D3 was obtained in accordance with the process of Example II-1, except that 550 g of Polyester B used in Example II-1, 550 g of Polyester C used in Example II-1, and 100 g of titanium dioxide were mixed and Polyester A used in Example II-1 was not added.
[0392] (Comparative Example II-4) Wire II-D4 was obtained in accordance with the process of Example II-1, except that 50 g of Polyester A used in Example II-1, 1 kg of Polyester B used in Example II-1, 50 g of Polyester C used in Example II-1, and 100 g of titanium dioxide were mixed.
[0393] (Comparative Example II-5) Wire II-D5 was obtained in accordance with the steps of Example II-1, except that the same weight of PBS (purchased from BASF, product name "1111HTA4") was used instead of Polyester A used in Example II-1.
[0394] (Comparative Example II-6) Wire II-D6 was obtained in accordance with the steps of Example II-1, except that the same weight of PBS (purchased from BASF, product name "1111HTA4") was used instead of Polyester C used in Example II-1.
[0395] (Comparative Example II-7) Wire II-D7 was obtained in the same manner as in Example II-1, except that 1.1 kg of Polyester A used in Example II-1 and 100 g of titanium dioxide were mixed.
[0396] (Comparative Example II-8) Wire II-D8 was obtained in the same manner as in Example II-1, except that 1.1 kg of the polyester B used in Example II-1 and 100 g of titanium dioxide were mixed.
[0397] (Comparative Example II-9) Wire II-D9 was obtained in the same manner as in Example II-1, except that 1.1 kg of the polyester C used in Example II-1 and 100 g of titanium dioxide were mixed.
[0398] (Comparative Example II-10) Wire II-D10 was obtained in accordance with the steps of Example II-1, except that 1.1 kg of PBT (purchased from DuPont under the trade name "Crastin SC164 NC010") and 100 g of titanium dioxide were mixed.
[0399] (Test Examples II-1 to II-20) 1. Gloss evaluation The polyester composition pellets obtained in Examples II-1 to II-10 and Comparative Examples II-1 to II-10 were cast into flat plates at room temperature (25°C) using a Haake mini-casting machine. After the cast sheets were completely cooled and solidified, the surface that was not in contact with the cooling plate was subjected to a gloss test. The gloss of the cast sheets obtained in Examples II-1 to II-10 and Comparative Examples II-1 to II-10 was evaluated according to GB / T9754-2007. The results are shown in Table 2.
[0400] 2. Hardness (or flexibility) evaluation The wires obtained in Examples II-1 to II-10 and Comparative Examples II-1 to II-10 were cut into particles. The particles were hot pressed at or above the melting point using a Carver hot press to obtain sheets of 7 cm x 7 cm x 4 mm. The Shore hardness (D type) of the sheets obtained in Examples II-1 to II-10 and Comparative Examples II-1 to II-10 was evaluated according to the method of GB / T2411-2008. The results are shown in Table 2.
[0401] 3.Minimum printing temperature and printing effect The wires obtained in Examples II-1 to II-10 and Comparative Examples II-1 to II-10 were loaded into a Makerbot Replicator 2X printer, and the nozzle temperature was increased until the flow rate of the wire through the nozzle reached 2.4 m / min. This temperature was defined as the minimum printing temperature. If the given 3D printing shape could be finally produced when 3D printing was performed with the default printing condition settings of the lamination equipment, the printing effect was deemed to be "good". If the actually printed shape deviated from the given 3D printing shape, the printing effect was deemed to be "poor". The results of the minimum printing temperature and printing effect are shown in Table 2.
[0402] 4.Degradability The biodegradability of the films produced in Examples II-1 to II-10 and Comparative Examples II-1 to II-10 was tested according to the following method. 18 g of compost (composting period 2 months, provided by Beijing Nangong Compost Factory) was used. 3 g of the wire to be tested was added, and an appropriate amount of distilled water was added and mixed. After appropriate stirring, the mixture was left to stand at room temperature (25°C). The pass / fail criteria for biodegradability was whether the weight loss after 3 months was 50% or more. The results are shown in Table 1.
[0403] In addition, the 3D printing wires obtained in Examples II-1 to II-10 could be stored for more than one year in a clean environment at room temperature and humidity without any obvious changes. Significant deterioration occurred only in the case of a soil environment, a nutrient-rich environment, or a compost environment.
[0404] [Table 2]
[0405] As can be seen from the results in Table 2 above, the polyester composition obtained by the present invention contains specific polyester A, polyester B, and polyester C in a specific ratio (polyester A: 51 to 98% by weight, polyester B: 1 to 48% by weight, polyester C: 1 to 48% by weight). The 3D printing wire made from the polyester composition has a higher gloss and can be printed at a lower temperature (105 to 165°C). In addition, the 3D printing wire can be used as a flexible wire (Shore hardness (D type): 35 to 50) and is degradable. Therefore, it has the advantage of being environmentally friendly and has the prospect of application.
[0406] <Heat shrink pipe> (Example III-1) Under stirring conditions (stirring speed 30 r / min, 10 min), 4 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeating units was 32 mol% relative to the total number of moles of BT repeating units and BS repeating units), 1 kg of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeating units was 55 mol% relative to the total number of moles of BT repeating units and BS repeating units), 0.05 kg of antioxidant 300 (hindered phenol antioxidant, manufactured by the Materials Synthesis Research Institute, Ministry of Chemical Industry), and 0.05 kg of carbon black were mixed. Then, the mixture was extruded through a twin-screw extruder, stretched, air-cooled, and pelletized. At this time, the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 190°C, 200°C, 210°C, 220°C, 220°C, and 210°C. The screw rotation speed was 10 rpm, and the torque was 20 N·m. A polyester composition III-A1 was obtained.
[0407] The pellets of the polyester composition III-A1 were fed to a screw extruder equipped with a ring-shaped die, extruded into a pipe at 180° C., and molded by water cooling at 40° C. The pipe was then heated to 90° C. and expanded to an inner diameter five times the original diameter, and cooled and molded at 40° C. to obtain a heat-shrinkable sleeve III-B1.
[0408] (Example III-2) Under stirring conditions (stirring speed 30 r / min, 10 min), 4.75 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeating units was 45 mol% based on the total number of moles of BT repeating units and BS repeating units), 0.25 kg of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeating units was 80 mol% based on the total number of moles of BT repeating units and BS repeating units), 0.05 kg of antioxidant 300 (hindered phenol antioxidant, manufactured by the Materials Synthesis Research Institute, Ministry of Chemical Industry), and 0.05 kg of carbon black were mixed. The mixture was then extruded through a twin-screw extruder, stretched, air-cooled, and pelletized. At this time, the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were successively set to 190°C, 200°C, 210°C, 220°C, 220°C, and 210°C. The screw rotation speed was 20 rpm and the torque was 10 N·m to obtain a polyester composition III-A2.
[0409] The pellets of the polyester composition III-A2 were fed to a screw extruder equipped with a ring-shaped die, extruded into a pipe at 120° C., and molded by water cooling at 20° C. The pipe was then heated to 70° C. and expanded to an inner diameter five times the original diameter, and cooled at 20° C. to obtain a heat-shrinkable sleeve III-B2.
[0410] (Example III-3) Under stirring conditions (stirring speed 30 r / min, 10 min), 4.25 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeating units was 40 mol% based on the total number of moles of BT repeating units and BS repeating units), 0.75 kg of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeating units was 70 mol% based on the total number of moles of BT repeating units and BS repeating units), 0.05 kg of antioxidant 300 (hindered phenol antioxidant, manufactured by the Materials Synthesis Research Institute, Ministry of Chemical Industry), and 0.05 kg of carbon black were mixed. The mixture was then extruded through a twin-screw extruder, stretched, air-cooled, and pelletized. At this time, the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were successively set to 190°C, 200°C, 210°C, 220°C, 220°C, and 210°C. The screw rotation speed was 10 rpm and the torque was 20 N·m to obtain polyester composition III-A3.
[0411] The pellets of the polyester composition III-A3 were fed to a screw extruder equipped with a ring-shaped die, extruded into a pipe at 160° C., and molded by water cooling at 25° C. The pipe was then heated to 80° C. and expanded to an inner diameter five times the original diameter, and cooled at 25° C. to obtain a heat-shrinkable sleeve III-B3.
[0412] (Example III-4) Under stirring conditions (stirring speed 30 r / min, 10 min), 4.95 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeating units was 49 mol% based on the total number of moles of BT repeating units and BS repeating units), 0.05 kg of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeating units was 99 mol% based on the total number of moles of BT repeating units and BS repeating units), 0.05 kg of antioxidant 300 (hindered phenol antioxidant, manufactured by the Materials Synthesis Research Institute, Ministry of Chemical Industry), and 0.05 kg of carbon black were mixed. The mixture was then extruded through a twin-screw extruder, stretched, air-cooled, and pelletized. At this time, the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were successively set to 190°C, 200°C, 210°C, 220°C, 220°C, and 210°C. The screw rotation speed was 10 rpm and the torque was 20 N·m. Polyester composition III-A4 was obtained.
[0413] The pellets of the polyester composition III-A4 were fed to a screw extruder equipped with a ring-shaped die, extruded into a pipe at 180° C., and molded by water cooling at 25° C. The pipe was then heated to 90° C. and expanded to an inner diameter five times the original diameter, and cooled at 25° C. to obtain a heat-shrinkable sleeve III-B4.
[0414] (Example III-5) Under stirring conditions (stirring speed 30 r / min, 10 min), 2.55 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeating units was 30 mol% relative to the total number of moles of BT repeating units and BS repeating units), 2.45 kg of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeating units was 50 mol% relative to the total number of moles of BT repeating units and BS repeating units), 0.05 kg of antioxidant 300 (hindered phenol antioxidant, manufactured by the Materials Synthesis Research Institute, Ministry of Chemical Industry), and 0.05 kg of carbon black were mixed. Then, the mixture was extruded through a twin-screw extruder, stretched, air-cooled, and pelletized. At this time, the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 190°C, 200°C, 210°C, 220°C, 220°C, and 210°C. The screw rotation speed was 10 rpm and the torque was 20 N·m to obtain a polyester composition III-A5.
[0415] The pellets of the polyester composition III-A5 were fed to a screw extruder equipped with a ring-shaped die, extruded into a pipe at 180° C., and molded by water cooling at 25° C. The pipe was then heated to 90° C. and expanded to an inner diameter five times the original diameter, and cooled at 25° C. to obtain a heat-shrinkable sleeve III-B5.
[0416] (Example III-6) Polyester composition III-A6 and heat-shrinkable sleeve III-B6 were obtained in accordance with the steps of Example III-1, except that polyester A was changed to BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeating units was 45 mol% relative to the total number of moles of BT repeating units and BA repeating units) and polyester B was changed to BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeating units was 70 mol% relative to the total number of moles of BT repeating units and BA repeating units).
[0417] (Example III-7) Polyester composition III-A7 and heat-shrinkable sleeve III-B7 were obtained in accordance with the steps of Example III-1, except that polyester A was changed to BT-ES (ethylene succinate) copolyester (weight average molecular weight 200,000, the content of BT repeating units was 45 mol% relative to the total number of moles of BT repeating units and ES repeating units) and polyester B was changed to BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating units was 70 mol% relative to the total number of moles of BT repeating units and ES repeating units).
[0418] (Example III-8) Polyester composition III-A8 and heat-shrinkable sleeve III-B8 were obtained in accordance with the steps of Example III-1, except that polyester A was changed to BT-BA copolyester (weight average molecular weight 500,000, the content of BT repeating units was 45 mol% relative to the total number of moles of BT repeating units and BA repeating units) and polyester B was changed to BT-ES copolyester (weight average molecular weight 500,000, the content of BT repeating units was 70 mol% relative to the total number of moles of BT repeating units and ES repeating units).
[0419] (Example III-9) A polyester composition III-A9 and a heat-shrinkable sleeve III-B9 were obtained in the same manner as in Example III-1, except that 0.05 kg of titanium dioxide was used instead of 0.05 kg of carbon black used in Example III-1.
[0420] (Example III-10) A polyester composition III-A10 and a heat-shrinkable sleeve III-B10 were obtained in accordance with the steps of Example III-1, except that 0.05 kg of antioxidant 300 and 0.05 kg of carbon black were not added.
[0421] (Comparative Example III-1) The process of Example III-1 was followed, except that Polyester A of Example III-1 was used directly to prepare Sleeve III-DB1, and the mixing step with Polyester B of Example III-1 was not included.
