Resin composition and film for covering material
A resin composition with ethylene-vinyl acetate copolymer and tackifier resin addresses the weakness of conventional adhesive resins for PET and polylactic acid containers, providing robust sealing and adhesive strength across temperature variations and transportation challenges.
Patent Information
- Application Number
- JP2020046352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-25
- Filing Date
- 2020-03-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-03-17
AI Technical Summary
Existing adhesive resins for container lids, particularly for polyethylene terephthalate (PET) and biodegradable plastics like polylactic acid, fail to provide sufficient sealing and adhesive strength, leading to issues such as lid opening during transportation or storage due to weak adhesive strength and decreased sealing performance in low-temperature environments.
A resin composition comprising an ethylene-vinyl acetate copolymer with a vinyl acetate content of 3% to 15% and a weight average molecular weight to number average molecular weight ratio (Qw) of 1.5 to 4.5, combined with a tackifier resin, enhances sealing and adhesive properties, especially for PET and polylactic acid containers.
The composition achieves excellent sealing and adhesive properties, ensuring the lids remain secure during transportation and maintain strength in varying temperatures, while also being suitable for biodegradable plastics.
Smart Images

Figure 0007585615000001 
Figure 0007585615000002 
Figure 0007585615000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition used for a lid material for a container, and more specifically to an adhesive resin composition that has high sealing and adhesive properties with respect to a container and can be suitably used as a sealant for a lid material, and a film for a lid material that has this as a sealant layer. [Background technology]
[0002] 2. Description of the Related Art Conventionally, plastic containers such as polyethylene, polypropylene, and polystyrene, and paper containers mainly made of paper have been used for packaging food and beverages, pharmaceuticals, industrial parts, etc., and the lids of these containers are made of easily peelable films that have stable adhesive properties to protect the contents and have appropriate peelability so that they can be opened when peeled off.
[0003] Although many materials for easily peelable films have been known for containers such as polypropylene and polystyrene, no practically excellent easily peelable films have been found for containers made of amorphous polyethylene terephthalate (hereinafter referred to as "A-PET"), which has been increasingly used in recent years due to its low cost, transparency, and cold resistance. When used as a lid material for A-PET containers, conventional easily peelable films have problems such as the lid opening due to vibration or dropping during transportation or storage due to weak adhesive strength, and the container deforming and losing its sealing ability as a result of setting a high heat sealing temperature in an attempt to obtain high adhesive strength. In addition, there is a drawback in that the sealing strength decreases when stored in a low-temperature environment after adhesion, making it difficult to use in practice.
[0004] Generally, mixtures of polyethylene, ethylene-vinyl acetate copolymer, ethylene-α-olefin copolymer, etc. and tackifiers are known as adhesives for lid sealants, but such materials may not provide sufficient adhesive strength or sealing strength for containers made of a wide range of materials from polyolefin to A-PET, and there are problems such as the lid opening due to vibration or dropping during transportation or storage due to weak adhesive strength, and the container deforming and the sealing ability decreasing as a result of setting a high heat sealing temperature in an attempt to obtain high adhesive strength. In addition, resin compositions consisting of ethylene-α-olefin copolymer, olefin-based elastomer and / or styrene-based elastomer and tackifier (see, for example, Patent Document 1), and sealing materials consisting of ethylene-α-olefin copolymer, ethylene-polar monomer copolymer, ABA block copolymer, and tackifier (see, for example, Patent Document 2) are used, but they do not satisfy all of moldability, sealing strength, and adhesive strength.
[0005] In recent years, the demand for biodegradable plastics has been increasing due to growing awareness of environmental conservation. In the field of food packaging materials, the amount of biodegradable plastics such as polylactic acid (PLA) used as container materials is increasing, but the conventional adhesive resins for sealants used in the lids of these containers do not have sufficient adhesiveness to PLA, etc., and an adhesive resin that can be used suitably for these applications has been desired. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 1999-269319 A [Patent Document 2] Patent No. 4438108 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a resin composition and a film for a lid material that have excellent sealing and adhesive properties for plastic containers, particularly containers made of polyethylene terephthalate, polylactic acid, polystyrene, and polypropylene, and that can be suitably used as a sealant layer for a container lid material. [Means for solving the problem]
[0008] As a result of intensive research into the above-mentioned problems, the inventors discovered that a resin composition containing an ethylene-vinyl acetate copolymer having specific properties and a tackifier has excellent sealing and adhesive properties for various plastic containers including A-PET and polylactic acid, and thus completed the present invention.
[0009] That is, the present invention relates to a resin composition comprising 60 to 95 parts by weight of an ethylene-vinyl acetate copolymer (A) having a vinyl acetate content (VA) of 3 to 15% by weight and a ratio Qw (=Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.5 to 4.5, and 5 to 40 parts by weight of a tackifier resin (B) (where the total of (A) and (B) is 100 parts by weight). Effect of the Invention
[0010] According to the present invention, it is possible to provide a resin composition that has excellent sealing and adhesive properties for various types of plastic containers, particularly containers made of polyethylene terephthalate, polylactic acid, polystyrene, and polypropylene, and is useful for producing a sealant adhesive layer for the container lid material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The resin composition according to one embodiment of the present invention will be described in detail below.
[0012] The ethylene-vinyl acetate copolymer (A) constituting the present invention has a vinyl acetate content of 3% by weight or more and 15% by weight or less, preferably 3% by weight or more and 13% by weight or less, and more preferably 5% by weight or more and 10% by weight or less. If the vinyl acetate content is less than 3% by weight, the resulting composition is undesirably inferior in low-temperature heat sealability. On the other hand, if the vinyl acetate content exceeds 15% by weight, the resulting composition is undesirably inferior in moldability and adhesive strength.
[0013] Here, the vinyl acetate content in the ethylene-vinyl acetate copolymer can be measured by a method in accordance with JIS K 6924-1.
