WC-based cemented carbide and its applications

By integrating high-entropy alloys into WC-based cemented carbide, the material achieves ductile machining and superior optical performance, addressing the processing challenges of brittle fracture and enhancing the quality of optical components.

JP7584671B2Active Publication Date: 2024-11-15XIAMEN TUNGSTEN CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023548996
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-18
Filing Date
2022-04-25
Publication Date
2024-11-15
Estimated Expiration
2042-04-25

AI Technical Summary

Technical Problem

Cemented carbide materials are difficult to process in a ductile mode, leading to brittle fracture during machining, which complicates the production of high-quality optical components like micro prisms and spherical lenses.

Method used

Incorporating high-entropy alloys (HEA) with specific elements into WC-based cemented carbide to enhance toughness, thermal conductivity, and oxidation resistance, while maintaining high hardness and strength, allowing for plastic deformation during machining.

Benefits of technology

The resulting WC-based cemented carbide exhibits improved toughness, thermal conductivity, and oxidation resistance, enabling high-precision machining with minimal surface defects and enhanced optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584671000001
    Figure 0007584671000001
  • Figure 0007584671000002
    Figure 0007584671000002
  • Figure 0007584671000003
    Figure 0007584671000003
Patent Text Reader

Abstract

The present invention relates to a WC-based cemented carbide having a molecular formula of T-WC-HEA, where T is a carbide, an oxide, or a phosphatase. The HEA is at least one of Al, Cu, Nb, Ti, Zr, Ge, Si, V, Ta, Cr, Mn, Ce, Mo, W, and Hf, and the HEA is a high-entropy alloy. The HEA is at least five elements selected from Al, Cu, Nb, Ti, Zr, Ge, Si, V, Ta, Cr, Mn, Ce, Mo, W, and Hf, and the T includes the element B. The WC-based cemented carbide has an HEA content of 0.5 wt% to 5 wt%, a T content of 35 wt% or less, and the remainder being WC and unavoidable impurities. The B content is 0.1 wt% to 3 wt%. The HEA has a melting point of 1850°C or less. The atomic ratio of each element contained in the HEA is 0.33 to 1, as measured by an energy spectrometer. This new WC-based cemented carbide has excellent strength and toughness, high thermal conductivity and thermal stability, and high density, and achieves optical surface conditions after processing.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hard metal, in particular to a WC-based hard metal. [Background technology]

[0002] Cemented carbide has features such as high hardness, wear resistance, corrosion resistance, and low thermal expansion coefficient, and is widely used in precision molds and wear-resistant and corrosion-resistant parts manufactured by optical glass molding and metal stretching. Molds made of cemented carbide have a long life, more than 10 times, or even several hundred times, of steel molds, and the surface of the products is very high performance, so the parts manufactured such as glass lenses can meet the optical surface quality requirements. However, since cemented carbide is a typical difficult-to-machine material, even higher properties of cemented carbide are required when machining cemented carbide molds such as micro prisms and spherical lenses that have optical surface quality. WC-based cemented carbide is a hard and brittle material, and in conventional cutting, it is removed in the form of brittle fracture. How to realize ductile mode cutting of cemented carbide and remove it in the form of plastic deformation to obtain good machined surface quality is a major challenge in the field of cemented carbide. Summary of the Invention

[0003] The object of the present invention is to overcome the shortcomings of the prior art and provide a new alloy system of WC-based cemented carbide, which includes high-entropy alloys and fully utilizes the role of the B element, giving the alloy as a whole excellent strength and toughness, high thermal conductivity, thermal stability, and high density, and can be processed to achieve a surface that meets optical requirements.