[0422] (Comparative Example III-2) The process of Example III-1 was followed, except that Polyester B of Example III-1 was used directly in the preparation of Sleeve III-DB2, and the mixing step with Polyester A of Example III-1 was not included.
[0423] (Comparative Example III-3) Sleeve III-DB3 was produced according to the process of Example III-1, except that the same weight of PBT (purchased from DuPont, product name "Crastin SC164 NC010", the same applies below) was used instead of Polyester A used in Example III-1.
[0424] (Comparative Example III-4) A sleeve III-DB4 was produced in accordance with the process of Example III-1, except that the same weight of PBT was used in place of the polyester B used in Example III-1.
[0425] (Comparative Example III-5) Sleeve III-DB5 was produced in accordance with the steps of Example III-1, except that the same weight of PBS (purchased from BASF, product name "1111HTA4", the same applies below) was used instead of Polyester A used in Example III-1.
[0426] (Comparative Example III-6) Sleeve III-DB6 was produced in accordance with the process of Example III-1, except that the same weight of PBS was used in place of Polyester B used in Example III-1.
[0427] (Comparative Example III-7) Sleeve III-DB7 was produced in accordance with the steps of Example III-1, except that the amount of Polyester A was changed to 1 kg and the amount of Polyester B was changed to 4 kg.
[0428] (Comparative Example III-8) Sleeve III-DB8 was produced in accordance with the steps of Example III-1, except that the amount of Polyester A was changed to 2.5 kg and the amount of Polyester B was changed to 2.5 kg.
[0429] (Comparative Example III-9) The steps of Example III-1 were followed, except that the sleeve III-DB9 was made directly from PBT.
[0430] Comparative Example 10 The procedure was the same as in Example III-1, except that Sleeve III-DB10 was prepared directly from PBS.
[0431] (Test Examples III-1 to III-20) Shrinkage Test: The outer diameter of the heat-shrinkable pipe before shrinkage was measured at 25°C using a vernier caliper. The heat-shrinkable pipe was placed in an oven at a constant temperature of 80°C for 1 hour, removed, and naturally cooled to 25°C. The outer diameter of the heat-shrinkable pipe after shrinkage was then measured using a vernier caliper. The shrinkage ratio results were recorded as "diameter before shrinkage: diameter after shrinkage". The shrinkage ratios of the sleeves produced in Examples III-1 to III-10 and Comparative Examples III-1 to III-10 were measured by the above-mentioned method. The results are shown in Table 3.
[0432] Dielectric breakdown test: Regarding dielectric breakdown strength, the sleeve materials prepared in Examples III-1 to III-10 and Comparative Examples III-1 to III-10 were tested according to the method of Chinese Standard GB / T1408.1-2006. As a result, the dielectric breakdown strengths of the sleeves prepared in Examples III-1 to III-10 were all 25 kv / mm or more. This shows that the sleeves obtained by the present invention have good insulating properties.
[0433] Degradability test: 18 kg of compost (composting period 2 months, provided by Beijing Nangong Compost Factory) was used. 3 g of the film to be tested was added, and an appropriate amount of distilled water was added and mixed. After appropriate stirring, the mixture was left to stand at room temperature. Whether the weight loss after 3 months was 50% or more was used as the criterion for evaluating the pass / fail of biodegradability. The results are shown in Table 1.
[0434] The results of the shrinkage test and the decomposition test are shown in Table 3.
[0435] The heat-shrinkable sleeves obtained in Examples III-1 to III-10 could be stored for more than one year in a clean environment at room temperature and humidity without any obvious changes. Significant deterioration occurred only in a soil environment, a nutrient-rich environment, or a compost environment.
[0436] [Table 3]
[0437] As can be seen from the results in Table 3 above, in the present invention, by blending specific copolymers (polyester A and polyester B) in specific ratios (polyester A content: 51-99% by weight, polyester B content: 1-49% by weight), a heat-shrinkable sleeve with high heat shrinkage ratio (5:4.5 or higher) and high insulating properties can be obtained. Furthermore, the heat-shrinkable sleeve does not require crosslinking during the manufacturing process, exhibits high degradability, and therefore has a wide market space.
[0438] <Functional layer (sports protector)> (Example IV-1) Under stirring conditions (stirring speed 30 rpm, 5 minutes), 150 g of BT-BA copolyester A (weight average molecular weight 100,000, the content of BT repeating units is 25 mol% relative to the total number of moles of BT repeating units and BA repeating units) particles, 20 g of BT-BS copolyester B (weight average molecular weight 110,000, the content of BT repeating units is 10 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 20 g of glass fiber (Taishan Fiberglass Inc, Tademark T536, the same below), and 10 g of anhydrous calcium sulfate (Tianjin Zhiyuan Chemical Reagents Co, Ltd., analytical) were thoroughly mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 40 N·m, and the temperatures in various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were successively 180°C, 190°C, 195°C, 195°C, 195°C, and 195°C) and pelletized to obtain polyester composition IV-A1.
[0439] (Example IV-2) Under stirring conditions (stirring speed 30 rpm, 5 min), 171 g of BT-BA copolyester A (weight average molecular weight 100,000, BT repeat unit content 40 mol% relative to the total number of moles of BT repeat units and BA repeat units) particles, 9.5 g of BT-BS copolyester B (weight average molecular weight 110,000, BT repeat unit content 15 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 9.5 g of glass fiber, and 10 g of anhydrous calcium sulfate were thoroughly mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 40 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 180°C, 190°C, 195°C, 195°C, 195°C, 195°C) and pelletized to obtain polyester composition IV-A2.
[0440] (Example IV-3) Under stirring conditions (stirring speed 30 rpm, 5 min), 114 g of BT-BA copolyester A (weight average molecular weight 100,000, BT repeat unit content 23 mol% relative to the total number of moles of BT repeat units and BA repeat units) particles, 57 g of BT-BS copolyester B (weight average molecular weight 110,000, BT repeat unit content 5 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 19 g of glass fiber, and 10 g of anhydrous calcium sulfate were thoroughly mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 40 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 180°C, 190°C, 195°C, 195°C, 195°C, 195°C) and pelletized to obtain polyester composition IV-A3.
[0441] (Example IV-4) Under stirring conditions (stirring speed 30 rpm, 5 min), 95 g of BT-BA copolyester A (weight average molecular weight 100,000, BT repeat unit content 45 mol% relative to the total number of moles of BT repeat units and BA repeat units) particles, 85.5 g of BT-BS copolyester B (weight average molecular weight 110,000, BT repeat unit content 20 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 9.5 g of basalt fiber, and 10 g of anhydrous calcium sulfate were thoroughly mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 40 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 180°C, 190°C, 195°C, 195°C, 195°C, 195°C) and pelletized to obtain polyester composition IV-A4.
[0442] (Example IV-5) Under stirring conditions (stirring speed 30 rpm, 5 min), 95 g of BT-BA copolyester A (weight average molecular weight 100,000, the content of BT repeating units is 20 mol % relative to the total number of moles of BT repeating units and BA repeating units) particles, 9.5 g of PBT (purchased from DuPont under the name of Crastin SC164 NC010) particles, 85.5 g of basalt fibers, and 10 g of anhydrous calcium sulfate were thoroughly mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was 40 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously 180°C, 190°C, 195°C, 195°C, 195°C, 195°C) and pelletized to obtain polyester composition IV-A5.
[0443] (Example IV-6) The method of Example IV-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeat unit was 25 mol% relative to the total moles of BT repeat unit and BA repeat unit); polyester B was BT-BA copolyester (weight average molecular weight 110,000, the content of BT repeat unit was 10 mol% relative to the total moles of BT repeat unit and BA repeat unit). Polyester composition IV-A6 was obtained.
[0444] (Example IV-7) The method of Example IV-1 was followed, except that polyester A was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating unit is 25 mol% based on the total moles of BT repeating unit and ES repeating unit); polyester B was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating unit is 10 mol% based on the total moles of BT repeating unit and ES repeating unit). Polyester composition IV-A7 was obtained.
[0445] (Example IV-8) The method of Example IV-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 500,000, the content of BT repeat unit is 25 mol% based on the total moles of BT repeat unit and BA repeat unit); polyester B was BT-ES copolyester (weight average molecular weight 500,000, the content of BT repeat unit is 10 mol% based on the total moles of BT repeat unit and ES repeat unit). Polyester composition IV-A8 was obtained.
[0446] (Example IV-9) The method of Example IV-1 was followed, except that no anhydrous calcium sulfate was added, to obtain polyester composition IV-A9.
[0447] (Comparative Example IV-1) The method of Example IV-1 was followed, except that 170g of polyester A used in Example IV-1, 20g of glass fiber and 10g of anhydrous calcium sulfate were mixed without adding polyester B used in Example IV-1. Polyester composition IV-D1 was obtained.
[0448] (Comparative example IV-2) The method of Example IV-1 was followed, except that 170g of polyester B used in Example IV-1, 20g of glass fiber and 10g of anhydrous calcium sulfate were mixed without adding polyester A used in Example IV-1. Polyester composition IV-D2 was obtained.
[0449] (Comparative Example IV-3) The method of Example IV-1 was followed, except that the same weight of PBT (trade name "Crastin SC164 NC010", purchased from DuPont) was used instead of the polyester A used in Example IV-1. Polyester composition IV-D3 was obtained.
[0450] (Comparative Example IV-4) The method of Example IV-1 was followed, except that the same weight of PBT (trade name "Crastin SC164 NC010", purchased from DuPont) was used instead of the polyester B used in Example IV-1. Polyester composition IV-D4 was obtained.
[0451] (Comparative Example IV-5) The same weight of PBS (trade name "1111HTA4", purchased from BASF, the same applies below) was used instead of the polyester A used in Example IV-1, and the same was repeated in the same manner as in Example IV-1 to obtain a polyester composition IV-D5.
[0452] (Comparative Example IV-6) The procedure of Example IV-1 was followed, except that no glass fiber was added, to obtain polyester composition IV-D6.
[0453] (Comparative example IV-7) The procedure of Example IV-1 was followed, except that the amount of Polyester A was 20 g and the amount of Polyester B was 150 g, to obtain Polyester Composition IV-D7.
[0454] (Comparative example IV-8) The method of Example IV-1 was followed, except that 190 g of PBT and 10 g of anhydrous calcium sulfate were mixed to obtain polyester composition IV-D8.
[0455] (Comparative Example IV-9) The method of Example IV-1 was followed, except that 190 g of PBS and 10 g of anhydrous calcium sulfate were mixed to obtain polyester composition IV-D9.
[0456] (Test Examples IV-1 to IV-18) 1.Hardness test The polyester compositions prepared in Examples IV-1 to IV-9 and Comparative Examples IV-1 to IV-9 were melted, treated at 170°C and 1000 MPa for 5 minutes, and pressed into plates with a thickness of 4 mm and a side length of 7 cm. The hot plates were removed and quenched for 1 minute with a cold iron block that had been left at room temperature for a long time, then removed and left at room temperature (25°C) for 1 hour. The plates were measured using a Drick shore D handheld durometer and the measurement results were recorded after 15 seconds. They were then heated to 90°C on a hot stage, and the Shore D hardness was also measured in the same manner. The results are shown in Table 4.
[0457] 2. Shape memory property test Test pieces were prepared from the polyester compositions produced in Examples IV-1 to IV-9 and Comparative Examples IV-1 to IV-9, and a shape memory property test was performed. The results are shown in Table 4. The shape memory property of the polyester compositions was measured using an Instron 5965 tensile tester (with incubator) as follows.
[0458] A test piece of the polyester composition had an initial length a at room temperature, and when the temperature of the incubator was raised to 80°C, it became sufficiently softened and was stretched to a length b at a stretching speed of 50 mm / min; the external force was maintained so that the stretched length did not change, and the temperature was lowered, and the test piece had a length "c" when the test piece was solidified and the external force was removed; the temperature of the test piece was again raised to 80°C, and the test piece had sufficiently shrunk to a length "d".
[0459] Deformation fixation rate (%) = (cA) / (bA) × 100%; Deformation recovery rate (%) = (cd) / (ca) × 100%; Maximum deformation rate (%) = b max / a×100% where b max was the maximum b value that the specimen could reach before it was damaged.