[0014] The ethylene-vinyl acetate copolymer (A) constituting the present invention has a ratio Mw / Mn (hereinafter referred to as "Qw") of its weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.5 to 4.5, preferably 2.0 to 4.5, more preferably 2.5 to 4.2. If Qw is less than 1.5, the extrusion load during molding increases, which is undesirable because it increases energy consumption. Also, if Qw exceeds 4.5, the adhesive strength and sealing strength of the composition of the present invention are undesirable. Here, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the ethylene-vinyl acetate copolymer (A) can be calculated as the molecular weight of linear polyethylene by measuring a universal calibration curve, for example, using gel permeation chromatography.
[0015] Furthermore, the ethylene-vinyl acetate copolymer (A) constituting the present invention is preferably such that the vinyl acetate content VA (unit: weight %) and Qw satisfy the following relational formula (1), since this increases the adhesive strength and sealing strength of the composition of the present invention. Qw<-1.9×lnVA+9.0 (1) Here, lnVA indicates the natural logarithm of the vinyl acetate content VA (% by weight).
[0016] The ethylene-vinyl acetate copolymer (A) constituting the present invention can be obtained by a known production method, and there is no particular restriction on the production method. However, a method of radical polymerization under high pressure using a tubular reactor is preferred because it can easily produce an ethylene-vinyl acetate copolymer having a vinyl acetate content and Qw that satisfy the requirements of the present application. The ethylene-vinyl acetate copolymer (A) in the present invention may be either a single component or a composition containing two or more types of copolymers. When the copolymer (A) is a composition, the vinyl acetate content of the composition means a value measured on the composition using the method of JIS K 6924-1 described above. Similarly, the Qw of the composition means a value measured on the composition using the method of gel permeation chromatography described above. It is sufficient that the vinyl acetate content and the ratio Qw of the weight average molecular weight to the number average molecular weight obtained for these compositions satisfy the requirements of the ethylene-vinyl acetate copolymer (A).
[0017] The tackifier resin (B) constituting the present invention can be any resin that falls within the category of tackifier resins. Examples of the tackifier resin (B) include synthetic petroleum resin-based tackifiers such as petroleum resin-based, coumarone resin-based, and styrene-based tackifiers, and natural resin-based tackifiers such as rosin-based, methyl ester-based, glycerin ester-based, pentaerythritol ester-based, terpene-based, and modified versions thereof. Among these tackifier resins, synthetic petroleum resin-based tackifiers include aliphatic petroleum resins, aliphatic hydrogenated petroleum resins, aromatic petroleum resins, aromatic hydrogenated petroleum resins, alicyclic petroleum resins, alicyclic hydrogenated petroleum resins, and copolymer hydrogenated petroleum resins. Among these, it is preferable to use either aromatic hydrogenated petroleum resins or alicyclic hydrogenated petroleum resins. In particular, a tackifier resin consisting of at least one type selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, alicyclic hydrogenated petroleum resins, and copolymerized petroleum resins is preferred because of its excellent sealing properties and adhesiveness. The tackifier resin (B) constituting the present invention preferably has a softening point measured by the ring and ball method in the range of 90° C. to 140° C., more preferably 100° C. to 135° C., and even more preferably 105° C. to 130° C. When the softening point is in the above range, blocking of the film after molding is small, and adhesive strength retention in a low-temperature environment is favorable.
[0018] The tackifier resin (B) constituting the present invention may be a commercially available product. Specifically, examples of petroleum resins include (trade names) Alcon P100, Alcon P125, Alcon P140, Alcon M90, Alcon M115, and Alcon M135 (all manufactured by Arakawa Chemical Industries Co., Ltd.), Imave S110, Imave P125 (all manufactured by Idemitsu Kosan Co., Ltd.), T-REZ RC115, and T-REZ HA125 (all manufactured by JXTG Energy Corporation). Examples of rosin resins include Pine Crystal KE-311 (manufactured by Arakawa Chemical Industries Co., Ltd.). Examples of terpene resins include YS Resin PX1150 and YS Resin PX1150N (all manufactured by Yasuhara Chemical Co., Ltd.).
[0019] The blending ratio of the ethylene-vinyl acetate copolymer (A) and the tackifier resin (B) constituting the present invention is as follows, where the total of (A) and (B) is 100 parts by weight. The blending ratio of the ethylene-vinyl acetate copolymer (A) constituting the present invention is 60 parts by weight or more and 95 parts by weight or less, preferably 70 parts by weight or more and 90 parts by weight or less, more preferably 75 parts by weight or more and 90 parts by weight or less. If the blending ratio of (A) is less than 60 parts by weight, the molding process stability of the resulting resin composition is inferior, which is not preferable. On the other hand, if it exceeds 95 parts by weight, the sealing property and adhesive property of the resulting resin composition are insufficient, which is not preferable. The blending ratio of (A) is preferably 81 parts by weight or more and 90 parts by weight or less. This allows the resin composition of the present application to maintain sufficient adhesive strength and sealing strength even if the blending amount of the tackifier (B) is reduced.
[0020] The blending ratio of the tackifier resin (B) constituting the present invention is 5 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, more preferably 10 parts by weight or more and 25 parts by weight or less. If the blending ratio of (B) is less than 5 parts by weight, the sealing property and adhesive property of the obtained resin composition will be insufficient, which is not preferable. On the other hand, if it exceeds 40 parts by weight, blocking between the films when molded into a film may become strong, which may adversely affect secondary processing, and the sealing property will decrease, which is not preferable. The blending ratio of (B) is preferably 10 parts by weight or more and 19 parts by weight or less. This allows the resin composition of the present application to maintain sufficient adhesive strength and sealing strength even if the blending amount of the tackifier (B) is reduced. That is, in the resin composition of the present application, the blending ratio of (A) is preferably 81 parts by weight or more and 90 parts by weight or less, and the blending ratio of (B) is preferably 10 parts by weight or more and 19 parts by weight or less (here, the total of (A) and (B) is 100 parts by weight).