[0004] One embodiment of the present invention is as follows. A WC-based cemented carbide with the molecular formula T-WC-HEA, where T is a small amount of carbide, oxide or boride. At least one of the HEAs is a high entropy alloy, and the HEA is selected from the group consisting of Al, Cu, Nb, Ti, Zr At least five elements are selected from the group consisting of Ge, Si, V, Ta, Cr, Mn, Ce, Mo, W, and Hf; The T contains the element B, and the WC-based cemented carbide contains 0.5 wt% to 5 wt% of HEA. The content of the T is 35 wt% or less, the remainder being WC and unavoidable impurities, the content of the element B is 0.1 wt% to 3 wt%, and the atomic ratio of each element contained in the HEA is The measured value by an Energy Dispersive Spectrometer (EDS) is 0.33 to 1. The melting point of the HEA is 1850° C. or lower, preferably 1700° C. or lower.

[0005] The inventor has conducted research for many years and has selected and combined five or more specific elements to form The HEA formed does not increase the hardness of the WC-based cemented carbide, but improves the wettability with the WC granules during sintering. It was found that the addition of WC to HEA improved toughness and at the same time suppressed the abnormal growth of WC granules to some extent. However, it is difficult to form a complete solid solution of WC and HEA in the WC-HEA system. Therefore, the oxidation resistance at high temperatures is poor. In addition, sintering is a competitive process between nucleation and growth, and HEA grains tend to grow rapidly, resulting in the formation of coarse grains and the deterioration of the mechanical properties of the alloy. Experiments have shown that B has a synergistic effect with HEA in the alloy system, and B can form free metal elements and metal borides stacked on the surface of HEA, reduce or eliminate crystal defects in the alloy system, improve the integrity of the alloy phase structure and the oxidation resistance at high temperatures, and also play the role of an HEA grain growth inhibitor and improve the grain size. In the alloy system, HEA and B have a synergistic effect, and the resulting WC-based cemented carbide is far superior to conventional WC-Co-based cemented carbide in terms of strength, toughness, and oxidation resistance at high temperatures. , conventional WC-Mo 2 In comparison with non-bonded phase cemented carbides such as C-SiC and WC-TiC-TaC, the hardness Although not superior, the toughness is clearly improved. Also, as the study shows, the addition of HEA Adding this material is advantageous in improving the thermal conductivity of the alloy and reducing the amount of thermal expansion, and it greatly improves the high-temperature processing performance of optical mold substrates, which require high molding accuracy.

[0006] In a preferred embodiment, T is Al 4 C 3 , HfC, TiC, Cr 3 C 2 , VC, ZrC, NbC, TaC, SiC , Mn 3 C, MoC, CuC, Mg 2 C 3 , W 2 C, CeO 2 , La 2 O 3 , MgO, ZrO 2 , Al 2 O 3 , ZrB 2 ,CrB 2 , TiB 2 also MnB 2 At least two of these are present.

[0007] In a preferred embodiment, B is ZrB 2 ,CrB 2 , TiB 2 Or MnB 2 Transition metal borides such as Exist in the form of a thing.

[0008] In a preferred embodiment, the atomic ratio of each element in the HEA is determined by the energy spectrum. The measured value of the energy dispersive spectrometer (EDS) is 0.5 to 1. The maximum difference of the atomic radius of each element contained in the HEA is 0.33 or less, preferably 0.25 or less, and more preferably 0.17 or less. The atomic ratio and the difference value of the atomic radius determine the composition of the high entropy alloy to some extent, and affect the solid solution structure characteristics and further the processing characteristics of the cemented carbide. If the difference in atomic radius of each element contained in the HEA is too large, some of the metal atoms are pushed out and become free metal during the formation of the HEA, and the oxidation resistance of the alloy decreases. On the other hand, the closer the radius of each atom is to the same value, the better it is. If the atomic radius of each element is close to the same value, the more face-centered cubic phases will be formed in the alloy, the harder the alloy will be, and the friction and wear properties may be affected.

