Carbonaceous material for electrochemical devices and method for producing the same, negative electrode for electrochemical devices, and electrochemical device
By controlling particle size, shape, and distribution through balanced manufacturing processes, the carbonaceous material maintains high electrode density and reduces irreversible capacity, enhancing the energy density of electrochemical devices like lithium-ion batteries.
Patent Information
- Application Number
- JP2021551666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-10
- Filing Date
- 2020-10-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-06
AI Technical Summary
Existing carbonaceous materials used in non-aqueous electrolyte secondary batteries, such as lithium-ion batteries, face an increase in irreversible capacity when particle size is reduced, leading to decreased discharge efficiency and insufficient energy density.
Control the particle size, shape, and distribution of carbonaceous materials to maintain high electrode density while minimizing irreversible capacity by adjusting parameters like BET specific surface area, aeration flow energy (AE), and average particle diameter, using a balanced manufacturing process involving primary and secondary pulverization and classification steps.
The solution results in a carbonaceous material suitable for high-capacity electrodes with reduced irreversible capacity, enabling smaller, more efficient electrochemical devices.
Smart Images

Figure 0007584430000001 
Figure 0007584430000002 
Figure 0007584430000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbonaceous material for electrochemical devices and a method for producing the same, as well as a negative electrode for electrochemical devices and an electrochemical device each containing the carbonaceous material for electrochemical devices. [Background technology]
[0002] In recent years, various electrochemical devices have been developed with the widespread use of small portable terminals such as mobile phones and notebook computers, electric vehicles, hybrid vehicles, etc. Among them, the use of nonaqueous electrolyte secondary batteries using carbonaceous materials as the negative electrode, such as lithium ion secondary batteries, is spreading, and while they are becoming smaller and lighter for in-vehicle applications, there is a demand for improved energy density. For example, Patent Document 1 discloses a carbonaceous material that can be used in nonaqueous electrolyte secondary batteries that have high electrode density and excellent input / output characteristics and cycle characteristics. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-073325 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as in Patent Document 1, when the particle size of a carbonaceous material is reduced, the specific surface area increases, and therefore non-aqueous electrolyte secondary batteries using such carbonaceous materials for electrodes are prone to increase in irreversible capacity and have reduced charge / discharge efficiency, which prevents a sufficient improvement in energy density. For this reason, there is a need to develop a carbonaceous material suitable for obtaining electrodes for electrochemical devices with small irreversible capacity while maintaining high electrode density.
[0005] In view of the above problems, the present invention aims to provide a carbonaceous material that is suitable as an electrode material for high-capacity electrochemical devices by ensuring high electrode density while suppressing an increase in irreversible capacity, and a method for producing the same. [Means for solving the problem]
[0006] The present inventors conducted extensive detailed studies on carbonaceous materials in order to solve the above problems, and as a result, they found that in order to ensure high electrode density while suppressing an increase in irreversible capacity, in addition to controlling the particle size of the carbonaceous material, various elements such as particle size distribution, shape of each particle, cohesiveness, and flowability are involved in a complex manner, and it is important that these elements are controlled in a well-balanced manner. They then found an index that reflects these elements in a complex manner, which led to the completion of the present invention.
[0007] That is, the present invention includes the following preferred embodiments. [1] The specific surface area measured by the BET method is 23 m 2 / g or less, and the flow energy during aeration (AE) measured by a powder rheometer is 40 mJ or more and 210 mJ or less. [2] The average particle diameter D at which the cumulative volume from the fine particle side becomes 50% in the particle size distribution measured by the laser scattering method 50 is 1 μm or more and 50 μm or less, and the particle diameter D at which the cumulative volume from the fine particle side is 10% 10 and average particle size D 50 Particle size distribution index D 50 / D 10 The carbonaceous material according to [1] above, wherein the MnO2 content is 1.9 or more. [3] The average interplanar spacing d of the (002) plane calculated using the Bragg equation by wide-angle X-ray diffraction 002 The carbonaceous material according to [1] or [2] above, wherein the average particle diameter is 0.36 nm or more. [4] The carbonaceous material according to any one of the above [1] to [3], wherein the carbonaceous material is derived from a plant. [5] A negative electrode for an electrochemical device, comprising the carbonaceous material according to any one of [1] to [4] above. [6] An electrochemical device comprising the negative electrode for electrochemical devices according to [5] above. [7] A step of subjecting the carbon precursor or the calcined product of the carbon precursor to primary grinding; A step of classifying the carbon precursor after the primary grinding or the calcined product of the carbon precursor; and A step of subjecting the classified carbon precursor or the calcined product of the carbon precursor to secondary pulverization; and Calcining the carbon precursor A method for producing a carbonaceous material, comprising: [8] In the primary grinding process, the average particle size D 50 The method according to [7] above, wherein the carbon precursor or the calcined product of the carbon precursor is pulverized to have a particle size of 2.7 μm or more and 300 μm or less. [9] The method for producing a carbonaceous material according to [7] or [8] above, wherein in the classification step, the carbon precursor after primary pulverization or the calcined product of the carbon precursor is classified so that the content of particles having a particle diameter of 1 μm or less is 6 vol.% or less.
[10] In the secondary grinding process, the average particle diameter D 50 is 1 μm or more and 50 μm or less, and the particle diameter D at which the cumulative volume is 10% 10 and average particle size D 50 Particle size distribution index D 50 / D 10 The method according to any one of the above [7] to [9], wherein the classified carbon precursor or the calcined product of the carbon precursor is pulverized so that the average molecular weight of the carbon precursor is 1.9 or more. Effect of the Invention
[0008] According to the present invention, it is possible to provide a carbonaceous material that is suitable as an electrode material for high-capacity electrochemical devices by ensuring high electrode density while suppressing an increase in irreversible capacity, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these.
[0010] [Carbonaceous material] The BET specific surface area of the carbonaceous material of the present invention is 23 m 2 / g or less. BET specific surface area is 23m 2 If the BET specific surface area exceeds 20 m / g, the area that reacts with the electrolyte becomes large when the material is used as an electrode material, leading to an increase in irreversible capacity and a decrease in discharge capacity. From the viewpoint of effectively suppressing the increase in irreversible capacity, the BET specific surface area is preferably 20 m 2 / g or less, more preferably 18m 2 / g or less, and more preferably 16m 2 In order to ensure a suitable reaction area with an electrolyte when the carbonaceous material is used as an electrode material and to increase the charge capacity when the carbonaceous material is used in an electrochemical device, the BET specific surface area is preferably 2 m 2 / g or more, more preferably 3m 2 / g or more, more preferably 4m 2 For example, the specific surface area tends to decrease by increasing the calcination temperature or the calcination time, and the BET specific surface area can be controlled to be within the desired range by adjusting the calcination temperature, the calcination time, etc. of the carbon precursor that provides the carbonaceous material. In the present invention, the BET specific surface area can be calculated by a nitrogen adsorption method, for example, by the method described in the Examples below.
[0011] The aerated flow energy of the carbonaceous material of the present invention measured by a powder rheometer is 40 mJ or more and 210 mJ or less. The aerated flow energy (AE, hereinafter also simply referred to as "AE") measured by a powder rheometer represents the powder state when the carbonaceous material is filled, and when the AE of the carbonaceous material is equal to or less than the upper limit value and equal to or more than the lower limit value, the density of the electrode obtained from the carbonaceous material can be increased, and the capacity per volume can be increased. On the other hand, when microparticles are present in excess, the AE tends to increase, but by setting the AE to the upper limit value or less, the coatability of the negative electrode is improved and good charge / discharge efficiency can be obtained. In the present invention, the AE is preferably 40 mJ or more, more preferably 50 mJ or more, even more preferably 55 mJ or more, and is preferably less than 210 mJ, more preferably 205 mJ or less, even more preferably 200 mJ or less.
[0012] In order to obtain an electrode for an electrochemical device having a high electrode density and a small irreversible capacity, it can be an effective means to increase the amount of carbonaceous material packed in the electrode while controlling the specific surface area within a suitable range. However, the electrode density cannot be simply controlled by, for example, tap density, which can generally be an index of the amount of packing, and various factors such as the particle size, particle size distribution, specific surface area, particle shape, cohesiveness, and flowability of the carbonaceous material, etc., of the carbonaceous material are involved in a complex manner, and it is important that these factors are controlled in a well-balanced manner. For this reason, it has been difficult to control the electrode density when packed with a carbonaceous material even if each of the above factors is used as an index.
[0013] In contrast, the present invention has found that the AE reflects various elements of the carbonaceous material in a composite manner and is a parameter closely correlated with the electrode density, and uses this as a new index. This makes it possible to accurately and easily control the electrode density when the carbonaceous material is filled, and to provide a carbonaceous material suitable for obtaining an electrode for an electrochemical device having a high electrode density and a small irreversible capacity. In other words, the AE does not simply individually reflect various elements such as the particle size distribution of the carbonaceous material, the shape of each particle, the chemical state due to the surface functional groups of the carbonaceous material, cohesiveness, and flowability, but reflects the characteristics due to these elements in a composite manner. Therefore, for example, the electrode density, which is difficult to control by adjusting only the particle size distribution, can be accurately and easily controlled by using the AE as an index.