[0460] [Table 4]
[0461] From the results of Table 4, it can be seen that the polyester compositions of Examples IV-1 to IV-9 have low hardness at high temperatures (90°C) and significantly increased hardness at low temperatures (25°C), and were easy to mold, as compared with Examples IV-1 to IV-9. In addition, the polyester compositions of Examples IV-1 to IV-9 had relatively high deformation fixation rates (90% or more), deformation recovery rates (90% or more), and maximum deformation rates (280% or more). The results show that the polyester compositions provided by the present invention have good low-temperature plasticity and shape memory properties.
[0462] (Example IV-10) The polyester composition IV-A1 obtained in Example IV-1 was molded into a tooth protector by injection molding at a temperature of 170° C. (The composition was poured into an aluminum mold and taken out as a U-shaped mold at room temperature (25° C.)). The obtained U-shaped mold was softened in hot water at 90° C., then rapidly cooled to 0° C., placed in the mouth, and the upper and lower teeth were brought together to form the tooth outline. After trimming, the completed tooth protector was obtained as shown in FIG. 1 and FIG. 2.
[0463] When the tooth protector was to be worn or was uncomfortable for use, it was softened again in 90°C hot water, rapidly cooled to 0°C, placed in the mouth and bitten by the upper and lower teeth to form the contours of the teeth, and after trimming, a new completed tooth protector with a shape that more closely matches the teeth was obtained.
[0464] (Example IV-11) The polyester composition IV-A1 obtained in Example IV-1 was injection molded at a temperature of 175°C to form the intermediate layer of the knee pad (injected into an aluminum mold and removed as a mold at room temperature (25°C)). The obtained mold was softened in hot water at 90°C, then quenched to 0°C, pressed against the surface of the knee joint to form the knee joint contour, and after trimming, the intermediate layer of the knee pad was obtained. Then, the inner surface of the intermediate layer of the obtained knee pad was taped to the inner layer of the cotton material, and the outer surface of the intermediate layer of the knee pad was fastened to the outer layer of the aluminum alloy material with an adhesive buckle, so that the intermediate layer can be removed at any time. As a result, the outer layer, intermediate layer and inner layer were assembled together to form a completed knee pad, as shown in Figures 3 and 4.
[0465] When the knee pad was to be worn or was uncomfortable for use, it was softened again in 90°C hot water, rapidly cooled to 0°C, and pressed against the surface of the knee joint to form the knee joint contour, and after trimming, a new middle layer of the knee pad was obtained with a shape that more closely matched the knee joint.
[0466] (Example IV-12) The polyester composition IV-A1 obtained in Example IV-1 was formed as the middle layer of an upper body protective suit by injection molding at a temperature of 180°C (injected into an aluminum mold and removed as a mold at room temperature (25°C)). The obtained mold was softened in hot water at 90°C, quenched to 0°C, and pressed around the surface of the upper body to form the contour of the upper body, and after trimming, the middle layer of the upper body protector was obtained. Then, the inner surface of the middle layer of the obtained upper body protective suit was taped to the inner layer of the spandex material, and the outer surface of the middle layer of the upper body protective suit was fastened to the outer layer of the PBS material with an adhesive buckle, so that the middle layer can be removed at any time. In this way, the outer layer, the middle layer and the inner layer were assembled together to form the completed upper body protective suit, as shown in Figures 5 and 6.
[0467] When the upper body protective gear is worn or becomes uncomfortable to use, the upper body protective gear is softened again in 90°C warm water, then rapidly cooled to 0°C, and pressed against the surface of the upper body to form the contour of the upper body, and after trimming, a new middle layer of the upper body protective gear having a shape that more closely matches the upper body is obtained.
[0468] (Example IV-13) The polyester composition IV-A1 obtained in Example IV-1 was formed as the intermediate layer of a helmet by injection molding at a temperature of 185°C (injected into an aluminum mold and removed as a mold at room temperature (25°C)). The obtained mold was softened in hot water at 90°C, quenched to 0°C, and pressed against the surface of the head to form the head contour, and after trimming, the intermediate layer of the helmet was obtained. Then, the inner surface of the intermediate layer of the obtained helmet was fastened to the inner layer of the sponge material with an adhesive buckle, and the outer surface of the intermediate layer of the knee pad was fastened to the outer layer of the aluminum alloy material with an adhesive buckle. As shown in Figure 7, the outer layer, intermediate layer and inner layer were also fixed by buckles and assembled together to form a completed helmet.
[0469] When the helmet was worn or was uncomfortable to use, it was softened again in 90°C hot water, rapidly cooled to 0°C, and pressed against the surface of the head to form the head contour, obtaining a new middle layer of the helmet with a shape that better fitted the head after trimming.
[0470] From the above Examples IV-10 to IV-13, when the polyester composition provided by the present invention is used in sports protectors, it can be molded according to different application parts, so that the protectors are more compatible with the body, more comfortable, and easier to manufacture. Furthermore, when the sports protectors of the present invention are worn or slightly damaged, they can be softened by increasing the temperature and remolding at low temperature, and can be restored to their original appearance again.
[0471] [Medical limb immobilization devices] (Example V-1) Under stirring conditions (stirring speed 30 rpm, 10 min), 7 kg of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content 30 mol % relative to the total number of moles of BT and BS repeat units) particles, 3 kg of BT-BA copolyester B (weight average molecular weight 100,000, BT repeat unit content 70 mol % relative to the total number of moles of BT and BA repeat units) particles, and 1 kg of iron oxide were mixed. The resulting mixture was extruded through a twin-screw extruder (screw rotation speed was controlled at 10 rpm, torque was set at 20 N m, and temperatures at various parts of the twin-screw extruder were continuously set at 150°C, 160°C, 170°C, 170°C, 170°C, 170°C from the feed inlet to the extrusion outlet) and pelletized to obtain polyester composition V-A1.
[0472] (Example V-2) Under stirring conditions (stirring speed 30 rpm, 10 min), 8 kg of BT-BS copolyester A (weight average molecular weight 200,000, BT repeat unit content 25 mol % based on the total number of moles of BT repeat units and BS repeat units) particles, 2 kg of BT-BA copolyester B (weight average molecular weight 200,000, BT repeat unit content 50 mol % based on the total number of moles of BT repeat units and BA repeat units) particles, and 1 kg of titanium dioxide were mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 150°C, 160°C, 170°C, 170°C, 170°C, 170°C) and pelletized to obtain polyester composition V-A2.
[0473] (Example V-3) Under stirring conditions (stirring speed 30 rpm, 10 min), 9 kg of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content 30 mol % based on the total moles of BT repeat units and BS repeat units) particles, 1 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content 60 mol % based on the total moles of BT repeat units and BS repeat units) particles, and 1 kg of titanium dioxide were mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 150°C, 160°C, 170°C, 170°C, 170°C, 170°C) and pelletized to obtain polyester composition V-A3.
[0474] (Example V-4) Under stirring conditions (stirring speed 30 rpm, 10 min), 9.9 kg of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content 40 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 0.1 kg of BT-BA copolyester B (weight average molecular weight 100,000, BT repeat unit content 80 mol% relative to the total number of moles of BT repeat units and BA repeat units) particles, and 1 kg of iron oxide were mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 150°C, 160°C, 170°C, 170°C, 170°C, 170°C) and pelletized to obtain polyester composition V-A4.
[0475] (Example V-5) Under stirring conditions (stirring speed 30 rpm, 10 min), 5.1 kg of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content 20 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 4.9 kg of BT-BA copolyester B (weight average molecular weight 100,000, BT repeat unit content 41 mol% relative to the total number of moles of BT repeat units and BA repeat units) particles, and 1 kg of iron oxide were mixed. The resulting mixture was extruded through a twin-screw extruder (the screw rotation speed was controlled at 10 rpm, the torque was set to 20 N·m, and the temperatures of various parts of the twin-screw extruder from the feed inlet to the extrusion outlet were continuously set to 150°C, 160°C, 170°C, 170°C, 170°C, 170°C) and pelletized to obtain polyester composition V-A5.
[0476] (Example V-6) The method of Example V-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 130,000, the content of BT repeat unit is 30 mol% based on the total moles of BT repeat unit and BA repeat unit); polyester B was BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeat unit is 70 mol% based on the total moles of BT repeat unit and BA repeat unit). Polyester composition V-A6 was obtained.
[0477] (Example V-7) The method of Example V-1 was followed, except that polyester A was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating unit is 30 mol% based on the total moles of BT repeating unit and ES repeating unit); polyester B was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating unit is 70 mol% based on the total moles of BT repeating unit and ES repeating unit). Polyester composition V-A7 was obtained.
[0478] (Example V-8) The method of Example V-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 500,000, the content of BT repeating unit is 30 mol% based on the total moles of BT repeating unit and BA repeating unit); polyester B was BT-ES copolyester (weight average molecular weight 500,000, the content of BT repeating unit is 70 mol% based on the total moles of BT repeating unit and ES repeating unit). Polyester composition V-A8 was obtained.
[0479] (Example V-9) The procedure of Example V-1 was followed, except that no iron oxide was added, to obtain polyester composition V-A9.
[0480] (Comparative example V-1) The method of Example V-1 was followed, except that 10 kg of polyester A used in Example V-1 and 1 kg of iron oxide were mixed without adding polyester B used in Example V-1. Composition V-D1 was obtained.
[0481] (Comparative Example V-2) The method of Example V-1 was followed, except that 10 kg of polyester B used in Example V-1 and 1 kg of iron oxide were mixed without adding polyester A used in Example V-1. Composition V-D2 was obtained.
[0482] (Comparative example V-3) The method of Example V-1 was followed, except that the polyester A used in Example V-1 was replaced with the same weight of PBT (trade name "Crastin SC164 NC010", purchased from DuPont). Composition V-D3 was obtained.
[0483] (Comparative Example V-4) The method of Example V-1 was followed, except that the same weight of PBT (trade name "Crastin SC164 NC010", purchased from DuPont) was used instead of the polyester B used in Example V-1. Composition V-D4 was obtained.
[0484] (Comparative example V-5) The procedure of Example V-1 was followed, except that the same weight of PBS (trade name "1111HTA4", purchased from BASF, the same applies below) was used instead of the polyester A used in Example V-1. Composition V-D5 was obtained.
[0485] (Comparative example V-6) The procedure of Example V-1 was followed, except that the same weight of PBS was used instead of the polyester B used in Example V-1, to obtain composition V-D6.
[0486] (Comparative example V-7) The procedure of Example V-1 was followed, except that the amount of polyester A was 3 kg and the amount of polyester B was 7 kg. Composition V-D7 was obtained.
[0487] (Comparative example V-8) The procedure of Example V-1 was followed, except that the amount of polyester A was 5 kg and the amount of polyester B was 5 kg. Composition V-D8 was obtained.
[0488] (Comparative example V-9) The procedure of Example V-1 was followed, except that 10 kg of PBT and 1 kg of iron oxide were mixed to obtain composition V-D9.
[0489] (Comparative example V-10) The method of Example V-1 was followed, except that 10 kg of PBS and 1 kg of iron oxide were mixed to obtain composition V-D10.
[0490] (Comparative example V-11) Medical grade calcium sulfate particles (Osteoset pellets, Wright, USA) were directly used as V-D11.
[0491] (Test Examples V-1 to V-20) 1.Shore A hardness test The materials obtained in Examples V-1 to V-9 and Comparative Examples V-1 to V-11 were melted and then treated at 170°C and 1000 MPa for 5 minutes and pressed into plates with a thickness of 4 mm and a side length of 7 cm. The hot plates were removed and quenched for 1 minute with a cold iron block that had been left at room temperature for a long time, and the zero time was recorded. The quenched plates were subjected to a test for Shore A hardness as a function of time (a Drick Shore A handheld durometer was used for the measurement and the measurement after 3 seconds was recorded). The results are shown in Table 5-1 below.
[0492] [Table 5]
[0493] As can be seen from the results of Table 5-1, the polyester compositions V-A1 to V-A9 obtained in Examples V-1 to V-9 had relatively low hardness (relatively high temperature) at the start of the test, and the hardness gradually increased with time after cooling. Nevertheless, the materials V-D1 to V-D11 obtained in Comparative Examples V-1 to V-11 had very high temperatures at the start of the test and did not change with time. In comparison, it was found that the polyester compositions V-A1 to V-A9 obtained in Examples V-1 to V-9 had good plasticity and fixation properties and were suitable for the manufacture of medical limb fixators.