[0021] The resin composition of the present invention may contain a thermoplastic block copolymer (C) containing at least one of an olefin and a diolefin as a structural unit and a vinyl aromatic hydrocarbon as a structural unit. The thermoplastic block copolymer (C) is represented by the following formula: (AB)n (AB)nA´ or (AB)mX (wherein A and A' each independently represent a vinyl aromatic hydrocarbon polymer block; B represents a polymer block of either an olefin or a diolefin; n represents an integer of 1 to 5; m represents an integer of 2 to 7; and X represents an m-valent polyfunctional compound.)
[0022] The thermoplastic block copolymer (C) is at least one of a linear structure, a radial structure, and a branched structure, and is a polymer having a block structure in which at least one end is a vinyl aromatic hydrocarbon polymer block. The thermoplastic block copolymer (c) may be a hydrogenated product thereof.
[0023] Examples of the vinyl aromatic hydrocarbons used herein include styrene, α-methylstyrene, vinyltoluene, p-tert-butylstyrene, vinylxylene, ethylvinylxylene, vinylnaphthalene, and mixtures thereof, etc. Of these, styrene is particularly preferred. Examples of the olefins that can be used include α-olefins such as ethylene, propylene, and 1-butene, and examples of the diolefins that can be used include conjugated diolefins such as butadiene and isoprene.
[0024] As the thermoplastic block copolymer (C), as long as the block B is predominantly an olefin unit, it is preferable to use a copolymer of either an olefin or a conjugated diolefin with a vinyl aromatic hydrocarbon, and it is more preferable to use a polymer block obtained by polymerizing a conjugated diolefin and hydrogenating it. In the present invention, a thermoplastic block copolymer of a vinyl aromatic hydrocarbon having vinyl aromatic hydrocarbon polymer blocks at both ends and an olefin or a diolefin is preferable, and in particular, a hydrogenated product of a polystyrene-polybutadiene-polystyrene block copolymer (styrene-ethylene / butylene-styrene triblock copolymer, hereinafter referred to as "hydrogenated SEBS") can be particularly preferably used from the viewpoint of improving thermal stability. The thermoplastic block copolymer (C) constituting the resin composition of the present invention may be a copolymer consisting of a single component, or a composition containing at least two or more types of copolymers. In particular, since it is a sealant adhesive excellent in moldability and adhesive strength, it is preferably a composition mixture of a hydrogenated styrene-butadiene-diblock copolymer and a hydrogenated styrene-butadiene-styrene-triblock copolymer, and the mixing ratio thereof is preferably 5 / 5 to 9 / 1 calculated as diblock copolymer / triblock copolymer. In addition, the styrene content in the mixture is preferably 10% by weight or more and 50% by weight or less based on the total amount of the thermoplastic block copolymer (C). The styrene content was measured by measuring the infrared absorption spectrum of a standard sample with a known styrene content at 700 cm -1An example of a method is to prepare a calibration curve using the absorption intensity due to nearby benzene rings, and then determine the styrene content from the absorption intensity due to the benzene rings of a sample with an unknown styrene content.
[0025] The blending ratio of the thermoplastic block copolymer (C) of vinyl aromatic hydrocarbon and olefin or diolefin constituting the present invention is preferably from 0.5 to 5 parts by weight, more preferably from 1 to 5 parts by weight, and even more preferably from 2 to 4 parts by weight, per 100 parts by weight of the mixture of ethylene-vinyl acetate copolymer (A) and tackifier resin (B). The thermoplastic block copolymer (C) of vinyl aromatic hydrocarbon and olefin or diolefin constituting the present invention may be a commercially available product, specifically, for example, Kraton G1726VS, Kraton G1657VS, Kraton G1730VS (all manufactured by Kraton Polymer Co., Ltd.), etc.
[0026] The resin composition of the present invention may contain an ethylene-α-olefin copolymer (D). As the ethylene-α-olefin copolymer (D), any copolymer that is generally within the category of ethylene-α-olefin copolymers may be used. The α-olefin is not particularly limited, but examples thereof include propene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, and 1-dodecane, each of which has 3 to 12 carbon atoms. These ethylene-α-olefin copolymers (D) can be suitably produced by copolymerizing ethylene and an α-olefin using a Ziegler catalyst, a chromium catalyst, or a metallocene catalyst. Examples of the polymerization method include a solution polymerization method, a high-pressure polymerization method, and a gas phase polymerization method. The ethylene-α-olefin copolymer (D) constituting the present invention has excellent low-temperature sealing property and sealing strength, and therefore has a density of 860 kg / m as measured according to JIS K6922-1 (1998). 3 More than 910kg / m 3 The following ranges are preferred: The blending ratio of the ethylene-α-olefin copolymer (D) constituting the present invention is preferably 5 parts by weight or more and 100 parts by weight or less, more preferably 10 parts by weight or more and 50 parts by weight or less, and even more preferably 18 parts by weight or more and 40 parts by weight or less, based on 100 parts by weight of the total mixture of the ethylene-vinyl acetate copolymer (A) and the tackifier resin (B).
[0027] The resin composition of the present invention may contain a low-density polyethylene (E). The low-density polyethylene (E) constituting the resin composition of the present invention is a low-density polyethylene obtained by polymerizing only ethylene using a known high-pressure polymerization method, and has a density range of 910 kg / m as measured according to JIS K6922-1. 3 More than 940kg / m 3 The number average molecular weight (Mn) of the low-density polyethylene (E) is preferably in the range of 500 to 18000, more preferably 1000 to 15000, and even more preferably 1000 to 13000. The melting point of the low-density polyethylene (E) is preferably in the range of 98°C or more and 120°C or less, and more preferably in the range of 100°C or more and 110°C or less.
[0028] The blending ratio of the low-density polyethylene (E) constituting the present invention is preferably from 1 to 50 parts by weight, more preferably from 5 to 30 parts by weight, and even more preferably from 8 to 25 parts by weight, per 100 parts by weight of the total mixture of the ethylene-vinyl acetate copolymer (A) and the tackifier resin (B). The low-density polyethylene (E) constituting the present invention may be a commercially available product, for example, Sanwax (manufactured by Sanyo Chemical Industries, Ltd.) or Hiwax (manufactured by Mitsui Chemicals, Inc.).