[0014] In the present invention, AE is measured by a powder rheometer, a powder fluidity analyzer. Specifically, the sample powder is filled in the apparatus, and the blade movement required to move the blade installed in the apparatus according to the blade height is measured as the energy value (J) in a state where air is passed through the bottom of the apparatus at a rate of 2 mm / sec. For example, a powder rheometer FT4 manufactured by Freeman Technology can be used as the AE measuring apparatus.
[0015] The AE in the present invention can be calculated, for example, by the method described in the Examples below. Specifically, the measurement using a powder rheometer FT4 manufactured by Freeman Technology Co., Ltd. is performed by passing air from the bottom of the device at a rate of 2 mm / sec, rotating a blade at a constant blade tip speed while entering a container filled with powder, and measuring the vertical stress F using a load cell at the bottom of the device and the rotational torque T using a torque meter at the top. From the vertical stress F, rotational torque T, and blade height at this time, the energy required for the blade to move through the powder can be calculated. The blade radius (also called the blade blade diameter) is R, the helical angle at which the blade tip moves is α°, and the blade movement energy according to the blade height is defined as the flow energy during aeration (AE). That is, the flow energy during aeration (AE) is calculated by the following formula: AE=T / (Rtanα)+F In the case of the Freeman Technology Powder Rheometer FT4, the following conditions were met: α = 5°, R = 48 mm, the diameter of the container in which the powder is to be filled is 50 mm, and the volume of the container is 160 mm 3 (See Hiramura Yukiyoshi, "Considerations on Rheological Evaluation and Fluidity of Powders," Journal of the Society of Powder Technology, 2017, Vol. 54, No. 9, pp. 604-608.) For example, the flow energy (AE) during aeration can be calculated by filling such a container with 120 mL of powder up to the brim, aerating air at a rate of 2 mm / sec from the bottom of the device, and letting air enter while rotating at a tip speed of 100 mm / sec.
[0016] In the carbonaceous material of the present invention, the AE can be controlled, for example, by adjusting the conditions, order, number of times, etc. of the pulverization and classification steps in the manufacturing method of the carbonaceous material. In this case, for example, in the manufacturing process of the carbonaceous material, the pulverization conditions and classification conditions can be controlled while checking the AE at an appropriate stage, such as each pulverization step and classification step. The AE can also be controlled by mixing a carbonaceous material with a relatively small particle size and a carbonaceous material with a relatively large particle size in an appropriate ratio.
[0017] In the present invention, the average particle diameter D at which the cumulative volume from the fine particle side becomes 50% in the particle size distribution measured by the laser scattering method of the carbonaceous material is 50 is preferably 1 μm or more and 50 μm or less. 50 When the average particle diameter D is within the above range, the increase in the specific surface area can be suppressed, the irreversible capacity can be reduced, and the formation of an electrode can be facilitated. 50 is more preferably 1.5 μm or more, even more preferably 2 μm or more, particularly preferably 2.5 μm or more, and is more preferably 30 μm or less, even more preferably 15 μm or less, particularly preferably 10 μm or less, and most preferably 8 μm or less. In the present invention, the average particle diameter D 50 can be measured by a laser scattering method, and can be measured and calculated, for example, by the method described in the Examples below.
[0018] In the carbonaceous material of the present invention, the particle diameter D at which the cumulative volume from the fine particle side becomes 10% is 10 and average particle size D 50 Particle size distribution index D 50 / D 10 is preferably 1.9 or more. 50 / D 10 When the particle size distribution index D is equal to or larger than the lower limit, the AE of the carbonaceous material is likely to be within the specific range, and the density of the electrode obtained from the carbonaceous material is likely to be high, making it easy to increase the capacity per volume. 50 / D 10is more preferably greater than 1.9, even more preferably 2.0 or more, particularly preferably 2.1 or more, and especially preferably 2.5 or more, and is preferably 10.0 or less, more preferably 5.0 or less, even more preferably 4.5 or less, and especially preferably 4.0 or less. Particle size distribution index D 50 / D 10 is measured and calculated by the laser scattering method. 10 and D 50 It can be calculated from:
[0019] The average interplanar spacing d of the (002) plane of the carbonaceous material of the present invention is calculated using the Bragg equation by wide-angle X-ray diffraction. 002 is preferably 0.36 nm or more, more preferably 0.37 nm or more, and even more preferably 0.38 nm or more, and is preferably 0.42 nm or less, more preferably 0.41 nm or less, and even more preferably 0.40 nm or less. 002 When the average interplanar spacing is within the above range, good input and output characteristics are exhibited. The average interplanar spacing can be controlled by adjusting the firing temperature of the carbonaceous material or the carbon precursor that provides the carbonaceous material.
[0020] [Method for producing carbonaceous material] The carbonaceous material of the present invention is, for example, A step of subjecting the carbon precursor or the calcined product of the carbon precursor to primary grinding; A step of classifying the carbon precursor after the primary grinding or the calcined product of the carbon precursor; and A step of subjecting the classified carbon precursor or the calcined product of the carbon precursor to secondary pulverization; and Calcining the carbon precursor Therefore, the present invention also relates to a method for producing a carbonaceous material, which includes the above steps.
[0021] The AE of the carbonaceous material can be controlled within the desired range by first grinding the carbon precursor or the burned product of the carbon precursor, which is a coarse particle (hereinafter, both are also collectively referred to as "carbon precursor, etc."), removing fine powder by classification, and then secondarily grinding to a desired particle size. Therefore, in the above method, the steps of primary grinding, classification, and secondary grinding are performed in this order. On the other hand, since the carbon precursor does not dissolve by firing, the average particle size of the carbon precursor does not substantially change before and after firing. For this reason, the order of performing the above grinding and classification steps and the firing step is not particularly limited, and the grinding and classification steps may be performed on the carbonaceous material before firing, or the grinding and classification steps may be performed on the carbonaceous material after firing (i.e., the burned product of the carbon precursor).
[0022] In the present invention, the step of subjecting a carbon precursor or a calcined product of the carbon precursor to primary pulverization (hereinafter also referred to as the "primary pulverization step") is a step of pulverizing the carbon precursor, which is a coarse particle, into fine particles. The average particle size of the carbon precursor, etc., to the primary pulverization can be appropriately determined depending on the carbon material and carbon precursor used as raw materials, and is not particularly limited. From the viewpoint of easy control to a desired particle size and excellent handleability, the average particle size D of the carbon precursor, etc., to the primary pulverization is preferably 100 to 2000 nm. 50 is usually 100 μm or more and 10,000 μm or less, preferably 200 μm or more, more preferably 400 μm or more, and preferably 8,000 μm or less, more preferably 5,000 μm or less. The average particle diameter D of the carbon precursor to be subjected to the primary grinding 50 is the average particle diameter D of the carbonaceous material of the present invention 50 It can be measured by a laser scattering method in the same manner as in the measurement of
[0023] In one embodiment of the present invention, the average particle diameter D 50It is preferable to pulverize the carbon precursor, etc., so that the AE is 2.7 μm or more and 300 μm or less. As described above, the AE of the carbonaceous material is determined by a complex reflection of many factors such as the particle size, particle size distribution, shape, and chemical state due to the surface functional groups of the carbonaceous material of the carbonaceous material. Therefore, control of the particle size of the carbon precursor, etc. in the primary pulverization does not directly determine the AE of the obtained carbonaceous material. However, by setting the particle size of the carbon precursor, etc. after the primary pulverization to the above range, it becomes easier to obtain a carbonaceous material having an AE in the range of 40 mJ or more and 210 mJ or less through the subsequent classification and secondary pulverization steps. In the present invention, the average particle size D of the carbon precursor, etc. after the primary pulverization 50 is preferably 3 μm or more, more preferably 4 μm or more, and is preferably 200 μm or less, more preferably 150 μm or less.
[0024] In the present invention, the primary pulverization step may be performed in one go or in multiple steps. In this specification, when the pulverization is performed in multiple steps, the pulverization step performed before the first classification step for classifying the pulverized carbon precursor or the like is regarded as the primary pulverization step.
[0025] The pulverizer used in the primary pulverization step is not particularly limited, and for example, a jet mill, a ball mill, a bead mill, a hammer mill, or a rod mill can be used. One type of pulverizer may be used, or two or more types may be used in combination. A method of pulverizing particles by contact between particles, such as a jet mill, takes a long time to pulverize and tends to reduce volume efficiency, so from the viewpoint of pulverization efficiency, a method of pulverizing in the presence of pulverizing media, such as a ball mill or a bead mill, is preferred. A bead mill is also suitable in that it can avoid the inclusion of impurities from the pulverizing media. Among them, a pulverizer having a classification mechanism is more preferred because it is taken out of the pulverized material and is easy to suppress excessive pulverization of carbon precursors, etc.
[0026] When a ball mill or a bead mill is used as the pulverizer, the material of the media (balls or beads) is not particularly limited, and for example, an organic polymer compound such as polyamide, or an inorganic oxide such as alumina, silica, titania, or zirconia can be used. From the viewpoint of preventing contamination from the media and easily shortening the pulverization time, the media is preferably alumina or zirconia. The filling rate of the media in the pulverizer is not particularly limited, but from the viewpoint of easily suppressing atypical shape during pulverization, it is preferably 10 to 90%, more preferably 20 to 80%. The pulverization time may be appropriately determined according to the particle size of the carbon precursor as the raw material and the type of pulverizer used, so that the powder can be pulverized to a desired particle size.
[0027] The pulverization may be either wet pulverization or dry pulverization, with dry pulverization being preferred from the viewpoint of easily suppressing surface oxidation of the carbon precursor and the like.