[0009] In a preferred embodiment, the HEA has the molecular formula Al 0.4 Hf 0.6 NbTaTiZr, AlMo 0.5 NbTa 0.5 TiZr , AlNbTaTiV, AlNb 1.5 Ta 0.5 Ti 1.5 Zr 0.5 , AlCr 2 Mo 2 Nb 2 Ti 2 Zr, HfMoNbTiZr, HfNbTaTiZr, HfNbTiVZr, CrNbTiVZr, CrMo 0.5 NbTa 0.5 At least one selected from TiZr, TiZrHfNbCr, TiNbMoTaW, TiVNbMoTaW, HfMoTaTiZr, or HfMoNbTaTiZr. The above molecular formula contains one metal element with a slightly larger atomic radius and another element with a similar atomic radius, and when the HEA is formed, the metal element with the slightly larger atomic radius enters the lattice, promoting the deformation of the lattice and facilitating the conversion from face-centered cubic phase to body-centered cubic phase. The selected elements are more likely to bond between atoms when sintered, forming a regular solid solution. In addition, the selected HEA is effective in improving the thermal conductivity and thermal stability of WC-based cemented carbide.

[0010] In a preferred embodiment, the HEA has a solid solution content of BCC phase of 80% or more. The BCC phase is predominant overall, which is suitable for the high hardness characteristics of WC-based cemented carbide, and the The occurrence of cracks and holes can be avoided.

[0011] In a preferred embodiment, the content of the solid solution of FCC phase in the HEA is 10% or more. If the material contains a large amount of FCC phase, the material as a whole becomes slightly soft and is more susceptible to plastic deformation during processing. This prevents adhesion to the surface and the generation of fine abrasive grains, improving the workability of WC-based cemented carbide.

[0012] In a preferred embodiment, the WC-based cemented carbide has a B content of 1.5 wt% to 3 wt%. The content of HEA is 2.5wt%~5wt%. As can be seen from the experiment, there is a correlation between the content of B and HEA. There is a correlation between them, and if the contents of both exceed the set ranges, excessive borides and boron carbides are generated in the cemented carbide, which makes sintering difficult and reduces toughness.

[0013] In a preferred embodiment, the WC-based cemented carbide has a B content of 0.1 wt% to 1.5 wt%. The content of HEA is 0.5wt%~2.5wt%. As can be seen from the experiment, the relationship between the content of B and HEA is There is a correlation between the two, and when the contents of both exceed the set range, the stable phase structure of HEA is lost. This can affect formation or increase the amount of free metal in the hardmetal, reducing its oxidation resistance.

[0014] In a preferred embodiment, the molecular formula of the WC-based cemented carbide is ZrC-ZrB 2 -WC-AlNb 1.5 Ta 0.5 Ti 1.5 Zr 0.5 It is.

[0015] In a preferred embodiment, the WC-based cemented carbide is provided with B contained in T and a compound formed by bonding with B. The elements that formed the compound are all contained in the HEA. Cemented carbide has high raw material utilization, uniform microstructure, and low cost.

[0016] In a preferred embodiment, the WC-based cemented carbide has an average particle size of 100 nm to 400 nm. The WC-based cemented carbide has a high density. The WC-based cemented carbide has a thermal conductivity of 72 W at room temperature. / m·K or more.

[0017] The wt% referred to in the present invention is % by weight. It should be noted that the ranges of values ​​disclosed herein include all values ​​within these ranges.

[0018] Another embodiment of the present invention provides a mold for optical glass, which is made of the above-mentioned WC-based cemented carbide, and the material of the optical glass includes one of silica, a resin material, and zinc selenide.

[0019] The resin material described in the present invention is not particularly limited, and may be, for example, polyester resin, polyamide resin, polyallyl sulfide resin, polyimide resin, polyether ether ketone resin, etc., and may also be polymethyl methacrylate, polystyrene, polycarbonate, polydiallyl diglycol carbonate, etc. may be also possible.

