Electrode manufacturing method, electrode and energy storage element

A dual-resin manufacturing method with controlled molecular weights improves peel strength and resistance to electrolyte dissolution in electrodes, addressing the issues of binder dissolution and high-temperature effects in dry coating processes.

JP7585605B2Active Publication Date: 2024-11-19GS YUASA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019200266
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-01
Publication Date
2024-11-19
Estimated Expiration
2039-11-01

AI Technical Summary

Technical Problem

The dissolution of binders in high-temperature electrolytes reduces the peel strength of coating layers in electrodes, and high heat treatment temperatures for dry coating can adversely affect electrode performance.

Method used

A manufacturing method involving a combination of first and second synthetic resins with specific molecular weight ranges (500,000 to 1,500,000 and 10,000 to 400,000, respectively) is used to form a dry coating layer, ensuring good peel strength while suppressing heat treatment temperatures.

Benefits of technology

The method enhances the peel strength of the coating layer by maintaining compatibility and viscosity, preventing binder dissolution in high-temperature electrolytes and minimizing heat impact on electrode performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585605000002
    Figure 0007585605000002
  • Figure 0007585605000003
    Figure 0007585605000003
  • Figure 0007585605000001
    Figure 0007585605000001
Patent Text Reader

Abstract

To provide a method for manufacturing an electrode, with which an electrode having a coating layer with good peel strength can be manufactured while heat treatment temperatures in dry coating are suppressed.SOLUTION: A method for manufacturing an electrode for a power storage element according to one aspect of the present invention includes the steps of: coating coating powder containing a first binder and a second binder, directly or indirectly on the surface of a base material; and heating the coating powder at a temperature of the melting point of the first binder and the second binder or above. The main component of the first binder is a first synthetic resin, and the main component of the second binder is a second synthetic resin. The weight average molecular weight of the first synthetic resin is 500,000 or more and 1,500,000 or less, and the weight average molecular weight of the second synthetic resin is 10,000 or more and 400,000 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an electrode, and an electrode and an energy storage element. [Background technology]

[0002] Secondary batteries, such as lithium-ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. The secondary batteries generally have a pair of electrodes consisting of a sheet-shaped positive electrode and a sheet-shaped negative electrode, and an electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring ions between the electrodes. In addition, capacitors such as lithium-ion capacitors and electric double layer capacitors are also widely used as storage elements other than secondary batteries.

[0003] The pair of electrodes is usually laminated or wound with a separator between them to form an electrode assembly. The separator has a function of electrically insulating the electrodes and a function of retaining an electrolyte and transferring ions between the electrodes. A porous membrane made of a resin is widely used as the separator.

[0004] In recent years, development of an electric storage element having an electrode with a porous insulating coating layer formed on the surface of an active material layer has been underway as a replacement for the separator or in addition to using a separator. In the prior art, an electrode has been proposed as an electric storage element having such an electrode with an insulating coating layer, for example, the electrode having a negative electrode disposed between a pair of insulating coating layers containing an insulating resin and a positive electrode bonded to the insulating coating layer (see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2006-147185 A Summary of the Invention [Problem to be solved by the invention]

[0006] When an electrode having such a coating layer is immersed in a high-temperature electrolyte, the binder contained in the coating layer may dissolve in the electrolyte, and the peel strength of the coating layer may decrease. Therefore, it is necessary to select a binder that is less soluble in a high-temperature electrolyte. In addition, when forming a coating layer, a dry coating method that does not use a solvent is preferable because the binder contained in the coating layer does not penetrate into other layers together with the solvent. However, when the heat treatment temperature of the dry coating is high, the peel strength of the coating layer is good, but other performances of the electrode may be affected.

[0007] The present invention has been made based on the above circumstances, and has an object to provide a method for manufacturing an electrode that can produce an electrode having good peel strength of a coating layer while suppressing the heat treatment temperature in dry coating. [Means for solving the problem]

[0008] A method for manufacturing an electrode for a storage element according to one aspect of the present invention includes the steps of applying a coating powder containing a first binder and a second binder directly or indirectly to a surface of a substrate, and heating the coating powder at a temperature equal to or higher than the melting points of the first binder and the second binder, wherein a main component of the first binder is a first synthetic resin, a main component of the second binder is a second synthetic resin, the first synthetic resin has a weight average molecular weight of 500,000 or more and 1,500,000 or less, and the second synthetic resin has a weight average molecular weight of 10,000 or more and 400,000 or less.

[0009] An electrode for a storage element according to one aspect of the present invention comprises a substrate and a dry coating layer formed directly or indirectly on a surface of the substrate, the dry coating layer containing a first binder and a second binder, the first binder mainly comprising a first synthetic resin and the second binder mainly comprising a second synthetic resin, the first synthetic resin having a weight average molecular weight of 500,000 or more and 1,500,000 or less, and the second synthetic resin having a weight average molecular weight of 10,000 or more and 400,000 or less.

[0010] An energy storage element according to one aspect of the present invention includes the electrode. Effect of the Invention

[0011] According to a method for producing an electrode for an energy storage element according to one aspect of the present invention, an electrode having a coating layer with good peel strength can be produced even when the heat treatment temperature in dry coating is suppressed. [Brief description of the drawings]

[0012] [Figure 1] 1 is an external perspective view showing a nonaqueous electrolyte secondary battery according to one embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing an electricity storage device formed by assembling a plurality of nonaqueous electrolyte secondary batteries according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] A method for manufacturing an electrode for a storage element according to one embodiment of the present invention includes the steps of applying a coating powder containing a first binder and a second binder directly or indirectly to a surface of a substrate, and heating the coating powder at a temperature equal to or higher than the melting points of the first binder and the second binder, wherein a main component of the first binder is a first synthetic resin, a main component of the second binder is a second synthetic resin, the first synthetic resin has a weight average molecular weight of 500,000 or more and 1,500,000 or less, and the second synthetic resin has a weight average molecular weight of 10,000 or more and 400,000 or less.