[0028] The method for producing a carbonaceous material of the present invention includes a step of classifying the carbon precursor, etc., after primary pulverization. This step is a step for removing fine powder portions from the carbon precursor, etc., after primary pulverization, and controlling the particle size of the carbon precursor, etc. By reducing the content of particles having a particle size significantly different from the average particle size generated in the primary pulverization, particularly fine particles having a small particle size significantly different from the average particle size, excessive pulverization can be suppressed, and an increase in irreversible capacity due to an increase in specific surface area can be suppressed.
[0029] In one embodiment of the present invention, in the classification step after the primary pulverization step, the content of particles having a particle diameter of 1 μm or less is preferably 6 vol.% or less, more preferably 5 vol.% or less, and even more preferably 3 vol.% or less. By removing particles having a particle diameter of 1 μm or less from the carbon precursor after the primary pulverization, excessive pulverization can be suppressed, and an increase in irreversible capacity due to an increase in specific surface area can be suppressed. The content of particles having a particle diameter of 1 μm or less after the classification step is preferably as low as possible, and may be 0 vol.%.
[0030] In the classification step, methods for classifying the carbon precursor, etc. (controlling the particle size of the carbon precursor, etc.) include, for example, a method of removing fine particles having a particle size of 1 μm or less contained in the carbon precursor, etc. after primary pulverization, a method of performing primary pulverization so that the average particle size becomes slightly larger, removing large particles contained in the carbon precursor, etc. after primary pulverization so that the average particle size becomes a desired one, and repeating the operation of pulverizing the large particles again to obtain the desired average particle size, etc. The latter method allows for more productive production of the carbonaceous material of the present invention that does not contain fine particles greater than a predetermined amount.
[0031] The classification method is not particularly limited, and examples thereof include classification using a sieve, wet classification, and dry classification. Examples of wet classifiers include classifiers that utilize the principles of gravity classification, inertia classification, hydraulic classification, centrifugal classification, etc. Examples of dry classifiers include classifiers that utilize the principles of sedimentation classification, mechanical classification, centrifugal classification, etc. From the viewpoint of economy, it is preferable to use a dry classification device. In addition, the primary pulverization and / or the secondary pulverization step described later and the classification step can be performed using one device.
[0032] The method for producing a carbonaceous material of the present invention includes a step of subjecting the classified carbon precursor, etc. to secondary pulverization (hereinafter also referred to as a "secondary pulverization step"). The AE of the carbonaceous material obtained by classifying the carbon precursor, etc. after the primary pulverization and removing fine powder from the carbon precursor, etc., tends to be high, and the density of an electrode produced using this can be improved.
[0033] In one embodiment of the present invention, in the secondary grinding step, the average particle diameter D 50 is 1 μm or more and 50 μm or less, and the particle diameter D at which the cumulative volume is 10% 10 and average particle size D 50 Particle size distribution index D 50 / D 10It is preferable to pulverize the carbon precursor etc. after classification so that the AE becomes 1.9 or more. The AE of the carbonaceous material is determined based on many factors such as the particle size, particle size distribution, shape, and chemical state due to the surface functional groups of the carbonaceous material of the carbonaceous material, so that control of the particle size of the carbon precursor etc. in the secondary pulverization does not directly determine the AE of the obtained carbonaceous material, but by setting the particle size of the carbon precursor etc. after the secondary pulverization in the above range, the AE of the carbonaceous material tends to increase, and it becomes easier to control the AE of the obtained carbonaceous material to a range of 40 mJ or more and 210 mJ or less.
[0034] In the present invention, the secondary pulverization step may be performed at once or may be performed in a plurality of steps. In this specification, when the pulverization is performed in a plurality of steps, the pulverization step performed after the first classification is the secondary pulverization step, and when further classification is performed thereafter, the pulverization step performed before the classification is the secondary pulverization step. The pulverizer, pulverization time, pulverization conditions, etc. that can be used in the secondary pulverization step are all the same as those in the primary pulverization step, and may be appropriately selected according to the desired particle size, particle size distribution, specific surface area, AE, etc.
[0035] In addition to the above-mentioned primary grinding, classification, and secondary grinding steps, the method for producing a carbonaceous material of the present invention may include a further grinding and / or classification step as long as the desired AE and specific surface area can be obtained. However, it is preferable that the final step of the grinding and classification steps included in the steps for obtaining a carbonaceous material is the grinding step. By not substantially performing classification after the secondary grinding or subsequent grinding, the finally obtained carbonaceous material contains particles having a relatively small particle size, and the particle size distribution can be appropriately broadened. As a result, the AE of the carbonaceous material is likely to be in the range of 40 mJ or more and 210 mJ or less, and the filling amount when filling the carbonaceous material can be increased, thereby improving the electrode density.
[0036] The carbonaceous material of the present invention can be obtained by calcining the carbon precursor that has been subjected to the above-mentioned steps of primary pulverization, classification, and secondary pulverization. In addition, when the carbon precursor before the above-mentioned primary pulverization is calcined, the carbonaceous material of the present invention can be obtained by subjecting the calcined carbon precursor (i.e., the calcined product of the carbon precursor) to the above-mentioned steps of primary pulverization, classification, and secondary pulverization.
[0037] The calcination (hereinafter also referred to as "main calcination") may be performed on the carbon precursor before the primary pulverization or on the carbon precursor after the secondary pulverization, and may be performed according to a normal calcination procedure. By performing the main calcination, a carbonaceous material for electrochemical devices such as non-aqueous electrolyte secondary batteries can be obtained. The main calcination step is a step for heating the carbon precursor to remove volatile components contained in the carbon precursor and construct a carbon skeleton.
[0038] The firing temperature of the main firing is usually 800 to 1500°C, preferably 850 to 1350°C, and more preferably 900 to 1300°C. The main firing is preferably carried out under an inert gas atmosphere. Examples of the inert gas include nitrogen and argon, and the main firing can also be carried out in an inert gas containing a halogen gas. The main firing may be carried out under reduced pressure, for example, at 10 kPa or less. The firing time of the main firing is not particularly limited, but is, for example, 0.05 to 10 hours, preferably 0.05 to 8 hours, and more preferably 0.05 to 6 hours.
[0039] In the present invention, when the carbon precursor is derived from a plant, the carbon precursor may be mixed with a volatile organic material and then fired. By firing a mixture of the carbon precursor and the volatile organic material, the specific surface area of the resulting carbonaceous material can be reduced. The mechanism has not been elucidated in detail, but can be considered as follows. However, the present invention is not limited by the following explanation. It is considered that by mixing a plant-derived carbon precursor with a volatile organic material and firing the mixture, a carbonaceous coating obtained by heat treatment of the volatile organic material is formed on the surface of the plant-derived carbon precursor. This carbonaceous coating reduces the specific surface area of the carbonaceous material generated from the plant-derived carbon precursor, and suppresses the formation reaction of a coating called SEI (Solid Electrolyte Interphase) due to the reaction of the carbonaceous material with lithium, so that it is expected to reduce the irreversible capacity. In addition, the generated carbonaceous coating can also be doped and dedoped with lithium, so that the effect of increasing the capacity can be expected.
[0040] Examples of volatile organic substances include thermoplastic resins and low molecular weight organic compounds. Specifically, examples of thermoplastic resins include polystyrene, polyethylene, polypropylene, poly(meth)acrylic acid, and poly(meth)acrylic acid esters. In this specification, (meth)acrylic is a general term for acrylic and methacrylic. Examples of low molecular weight organic compounds include toluene, xylene, mesitylene, styrene, naphthalene, phenanthrene, anthracene, and pyrene. Since it is preferable that the surface of the carbon precursor is oxidized and activated when it is thermally decomposed, polystyrene, polyethylene, and polypropylene are preferable as thermoplastic resins. Furthermore, it is preferable that the low molecular weight organic compound is less volatile at room temperature from the viewpoint of safety, and naphthalene, phenanthrene, anthracene, pyrene, and the like are preferable.
[0041] In one embodiment of the present invention, examples of the thermoplastic resin include olefin resins, styrene resins, and (meth)acrylic acid resins. Examples of the olefin resins include polyethylene, polypropylene, random copolymers of ethylene and propylene, and block copolymers of ethylene and propylene. Examples of the styrene resins include polystyrene, poly(α-methylstyrene), and copolymers of styrene and (meth)acrylic acid alkyl esters (the number of carbon atoms in the alkyl group is 1 to 12, preferably 1 to 6). Examples of the (meth)acrylic acid resins include polyacrylic acid, polymethacrylic acid, and (meth)acrylic acid alkyl ester polymers (the number of carbon atoms in the alkyl group is 1 to 12, preferably 1 to 6).