[0494] 2.Water resistance test The materials obtained in Examples V-1 to V-9 and Comparative Examples V-1 to V-11 were melted, treated at 170°C and 1000 MPa for 5 minutes, and pressed into plates with a thickness of 2 mm and a side length of 7 cm. The plates were weighed, measured, photographed, and observed for their appearance. The plates were immersed in water at 25°C for 24 hours, removed, dried, observed, weighed, measured, photographed, and observed for their appearance. If the appearance of the plate after immersion in water did not change compared to the appearance before immersion in water, it was recorded as "no change", otherwise it was recorded as "changed". If the size of the plate after immersion in water changed within about ±2% compared to the size before immersion in water, it was recorded as "no change", otherwise it was recorded as "changed". If the weight of the board after immersion in water changed within about ±2% compared to before immersion in water, it was recorded as "no change", otherwise it was recorded as "changed". The results are shown in Table 5-2.
[0495] 3. Storage time test The materials obtained in Examples V-1 to V-9 and Comparative Examples V-1 to V-11 were melted, treated at 170°C and 1000 MPa for 5 minutes, and pressed into plates with a thickness of 2 mm and a side length of 7 cm. The plates were weighed, their size was measured, photographed, and their appearance was observed. Next, the obtained plates were left in a room temperature (25°C) and normal pressure environment for 2 years, and the plates were weighed, their size was measured, photographed, and their appearance was observed. If the appearance of the plate did not change after being left for 2 years compared to before being left, it was recorded as "no change", and if not, it was recorded as "changed". If the plate size did not change after being left for 2 years compared to before being left, it was recorded as "no change", and if not, it was recorded as "changed". If the weight of the plate after being left for 2 years changed within about ±2% compared to before being left, it was recorded as "no change", and if not, it was recorded as "changed". The results are shown in Table 5-2.
[0496] 4. X-ray transmittance test The materials obtained in Examples V-1 to V-9 and Comparative Examples V-1 to V-11 were melted, and then treated at 170°C and 1000MPa for 5 minutes, pressed to a thickness of 2 mm and a side length of 1 cm, and cut into a square plate. The cut plate was placed on a Bruker D8 Discovery 2D WAXD scatterometer and measured by a transmission method to obtain a scattering curve of the scattering intensity versus the scattering angle, and the peak area within a scattering angle of 5° to 30° was integrated, and the integral value was defined as Int-1. In addition, a small amount of water was added to the anhydrous calcium sulfate of Comparative Example V-11 to make a paste, and the paste was placed in a 1 cm x 1 cm square groove up to 2 mm from the bottom of the groove, and the mixture was left for about 15 minutes to make a 1 cm x 1 cm x 2 mm gypsum plate. The gypsum plate was subjected to X-ray scattering measurement in the same manner as above, and the obtained peak area integral value was defined as Int-2. When the value of Int-1 / Int-2 is greater than 10, it indicates that the sample has excellent X-ray transmittance and is recorded as "good"; when the ratio is between 2 and 10, it indicates that the sample has normal X-ray transmittance and is recorded as "normal"; when the ratio is less than 2, it indicates that the sample has no X-ray transmittance and is recorded as "no transmittance". The results are shown in Table 5-2.
[0497] [Table 6]
[0498] From the results of Table 5-2, it can be seen that the polyester composition of the present invention has good water resistance, does not require special packaging such as waterproof packaging during storage and transportation, and remains undegraded for at least two years at room temperature. It has a small weight, only about 1 / 5 of the weight of the conventional plate made of calcium sulfate, and at the same time, has excellent X-ray transmittance.
[0499] (Example V-10) The polyester composition V-A1 obtained in Example V-1 was melted and pressed at 170°C and 1000 MPa to obtain a plate having a thickness of 2 mm and a side length of 7 cm. While the plate was still hot, it was punched with a puncher having a diameter of 7 mm to make four holes evenly spaced apart. After about 1 hour, the plate was completely cured and could be used as a medical limb immobilization brace.
[0500] When in use, the medical limb immobilization brace was placed in hot water (about 100°C) for about 10 seconds to sufficiently soften the medical limb immobilization brace. The medical limb immobilization brace was then taken out, cooled in cold water until it was not too hot to the hand, dried, and wrapped around the limb (such as a finger) that needed to be immobilized, and gently pressed so that the medical limb immobilization brace conformed to the limb. After waiting for about 5 minutes, the medical limb immobilization brace was partially cured and fixed to conform to the shape of the limb. Large movements of the limb were avoided, and after waiting for about 30 minutes, the medical limb immobilization brace was fully cured to achieve the purpose of protecting and immobilizing the limb. A specific cured medical limb immobilization brace is shown in Figures 8 and 9.
[0501] If the fit between the hardened medical limb immobilization brace and the limb was not sufficient, the hardened medical limb immobilization brace was placed again in hot water at 100°C to soften it again, and then rewrapped around the part of the limb that required immobilization, so that it was shaped to fit the limb after hardening.
[0502] The above results show that the medical limb immobilization brace made by using the polyester composition provided by the present invention can be fully softened under high temperature conditions (e.g., in hot water, especially boiling water), and the softened material can be cut into appropriate sizes and shapes, wrapped around the part of the limb that needs to be immobilized, and then easily cut, hardened, and self-adhesive, thereby achieving good molding and immobilization purposes. Moreover, the process is reversible, and remolding can be achieved according to the part of the limb.
[0503] In addition, the medical limb immobilization brace was easy to remove and clean, and at the same time, since it did not use thermoplastic processing (no cross-linking agent), it had good degradability, and the remainder could be recycled and reused.
[0504] [Heat-shrinkable film] (Example VI-1) Under stirring conditions (stirring speed 30 r / min, 10 min), 2 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeat units is 35 mol% based on the total moles of BT repeat units and BS repeat units) particles, BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeat units is 15 mol% based on the total moles of BT repeat units and BS repeat units) particles, 0.5 kg of calcium carbonate, and 0.01 kg of erucylamide were mixed. Then, the mixture was extruded through a twin-screw extruder (the temperatures of various parts in the twin-screw extruder from the feed inlet to the extrusion outlet were continuously 170°C, 180°C, 190°C, 190°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VI-A1 was obtained.
[0505] The polyester composition VI-A1 pellets were passed through an injection molding machine and injection molded at 150° C. to obtain a film having a thickness of 0.2 mm. This film was left at room temperature (25° C.) for 10 hours, and then stretched to 5 times its original length at 60° C. in a uniaxial tensile machine to produce heat-shrinkable film VI-B1.
[0506] (Example VI-2) Under stirring conditions (stirring speed 30 r / min, 10 min), 1.8 kg of BT-BS copolyester A (weight average molecular weight 100,000, the content of BT repeat units is 38 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 1.2 kg of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeat units is 3 mol% based on the total number of moles of BT repeat units) particles, 0.5 kg of calcium carbonate, and 0.01 kg of erucylamide were mixed, then extruded through a twin-screw extruder (the temperatures of various parts in the twin-screw extruder from the feed inlet to the extrusion outlet were continuously 170°C, 180°C, 190°C, 190°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VI-A2 was obtained.
[0507] The polyester composition VI-A2 pellets were passed through an injection molding machine and injection molded at 150° C. to obtain a film having a thickness of 0.2 mm. This film was left at room temperature (25° C.) for 10 hours, and then stretched to 4.5 times its original length at 60° C. in a uniaxial tensile machine to produce a heat-shrinkable film VI-B2.
[0508] (Example VI-3) Under stirring conditions (stirring speed 30 r / min, 10 min), 2.7 kg of BT-BS copolyester A (weight average molecular weight 100,000, BT repeat unit content is 28 mol% based on the total moles of BT repeat units and BS repeat units) particles, 0.3 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 15 mol% based on the total moles of BT repeat units and BS repeat units) particles, 0.5 kg of calcium carbonate, and 0.01 kg of erucylamide were mixed, then extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts in the twin-screw extruder were continuously 170°C, 180°C, 190°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VI-A3 was obtained.
[0509] The polyester composition VI-A3 pellets were passed through an injection molding machine and injection molded at 150° C. to obtain a film having a thickness of 0.2 mm. This film was left at room temperature (25° C.) for 10 hours, and then stretched to 4 times its original length at 60° C. in a uniaxial tensile machine to produce heat-shrinkable film VI-B3.
[0510] (Example VI-4) Under stirring conditions (stirring speed 30 r / min, 10 min), 2.97 kg of BT-BS copolyester A (weight average molecular weight 100,000, BT repeat unit content 40 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 0.03 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content 20 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 0.5 kg of calcium carbonate, and 0.01 kg of erucylamide were mixed, then extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts of the twin-screw extruder were continuously set to 170°C, 180°C, 190°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VI-A4 was obtained.
[0511] The polyester composition VI-A4 pellets were passed through an injection molding machine and injection molded at 150° C. to obtain a film having a thickness of 0.2 mm. This film was left at room temperature (25° C.) for 10 hours, and then stretched to 4 times its original length at 60° C. in a uniaxial tensile machine to produce heat-shrinkable film VI-B4.
[0512] (Example VI-5) Under stirring conditions (stirring speed 30 r / min, 10 min), 1.53 kg of BT-BS copolyester A (weight average molecular weight 100,000, BT repeat unit content is 20 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 1.47 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 1 mol% based on the total number of moles of BT repeat units) particles, 0.5 kg of calcium carbonate, and 0.5 kg of erucylamide were mixed, then extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts of the twin-screw extruder were continuously set to 170°C, 180°C, 190°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VI-A5 was obtained.
[0513] The polyester composition VI-A5 pellets were passed through an injection molding machine and injection molded at 150° C. to obtain a film having a thickness of 0.2 mm. The film was left at room temperature (25° C.) for 10 hours, and then stretched to 1.5 times its original length at 60° C. in a uniaxial tensile machine to produce a heat-shrinkable film VI-B5.
[0514] (Example VI-6) The method of Example VI-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeating units is 35 mol% based on the total moles of BT repeating units and BA repeating units); polyester B was BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeating units is 15 mol% based on the total moles of BT repeating units and BA repeating units). Polyester composition VI-A6 and heat shrinkable film VI-B6 were obtained.
[0515] (Example VI-7) The method of Example VI-1 was followed, except that polyester A was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating units is 35 mol% based on the total moles of BT repeating units and ES repeating units); polyester B was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating units is 15 mol% based on the total moles of BT repeating units and ES repeating units). Polyester composition VI-A7 and heat shrinkable film VI-B7 were obtained.
[0516] (Example VI-8) The method of Example VI-1 was followed, except that polyester A was BT-BO (butylene oxalate) copolyester (weight average molecular weight 500,000, the content of BT repeating units is 35 mol% relative to the total mole number of BT repeating units and BO repeating units); polyester B was BT-ES copolyester (weight average molecular weight 500,000, the content of BT repeating units is 15 mol% relative to the total mole number of BT repeating units and ES repeating units). Polyester composition VI-A8 and heat shrinkable film VI-B8 were obtained.
[0517] (Example VI-9) The procedure of Example VI-1 was followed, except that 0.2 kg of carbon black and 0.2 kg of titanium dioxide were used instead of 0.5 kg of calcium carbonate and 0.01 kg of erucylamide used in Example VI-1, to obtain polyester composition VI-A9 and heat-shrinkable film VI-B9.
[0518] (Example VI-10) The method of Example VI-1 was followed, except that 0.5 kg of calcium carbonate and 0.01 kg of erucylamide were not added, to obtain polyester composition VI-A10 and heat-shrinkable film VI-B10.
[0519] (Comparative Example VI-1) The method of Example VI-1 was followed, except that Polyester A of Example VI-1 was directly produced into membrane VI-DB1 without the step of mixing with Polyester B of Example VI-1.
[0520] (Comparative Example VI-2) The method of Example VI-1 was followed, except that Polyester B of Example VI-1 was directly produced into membrane VI-DB2 without the step of mixing with Polyester A of Example VI-1.
[0521] (Comparative Example VI-3) The method of Example VI-1 was followed to prepare membrane VI-DB3, except that the same weight of PBT (trade name "Crastin SC164 NC010", purchased from DuPont, the same below) was used in place of the polyester A used in Example VI-1.
[0522] (Comparative Example VI-4) The procedure of Example VI-1 was followed, except that the same weight amount of PBT was used instead of the polyester B used in Example VI-1 to prepare membrane VI-DB4.
[0523] (Comparative Example VI-5) To prepare membrane VI-DB5, the method of Example VI-1 was followed, except that the same weight of PBS (trade name "1111HTA4", purchased from BASF, the same below) was used instead of the polyester A used in Example VI-1.
[0524] (Comparative Example VI-6) The method of Example VI-1 was followed, except that the same weight of PBS was used instead of the polyester B used in Example VI-1 to prepare membrane VI-DB6.