[0029] The resin composition of the present invention may contain a saponified ethylene-vinyl acetate copolymer (F). The saponified ethylene-vinyl acetate copolymer (F) constituting the present invention can be obtained by a known production method, for example, it can be produced by hydrolysis reaction of ethylene-vinyl acetate copolymer using an alkali or acid as a catalyst, and more specific production methods include, for example, a homogeneous saponification method in which the raw material ethylene-vinyl acetate copolymer is dissolved in a good solvent and reacted in a homogeneous system, or a heterogeneous saponification method in which the ethylene-vinyl acetate copolymer is reacted in a heterogeneous system in a poor solvent such as methanol or ethanol as pellets or powder, etc. The ethylene-vinyl acetate copolymer in this case may be one produced by a known production method, for example, a high-pressure method, an emulsion method, or a commercially available product.
[0030] The melting point of the ethylene-vinyl alcohol copolymer (F) constituting the present invention, as measured according to JIS K6924-2, is preferably 90°C or higher and 120°C or lower, more preferably 100°C or higher and 115°C or lower. The saponified ethylene-vinyl acetate copolymer (F) constituting the present invention may contain vinyl acetate in its molecular structure. The vinyl acetate content is preferably 40% by weight or less, more preferably 25% by weight or less. In the saponified product, when the saponification rate is 100%, vinyl acetate is not contained, so the vinyl acetate content is 0%. In other words, the vinyl acetate content is 0% or more.
[0031] The vinyl alcohol content of the saponified ethylene-vinyl acetate copolymer (F) constituting the present invention is preferably 1.2% by weight or more and 50% by weight or less, more preferably 3% by weight or more and 20% by weight or less. The vinyl alcohol content is preferably higher than the vinyl acetate content. The blending ratio of the saponified ethylene-vinyl acetate copolymer (F) constituting the present invention is preferably 1 part by weight or more and 100 parts by weight or less, more preferably 5 parts by weight or more and 30 parts by weight or less, and even more preferably 8 parts by weight or more and 20 parts by weight or less, per 100 parts by weight of the mixture of the ethylene-vinyl acetate copolymer (A) and the tackifier resin (B), in order to achieve excellent low-temperature sealability and heat seal strength. The saponified ethylene-vinyl acetate copolymer (F) constituting the present invention can be a commercially available product, specifically, for example, Mersen H (trade name, manufactured by Tosoh Corporation).
[0032] The resin composition of the present invention comprises an ethylene-vinyl acetate copolymer (A) and a tackifier resin (B), and further comprises, per 100 parts by weight of the total of (A) and (B), 0.5 to 5 parts by weight of a thermoplastic block copolymer (C) which contains at least one of an olefin or a diolefin as a constituent unit and which contains a vinyl aromatic hydrocarbon as a constituent unit, and further comprises a density of 860 kg / m as measured according to JIS K6922-1 (1998). 3 More than 910kg / m 3 The composition may contain 5 parts by weight or more and 100 parts by weight or less of an ethylene-α-olefin copolymer (D) in the following range.
[0033] The resin composition of the present invention comprises an ethylene-vinyl acetate copolymer (A) and a tackifier resin (B), and may further comprise, relative to a total of 100 parts by weight of (A) and (B), 0.5 to 5 parts by weight of a thermoplastic block copolymer (C) which contains at least either an olefin or a diolefin as a constituent unit and which contains a vinyl aromatic hydrocarbon as a constituent unit, and may further comprise 1 to 50 parts by weight of a low-density polyethylene (E) having a number average molecular weight in the range of 500 to 18,000 and a melting point in the range of 98°C to 120°C.
[0034] The resin composition of the present invention comprises an ethylene-vinyl acetate copolymer (A) and a tackifier resin (B), and may further comprise, relative to a total of 100 parts by weight of (A) and (B), 0.5 to 5 parts by weight of a thermoplastic block copolymer (C) which contains at least either an olefin or a diolefin as a structural unit and which contains a vinyl aromatic hydrocarbon as a structural unit, and may further comprise 1 to 100 parts by weight of a saponified ethylene-vinyl acetate copolymer (F) having a melting point of 90°C to 120°C as measured according to JIS K6924-2.
[0035] The resin composition of the present invention may be blended with other thermoplastic resins or rubbers, as well as light stabilizers, ultraviolet absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, flow improvers, release agents, flame retardants, colorants, inorganic neutralizing agents, hydrochloric acid absorbers, fillers, conductive agents, and the like, within the scope of not impairing the effects of the present invention.
[0036] There are no particular limitations on the method for preparing the resin composition of the present invention. For example, the ethylene-vinyl acetate copolymer (A), the tackifier resin (B) and the materials to be added thereto are pre-blended simultaneously in a mixer such as a Henschel mixer or a tumbler, and then melt-kneaded in a single-screw or twin-screw extruder.
[0037] The sealant adhesive according to one embodiment of the present invention will be described in detail below.
[0038] The resin composition of the present invention can be used as an adhesive. In particular, the resin composition can be suitably used as a sealant adhesive for plastic containers mainly composed of resins such as polyethylene terephthalate, polystyrene, polypropylene, etc., and other various resins, particularly as a lid sealant adhesive. Here, the term "sealant" refers to use for sealing a container. By using the lid sealant adhesive of the present invention, the lid and the container can be sealed.
[0039] Specific examples of materials for the plastic container include polyolefin resins, acrylic resins, polyamide resins, polyester resins, polycarbonate resins, polystyrene resins, styrene-acrylonitrile copolymers, and polyvinyl chloride resins. Examples of polyolefin resins include low-density polyethylene, high-density polyethylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, and polypropylene. Examples of the acrylic acid resin include polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyoctyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, and polyoctyl methacrylate.
[0040] Examples of polyamide resins include nylon 6, nylon 6,6, nylon 11, and nylon 12.
[0041] Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly 3-hydroxybutyrate, and polycaprolactone. When the resin composition of the present invention is used as an adhesive for adhering a plastic container containing these materials, the main component of the plastic container may be a single component or a composition of multiple resins. The container may also be a multi-layered laminate in which multiple materials are laminated. The resin composition of the present invention can be suitably used for containers made of, inter alia, polyethylene terephthalate, polylactic acid, polystyrene, or polypropylene.