[0042] In one embodiment of the present invention, for example, a hydrocarbon compound having 1 to 20 carbon atoms can be used as the low molecular weight organic compound. The number of carbon atoms in the hydrocarbon compound is preferably 2 to 18, more preferably 3 to 16. The hydrocarbon compound may be a saturated or unsaturated hydrocarbon compound, a chain-like hydrocarbon compound, or a cyclic hydrocarbon compound. In the case of an unsaturated hydrocarbon compound, the unsaturated bond may be a double bond or a triple bond, and the number of unsaturated bonds contained in one molecule is not particularly limited. For example, the chain-like hydrocarbon compound is an aliphatic hydrocarbon compound, and examples of the chain-like hydrocarbon compound include linear or branched alkanes, alkenes, or alkynes. Examples of the cyclic hydrocarbon compound include alicyclic hydrocarbon compounds (e.g., cycloalkanes, cycloalkenes, cycloalkynes) or aromatic hydrocarbon compounds. Specifically, examples of the aliphatic hydrocarbon compound include methane, ethane, propane, butane, pentane, hexane, octane, nonane, decane, ethylene, propylene, butene, pentene, hexene, and acetylene. Examples of the alicyclic hydrocarbon compound include cyclopentane, cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclopropane, cyclopentene, cyclohexene, cycloheptene, cyclooctene, decalin, norbornene, methylcyclohexane, and norbornadiene. Examples of the aromatic hydrocarbon compound include monocyclic aromatic compounds such as benzene, toluene, xylene, mesitylene, cumene, butylbenzene, styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, vinylxylene, p-tert-butylstyrene, and ethylstyrene, and condensed polycyclic aromatic compounds having 3 to 6 rings such as naphthalene, phenanthrene, anthracene, and pyrene, and preferably condensed polycyclic aromatic compounds, more preferably naphthalene, phenanthrene, anthracene, or pyrene. Here, the hydrocarbon compound may have any substituent.The substituent is not particularly limited, and examples thereof include an alkyl group having 1 to 4 carbon atoms (preferably an alkyl group having 1 to 2 carbon atoms), an alkenyl group having 2 to 4 carbon atoms (preferably an alkenyl group having 2 carbon atoms), and a cycloalkyl group having 3 to 8 carbon atoms (preferably a cycloalkyl group having 3 to 6 carbon atoms).
[0043] From the viewpoint of ease of mixing and avoidance of uneven distribution, the volatile organic substance is preferably in a solid state at room temperature, and more preferably, for example, a thermoplastic resin that is solid at room temperature, such as polystyrene, polyethylene, or polypropylene, or a low molecular weight organic compound that is solid at room temperature, such as naphthalene, phenanthrene, anthracene, or pyrene. Since it is preferable that the surface of the plant-derived carbon precursor is not oxidized and activated when it volatilizes and is thermally decomposed at the firing temperature, the thermoplastic resin is preferably an olefin-based resin or a styrene-based resin, and more preferably polystyrene, polyethylene, or polypropylene. As the low molecular weight organic compound, it is preferable for safety that the volatility is small at room temperature, so a hydrocarbon compound having 1 to 20 carbon atoms is preferable, a condensed polycyclic aromatic compound is more preferable, and naphthalene, phenanthrene, anthracene, or pyrene is even more preferable. Furthermore, from the viewpoint of ease of mixing with the carbon precursor, a thermoplastic resin is preferable, an olefin-based resin or a styrene-based resin is more preferable, polystyrene, polyethylene, or polypropylene is even more preferable, and polystyrene and polyethylene are particularly preferable.
[0044] The volatile organic matter is an organic matter having a carbon residue ratio of preferably less than 5% by mass, more preferably less than 3% by mass, from the viewpoint of stable operation of the calcination equipment. The carbon residue ratio in the present invention is preferably the carbon residue ratio when incinerated at 800°C. The volatile organic matter is preferably one that generates volatile substances (e.g., hydrocarbon gases and tar components) that can reduce the specific surface area of the carbon precursor produced from the plant-derived char. In addition, from the viewpoint of maintaining the properties of the carbonaceous material produced after calcination, the carbon residue ratio is preferably less than 5% by mass. If the carbon residue ratio is less than 5%, it is difficult to produce a carbonaceous material with locally different properties.
[0045] The carbon content can be measured by igniting the sample in an inert gas and quantifying the carbon content of the ignition residue. Ignition is performed by measuring the carbon content of approximately 1 g of volatile organic matter (the exact mass is called W 1 The mixture is placed in a crucible, and the crucible is heated from room temperature to 800°C at a rate of 10°C / min while flowing nitrogen at 20 liters per minute. The crucible is then ignited at 800°C for 1 hour. The residue is called the ignition residue, and its mass is W 2 (g).
[0046] Next, the ignition residue was subjected to elemental analysis in accordance with the method specified in JIS M8819, and the mass percentage of carbon, P 1 Measure the residual carbon percentage P 2 (% by mass) can be calculated by the following formula (I).
[0047]
number
[0048] When the carbon precursor and the volatile organic substance are mixed, the mass ratio of the carbon precursor to the volatile organic substance in the mixture is not particularly limited, but is preferably 99:1 to 40:60. The mass ratio of the carbon precursor to the volatile organic substance in the mixture is more preferably 97:3 to 40:60, further preferably 95:5 to 60:40, and particularly preferably 93:7 to 80:20. For example, when the volatile organic substance is 1 part by mass or more, the specific surface area can be sufficiently reduced. In addition, when the volatile organic substance is 60 parts by mass or less, the effect of reducing the specific surface area is not saturated, and the volatile organic substance is unlikely to be excessively consumed, which is industrially advantageous.
[0049] When the carbon precursor is mixed with the volatile organic substance, the mixing may be performed at any stage before the calcination of the carbon precursor, and may be performed before the above-mentioned primary crushing step or after the primary crushing, classification and secondary crushing.
[0050] The carbon precursor serving as the raw material of the carbonaceous material of the present invention is a precursor of the carbonaceous material that supplies a carbon component when producing the carbonaceous material, and can be broadly selected from carbon precursors derived from plants, carbon precursors derived from minerals, carbon precursors derived from natural materials, carbon precursors derived from synthetic materials, etc. From the viewpoints of reducing harmful impurities, environmental protection, and commercial viewpoints, it is preferable that the carbonaceous material of the present invention is based on a carbon precursor derived from plants, in other words, it is preferable that the carbon precursor serving as the raw material of the carbonaceous material of the present invention is derived from plants.
[0051] Carbon precursors derived from minerals include, for example, petroleum-based and coal-based pitches and coke. Carbon precursors derived from natural materials include, for example, natural fibers such as cotton and hemp, regenerated fibers such as rayon and viscose rayon, and carbonized semi-synthetic fibers such as acetate and triacetate. Carbon precursors derived from synthetic materials include, for example, carbonized polyamides such as nylon, polyvinyl alcohols such as vinylon, polyacrylonitriles such as acrylic, polyolefins such as polyethylene and polypropylene, polyurethanes, phenolic resins, and vinyl chloride resins.
[0052] The plant-derived carbon precursor can be produced by using a plant-derived carbon material (hereinafter also referred to as "plant-derived char") as a raw material and subjecting it to activation, deashing and other treatments. Therefore, the method for producing a carbonaceous material of the present invention includes, in addition to the above-mentioned steps of pulverization, classification, and firing, for example: (i) activating a plant-derived carbonaceous material as a raw material; and / or (ii) A process for deashing the plant-derived carbonaceous material that is to be used as the raw material It may also include the following. In addition, char generally refers to a powdered solid rich in carbon that does not melt or soften and is obtained when coal is heated, but here it also refers to a powdered solid rich in carbon that does not melt or soften and is obtained by heating organic matter.
[0053] The plant (hereinafter also referred to as "plant raw material") that is the raw material for plant-derived char is not particularly limited. Examples of plant raw materials include coconut shells, coffee beans, tea leaves, sugar cane, fruits (e.g., mandarin oranges, bananas), straw, rice husks, broad-leaved trees, coniferous trees, and bamboo. These examples include waste after their original use (e.g., used tea leaves), or parts of plant raw materials (e.g., banana or mandarin peels). These plant raw materials may be used alone or in combination of two or more kinds. Among these plant raw materials, coconut shells are preferred from the viewpoint of easy mass acquisition.
[0054] The coconut shell is not particularly limited, but examples thereof include coconut shells of palm (oil palm), coconut, salak, and oat palm. These coconut shells may be used alone or in combination of two or more. Coconut and palm shells are biomass wastes generated in large quantities after coconuts are used as food, detergent raw materials, biodiesel oil raw materials, and the like, and are particularly preferred from the viewpoint of easy availability.
[0055] The method for producing plant-derived char from plant raw materials is not particularly limited. For example, plant raw materials can be heat-treated (hereinafter also referred to as "pre-calcination") at a temperature of 300°C or higher in an inert gas atmosphere.
[0056] The heat treatment temperature for the calcination is not particularly limited as long as it is 300°C or higher. If the heat treatment temperature for the calcination is too high, the char may become highly crystallized, making the subsequent pulverization difficult. Therefore, the heat treatment temperature for the calcination is usually 300°C to 1000°C, preferably 400°C to 900°C, and more preferably 500°C to 800°C.
[0057] The heat treatment time of the calcination is not particularly limited. If the heat treatment time of the calcination is too long, the char may become highly crystallized, which may make the subsequent pulverization difficult. Therefore, the heat treatment time of the calcination is usually 1 to 24 hours, preferably 1.5 to 20 hours, and more preferably 2 to 15 hours.
[0058] It can also be obtained in the form of plant-derived char (eg, coconut shell char).
[0059] Carbonaceous materials produced from plant-derived char can be doped with a large amount of active material, and are therefore basically suitable as carbonaceous materials for electrochemical devices such as nonaqueous electrolyte secondary batteries. However, plant-derived char generally contains a large amount of metal elements (especially potassium, iron, etc.) contained in the plant raw material, and when an electrode containing a carbonaceous material with a high content of such metal elements is used in an electrochemical device, it may have an undesirable effect on the electrochemical properties and safety. Therefore, it is preferable to reduce the content of potassium element, iron element, etc. contained in the carbonaceous material as much as possible.