[0014] According to the manufacturing method of the electrode, an electrode having a good peel strength of the coating layer can be manufactured even when the heat treatment temperature of the dry coating is suppressed. The reason why such an effect occurs is not clear, but it is thought to be as follows. When an electrode having a coating layer containing a binder is immersed in a high-temperature electrolyte, the binder contained in the coating layer may dissolve in the electrolyte, and the peel strength of the coating layer may decrease. The present inventor has found that the above problem can be solved by increasing the molecular weight of the binder. On the other hand, in dry coating, the electrode is heat-treated at a temperature equal to or higher than the melting point of the binder in order to melt the binder. However, when the binder is made of only a high-molecular-weight resin, the viscosity of the molten binder is high, so that it does not wet and spread on the substrate unless the heat treatment temperature is increased. For this reason, it has become clear that the contact area between the binder and the substrate is small and sufficient peel strength cannot be obtained. If the heat treatment temperature is excessively high, sufficient peel strength can be obtained, but other performances of the electrode may be affected. The manufacturing method of the electrode uses two types of binders, a first synthetic resin with a high molecular weight of 500,000 to 1,500,000 and a second synthetic resin with a low molecular weight of 10,000 to 400,000, as the main components of the binder, and the viscosity of the molten binder is appropriately low while incorporating the characteristics of the binder with a high molecular weight that increases the peel strength of the coating layer, and the binder spreads sufficiently on the substrate even at a low heat treatment temperature. Therefore, the contact area between the binder in the coating layer and the substrate increases, improving the peel strength. Therefore, according to the manufacturing method of the electrode, an electrode with good peel strength of the coating layer can be manufactured even when the heat treatment temperature of the dry coating is suppressed.

[0015] In the method for producing an electrode, the first synthetic resin and the second synthetic resin preferably have the same structural unit, which makes the melting points of the first synthetic resin and the second synthetic resin closer to each other, improves compatibility, and improves coating performance.

[0016] In the method for producing an electrode, it is preferable that the structural units of the first synthetic resin and the second synthetic resin are identical to each other. By making the structural units of the first synthetic resin and the second synthetic resin identical to each other, the melting points of the first synthetic resin and the second synthetic resin become closer to each other, and the compatibility is improved, thereby improving the coating performance.

[0017] An electrode for an energy storage element according to one embodiment of the present invention comprises a substrate and an insulating dry coating layer formed directly or indirectly on a surface of the substrate, the dry coating layer containing a first binder and a second binder, the first binder mainly comprising a first synthetic resin and the second binder mainly comprising a second synthetic resin, the first synthetic resin having a weight average molecular weight of 500,000 or more and 1,500,000 or less, and the second synthetic resin having a weight average molecular weight of 10,000 or more and 400,000 or less.

[0018] According to the electrode, the dry coating layer uses two types of binders, namely, a first binder mainly composed of a first synthetic resin having a high molecular weight of 500,000 to 1,500,000 and a second binder mainly composed of a second synthetic resin having a low molecular weight of 10,000 to 400,000, so that the viscosity of the molten binder is appropriately reduced, and the binder spreads sufficiently on the substrate even at a low heat treatment temperature. Therefore, the contact area between the binder in the coating layer and the substrate increases, and the peel strength is improved. Therefore, the electrode has a good peel strength of the coating layer because the dissolution of the binder in the high-temperature electrolyte is suppressed. Here, "insulating" means that the conductivity is lower than that of the substrate and the active material layer. Specifically, "insulating" means that when the two-point probe of a low resistivity meter "Loresta EP MCP T360" manufactured by Mitsubishi Chemical Analytech is pressed against an insulating layer or an active material layer without an insulating layer to measure the surface resistance of both, the resistance value of the insulating layer is increased by 50 times or more compared to the resistance value of the active material layer without an insulating layer.

[0019] It is preferable that the first synthetic resin and the second synthetic resin have the same structural unit. By having the same structural unit, the melting points of the first synthetic resin and the second synthetic resin become close to each other, and the compatibility is improved, thereby improving the peel strength of the coating layer.

[0020] It is preferable that the structural units of the first synthetic resin and the second synthetic resin are identical to each other. By making the structural units of the first synthetic resin and the second synthetic resin identical to each other, the melting points of the first synthetic resin and the second synthetic resin become closer to each other, and the compatibility is improved, thereby improving the peel strength of the coating layer.

[0021] It is preferable that the battery has an active material layer formed directly or indirectly on the surface of the base material, and the dry coating layer is formed on the surface of the active material layer. By forming an insulating dry coating layer on the surface of the active material layer, insulation between the positive and negative electrodes can be ensured even if the separator shrinks or breaks.

[0022] It is preferable that the dry coating layer contains an active material. When the insulating dry coating layer contains an active material, the surface of the active material is covered with an insulating film. Therefore, even if the separator shrinks or breaks, the insulation between the positive electrode and the negative electrode can be ensured.

[0023] An electric storage element according to one embodiment of the present invention includes the electrode. By including the electrode, the electric storage element is prevented from dissolving the binder of the dry coating layer of the electrode of the electric storage element in a high-temperature electrolyte solution. Therefore, the peel strength of the dry coating layer of the electrode of the electric storage element is good.

[0024] A method for producing an electrode according to one embodiment of the present invention, an electrode according to one embodiment, and a nonaqueous electrolyte secondary battery (hereinafter, sometimes simply referred to as a "secondary battery") as one embodiment of the energy storage element of the present invention will be described in detail below. Note that the names of the components (elements) used in each embodiment may differ from the names of the components (elements) used in the background art.

[0025] <Electrode manufacturing method> The method for manufacturing an electrode for a storage element according to one embodiment of the present invention can be manufactured by forming an active material layer on the surface of a substrate of the electrode, and forming a dry coating layer serving as an insulating layer on the surface of the active material layer. The "dry coating layer" refers to a layer formed by dry coating. The method for manufacturing an electrode according to one embodiment of the present invention includes a step of directly or indirectly coating a coating powder containing a first binder and a second binder on the surface of the substrate (hereinafter also referred to as a coating step), and a step of heating the coating powder at a temperature equal to or higher than the melting points of the first binder and the second binder (hereinafter also referred to as a heating step). The coating step and the heating step form a dry coating layer directly or indirectly on the surface of the substrate. The method for manufacturing the electrode includes, for example, a step of forming an active material layer on the substrate, and then coating a coating powder containing a first binder and a second binder, and a step of heating the coating powder at a temperature equal to or higher than the melting points of the first binder and the second binder. The method for manufacturing the electrode may also include, for example, forming an intermediate layer on the surface of the substrate.

