Inkjet ink set and recording method
The inkjet ink set with anionic and cationic inks having resin-coated pigments addresses the need for pretreatment in textile printing, achieving good color development and abrasion resistance through ink aggregation on the medium, simplifying the process and expanding color options.
Patent Information
- Application Number
- JP2020165274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Inkjet textile printing methods require a pretreatment step to achieve good color development and abrasion fastness, complicating the process and limiting color options.
An inkjet ink set comprising an anionic ink with an anionic resin-coated pigment and a cationic ink with a cationic resin-coated pigment, where both inks have similar colors and at least one resin has a urethane or polyester skeleton, allowing aggregation and adhesion without pretreatment, enhancing color development and abrasion resistance.
The ink set enables good color development and abrasion fastness without pretreatment, expanding color options and simplifying the printing process by aggregating the inks on the medium, ensuring effective adhesion and resistance.
Smart Images

Figure 0007585691000008 
Figure 0007585691000001 
Figure 0007585691000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an inkjet ink set and a recording method. [Background technology]
[0002] An inkjet recording method is known in which minute ink droplets are ejected from the nozzles of an inkjet head of an inkjet recording device to record an image on a recording medium, and research has been actively conducted not only on inkjet recording devices but also on the ink compositions used. In recent years, inkjet recording methods have also been used to dye (print) fabrics and the like. Conventionally, screen printing, roller printing, and the like have been used as methods for printing fabrics (woven fabrics and nonwoven fabrics), but from the viewpoints of high-mix low-volume productivity and real-time printability, etc., it is advantageous to apply inkjet recording methods, and various methods have been studied.
[0003] In such a method of printing using an inkjet recording method, the recording medium is treated (pretreated) with a cationic compound or the like in order to obtain good color development of the printed material. By pretreating the recording medium, the ink composition containing an anionic dispersed pigment or the like can be aggregated when the ink composition adheres to the recording medium. This makes it easier for the ink composition to remain near the surface of the recording medium, thereby obtaining good color development.
[0004] For example, Patent Document 1 describes an inkjet textile printing method in which a pigment textile printing ink composition is applied to a fabric that has been treated with a pretreatment liquid containing a cationic organic compound, and then the fabric is printed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-003184 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the inkjet textile printing method described in Patent Document 1, it is essential to pretreat the recording medium in order to obtain good color development of the printed textile, and the necessity of going through a pretreatment step for improving color development makes the inkjet textile printing method complicated. Therefore, it is desired to be able to obtain good color development and excellent friction fastness (abrasion resistance) of the printed textile, without the aggregation of the ink composition being dependent on the surface charge state of the recording medium and without carrying out a pretreatment for the purpose of improving color development. [Means for solving the problem]
[0007] One aspect of the inkjet ink set according to the present invention comprises: 1. An inkjet ink set comprising: an anionic ink containing an anionic resin, a pigment, and water; A cationic ink containing a cationic resin, a pigment, and water, the anionic ink and the cationic ink are similar in color to each other, the pigment in the anionic ink is coated with the anionic resin; the pigment in the cationic ink is coated with the cationic resin, At least one of the anionic resin and the cationic resin has a urethane skeleton or a polyester skeleton.
[0008] One aspect of the recording method according to the present invention is to A recording method using the inkjet ink set of the above aspect, an anionic ink depositing step of ejecting the anionic ink from an inkjet head and depositing the anionic ink on a recording medium; a cationic ink applying step of ejecting the cationic ink from the inkjet head and applying the cationic ink to the recording medium, The area on the recording medium to which the anionic ink has been applied and the area on the recording medium to which the cationic ink has been applied overlap in part or in whole. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic perspective view of an inkjet recording apparatus used in a recording method according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described. The embodiment described below is an example of the present invention. The present invention is not limited to the following embodiment, and includes various modified forms that are implemented within the scope that does not change the gist of the present invention. Note that not all of the configurations described below are necessarily essential configurations of the present invention.
[0011] 1. Inkjet ink set An inkjet ink set according to one embodiment of the present invention is an inkjet ink set comprising an anionic ink containing an anionic resin, a pigment, and water, and a cationic ink containing a cationic resin, a pigment, and water, wherein the anionic ink and the cationic ink are similar colors, the pigment in the anionic ink is coated with the anionic resin, and the pigment in the cationic ink is coated with the cationic resin, and at least one of the anionic resin and the cationic resin has a urethane skeleton or a polyester skeleton.
[0012] According to the inkjet ink set of the present embodiment, the ink composition can be aggregated by mixing the two inks, since the ink set has an anionic ink containing a pigment coated with an anionic resin and a cationic ink containing a pigment coated with a cationic resin. That is, unlike the mechanism in which aggregation occurs when the ink composition adheres to a recording medium treated with a cationic compound or the like, the ink composition can be aggregated by mixing the anionic ink and the cationic ink. This allows the ink composition to be aggregated regardless of whether or not the recording medium is pre-treated, and good color development can be obtained. Furthermore, since the anionic ink and the cationic ink are of similar colors, the color range in which aggregation can be performed can be expanded. That is, it is possible to obtain good color development by aggregation even in each color before mixing, which could not be realized by a configuration in which aggregation occurs only when two different colors are mixed.
[0013] Furthermore, when the ink composition aggregates, it tends to remain in the vicinity of the surface of the recording medium, which results in poor resistance to friction. However, by having at least one of the anionic resin and the cationic resin have a urethane skeleton or a polyester skeleton, it is possible to achieve good resistance to friction.
[0014] In the present invention, "similar colors" means that the difference between the hue angles of the anionic ink and the cationic ink is within 30 degrees. In this case, the "hue angle" refers to the angle in the counterclockwise direction, i.e., the positive direction, with the red direction being 0 degrees in the Lab color system chromaticity diagram. According to the Lab color system chromaticity diagram, all colors are defined by hue angles ranging from 0 degrees to 360 degrees. In this embodiment, the hue angles of the anionic ink and the cationic ink are determined based on the results of printing with each ink on a recording medium. More specifically, each ink is applied at a coating density of 39 mg / inch 2The resulting print was dried at 160°C for 5 minutes using an M&R conveyor drying oven "Economax D" and then returned to 25°C to obtain a printed item. The hue angle of the printed item was measured using a colorimeter "Spectrolino" (Gretag).
[0015] Hereinafter, the components contained in the anionic ink and cationic ink constituting the inkjet ink set according to this embodiment will be described separately for the anionic ink and the cationic ink.
[0016] 1.1.Anionic ink The anionic ink constituting the inkjet ink set according to this embodiment contains an anionic resin, a pigment, and water, and the anionic ink and the cationic ink described below are of similar colors, the pigment in the anionic ink is coated with the anionic resin, and at least one of the anionic resin and the cationic resin contained in the cationic ink has a urethane skeleton or a polyester skeleton.
[0017] 1.1.1.Pigments The anionic ink constituting the inkjet ink set according to this embodiment contains a pigment. Pigments that can be used in this embodiment are not particularly limited, and include inorganic pigments and organic pigments. In addition to titanium oxide and iron oxide, carbon black produced by a known method such as a contact method, a furnace method, or a thermal method can be used as the inorganic pigment.
[0018] Examples of organic pigments that can be used include azo pigments, polycyclic pigments, nitro pigments, nitroso pigments, aniline black, etc. Examples of azo pigments include azo lakes, insoluble azo pigments, condensed azo pigments, chelate azo pigments, etc. Examples of polycyclic pigments include phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinophthalone pigments, etc.
[0019] Examples of pigments used in black ink include carbon black. Carbon black is not particularly limited, but examples include furnace black, lamp black, acetylene black, channel black, etc. (CI Pigment Black 7), and commercially available products include No. 2300, 900, MCF88, No. 20B, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA77, MA100, No. 2200B, etc. (all trade names, manufactured by Mitsubishi Chemical Corporation), color black FW1, FW2, FW2V, FW18, FW200, S150, S160, Examples of such carbon fibers include S170, Pretex 35, U, V, 140U, Special Black 6, 5, 4A, 4, 250, etc. (all trade names, manufactured by Degussa Corporation), Conductex SC, Raven 1255, 5750, 5250, 5000, 3500, 1255, 700, etc. (all trade names, manufactured by Columbia Carbon Corporation), Regal 400R, 330R, 660R, Mogul L, Monarch 700, 800, 880, 900, 1000, 1100, 1300, 1400, Elftex 12, etc. (all trade names, manufactured by Cabot Corporation).
[0020] The pigment used in the white ink is not particularly limited, but examples thereof include white inorganic pigments such as CI Pigment White 6, 18, 21, titanium oxide, zinc oxide, zinc sulfide, antimony oxide, magnesium oxide, and zirconium oxide. In addition to the white inorganic pigments, white organic pigments such as white hollow resin particles and polymer particles can also be used.
[0021] The pigment used in the yellow ink is not particularly limited, but examples thereof include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 150, 151, 153, 154, 155, 167, 172, 180, and 185.
[0022] The pigment used in the magenta ink is not particularly limited, but may be, for example, CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48(Ca), 48(Mn), 57(Ca), 57:1, 88, 112, 114, 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, 245, 254, or CI Pigment Violet. 19, 23, 32, 33, 36, 38, 43, and 50.
[0023] Pigments used in cyan inks are not particularly limited, but examples thereof include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:34, 15:4, 16, 18, 22, 25, 60, 65, and 66, and CI Vat Blue 4 and 60.
[0024] Furthermore, pigments used in color inks other than magenta, cyan, and yellow are not particularly limited, but examples thereof include CI Pigment Green 7, 10, and 36, CI Pigment Brown 3, 5, 25, and 26, and CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43, and 63.
[0025] The pearl pigment is not particularly limited, but examples thereof include pigments having a pearlescent luster or an interference luster, such as titanium dioxide-coated mica, fish scale foil, and bismuth oxychloride.
[0026] The metallic pigment is not particularly limited, but examples thereof include particles of a simple substance such as aluminum, silver, gold, platinum, nickel, chromium, tin, zinc, indium, titanium, copper, or an alloy thereof.
[0027] The lower limit of the pigment content that can be contained in the anionic ink is preferably 1.5% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on the total mass of the anionic ink. Meanwhile, the upper limit of the pigment content that can be contained in the anionic ink is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 6% by mass or less, based on the total mass of the anionic ink. By having the pigment content within the above range, the image formed on the recording medium has excellent water resistance, gas resistance, light resistance, etc., and good storage stability.
[0028] 1.1.2.Anionic resins The anionic ink constituting the inkjet ink set according to the present embodiment contains an anionic resin, and at least one of the anionic resin and the cationic resin described later has a urethane skeleton or a polyester skeleton. By adopting such an embodiment, it is possible to improve the abrasion fastness. In the present invention, the term "urethane skeleton" refers to a skeleton containing a urethane bond, a urea bond, an allophanate bond, etc., formed by the reaction of an isocyanate group with another reactive group, for example, a hydroxyl group, an amino group, a urethane bond group, a carboxy group, etc. In the present invention, the term "polyester skeleton" refers to a skeleton containing a structure obtained by a polycondensation reaction of a diol unit and a dicarboxylic acid unit, which includes a skeleton other than a urethane skeleton. In addition, at least one of the anionic resin and the cationic resin described later may have a urethane skeleton and a polyester skeleton.
[0029] The anionic resin is not particularly limited as long as it exhibits anionic properties in the anionic ink, but for example, anionic resins having a urethane skeleton, anionic resins having a polyester skeleton, anionic resins having a styrene acrylic skeleton, anionic resins having a polycarboxylic acid skeleton, anionic resins having an olefin skeleton, etc. can be used. These resins can be used alone or in combination of two or more. Among these resins, anionic resins having a urethane skeleton are preferable from the viewpoint of further improving the friction fastness.
[0030] 1.1.2.1. Anionic resin with a urethane skeleton The anionic resin having a urethane skeleton is a polymer synthesized by reacting a polyisocyanate, a polyol, and a monomer for imparting an anionic group.