[0060] In addition, in addition to potassium and iron elements, plant-derived char often contains alkali metals (e.g., sodium), alkaline earth metals (e.g., magnesium or calcium), transition metals (e.g., copper), and other elements (hereinafter, these are also collectively referred to as "ash content"). When an electrode containing a carbonaceous material containing these metal elements is used as the negative electrode of a nonaqueous electrolyte secondary battery such as a lithium ion secondary battery, impurities may dissolve into the electrolyte during dedoping from the negative electrode, adversely affecting the battery performance and impairing the reliability of the nonaqueous electrolyte secondary battery, so it is preferable to reduce the content of these metals. In addition, by reducing the ash content in the carbonaceous material, it is possible to suppress pore blockage of the carbonaceous material and improve the charge / discharge capacity of the battery.
[0061] Therefore, it is preferable to reduce the content of ash (alkali metal elements, alkaline earth metal elements, transition metal elements, and other elements) in the plant raw material or plant-derived char before calcining the carbon precursor to obtain a carbonaceous material. Hereinafter, reducing the content of ash in the char of the plant raw material or plant-derived raw material is also referred to as "decalcification". The decalcification method is not particularly limited, and may be, for example, a method of extracting and decalcifying metals using an acidic solution containing a mineral acid such as hydrochloric acid or sulfuric acid, or an organic acid such as acetic acid or formic acid (liquid-phase decalcification), or a method of decalcifying by exposing to a high-temperature gas phase containing a halogen compound such as hydrogen chloride (gas-phase decalcification).
[0062] Liquid phase demineralization may be carried out in the form of either plant raw material or plant-derived char. Liquid phase demineralization can be carried out, for example, by immersing plant raw material or plant-derived char in an acidic solution. The acidic solution is a mixture of an acid and an aqueous solution. The acid is not particularly limited, but examples thereof include aqueous solutions of mineral acids such as hydrochloric acid and sulfuric acid, and organic acids such as acetic acid, butyric acid, and citric acid. From the viewpoint of avoiding unnecessary ions remaining in the demineralized material, it is preferable to use an organic acid as the acid, and from the viewpoints of efficiency of demineralization, economic efficiency such as the price of the acid, and relatively easy waste liquid treatment after use, it is more preferable to use acetic acid and / or citric acid. Examples of the aqueous solution include water, and mixtures of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include alcohols such as methanol, ethanol, propylene glycol, and ethylene glycol.
[0063] The acid concentration in the acidic solution is not particularly limited, but since the deashing rate is affected by the acid concentration, it is preferably in the range of 0.001 to 1 M, more preferably in the range of 0.002 to 0.9 M, and even more preferably in the range of 0.005 to 0.5 M. The amount of the acidic solution used is also not particularly limited, but it is preferably such that the plant raw material or plant-derived char to be immersed is immersed in the acidic solution, and for example, the mass of the acidic solution relative to the mass of the plant raw material or plant-derived char to be immersed is preferably 100 to 1000 mass%, more preferably 200 to 900 mass%, and even more preferably 250 to 800 mass%.
[0064] The temperature of liquid phase de-ashing may be determined depending on the plant raw material or plant-derived char to be de-ashed, and may be, for example, 10 to 120° C., preferably 20 to 100° C., and more preferably 25 to 95° C. When the de-ashing temperature is within the above range, de-ashing can be carried out efficiently while suppressing a decrease in carbon content due to hydrolysis of organic matter constituting the plant.
[0065] The time for liquid phase demineralization is not particularly limited, but may be, for example, 0.1 to 100 hours, preferably 0.2 to 50 hours, and more preferably 0.5 to 20 hours. Liquid phase demineralization may be performed by continuously immersing the plant raw material or plant-derived char in an acidic solution, or may be performed in several separate steps while refreshing the acidic solution used for demineralization. When liquid phase demineralization is performed in several separate steps, the total demineralization time is taken as the liquid phase demineralization time.
[0066] The apparatus used for liquid-phase demineralization is not particularly limited as long as it is an apparatus capable of immersing the plant raw material or plant-derived char in an acidic solution. For example, a glass-lined stirring tank can be used.
[0067] Gas phase demineralization may be carried out in the form of either plant raw material or plant-derived char. For example, gas phase demineralization may be carried out by heat treating plant raw material or plant-derived char in a gas phase containing a halogen compound. The halogen compound is not particularly limited, and examples thereof include fluorine, chlorine, bromine, iodine, hydrogen fluoride, hydrogen chloride, hydrogen bromide, iodine bromide, chlorine fluoride (ClF), iodine chloride (ICl), iodine bromide (IBr), bromine chloride (BrCl), and the like. Compounds that generate these halogen compounds by thermal decomposition or mixtures thereof may also be used. The halogen compound is preferably hydrogen chloride from the viewpoint of supply stability and stability of the halogen compound used.
[0068] Gas phase deashing may be carried out in a gas phase in which a halogen compound and an inert gas are mixed. The inert gas is not particularly limited as long as it does not react with the deashed material (plant raw material or plant-derived char) and the deashed plant raw material or plant-derived char at the deashing temperature. Examples of the inert gas include nitrogen, helium, argon, krypton, and mixtures thereof. From the viewpoints of supply stability and economic efficiency, the inert gas is preferably nitrogen.
[0069] When gas-phase deashing is performed in a gas phase in which a halogen compound and an inert gas are mixed, the mixing ratio of the halogen compound and the inert gas is not particularly limited as long as sufficient deashing can be achieved. For example, the amount of the halogen compound relative to the inert gas is preferably 0.01 to 10.0% by volume, more preferably 0.05 to 8.0% by volume, and even more preferably 0.1 to 5.0% by volume.
[0070] The temperature of the gas phase de-ashing may be determined depending on the plant raw material or plant-derived char to be de-ashed, and may be, for example, 500 to 1100°C, preferably 600 to 1050°C, more preferably 650 to 1000°C, and further preferably 850 to 1000°C. If the de-ashing temperature is too low, the de-ashing efficiency decreases and de-ashing may not be sufficient. If the de-ashing temperature is too high, activation by halogen compounds may occur.
[0071] The time for gas phase demineralization is not particularly limited, but is, for example, 5 to 300 minutes, preferably 10 to 200 minutes, and more preferably 15 to 150 minutes.
[0072] The supply rate (flow rate) of the gas phase in gas-phase deashing is not particularly limited, and is, for example, preferably 1 ml / min or more, more preferably 5 ml / min or more, and even more preferably 10 ml / min or more per gram of plant raw material or plant-derived char.
[0073] The apparatus used for gas-phase demineralization is not particularly limited as long as it is an apparatus capable of heating the plant raw material or plant-derived char and the gas phase containing a halogen compound while mixing them. For example, a continuous or batch type in-bed flow type apparatus using a fluidized bed or the like using a fluidized furnace can be used.
[0074] When gas-phase demineralization is performed, a heat treatment in the absence of a halogen compound may be performed after the heat treatment in the gas phase containing a halogen compound. Usually, a halogen is contained in the plant raw material or the char derived from a plant by the heat treatment in the gas phase containing a halogen compound. The halogen contained in the plant raw material or the char derived from a plant can be removed by the heat treatment in the absence of a halogen compound. For example, the halogen can be removed by performing the heat treatment after the heat treatment in the gas phase containing the halogen compound by cutting off the supply of the halogen compound. Specifically, the heat treatment in the absence of a halogen compound may be performed by performing the heat treatment at 500°C to 1100°C, preferably 600°C to 1050°C, more preferably 650°C to 1000°C, and even more preferably 850°C to 1000°C in an inert gas atmosphere not containing a halogen compound. The temperature of the heat treatment in the absence of a halogen compound is preferably the same as or higher than the temperature of the heat treatment in the gas phase containing a halogen compound. The time for the heat treatment in the absence of a halogen compound is not particularly limited, but is preferably 5 to 300 minutes, more preferably 10 to 200 minutes, and even more preferably 10 to 100 minutes.
[0075] The liquid-phase demineralization and gas-phase demineralization in this embodiment are treatments for removing ash such as potassium and iron contained in the plant raw material or plant-derived char. The potassium element content of the carbon precursor obtained after the liquid-phase demineralization treatment or the gas-phase demineralization treatment is preferably 1000 ppm (0.1 wt%) or less, more preferably 500 ppm or less, and even more preferably 300 ppm or less. The iron element content of the carbon precursor obtained after the liquid-phase demineralization treatment or the gas-phase demineralization treatment is preferably 200 ppm or less, more preferably 150 ppm or less, and even more preferably 100 ppm or less. If the potassium element or iron element content of the carbon precursor is the above upper limit or less, when the obtained carbonaceous material is used for an electrode for an electrochemical device such as a nonaqueous electrolyte secondary battery, the elution of impurities into the electrolyte during dedoping can be reduced, which is preferable in terms of improving the performance and reliability of the electrochemical device.
[0076] When a plant raw material is used for liquid-phase demineralization or vapor-phase demineralization, char derived from the plant after liquid-phase demineralization or vapor-phase demineralization can be produced by calcining the plant raw material after the liquid-phase demineralization or vapor-phase demineralization treatment in an inert gas atmosphere at a temperature of 300° C. or higher. The heat treatment temperature and heat treatment time for the calcination in this case are also as described above.