[0026] The electrode manufacturing method may be used for either the positive electrode or the negative electrode of an electricity storage element, or may be used for both the positive electrode and the negative electrode.

[0027] The active material layer can be formed by a known method. The active material layer can be formed, for example, by applying an active material mixture paste to a substrate. The active material layer can be formed by wet coating. Specifically, an active material, a conductive assistant, and a binder are mixed, and a dispersion solvent is added to the mixture and kneaded to prepare an active material mixture paste. This active material mixture paste is applied onto a substrate. Then, the dispersion solvent is removed by volatilizing the applied active material mixture paste, and an active material layer is formed.

[0028] [Coating process] In the coating step, a coating powder containing a first binder and a second binder is applied directly or indirectly to the surface of a substrate described later. The coating powder is a mixture of the first binder, the second binder, and a filler. That is, the dry coating layer is formed by applying a coating powder containing a mixture of a binder and a filler to the surface of an active material layer. When the coating powder is applied, the active material layer may still contain a dispersion solvent, or the dispersion solvent may have already been removed from the active material layer.

[0029] (Binder) The main component of the first binder is a first synthetic resin, and the main component of the second binder is a second synthetic resin. The weight average molecular weight of the first synthetic resin is 500,000 to 1,500,000, and the weight average molecular weight of the second synthetic resin is 10,000 to 400,000. The electrode manufacturing method uses two types of resins as the main components of the binder: a first synthetic resin having a high molecular weight of 500,000 to 1,500,000 and a second synthetic resin having a low molecular weight of 10,000 to 400,000, so that the viscosity of the molten binder is appropriately reduced, and the binder spreads sufficiently on the substrate even at a low heat treatment temperature. Therefore, the contact area between the binder in the dry coating layer and the substrate is increased, and the peel strength is improved. Therefore, according to the electrode manufacturing method, an electrode having a good peel strength of the dry coating layer can be manufactured even when the heat treatment temperature of the dry coating is suppressed.

[0030] The first and second synthetic resins, which are the main components of the first and second binders, are either water-soluble aqueous polymers that, when made into a 1.0% by mass aqueous solution, have a viscosity of less than 100 mPa·sec at a liquid temperature of 25°C, measured at a rotor rotation speed of 60 rpm using a B-type viscometer, or water-insoluble non-aqueous polymers.

[0031] The first synthetic resin and the second synthetic resin may be the same resin or different resins.

[0032] The lower limit of the weight average molecular weight of the first synthetic resin which is the main component of the first binder is 500,000, preferably 600,000. On the other hand, the upper limit of the weight average molecular weight of the first synthetic resin is 1,500,000, preferably 2,000,000. Also, the lower limit of the weight average molecular weight of the second synthetic resin which is the main component of the second binder is 10,000, preferably 50,000. On the other hand, the upper limit of the weight average molecular weight of the second synthetic resin is 400,000, preferably 300,000. By the range of the weight average molecular weight of the first synthetic resin and the weight average molecular weight of the second synthetic resin being within the above range, the viscosity of the molten binder is appropriately lowered while incorporating the characteristics of the first binder with a large molecular weight which increases the peel strength of the coating layer, and the binder spreads sufficiently on the substrate even at a low heat treatment temperature. Therefore, the contact area between the binder in the coating layer and the substrate is increased, and the peel strength is improved. Therefore, according to the manufacturing method of the electrode, an electrode having a good peel strength of the coating layer can be manufactured even when the heat treatment temperature of the dry coating is suppressed. Here, the term "weight average molecular weight" refers to the average molecular weight measured using gel permeation chromatography (GPC) in accordance with JIS-K7252-1 (2008) "Plastics - Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography - Part 1: General rules."

[0033] In the method for manufacturing the electrode, the first synthetic resin and the second synthetic resin preferably have the same structural unit. When the first synthetic resin and the second synthetic resin have the same structural unit, the melting points of the first synthetic resin and the second synthetic resin become close to each other, and the compatibility is improved, thereby improving the coating performance. Here, "the first synthetic resin and the second synthetic resin have the same structural unit" includes a case where the structural unit of the first synthetic resin and a part of the structural unit of the second synthetic resin are the same, and a case where the structural unit of the first synthetic resin and the structural unit of the second synthetic resin are the same. The above "the structural units of the first synthetic resin and the structural units of the second synthetic resin are the same" means that all the structural units of the first synthetic resin and all the structural units of the second synthetic resin are the same. An example of a combination in which the structural units of the first synthetic resin and the structural units of the second synthetic resin are partly the same is when the first synthetic resin is polyvinylidene fluoride and the second synthetic resin is a copolymer of vinylidene fluoride and hexafluoropropylene (PVDF-HFP). An example of a combination in which the structural units of the first synthetic resin and the structural units of the second synthetic resin are the same is when the first synthetic resin and the second synthetic resin have the same structure and the molecular weight of the second synthetic resin is smaller than the molecular weight of the first synthetic resin. An example of such a combination of the first synthetic resin and the second synthetic resin is when the first synthetic resin is polyvinylidene fluoride with a high molecular weight and the second synthetic resin is polyvinylidene fluoride with a low molecular weight. Among these, it is preferable that the structural units of the first synthetic resin and the structural units of the second synthetic resin are the same. When the structural units of the first synthetic resin and the second synthetic resin are the same, the melting points of the first synthetic resin and the second synthetic resin become closer, and the compatibility is improved, thereby enabling the coating performance to be improved.

[0034] The lower limit of the difference between the melting point of the first binder and the melting point of the second binder in the insulating layer is preferably 0°C, and more preferably 5°C. By making the difference in melting point between the second binder and the first binder equal to or greater than the above lower limit, the compatibility between the first binder and the second binder can be further improved. The upper limit of the difference between the melting point of the first binder and the melting point of the second binder in the insulating layer is preferably 50°C, and more preferably 30°C. By making the difference in melting point between the second binder and the first binder equal to or less than the above upper limit, the manufacturability of the insulating layer can be improved.