[0525] (Comparative Example VI-7) Membrane VI-DB7 was prepared according to the method of Example VI-1, except that the amount of Polyester A was 1 kg and the amount of Polyester B was 2 kg.
[0526] (Comparative Example VI-8) Membrane VI-DB8 was prepared according to the method of Example VI-1, except that the amount of Polyester A was 1.5 kg and the amount of Polyester B was 1.5 kg.
[0527] (Comparative Example VI-9) The procedure of Example VI-1 was followed except that the PBT was made directly into film VI-DB9.
[0528] (Comparative Example VI-10) The method of Example VI-1 was followed, except that PBS was directly applied to film VI-DB10.
[0529] (Test Examples VI-1 to VI-20) Heat shrinkage test: The films produced in Examples VI-1 to VI-10 and Comparative Examples VI-1 to VI-10 were each tested for heat shrinkage (%) by heating in a 70°C environment for 5 seconds with a Labthink Thermotek 2710 heat shrinkage instrument.
[0530] Heat seal strength test: after wrapping with 25μm polytetrafluoroethylene using Brugger Munchen HSG-C heat sealer, each two layers of the corresponding membrane were heat sealed at 90℃ under 100N pressure for 2 seconds, then the heat seal strength (N / 15mm) of the membranes prepared in Examples VI-1~VI-10 and Comparative Examples VI-1~VI-10 were tested respectively by Instron 5965 tensile tester (speed of 50mm / min) according to the test method of QB / T 2358-1998.
[0531] The biodegradability test of the films produced in Examples VI-1 to VI-10 and Comparative Examples VI-1 to VI-10 was carried out by the following method. Specifically, 18 g of compost (age 2 months) provided by the Beijing Nanjing Compost Factory was used, 3 g of the test film was added, and an appropriate amount of distilled water was added, mixed, appropriately stirred, and then left at room temperature (25°C). Whether the mass loss exceeded 50% in 3 months was the criterion for evaluating whether biodegradation was acceptable.
[0532] The results of the above tests are shown in Table 6.
[0533] Furthermore, the heat-shrinkable films obtained in Examples VI-1 to VI-10 could be stored for at least one year in a clean environment at room temperature and humidity without any obvious changes, and significant decomposition occurred only in the case of soil, eutrophication or compost.
[0534] [Table 7]
[0535] As can be seen from the results in Table 6, the present invention can obtain a heat shrinkable film having a heat shrinkage rate of 70% or more, and by mixing a specific copolymer (polyester A and polyester B) in a specific ratio (polyester A content is 51-99% by weight, polyester B content is 1-49% by weight), a film having a heat shrinkage rate of 10% can be obtained, which shows that the present invention can change the heat shrinkage rate of the film in a wide range by adjusting the blending and polyester structure. Furthermore, the heat shrinkable film obtained by the present invention has a suitable heat seal strength (up to 11-19N / 15mm), the film has a flat surface and good gloss, is degradable, and can be repeatedly thermoplastically processed and recycled, and therefore has obvious environmentally friendly advantages and industrial application prospects.
[0536] [Nonwoven fabric base material] Example VII-1 Under stirring conditions (stirring speed 30r / min, 10 min), 3 kg of BT-BS copolyester A (weight average molecular weight 120,000, BT repeat unit content is 18 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 2 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 50 mol% based on the total number of moles of BT repeat units) particles, and 0.25 kg of antioxidant 300 (hindered phenol antioxidant manufactured by the Material Synthesis Laboratory of the University of Chemical Technology, the same below) were mixed, stretched through a twin-screw extruder (the temperatures of various parts of the twin-screw extruder from the feed port were continuously set to 170°C, 180°C, 185°C, 185°C, 190°C, 190°C), air-cooled, and pelletized. Polyester composition VII-A1 was obtained.
[0537] The polyester polymer VII-A1 was added to the screw of a spunbonding machine (the temperature of the first section of the screw was 185°C, the temperature of the second section was 190°C, the temperature of the third section was 205°C, the spinning temperature was 195°C, the rotation speed of the metering pump was 20r / min, the web forming speed was 17m / min, and the hot rolling temperature was 105°C) to obtain nonwoven fabric VII-B1.
[0538] (Example VII-2) Under stirring conditions (stirring speed 30 r / min, 10 min), 3.5 kg of BT-BS copolyester A (weight average molecular weight 120,000, BT repeat unit content is 5 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 1.5 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 60 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, and 0.25 kg of antioxidant 300 were mixed, extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts of the twin-screw extruder were continuously set to 170°C, 180°C, 185°C, 185°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VII-A2 was obtained.
[0539] The polyester polymer VII-A2 was added to the screw of a spunbonding machine (the temperature of the first section of the screw was 185°C, the temperature of the second section was 190°C, the temperature of the third section was 205°C, the spinning temperature was 195°C, the rotation speed of the metering pump was 20r / min, the web forming speed was 17m / min, and the hot rolling temperature was 105°C) to obtain nonwoven fabric VII-B2.
[0540] (Example VII-3) Under stirring conditions (stirring speed 30 r / min, 10 min), 2.75 kg of BT-BS copolyester A (weight average molecular weight 120,000, BT repeat unit content is 12 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 30 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, and 0.25 kg of antioxidant 300 were mixed, extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts of the twin-screw extruder were continuously set to 170°C, 180°C, 185°C, 185°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VII-A3 was obtained.
[0541] The polyester polymer VII-A3 was added to the screw of a spunbonding machine (the temperature of the first section of the screw was 185°C, the temperature of the second section was 190°C, the temperature of the third section was 205°C, the spinning temperature was 195°C, the rotation speed of the metering pump was 20r / min, the web forming speed was 17m / min, and the hot rolling temperature was 105°C) to obtain nonwoven fabric VII-B3.
[0542] (Example VII-4) Under stirring conditions (stirring speed 30 r / min, 10 min), 4.95 kg of BT-BS copolyester A (weight average molecular weight 120,000, BT repeat unit content is 25 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 0.05 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 80 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, and 0.25 kg of antioxidant 300 were mixed, extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts in the twin-screw extruder were continuously set to 170°C, 180°C, 185°C, 185°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VII-A4 was obtained.
[0543] The polyester polymer VII-A4 was added to the screw of a spunbonding machine (the temperature of the first section of the screw was 185°C, the temperature of the second section was 190°C, the temperature of the third section was 205°C, the spinning temperature was 195°C, the rotation speed of the metering pump was 20r / min, the web forming speed was 17m / min, and the hot rolling temperature was 105°C) to obtain nonwoven fabric VII-B4.
[0544] (Example VII-5) Under stirring conditions (stirring speed 30 r / min, 10 min), 2.55 kg of BT-BS copolyester A (weight average molecular weight 120,000, BT repeat unit content is 1 mol% based on the total moles of BT repeat units and BS repeat units) particles, 2.45 kg of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 26 mol% based on the total moles of BT repeat units and BS repeat units) particles, and 0.25 kg of antioxidant 300 were mixed, extruded through a twin-screw extruder (from the feed inlet to the extrusion outlet, the temperatures of various parts in the twin-screw extruder were continuously set to 170°C, 180°C, 185°C, 185°C, 190°C, 190°C), stretched, air-cooled, and pelletized. Polyester composition VII-A5 was obtained.
[0545] The polyester polymer VII-A5 was added to the screw of a spunbonding machine (the temperature of the first section of the screw was 185°C, the temperature of the second section was 190°C, the temperature of the third section was 205°C, the spinning temperature was 195°C, the rotation speed of the metering pump was 20r / min, the web forming speed was 17m / min, and the hot rolling temperature was 105°C) to obtain nonwoven fabric VII-B5.
[0546] (Example VII-6) The method of Example VII-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 120,000, the content of BT repeat unit is 18 mol% based on the total moles of BT repeat unit and BA repeat unit); polyester B was BT-BA copolyester (weight average molecular weight 100,000, the content of BT repeat unit is 50 mol% based on the total moles of BT repeat unit and BA repeat unit). Polyester composition VII-A6 and nonwoven fabric VII-B6 were obtained.
[0547] (Example VII-7) The method of Example VII-1 was followed, except that polyester A was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating unit is 18 mol% based on the total moles of BT repeating unit and ES repeating unit); polyester B was BT-ES copolyester (weight average molecular weight 200,000, the content of BT repeating unit is 50 mol% based on the total moles of BT repeating unit and ES repeating unit). Polyester composition VII-A7 and nonwoven fabric VII-B7 were obtained.
[0548] (Example VII-8) The method of Example VII-1 was followed, except that polyester A was BT-BO copolyester (weight average molecular weight 500,000, the content of BT repeating unit is 18 mol% based on the total mole number of BT repeating unit and BO repeating unit); polyester B was BT-ES copolyester (weight average molecular weight 500,000, the content of BT repeating unit is 50 mol% based on the total mole number of BT repeating unit and ES repeating unit). Polyester composition VII-A8 and nonwoven fabric VII-B8 were obtained.
[0549] (Example VII-9) The method of Example VII-1 was followed, except that 0.25 kg of titanium dioxide was used instead of 0.25 kg of antioxidant 300 used in Example VII-1, to obtain polyester composition VII-A9 and nonwoven fabric VII-B9.
[0550] (Example VII-10) The method of Example VII-1 was followed, except that 0.25 kg of antioxidant 300 was not added. A polyester composition VII-A10 and a heat-shrinkable film VII-B10 were obtained.
[0551] (Comparative Example VII-1) The method of Example VII-1 was followed, except that Polyester A of Example VII-1 was directly manufactured into nonwoven fabric VII-DB1 without the step of blending Polyester A of Example VII-1 with Polyester B of Example VII-1.
[0552] (Comparative Example VII-2) The method of Example VII-1 was followed, except that Polyester B of Example VII-1 was directly manufactured into nonwoven fabric VII-DB2 without the step of blending Polyester B of Example VII-1 with Polyester A of Example VII-1.
[0553] (Comparative Example VII-3) The method of Example VII-1 was followed, except that the same weight of PBT (trade name "Crastin SC164 NC010", purchased from DuPont, the same below) was used instead of the polyester A used in Example VII-1 to obtain nonwoven fabric VII-DB3.
[0554] (Comparative Example VII-4) A nonwoven fabric VII-DB4 was obtained according to the method of Example VII-1, except that the same weight of PBT was used instead of the polyester B used in Example VII-1.
[0555] (Comparative Example VII-5) To obtain nonwoven fabric VII-DB5, the method of Example VII-1 was followed, except that the polyester A used in Example VII-1 was replaced with the same weight of PBS (trade name "1111HTA4", purchased from BASF, the same below).
[0556] (Comparative Example VII-6) A nonwoven fabric VII-DB6 was obtained according to the method of Example VII-1, except that the same weight of PBS was used instead of the polyester B used in Example VII-1.
[0557] (Comparative Example VII-7) Nonwoven fabric VII-DB7 was obtained according to the method of Example VII-1, except that the amount of Polyester A was 2 kg and the amount of Polyester B was 3 kg.
[0558] (Comparative Example VII-8) A membrane VII-DB8 was obtained according to the method of Example VII-1, except that the amount of Polyester A was 2.5 kg and the amount of Polyester B was 2.5 kg.
[0559] (Comparative Example VII-9) The method of Example VII-1 was followed, except that nonwoven fabric VII-DB9 was made directly from PBT.
[0560] (Comparative Example VII-10) The method of Example VII-1 was followed, except that nonwoven fabric VII-DB10 was prepared directly from PBS.
[0561] (Test Examples VII-1 to VII-20) The water absorption test was verified by two methods, namely, the nonwoven fabric water drop test and the material itself water contact angle test. The specific test methods were as follows:
[0562] Water Drop Test: Deionized water was dropped onto the surface of the obtained nonwoven fabric with a pipette. If the water droplet penetrated through the nonwoven fabric without any hindrance, the result was recorded as "penetrated". If the water droplet floated on the surface and maintained a good shape (similar to the water droplet on the surface of a lotus leaf), the result was recorded as "drop".
[0563] Contact angle test: The compositions obtained in each Example or Comparative Example were pressed into a 70 mm x 70 mm x 1 mm plate at 170°C and a pressure of 4000 kg. Then, deionized water was carefully dropped onto the surface of the pressed plate using a pipetting gun, the shape of the water droplet was photographed from the macro mode side of the camera, and the contact angle of the water droplet with respect to the material surface was read from the photograph. When the contact angle was less than 90°, the result was recorded as "hydrophilic", and when the contact angle was greater than 90°, the result was recorded as "hydrophobic".