[0031] Examples of polyisocyanates include chain aliphatic isocyanates such as tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, dodecamethylene diisocyanate, trimethylhexamethylene diisocyanate, and lysine diisocyanate; aliphatic isocyanates having a cyclic structure such as 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-dicyclohexylmethane diisocyanate; 2,4-tolylene diisocyanate, 2,6-trimethyl-4,4'-tolylene diisocyanate, and 2,6-trimethyl-4,4'-tolylene diisocyanate; Examples of the aromatic isocyanates include rylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dichloro-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate. When synthesizing an anionic resin having a urethane skeleton, the above polyisocyanates may be used alone or in combination of two or more.
[0032] From the viewpoint of further improving the friction fastness, the anionic resin having a urethane skeleton preferably contains one or more selected from polycarbonate, polyether, and polyester. Accordingly, examples of the polyol include polycarbonate polyol, polyether polyol, and polyester polyol.
[0033] The polycarbonate polyol is not particularly limited, but examples thereof include reaction products of diols such as 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, polyethylene glycol, polypropylene glycol, or polytetramethylene glycol with dialkyl carbonates such as phosgene or dimethyl carbonate, or cyclic carbonates such as ethylene carbonate. These may be used alone or in combination of two or more.
[0034] Examples of polyether polyols include polymers obtained by ring-opening polymerization of cyclic ether compounds such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide, tetrahydrofuran, or epichlorohydrin, either alone or in combination of two or more, using a compound having an active hydrogen atom as a catalyst.Specific examples include polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.These may be used alone or in combination of two or more.
[0035] The polyester polyol is not particularly limited, but examples thereof include polyester polyols obtained by reacting dibasic acids such as terephthalic acid, isophthalic acid, adipic acid, azelaic acid, and sebacic acid, or their dialkyl esters, or mixtures thereof, with glycols such as ethylene glycol, propylene glycol, diethylene glycol, butylene glycol, neopentyl glycol, 1,6-hexane glycol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene ether glycol, or mixtures thereof. These may be used alone or in combination of two or more.
[0036] Examples of monomers for imparting anionic groups include monomers having a carboxyl group or a sulfone group, etc. Examples of such monomers include monohydroxycarboxylic acids such as lactic acid, dihydroxycarboxylic acids such as α,α-dimethylolacetic acid, α,α-dimethylolpropionic acid, and α,α-dimethylolbutyric acid, and diaminosulfonic acids such as 3,4-diaminobutanesulfonic acid and 3,6-diamino-2-toluenesulfonic acid.
[0037] 1.1.2.2. Anionic resins with polyester skeletons The anionic resin having a polyester skeleton is a polymer obtained by polycondensation of a polyol and a polycarboxylic acid.
[0038] Examples of polyols include ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, trimethylolpropane, pentaerythritol, etc. When synthesizing an anionic resin having a polyester skeleton, the above polyols may be used alone or in combination of two or more kinds.
[0039] Specific examples of polycarboxylic acids include oxalic acid, succinic acid, tartaric acid, malic acid, citric acid, phthalic acid, isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, etc. When synthesizing an anionic resin having a polyester skeleton, the above polycarboxylic acids may be used alone or in combination of two or more kinds.
[0040] 1.1.2.3. Anionic resins with blocked isocyanate groups In addition, the anionic resin in the present embodiment may have a blocked isocyanate group from the viewpoint of further improving the friction fastness. The blocked isocyanate group is a crosslinkable group in which an isocyanate group is chemically protected, that is, capped or blocked. The blocked isocyanate group is deprotected and activated by the application of heat, and forms a bond, for example, a urethane bond, a urea bond, an allophanate bond, or the like.
[0041] The anionic resin having a blocked isocyanate group is preferably an anionic resin having a urethane skeleton described above that has a blocked isocyanate group. Such an anionic resin tends to have better friction fastness. In addition, the blocked isocyanate group of the anionic resin having a blocked isocyanate group is preferably provided in three or more per molecule, and the blocked isocyanate group is deprotected, activated, and reacted to form a crosslinked structure. In addition, the anionic resin having a urethane skeleton described above that has a blocked isocyanate group may be synthesized by reacting a polyisocyanate and / or a blocked isocyanate, a polyol, and a monomer for imparting an anionic group.
[0042] A blocked isocyanate (chemically protected isocyanate) contains a latent isocyanate group in which the isocyanate group is blocked with a blocking agent, and can be obtained, for example, by reacting a polyisocyanate compound with a blocking agent.
[0043] Examples of the polyisocyanate compound include polyisocyanate monomers and polyisocyanate derivatives. Examples of the polyisocyanate monomers include polyisocyanates such as aromatic polyisocyanates, araliphatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates. These polyisocyanate monomers can be used alone or in combination of two or more kinds.
[0044] Examples of the polyisocyanate derivative include multimers of the above-mentioned polyisocyanate monomers (e.g., dimers, trimers (e.g., isocyanurate-modified products, iminooxadiazinedione-modified products), pentamers, heptamers, etc.), allophanate-modified products (e.g., allophanate-modified products produced by the reaction of the above-mentioned polyisocyanate monomers with low-molecular-weight polyols described below), polyol-modified products (e.g., polyol-modified products (alcohol adducts) produced by the reaction of the polyisocyanate monomers with low-molecular-weight polyols described below), biuret-modified products (e.g., Examples of such modified compounds include biuret modified compounds produced by the reaction of the above-mentioned polyisocyanate monomer with water or amines, urea modified compounds (e.g., urea modified compounds produced by the reaction of the above-mentioned polyisocyanate monomer with diamines), oxadiazinetrione modified compounds (e.g., oxadiazinetrione modified compounds produced by the reaction of the above-mentioned polyisocyanate monomer with carbon dioxide), carbodiimide modified compounds (carbodiimide modified compounds produced by the decarboxylation condensation reaction of the above-mentioned polyisocyanate monomers), uretdione modified compounds, and uretonimine modified compounds.
[0045] When two or more types of polyisocyanate compounds are used in combination, for example, when producing a blocked isocyanate, two or more types of polyisocyanate compounds may be reacted simultaneously, or blocked isocyanates obtained by using each polyisocyanate compound individually may be mixed.
[0046] The blocking agent blocks and inactivates the isocyanate group, while regenerating or activating the isocyanate group after deblocking. The blocking agent also has a catalytic action to activate the isocyanate group in both the blocked and deblocked states.
[0047] Examples of blocking agents include imidazole compounds, imidazoline compounds, pyrimidine compounds, guanidine compounds, alcohol compounds, phenol compounds, active methylene compounds, amine compounds, imine compounds, oxime compounds, carbamic acid compounds, urea compounds, acid amide (lactam) compounds, acid imide compounds, triazole compounds, pyrazole compounds, mercaptan compounds, and bisulfites.
[0048] Examples of imidazole compounds include imidazole (dissociation temperature 100°C), benzimidazole (dissociation temperature 120°C), 2-methylimidazole (dissociation temperature 70°C), 4-methylimidazole (dissociation temperature 100°C), 2-ethylimidazole (dissociation temperature 70°C), 2-isopropylimidazole, 2,4-dimethylimidazole, and 2-ethyl-4-methylimidazole.
[0049] Examples of the imidazoline compounds include 2-methylimidazoline (dissociation temperature: 110° C.) and 2-phenylimidazoline.
[0050] An example of the pyrimidine compound is 2-methyl-1,4,5,6-tetrahydropyrimidine.
[0051] Examples of the guanidine compounds include 3,3-dialkylguanidines such as 3,3-dimethylguanidine, 1,1,3,3-tetraalkylguanidines such as 1,1,3,3-tetramethylguanidine (dissociation temperature 120° C.), and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.
[0052] Examples of alcohol compounds include methanol, ethanol, 2-propanol, n-butanol, s-butanol, 2-ethylhexyl alcohol, 1- or 2-octanol, cyclohexyl alcohol, ethylene glycol, benzyl alcohol, 2,2,2-trifluoroethanol, 2,2,2-trichloroethanol, 2-(hydroxymethyl)furan, 2-methoxyethanol, methoxypropanol, 2-ethoxyethanol, n-propoxyethanol, 2-butoxyethanol, and 2-ethoxyethoxyethanol. , 2-ethoxybutoxyethanol, butoxyethoxyethanol, 2-butoxyethylethanol, 2-butoxyethoxyethanol, N,N-dibutyl-2-hydroxyacetamide, N-hydroxysuccinimide, N-morpholineethanol, 2,2-dimethyl-1,3-dioxolane-4-methanol, 3-oxazolidineethanol, 2-hydroxymethylpyridine (dissociation temperature 140°C), furfuryl alcohol, 12-hydroxystearic acid, triphenylsilanol, 2-hydroxyethyl methacrylate, and the like.
[0053] Examples of the phenolic compounds include phenol, cresol, ethylphenol, n-propylphenol, isopropylphenol, n-butylphenol, s-butylphenol, t-butylphenol, n-hexylphenol, 2-ethylhexylphenol, n-octylphenol, n-nonylphenol, di-n-propylphenol, diisopropylphenol, isopropylcresol, di-n-butylphenol, di-s-butylphenol, di-t-butylphenol, di-n-octylphenol, di-2-ethylhexylphenol, and di-n-nonylphenol. Examples of the phenols include phenol, nitrophenol, bromophenol, chlorophenol, fluorophenol, dimethylphenol, styrenated phenol, methyl salicylate, methyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, 2-ethylhexyl hydroxybenzoate, 4-[(dimethylamino)methyl]phenol, 4-[(dimethylamino)methyl]nonylphenol, bis(4-hydroxyphenyl)acetic acid, 2-hydroxypyridine (dissociation temperature 80°C), 2- or 8-hydroxyquinoline, 2-chloro-3-pyridinol, and pyridine-2-thiol (dissociation temperature 70°C).
[0054] Examples of active methylene compounds include Meldrum's acid, dialkyl malonates (e.g., dimethyl malonate, diethyl malonate, di-n-butyl malonate, di-t-butyl malonate, di-2-ethylhexyl malonate, methyl n-butyl malonate, ethyl n-butyl malonate, methyl s-butyl malonate, ethyl s-butyl malonate, methyl t-butyl malonate, ethyl t-butyl malonate, diethyl methylmalonate, dibenzyl malonate, diphenyl malonate, benzyl methyl malonate, ethyl phenyl malonate, t-butylphenyl malonate, isopropylidene malonate, etc.), alkyl acetoacetates (e.g., methyl acetoacetate, ethyl acetoacetate, n-propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, t-butyl acetoacetate, benzyl acetoacetate, phenyl acetoacetate, etc.), 2-acetoacetoxyethyl methacrylate, acetylacetone, ethyl cyanoacetate, etc.
[0055] Examples of the amine compounds include dibutylamine, diphenylamine, aniline, N-methylaniline, carbazole, bis(2,2,6,6-tetramethylpiperidinyl)amine, di-n-propylamine, diisopropylamine (dissociation temperature 130° C.), isopropylethylamine, 2,2,4- or 2,2,5-trimethylhexamethyleneamine, N-isopropylcyclohexylamine (dissociation temperature 140° C.), dicyclohexylamine (dissociation temperature 130° C.), bis(3,5,5-trimethylcyclohexyl)amine, piperidine, 2, Examples of the amines include 6-dimethylpiperidine (dissociation temperature 130° C.), t-butylmethylamine, t-butylethylamine (dissociation temperature 120° C.), t-butylpropylamine, t-butylbutylamine, t-butylbenzylamine (dissociation temperature 120° C.), t-butylphenylamine, 2,2,6-trimethylpiperidine, 2,2,6,6-tetramethylpiperidine (dissociation temperature 80° C.), (dimethylamino)-2,2,6,6-tetramethylpiperidine, 2,2,6,6-tetramethyl-4-piperidine, 6-methyl-2-piperidine, and 6-aminocaproic acid.
[0056] Examples of the imine compounds include ethyleneimine, polyethyleneimine, 1,4,5,6-tetrahydropyrimidine, and guanidine.
[0057] Examples of oxime compounds include formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime (dissociation temperature 130°C), cyclohexanone oxime, diacetyl monooxime, benzophenone oxime, 2,2,6,6-tetramethylcyclohexanone oxime, diisopropyl ketone oxime, methyl t-butyl ketone oxime, diisobutyl ketone oxime, methyl isobutyl ketone oxime, methyl isopropyl ketone oxime, methyl 2,4-dimethylpentyl ketone oxime, methyl 3-ethylheptyl ketone oxime, methyl isoamyl ketone oxime, n-amyl ketone oxime, 2,2,4,4-tetramethyl-1,3-cyclobutanedione monooxime, 4,4'-dimethoxybenzophenone oxime, and 2-heptanone oxime.