[0035] The upper limit of the melting point of the first binder and the second binder is preferably 190°C, and more preferably 180°C. By setting the melting point of the first binder to the above upper limit or lower, the first binder and the second binder melt at a lower temperature, so that the effect of heating on the electrode performance can be suppressed. In addition, the amount of heat required in the step of heating the insulating layer is reduced. On the other hand, the lower limit of the melting point of the first binder and the second binder is preferably 85°C, and more preferably 95°C. By setting the melting point of the first binder to the above lower limit or higher, the coating performance can be improved.

[0036] The melting point of the binder can be measured, for example, by the method described in JIS-K-7121 (1987). In this specification, the melting point of the binder refers to the melting temperature read from a DSC curve obtained by differential scanning calorimetry (DSC) of the binder. The melting temperature is determined by the method of reading the DSC curve described in JIS-K-7121 (1987).

[0037] The lower limit of the content of the first binder in the coating powder is preferably 0.5 mass%, more preferably 2.5 mass%, and even more preferably 5 mass%. The upper limit of the content of the first binder is preferably 30 mass%, more preferably 25 mass%, and even more preferably 20 mass%. By having the content of the first binder within the above range, the adhesion of the dry coating layer when immersed in the electrolyte in the secondary battery is improved.

[0038] The lower limit of the content of the second binder in the coating powder is preferably 0.5% by mass, more preferably 2.5% by mass, and even more preferably 5% by mass. The upper limit of the content of the second binder is preferably 30% by mass, more preferably 25% by mass, and even more preferably 20% by mass or less. By having the content of the second binder in the above range, the adhesion of the dry coating layer during production is improved.

[0039] The lower limit of the total content of the first binder and the second binder in the coating powder is preferably 1 mass%, more preferably 5 mass%, and even more preferably 10 mass%. The upper limit of the content of the first binder and the second binder is preferably 50 mass%, more preferably 40 mass%, and even more preferably 30 mass%. When the total content of the first binder and the second binder is within the above range, the adhesion of the dry coating layer during production and in the secondary battery is good.

[0040] The lower limit of the mass ratio of the second binder to the first binder in the coating powder is preferably 0.15, more preferably 0.4. The upper limit of the mass ratio is preferably 7, more preferably 3. By having the mass ratio in the above range, the adhesion of the dry coating layer during production and inside the secondary battery is improved.

[0041] (Filler) The filler is a non-conductive particle. Here, "conductive" means that the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 7 "Non-conductive" means that the volume resistivity is 10 7 This means that the resistance is greater than Ω·cm.

[0042] The filler may be inorganic particles or organic particles. From the viewpoint of heat resistance, inorganic particles are preferred. Examples of inorganic particles include inorganic oxides such as silica, alumina, titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide, inorganic nitrides such as silicon nitride, titanium nitride, and boron nitride, inorganic hydroxides such as aluminum hydroxide, and others, such as silicon carbide, calcium carbonate, lithium carbonate, aluminum sulfate, potassium titanate, talc, kaolin clay, kaolinite, boehmite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, aluminosilicate, calcium silicate, magnesium silicate, diatomaceous earth, silica sand, and glass. Among these, inorganic oxides or inorganic hydroxides are preferred because they are thermally stable, and alumina is more preferred because it has high stability against halide ions such as fluoride ions.

[0043] The lower limit of the average particle size (median diameter) of the filler is preferably 0.1 μm, more preferably 1 μm. The upper limit of the average particle size (median diameter) of the filler is preferably 10 μm, more preferably 7 μm. By setting the particle size of the filler in the above range, it is possible to further increase the electrolyte permeability while maintaining sufficient non-conductivity. The above-mentioned "median diameter" means the value (D50) at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%. Specifically, it can be measured by the following method. Measurement is performed using a laser diffraction particle size distribution measuring device (Shimadzu Corporation's "SALD-2200") as the measuring device and Wing SALD-2200 as the measurement control software. A scattering measurement mode is adopted, and a laser beam is irradiated onto a wet cell in which a dispersion liquid in which the measurement sample is dispersed in a dispersion solvent is circulated, and a scattered light distribution is obtained from the measurement sample. The scattered light distribution is then approximated by a log-normal distribution, and the particle diameter at a cumulative degree of 50% is taken as the median diameter (D50).

[0044] The lower limit of the filler content in the coating powder is preferably 50% by mass, more preferably 60% by mass, and even more preferably 70% by mass. The upper limit of the filler content is preferably 99% by mass, more preferably 95% by mass, and even more preferably 90% by mass. By keeping the filler content within the above range, coating performance can be improved.

[0045] The coating layer is formed by dry coating. Dry coating refers to a coating method that does not use a solvent. In conventional wet coating, the binder of the coating layer may flow into the active material layer. When the binder flows into the active material layer, the binder of the active material layer and the binder of the coating layer are mixed in the active material layer. When the binder of the coating layer flows into the active material layer, the binder of the flowed coating layer may block the pores of the active material layer, which may deteriorate the high-rate discharge characteristics of the storage element. In contrast, in dry coating, the binder of the dry coating layer is prevented from flowing into the active material layer, so that a sufficient amount of binder can be retained inside the dry coating layer. In addition, dry coating can uniformly coat the filler in the coating powder. Therefore, when forming a coating layer, dry coating without using a solvent is preferable because the binder does not penetrate into other layers together with the solvent.

[0046] As the dry coating, electrostatic coating in which an electrically charged coating powder is layered on an active material layer is preferred, powder coating using a powder-like coating powder is also preferred, and electrostatic powder coating in which electrostatic coating and powder coating are combined is more preferred. As the powder coating, a fluidized bed method or the like can be mentioned. As the electrostatic coating, an electrospinning method or the like can be mentioned.

[0047] In powder coating, a powder in which a particulate filler is mixed with a particulate first binder and a particulate second binder, or a powder in which the first binder and the second binder are attached to the surface of a particulate filler can be used, but it is preferable to use a powder in which the first binder and the second binder are attached to the surface of a particulate filler. By selectively having a binder present on the surface of the filler, the binder present in the space between the filler particles can be reduced, and the space between the filler particles can be secured, so that the permeability of the electrolyte in the dry coating layer becomes better. In addition, by using a powder in which the binder is attached to the surface of the particulate filler, the binder can be uniformly distributed in the thickness direction of the dry coating layer.