[0020] The novel WC-based cemented carbide alloy of the present invention is applied to optical glass molds and shows excellent performance in terms of workability. Optical glass die forming (compression molding) technology involves applying pressure to a mold at high temperature, reproducing the shape of the microlens array on the mold surface on the glass surface softened by heating, and then cooling and hardening through annealing treatment to obtain the desired glass microlens array. The WC-based cemented carbide according to the present invention has superior workability compared to conventional cemented carbide, and has a thermal conductivity of ≥ 72 W / m K and a density of ≥ 12 g cm -3 , hardness HRA≧70, fracture toughness ≧10 MPa·M 1 / 2 , bending strength ≧1600 N mm -2 , Oxidation weight gain ≦1.16 mg cm -2 This is due to the introduction of HEA and the synergistic effect with B. It is estimated that an effective distribution is formed in the WC-based cemented carbide, the material has good uniformity, there are no internal defects, and the surface roughness after processing is Ra≦10 nm. In addition, the increase in the thermal conductivity of the material itself This allows for quick heat transfer during high-temperature pressurization and reduced-pressure annealing, and the thermal expansion of the mold is very small, so mold deformation before and after molding is virtually zero. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will now be described in more detail with reference to examples. XRD: X-ray diffraction phase analysis was performed using a Bruker D8 DISCOVER X-ray diffractometer from Germany. The target is a rotating target with a light monochromator, operating voltage of 40 kV and current of 250 mA. The speed is 8° / min, and the range of the selected diffraction angle is 2θ=5 to 90°. Measurement of components: No gas using an inductively coupled plasma optical emission spectrometer (ICP-OES). Elemental impurities were determined. Morphological analysis: Surface observation and analysis were carried out on the grain morphology and crystalline phase of the cemented carbide by scanning electron microscope (SEM) and electron back-scattered diffraction (EBSD). Hardness test: Refer to GB / T 7997-2014 "Vickers hardness test method for cemented carbide". Bending strength: measured by CMT5305 microcomputer controlled universal testing machine, refer to GB / T 3851-2015 "Determination method for transverse fracture strength of cemented carbide". Toughness test: Refer to GB / T 33819-2017 "Low temperature toughness test of cemented carbide". Thermal conductivity: A laser thermal conductivity meter LFA457 manufactured by NETZSCH, Germany was used. Refer to the standard GB / T 22588-2008. Density: Measurements were performed using an AccuPyc II 1340 true density analyzer manufactured by Mike Corporation, USA. Oxidation resistance: Refer to GB / T 13303-1991 "Method of measurement of oxidation resistance of steel materials". Surface roughness: Measured by shadow retention method. GB / T 15056-2017 "Casting surface roughness" Please refer to the "Evaluation Method" for details. The ball mill used in the present invention is a planetary ball mill PULVERISETTE 5. The sintering described in this invention was carried out using a PVSGgr20 / 20 / Shimadzu Vacuum Sintering Furnace and / or an Agilent 1260Lnifntiy Spark Plasma Sintering Furnace and / or an Erinvicor HP20-36 Hot Isostatic Pressing Sintering Furnace.

[0022] The novel WC-based hard alloy of the present invention may be manufactured by any method, and there is no particular restriction on the manufacturing method, and it may be a powder sintering method or an alloy melting method. However, from an economical point of view, it is preferable to include the steps of raw material preparation, powder mixing, ball milling, pressing, and sintering. The raw materials include WC powder, powders of elements constituting the HEA, and ceramics consisting of carbides, oxides, and borides. Powders and the like are included. The WC powder is not particularly limited and may be appropriately selected as required. For example, WC powder having a particle size of 0.1 μm to 3 μm may be used. The single powder constituting the HEA is not particularly limited and may be appropriately selected as needed. For example, a simple powder having a particle size of 0.5 μm or less may be used, and the simple powder is successively subjected to operations such as vacuum melting, powdering by real air atomization, and sieving. The ceramic powder made of the above carbide, oxide or boride is not particularly limited and may be appropriately selected according to need, for example, a powder having a particle size of 0.5 μm to 5 μm. The ball milling process is not particularly limited and may be a dry or wet process. From the viewpoint of reducing the amount of oxygen, the dry ball mill method is preferred. The pressing method is not particularly limited, and any of dry pressing, cold isostatic pressing molding, and injection molding may be selected.