[0058] An example of the carbamic acid compound is N-phenylcarbamate phenyl.
[0059] Examples of the urea-based compounds include urea, thiourea, and ethyleneurea.
[0060] Examples of acid amide (lactam) compounds include acetanilide, N-methylacetamide, acetic acid amide, ε-caprolactam, δ-valerolactam, γ-butyrolactam, pyrrolidone, 2,5-piperazinedione, and laurolactam.
[0061] Examples of the acid imide compounds include succinimide, maleimide, and phthalimide.
[0062] Examples of triazole compounds include 1,2,4-triazole and benzotriazole.
[0063] Examples of pyrazole compounds include pyrazole, 3,5-dimethylpyrazole (dissociation temperature 120° C.), 3,5-diisopropylpyrazole, 3,5-diphenylpyrazole, 3,5-di-t-butylpyrazole, 3-methylpyrazole, 4-benzyl-3,5-dimethylpyrazole, 4-nitro-3,5-dimethylpyrazole, 4-bromo-3,5-dimethylpyrazole, and 3-methyl-5-phenylpyrazole.
[0064] Examples of the mercaptan compounds include butyl mercaptan, dodecyl mercaptan, and hexyl mercaptan.
[0065] An example of the bisulfite is sodium bisulfite.
[0066] Furthermore, the blocking agent is not limited to the above, and other blocking agents such as benzoxazolone, isatoic anhydride, and tetrabutylphosphonium acetate can also be used.
[0067] For some of the compounds given as examples above, the dissociation temperature is also shown as the temperature at which the isocyanate group is regenerated.
[0068] Such blocking agents can be used alone or in combination of two or more kinds. The dissociation temperature of the blocking agent can be appropriately selected. The dissociation temperature is, for example, 60°C or more and 230°C or less, preferably 80°C or more and 200°C or less, more preferably 100°C or more and 180°C or less, and further preferably 110°C or more and 160°C or less. Within this temperature range, the pot life of the anionic ink can be sufficiently extended, and the temperature in the heating step can be prevented from being too high.
[0069] 1.1.3.Anionic resin-coated pigments In the anionic ink constituting the inkjet ink set according to this embodiment, the above-mentioned pigment is coated with the above-mentioned anionic resin. Note that the coating with the anionic resin is intended to disperse the pigment in water. If the pigment can be dispersed in water, it can be considered that the pigment is sufficiently coated with the anionic resin.
[0070] A preferred method for producing a pigment coated with an anionic resin (hereinafter also referred to as an "anionic resin-coated pigment") is a phase inversion emulsification method. The anionic resin used in the phase inversion emulsification method is preferably synthesized by solution polymerization. It is also preferably synthesized by solution polymerization using a radical polymerization initiator. The polymer dispersion obtained by solution polymerization can be used as it is in the pigment dispersion step. An example of the phase inversion emulsification method can include a pigment dispersion step in which a mixed liquid containing a polymer, a pigment, an organic solvent, and an excess amount of water relative to the organic solvent is prepared, and the pigment is dispersed in the aqueous phase of the mixed liquid in a state in which at least a part of the polymer coats the pigment. The polymer and pigment present in the aqueous phase of the pigment dispersion thus obtained can be used together with at least a part of the aqueous phase or in a state in which they are separated from the aqueous phase to prepare an anionic ink. During the phase inversion emulsification, the organic solvent can be distilled off.
[0071] The pigment dispersion step can be carried out, for example, as follows. That is, a pigment dispersion (organic solvent) is prepared by dispersing a pigment in an organic solvent, a polymer dispersion is prepared by dispersing or dissolving a polymer in water, and the pigment dispersion (organic solvent) and the polymer dispersion are mixed. In this way, a state in which the polymer is unevenly distributed near the pigment surface and covers the pigment can be formed in the aqueous phase (phase inversion emulsification). Alternatively, a dispersion of an organic solvent containing a pigment and a polymer (containing any one or a combination of a neutralizing agent, water, and a surfactant as appropriate) can be prepared, and this can be mixed with a large amount of water (preferably in excess of the organic solvent) to transfer the pigment and polymer from the organic solvent phase to the aqueous phase, thereby forming a state in which the pigment is covered (encapsulated) by the polymer in the aqueous phase.
[0072] In the pigment dispersion step, the pigment is dispersed in the aqueous phase by stirring the pigment in a mixed medium of an organic solvent and water using various dispersing means. In addition to ultrasonic waves, a high-pressure homogenizer, an ultra-high-pressure homogenizer, a high-speed mixer, a sand mill, a bead mill, a roll mill, or the like can be appropriately selected and used to disperse the pigment. The pigment dispersion step in the phase inversion emulsification method is preferably carried out using a device that mixes and stirs while applying an appropriate shear so that the polymer and the pigment come into contact with each other and the polymer can adhere to the pigment surface.
[0073] The organic solvent used in the process of preparing the pigment dispersion is not particularly limited, but in consideration of the ease of distilling off the organic solvent in the end, an organic solvent having a low boiling point is preferred. Examples of the organic solvent include ketone-based organic solvents such as acetone and methyl ethyl ketone, ester-based organic solvents such as ethyl acetate, alcohol-based organic solvents such as ethanol and isopropyl alcohol, and aromatic hydrocarbon-based organic solvents such as benzene.
[0074] In order to dissolve or disperse a polymer having an acidic group such as a carboxyl group in water, various inorganic alkalis as well as various organic amines can be used as neutralizing agents, but it is preferable to use inorganic alkalis.
[0075] To separate the polymer and pigment (polymer-coated pigment) from the aqueous phase, the organic solvent can be removed from the pigment dispersion having an aqueous phase in which the pigment coated with an anionic resin is dispersed by a method such as heating, or a method such as centrifugation, water washing, ultrafiltration, or pressure filtration can be appropriately selected.
[0076] As a method for producing an anionic resin-coated pigment having a urethane skeleton, a production method including the following steps is preferably used. (i) A step of obtaining a polyurethane prepolymer (T). (ii) A process in which a liquid in which a polyurethane prepolymer (T) is dissolved in an organic solvent (L) is mixed with a pigment (P0) and the mixture is finely divided by mechanical crushing to obtain an organic solvent-based pigment slurry (S). (iii) A step of neutralizing with a neutralizing agent (K). (iv) A step of dispersing the obtained neutralized product in water, reacting it with a chain extender (H), a reaction terminator (J) and / or water, and then removing the organic solvent (L) as necessary.
[0077] <Manufacturing process (i)> The polyurethane prepolymer (T) is obtained by heating and reacting polyester polyol (A1) and / or polycarbonate polyol (A2) and / or polyether polyol (A3), aliphatic isocyanate (B1) and / or aliphatic isocyanate having a cyclic structure (B2), and monomer having a carboxyl group (D) in a heating facility. For example, a method of charging (A1) and / or (A2) and / or (A3), (B1) and / or (B2), and (D) in a container, uniformly stirring, and then heating without stirring in a heating dryer or heating furnace, or a method of heating and reacting while stirring or kneading in a simple pressure reaction device (autoclave), a Kolben, a single-screw or twin-screw kneader, a plastomill, a universal kneader, or the like, can be mentioned. Among these, the method of reacting by heating with stirring or kneading is preferred because the homogeneity of the resulting (T) is high and the mechanical properties, durability, chemical resistance, abrasion resistance, etc. of the resulting coating tend to be superior.
[0078] The reaction temperature in producing the polyurethane prepolymer (T) is preferably 60 to 120° C., more preferably 60 to 110° C., and most preferably 60 to 100° C., from the viewpoint of the contents of allophanate groups and biuret groups in (T). The time in producing (T) can be appropriately selected depending on the equipment used, but is generally preferably 1 minute to 100 hours, more preferably 3 minutes to 30 hours, and particularly preferably 5 minutes to 20 hours. Within this range, (T) that can fully exhibit the effects of the present invention can be obtained.
[0079] The polyurethane prepolymer (T) can be diluted with an organic solvent (L). Examples of the organic solvent (L) include ketone-based solvents (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), ester-based solvents (ethyl acetate, butyl acetate, γ-butyrolactone, etc.), ether-based solvents (THF, etc.), amide-based solvents [N,N-dimethylformamide (hereinafter abbreviated as DMF), N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-methylcaprolactam, etc.], alcohol-based solvents (methanol, ethanol, isopropyl alcohol, etc.), and aromatic hydrocarbon-based solvents (toluene, xylene, etc.). These organic solvents may be used alone or in combination of two or more. Among these, amide-based solvents are preferred from the viewpoint of the solubility of the polyurethane prepolymer (T).
[0080] The organic solvent (L) may be added at any time before, during, or after the urethanization reaction, or before emulsification, but is preferably used before the urethanization reaction from the viewpoint of uniformity of the reaction system.
[0081] In order to control the urethanization reaction rate, known reaction catalysts (such as tin octylate and bismuth octylate) and reaction retarders (such as phosphoric acid) can be used. The amount of these catalysts or reaction retarders added is preferably 0.001 to 3% by weight, more preferably 0.005 to 2% by weight, and particularly preferably 0.01 to 1% by weight, based on the weight of (T).
[0082] <Manufacturing process (ii)> As an apparatus for mixing the polyurethane prepolymer (T) and the pigment (P0), the apparatus used for synthesizing (T) can be used as is. Examples of dispersing machines used for pulverizing the pigment (P0) by mechanical crushing include a paint shaker, a ball mill, a sand mill, and a nano mill. Specific examples include the SC Mill (manufactured by Nippon Coke & Engineering Co., Ltd.), TSU-6U (manufactured by Imex Co., Ltd.), and Labostar Mini HFM02 (manufactured by Ashizawa Finetech Co., Ltd.).
[0083] <Manufacturing process (iii)> If necessary, the carboxyl group portion introduced into the polyurethane prepolymer (T) is neutralized with a neutralizer (K). The neutralizer (K) may be added at any time before, during, or after the urethanization reaction, before, during, or after emulsification and dispersion in an emulsified aqueous medium, but is preferably added before or during emulsification from the viewpoints of the stability of the urethane resin and the stability of the composite particle dispersion for ink.
[0084] The neutralizing agent used in (K) may be added at any time before, during, or after the urethanization reaction, or before, during, or after the water dispersion step, but from the viewpoint of the stability of the urethane resin and the stability of the aqueous dispersion, it is preferable to add the neutralizing agent before or during the water dispersion step. In addition, the neutralizing agent that has volatilized during the desolvation may be added after the desolvation, and the type of neutralizing agent to be added may be freely selected from those described above.
[0085] The amount of (K) used is adjusted so that the content of the monomer having a carboxyl group based on the weight of the polyurethane resin (U) is 23 to 80 mg / g from the viewpoint of the stability of the anionic resin-coated pigment aqueous dispersion. The neutralization rate of the carboxyl group in the neutralization step is preferably 20 to 100%, more preferably 60 to 100%, from the viewpoint of dispersion stability.
[0086] <Manufacturing process (iv)> The method for emulsifying the neutralized product obtained in step (iii) may, for example, be a method in which the product is dispersed in an aqueous medium in the presence of an organic solvent (L), a dispersant (e), a chain extender (H) and a reaction terminator (J) as necessary, and reacted [chain extension by water and (H), and optionally reaction termination by (J)] until isocyanate groups are substantially eliminated, and the organic solvent (L) used is distilled off as necessary.
[0087] The aqueous medium in the present invention means water and a mixture of water and the organic solvent (L). The organic solvent used in the aqueous medium is preferably a water-soluble organic solvent from the viewpoint of dispersibility. When the organic solvent (L) is used, it may be distilled off as necessary during and / or after the production of the anionic resin-coated pigment aqueous dispersion.
[0088] The dispersant (e) may be a nonionic surfactant, an anionic surfactant, a cationic surfactant, an amphoteric surfactant, or other emulsifying dispersant. (e) may be used alone or in combination of two or more kinds.