[0048] In powder coating, powder-like coating powder is applied (sprayed) onto the active material layer using various feeders such as air flow feeders and vibrating feeders. After or during spraying, the applied powder-like coating powder is heated, so that the powder-like coating powder fuses and forms a dry coating layer on the surface of the active material layer. An electrostatic powder coating method can be used in which the powder is electrostatically charged during spraying. By using the electrostatic powder coating method, a dry coating layer with high uniformity and in which the filler is laminated in layers can be efficiently formed, and a stable dry coating layer with small variation in thickness can be formed.

[0049] The applied dry coating layer may be pressed with a press or roller to form it into a predetermined thickness. If the thickness of the dry coating layer can be sufficiently set during coating, the pressing step may be omitted.

[0050] [Heating process] The applied dry coating layer is heated to a temperature equal to or higher than the melting points of the first and second binders. This melts the binders contained in the dry coating layer, and the binders in the dry coating layer are thermally welded together. The dry coating layer is heated, for example, by introducing it into a furnace equipped with a mechanism (for example, a heater and a fan) for blowing hot air onto the surface of the electrode.

[0051] The temperature to which the dry coating layer is heated is preferably from 80° C. to 230° C., and more preferably from 90° C. to 200° C. By heating at the above temperatures, the effect of heating on the electrodes can be suppressed, and the time required for the heating step can be shortened.

[0052] The temperature to which the dry coating layer is heated is preferably 30° C. to 50° C. higher than the melting point of the binder, and more preferably 10° C. to 20° C. higher. By heating at the above temperatures, the effect of heating on the electrodes can be suppressed, while the time required for the heating step can be shortened.

[0053] <Electrode> [First embodiment] The electrode according to the first embodiment of the present invention comprises a substrate and an insulating layer formed directly or indirectly on the surface of the substrate. In the electrode according to the first embodiment, the insulating layer is a dry-coated layer. The electrode according to the first embodiment can be manufactured, for example, by forming an active material layer on the surface of the substrate and forming an insulating layer on the surface of the active material layer. When the insulating layer is a dry-coated layer, the first binder and the second binder of the insulating layer can be prevented from eluting into other layers, so that the content of the first binder and the second binder in the insulating layer can be easily increased.

[0054] An electrode according to one embodiment of the present invention includes a conductive substrate and an active material layer. The active material layer may be formed on only one side of the substrate, or on both sides. The insulating layer may be formed on the surface of the active material layer on at least one side of the substrate. The electrode may include an intermediate layer, and may be laminated on only one side of the substrate, or on both sides. The electrode may be a positive electrode or a negative electrode.

[0055] When the energy storage element using the electrode of this embodiment includes a separator containing a resin substrate, the resin substrate can be prevented from being oxidized by providing an insulating layer on the surface of the positive electrode active material layer. From this viewpoint, the electrode of this embodiment is preferably used as a positive electrode. When the energy storage element using the electrode of this embodiment does not include a separator containing a resin substrate, the electrode of this embodiment is preferably used as a negative electrode from the viewpoint of preventing short circuits at the electrode end. In addition, the electrode can be used in both the positive electrode and the negative electrode.

[0056] (base material) The substrate has a sheet shape and is conductive.

[0057] When the electrode is a positive electrode, the material of the substrate is a metal such as aluminum, titanium, tantalum, stainless steel, or an alloy thereof. Among these, aluminum and aluminum alloys are preferred in terms of the balance between potential resistance, high conductivity, and cost. In addition, the form of the positive electrode substrate may be foil, vapor deposition film, or the like, and foil is preferred in terms of cost. That is, aluminum foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, etc., as specified in JIS-H4000 (2014).

[0058] The lower limit of the average thickness of the positive electrode substrate is preferably 5 μm, more preferably 10 μm. The upper limit of the average thickness of the positive electrode substrate is preferably 50 μm, more preferably 40 μm. By making the average thickness of the positive electrode substrate equal to or greater than the lower limit, the strength of the positive electrode substrate can be increased. By making the average thickness of the positive electrode substrate equal to or less than the upper limit, the energy density per volume of the secondary battery can be increased. Hereinafter, the term "average thickness of the substrate" refers to the average value of thicknesses measured at any ten points.

[0059] When the electrode is a negative electrode, the material of the negative electrode substrate is a metal such as copper, nickel, stainless steel, nickel-plated steel, or an alloy thereof, and copper or a copper alloy is preferred. The form of the negative electrode substrate may be a foil, a vapor deposition film, or the like, and foil is preferred from the viewpoint of cost. That is, copper foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0060] The lower limit of the average thickness of the negative electrode substrate is preferably 3 μm, more preferably 5 μm. The upper limit of the average thickness of the negative electrode substrate is preferably 30 μm, more preferably 20 μm. By making the average thickness of the negative electrode substrate equal to or greater than the lower limit, the strength of the negative electrode substrate can be increased. By making the average thickness of the negative electrode substrate equal to or less than the upper limit, the energy density per volume of the secondary battery can be increased.

[0061] (active material layer) The active material layer is laminated on a substrate. The active material layer includes an active material. The active material layer includes optional components such as a conductive agent, a binder, a thickener, and a filler, as necessary. Each of these components can be a known component used in a general active material layer.

[0062] When the electrode is a positive electrode, the positive electrode active material can be appropriately selected from, for example, known positive electrode active materials. As the positive electrode active material for a lithium ion secondary battery, a material capable of absorbing and releasing lithium ions is usually used. As the positive electrode active material, for example, α-NaFeO 2 Lithium transition metal composite oxides having a crystalline structure, lithium transition metal composite oxides having a spinel crystalline structure, polyanion compounds, chalcogen compounds, sulfur, etc. 2 As an example of a lithium transition metal composite oxide having a crystalline structure, Li[Li x Ni 1-x ]O 2 (0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1), Li[Li x Co(1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1). Lithium transition metal composite oxides with spinel crystal structure include Li x Mn 2 O 4 , Li x Ni γ Mn (2-γ) O 4 Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 3 V 2 (PO 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 Examples of the chalcogen compound include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. The atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more of them may be mixed and used. In the positive electrode active material layer, one of these compounds may be used alone, or two or more of them may be mixed and used.