[0042] The covering film, which is one embodiment of the present invention, will be described in detail below.
[0043] When the resin composition of the present invention is used as an adhesive, it is preferably used as an adhesive layer containing the composition (hereinafter referred to as a "sealant adhesive layer"). Furthermore, it can be suitably used as a film for a covering material having a configuration including at least two layers, a supporting substrate layer and a sealant adhesive layer, with the sealant adhesive layer being the outermost layer. The supporting substrate constituting the supporting substrate layer is not particularly limited as long as it has self-supporting properties, and examples thereof include olefin-based resins such as polyethylene, polypropylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, and saponified ethylene-vinyl acetate copolymer, polyethylene terephthalate, polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene Examples of the material include plastic films made of thermoplastic resins such as polyester resins such as poly(3-hydroxybutyrate / hydroxyhexanoate), poly(succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly(3-hydroxybutyrate), and polycaprolactone; polyamide resins such as nylon 6, nylon 6,6, nylon 11, and nylon 12; paper such as Japanese paper and composite paper; metal foils made of metals such as aluminum; vapor-deposited films in which aluminum or silica is vapor-deposited on the surface of polyester resin films; and films made of these alone or laminates. The thickness of the support substrate layer can be selected according to the application as long as the mechanical strength, workability, and the like are not impaired, but is generally about 5 to 100 μm, and preferably 10 to 50 μm.
[0044] When used as a film for a covering material, the thickness of the sealant adhesive layer can be selected according to the application as long as the adhesiveness, workability, etc. are not impaired, but is generally about 5 to 50 μm, preferably 10 μm to 40 μm, and more preferably 15 to 30 μm. In the present invention, an intermediate layer may be provided between the support substrate layer and the sealant adhesive layer to enhance the adhesion between the two layers. The intermediate layer may be composed of components such as thermoplastic resins, such as polyolefins, and thermoplastic elastomers, and these components may be used alone or in combination of two or more. For example, polyolefins include polyethylene and ethylene copolymers (ethylene-α-olefin copolymers, propylene-ethylene copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl acrylate copolymers, etc.) and modified products thereof. The intermediate layer may contain various additives, such as antioxidants, lubricants, antistatic agents, conductive agents, antiblocking agents, and tackifiers, within the scope of the present invention.
[0045] The thickness of the intermediate layer can be selected depending on the application as long as workability is not impaired, but is generally about 5 to 30 μm. In the present invention, an anchor coat layer of polyurethane or the like can be provided between the supporting substrate layer and the sealant adhesive layer, or between the supporting substrate layer and the intermediate layer, in order to improve adhesion between the two layers.
[0046] The lid material film having the sealant adhesive layer of the present invention as the outermost layer is suitable as a lid material for various types of plastic containers such as A-PET, and has high sealing strength and easy peelability. There are no particular limitations on the method for producing the covering film, but examples include a method in which the sealant adhesive and the supporting substrate layer are laminated together, and a method in which the sealant adhesive and the supporting substrate layer are co-extruded together. Examples of lamination methods include: (1) an extrusion lamination method in which an anchor coating agent is applied to a supporting substrate layer, and an adhesive layer is melt-extruded; (2) an extrusion lamination method in which an anchor coating agent is applied to a supporting substrate layer, and an intermediate layer is melt-extruded, and then an adhesive layer for a sealant is melt-extruded thereon; (3) an extrusion lamination method in which an intermediate layer having excellent adhesion to the supporting substrate, such as an ethylene-methacrylic acid copolymer or an ethylene-methyl methacrylate copolymer, is melt-extruded onto the supporting substrate layer, and then an adhesive layer for a sealant is melt-extruded thereon; (4) a co-extrusion lamination method in which an anchor coating agent is applied to a supporting substrate layer, and then the intermediate layer and the adhesive layer are melt-extruded simultaneously; and (5) Examples of the method include a coextrusion lamination method in which an intermediate layer having excellent adhesion to the support substrate, such as an ethylene-methacrylic acid copolymer or an ethylene-methyl methacrylate copolymer, and a sealant adhesive layer are simultaneously melt-extruded onto the support substrate layer, (6) a dry lamination method in which a film containing at least one layer of sealant adhesive is formed in advance by an inflation molding method or a cast molding method, and then laminated to a support substrate layer coated with an anchor coating agent, and (7) a sandwich extrusion lamination method in which an intermediate layer is melt-extruded using an extrusion lamination to laminate between a support substrate layer coated with an anchor coating agent and a film containing at least one layer of sealant adhesive. On the other hand, examples of the method of coextrusion of the sealant adhesive and the support substrate layer include a coextrusion inflation method and a coextrusion T-die method. EXAMPLES
[0047] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0048] (Measurement of molecular weight of ethylene-vinyl acetate copolymer (A)) The weight average molecular weight (Mw) and number average molecular weight (Mn) of the ethylene-vinyl acetate copolymer (A) were determined by gel permeation chromatography under the conditions shown below, using a universal calibration curve measured with monodisperse polystyrene, and calculated as the molecular weight of linear polyethylene. Model: Waters 150C ALC / GPC Solvent: 1,2,4-trichlorobenzene Flow rate: 1ml / min Temperature: 140℃ Measured concentration: 30mg / 30ml Injection volume: 100μl Column: 3 TSKgel GMH HR-H columns manufactured by Tosoh Corporation The ratio of Mw to Mn is shown in Table 5.