[0089] The type of device for adding water while stirring the slurry (S) and dispersing the anionic resin-coated pigment (P) is not particularly limited, and examples thereof include emulsifiers such as (1) anchor-type stirring type, (2) rotor-stator type [e.g., Homomixer (manufactured by AS ONE)], (3) line mill type [e.g., Line Flow Mixer], (4) stationary tube mixing type [e.g., static mixer], (5) vibration type [e.g., "VIBRO MIXER" (manufactured by Reika Kogyo Co., Ltd.)], (6) ultrasonic impact type [e.g., ultrasonic homogenizer], (7) high pressure impact type [e.g., Gaulin Homogenizer (manufactured by Gaulin Co., Ltd.)], (8) membrane emulsification type [e.g., membrane emulsification module], and (9) centrifugal thin film contact type [e.g., "Filmix" (manufactured by Primix Co., Ltd.)]. Among these, (2) is preferred.
[0090] 1.1.4.Water The anionic ink constituting the inkjet ink set according to this embodiment contains water as a main solvent. As the water, it is preferable to use pure water or ultrapure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, distilled water, etc. In particular, it is preferable to use water that has been sterilized by ultraviolet irradiation or addition of hydrogen peroxide, etc., in order to prevent the growth of mold and bacteria and enable long-term storage of the ink composition.
[0091] The water content is not particularly limited, but is preferably 30% by mass or more, more preferably 35% by mass or more, and particularly preferably 40% by mass or more, based on the total mass of the anionic ink.
[0092] 1.1.5.Other Ingredients The anionic ink constituting the inkjet ink set according to this embodiment may contain components other than those described above. Examples of such components are shown below.
[0093] <Wetting agent> The anionic inks constituting the inkjet ink set according to this embodiment preferably contain an organic solvent with a wetting effect, for the purpose of preventing clogging in the vicinity of the nozzles of the inkjet head.
[0094] Examples of the wetting agent include polyhydric alcohols such as glycerin, 1,2,6-hexanetriol, trimethylolpropane, pentamethylene glycol, trimethylene glycol, ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, polyethylene glycols having a number average molecular weight of 2000 or less, dipropylene glycol, tripropylene glycol, isobutylene glycol, 2-butene-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, mesoerythritol, and pentaerythritol, as well as glucose, mannose, fructooligosaccharides, and the like. Examples of suitable wetting agents include sugars such as tallow, ribose, xylose, arabinose, galactose, aldonic acid, glucitol (sorbitol), maltose, cellobiose, lactose, sucrose, trehalose, and maltotriose; so-called solid wetting agents such as sugar alcohols, hyaluronic acids, and ureas; alkyl alcohols having 1 to 4 carbon atoms such as ethanol, methanol, butanol, propanol, and isopropanol; and 2-pyrrolidone, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, formamide, acetamide, dimethyl sulfoxide, sorbitol, sorbitan, acetin, diacetin, triacetin, and sulfolane.
[0095] The wetting agent may be used alone or in combination of two or more kinds.
[0096] The content of the humectant is preferably from 2.0% to 20.0% by mass, more preferably from 5.0% to 15.0% by mass, based on the total mass of the anionic ink. If the content of the humectant is within this range, appropriate physical properties (such as viscosity) of the anionic ink can be ensured, and recording quality and reliability can be ensured.
[0097] <Surfactant> The anionic ink constituting the inkjet ink set according to this embodiment preferably contains a surfactant. The surfactant can be used as a wetting agent to reduce the surface tension of the anionic ink and adjust the wettability, i.e., the permeability, of the ink to the recording medium. Furthermore, the inclusion of a surfactant in the anionic ink ensures ejection stability from the inkjet head.
[0098] As the surfactant, any of nonionic surfactants, anionic surfactants, cationic surfactants, and amphoteric surfactants can be used, and these may be used in combination. Among the surfactants, acetylene glycol surfactants, silicone surfactants, and fluorine surfactants can be preferably used.
[0099] The acetylene glycol surfactant is not particularly limited, but examples thereof include Surfynol (registered trademark) 104, 104E, 104H, 104A, 104BC, 104DPM, 104PA, 104PG-50, 104S, 420, 440, 465, 485, SE, SE-F, 504, 61, DF37, CT111, CT121, CT131, CT136, TG, GA, and DF110D (all trade names, manufactured by Nissin Chemical Industry Co., Ltd.), Olfine (registered trademark) B, Y , P, A, STG, SPC, E1004, E1010, PD-001, PD-002W, PD-003, PD-004, PD-005, EXP.4001, EXP.4300, EXP.4036, EXP.4051, AF-103, AF-104, AK-02, SK-14, AE-3 (all trade names, manufactured by Nissin Chemical Industry Co., Ltd.), Acetylenol (registered trademark) E00, E00P, E40, E100 (all trade names, manufactured by Kawaken Fine Chemical Co., Ltd.).
[0100] The silicone surfactant is not particularly limited, but a polysiloxane compound is preferred. The polysiloxane compound is not particularly limited, but an example thereof is a polyether-modified organosiloxane. Examples of commercially available polyether-modified organosiloxanes include BYK (registered trademark)-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, BYK-348, and BYK-349 (all trade names, manufactured by BYK Co.), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, and KF-6017 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.).
[0101] As the fluorine-based surfactant, it is preferable to use a fluorine-modified polymer, and although there is no particular limitation, an example thereof is BYK (registered trademark)-340 (product name, manufactured by BYK Japan KK).
[0102] When the anionic ink contains a surfactant, multiple types of the above surfactants can be used, and the total content of the surfactants relative to the anionic ink is preferably 0.01% by mass or more and 3.0% by mass or less, more preferably 0.05% by mass or more and 2.0% by mass or less, even more preferably 0.1% by mass or more and 1.5% by mass or less, and particularly preferably 0.2% by mass or more and 1.0% by mass or less.
[0103] <Other> The anionic inks constituting the inkjet ink set according to this embodiment may contain, in addition to the above-mentioned components, preservatives, antifungal agents, rust inhibitors, chelating agents, viscosity adjusters, antioxidants, ureas, amines, sugars, etc.
[0104] 1.2.Cation Ink The cationic ink constituting the inkjet ink set according to this embodiment contains a cationic resin, a pigment, and water, the cationic ink is of a similar color to the anionic ink described above, the pigment in the cationic ink is coated with the cationic resin, and at least one of the cationic resin and the anionic resin contained in the anionic ink has a urethane-based skeleton or a polyester-based skeleton.
[0105] 1.2.1.Pigments The cationic ink constituting the inkjet ink set according to this embodiment contains a pigment. The pigment is the same as that in the anionic ink described above, and therefore description thereof is omitted.
[0106] 1.2.2.Cationic resin The cationic ink constituting the inkjet ink set according to this embodiment contains a cationic resin, and at least one of the cationic resin and the anionic resin described above has a urethane skeleton or a polyester skeleton. By adopting such an embodiment, it is possible to improve the abrasion fastness.
[0107] The cationic resin is not particularly limited as long as it exhibits cationic properties in the cationic ink, but for example, cationic resins having a urethane skeleton, cationic resins having a polyester skeleton, acrylic cationic resins, polyammonium salt cationic resins, olefin cationic resins, etc. can be used. These resins can be used alone or in combination of two or more. Among these resins, cationic resins having a urethane skeleton are preferred from the viewpoint of further improving the friction fastness.
[0108] 1.2.2.1.Cationic resin with urethane skeleton The cationic resin having a urethane skeleton is a polymer synthesized by reacting a polyisocyanate, a polyol, and a compound for imparting cationic properties.
[0109] The polyisocyanate is the same as that in the anionic ink described above, and so a description thereof is omitted.
[0110] The polyol is the same as that in the anionic ink described above, and so a description thereof is omitted.
[0111] Examples of compounds for imparting cationicity include various ammonium salts such as primary ammonium salts, secondary ammonium salts, tertiary ammonium salts, and quaternary ammonium salts. More specific examples include (mono)alkylamine salts, dialkylamine salts, trialkylamine salts, tetraalkylamine salts, benzalkonium salts, alkylpyridinium salts, and imidazolinium salts.
[0112] 1.2.2.2.Cationic resin with ester skeleton The cationic resin having an ester skeleton is a polymer obtained by polycondensation of a polyol and a cationic polymer.
[0113] Examples of polyols include ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, trimethylolpropane, pentaerythritol, etc. When synthesizing an anionic resin having a polyester skeleton, the above polyols may be used alone or in combination of two or more kinds.
[0114] Examples of the cationic polymer include polymers having primary to tertiary amines and quaternary ammonium salts in the molecule. Specific examples of the cationic polymer include polyalkylene polyamines such as polyethylene polyamine and polypropylene polyamine or derivatives thereof, acrylic resins having secondary amines, tertiary amines and quaternary ammonium salts, polyvinylamines, polyvinylamidines, dicyandiamide-formaldehyde polycondensates as typified by dicyandiamide-diethylenetriamine polycondensates, polyamine-based cationic resins as typified by dicyandiamide-diethylenetriamine polycondensates, epichlorohydrin-dimethylamine addition polymers, dimethyldiallylammonium chloride polymers, diallylamine salt polymers, dimethyldiallylammonium chloride polymers, allylamine salt polymers, dialkylaminoethyl (meth)acrylate quaternary salt polymers, acrylamide-diallylamine salt copolymers, and polyvinyl alcohol-cationic monomer graft polymers.
[0115] 1.2.2.3.Cationic resins with blocked isocyanate groups In addition, the cationic resin in the present embodiment may have a blocked isocyanate group from the viewpoint of further improving the friction fastness. The cationic resin having a blocked isocyanate group is preferably the cationic resin having a urethane skeleton described above that has a blocked isocyanate group. Such a cationic resin tends to have better friction fastness.
[0116] The polyisocyanate compound and blocking agent used for the blocked isocyanate group are the same as those in the anionic ink described above, and therefore description thereof is omitted.
[0117] 1.2.3.Cationic resin-coated pigment In the cationic inks constituting the inkjet ink set according to this embodiment, the above-mentioned pigment is coated with the above-mentioned cationic resin.
[0118] A preferred method for producing a pigment coated with a cationic resin (hereinafter also referred to as a "cationic resin-coated pigment") is similar to that for the anionic resin-coated pigment described above, and therefore the description thereof will be omitted.
[0119] The water and other components that may be contained in the cationic ink constituting the inkjet ink set according to this embodiment are similar to those in the anionic ink described above, and therefore description thereof will be omitted.
[0120] 1.3. Methods for preparing anionic and cationic inks In this embodiment, the anionic ink and cationic ink are obtained by mixing the above-mentioned components in any order and removing impurities by filtration or the like as necessary. As a method for mixing each component, a method in which materials are added sequentially to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed is preferably used. As a filtration method, centrifugal filtration, filter filtration, etc. can be performed as necessary.
[0121] 1.4. Physical properties of anionic and cationic inks In this embodiment, from the viewpoint of a balance between image quality and reliability as an ink for inkjet recording, the anionic ink and cationic ink preferably have a surface tension of 20 mN / m to 40 mN / m, and more preferably 20 mN / m to 35 mN / m, at 20° C. The surface tension can be measured, for example, by using an automatic surface tensiometer CBVP-Z (product name, manufactured by Kyowa Interface Science Co., Ltd.) to confirm the surface tension when a platinum plate is wetted with the ink in an environment of 20° C.
[0122] From the same viewpoint, in this embodiment, the viscosity of the anionic ink and cationic ink at 20° C. is preferably 3 mPa·s or more and 10 mPa·s or less, and more preferably 3 mPa·s or more and 8 mPa·s or less. The viscosity can be measured in an environment of 20° C. using, for example, a viscoelasticity tester MCR-300 (product name, manufactured by Pysica).
[0123] 2. Recording method A recording method according to one embodiment of the present invention is a recording method using the inkjet ink set of the above aspect, comprising an anionic ink application step of ejecting the anionic ink from an inkjet head and applying it to a recording medium, and a cationic ink application step of ejecting the cationic ink from the inkjet head and applying it to the recording medium, wherein the area on the recording medium to which the anionic ink is applied and the area on the recording medium to which the cationic ink is applied overlap in part or in whole.