[0564] Gas permeability test: The balloon was pushed into a capillary tube with an inner diameter of about 1 mm, and the balloon was filled with gas to the same size. The balloon was allowed to freely shrink through the capillary tube, and the time was recorded as t1. Then, a small piece of nonwoven fabric of the example or comparative example was used to block the mouth of the capillary tube, and the time it took to empty was tested and recorded as t2. If t2 was less than 2×t1, the result was recorded as “gas permeable”, otherwise the result was recorded as “gas impermeable”.
[0565] Ethanol tolerance test: The ethanol tolerance test was used to show whether the nonwoven fabric reacts with ethanol or dissolves in ethanol during ethanol sterilization (reflecting the ease of sterilization of the nonwoven fabric). Specifically, a 2g nonwoven fabric sample was placed in 75vol% ethanol and left at room temperature for 24 hours, then air-dried, its surface was observed, and it was weighed. When the sample simultaneously met the conditions of (1) no obvious change in appearance and (2) weight of 99% or more of the original weight, the result was recorded as "resistant", otherwise the result was recorded as "unstable".
[0566] Heat shrinkage test: 10 cm x 10 cm pieces of nonwoven fabric were placed in hot water (80°C, 90°C, 95°C) for 10 seconds, then removed and the size was measured. The area of the shrunken part of the nonwoven fabric was calculated as a percentage of the initial area.
[0567] The results of the water drop test, contact angle test, gas permeability test, ethanol resistance test and heat shrinkage test are shown in Tables 7-1 and 7-2.
[0568] [Table 8]
[0569] [Table 9]
[0570] (Test Examples VII-1 to VII-20) Disposable surgical gowns were prepared from each of the nonwoven fabrics produced in Examples VII-1 to VII-10 and Comparative Examples VII-1 to VII-10, and the disposable surgical gowns discarded after clinical use were immersed in boiling water for sterilization.
[0571] It was found that the disposable surgical gowns manufactured from the nonwoven fabrics VII-B1 to VII-B10 obtained in Examples VII-1 to VII-10 were greatly shrunk in boiling water, and the volume was significantly reduced, facilitating regeneration. Furthermore, the recovered starting material was added to a spunbond machine as a raw material for making a nonwoven fabric, and a new nonwoven fabric was obtained according to the conditions of the spunbond method in Example VII-1. It was also found that the newly obtained nonwoven fabric had similar properties to the nonwoven fabrics VII-B1 to VII-B10 manufactured in Examples VII-1 to VII-10, and was suitable for continued function as a starting material for disposable medical textiles, and that material recycling was achieved.
[0572] The disposable surgical gowns made from the nonwoven fabrics VII-DB1 to VII-DB10 obtained in Comparative Examples VII-1 to VII-10 have almost no change in volume in boiling water, which makes the recycling process very complicated. Furthermore, the recovered starting materials were added to a spunbond machine as raw materials for making nonwoven fabrics, and new nonwoven fabrics were obtained according to the conditions of the spunbond method in Example VII-1. It was found that some could not be molded well, while others did not have good heat shrinkage properties and were not suitable to continue to serve as starting materials for disposable medical textiles.
[0573] As can be seen from the results of the above Test Examples VII-1 to VII-20 and Test Examples VII-1 to VII-20, the nonwoven fabric of the present invention obtained by mixing a specific copolymer (polyester A and polyester B) in a specific ratio (the content of polyester A was 51 to 99% by weight, and the content of polyester B was 1 to 49% by weight) has good water absorption, gas permeability and easy sterilization, in particular, the nonwoven fabric of the present invention can be disinfected in hot water (e.g., 100°C), they can be easily compressed into a small volume, and the material (especially the disposable remanufactured nonwoven fabric) has similar properties to the nonwoven fabric originally used, and is suitable for continuing to function as a starting material for disposable nonwoven fabric articles (especially disposable medical textile articles), thereby fully solving the problem of recycling materials.
[0574] [Elastic fiber] (Example VIII-1) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 150 g of BT-BS copolyester A (weight average molecular weight 130,000, the content of BT repeat units is 30 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 30 g of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeat units is 10 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 20 g of BT-BA copolyester C (weight average molecular weight 100,000, the content of BT repeat units is 60 mol% relative to the total number of moles of BT repeat units and BA repeat units) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder, melt extruded at a temperature of 220 ° C, and pelletized to obtain polyester composition VIII-A1.
[0575] (2) Manufacturing of elastic fibers The polyester polymer VIII-A1 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, an elastic fiber VIII-B1 was obtained.
[0576] (Example VIII-2) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 186 g of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit 30 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 12 g of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit 10 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content 60 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder and pelletized at a temperature of 220 ° C. to obtain polyester composition VIII-A2.
[0577] (2) Manufacturing of elastic fibers The polyester polymer VIII-A2 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, an elastic fiber VIII-B2 was obtained.
[0578] (Example VIII-3) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 120 g of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content is 40 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 40 g of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 17 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 40 g of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 85 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder, melt extruded at a temperature of 220 ° C, and pelletized to obtain polyester composition VIII-A3.
[0579] (2) Manufacturing of elastic fibers The polyester polymer VIII-A3 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, an elastic fiber VIII-B3 was obtained.
[0580] (Example VIII-4) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 120 g of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content is 25 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 70 g of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 5 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 10 g of BT-BS copolyester C (weight average molecular weight 100,000, BT repeat unit content is 55 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder, melt extruded at a temperature of 220 ° C, and pelletized to obtain polyester composition VIII-A4.
[0581] (2) Manufacturing of elastic fibers The polyester polymer VIII-A4 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, an elastic fiber VIII-B4 was obtained.
[0582] (Example VIII-5) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 60 g of BT-BS copolyester A (weight average molecular weight 130,000, the content of BT repeating units is 49 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 138 g of BT-BS copolyester B (weight average molecular weight 100,000, the content of BT repeating units is 19 mol% relative to the total number of moles of BT repeating units and BS repeating units) particles, 2 g of PBT (trade name "Crastin SC164 NC010", purchased from DuPont) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder, melt extruded at a temperature of 220 ° C, and pelletized to obtain polyester composition VIII-A5.
[0583] (2) Manufacturing of elastic fibers The polyester polymer VIII-A5 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, an elastic fiber VIII-B5 was obtained.
[0584] (Example VIII-6) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 60 g of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content is 20 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, 2 g of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 51 mol% based on the total number of moles of BT repeat units and BS repeat units) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder, melt extruded at a temperature of 220°C, and pelletized to obtain polyester composition VIII-A6.
[0585] (2) Manufacturing of elastic fibers The polyester polymer VIII-A6 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, an elastic fiber VIII-B6 was obtained.
[0586] (Example VIII-7) (1) Production of polyester composition Under stirring conditions (stirring speed 10 r / min, 10 min), 196 g of BT-BS copolyester A (weight average molecular weight 130,000, BT repeat unit content is 30 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 2 g of BT-BS copolyester B (weight average molecular weight 100,000, BT repeat unit content is 10 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, 2 g of BT-BS copolyester C (weight average molecular weight 100,000, BT repeat unit content is 60 mol% relative to the total number of moles of BT repeat units and BS repeat units) particles, and 10 g of titanium dioxide were mixed and stirred at a speed of 10 r / min for 10 min. The mixture was added to a twin-screw extruder, melt extruded at a temperature of 220 ° C, and pelletized to obtain polyester composition VIII-A7.
[0587] (2) Manufacturing of elastic fibers The polyester polymer A7 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 40° C. for 60 minutes, then heated to 70° C. and stretched to 4 times its original length. After cooling, elastic fiber VIII-B7 was obtained.
[0588] (Example VIII-8) The method of Example VIII-1 was followed, except that polyester A was BT-BA copolyester (weight average molecular weight 130,000, the content of BT repeating unit is 30 mol% relative to the total moles of BT repeating unit and BA repeating unit); polyester B was BT-ES polyester (weight average molecular weight 100,000, the content of BT repeating unit is 10 mol% relative to the total moles of BT repeating unit and ES repeating unit); and polyester C was BT-ES ester (weight average molecular weight 100,000, the content of BT repeating unit is 60 mol% relative to the total moles of BT repeating unit and ES repeating unit). Polyester composition VIII-A8 and elastic fiber VIII-B8 were obtained.
[0589] (Example VIII-9) The method of Example VIII-1 was followed, except that polyester A was BT-ES copolyester (weight average molecular weight 130,000, the content of BT repeating unit is 30 mol% relative to the total moles of BT repeating unit and ES repeating unit); polyester B was BT-BA ester (weight average molecular weight 100,000, the content of BT repeating unit is 10 mol% relative to the total moles of BT repeating unit and BA repeating unit); and polyester C was BT-BA ester (weight average molecular weight 100,000, the content of BT repeating unit is 60 mol% relative to the total moles of BT repeating unit and BA repeating unit). Polyester composition VIII-A9 and elastic fiber VIII-B9 were obtained.
[0590] (Example VIII-10) The procedure of Example VIII-1 was followed, except that the titanium dioxide of Example VIII-1 was replaced with the same weight of calcium carbonate, to obtain polyester composition VIII-A10 and elastic fiber VIII-B10.
[0591] (Example VIII-11) The method of Example VIII-1 was followed, except that 10 g of titanium dioxide was not added. Polyester composition VIII-A11 and elastic fiber VIII-B11 were obtained.
[0592] (Example VIII-12) (1) Production of polyester composition According to the method of Example VIII-1, a polyester composition VIII-A1 was obtained.
[0593] (2) Manufacturing of elastic fibers The polyester polymer VIII-A1 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 55° C. for 120 minutes, then heated to 110° C. and stretched to 10 times its original length. After cooling, an elastic fiber VIII-B12 was obtained.
[0594] (Example VIII-13) (1) Production of polyester composition According to the method of Example VIII-1, a polyester composition VIII-A1 was obtained.
[0595] (2) Manufacturing of elastic fibers The polyester polymer VIII-A1 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170° C. The fiber was placed at 20° C. for 2 minutes, then heated to 56° C. and stretched to 1.2 times its original length. After cooling, an elastic fiber VIII-B13 was obtained.
[0596] (Example VIII-14) (1) Production of polyester composition According to the method of Example VIII-1, a polyester composition VIII-A1 was obtained.
[0597] (2) Manufacturing of elastic fibers The polyester polymer VIII-A1 was spun into a fiber having a fiber count of 72 dtex by melt spinning at 170°C, and then the temperature was directly lowered to 70°C without the step of leaving the fiber at 40°C as in Example VIII-1, and the fiber was stretched to 4 times its original length. After cooling, elastic fiber VIII-B14 was obtained.
[0598] (Comparative Example VIII-1) The method of Example VIII-1 was followed, except that 150g of polyester A used in Example VIII-1, 50g of polyester B used in Example VIII-1, and 10g of titanium dioxide were mixed without adding polyester C used in Example VIII-1. Polyester composition VIII-DA1 and elastic fiber VIII-DB1 were obtained.
[0599] (Comparative Example VIII-2) The method of Example VIII-1 was followed, except that 150g of polyester A used in Example VIII-1, 50g of polyester C used in Example VIII-1, and 10g of titanium dioxide were mixed without adding polyester B used in Example VIII-1. Polyester composition VIII-DA2 and elastic fiber VIII-DB2 were obtained.
[0600] (Comparative Example VIII-3) The method of Example VIII-1 was followed, except that 120g of polyester B used in Example VIII-1, 80g of polyester C used in Example VIII-1, and 10g of titanium dioxide were mixed without adding polyester A used in Example VIII-1. Polyester composition VIII-DA3 and elastic fiber VIII-DB3 were obtained.
[0601] (Comparative Example VIII-4) The method of Example VIII-1 was followed, except that in step (1), 20g of polyester A used in Example VIII-1, 160g of polyester B used in Example VIII-1, 20g of polyester C used in Example VIII-1, and 10g of titanium dioxide were mixed. Polyester composition VIII-DA4 and elastic fiber VIII-DB4 were obtained.
[0602] (Comparative Example VIII-5) The same weight of PBS (trade name "1111HTA4", purchased from BASF) was used in place of the polyester A used in Example VIII-1 in step (1) in the same manner as in Example VIII-1, to obtain polyester composition VIII-DA5 and elastic fiber VIII-DB5.