[0049] The sealing strength and adhesive strength of the covering films obtained in the examples were measured by the methods described below. (Seal strength measurement) The adhesive surface of the lid material film was placed on a cup made of amorphous polyethylene terephthalate (A-PET) (mouth diameter 65 mm, flange width 2 mm, capacity 215 ml) and pressure-heated and bonded using a cup sealer (Sunny Cup Co., Ltd., model UF-500) at 160°C, 40 kgf / cup, and 1 second. After cooling, the burst strength was measured using a seal tester (Sun Science Co., Ltd., model FKT-100J) at an air injection rate of 0.8 L / min. The strength obtained here is the sealing strength. (Adhesive strength measurement) The adhesive strength was measured according to the method described in JIS Z0238. The adhesive surface of the lid material film was overlapped with an A-PET sheet (Minelon Chemical Industry Co., Ltd.) having a thickness of 0.35 mm, and pressure-heated and bonded with a 20 mm wide seal bar under conditions of 170 ° C, 0.2 MPa, and 1 second using a heat seal tester (Tester Sangyo Co., Ltd., TP-701 type). After cooling, the test piece was cut into a strip shape with a width of 15 mm perpendicular to the width direction of the adhesive surface. The tensile strength of this test piece was measured using a tensile tester (A & D Co., Ltd., RTE-1210) under conditions of a peel angle of 180 degrees, a peel speed of 300 mm / min, and a chuck distance of 40 mm. The measured value at the point where the tensile strength stabilized was taken as the adhesive strength.
[0050] Example 1 As the ethylene-vinyl acetate copolymer (A), 85 parts by weight of resin (A-1) having a vinyl acetate content of 5.0%, a melt mass flow rate of 1.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 3.8, and as the tackifier resin (B), 15 parts by weight of fully hydrogenated petroleum resin (B-1) (manufactured by Arakawa Chemical Industries Co., Ltd., product name Alcon P125; softening temperature 125 ° C.) were pre-blended in a tumbler mixer, and then melt-kneaded at 180 ° C. using a twin-screw extruder to obtain pellets of the resin composition. In addition, in consideration of thermal stability, 0.05 parts by weight of a phenolic antioxidant (manufactured by BASF Co., Ltd., product name Irganox 1010) and 0.2 parts by weight of a slip agent (manufactured by Lion Akzo Co., Ltd., product name Armowax E) were added to the resin composition per 100 parts by weight of the sealant adhesive. Thereafter, the resin composition pellets were extrusion laminated at a processing temperature of 230°C onto the low-density polyethylene surface of the two-layer film, which had a biaxially oriented polyester film (12 μm thick) as a supporting substrate layer and a low-density polyethylene intermediate layer (25 μm thick, product name Petrothene 203, manufactured by Tosoh Corporation) using an extrusion laminator (manufactured by Placo Corporation, screw diameter 25 mmφ), to obtain a lid material film with a resin composition layer thickness of 15 μm. The evaluation results of the obtained resin composition and the covering film are shown in Table 1.
[0051] Example 2 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that the resin composition containing the ethylene-vinyl acetate copolymer (A-1) and the tackifier resin (B-1) of Example 1 was further compounded with 3 parts by weight of a thermoplastic block copolymer (C-1) (Kraton G1726VS) of a vinyl aromatic hydrocarbon and a diolefin, in which the mixing ratio of a hydrogenated styrene-butadiene-diblock copolymer and a hydrogenated styrene-butadiene-styrene-triblock copolymer was 7 / 3 and the styrene content was 30% by weight. The evaluation results of the obtained resin composition and the covering film are shown in Table 1.
[0052] Example 3 A resin composition and a film for a covering material were obtained in the same manner as in Example 1, except that 85 parts by weight of a resin (A-2) having a vinyl acetate content of 7.5%, a melt mass flow rate of 2.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 4.2 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0053] Example 4 A resin composition and a film for a covering material were obtained in the same manner as in Example 2, except that 85 parts by weight of a resin (A-2) having a vinyl acetate content of 7.5%, a melt mass flow rate of 2.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 4.2 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0054] Example 5 For the resin composition of Example 2, an ethylene-α-olefin copolymer (D) having a density of 860 kg / m 3 A resin composition and a film for covering material were obtained in the same manner as in Example 1, except that 20 parts by weight of an ethylene-α-olefin copolymer (D-1) (manufactured by Mitsui Chemicals, Inc., trade name Tafmer P-0375) was added. The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0055] Example 6 A resin composition and a film for a covering material were obtained in the same manner as in Example 1, except that 10 parts by weight of a low-density polyethylene (E-1) (manufactured by Sanyo Chemical Industries, Ltd., product name: Sanwax 151P) having a number average molecular weight (Mn) of 2000 and a melting point of 107°C was blended with the resin composition of Example 2 as the low-density polyethylene (E). The evaluation results of the obtained sealant adhesive and covering film are shown in Table 1.
[0056] Example 7 A resin composition and a film for a covering material were obtained in the same manner as in Example 1, except that 10 parts by weight of an ethylene-vinyl acetate copolymer saponified product (F-1) (manufactured by Tosoh Corporation, product name Mersen H6051) having a melting point of 107°C and a melt mass flow rate of 5.5 g / 10 min was blended with the resin composition of Example 2. The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0057] Comparative Example 1 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that 85 parts by weight of a resin (A-3) (manufactured by Tosoh Corporation, product name Ultrathene 520F) having a vinyl acetate content of 7.5%, a melt mass flow rate of 2.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 6.4 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 2. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0058] Comparative Example 2 A resin composition and a film for a covering material were obtained in the same manner as in Example 1, except that 85 parts by weight of a resin (A-4) (manufactured by Tosoh Corporation, product name Ultrathene 540) having a vinyl acetate content of 10%, a melt mass flow rate of 3.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 6.1 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 2. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0059] Comparative Example 3 A resin composition and a film for covering material were obtained in the same manner as in Example 1, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed to 50 parts by weight, and the blending ratio of the tackifier resin (B-1) was changed to 50 parts by weight. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 2. The obtained film for a covering material had poor sealing strength.
[0060] Comparative Example 4 A sealant adhesive and a covering film were obtained in the same manner as in Example 1, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed to 97 parts by weight and the blending ratio of the tackifier resin (B-1) was changed to 3 parts by weight. The evaluation results of the resulting sealant adhesive and covering film are shown in Table 2. The resulting covering film was poor in adhesive strength and sealing strength.