[0023] Example I The WC-based cemented carbide having the composition shown in Example I of Table 1 was prepared and obtained by the following procedure. (1) Preparation of raw materials The WC powder has an average particle size of 0.1 μm, the five metal powders (Al, Nb, Ta, Ti, Zr) that make up the HEA all have a particle size of 0.5 μm, and the ceramic powders made of boron carbide, titanium carbide, tantalum carbide, or alumina have a particle size of 0.5 μm. (2) Ball Mill a. High-energy ball milling (HEBM) of the single powders constituting the HEA was carried out under an inert atmosphere with a ball to powder weight ratio of 15:1, a rotation speed of 400 r / min, and cemented carbide balls as ball milling media for 24 hours to obtain the HEA alloy powder. b.WC powder and ceramic powder were added, and then ball milled in vacuum, with a ball-to-material ratio of 5:1, and a rotation speed of 100 r / rpm for 40 hours. (3) Press processing The raw billet was obtained by pressing at a pressure of 180 MPa and holding for 120 seconds. (4) Sintering The raw billet is placed in a sintering furnace, and sintered at a temperature of 1600°C and a sintering pressure of 60Mpa under a vacuum of 10 Pa or more. The WC-based cemented carbide was obtained after 30 minutes of spark plasma sintering and cooling, and the surface was polished using nano-diamond grind paste.

[0024] The method for producing a WC-based cemented carbide having the composition shown in Comparative Example 3 in Table 1 differs from Example 1 in that the raw materials do not contain a simple substance powder of HEA. The method for producing a WC-based cemented carbide having the composition shown in Comparative Example 4 in Table 1 differs from Example 1 in that the raw materials do not contain ceramic powder made of carbide, oxide or boride. [Table 1] The molecular formula of the HEA in Example I is AlNb 1.5 Ta 0.5 Ti 1.5 Zr 0.5 It was measured to be. The cemented carbide of each of the examples and comparative examples was subjected to a performance test and a measurement of the surface roughness Ra. The results are shown in Table 2. [Table 2]

[0025] In Examples 1 to 7, the alloys of each Example had a thermal conductivity of ≥ 72 W / m K and a density of ≥ 12 g cm -3 , Hardness HRA≧70, fracture toughness ≧10 MPa·M 1 / 2 , bending strength ≥ 1600 N mm -2 , Oxidation weight gain ≦1.16 mg cm -2In each example, the surface roughness of the polished cemented carbide was Ra≦10 nm, which satisfies the conditions for alloy dies for manufacturing optical lenses.

[0026] Compared with Examples 1 to 7, the toughness of the alloy in Example 8 is obviously low, and the oxidation resistance of the alloy in Example 9 is obviously low. This is because there is some correlation between the B content and the HEA. When the HEA content is 2.5wt% to 5wt%, the preferred blending amount of B is 1.5wt%. %~3wt%, whereas the preferred formulation of B is when the content of HEA is 0.5wt%~2.5wt%. The amount is 0.1wt%~1.5wt%. If the contents of HEA and B in Examples 8 and 9 do not match the preferred amounts, the HEA and B in the alloy system cannot exert a synergistic effect, and the properties of the alloy cannot be further improved. In comparison with Example 1, Comparative Example 1 has a HEA content higher than 5 wt%, and as a result, the hardness HRA is 70 or less. The oxidation weight gain was 1.16 mg cm -2 As a result, the polished surface roughness Ra of the obtained alloy was 10 nm or more, which clearly does not satisfy the requirements for a mold for manufacturing optical lenses. In comparison with Example 4, Comparative Example 2 has a higher B content of 3 wt%, and as a result, the fracture toughness is 10 MPa M 1 / 2 The oxidation weight gain was 1.16 mg cm -2 The polished surface roughness of the obtained alloy is The thickness Ra is 10 nm or more, which clearly does not satisfy the requirements for a mold for manufacturing optical lenses. Compared to Example 1, in which 5 wt% HEA was added, the HEA in Comparative Example 3 was 0, and the fracture toughness was 10 MPa M 1 / 2 The oxidation weight gain was 1.16 mg cm -2 The obtained total Since the polished surface roughness Ra of gold is clearly greater than 10 nm, it is clear that this does not meet the requirements for molds for manufacturing optical lenses. In comparison with Example 1, in Comparative Example 4, no B was added, the hardness HRA of the alloy was 70 or less, and the oxidation weight gain was 1.16 mg cm -2 The polished surface roughness Ra of the obtained alloy is 10 nm or more. It is clear that this does not meet the requirements for molds for manufacturing optical lenses.