[0124] According to the recording method of this embodiment, even if the recording medium is not pretreated with a cationic compound or the like for the purpose of improving color development, good color development of the printed material and excellent friction fastness (abrasion resistance) can be obtained. Therefore, by using the recording method of this embodiment, it is possible to eliminate the troublesome pretreatment process that must be performed mainly manually, and it is possible to in-line the recording method process. In addition, since the ink composition is aggregated by mixing the anionic ink and the cationic ink, good color development and reduced bleeding can be obtained regardless of whether the recording medium is pretreated, i.e., regardless of the surface charge state of the recording medium.
[0125] The recording method according to this embodiment will be described below in the order of an inkjet recording apparatus applicable to the recording method according to this embodiment, a recording medium, and each step of the recording method.
[0126] 2.1. Inkjet recording device
[0127] An example of an inkjet recording apparatus in which the recording method according to the present embodiment is carried out will be described with reference to the drawings. Fig. 1 is a schematic cross-sectional view showing an inkjet recording apparatus. As shown in Fig. 1, the inkjet recording apparatus 1 includes an inkjet head 2, an IR heater 3, a platen heater 4, a curing heater 5, a cooling fan 6, a pre-heater 7, and a ventilation fan 8. The inkjet recording apparatus 1 includes a control unit (not shown), and the operation of the entire inkjet recording apparatus 1 is controlled by the control unit.
[0128] The inkjet head 2 is a means for ejecting and depositing anionic ink and cationic ink (hereinafter, these are collectively referred to as "ink composition" or simply "ink") onto a recording medium M.
[0129] The inkjet head 2 includes a nozzle (not shown) for ejecting an ink composition. Methods for ejecting ink from a nozzle include, for example, a method in which a strong electric field is applied between the nozzle and an acceleration electrode placed in front of the nozzle, ink droplets are continuously ejected from the nozzle, and the ink droplets are ejected in response to a recording information signal while flying between deflection electrodes (electrostatic attraction method); a method in which pressure is applied to the ink with a small pump and the nozzle is mechanically vibrated with a quartz oscillator or the like to forcibly eject ink droplets; a method in which pressure and a recording information signal are simultaneously applied to the ink with a piezoelectric element to eject and record ink droplets (piezo method); and a method in which ink is heated and foamed with a microelectrode in accordance with a recording information signal to eject and record ink droplets (thermal jet method).
[0130] As the inkjet head 2, either a line type inkjet head or a serial type inkjet head can be used.
[0131] Here, an inkjet recording device equipped with a serial type inkjet head is one that performs recording by performing multiple scans (passes) to eject an ink composition while moving an inkjet head for recording relative to the recording medium. A specific example of a serial type inkjet head is one in which an inkjet head is mounted on a carriage that moves in the width direction of the recording medium, i.e., in a direction intersecting the transport direction of the recording medium, and the inkjet head moves with the movement of the carriage to eject droplets onto the recording medium.
[0132] On the other hand, an inkjet recording device equipped with a line type inkjet head performs recording by performing one scan (pass) to eject an ink composition while moving the recording inkjet head relative to the recording medium. A specific example of a line type inkjet head is one in which the inkjet head is formed wider than the width of the recording medium and ejects droplets onto the recording medium without moving the recording inkjet head.
[0133] In this embodiment, an inkjet recording apparatus equipped with a serial type inkjet head is used as the inkjet recording apparatus 1, and an inkjet head 2 using a piezo system for ejecting ink from the nozzles is used.
[0134] The inkjet recording apparatus 1 includes an IR heater 3 and a platen heater 4 for heating the recording medium M when the ink composition is ejected from the inkjet head 2, i.e., for primary heating or primary drying. In this embodiment, when the recording medium M is heated in the ink composition application step described below, at least one of the IR heater 3 and the platen heater 4 may be used.
[0135] Note that, when the IR heater 3 is used, the recording medium M can be heated from the inkjet head 2 side. As a result, the inkjet head 2 is also likely to be heated at the same time, but compared to heating the recording medium M from the back side thereof using the platen heater 4 or the like, the temperature can be increased without being affected by the thickness of the recording medium M. Also, when the platen heater 4 is used to heat the recording medium M, the recording medium M can be heated from the side opposite the inkjet head 2 side. As a result, the inkjet head 2 is relatively less likely to be heated.
[0136] The upper limit of the surface temperature of the recording medium M by the IR heater 3 and the platen heater 4 is preferably 45° C. or less, more preferably 40° C. or less, and even more preferably 35° C. or less. The lower limit of the surface temperature of the recording medium M is preferably 25° C. or more, more preferably 28° C. or more, and even more preferably 30° C. or more. This reduces or eliminates the radiant heat received from the IR heater 3 and the platen heater 4, thereby suppressing drying and composition fluctuation of the ink composition in the inkjet head 2 and suppressing adhesion of the ink or resin to the inner wall of the inkjet head 2. Furthermore, the ink can be fixed early, improving image quality.
[0137] The curing heater 5 is a heater for drying and solidifying the ink composition attached to the recording medium M, that is, for secondary heating or secondary drying. When the curing heater 5 heats the recording medium M on which an image has been recorded, the moisture contained in the ink composition evaporates and dissipates more quickly, and an ink film is formed by the resin contained in the ink composition. In this way, the ink film is firmly fixed or adhered to the recording medium M, and has excellent film-forming properties, so that an excellent high-quality image can be obtained in a short time. The upper limit of the surface temperature of the recording medium M by the curing heater 5 is preferably 120° C. or less, more preferably 100° C. or less, and even more preferably 90° C. or less. In addition, the lower limit of the surface temperature of the recording medium M is preferably 60° C. or more, more preferably 70° C. or more, and even more preferably 80° C. or more. By setting the temperature within the above range, a high-quality image can be obtained in a short time.
[0138] The inkjet recording apparatus 1 may have a cooling fan 6. After the ink composition recorded on the recording medium M is dried, the ink composition on the recording medium M is cooled by the cooling fan 6, whereby an ink coating film with good adhesion can be formed on the recording medium M.
[0139] The inkjet recording apparatus 1 may also include a preheater 7 that preheats the recording medium M before the ink composition is applied to the recording medium M. Furthermore, the recording apparatus 1 may also include a ventilation fan 8 so that the ink composition applied to the recording medium M can be dried more efficiently.
[0140] 2.2. Recording medium The recording method according to this embodiment can be used for recording on various recording media.
[0141] The recording medium is not particularly limited, and may be fabrics such as cotton, silk, polyester, polyurethane, nylon, and blends of the above-mentioned different fibers, which have high ink absorbency, as well as plain paper, inkjet paper, medium-absorbency high-quality paper, and copy paper, and may also be low-absorbency or non-absorbency recording media, although it is preferable to use fabrics.
[0142] The low-absorbency recording medium is not particularly limited, but may be, for example, coated paper having a coating layer formed on the surface by applying a paint, etc. The coated paper is not particularly limited, but may be, for example, printing paper such as art paper, coated paper, and matte paper.
[0143] The non-absorbing recording medium is not particularly limited, but examples thereof include a plastic film having no ink absorbing layer, a substrate such as paper coated with plastic, or a substrate with a plastic film adhered thereto, etc. Examples of plastics include polyvinyl chloride, polyethylene terephthalate, polycarbonate, polystyrene, polyurethane, polyethylene, polypropylene, etc.
[0144] In this specification, the term "a recording medium having low ink absorption or no ink absorption" refers to a recording medium that is capable of being held in contact with the ink for 30 msec in the Bristow method. 1 / 2 Water absorption up to 10mL / m 2 The following recording medium is used. The Bristow method is the most widely used method for measuring the amount of liquid absorbed in a short period of time, and is also used by the Japan Pulp and Paper Technical Association (JAPAN TAPPI). Details of the test method are described in Standard No. 51 "Paper and paperboard - Liquid absorbency test method - Bristow method" of the "JAPAN TAPPI Paper and Pulp Test Method 2000 Edition."
[0145] In the present embodiment, the fabric may be treated with a treatment liquid composition (hereinafter, simply referred to as a "treatment liquid"). The treatment liquid composition is applied in advance to the fabric that is the base material of the printed textile during inkjet textile printing, and contains, for example, a cationic compound and the above-mentioned water or organic solvent.
[0146] The cationic compound has a function of aggregating the components in the ink composition. Therefore, when the ink composition is applied to a fabric to which a treatment liquid has been applied, the cationic compound promotes the aggregation of the ink particles and increases the viscosity of the ink, suppressing absorption into the gaps or inside of the fibers that make up the fabric. In this way, the cationic compound holds the ink on the surface of the fabric, improving the color development of the ink on the printed material. In addition, bleeding and smearing are suppressed.
[0147] Examples of cationic compounds include polyvalent metal salts such as calcium salts and magnesium salts, cationic resins such as cationic urethane resins, olefin resins, and allylamine resins, cationic surfactants, inorganic acids, or organic acids. Among these, it is preferable to use polyvalent metal salts because they improve the color development of the pigment and are suitable for cotton fabrics. These cationic compounds may be used alone or in combination of two or more.
[0148] The content of the cationic compound contained in the treatment liquid is not particularly limited, but is preferably 0.1% by mass or more, more preferably 2.0% by mass or more, and even more preferably 5.0% by mass or more, based on the total amount of the treatment liquid. The content of the cationic compound contained in the treatment liquid is preferably 40.0% by mass or less, more preferably 25.0% by mass or less, and even more preferably 10.0% by mass or less, based on the total amount of the treatment liquid. By setting the content of the cationic compound within the above range, precipitation or separation of the cationic compound in the treatment liquid is suppressed, aggregation of the pigment in the ink is promoted, and absorption into the gaps or inside of the fibers constituting the fabric is suppressed. This reduces the phenomenon of the coloring material striking through to the back side of the printed surface, improving the color development of the printed material.
[0149] 2.3.Each process Each step of the recording method according to this embodiment will be described below using an example of recording using the inkjet recording apparatus and inkjet ink set described above.
[0150] 2.3.1. Anionic ink application process The anionic ink application step is a step of applying the above-mentioned anionic ink to the recording medium M by ejecting it from the inkjet head 2 in Fig. 1. The anionic ink is applied to the surface of the recording medium M by this step.
[0151] The maximum amount of anionic ink attached per unit area on the recording medium M is preferably 5 mg / inch 2 More preferably, 7 mg / inch 2 More preferably, it is 10 mg / inch or more. 2 The upper limit of the amount of the anionic ink attached per unit area of the recording medium is not particularly limited, but is, for example, 20 mg / inch 2 Less than or equal to 18 mg / inch is preferred. 2 It is particularly preferably 16 mg / inch or less. 2 The following is the result.
[0152] The anionic ink application step may include a heating step of heating the recording medium M with an IR heater 3 or a platen heater 4 before or simultaneously with the anionic ink application step, and is preferably performed on the recording medium M that has been heated in the heating step. This allows the ink to be dried quickly on the recording medium M, and bleeding is suppressed. Furthermore, it is possible to provide a recording method that can form images with excellent quality and generate a small amount of VOCs.
[0153] The upper limit of the surface temperature (primary heating temperature) of the recording medium M when the anionic ink is applied is preferably 45° C. or less, more preferably 40° C. or less, and even more preferably 38° C. or less. When the surface temperature of the recording medium when the anionic ink is applied is within the above range, the influence of heat on the inkjet head 2 can be suppressed, and clogging of the inkjet head 2 and the nozzles can be prevented. In addition, the lower limit of the surface temperature of the recording medium M during inkjet recording is preferably 25° C. or more, more preferably 28° C. or more, even more preferably 30° C. or more, and particularly preferably 32° C. or more. When the surface temperature of the recording medium M during inkjet recording is within the above range, the ink can be quickly dried on the recording medium M and fixed early, bleeding can be suppressed, and an image with excellent abrasion resistance and image quality can be formed.
[0154] 2.3.2.Cation ink application process The cationic ink applying step is a step of applying the above-mentioned cationic ink to the recording medium M so as to overlap in part or in whole with the area to which the anionic ink has been applied or will be applied in the anionic ink applying step. The cationic ink applying step may be performed after the anionic ink applying step, before the anionic ink applying step, or simultaneously with the anionic ink applying step.