[0063] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but the lower limit is preferably 50 mass%, more preferably 80 mass%, and even more preferably 90 mass%, while the upper limit of this content is preferably 99 mass%, and more preferably 98 mass%.

[0064] When the electrode is a negative electrode, a material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material. Specific examples of the negative electrode active material include metals or semimetals such as Si and Sn, metal oxides or semimetal oxides such as Si oxide and Sn oxide, polyphosphate compounds, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon).

[0065] Furthermore, the negative electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, and Ge; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W.

[0066] The lower limit of the content of the negative electrode active material in the negative electrode active material layer is preferably 60 mass%, more preferably 80 mass%, and even more preferably 90 mass%. By making the content of the negative electrode active material equal to or greater than the lower limit, the electric capacity of the secondary battery can be increased. The upper limit of the content of the negative electrode active material is preferably 99 mass%, more preferably 98 mass%. By making the content of the negative electrode active material particles equal to or less than the upper limit, the production of the negative electrode becomes easier.

[0067] The conductive agent is not particularly limited as long as it is a conductive material. Examples of the conductive agent include carbonaceous materials, metals, conductive ceramics, and the like. Examples of the carbonaceous material include graphitized carbon, non-graphitized carbon, graphene-based carbon, and the like. Examples of non-graphitized carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the conductive material include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. These materials may also be used in combination. For example, a material in which carbon black and CNT are combined may be used. Among these, carbon black is preferable from the viewpoint of electronic conductivity and coating performance, and acetylene black is preferable among them.

[0068] Examples of the binder include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.

[0069] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. In addition, when the thickener has a functional group that reacts with lithium, it is preferable to deactivate this functional group in advance by methylation or the like.

[0070] The filler is not particularly limited. Examples of the main component of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, aluminum oxide, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof.

[0071] (insulating layer) The insulating layer is laminated on the surface of the active material layer. The insulating layer means a layer having insulating properties.

[0072] The insulating layer contains a filler, a first binder, and a second binder. This allows the insulating layer to exhibit insulating properties. The insulating layer may contain components other than the filler and the binder.

[0073] The details of each element constituting the insulating layer are as described above.

[0074] The lower limit of the average thickness of the insulating layer is preferably 3 μm, more preferably 4 μm, further preferably 6 μm, and even more preferably 7 μm. By setting the average thickness of the insulating layer to the above lower limit or more, more sufficient insulation can be exhibited. The upper limit of the average thickness of the insulating layer is, for example, 30 μm, may be 20 μm, or may be 16 μm. By setting the average thickness of the insulating layer to the above upper limit or less, the electric storage element can be made thin and the energy density can be improved. In addition, even if the insulating layer is formed relatively thick in the electric storage element, the deterioration of the high-rate discharge performance of the electric storage element is small, and good high-rate discharge performance can be exhibited. The "average thickness of the insulating layer" is a value measured by the following method. An electron microscope image of a cross section of three arbitrary positions of an electrode on which an insulating layer is formed is observed, and the thickness of the insulating layer at three arbitrary positions for each cross section is measured. The average value of the thicknesses of the insulating layer at all measured positions (total of nine positions) is taken as the average thickness of the insulating layer.

[0075] According to the electrode of the first embodiment, an insulating dry coating layer is formed on the surface of the active material layer, so that insulation between the positive and negative electrodes can be ensured even if the separator shrinks or breaks.

[0076] [Second embodiment] The electrode according to the second embodiment of the present invention has a substrate and an active material layer. In the electrode according to the second embodiment, the active material layer is a dry-coated layer. Thus, the active material layer is formed by dry coating. By containing an active material in the insulating dry-coated layer, the surface of the active material is covered with an insulating film. Therefore, even if the separator shrinks or breaks, the insulation between the positive and negative electrodes can be ensured.

[0077] Details of the filler, the first binder, and the second binder in the active material layer in the electrode according to the second embodiment are the same as those of the insulating layer in the electrode according to the first embodiment. Details of the active material and optional components in the active material layer in the electrode according to the second embodiment are the same as those of the active material layer in the electrode according to the first embodiment.

[0078] According to the electrode of the second embodiment, since the insulating dry coating layer contains an active material, the surface of the active material is covered with an insulating film, and therefore, even if the separator shrinks or breaks, the insulation between the positive and negative electrodes can be ensured.

[0079] <Electricity storage element> An electric storage element according to one embodiment of the present invention includes the electrode. By including the electrode, the electric storage element is prevented from dissolving the binder of the dry coating layer of the electrode of the electric storage element in a high-temperature electrolyte solution. Therefore, the peel strength of the dry coating layer of the electrode of the electric storage element is good.

[0080] The storage element of the present invention has a negative electrode, a positive electrode, and a non-aqueous electrolyte. Hereinafter, a non-aqueous electrolyte secondary battery (particularly a lithium ion non-aqueous electrolyte secondary battery) will be described as an example of the storage element, but this is not intended to limit the scope of application of the present invention. The negative electrode and the positive electrode are usually stacked or wound alternately with a separator interposed therebetween to form an electrode body. This electrode body is housed in a case (battery container), and the case is filled with a non-aqueous electrolyte. The non-aqueous electrolyte is interposed between the positive electrode and the negative electrode. In addition, as the case, a known metal case or the like that is usually used as a case for a non-aqueous electrolyte secondary battery can be used.

[0081] At least one of the positive electrode and the negative electrode is the electrode described above. Note that an electrode other than the electrode may be used as one of the positive electrode and the negative electrode. Such an electrode may be an electrode that does not have a dry coating layer.

[0082] [Electrode body] As the electrode body of the energy storage element, it is preferable to use a laminated electrode body in which flat positive and negative electrodes are alternately laminated. When a laminated electrode body is used, the electrodes are not bent, so that peeling of the dry coating layer can be suppressed. Note that, as the laminated electrode body, an electrode plate without a dry coating layer laminated thereon may be laminated by folding it in an accordion shape while sandwiching an electrode with a dry coating layer formed thereon without bending it.

[0083] When dry coated layers are formed on both the positive electrode and the negative electrode, the average thickness, composition, etc. of these dry coated layers may be the same or different.

[0084] [Positive electrode] The positive electrode has a positive electrode substrate and a positive electrode active material layer. The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer is laminated directly or via an intermediate layer along at least one surface of the positive electrode substrate.