[0027] Example II The difference between the manufacturing methods of the WC-based cemented carbide in Examples 8 to 12 and Example 1 is that the raw material HEA powder The composition of the WC-based cemented carbide is shown in Table 3. It is. [Table 3] The cemented carbide of each example was subjected to a performance test, and the results are shown in Table 4. [Table 4] In Examples 8 to 12, the thermal conductivity, density, hardness, fracture toughness, bending strength, and oxidation weight of each alloy were measured. The mass growth rate meets the requirements for alloys used in optical lens manufacturing, i.e. thermal conductivity ≥ 72 W / m K, density ≥ 12 g cm -3 , hardness HRA≧70, fracture toughness ≧10MPa·M 1 / 2 , bending strength ≥ 1600 N mm -2 , Oxidation weight gain ≦1.16 mg cm -2 The surface roughness of the polished alloy is Ra≦10 nm.

[0028] Example III The manufacturing method of the WC-based cemented carbide of Example 13 differs from that of Example 1 in the sintering step. The sintering step of Example 13 is as follows. The raw billet is placed in a hot isostatic pressing sintering furnace, and hot isostatic pressing sintering is carried out at a temperature of 1600°C and a sintering pressure of 60 MPa for 1.5 hours under vacuum conditions of 10 Pa or more, and a WC-based cemented carbide is obtained after cooling.

[0029] The manufacturing method of the WC-based cemented carbide of Example 14 differs from Example 1 in the ball milling process. The ball milling process of Example 14 is as follows. a. The single powder that constitutes the HEA is subjected to high energy ball milling in an inert atmosphere, with a ball to material ratio of 18:1, a rotation speed of 500 r / min, and cemented carbide balls as ball mill media. The reaction is carried out for 45 hours using a sintered alloy powder. b.Add WC powder and ceramic powder, in vacuum, ball to material ratio 5:1, rotation speed 150r / min, 60 hours.

[0030] The difference between the manufacturing method of the WC-based cemented carbide of Example 15 and that of Example 1 is that the sintered alloy The annealing treatment in Example 15 is as follows. The WC-based cemented carbide obtained after sintering is placed in a hot isostatic pressing sintering furnace, heated to 200°C under vacuum conditions of 10 Pa or more, and kept at that temperature for 2 hours. After that, it is cooled to room temperature together with the sintering furnace, and the alloy is taken out and used for testing.

[0031] As a result of the measurement, the structures of the HEA phases in Example 1 and Examples 13 to 15 are shown in Table 5. [Table 5] The cemented carbide of each example was subjected to a performance test, and the results are shown in Table 6. [Table 6]

[0032] In Examples 13 to 15, the thermal conductivity, density, hardness, fracture toughness, bending strength, and oxidation weight gain rate of the alloys in each Example all meet the requirements for alloys for manufacturing optical lenses, i.e., thermal conductivity ≥ 72 W / m K, density ≥ 12 g cm -3 , hardness HRA≧70, fracture toughness ≧10MPa·M 1 / 2, bending strength ≥ 1600 N mm -2 , Oxidation weight gain ≦1.16 mg cm -2 The surface roughness of the polished alloy is Ra≦10 nm.

[0033] Compared with Example 13, the phase content (BCC+FCC) of the alloy in the hot isostatic pressing sintering furnace was increased by 0.7%, so that the properties of the alloy, such as hardness, fracture toughness, bending strength and oxidation resistance, were improved. Comparing Example 14 with Example 1, the ball milling process was changed, the rotation speed was increased, and the ball By extending the milling time, more sufficient HEA and WC-based hard alloy powders were obtained, and the mixture was then sintered. The gold phase content (BCC+FCC) increased by 0.9%, improving the thermal conductivity, hardness, fracture toughness and bending strength of the alloy. and oxidation resistance were clearly improved. Comparing Example 15 with Example 1, the alloy structure is homogenized by the annealing treatment, the solid solution effect of HEA is weakened, that is, the content of BCC+FCC phase is reduced by 0.8%, and the density, hardness and bending strength of the alloy are improved. Although some properties such as hardness were deteriorated, other properties such as thermal conductivity, fracture toughness, and oxidation resistance were improved.