[0061] Comparative Example 5 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that 85 parts by weight of an ethylene-vinyl acetate copolymer (A-1) was replaced with 85 parts by weight of an ethylene-vinyl acetate copolymer (A-5) (manufactured by Tosoh Corporation, product name Ultrathene 537) having a vinyl acetate content of 5.5%, a melt mass flow rate of 8.5 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 5.8. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0062] Comparative Example 6 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that 85 parts by weight of an ethylene-vinyl acetate copolymer (A-6) (manufactured by Tosoh Corporation, product name Ultrathene 626) having a vinyl acetate content of 15%, a melt mass flow rate of 3.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 4.7 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0063] Comparative Example 7 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that 85 parts by weight of an ethylene-vinyl acetate copolymer (A-7) (manufactured by Tosoh Corporation, product name Ultrathene 541) having a vinyl acetate content of 10%, a melt mass flow rate of 9.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 5.4 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0064] Comparative Example 8 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that 85 parts by weight of an ethylene-vinyl acetate copolymer (A-1) was replaced with 85 parts by weight of an ethylene-vinyl acetate copolymer (A-8) (manufactured by Tosoh Corporation, product name Ultrathene 633) having a vinyl acetate content of 20%, a melt mass flow rate of 20 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 3.5. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0065] Comparative Example 9 A resin composition and a film for a lid material were obtained in the same manner as in Example 1, except that 85 parts by weight of an ethylene-vinyl acetate copolymer (A-9) (manufactured by Tosoh Corporation, product name Ultrathene 625) having a vinyl acetate content of 15%, a melt mass flow rate of 14 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 4.3 was blended in place of 85 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and covering film are shown in Table 3.
[0066] Comparative Example 10 A resin composition and a film for a covering material were obtained in the same manner as in Example 1, except that 42.5 parts by weight of ethylene-vinyl acetate copolymer (A-5) and 42.5 parts by weight of ethylene-vinyl acetate copolymer (A-6) were blended instead of 85 parts by weight of ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0067] Comparative Example 11 A resin composition and a film for covering material were obtained in the same manner as in Comparative Example 10, except that 3 parts by weight of the thermoplastic block copolymer (C-1) was added to the resin composition of Comparative Example 10. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength and sealing strength.
[0068] Comparative Example 12 A resin composition and a film for a covering material were obtained in the same manner as in Comparative Example 10, except that 3 parts by weight of a thermoplastic block copolymer (C-1) and 20 parts by weight of an ethylene-α-olefin copolymer (D-1) were added to the resin composition of Comparative Example 10. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained film for a covering material was poor in adhesive strength.
[0069] Example 8 Using the film for covering material obtained by the method of Example 1, the sealing strength was measured by the same method as that described in (Measurement of sealing strength), except that a polystyrene (PS) cup (mouth diameter 65 mm, flange width 2 mm, capacity 215 ml) was used instead of the A-PET cup. Also, the adhesive strength was measured by the same method as that described in (Measurement of adhesive strength), except that a PS sheet having a thickness of 0.4 mm was used instead of the A-PET sheet. The evaluation results of the covering film are shown in Table 4.
[0070] Example 9 Using the covering film obtained by the method of Example 2, the sealing strength and adhesive strength were measured in the same manner as in Example 8. The evaluation results of the covering film are shown in Table 4.
[0071] Example 10 The sealing strength was measured by the same method as described in (Measurement of sealing strength) except that a polypropylene (PP) cup (mouth diameter 65 mm, flange width 2 mm, capacity 215 ml) was used instead of the A-PET cup, using the film for covering material obtained by the method of Example 1. Also, the adhesive strength was measured by the same method as described in (Measurement of adhesive strength) except that a PP sheet having a thickness of 0.3 mm was used instead of the A-PET sheet. The evaluation results of the covering film are shown in Table 4.
[0072] Example 11 The sealing strength and adhesive strength of the covering film obtained in the method of Example 2 were measured in the same manner as in Example 10. The evaluation results of the covering film are shown in Table 4.
[0073] Example 12 The sealing strength was measured by the same method as described in (Measurement of sealing strength) except that a polylactic acid (PLA) cup (mouth diameter 65 mm, flange width 2 mm, capacity 215 ml) was used instead of the A-PET cup, using the film for covering material obtained by the method of Example 1. Also, the adhesive strength was measured by the same method as described in (Measurement of adhesive strength) except that a PLA sheet having a thickness of 0.3 mm was used instead of the A-PET sheet. The evaluation results of the covering film are shown in Table 4.
[0074] Example 13 The sealing strength and adhesive strength of the covering film obtained in the method of Example 2 were measured in the same manner as in Example 12. The evaluation results of the covering film are shown in Table 4.
[0075] Comparative Example 13 The sealing strength and adhesive strength were measured in the same manner as in Example 8, except that the covering film obtained in the method of Comparative Example 1 was used. The evaluation results of the covering film are shown in Table 4. The covering film was poor in adhesive strength and sealing strength.
[0076] Comparative Example 14 The sealing strength and adhesive strength were measured in the same manner as in Example 10, except that the covering film obtained in the method of Comparative Example 1 was used. The evaluation results of the covering film are shown in Table 4. The covering film was poor in adhesive strength and sealing strength.
[0077] Comparative Example 15 The sealing strength and adhesive strength were measured in the same manner as in Example 12, except that the covering film obtained in the method of Comparative Example 1 was used. The evaluation results of the covering film are shown in Table 4. The covering film was poor in adhesive strength and sealing strength.
[0078] By comparing the examples of the present invention with the comparative examples, it is clear that the resin composition containing the ethylene-vinyl acetate copolymer of the present invention having both VA and Qw has high adhesive strength and sealing strength superior to a composition containing the same amount of a composition containing a single component or multiple components of an ethylene-vinyl acetate copolymer not having both VA and Qw.