[0155] Here, "area to which anionic ink has been applied or will be applied" refers to an area to which dots of anionic ink have been attached or will be applied.
[0156] In this specification, the term "region" refers to a portion occupying a certain area on a recording medium, where the amount of ink composition applied to the region is approximately constant. A region is a region that can be visually recognized as having the same color, for example, a region having an area of 1 mm 2Furthermore, the term "approximately constant amount of adhesion" means that, for example, when the duty is low, the amount of adhesion of the ink composition strictly differs between the position where the ink composition dot has landed and the position where the ink composition has not landed, but the region is a macroscopic (macro) range larger than the area of one dot, and macroscopically, the amount of adhesion of the ink composition is constant within the region, and unevenness in the amount of adhesion due to the presence or absence of adhesion of ink dots is ignored.
[0157] Furthermore, when the duty is low, even in a region where both anionic ink and cationic ink are attached, there may be some areas where the anionic ink and cationic ink do not overlap microscopically (for example, on the scale of droplets (landed dots) in the inkjet method), but these are considered to be overlaps of ink compositions seen macroscopically, and the presence of areas where dots do not overlap when viewed dot by dot is ignored. Therefore, the attachment region here is considered to be the region where the anionic ink and cationic ink overlap as a whole region.
[0158] In this specification, the term "Duty" refers to a value calculated by the following formula (1). Duty(%)={actual print dot count / (vertical resolution x horizontal resolution)} x 100 …(1) (In the formula, "actual print dot number" is the number of actual print dots per unit area, and "vertical resolution" and "horizontal resolution" are the resolutions per unit area, respectively.)
[0159] When the cationic ink is applied to the recording medium so as to overlap a part or all of the area to which the anionic ink is applied, the cationic ink may be applied so as to overlap at least a part of the area to which the anionic ink is applied. Specifically, the cationic ink is preferably applied so as to overlap 50% or more of the area to which the anionic ink is applied, more preferably to overlap 60% or more, and even more preferably to overlap 70% or more. By applying the cationic ink in this manner, the anionic ink and the cationic ink can be effectively mixed, and the color development and abrasion resistance tend to be good.
[0160] The maximum amount of the cationic ink attached per unit area on the recording medium M is preferably 5 mg / inch 2 More preferably, 7 mg / inch 2 More preferably, it is 10 mg / inch or more. 2 The upper limit of the amount of the ink composition applied per unit area of the recording medium is not particularly limited, but is, for example, 20 mg / inch 2 Less than or equal to 18 mg / inch is preferred. 2 It is particularly preferably 16 mg / inch or less. 2 The following is the result.
[0161] In addition, the cationic ink applying step may also include a heating step of heating the recording medium M with an IR heater 3 or a platen heater 4 before or simultaneously with the cationic ink applying step, similar to the anionic ink applying step described above, and is preferably performed on the recording medium M that has been heated in the heating step. This allows the ink on the recording medium M to dry quickly.
[0162] The upper limit of the surface temperature of the recording medium M when the cationic ink is applied is preferably 45° C. or less, more preferably 40° C. or less, and even more preferably 38° C. or less. When the surface temperature of the recording medium M when the ink is applied is within the above range, the effect of heat on the inkjet head 2 can be suppressed, and clogging of the inkjet head 2 and the nozzles can be prevented. Furthermore, the lower limit of the surface temperature of the recording medium M during inkjet recording is preferably 25° C. or more, more preferably 28° C. or more, even more preferably 30° C. or more, and particularly preferably 32° C. or more. When the surface temperature of the recording medium M is within the above range, the ink can be dried quickly on the recording medium M and fixed early.
[0163] 2.3.3. Other processes The recording method according to this embodiment may have a secondary heating step of heating the recording medium M to which the ink composition has been attached using a curing heater 5 shown in Fig. 1 after the anionic ink attachment step and cationic ink attachment step. This causes the fixing resin and the like contained in the ink composition on the recording medium M to melt and form an ink film, and the ink film is firmly fixed (adhered) onto the recording medium M, resulting in excellent film-forming properties, making it possible to obtain a high-quality image with excellent abrasion resistance in a short period of time.
[0164] The upper limit of the surface temperature of the recording medium M by the curing heater 5 is preferably 120° C. or less, more preferably 110° C. or less, and even more preferably 100° C. or less. The lower limit of the surface temperature of the recording medium M is preferably 60° C. or more, more preferably 70° C. or more, and even more preferably 80° C. or more. By keeping the temperature within the above range, a high-quality image can be obtained in a short time.
[0165] After the secondary heating step, a step of cooling the ink composition on the recording medium M by a cooling fan 6 shown in FIG.
[0166] Furthermore, the recording method according to this embodiment may also include a cleaning step in which the ink composition is discharged by a means other than the pressure generating means for ejecting ink for recording, that is, by a mechanism other than the mechanism for ejecting ink for recording that is provided in the inkjet head 2.
[0167] The mechanism for ejecting ink for recording provided in the inkjet head 2 includes a piezoelectric element or a heater element provided in a pressure chamber (not shown) for applying pressure to the ink. This cleaning step may be a step of applying pressure from the outside to the inkjet head 2 to eject the ink composition or the treatment liquid from the nozzle. By providing this step, even if there is a concern that the resin may melt onto the inner wall of the inkjet head 2, this can be suppressed, and ejection stability can be further improved.
[0168] The other mechanisms mentioned above include mechanisms that apply pressure, such as applying suction (negative pressure) or applying positive pressure from the upstream of the inkjet head. These are not ink discharge (flushing) by the function of the inkjet head itself. In other words, they are not discharged by using the function of ejecting ink from the inkjet head during recording.
[0169] 3. Working Example The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "%" and "parts" are based on mass unless otherwise specified.
[0170] 3.1. Preparation of Dispersion Anionic dispersions 1-17, cationic dispersions 1-17, and other dispersions 1-6 were prepared so as to obtain the blend amounts shown in Tables 1-3 below. The values shown for the pigment and dispersant are calculated as solid content. In Tables 1-3 below, "Y" stands for yellow, "M" for magenta, "C" for cyan, "K" for black, and "W" for white. In Tables 1-3 below, "PCD" stands for polycarbonate diol, "PES" for polyester diol, "PE" for polyether diol, and "BI" for containing a blocked isocyanate group.
[0171] [Table 1]
[0172] [Table 2]
[0173] [Table 3]
[0174] The detailed preparation method of each dispersion will be described below.
[0175] 3.1.1. Anionic dispersions <Anionic dispersion 1> In a simple pressurized reaction apparatus equipped with a stirrer and a heater, 57.8 parts of "UH-200" (manufactured by Ube Industries, product name) as polycarbonate diol, 10.5 parts of hexamethylene diisocyanate, 1.7 parts of 2,2-dimethylolpropionic acid, and 30 parts of methyl ethyl ketone were charged and stirred at 85 ° C for 10 hours to carry out a urethane reaction, producing a methyl ethyl ketone solution of polyurethane prepolymer. Next, 17.5 parts of CI Pigment Blue 15:3 (manufactured by Dainichi Seika Chemicals Co., Ltd., product name, hereinafter also referred to as "PB15:3") were added as a pigment, and 282 parts of zirconia beads "YTZ-01" (manufactured by Nikkato Corporation, product name) were added, and the mixture was disintegrated for 4 hours with a pigment disperser "Labostar Mini HFM02" (manufactured by Ashizawa Finetech Co., Ltd.) to obtain a pigment slurry.
[0176] 1.0 part of triethylamine was added as a neutralizing agent to 235 parts of the pigment slurry and homogenized, and then 38 parts of ion-exchanged water was added while stirring at 200 rpm to disperse the mixture. 5.2 parts of a 10% by weight aqueous solution of diethylenetriamine as a chain extender was added to the resulting dispersion, and methyl ethyl ketone was distilled off under reduced pressure at 65°C for 8 hours, and the zirconia beads were removed by filtration to obtain an anionic dispersion 1 coated with a polyurethane resin, with a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass as solids.
[0177] <Anionic dispersion 2> In the production of the anionic dispersion 1, except that 57.8 parts of the polycarbonate diol was replaced with 57.8 parts of polyester diol "Sun Estar 4620" (product name, manufactured by Sanyo Chemical Industries), a similar production method was used to obtain anionic dispersion 2 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0178] <Anionic dispersion 3> In the production of the anionic dispersion 1, except that 57.8 parts of the polycarbonate diol was replaced with 57.8 parts of polyether diol "PTMG2000" (product name, manufactured by Mitsubishi Chemical Corporation, poly(oxytetramethylene) glycol with Mn = 2,000), anionic dispersion 3 was obtained in the same manner as in the production of the anionic dispersion 1, with a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0179] <Anionic dispersion 4> In producing the above anionic dispersion 1, after neutralization, 5.2 parts of a 10% by weight aqueous solution of diethylenetriamine as a chain extender was added, 1.0 part of a polycarbonate-based urethane resin having a blocked isocyanate group was added, and the methyl ethyl ketone was distilled off under reduced pressure at 65°C for 8 hours. The zirconia beads were removed by filtration to obtain anionic dispersion 4 coated with polyurethane resin, having a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass as solids.
[0180] <Anionic dispersion 5> 20 parts by mass of an organic solvent (methyl ethyl ketone), 0.03 parts by mass of a polymerization chain transfer agent (2-mercaptoethanol), a polymerization initiator, 15 parts by mass of polypropylene glycol monomethacrylate (propylene oxide=9), 15 parts by mass of poly(ethylene glycol·propylene glycol) monomethacrylate (propylene oxide group=7, ethylene oxide group=5), 12 parts by mass of methacrylic acid, 50 parts by mass of styrene monomer, 10 parts by mass of styrene macromer, and 10 parts by mass of benzyl methacrylate were used and placed in a reaction vessel that had been thoroughly purged with nitrogen gas and polymerized at 75°C under stirring. 0.9 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile dissolved in 40 parts by mass of methyl ethyl ketone was added per 100 parts by mass of the monomer components, and the mixture was aged at 80°C for 1 hour to obtain a polymer solution.
[0181] 7.5 parts by mass of the water-insoluble polymer obtained above was dissolved in 45 parts by mass of methyl ethyl ketone, a predetermined amount of 20% aqueous sodium hydroxide solution (neutralizing agent) was added thereto to neutralize the salt-forming group, and 20 parts by mass of PB15:3 was further added as a pigment and kneaded with a bead mill for 2 hours. 120 parts by mass of ion-exchanged water was added to the kneaded product obtained in this way and stirred, and then methyl ethyl ketone was removed at 6°C under reduced pressure, and a part of the water was further removed to obtain an anionic dispersion 5 having a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass as solids.
[0182] <Anionic dispersion 6> After replacing the atmosphere in a reaction vessel equipped with a stirrer, a thermometer, a reflux tube, and a dropping funnel with nitrogen, 20 parts by mass of cyclohexyl acrylate, 5 parts by mass of 2-ethylhexyl acrylate, 15 parts by mass of butyl acrylate, 10 parts by mass of lauryl acrylate, 2 parts by mass of acrylic acid, and 0.3 parts by mass of t-dodecyl mercaptan were mixed. This mixture was heated at 70°C, and 150 parts by mass of benzyl acrylate, 15 parts by mass of acrylic acid, 50 parts by mass of butyl acrylate, 1 part by mass of t-dodecyl mercaptan, 20 parts by mass of methyl ethyl ketone, and 1 part by mass of azobisisovaleronitrile were added to the dropping funnel and dropped into the reaction vessel over a period of 4 hours to polymerize the dispersed polymer. Next, methyl ethyl ketone was added to the reaction vessel to prepare a dispersed polymer solution with a concentration of 40% by mass.
[0183] 40 parts by mass of the above dispersion polymer solution, 30 parts by mass of Pigment Blue 15:3 (copper phthalocyanine pigment, Clariant), 100 parts by mass of 0.1 mol / L sodium hydroxide aqueous solution, and 30 parts by mass of methyl ethyl ketone were mixed and stirred with a homogenizer for 30 minutes. Then, 300 parts by mass of ion-exchanged water were added and stirred for another hour. Then, the entire amount of methyl ethyl ketone and a part of the water were distilled off using a rotary evaporator, neutralized with 0.1 mol / L sodium hydroxide to adjust the pH to 9, filtered with a 0.3 μm membrane filter, and adjusted with ion-exchanged water to obtain an anionic dispersion 6 coated with polycarboxylic acid, with a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass.