[0603] (Comparative Example VIII-6) The same weight of PBS (trade name "1111HTA4", purchased from BASF) was used in place of the polyester B used in Example VIII-1 in step (1) in the same manner as in Example VIII-1 to obtain polyester composition VIII-DA6 and elastic fiber VIII-DB6.
[0604] (Comparative Example VIII-7) The method of Example VIII-1 was followed, except that in step (1), the same weight of PBA was used instead of the polyester C used in Example VIII-1. The method of producing PBA consisted of the following steps: in a nitrogen atmosphere, adipic acid and butanediol were stirred and reacted at 240°C in the presence of both tetrabutyl titanate and lanthanum acetylacetonate; the ratio of adipic acid, butanediol, tetrabutyl titanate and lanthanum acetylacetate in VIII- was 1800:2000:1:1; after 2 hours of reaction, the system was evacuated for 30 minutes until the pressure was stable at 100 Pa; the material remaining in the system was the product. Polyester composition VIII-DA7 and elastic fiber VIII-DB7 were obtained.
[0605] (Comparative Example VIII-8) The method of Example VIII-1 was followed, except that in step (1), 200g of polyester A used in Example VIII-1 was mixed with 10g of titanium dioxide to obtain polyester composition VIII-DA8 and elastic fiber VIII-DB8.
[0606] (Comparative Example VIII-9) The method of Example VIII-1 was followed, except that in step (1), 200g of polyester B used in Example VIII-1 and 10g of titanium dioxide were mixed to obtain polyester composition VIII-DA9 and elastic fiber VIII-DB9.
[0607] (Comparative Example VIII-10) The method of Example VIII-1 was followed, except that in step (1), 200g of polyester C used in Example VIII-1 was mixed with 10g of titanium dioxide. Polyester composition VIII-DA10 and elastic fiber VIII-DB10 were obtained.
[0608] (Test Examples VIII-1 to VIII-24) The elastic fibers obtained in Examples VIII-1 to VIII-14 and Comparative Examples VIII-1 to VIII-10 were evaluated for breaking strength, breaking elongation, stress relaxation, and permanent set rate by the following methods. The results are shown in Table 8.
[0609] Specifically, a 2 cm long (L1) sample was stretched to twice its original length (100% strain) at a rate of 50 mm / min in an Instron 5965 tensile tester, the stress at this time being designated as E1. This length was then maintained for 20 seconds, after which the stress at this time was recorded as E2. The strain was then decreased until the stress was zero, at which point the sample length was L2. It was then stretched at a rate of 50 mm / min until break, at which point the sample length was L3 and the stress value was E3. The formulas for calculating the above parameters were as follows: Breaking strength = E3 Elongation at break % = 100% × (L3-L1) / L1 Stress relaxation rate% = 100% × (E1-E2) / E1 Permanent strain rate %=100%×(L2-L1) / L1.
[0610] [Table 10]
[0611] As can be seen from the results in Table 8 above, the elastic fiber produced using the polyester composition of the present invention obtained by mixing specific polyester A, polyester B, and polyester C in a specific ratio (30-98% by weight of polyester A, 1-69% by weight of polyester B, and 1-69% by weight of polyester C) has good elastic properties, and the breaking strength is ≧1 cN / dtex, which can be changed in a wide range by adjusting the blending and molecular structure, and the maximum breaking strength is close to 20 cN / dtex. Furthermore, the breaking elongation of the elastic fiber provided by the present invention is as high as 130% or more, and the stress relaxation and permanent set rate are ≦12%, so that the elastic fiber provided by the present invention has both moderate elasticity and strength, and the properties can be adjusted in a wide range, and therefore has good application prospects.
[0612] Also, by comparing the results of Example VIII-1 with Examples VIII-12 to VIII-14, it is clear that the present invention, by using the method and conditions of high temperature filamentation-low temperature placement-high temperature drawing, specifically produces elastic fibers, which can further improve the breaking strength of elastic fibers, extend the adjustable range of properties, and reduce the stress relaxation and permanent set rate of elastic fibers.
[0613] The ranges and any value endpoints disclosed herein are not limited to the exact ranges or values, and these ranges or values should be understood to include the values close to the ranges or values.For numerical ranges, combinations can be made between the endpoints of various ranges, between the endpoints of various ranges and individual single-point values, and between individual single-point values and individual single-point values to obtain one or more new numerical ranges.These numerical ranges should be considered as specifically disclosed herein.
[0614] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited thereto. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, including combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the disclosure of the present invention, and all are within the protection scope of the present invention.
[0615] Furthermore, various different embodiments of the present invention can be randomly combined with each other, and such combinations are also considered as the disclosure of the present invention, as long as they do not deviate from the spirit of the present invention.
Claims
1. A polyester composition comprising at least two polyesters, the at least two polyesters being selected from the group consisting of: (1) a first polyester which is one or more selected from aliphatic-aromatic copolyesters, A copolymer consisting of a repeating unit A represented by formula (I) and a repeating unit B represented by formula (II), [Case 1] In the formula, the content of the repeating unit A is 51 to 95 mol %, the content of the repeating unit B is 5 to 49 mol %, and preferably, the content of the repeating unit A is 55 to 80 mol %, and the content of the repeating unit B is 20 to 45 mol %, based on the total molar amount of the repeating unit A and the repeating unit B in the aliphatic-aromatic copolyester; m is an integer of 2 to 10, preferably 2 to 6, more preferably 2 to 4; n is an integer of 2 to 8, preferably 2 to 4; p is an integer of 2 to 10, preferably 2 to 4; m, n and p are the same or different from each other, a first polyester, wherein the aliphatic-aromatic copolyester as the first polyester is a random copolymer; (2) a second polyester which is (i) an aliphatic polyester and an aliphatic-aromatic copolyester different from the first polyester, or (ii) an aliphatic-aromatic copolyester different from the first polyester; The aliphatic polyester comprises a repeat unit D represented by formula (I'"), [Case 2] In the formula, m3 is the same as defined for m; n3 is the same as defined for n; and n3 are the same or different from each other, and the aliphatic polyester has a weight average molecular weight of 50,000 to 900,000 as measured by GPC; a second polyester, the aliphatic-aromatic copolyester different from the first polyester, consisting of the repeating unit A represented by formula (I) and the repeating unit B represented by formula (II); The content of the first polyester is 51 to 99% by weight based on the total weight of the first polyester and the second polyester, The content of the second polyester is 1 to 49% by weight based on the total weight of the first polyester and the second polyester. Polyester composition.
2. 2. The polyester composition according to claim 1, wherein the aliphatic polyester has a weight average molecular weight of 100,000 to 500,000 as measured by GPC.
3. 2. The polyester composition according to claim 1, characterized in that the weight average molecular weight of the aliphatic-aromatic copolyester as the first polyester or the second polyester is 50,000 to 900,000, preferably 100,000 to 500,000, as measured by GPC, and the molecular weight distribution, preferably measured by GPC, is 1.2 to 3.
4. 2. The polyester composition according to claim 1, wherein the aliphatic-aromatic copolyester as the second polyester is a random copolymer, an alternating copolymer, a block copolymer or a graft copolymer.
5. 2. The polyester composition according to claim 1, characterized in that the polyester composition further comprises one or more additives selected from the group consisting of nucleating agents, fibrous fillers, auxiliary fillers that have the functions of accelerating solidification of the composition melt, adjusting the mechanical strength of the composition, adjusting the color and gloss of the composition, and improving the flame retardancy and oxidation resistance of the composition, and white oil.
6. the auxiliary filler is at least one, preferably at least two, selected from the group consisting of carbonates, silicates, sulfates, inorganic hollow microspheres, metal powders, carbon black, talc, erucylamide, titanium dioxide, iron oxide, metal carboxylates, metal phosphates, tetrabromobisphenol A, decabromodiphenyl ether, hexabromocyclododecane, low-density polyethylene, polyphosphates or polyphosphates, phosphites, hindered phenols, hindered amines, dibenzyl sorbitol and derivatives thereof, highly branched polyamides, ethylene-methacrylic acid ionomers, ethylene bisstearamide, silicone powders, and pentaerythritol stearate; Preferably, at least one, preferably at least two, selected from the group consisting of calcium carbonate, anhydrous calcium sulfate, copper powder, iron oxide, carbon black, titanium dioxide, tris(2,3-dibromopropyl)phosphate, low-density polyethylene, highly branched polyamide, ethylene bisstearamide, and erucylamide; 6. The polyester composition according to claim 5, characterized in that the content of said auxiliary filler is preferably from 0.1 to 60% by weight, preferably from 0.1 to 50% by weight, more preferably from 1 to 25% by weight, more preferably from 1 to 20% by weight, even more preferably from 2 to 10% by weight, relative to the total weight of the polyester composition.
7. the nucleating agent is one or more selected from the group consisting of talc, calcium oxide, carbon black, calcium carbonate, inorganic pigments, kaolin, metal carboxylates, metal phosphates, dibenzyl sorbitol and derivatives thereof, polyvinylcyclohexane, polyvinylcyclopentane, low density polyethylene, highly branched polyamides, and ethylene-methacrylic acid ionomers; Preferably, it is one or more selected from the group consisting of calcium carbonate, low-density polyethylene, dibenzyl sorbitol and its derivatives, and hyperbranched polyamides; 6. The polyester composition according to claim 5, characterized in that the content of said nucleating agent is preferably between 0.01 and 20% by weight, preferably between 0.2 and 5% by weight, relative to the total weight of said polyester composition.
8. The fiber filler is one or more selected from the group consisting of carbon fiber, glass fiber, basalt fiber, aramid fiber, and PET fiber; Preferably, it is one or more selected from the group consisting of glass fiber, carbon fiber, and basalt fiber; A polyester composition according to claim 5, characterised in that the length of said fibrous fillers is preferably between 0.1 and 10 mm, preferably between 0.5 and 2 mm.
9. The at least two polyesters consist of: (1) Polyester A, which is a copolymer consisting of a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1); (2) Polyester B, which is a copolymer consisting of a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1); (3) The aliphatic polyester as defined in claim 1; Includes [C3] In the formula, m1 and m2 are each independently the same as defined for m in claim 1, n1 and n2 are each independently the same as defined for n in claim 1, m1 and n1 are the same or different from each other, m2 and n2 are the same or different from each other, and n1 is less than n2; The polyester composition according to any one of claims 1 to 8, wherein the content of the repeating unit B is 5 to 49 mol%, preferably 10 to 45 mol%, and more preferably 20 to 40 mol%, based on the total number of moles of the polyester A, the polyester B, and the aliphatic polyester.
10. the content of the repeating unit A is 51 to 90 mol % and the content of the repeating unit B is 10 to 49 mol % based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; The polyester composition according to claim 9, wherein the content of the repeating unit C is 40 to 95 mol %, preferably 50 to 90 mol %, and the content of the repeating unit B is 5 to 60 mol %, preferably 10 to 50 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B.
11. The polyester composition according to claim 9 or 10, characterized in that the molar ratio of the polyester A, the polyester B and the aliphatic polyester is 20-90:1-90:1-20, preferably 20-90:1-70:1-20.
12. The at least two polyesters consist of: (1) 51 to 98% by weight of polyester A, which is a copolymer consisting of a repeating unit A represented by formula (I-1) and a repeating unit B represented by formula (II-1), a polyester A, in which the content of the repeating unit A is 56 to 80 mol %, preferably 60 to 75 mol %, and the content of the repeating unit B is 20 to 44 mol %, preferably 25 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; [C4] (2) 1 to 48% by weight of polyester B, which is a copolymer consisting of a repeating unit C represented by formula (I') and a repeating unit D' represented by formula (IV'), the content of the repeating unit C in the polyester B is 81 to 99 mol %, preferably 85 to 95 mol %, and the content of the repeating unit D' is 1 to 19 mol %, preferably 5 to 15 mol %, based on the total number of moles of the repeating unit C and the repeating unit D' in the polyester B; [C5] Polyester B, wherein m1 is as defined for m in claim 1, n1 is as defined for n in claim 1, m1 and n1 are the same or different from each other, a1 is as defined for p in claim 1, and a1 and m1 are the same or different from each other; (3) A polyester C which is a copolymer consisting of a repeating unit E represented by formula (I″) and a repeating unit F represented by formula (IV″), the content of the repeating unit E in the polyester C is 0 to 50 mol %, preferably 15 to 50 mol %, and the content of the repeating unit F in the polyester C is 50 to 100 mol %, preferably 50 to 85 mol %, based on the total number of moles of the repeating unit E and the repeating unit F; [C6] Polyester C, wherein m2 is as defined for m in claim 1, n2 is as defined for n in claim 1, m2 and n2 are the same or different from each other, a2 is as defined for p in claim 1, and a2 and m2 are the same or different from each other; The polyester composition comprises, relative to the total weight of the various components: 51 to 98% by weight of the polyester A; 1 to 48% by weight of said polyester B; 1 to 48% by weight of the polyester C; The polyester composition according to any one of claims 1 to 8, comprising:
13. 13. The polyester composition of claim 12, wherein the polyester composition comprises 70 to 94% by weight of the polyester A, 3 to 25% by weight of the polyester B, and 3 to 20% by weight of the polyester C.