[0085] The positive electrode active material layer is formed from a so-called positive electrode mixture containing a positive electrode active material. The positive electrode mixture forming the positive electrode active material layer further contains optional components such as a conductive agent, a binder, a thickener, and a filler as necessary.

[0086] The intermediate layer is a coating layer on the surface of the positive electrode substrate, and contains conductive particles such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and can be formed, for example, from a composition containing a resin binder and conductive particles.

[0087] [Negative electrode] The negative electrode has a negative electrode substrate and a negative electrode active material layer. The negative electrode active material layer contains a negative electrode active material. The negative electrode active material layer is laminated directly or via an intermediate layer along at least one surface of the negative electrode substrate.

[0088] The negative electrode active material layer is formed from a so-called negative electrode mixture containing a negative electrode active material. The negative electrode mixture forming the negative electrode active material layer further contains optional components such as a conductive agent, a binder, a thickener, and a filler as necessary. The optional components such as the conductive agent, the binder, the thickener, and the filler can be the same as those in the positive electrode active material layer.

[0089] The configuration of the intermediate layer in the negative electrode is not particularly limited, and may be formed to have the same configuration as the intermediate layer in the positive electrode described above.

[0090] [Separator] The separator may be made of, for example, a woven fabric, a nonwoven fabric, or a porous resin film. Among these, a porous resin film is preferred. From the viewpoint of strength, the main component of the porous resin film is preferably a polyolefin such as polyethylene or polypropylene. A porous resin film obtained by combining these resins with a resin such as aramid or polyimide may also be used. The term "separator" refers to a member different from the dry coating layer in the present invention.

[0091] The energy storage element according to one embodiment of the present invention may not include a separator between the positive electrode and the negative electrode. By not including a separator, the manufacturing cost of the energy storage element can be reduced.

[0092] [Non-aqueous electrolyte] As the non-aqueous electrolyte, a known electrolyte that is usually used in non-aqueous electrolyte secondary batteries can be used, and an electrolyte salt dissolved in a non-aqueous solvent can be used.

[0093] Examples of the non-aqueous solvent include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC); and chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC).

[0094] Examples of the electrolyte salt include lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts, and the like. The lithium salt is preferably LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 Inorganic lithium salts such as LiSO 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C2 F 5 ) 2 , LiN(SO 2 CF 3 )(SO 2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 and the like.

[0095] As the non-aqueous electrolyte, a room temperature molten salt, an ionic liquid, a polymer solid electrolyte, or the like can also be used.

[0096] The details of each element constituting the energy storage element are as described above.

[0097] [Specific configuration of the energy storage element] FIG. 1 is a schematic diagram of a rectangular energy storage element 1 (non-aqueous electrolyte secondary battery) which is one embodiment of the energy storage element according to the present invention. The figure is a see-through view of the inside of the case. In the energy storage element 1 shown in FIG. 1, an electrode body 2 is housed in a case 3. The electrode body 2 is formed by winding a positive electrode having a positive electrode active material layer and a negative electrode having a negative electrode active material layer with a separator interposed therebetween. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode current collector 4', and the negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode current collector 5'. A non-aqueous electrolyte is injected into the case 3.

[0098] The configuration of the energy storage element according to the present invention is not particularly limited, and examples include a cylindrical battery, a prismatic battery (a rectangular battery), and a flat battery.

[0099] [Method of manufacturing the energy storage element] The method for producing an electric storage element according to an embodiment of the present invention includes, for example, a step of housing a positive electrode, a negative electrode, and a non-aqueous electrolyte in a case. The positive electrode can be obtained by laminating the positive electrode active material layer directly or via an intermediate layer on a positive electrode substrate. The lamination of the positive electrode active material layer is performed by applying a positive electrode mixture paste to the positive electrode substrate. Similarly to the positive electrode, the negative electrode can be obtained by laminating the negative electrode active material layer directly or via an intermediate layer on a negative electrode substrate. The lamination of the negative electrode active material layer is performed by applying a negative electrode mixture paste to the negative electrode substrate. The positive electrode mixture paste and the negative electrode mixture paste may contain a dispersion solvent. As the dispersion solvent, for example, an aqueous solvent such as water or a mixed solvent mainly composed of water; or an organic solvent such as N-methylpyrrolidone or toluene can be used.

[0100] The method for producing the energy storage element further includes, as another step, for example, a step of stacking the negative electrode and the positive electrode with a separator interposed therebetween. An electrode body is formed by the step of stacking the negative electrode and the positive electrode with a separator interposed therebetween.

[0101] The negative electrode, the positive electrode, the non-aqueous electrolyte, and the like can be housed in a case by a known method. After the housing, the housing opening is sealed to obtain an electric storage element. The details of each element constituting the electric storage element obtained by the above manufacturing method are as described above.

[0102] <Other embodiments> The present invention is not limited to the above-described embodiment, and can be embodied in various other forms in addition to the above-described forms with various modifications and improvements.

[0103] In the above embodiment, the dry coated layer of the energy storage element is an insulating layer or an active material layer, but the energy storage element may have a configuration in which the dry coated layer is an intermediate layer, an edge coat layer, etc. Furthermore, the energy storage element may have a plurality of dry coated layers.

[0104] In the above embodiment, the insulating layer is formed on the entire surface of the active material layer, but the insulating layer may be formed only on a portion of the surface of the active material layer.

[0105] In the above embodiment, the description has been given mainly of the case where the power storage element is a non-aqueous electrolyte secondary battery, but other power storage elements may be used. Examples of other power storage elements include capacitors (electric double layer capacitors, lithium ion capacitors), etc. Examples of non-aqueous electrolyte secondary batteries include lithium ion non-aqueous electrolyte secondary batteries.

[0106] The present invention can also be realized as an electricity storage device including a plurality of the above-mentioned electricity storage elements. Also, an electricity storage unit can be configured by using one or a plurality of the electricity storage elements of the present invention, and further, an electricity storage device can be configured by using this electricity storage unit. The electricity storage device can be used as a power source for automobiles such as electric vehicles (EVs), hybrid vehicles (HEVs), plug-in hybrid vehicles (PHEVs), etc. Furthermore, the electricity storage device can be used in various power supply devices such as engine starting power supply devices, auxiliary power supply devices, and uninterruptible power supplies (UPS).