[0077] In addition, the average particle size of the plant raw material or plant-derived char to be deashed is not particularly limited. When performing liquid-phase deashing, from the viewpoint of easily separating the carbon precursor after deashing from the extract, the lower limit of the average particle size is preferably 500 μm or more, more preferably 1 mm or more, and even more preferably 2 mm or more. The upper limit of the average particle size is preferably 40 mm or less, more preferably 35 mm or less, and even more preferably 30 mm or less. When performing gas-phase deashing, if the average particle size is too small, it may be difficult to separate the gas phase containing potassium and the like removed by deashing from the carbon precursor after deashing, so the lower limit of the average particle size is preferably 100 μm or more, more preferably 200 μm or more, and even more preferably 400 μm or more. The upper limit of the average particle size is preferably 10000 μm or less, more preferably 8000 μm or less, and even more preferably 5000 μm or less.
[0078] The carbon precursor obtained through such treatment can be subjected to the above-described primary pulverization, classification, secondary pulverization, and firing to obtain the carbonaceous material of the present invention.
[0079] In addition, in the present invention, the carbonaceous material of the present invention having a desired AE can also be prepared by mixing two or more types of carbon precursors or carbonaceous materials having different physical properties (for example, average particle size, particle size distribution, etc.). When preparing the carbonaceous material of the present invention having a desired AE by mixing two or more types of carbon precursors or carbonaceous materials, the types of carbon precursors or carbonaceous materials to be mixed and their blending ratios can be appropriately determined according to the desired AE. In this case, it is also preferable that at least one carbon precursor or carbonaceous material to be mixed is a carbon precursor or carbonaceous material obtained through each of the above-mentioned steps of primary grinding, classification, and secondary grinding. By using at least one carbon precursor or carbonaceous material obtained through each of the above-mentioned steps, it is easier to control the AE of the obtained carbonaceous material to a desired range.
[0080] When preparing the carbonaceous material of the present invention by mixing two or more kinds of carbon precursors or carbonaceous materials, the blending amount of the carbon precursor or carbonaceous material produced through each of the steps of the primary grinding, classification, and secondary grinding may be appropriately determined depending on the physical properties of the carbon precursor or carbonaceous material used, and is, for example, 20 mass% or more based on the total mass of the final carbon precursor or carbonaceous material mixture. There is no particular upper limit to the blending amount of the carbon precursor or carbonaceous material produced through each of the steps of the primary grinding, classification, and secondary grinding in the carbon precursor or carbonaceous material mixture, and all of them may be carbon precursors or carbonaceous materials produced according to the above method.
[0081] [Electrodes for electrochemical devices] The carbonaceous material of the present invention is suitable as a material for electrodes for electrochemical devices, particularly negative electrodes for electrochemical devices. By using the carbonaceous material of the present invention, the density of the obtained electrode can be increased and the irreversible capacity can be reduced, so that a small-sized, high-capacity electrochemical device can be obtained. Electrochemical devices suitable for use with the carbonaceous material of the present invention include secondary batteries such as lithium ion secondary batteries, nickel hydrogen secondary batteries, and nickel cadmium secondary batteries, and capacitors such as electric double layer capacitors. Of these, the electrochemical device may be particularly a non-aqueous electrolyte secondary battery (e.g., lithium ion secondary battery, sodium ion battery, lithium sulfur battery, lithium air battery, all-solid-state battery, organic radical battery, etc.), and more particularly a lithium ion secondary battery.
[0082] In the following, the negative electrode for electrochemical devices of the present invention will be described using a negative electrode for a non-aqueous electrolyte secondary battery as an example. The negative electrode of the present invention can be produced by applying an electrode mixture to a current collector plate and forming an electrode active material layer on the current collector plate. The electrode mixture can be obtained by adding an appropriate amount of a binder, an optional conductive assistant, and an appropriate solvent to the carbonaceous material of the present invention and kneading them. The electrode active material layer can be formed, for example, by applying the electrode mixture to a current collector plate, drying it, and then pressure molding it. As the current collector plate, for example, a metal plate may be used.
[0083] The binder is not particularly limited as long as it does not react with the electrolyte, and examples thereof include PVDF (polyvinylidene fluoride), polytetrafluoroethylene, and a mixture of SBR (styrene butadiene rubber) and CMC (carboxymethyl cellulose). Among these, PVDF is preferable because PVDF attached to the surface of the active material does not inhibit lithium ion movement and is easy to obtain good input / output characteristics. One type of binder may be used, or two or more types may be used in combination. The amount of binder added may be appropriately selected depending on the type of binder used, and is preferably 1 to 20 mass%, and more preferably 1 to 15 mass%. For example, in the case of a PVDF-based binder, it is preferably 3 to 13 mass%, and more preferably 3 to 10 mass%. Here, the amount of binder added is calculated as the amount of active material (carbonaceous material) + the amount of binder + the amount of conductive assistant = 100 mass%. When the amount of binder added is within the above range, an increase in resistance in the obtained electrode can be suppressed, the internal resistance of the battery can be reduced, and the bonds between the particles of the carbonaceous material in the electrode and between the carbonaceous material and the current collector can be improved.
[0084] The solvent may be appropriately selected depending on the type of binder used. One type of solvent may be used, or two or more types may be used in combination. For example, when PVDF is used as the binder, it is preferable to use a polar solvent such as N-methylpyrrolidone (NMP) from the viewpoint of easily dissolving PVDF to obtain a slurry. When SBR or the like is used as the binder, the binder may be used in the form of an aqueous emulsion. When CMC is used as the binder, the binder may be used by dissolving it in a solvent such as water.
[0085] For example, water is often used as a solvent, and two or more binders, such as a mixture of SBR and CMC, are used in combination. In this embodiment, when two or more binders are used, the total amount of binders added is preferably 0.5 to 5 mass%, more preferably 1 to 4 mass%. Here, the amount of binder added is calculated as the amount of active material (carbonaceous material) + the amount of binder + the amount of conductive assistant = 100 mass%.
[0086] For the purpose of imparting even higher conductivity, a conductive assistant may be added as necessary when preparing the electrode mixture. As the conductive assistant, conductive carbon black, vapor grown carbon fiber (VGCF), nanotubes, etc. can be used. The amount of the conductive assistant added varies depending on the type of conductive assistant used, but is preferably 0.5 to 10 mass%, more preferably 0.5 to 7 mass%, and even more preferably 0.5 to 5 mass%. Here, the amount of the conductive assistant added is calculated as the amount of active material (carbonaceous material) + the amount of binder + the amount of conductive assistant = 100 mass%. When the amount of the conductive assistant added is within the above range, the conductivity is easily improved, and the dispersion of the conductive assistant in the electrode mixture is also good.
[0087] The electrode active material layer is usually formed on both sides of the current collector plate, but may be formed on one side of the current collector plate as necessary. The thickness of the electrode active material layer per side is preferably 10 to 80 μm, more preferably 20 to 75 μm, and even more preferably 20 to 60 μm. When the thickness of the electrode active material layer is equal to or greater than the above lower limit, the proportion of the current collector plate, separator, etc. in the secondary battery can be reduced, which is preferable from the viewpoint of facilitating the increase in the capacity of the battery. When the thickness of the electrode active material layer is equal to or less than the above upper limit, it is preferable from the viewpoint of facilitating the increase in the input / output characteristics, since the larger the electrode area facing the counter electrode, the more advantageous it is for improving the input / output characteristics.
[0088] In addition, for the purpose of reducing the irreversible capacity of the obtained electrode active material layer, lithium pre-doping can be carried out by a known method.
[0089] [Electrochemical Devices] The electrochemical device of the present invention includes the negative electrode for electrochemical devices of the present invention, and has high electrode density, small irreversible capacity, and high capacity.
[0090] For example, when the electrochemical device of the present invention is a non-aqueous electrolyte secondary battery, other materials constituting the battery, such as the positive electrode material, the separator, and the electrolyte, are not particularly limited, and various materials that have conventionally been used or proposed in non-aqueous electrolyte secondary batteries can be used.
[0091] For example, the positive electrode material is a layered oxide system (LiMO 2 where M is a metal, e.g. LiCoO 2 , LiNiO 2 , LiMnO 2 , or LiNi x Co y Mo z O 2 (where x, y, and z represent the composition ratios)), olivine system (LiMPO 4 where M is a metal: for example, LiFePO 4 etc.), spinel type (LiM 2 O 4 where M is a metal: for example, LiMn 2 O 4 As the positive electrode material, one of these chalcogen compounds may be used, or two or more of them may be mixed as necessary. The positive electrode can be manufactured by molding these positive electrode materials together with a suitable binder and a carbonaceous material for imparting electrical conductivity to the electrode, and forming a layer on a conductive current collector.
[0092] The non-aqueous electrolyte used in combination with the positive and negative electrodes can generally be obtained by dissolving an electrolyte in a non-aqueous solvent. Examples of the non-aqueous solvent include organic solvents such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, dimethoxyethane, diethoxyethane, γ-butyllactone, tetrahydrofuran, 2-methyltetrahydrofuran, sulfolane, and 1,3-dioxolane. As the organic solvent, one type of organic solvent may be used, or two or more types of organic solvents may be used in combination. Examples of the electrolyte include LiClO 4 , LiPF 6 , LiBF 4 , LiCF 3 SO 3 , LiAsF 6 , LiCl, LiBr, LiB(C 6 H 5 ) 4 , or LiN(SO 3 CF 3 ) 2 etc.