[0034] Example IV The WC-based cemented carbide obtained in Examples 1, 8, 9, 13, and 15 and Comparative Examples 1 to 4 were mixed with polycarbonate. This was applied to dies for processing optical glass. After coating the surface of the die, the coated die was used to press mold an optical lens. The optical lens was placed 3 cm in front of the square hole in front of the light source, and the lens was tilted slightly to perform the measurement. A 20W fluorescent lamp or a 100W light bulb was used as the light source. The measurement environment was black with no reflection in front, above, below, left, and right, and a magnifying glass (4 Use a test piece measuring 100x magnification to check for scratches of #60 or smaller. Optical glasses manufactured using dies made of WC-based cemented carbide in Examples 1, 8, 9, 13, and 15 The appearance is good and the product is of good quality. The optical glasses manufactured using the molds using the materials of Comparative Examples 1 to 4 did not have a good appearance and were defective products.

[0035] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these embodiments. Various embodiments that fall within the technical concept of the present invention are within the scope of protection of the present invention. Those skilled in the art will recognize that any changes or modifications made to the above embodiments without departing from the technical concept of the present invention are within the scope of protection of the present invention.

Claims

1. A WC-based cemented carbide alloy comprising a T phase, a WC phase and a HEA phase, the T phase being composed of at least two selected from the group consisting of Al 4 C 3 , TiC, ZrC, TaC, ZrB 2 and TiB 2 , and the HEA phase having a composition formula of is one selected from the group consisting of Al0.4Hf0.6NbTaTiZr, AlNb1.5Ta0.5Ti1.5Zr0.5, AlCr2Mo2Nb2Ti2Zr, HfNbTaTiZr, CrMo0.5NbTa0.5TiZr, and TiVNbMoTaW, the T phase contains element B, which exists in the form of a transition metal boride, and the WC-based cemented carbide is one selected from the group consisting of the HEA phase, The content is 0.5wt% to 5wt%, the content of the T phase is 35wt% or less, and the remainder is the WC phase. and unavoidable impurities, and the content of the element B is 0.1wt% to 3wt%. WC-based cemented carbide.

2. The WC-based cemented carbide has a B content of 1.5 wt% to 3 wt%, and a HEA phase content of 2.5 wt%.

2. The WC-based cemented carbide according to claim 1, characterized in that the WC content is between 5wt% and 5wt%.

3. The WC-based cemented carbide according to claim 1, characterized in that the WC-based cemented carbide has a B content of 0.1wt% to 1.5wt% and a HEA phase content of 0.5wt% to 2.5wt%.

4. The composition formula of the WC-based cemented carbide is ZrC-ZrB 2 -WC-AlNb 1.5 Ta 0.5 Ti 1.5 Zr 0.5 2. The WC-based cemented carbide according to claim 1,

5. The WC-based cemented carbide has a thermal conductivity of 72 W / m·K or more at room temperature. WC-based cemented carbide according to any one of claims 1 to 10.

6. 5. A mold for optical glass, comprising: a material for the mold being the WC-based cemented carbide according to any one of claims 1 to 4; a material for the optical glass including one of silica, a resin material, and zinc selenide; and a resin material being one of polymethyl methacrylate, polystyrene, polycarbonate, and polydiallyl diglycol carbonate.

Citation Information

Patent Citations

  • Preparation method for hard high-entropy alloy composite material

    CN108060322A

  • Hard alloy sintered by high-entropy alloy binder and compound carbide and preparation method thereof

    CN1827817A

  • Superhard tungsten carbide alloy for member of hot working apparatus

    JP1983031060A

  • Cemented carbide

    JP2005220372A

  • WC-based hard metal, and member coated with hard film

    JP2009114469A