[0184] <Anionic dispersion 7> In producing the above anionic dispersion 1, except that 17.5 parts of PB15:3 was replaced with 17.5 parts of CI Pigment Yellow 74 (trade name, manufactured by Dainichiseika Chemical Industry Co., Ltd., hereinafter also referred to as "PY74"), anionic dispersion 7 was obtained in the same manner as the above anionic dispersion 1, with a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0185] <Anionic dispersion 8> In producing the above anionic dispersion 1, except that 17.5 parts of PB15:3 was replaced with 17.5 parts of CI Pigment Red 122 (trade name, manufactured by Dainichiseika Chemical Industry Co., Ltd., hereinafter also referred to as "PR122"), anionic dispersion 8 was obtained in the same manner as for the above anionic dispersion 1, with a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0186] <Anionic dispersion 9> In the production of the above anionic dispersion 1, except that 17.5 parts of S170 (product name manufactured by Degussa), a commercially available carbon black, was used instead of 17.5 parts of PB15:3, a similar production method to the above anionic dispersion 1 was used to obtain anionic dispersion 9, which has a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0187] <Anionic Dispersion 10> In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 714 parts (2.00 mol parts) of 1,2-propylene glycol, 679 parts (0.87 mol parts) of terephthalic acid, 89 parts (0.13 mol parts) of adipic acid, and 5 parts of titanium diisopropoxy bistriethanolamine as a polymerization catalyst were placed, and reacted for 12 hours at 180°C under a nitrogen stream while distilling off the water generated. The temperature was then gradually raised to 230°C, and the reaction was continued for 4 hours under a nitrogen stream while removing the water generated, and the reaction was continued under a reduced pressure of 5 to 20 mmHg, and the reaction was cooled when the softening point reached 99°C. The amount of 1,2-propylene glycol recovered was 338 parts (0.95 mol parts). Then, the mixture was cooled to 180°C, 29 parts (0.03 mol parts) of trimellitic anhydride was added, and the mixture was reacted under normal pressure for 1 hour, followed by reaction at the same temperature for 1 hour while distilling off water under reduced pressure of 5 to 20 mmHg. 70 parts of the synthesis material was taken out, 30 parts of methyl ethyl ketone was added, and then 17.5 parts of CI Pigment Blue 15:3 (manufactured by Dainichi Seika Chemicals Co., Ltd., trade name, hereinafter also referred to as "PB15:3") was added as a pigment, and 282 parts of zirconia beads "YTZ-01" (manufactured by Nikkato Co., Ltd., trade name) were added, followed by disintegration for 4 hours with a pigment disperser "Labostar Mini HFM02" (manufactured by Ashizawa Finetech Co., Ltd.) to obtain a pigment slurry.
[0188] 1.0 part of triethylamine was added as a neutralizing agent to 235 parts of the pigment slurry and homogenized, and then 38 parts of ion-exchanged water was added while stirring at 200 rpm to disperse the mixture. Methyl ethyl ketone was distilled off under reduced pressure at 65°C for 8 hours, and the zirconia beads were removed by filtration to obtain an anionic dispersion 10 coated with a polyurethane resin, with a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% as solids.
[0189] <Anionic Dispersion 11> In the production of the anionic dispersion 1, 57.8 parts of polycarbonate diol, 10.5 parts of hexamethylene diisocyanate, and 1.7 parts of 2,2-dimethylolpropionic acid were replaced with 19.3 parts of polycarbonate diol, 3.5 parts of hexamethylene diisocyanate, and 0.57 parts of 2,2-dimethylolpropionic acid, respectively. An anionic dispersion 11 having a pigment concentration of 10% by mass and a dispersant concentration of 5% by mass, as solid contents, was obtained in the same manner as the anionic dispersion 1.
[0190] <Anionic Dispersion 12> In the production of the anionic dispersion 1, 57.8 parts of polycarbonate diol, 10.5 parts of hexamethylene diisocyanate, and 1.7 parts of 2,2-dimethylolpropionic acid were replaced with 77.1 parts of polycarbonate diol, 14 parts of hexamethylene diisocyanate, and 2.3 parts of 2,2-dimethylolpropionic acid, respectively. An anionic dispersion 12 having a pigment concentration of 10% by mass and a dispersant concentration of 20% by mass as solids was obtained in the same manner as in the production of the anionic dispersion 1.
[0191] <Anionic Dispersion 13> In producing the above anionic dispersion 10, except that 17.5 parts of PY74 was used instead of 17.5 parts of PB15:3, a similar production method was used to obtain anionic dispersion 13 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0192] <Anionic Dispersion 14> In producing the above anionic dispersion 10, except that 17.5 parts of PR122 was used instead of 17.5 parts of PB15:3, a similar production method was used to obtain anionic dispersion 14 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0193] <Anionic Dispersion 15> In producing the above anionic dispersion 10, except that 17.5 parts of PB15:3 was replaced with 17.5 parts of S170 (a product name manufactured by Degussa), a commercially available carbon black, a similar production method to that for the above anionic dispersion 10 was used to obtain anionic dispersion 15 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0194] <Anionic Dispersion 16> In producing the above anionic dispersion 1, except that 17.5 parts of PB15:3 was replaced with 17.5 parts of titanium oxide "R62N" (manufactured by Sakai Chemical Industry Co., Ltd.), a similar production method was used to obtain anionic dispersion 16, which has a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0195] <Anionic Dispersion 17> In producing the above anionic dispersion 10, except that 17.5 parts of PB15:3 was replaced with 17.5 parts of titanium oxide "R62N" (manufactured by Sakai Chemical Industry Co., Ltd.), a similar production method was used to obtain anionic dispersion 17, which has a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solids.
[0196] 3.1.2. Cationic dispersions <Cationic dispersion 1> Cationic dispersion 1 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass%, as solid contents, was obtained in the same manner as in the production of anionic dispersion 1, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0197] <Cationic dispersion 2> Cationic dispersion 2 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass%, as solid contents, was obtained in the same manner as in the production of anionic dispersion 2, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0198] <Cationic dispersion 3> Cationic dispersion 3 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass%, in terms of solid content, was obtained in the same manner as in the production of anionic dispersion 3, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0199] <Cationic dispersion liquid 4> Cationic dispersion 4 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass%, as solid contents, was obtained in the same manner as in the production of anionic dispersion 4, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0200] <Cationic dispersion liquid 5> In the production of the anionic dispersion liquid 5, 12 parts by mass of methacrylic acid was replaced with 12 parts by mass of 4-vinylpyridine as a monomer having a cationic group, and 1.0 part of triethylamine was replaced with 1.0 part of dimethyl sulfate. In the same manner as in the production of the anionic dispersion liquid 5, a cationic dispersion liquid 5 having a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass, in terms of solid content, was obtained.
[0201] <Cationic dispersion 6> In the production of the anionic dispersion liquid 6, 2 parts by mass of the first acrylic acid was replaced with 2 parts by mass of 4-vinylpyridine as a monomer having a cationic group, and 15 parts by mass of the second acrylic acid was replaced with 15 parts by mass of 4-vinylpyridine as a monomer having a cationic group, and 1.0 part of triethylamine was replaced with 1.0 part of dimethyl sulfate. In a similar manner to the production of the anionic dispersion liquid 6, cationic dispersion liquid 6 was obtained, having a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass, as solid contents.
[0202] <Cationic dispersion 7> Cationic dispersion 7 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass%, as solid contents, was obtained in the same manner as in the production of anionic dispersion 7, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0203] <Cationic dispersion 8> Cationic dispersion 8 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content was obtained in the same manner as in the production of anionic dispersion 8, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0204] <Cationic dispersion 9> Cationic dispersion 9 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass%, as solid contents, was obtained in the same manner as in the production of anionic dispersion 9, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was used as 1.0 part of dimethyl sulfate.
[0205] <Cationic dispersion liquid 10> In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 1120 parts (2.00 mol parts) of N-methyldiethanolamine, 679 parts (0.87 mol parts) of terephthalic acid, 89 parts (0.13 mol parts) of adipic acid, and 5 parts of titanium diisopropoxy bistriethanolamine as a polymerization catalyst were placed, and reacted for 12 hours at 180°C under a nitrogen stream while distilling off the water generated. The temperature was then gradually raised to 230°C, and the reaction was carried out for 4 hours under a nitrogen stream while removing the water generated, and the reaction was further carried out under a reduced pressure of 5 to 20 mmHg, and cooled when the softening point reached 99°C. The amount of N-methyldiethanolamine recovered was 532 parts (0.95 mol parts). Thereafter, the reaction was carried out for 1 hour at the same temperature while distilling off the water under a reduced pressure of 5 to 20 mmHg. 70 parts of the synthetic material were taken out, and 30 parts of methyl ethyl ketone were added. Next, 17.5 parts of CI Pigment Blue 15:3 (trade name, manufactured by Dainichi Seika Chemical Industry Co., Ltd., hereinafter also referred to as "PB15:3") were added as a pigment, and 282 parts of zirconia beads "YTZ-01" (trade name, manufactured by Nikkato Corporation) were added. After that, the mixture was disintegrated for 4 hours using a pigment disperser "Labostar Mini HFM02" (manufactured by Ashizawa Finetech Co., Ltd.) to obtain a pigment slurry.
[0206] 1.0 part of dimethyl sulfate as a neutralizer was added to 235 parts of the pigment slurry and homogenized, and then 38 parts of ion-exchanged water was added while stirring at 200 rpm to disperse the mixture. Methyl ethyl ketone was distilled off under reduced pressure at 65°C for 8 hours, and the zirconia beads were removed by filtration to obtain cationic dispersion 10 coated with a polyurethane resin, with a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% as solids.
[0207] <Cationic Dispersion 11> In the production of the anionic dispersion 11, 0.57 parts of 2,2-dimethylolpropionic acid was replaced with 0.57 parts of N-methyldiethanolamine as a monomer having a cationic group, and 1.0 part of triethylamine was replaced with 1.0 part of dimethyl sulfate. In the same manner as in the production of the anionic dispersion 11, a cationic dispersion 11 was obtained having a pigment concentration of 10 mass% and a dispersant concentration of 5 mass%, as solid contents.
[0208] <Cationic dispersion 12> In producing the anionic dispersion 12, 2.3 parts of 2,2-dimethylolpropionic acid were replaced with 2.3 parts of N-methyldiethanolamine as a monomer having a cationic group, and 1.0 part of triethylamine was replaced with 1.0 part of dimethyl sulfate. In the same manner as in producing the anionic dispersion 12, a cationic dispersion 12 was obtained having a pigment concentration of 10% by mass and a dispersant concentration of 20% by mass as solids.
[0209] <Cationic dispersion 13> In producing the above cationic dispersion 10, except for changing 17.5 parts of PB15:3 to 17.5 parts of CI Pigment Yellow 74 (trade name, manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., hereinafter also referred to as "PY74"), a cationic dispersion 13 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content was obtained in the same manner as for the above cationic dispersion 10.
[0210] <Cationic dispersion 14> In producing the above cationic dispersion 10, except for changing 17.5 parts of PB15:3 to 17.5 parts of CI Pigment Red 122 (trade name, manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., hereinafter also referred to as "PR122"), a cationic dispersion 14 was obtained in the same manner as for the above cationic dispersion 10, having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solid content.
[0211] <Cationic dispersion 15> Cationic dispersion 15 was obtained in the same manner as cationic dispersion 10, except that 17.5 parts of S170 (product name manufactured by Degussa) which is a commercially available carbon black was used instead of 17.5 parts of PB15:3. The solid content of cationic dispersion 15 was 10% by mass of pigment and 15% by mass of dispersant.