[0093] A non-aqueous electrolyte secondary battery can generally be produced by immersing a positive electrode and a negative electrode, optionally with a separator between them, in an electrolyte solution. As the separator, a liquid-permeable separator made of a nonwoven fabric or other porous material that is commonly used in secondary batteries can be used. Instead of or together with the separator, a solid electrolyte made of a polymer gel impregnated with an electrolyte solution can also be used.
[0094] The carbonaceous material of the present invention is suitable as a carbonaceous material for a battery (typically a nonaqueous electrolyte secondary battery for driving a vehicle) mounted on a vehicle such as an automobile. In the present invention, the vehicle can be, without particular limitation, what is usually known as an electric vehicle, a hybrid vehicle with a fuel cell or an internal combustion engine, etc., and is equipped with at least a power supply device equipped with the above-mentioned battery, an electric drive mechanism driven by power supply from the power supply device, and a control device for controlling the same. The vehicle may further be equipped with a dynamic brake or a regenerative brake, and may be equipped with a mechanism for converting energy generated by braking into electricity and charging the nonaqueous electrolyte secondary battery. EXAMPLES
[0095] The present invention will be described in detail below with reference to examples, but the scope of the present invention is not limited thereto. Note that, although the measurement methods of the physical properties of the carbonaceous material are described below, the physical properties described in this specification, including the examples, are based on values determined by the following methods.
[0096] (1) Average particle diameter D 50 and particle size distribution index D 50 / D 10 Measurement and calculation Average particle size D of carbon precursor and carbonaceous material 50 (Particle size distribution) was measured by a laser scattering method as follows. Samples of the carbon precursor and carbonaceous material prepared in the examples and comparative examples described below were placed in an aqueous solution containing 0.3 mass % of a surfactant ("ToritonX100" manufactured by Wako Pure Chemical Industries, Ltd.), treated with an ultrasonic cleaner for 10 minutes or more, and dispersed in the aqueous solution. The particle size distribution was measured using this dispersion. The particle size distribution was measured using a particle size / particle size distribution measuring instrument ("Microtrac MT3000" manufactured by Nikkiso Co., Ltd.), with the solvent refractive index set to 1.33 and particle permeability set to absorption. The particle size at which the cumulative volume reached 50% was defined as the average particle size D 50 It was decided. The particle size at which the cumulative volume becomes 10% is D 10 The particle size distribution index D is calculated using the following formula: 50 / D 10 was calculated. Particle size distribution index D50 / D 10 =Average particle diameter D 50 / D 10
[0097] (2) Measurement of BET specific surface area In this specification, the specific surface area of the carbonaceous material and the carbon precursor is determined by the BET method (nitrogen adsorption BET three-point method) (BET specific surface area). The approximate formula derived from the BET formula is shown below.
[0098]
number
[0099] Using the above approximation, v is calculated by the three-point method using nitrogen adsorption at liquid nitrogen temperature. m and calculate the specific surface area of the sample using the following formula:
[0100]
number
[0101] At this time, v m is the amount of adsorption (cm) required to form a monolayer on the sample surface. 3 / g), v is the measured adsorption amount (cm 3 / g), p 0 is the saturated vapor pressure, p is the absolute pressure, c is a constant (reflecting the heat of adsorption), and N is Avogadro's number 6.022 × 10 23 , a(nm 2 ) is the area that the adsorbate molecule occupies on the sample surface (molecular occupancy cross-sectional area).
[0102] More specifically, the amount of nitrogen adsorbed to a sample at liquid nitrogen temperature can be measured using, for example, "BELL Sorb Mini" manufactured by BELL Japan, as follows: The sample is filled into a sample tube, and the tube is cooled to -196°C, and then the pressure is reduced once, and nitrogen (purity 99.999%) is adsorbed to the sample at a desired relative pressure. The amount of nitrogen adsorbed to the sample when equilibrium pressure is reached at each desired relative pressure is defined as the amount of adsorbed gas v.
[0103] (3) Measurement of flow energy (AE) during ventilation The measurements were carried out using a Freeman Technology FT4 powder rheometer. The measurement vessel (diameter 50 mm, volume 160 mm 3 ) was filled to the brim with the carbonaceous material to be measured for AE (120 mL), and then placed in the device. Air was then passed through the bottom of the device at a rate of 2 mm / sec, and a blade (radius: 48 mm) was rotated at a blade tip speed of 100 mm / sec while entering the device. At this time, the helical angle α at which the blade tip moved was 5°. The energy of the blade movement according to the blade height was calculated using the following formula: AE=T / (Rtanα)+F The flow energy during aeration (AE) was calculated according to the following formula.
[0104] (4) Average interplanar spacing d of (002) plane by X-ray diffraction method 002 Using "MiniFlexII manufactured by Rigaku Corporation," the carbonaceous material powder was filled into the sample holder, and an X-ray diffraction pattern was obtained using CuKα radiation monochromatized by a Ni filter as the radiation source. The peak positions of the diffraction pattern were determined by the centroid method (a method of determining the centroid position of the diffraction line and determining the peak position at the corresponding 2θ value), and were corrected using the diffraction peak of the (111) plane of high-purity silicon powder for standard material. The wavelength λ of CuKα radiation was set to 0.15418 nm, and d002 was calculated using the Bragg formula (formula (IV)) shown below.
number
[0105] 1. Example 1 (1) Preparation of carbon precursor <Preparation Example 1> Gas-phase demineralization: Coconut shells were dry-distilled at 500°C and then crushed to obtain coconut shell char with an average particle size of approximately 2 mm. 100 g of this coconut shell char was subjected to halogen heat treatment at 900°C for 30 minutes while supplying nitrogen gas containing 1% by volume of hydrogen chloride gas at a flow rate of 18 L / min. After that, the supply of hydrogen chloride gas was stopped, and while supplying nitrogen gas at a flow rate of 18 L / min, a gas-phase deoxidation treatment was performed by further heat treatment at 900°C for 30 minutes to obtain a carbon precursor.
[0106] (2) Preparation of carbonaceous materials Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 4.1 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 3.3 volume %. Secondary pulverization process: The classified carbon precursor is pulverized to an average particle size D using the same fine mill SF5 as used in the primary pulverization. 50 The carbon precursor was obtained by crushing the powder to a diameter of 2.8 μm. 50 / D 10 was 3.9. Calcination step: 6.4 g of the carbon precursor prepared above was mixed with 0.6 g of polystyrene (manufactured by Sekisui Chemical Co., Ltd., average particle size 400 μm, residual carbon rate 1.2%). 7 g of this mixture was placed in a graphite sheath so that the sample layer height was approximately 3 mm, and in a tubular furnace manufactured by Motoyama Co., Ltd., the temperature was raised to 1250°C at a rate of 10°C per minute under a nitrogen flow rate of 6 L per minute, and then the material was held for 10 minutes and allowed to cool naturally. After confirming that the temperature inside the furnace had dropped to 200°C or less, the carbonaceous material was removed from the furnace. The average particle diameter D of the obtained carbonaceous material was 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0107] 2. Example 2 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 8.9 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 0 volume %. Secondary pulverization process: The classified carbon precursor is pulverized into particles with an average particle diameter D using the same ball mill as that used for the primary pulverization. 50 The carbon precursor was obtained by crushing the powder to a diameter of 2.9 μm. 50 / D 10 was 3.9. After the secondary pulverization, the carbonaceous material was obtained by performing a firing treatment in the same manner as in Example 1. The average particle diameter D 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0108] 3. Example 3 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 102 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 0 volume %. Secondary pulverization process: The classified carbon precursor is pulverized into particles with an average particle diameter D using the same ball mill as that used for the primary pulverization. 50 The carbon precursor was obtained by crushing the powder to a diameter of 2.8 μm. 50 / D 10 was 3.1. After the secondary pulverization, the carbonaceous material was obtained by performing a firing treatment in the same manner as in Example 1. The average particle diameter D 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0109] 4. Comparative Example 1 The carbon precursor obtained in Preparation Example 1 was pulverized to an average particle size of 2.5 μm using a fine mill SF5 (manufactured by Nippon Coke). Thereafter, without classification or secondary pulverization, the carbonaceous material was obtained by performing a firing treatment in the same manner as in Example 1. The average particle diameter D 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0110] 5. Comparative Example 2 The carbon precursor obtained in the same manner as in the primary grinding of Comparative Example 1 was classified using Labocrasseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 6.1% by volume. Next, the classified carbon precursor was crushed into particles having an average particle diameter D 50 The powder was crushed to a diameter of 1.4 μm. 50 / D 10 After the secondary pulverization, the carbonaceous material was subjected to a firing treatment in the same manner as in Example 1 to obtain a carbonaceous material. The average particle diameter D 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0111] 6. Comparative Example 3 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 310 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 0 volume %. Secondary pulverization process: The classified carbon precursor is pulverized into particles with an average particle diameter D using the same ball mill as that used for the primary pulverization. 