[0107] 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected energy storage elements 1, are further assembled. The energy storage device 30 may include a bus bar (not shown) that electrically connects the two or more energy storage elements 1, and a bus bar (not shown) that electrically connects the two or more energy storage units 20. The energy storage units 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of the one or more energy storage elements. EXAMPLES

[0108] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0109] [Example 1 and Comparative Examples 1 to 2] (Preparation of dry coating layer) α-NaFeO 2LiNi with type crystal structure γ Mn β Co (1-γ-β) O 2 A dry coating layer having the configuration shown in Table 1 was formed on one surface of a positive electrode active material layer containing as a positive electrode active material, and positive electrode plates of Example 1 and Comparative Example 1 to Comparative Example 2 were produced. The heating temperature in the heating step was set so that the surface of the positive electrode plate was 210°C, and the heating time was about 1 minute. The average thickness of the formed dry coating layer was 15 μm. The first synthetic resin of the first binder, the second synthetic resin of the second binder, and the filler used were as follows. (1) First synthetic resin Polyvinylidene fluoride with a weight average molecular weight of 800,000 and a melting point of about 170°C (2) Second synthetic resin Polyvinylidene fluoride with a weight average molecular weight of 200,000 and a melting point of about 170°C (3) Filler Boehmite with an average particle size of several micrometers

[0110] [evaluation] (peel strength) In accordance with JIS-Z-0237 (2009), adhesive tape was applied to the dry coating layer at room temperature, and a 180° peel test was performed at a peeling speed of 100 mm / min to evaluate the adhesion between the substrate and the dry coating layer. The measurement results are shown in Table 1.

[0111] (Solubility in high-temperature non-aqueous electrolyte) The solubility of the binder in a high-temperature nonaqueous electrolyte was simulated and evaluated according to the following procedure: The positive electrode plates of Example 1 and Comparative Examples 1 to 2, cut into 4 cm x 4 cm squares, were immersed in a polypropylene container containing propylene carbonate for 2 minutes at 140°C, and the dry coating layer was visually observed. Those in which the dry coating layer peeled off were judged to have dissolved the binder, and those in which the dry coating layer did not peel off were judged to have not dissolved the binder.

[0112] [Table 1]

[0113] As shown in Table 1, the dry coating layer of Example 1, which contains a first binder mainly composed of a first synthetic resin having a weight-average molecular weight of 500,000 or more and 1,500,000 or less, and a second binder mainly composed of a second synthetic resin having a weight-average molecular weight of 10,000 or more and 400,000 or less, had a peel strength superior to that of the comparative example. On the other hand, Comparative Example 1, which contained only the first binder, had a lower peel strength than Example 1. Moreover, in Comparative Example 2, which contained only the second binder, the second binder was dissolved in high-temperature propylene carbonate.

[0114] The above results demonstrate that the method for producing an electrode for an energy storage element can produce an electrode having good peel strength of the coating layer even when the heat treatment temperature in dry coating is suppressed. [Explanation of symbols]

[0115] 1 Energy storage element 2 Electrode body 3 Cases 4 Positive terminal 4' Positive lead 5 Negative terminal 5' Negative lead 20 Energy Storage Unit 30 Energy storage device

Claims

1. A step of dry-coating a coating powder containing a first binder and a second binder directly or indirectly onto a surface of a substrate; heating the coating powder at or above the melting points of the first binder and the second binder; Equipped with The first binder contains a first synthetic resin as a main component, The second binder is mainly composed of a second synthetic resin, The weight average molecular weight of the first synthetic resin is 500,000 or more and 1,500,000 or less, The weight average molecular weight of the second synthetic resin is 10,000 or more and 400,000 or less, A method for manufacturing an electrode for a storage element, wherein the content of the first binder in the coating powder is 0.5 mass% or more and 30 mass% or less, the content of the second binder is 0.5 mass% or more and 30 mass% or less, and the mass ratio of the second binder to the first binder is 0.15 or more and 7 or less.

2. 2. The method for producing an electrode for an electric storage element according to claim 1, wherein the first synthetic resin and the second synthetic resin have the same structural unit.

3. 3. The method for producing an electrode for an electric storage element according to claim 2, wherein the structural unit of the first synthetic resin and the structural unit of the second synthetic resin are identical to each other.

4. A substrate; An insulating dry coating layer formed directly or indirectly on the surface of the substrate; Equipped with The dry coating layer contains a first binder and a second binder, The first binder contains a first synthetic resin as a main component, The second binder is mainly composed of a second synthetic resin, The weight average molecular weight of the first synthetic resin is 500,000 or more and 1,500,000 or less, The weight average molecular weight of the second synthetic resin is 10,000 or more and 400,000 or less, the first binder and the second binder are welded together, An electrode for a storage element, wherein the content of the first binder in the dry coating layer is 0.5% by mass or more and 30% by mass or less, the content of the second binder is 0.5% by mass or more and 30% by mass or less, and the mass ratio of the second binder to the first binder is 0.15 or more and 7 or less.

5. 5. The electrode for a storage element according to claim 4, wherein the first synthetic resin and the second synthetic resin have the same structural unit.

6. 6. The electrode for a storage element according to claim 5, wherein the structural unit of the first synthetic resin and the structural unit of the second synthetic resin are identical to each other.

7. An active material layer is formed directly or indirectly on the surface of the substrate, 7. The electrode for a storage element according to claim 4, 5 or 6, wherein the dry coating layer is formed on a surface of the active material layer.

8. 7. The electrode for a storage element according to claim 4, claim 5 or claim 6, wherein the dry coating layer contains an active material.

9. An energy storage element comprising the electrode according to any one of claims 4 to 8.

Citation Information

Patent Citations

  • Wound electrode, its manufacturing method, and battery using it

    JP2006147185A

  • Anode and battery

    JP2006179439A

  • Electrode, lithium secondary battery, and method of manufacturing electrode

    JP2013137928A

  • Electrode and manufacturing method therefor and nonaqueous electrolyte battery having the electrode

    JP2013218895A

  • Porous membrane of vinylidene fluoride resin and process for producing the same

    WO2004081109A1