14. The at least two polyesters consist of: (1) A polyester A is a copolymer comprising a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1), the content of the repeating unit A is 51 to 70 mol %, preferably 55 to 68 mol %, and the content of the repeating unit B is 30 to 49 mol %, preferably 32 to 45 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; [C7] wherein m1 is the same as defined for m in claim 1, n1 is the same as defined for n in claim 1, and m1 and n1 are the same or different; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, preferably 2; (2) A polyester B which is a copolymer consisting of a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1), the content of the repeating unit C in the polyester B is 1 to 50 mol %, preferably 20 to 45 mol %, and the content of the repeating unit B is 50 to 99 mol %, preferably 55 to 80 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; [C8] Polyester B, wherein m2 is the same as defined for m in claim 1, n2 is the same as defined for n in claim 1, and m2 and n2 are the same or different; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, preferably 2; The polyester composition comprises, relative to the total weight of the various components: 51 to 99% by weight of the polyester A; 1 to 49% by weight of the polyester B; The polyester composition according to any one of claims 1 to 8, comprising:
15. 15. The polyester composition according to claim 14, characterized in that the polyester composition comprises 80 to 95% by weight of the polyester A and 5 to 20% by weight of the polyester B.
16. The at least two polyesters consist of: (1) A polyester A is a copolymer comprising a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1), the content of the repeating unit A is 60 to 80 mol %, preferably 62 to 78 mol %, and the content of the repeating unit B is 20 to 40 mol %, preferably 22 to 38 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; [C9] wherein m1 is the same as defined for m in the claims, n1 is the same as defined for n in the claims, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, preferably 2; (2) A polyester B which is a copolymer consisting of a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1), the content of the repeating unit C in the polyester B is 20 to 59 mol %, preferably 30 to 55 mol %, and the content of the repeating unit B is 41 to 80 mol %, preferably 45 to 70 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; [C10] Polyester B, wherein m2 is the same as defined for m in claim 1, n2 is the same as defined for n in claim 1, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, and preferably, n2 is 2; The polyester composition comprises, relative to the total weight of the various components: 51 to 99% by weight of the polyester A; 1 to 49% by weight of the polyester B; The polyester composition according to any one of claims 1 to 8, comprising:
17. 17. The polyester composition according to claim 16, characterized in that the polyester composition comprises 70 to 90% by weight of the polyester A and 10 to 30% by weight of the polyester B.
18. The at least two polyesters consist of: (1) A polyester A is a copolymer comprising a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1), the content of the repeating unit A in the polyester A is 75 to 95 mol %, preferably 81 to 95 mol %, and the content of the repeating unit B in the polyester A is 5 to 25 mol %, preferably 5 to 19 mol %, based on the total number of moles of the repeating unit A and the repeating unit B; [C11] Polyester A, wherein m1 is the same as defined for m in claim 1, n1 is the same as defined for n in claim 1, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4, and preferably, n1 is 2; (2) A polyester B which is a copolymer consisting of a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1), the content of the repeating unit C in the polyester B is 20 to 74 mol %, preferably 40 to 70 mol %, and the content of the repeating unit B is 26 to 80 mol %, preferably 30 to 60 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; [C12] Polyester B, wherein m2 is the same as defined for m in claim 1, n2 is the same as defined for n in claim 1, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4, and preferably, n2 is 2; The polyester composition comprises, relative to the total weight of the various components: 51 to 99% by weight of the polyester A; 1 to 49% by weight of the polyester B; The polyester composition according to any one of claims 1 to 8, comprising:
19. 19. The polyester composition according to claim 18, characterized in that the polyester composition comprises 55-70% by weight of the polyester A and 30-45% by weight of the polyester B.
20. The at least two polyesters consist of: (1) A polyester A is a copolymer comprising a repeating unit A represented by formula (I') and a repeating unit B represented by formula (II-1), the content of the repeating unit A is 51 to 80 mol %, preferably 60 to 75 mol %, and the content of the repeating unit B is 20 to 49 mol %, preferably 25 to 40 mol %, based on the total number of moles of the repeating unit A and the repeating unit B in the polyester A; [C13] Polyester A, wherein m1 is the same as defined for m in claim 1, n1 is the same as defined for n in claim 1, and m1 and n1 are the same or different from each other; preferably, m1 is an integer from 2 to 8, and n1 is an integer from 2 to 6, and more preferably, m1 is an integer from 2 to 4, and n1 is an integer from 2 to 4; ; (2) A polyester B which is a copolymer consisting of a repeating unit C represented by formula (I″) and a repeating unit B represented by formula (II-1), the content of the repeating unit C in the polyester B is 81 to 99 mol %, preferably 83 to 95 mol %, and the content of the repeating unit B is 1 to 19 mol %, preferably 5 to 17 mol %, based on the total number of moles of the repeating unit C and the repeating unit B in the polyester B; [C14] Polyester B, wherein m2 is the same as defined for m in claim 1, n2 is the same as defined for n in claim 1, and m2 and n2 are the same or different from each other; preferably, m2 is an integer from 2 to 8, and n2 is an integer from 2 to 6, and more preferably, m2 is an integer from 2 to 4, and n2 is an integer from 2 to 4; (3) A polyester C which is a copolymer consisting of a repeating unit D represented by formula (I''') and a repeating unit B represented by formula (II-1), the content of the repeating unit D in the polyester C is 0 to 49 mol %, preferably 15 to 45 mol %, and the content of the repeating unit B in the polyester C is 51 to 100 mol %, preferably 55 to 85 mol %, based on the total number of moles of the repeating unit D and the repeating unit B; [C15] wherein m3 is the same as defined for m in claim 1, n3 is the same as defined for n in claim 1, and m3 and n3 are the same or different from each other; preferably, m3 is an integer from 2 to 8, and n3 is an integer from 2 to 6, and more preferably, m3 is an integer from 2 to 4, and n3 is an integer from 2 to 4; The polyester composition comprises, relative to the total weight of the various components: 30 to 98% by weight of the polyester A; 1 to 69% by weight of said polyester B; 1 to 69% by weight of the polyester C; The polyester composition according to any one of claims 1 to 8, comprising:
21. 21. The polyester composition of claim 20, wherein the polyester composition comprises 60 to 93% by weight of the polyester A, 5 to 38% by weight of the polyester B, and 1 to 20% by weight of the polyester C.
22. mixing all ingredients including a first polyester and a second polyester, and then extruding and pelletizing the resulting mixture to obtain a polyester composition; Preferably, no compatibilizer is added during the mixing step. A method for producing the polyester composition according to any one of claims 1 to 21.
23. 23. The method of claim 22, wherein the mixing step is performed under agitation.
24. The extrusion and pelletization is carried out in a twin screw extruder; 23. The process according to claim 22, characterized in that it is carried out at a temperature of preferably 80 to 270°C, preferably 110 to 220°C, at a screw rotation speed of 10 to 70 rpm and a torque of 2 to 80 Nm.
25. Use of the polyester composition according to any one of claims 1 to 21 in one or more of the following aspects: shape memory materials, 3D printed wires, heat shrinkable sleeves, medical limb braces, nonwovens and nonwoven articles (in particular disposable nonwoven articles, more preferably disposable medical nonwoven articles).
26. A shape-memory material comprising the polyester composition according to any one of claims 9 to 11.
27. 3D printing wire comprising a polyester composition according to claim 12 or 13, preferably having a diameter of 0.1 to 10 mm, preferably 1 to 4 mm.
28. continuously extruding and cooling the polyester composition to obtain a 3D printed wire; Preferably, the extrusion temperature is 90 to 260°C and the cooling temperature is 0 to 60°C.
28. A method for producing a 3D printed wire according to claim 27.
29. A heat shrinkable sleeve comprising the polyester composition of claim 14 or 15.
30. comprising the steps of continuously extruding, stretching, cooling and forming a polyester composition into a heat shrinkable sleeve; Preferably, the extrusion temperature is 90 to 240°C, preferably 120 to 180°C, and the cooling temperature is 0 to 60°C, preferably 20 to 40°C.
30. A method for making the heat shrinkable sleeve of claim 29.
31. the method further comprising the steps of sequentially heating, diameter expanding, secondary cooling, and forming the cooled pipe; Preferably, the heating temperature is 65-120°C, preferably 70-90°C; preferably, the diameter expansion ratio is 1.5-5 times, preferably 3-5 times, of the original size; preferably, the secondary cooling temperature is 0-60°C, preferably 20-40°C. The method of claim 30.
32. The polyester composition according to claim 16 or 17, Preferably, the thickness of the medical limb fixation device is 0.2 to 10 mm, preferably 1 to 3 mm; preferably, the medical limb fixation device has and / or does not have a pore structure, preferably has a pore structure, more preferably the pore size of said pore structure is 1 to 10 mm, preferably 1 to 5 mm; Medical limb immobilizer.
33. The method includes the steps of continuously extruding, molding, and optionally punching a polyester composition to obtain a medical limb fixation device, Preferably, the extrusion temperature is 90 to 230°C, preferably 110 to 170°C, and preferably, the molding is injection molding and / or compression molding; preferably, the molding step results in a thickness of the medical limb fixation device of 0.2 to 10 mm, preferably 1 to 3 mm; preferably, the diameter of the puncher used in the hole punching step is 1 to 10 mm, preferably 1 to 5 mm. A method for producing the medical limb fixation device according to claim 32.
34. A nonwoven fabric comprising the polyester composition of claim 18 or 19.
35. The method includes the steps of producing a nonwoven fabric from the polyester composition by a spunbonding process, Preferably, the spunbonding method includes an extrusion step, a spinning step, a reticulation step, and a consolidation step; preferably, the extrusion step has three temperature zones, where the temperature of the first temperature zone is 140-250°C, the temperature of the second temperature zone is 150-260°C, and the temperature of the third temperature zone is 170-260°C; preferably, the spinning temperature is 150-240°C, the spinning speed is 10-40 r / min; preferably, the reticulation speed is 5-30 r / min; preferably, the consolidation step adopts a method of hot rolling, and the hot rolling temperature is 80-170°C. A method for producing the nonwoven fabric of claim 34.
36. 22. An elastic fiber comprising the polyester composition according to claim 20 or 21, Preferably, the number of fibers of the elastic fibers is 5 to 500 dtex; the breaking strength according to GB / T 14337-2008 standard is 3 to 19 cN / dtex; the breaking elongation according to GB / T 14337-2008 standard is 130 to 620%; the stress relaxation rate according to GB / T 14337-2008 standard is 1 to 12%; and the permanent set rate according to GB / T 14337-2008 standard is 1 to 11%. Elastic fiber.
37. The polyester composition is continuously filament-formed, and then cold-set and stretched to obtain an elastic fiber; Preferably, the method of filament formation is melt spinning; preferably, the temperature of the filament formation is 120-270°C, preferably 150-220°C; preferably, the conditions of the low temperature placement are a temperature of 20-55°C, preferably 25-45°C; a time of 2-120 minutes, preferably 15-60 minutes; preferably, the conditions of drawing are a temperature of 56-110°C, preferably 60-90°C; and a draw ratio of 1.2-10 times, preferably 2-5 times. A method for producing the elastic fiber according to claim 36.
38. Use of an aliphatic-aromatic copolyester as a first polyester as defined in any one of claims 1 to 21 in one or more of the following aspects: shape memory materials, 3D printed wires, heat shrinkable sleeves, medical limb braces, nonwovens and nonwoven articles (in particular disposable nonwoven articles, more preferably disposable medical nonwoven articles).
Citation Information
Patent Citations
Polymer blends with improved notched impact strength
JP2007515543A
Injection molded article comprising thermoplastic composition
JP2008156508A
Black polyester resin composition for laser welding and molded material by using the same
JP2008189764A
Biodegradable Composite, The Preparation Process Thereof, And A Disposable Article Made Therefrom
US20120329924A1
Biodegradable polyester mixture
US20140134363A1