50 The carbon precursor was obtained by crushing the powder to a diameter of 2.6 μm. 50 / D10 was 1.9. After the secondary pulverization, the carbonaceous material was obtained by performing a firing treatment in the same manner as in Example 1. The average particle diameter D 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0112] 7. Comparative Example 4 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 8.9 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 0 volume %. Thereafter, without carrying out secondary pulverization, a calcination treatment was carried out in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0113] 8. Comparative Example 5 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 It was ground to a size of 25 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 0 volume %. Thereafter, without carrying out secondary pulverization, a calcination treatment was carried out in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0114] 9. Comparative Example 6 The carbon precursor obtained in Example 2 was subjected to a d 50 The particles were classified so that the particle size was 3.4 μm. Thereafter, a firing treatment was carried out in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0115] 10. Comparative Example 7 The carbon precursor obtained in Comparative Example 5 was subjected to a d 50 The particles were classified so that the particle size was 51.0 μm. Thereafter, a firing treatment was carried out in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0116] 11. Comparative Example 8 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 4.1 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 3.3 volume %. Secondary pulverization process: The classified carbon precursor is pulverized into particles with an average particle diameter D using the same ball mill as that used for the primary pulverization. 50 The carbon precursor was obtained by crushing the powder to a diameter of 0.9 μm. 50 / D 10 was 2.2. After the secondary pulverization, the carbonaceous material was obtained by performing a firing treatment in the same manner as in Example 1. The average particle diameter D 50 , D 50 / D 10, BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0117] 12. Example 4 Blending: The carbon precursor of Example 2 and the carbon precursor of Comparative Example 4 were mixed in a mass ratio of 1:1 to obtain a carbon precursor mixture. The obtained mixture of carbon precursors was added with polystyrene and subjected to a firing treatment in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0118] 13. Example 5 Blending: The carbon precursor of Example 2 and the carbon precursor of Comparative Example 5 were mixed in a mass ratio of 1:1 to obtain a carbon precursor mixture. The obtained mixture of carbon precursors was added with polystyrene and subjected to a firing treatment in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0119] 14. Example 6 Blending: The carbon precursor of Example 2 and the carbon precursor of Comparative Example 7 were mixed in a mass ratio of 1:1 to obtain a carbon precursor mixture. The obtained mixture of carbon precursors was added with polystyrene and subjected to a firing treatment in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0120] 15. Comparative Example 9 Blend: The carbon precursor of Comparative Example 2 and the carbon precursor of Comparative Example 4 were mixed in a mass ratio of 1:1 to obtain a carbon precursor mixture. The obtained mixture of carbon precursors was added with polystyrene and subjected to a firing treatment in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0121] 16. Comparative Example 10 Primary pulverization step: The carbon precursor obtained in Preparation Example 1 was milled using a fine mill SF5 (manufactured by Nippon Coke) to a mean particle size D 50 The powder was ground to a size of 4.1 μm. Classification step: The carbon precursor after the primary grinding was classified using Labocruseal N-01 (manufactured by Seishin Enterprise Co., Ltd.) so that the volume ratio of particles of 1 μm or less became 3.3 volume %. Secondary pulverization process: The classified carbon precursor is pulverized into particles with an average particle diameter D using the same ball mill as that used for the primary pulverization. 50 The carbon precursor was obtained by crushing the powder to a diameter of 1.2 μm. 50 / D 10 was 2.5. After the secondary pulverization, the carbonaceous material was obtained by performing a firing treatment in the same manner as in Example 1. The average particle diameter D 50 , D 50 / D 10 , BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0122] 17. Example 7 Blend: The carbon precursor of Comparative Example 4 and the carbon precursor of Comparative Example 10 were mixed in a mass ratio of 55:45 to obtain a carbon precursor mixture. The obtained mixture of carbon precursors was added with polystyrene and subjected to a firing treatment in the same manner as in Example 1 to obtain a carbonaceous material. 50 , D 50 / D 10, BET specific surface area, AE and average interplanar spacing d 002 The results are shown in Table 1.
[0123] [Table 1]
[0124] The carbonaceous materials obtained in the examples and comparative examples were used to evaluate the battery characteristics according to the following methods. The results are shown in Table 2.
[0125] <Creating electrodes and checking their status> 96.2 parts by mass of each carbonaceous material obtained in the examples and comparative examples, 2 parts by mass of conductive carbon black ("Super-P (registered trademark)" manufactured by TIMCAL), 1 part by mass of CMC, 0.8 parts by mass of SBR, and water were mixed to obtain a slurry. Each of the obtained slurries was applied to copper foil, dried, and pressed to obtain a negative electrode (negative electrode layer).
[0126] <Electrode density> The thickness of the negative electrode layer was determined by measuring the thickness of the produced negative electrode layer with a micrometer and then subtracting the thickness of the current collector plate from the measured thickness. Electrode density (g / cm 3 ) is the mass (g) of the carbonaceous material mixed in the slurry when preparing the negative electrode layer, and the volume (cm) of the prepared negative electrode layer. 3 ) divided by (g / cm 3 ) The volume of the negative electrode layer was calculated using the thickness and diameter (14 mm) of the negative electrode layer. When an electrode that could be evaluated was created, the electrode condition was evaluated as ○, and when lumps, air bubbles, falling off of the negative electrode layer, etc. occurred during electrode creation, making the electrode inevaluable, the electrode condition was evaluated as ×.
[0127] <Measurement of charge capacity, discharge capacity, charge / discharge efficiency and initial DC resistance> Each electrode prepared above was used as the working electrode, and metallic lithium was used as the counter electrode and reference electrode. A mixture of ethylene carbonate and methyl ethyl carbonate (volume ratio 3:7) was used as the solvent. LiPF 6The electrolyte was prepared by dissolving 1 mol / L of the above. A glass fiber nonwoven fabric was used as the separator. Coin cells were prepared in a glove box under an argon atmosphere. A charge / discharge test was performed on the lithium ion secondary battery having the above configuration using a charge / discharge tester (manufactured by Toyo Systems Co., Ltd., "TOSCAT"). The initial DC resistance was the resistance value generated when 0.5 mA was applied for 3 seconds. Lithium doping was performed at a rate of 70 mA / g relative to the active material mass, and doping was continued until the lithium potential reached 1 mV. A constant voltage of 1 mV was further applied to the lithium potential for 8 hours to terminate the doping. The capacity (mAh / g) at this time was taken as the charge capacity. Next, dedoping was performed at a rate of 70 mA / g relative to the active material mass until the lithium potential reached 2.5 V, and the capacity discharged at this time was taken as the discharge capacity. Discharge capacity x electrode density was taken as the volumetric capacity. The percentage of discharge capacity / charge capacity was taken as the charge / discharge efficiency, which was used as an index of the utilization efficiency of lithium ions in the battery.
[0128] [Table 2]
Claims
1. The specific surface area measured by the BET method is 23 m 2 / g or less, and an aeration flow energy (AE) measured by a powder rheometer is 40 mJ or more and 210 mJ or less.
2. The average particle diameter D at which the cumulative volume from the fine particle side becomes 50% in the particle size distribution measured by the laser scattering method 50 is 1 μm or more and 50 μm or less, and the particle diameter D at which the cumulative volume from the fine particle side becomes 10% 10 and average particle diameter D 50 Particle size distribution index D 50 / D 10 The carbonaceous material according to claim 1 , wherein the MnO 2 is 1.9 or more.
3. The average interplanar spacing d of the (002) plane calculated using the Bragg equation by wide-angle X-ray diffraction method 002 The carbonaceous material according to claim 1 or 2, wherein the average particle diameter is 0.36 nm or more.
4. The carbonaceous material according to any one of claims 1 to 3, wherein the carbonaceous material is derived from a plant.
5. A negative electrode for a non-aqueous electrolyte secondary battery, comprising the carbonaceous material according to any one of claims 1 to 4.
6. A non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte secondary battery according to claim 5 .
7. A step of subjecting the carbon precursor or the calcined product of the carbon precursor to primary grinding; A step of classifying the carbon precursor after the primary grinding or the calcined product of the carbon precursor; and A step of subjecting the classified carbon precursor or the calcined product of the carbon precursor to secondary pulverization; and Calcining the carbon precursor The method for producing the carbonaceous material according to any one of claims 1 to 4, comprising:
8. In the primary grinding process, the average particle diameter D 50The method according to claim 7 , wherein the carbon precursor or the calcined product of the carbon precursor is pulverized to have a particle size of 2.7 μm or more and 300 μm or less.
9. 9. The method for producing a carbonaceous material according to claim 7 or 8, wherein in the classification step, the carbon precursor after the primary grinding or the calcined product of the carbon precursor is classified so that a content of particles having a particle diameter of 1 μm or less is 6 vol % or less.
10. In the secondary grinding process, the average particle diameter D 50 is 1 μm or more and 50 μm or less, and the particle diameter D at which the cumulative volume is 10% 10 and average particle diameter D 50 Particle size distribution index D 50 / D 10 The method according to any one of claims 7 to 9, wherein the carbon precursor after classification or the calcined product of the carbon precursor is pulverized so that the average particle size distribution becomes 1.9 or more.
Citation Information
Patent Citations
Carbonaceous substance for electrode material
JP2006269961A
Negative electrode material for lithium ion secondary battery and lithium ion secondary battery
JP2014089887A
Carbonaceous material for nonaqueous electrolyte secondary battery, negative electrode and nonaqueous electrolyte secondary battery
JP2017073325A
Hardly graphitizable carbonaceous material for nonaqueous electrolyte secondary batteries used in fully charged state, method for producing same, negative electrode material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery in fully charged state
WO2017022486A1
Carbonaceous material for non-aqueous electrolyte secondary battery, negative electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for producing carbonaceous material for non-aqueous electrolyte secondary battery
WO2017073687A1