[0079] [Table 1]
[0080] [Table 2]
[0081] [Table 3]
[0082] [Table 4]
[0083]
Table 5
Claims
1. The vinyl acetate content (VA) is 3% by weight or more and 13% by weight or less, and the weight average molecular weight (Mw The ratio Qw of the number average molecular weight (Mn) to the ethylene-vinyl acetate copolymer is 1.5 or more and 4.5 or less. 60 parts by weight or more and 95 parts by weight or less of copolymer (A), 5 parts by weight or less of tackifier resin (B), Resin composition containing 40 parts by weight or less (where the total of (A) and (B) is 100 parts by weight) Sealant adhesives, including:
2. 2. The sealant adhesive according to claim 1, further comprising a resin composition containing 0.5 parts by weight or more and 5 parts by weight or less of a thermoplastic block copolymer (C) containing at least one of an olefin and a diolefin as a constituent unit and containing a vinyl aromatic hydrocarbon as a constituent unit, relative to 100 parts by weight of the resin composition.
3. The density measured according to JIS K6922-1 (1998) is 860 kg / m for 100 parts by weight of the resin composition. 3 More than 910kg / m 3 2. The sealant adhesive according to claim 1, comprising a resin composition containing 5 parts by weight or more and 100 parts by weight or less of an ethylene / α-olefin copolymer (D) in the following range:
4. 2. The sealant adhesive according to claim 1, comprising a resin composition containing 1 part by weight or more and 50 parts by weight or less of a low-density polyethylene (E) having a number average molecular weight in the range of 500 to 18,000 and a melting point in the range of 98°C or more and 120°C or less, measured according to JIS K6924-2, relative to 100 parts by weight of the resin composition.
5. 2. The sealant adhesive according to claim 1, comprising a resin composition containing 1 part by weight or more and 100 parts by weight or less of a saponified ethylene-vinyl acetate copolymer (F) having a melting point of 90° C. or more and 120° C. or less, measured according to JIS K6924-2, relative to 100 parts by weight of the resin composition.
6. The resin composition contains 0.5 parts by weight or more and 5 parts by weight or less of a thermoplastic block copolymer (C) containing at least one of an olefin and a diolefin as a constituent unit and containing a vinyl aromatic hydrocarbon as a constituent unit, based on 100 parts by weight of the resin composition, and further contains a density measured according to JIS K6922-1 (1998) of 860 kg / m 3 More than 910kg / m 3 2. The sealant adhesive according to claim 1, comprising a resin composition containing 5 parts by weight or more and 100 parts by weight or less of an ethylene / α-olefin copolymer (D) in the following range:
7. 2. The sealant adhesive according to claim 1, comprising a resin composition comprising, per 100 parts by weight of the resin composition, 0.5 parts by weight or more and 5 parts by weight or less of a thermoplastic block copolymer (C) which contains at least either an olefin or a diolefin as a constituent unit and which contains a vinyl aromatic hydrocarbon as a constituent unit, and further comprising 1 part by weight or more and 50 parts by weight or less of a low-density polyethylene (E) having a number average molecular weight in the range of 500 to 18,000 and a melting point in the range of 98°C or more and 120°C or less as measured according to JIS K6924-2.
8. 2. The sealant adhesive according to claim 1, comprising a resin composition comprising, relative to 100 parts by weight of the resin composition, 0.5 to 5 parts by weight of a thermoplastic block copolymer (C) which contains at least either an olefin or a diolefin as a constituent unit and which contains a vinyl aromatic hydrocarbon as a constituent unit, and further comprising 1 to 100 parts by weight of a saponified ethylene-vinyl acetate copolymer (F) having a melting point of 90° C. or more and 120° C. or less, as measured in accordance with JIS K6924-2.
9. 9. The sealant adhesive according to claim 1, wherein the tackifier resin (B) is at least one member selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, alicyclic hydrogenated petroleum resins, and copolymer petroleum resins.
10. Polyethylene terephthalate, polystyrene, polypropylene, polylactic acid The sealant adhesive according to any one of claims 1 to 9, which is used in at least one type of container.
11. A film for use as a covering material for containers, which is composed of at least two layers, the film comprising a layer containing the sealant adhesive according to any one of claims 1 to 10 and a supporting substrate layer.
12. The vinyl acetate content (VA) is 3% by weight or more and 13% by weight or less, and the weight average molecular weight (Mw The ratio Qw of the number average molecular weight (Mn) to the ethylene-vinyl acetate copolymer is 1.5 or more and 4.5 or less. 60 parts by weight or more and 95 parts by weight or less of copolymer (A), 5 parts by weight or less of tackifier resin (B), Resin composition containing 40 parts by weight or less (where the total of (A) and (B) is 100 parts by weight) The resin composition comprises, per 100 parts by weight of the resin composition, 1 part by weight or more and 100 parts by weight or less of a saponified ethylene-vinyl acetate copolymer (F) having a melting point of 90° C. or more and 120° C. or less as measured in accordance with JIS K6924-2.
13. The vinyl acetate content (VA) is 3% by weight or more and 13% by weight or less, and the weight average molecular weight (Mw The ratio Qw of the number average molecular weight (Mn) to the ethylene-vinyl acetate copolymer is 1.5 or more and 4.5 or less. 60 parts by weight or more and 95 parts by weight or less of copolymer (A), 5 parts by weight or less of tackifier resin (B), Resin composition containing 40 parts by weight or less (where the total of (A) and (B) is 100 parts by weight) The resin composition comprises, per 100 parts by weight of the copolymer, 0.5 parts or more and 5 parts by weight or less of a thermoplastic block copolymer (C) which contains at least one of an olefin and a diolefin as a constituent unit and which contains a vinyl aromatic hydrocarbon as a constituent unit, and further comprises 1 part by weight or more and 100 parts by weight or less of a saponified ethylene-vinyl acetate copolymer (F) having a melting point of 90° C. or more and 120° C. or less as measured in accordance with JIS K6924-2.
14. A film for use as a lid material for a container, which is composed of at least two layers, the layer including the resin composition according to claim 12 and the supporting substrate layer.
Citation Information
Patent Citations
Co-extruded adhesive film
JP1994328632A
Surface protecting film
JP1997111208A
Thermoplastic resin composition
JP1999269319A
Ethylene-vinyl acetate copolymer and hot-melt adhesive composition
JP2003002923A
Resin composition and surface-protecting film formed using the same
JP2009029901A