[0212] <Cationic dispersion 16> Cationic dispersion 16 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% in terms of solids was obtained in the same manner as in the production of anionic dispersion 16, except that in place of 1.7 parts of 2,2-dimethylolpropionic acid, 1.7 parts of N-methyldiethanolamine was used as the monomer having a cationic group, and 1.0 part of triethylamine was changed to 1.0 part of dimethyl sulfate.
[0213] <Cationic dispersion liquid 17> Cationic dispersion 17 was obtained in the same manner as cationic dispersion 10, except that 17.5 parts of PB15:3 was replaced with 17.5 parts of titanium oxide "R62N" (manufactured by Sakai Chemical Industry Co., Ltd.). The solid content of the pigment concentration was 10% by mass and the dispersant concentration was 15% by mass.
[0214] 3.1.3. Other (non-ionic) dispersions <Other dispersion liquid 1> Other dispersion 1 was obtained in the same manner as anionic dispersion 1 above, except that Newpol PE108 (manufactured by Sanyo Chemical Industries, Ltd.) was used as a dispersant instead of the urethane prepolymer. The solid content of the pigment concentration was 10 mass % and the dispersant concentration was 15 mass %.
[0215] <Other dispersion liquid 2> Other dispersion 2 having a pigment concentration of 10 mass% and a dispersant concentration of 15 mass% as solid contents was obtained in the same manner as in the production of anionic dispersion 1, except that 1.7 parts of 2,2-dimethylolpropionic acid was replaced with 1.7 parts of 2,2-dimethylolpropionic acid PEG ester in the production of anionic dispersion 1. Note that "2,2-dimethylolpropionic acid PEG ester" refers to an ester compound of 2,2-dimethylolpropionic acid and polyethylene glycol.
[0216] <Other dispersions 3> In the production of the anionic dispersion 5, except that 12 parts by mass of methacrylic acid was replaced with 12 parts by mass of polyethylene glycol methacrylate, a similar production method was used to obtain another dispersion 3 having a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass, as solid contents.
[0217] <Other dispersion liquid 4> Other dispersion 4 was obtained in the same manner as in the production of other dispersion 1, except that 17.5 parts of PY74 was used instead of 17.5 parts of PB15:3. The other dispersion 4 had a pigment concentration of 10% by mass and a dispersant concentration of 15% by mass, as solid contents.
[0218] <Other dispersions 5> Other dispersion 5 was obtained in the same manner as other dispersion 1, except that in the production of other dispersion 1, 17.5 parts of PR122 was used instead of 17.5 parts of PB15:3. The solid content of other dispersion 5 was 10% by mass of pigment and 15% by mass of dispersant.
[0219] <Other dispersions 6> Other Dispersion Liquid 6 was obtained in the same manner as Other Dispersion Liquid 1, except that 17.5 parts of S170 (product name manufactured by Degussa) which is a commercially available carbon black was used instead of 17.5 parts of PB15:3. The pigment concentration was 10% by mass and the dispersant concentration was 15% by mass, in terms of solid content.
[0220] 3.2. Preparation of inks and ink sets Using each dispersion obtained above, each component was mixed in the amounts shown in Tables 4 to 6 below, stirred at room temperature for 2 hours, and then filtered using a membrane filter with a pore size of 5 μm to obtain each ink composition shown in Tables 4 to 6 below. Furthermore, each ink composition prepared in the same manner as above and shown in Table 7 below was combined as shown in Table 7 below to prepare an ink set. Note that with regard to the ink colors in Tables 4 to 7 below, "Y" stands for yellow, "M" for magenta, "C" for cyan, "K" for black, and "W" for white, respectively.
[0221] [Table 4]
[0222] [Table 5]
[0223] [Table 6]
[0224] [Table 7]
[0225] Details of the surfactants in Tables 4 to 7 are as follows. BYK348 (product name, manufactured by BYK Japan Co., Ltd., silicone surfactant)
[0226] Furthermore, "fabric without pretreatment" refers to fabric that has not been treated with a cationic compound, "fabric with pretreatment" refers to fabric that has been treated with a water-soluble cationic polymer, which is a cationic compound described below, and "non-absorbent media" refers to a non-absorbent recording medium as defined in this specification.
[0227] 3.3. Recording method As the recording medium, white cotton broadcloth was used for the "fabric without pretreatment". For the "fabric with pretreatment", a pretreatment agent consisting of 6.7 parts of "Unisense 104L" (trade name, manufactured by Senka Co., Ltd.) as a water-soluble cationic polymer and 93.3 parts of water was padded on white cotton broadcloth at a squeezing rate of 70% by padding method, and then dried at 120°C for 5 minutes and returned to 25°C. For the "non-absorbent media", a plastic film (manufactured by Futamura Chemical Co., Ltd., trade name "FOR-BT") was used. Next, as an inkjet recording device, a printer manufactured by Seiko Epson Corporation (trade name "SC-F2000") was prepared which was modified so that each of the ink compositions or each of the ink sets obtained above could be printed in the combinations described in Tables 4 to 7 above (modified machine of trade name "SC-F2000").
[0228] 3.4. Evaluation method 3.4.1. Evaluation of physical property stability The temperature of each ink composition or ink set obtained above was adjusted to 25°C, and the static viscosity was measured at a shear rate of 200 (1 / s) using a viscoelasticity tester "MCR-300" manufactured by Pysica. After sealing in a screw cap bottle, the mixture was left at a high temperature of 70°C for 10 days, and then left at 25°C, and the static viscosity was measured in the same manner. The physical property stability was evaluated based on the rate of change in viscosity before and after leaving the mixture, according to the following criteria. (Evaluation Criteria) S: (rate of change)≦3% AA: 3%<(rate of change)≦5% A: 5%<(rate of change)≦7.5% B: 7.5%<(rate of change)≦10% C: 10%<(rate of change)≦15% D 15%<(rate of change)
[0229] 3.4.2. Evaluation of color development The cartridge of the modified inkjet recording device was filled with each of the ink compositions or ink sets obtained above so that printing could be performed in the combinations shown in Tables 4 to 7. Next, each ink composition was applied to one side of each of the recording media at a coating density of 39 mg / inch 2The resulting print was dried by heating at 160°C for 5 minutes using an Economax D conveyor drying oven manufactured by M&R, and then cooled to 25°C to obtain a printed item. The resulting printed item was evaluated according to the following criteria based on the OD (optical density) value measured using a Spectrolino colorimeter (Gretag). (Evaluation Criteria) S:OD value is 1.5 or more AA:OD value is less than 1.5 and more than 1.4 A:OD value is less than 1.4 and more than 1.3 B:OD value is less than 1.3 and 1.2 or more C:OD value is less than 1.2 and 1.0 or more D:OD value is less than 1.0
[0230] In addition, ΔE was evaluated as an index of color difference. Specifically, the hue (L*α, a*α, b*α) of the area α where the anionic ink was applied and the hue (L*β, a*β, b*β) of the area β where the cationic ink was applied were measured using a colorimeter "Spectrolino" (Gretag), and ΔE (Delta E) was calculated and evaluated according to the following criteria. The following formula (1) was used to calculate ΔE. △E=((L*α-L*β) 2 +(a*α-a*β) 2 +(b*α-b*β) 2 ) 1 / 2 ... (1) (Evaluation Criteria) ○: ΔE≦1 ×:ΔE>1
[0231] 3.4.3. Evaluation of abrasion resistance <Fabrics with and without pretreatment> The cartridge of the modified inkjet recording device was filled with each of the ink compositions or ink sets obtained above so that printing could be performed in the combinations shown in Tables 4 to 7. Next, each ink composition was applied to one side of the pretreated fabric or the non-pretreated fabric at a coating density of 39 mg / inch 2Thereafter, the mixture was subjected to a heat drying treatment at 160° C. for 5 minutes using a conveyor drying oven “Economax D” manufactured by M&R, and then returned to 25° C. to obtain a printed product.
[0232] The resulting printed fabric was thoroughly dried and subjected to a rub fastness test in which the fabric was rubbed 100 times with a load of 200 g using a Gakushin rub fastness tester "AB-301S" manufactured by Tester Sangyo Co., Ltd. The level of dryness was judged according to the following criteria in accordance with the Japanese Industrial Standards (JIS) L0849, which checks the degree of ink peeling. (Evaluation Criteria) S: 4-5 grade AA: Level 4 A: 3.5-4 grade B: 3.5 grade C: 2.5-3.5 grade D: 2.5 grade or lower <Non-absorbent media> The abrasion resistance of the pretreated and non-pretreated fabrics was evaluated using the same procedures and evaluation criteria, except that the heat drying treatment at 100°C for 10 minutes was changed from 160°C for 5 minutes.
[0233] 3.5.Evaluation Results The results of the evaluation tests are shown in Tables 4 to 7 above.
[0234] From the above evaluation results, in Examples 1 to 33, by mixing an anionic ink containing a pigment coated with an anionic resin and a cationic ink containing a pigment coated with a cationic resin, the ink composition was aggregated regardless of whether the recording medium was pretreated, and good color development was obtained. In addition, by having at least one of the anionic resin and the cationic resin have a urethane skeleton or a polyester skeleton, it was possible to obtain good friction fastness (abrasion resistance).
[0235] In contrast, in Comparative Examples 1 to 11, in which the anionic ink and the cationic ink were not mixed, excellent color development could not be obtained regardless of whether the recording medium was pretreated or not. In other words, the aggregation of the ink composition depends on the surface state of the recording medium, and if the ink composition and the recording medium are not compatible, excellent color development could not be obtained. In addition, in Comparative Examples 12 and 13, in which at least one of the anionic resin and the cationic resin does not have a urethane skeleton or a polyester skeleton, the friction fastness (abrasion resistance) was poor, and in Comparative Examples 14 and 15, in which the inks were not of the same color, the color difference was large and the color development was poor.
[0236] The following can be derived from the above-described embodiment.
[0237] One embodiment of the inkjet ink set comprises: 1. An inkjet ink set comprising: an anionic ink containing an anionic resin, a pigment, and water; A cationic ink containing a cationic resin, a pigment, and water, the anionic ink and the cationic ink are similar in color to each other, the pigment in the anionic ink is coated with the anionic resin; the pigment in the cationic ink is coated with the cationic resin, At least one of the anionic resin and the cationic resin has a urethane skeleton or a polyester skeleton.
[0238] In the above-mentioned embodiment of the inkjet ink set, The anionic resin and the cationic resin may each have a urethane skeleton.
[0239] In the above-mentioned embodiment of the inkjet ink set, The urethane skeleton may contain one or more selected from polycarbonate, polyether, and polyester.
[0240] In the above-mentioned embodiment of the inkjet ink set, The anionic resin and the cationic resin may each have a blocked isocyanate group.
[0241] One aspect of the recording method is A recording method using the inkjet ink set of the above aspect, an anionic ink depositing step of ejecting the anionic ink from an inkjet head and depositing the anionic ink on a recording medium; a cationic ink applying step of ejecting the cationic ink from the inkjet head and applying the cationic ink to the recording medium, The area on the recording medium to which the anionic ink has been applied and the area on the recording medium to which the cationic ink has been applied overlap in part or in whole.
[0242] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the present invention includes a configuration that is substantially the same as the configuration described in the embodiment, for example, a configuration that has the same function, method, and result, or a configuration that has the same purpose and effect. The present invention also includes a configuration in which non-essential parts of the configuration described in the embodiment are replaced. The present invention also includes a configuration that has the same action and effect as the configuration described in the embodiment, or a configuration that can achieve the same purpose. The present invention also includes a configuration in which publicly known technology is added to the configuration described in the embodiment. [Explanation of symbols]
[0243] Reference Signs List 1: Inkjet recording device, 2: Inkjet head, 3: IR heater, 4: Platen heater, 5: Curing heater, 6: Cooling fan, 7: Pre-heater, 8: Ventilation fan, M: Recording medium
Claims
1. 1. An inkjet ink set comprising: an anionic ink containing an anionic resin, a pigment, and water; A cationic ink containing a cationic resin, a pigment, and water, the anionic ink and the cationic ink are similar in color to each other, the pigment in the anionic ink is coated with the anionic resin; the pigment in the cationic ink is coated with the cationic resin, At least one of the anionic resin and the cationic resin is urethane. having a styrene-based or polyester-based skeleton, The anionic resin and the cationic resin each have a blocked isocyanate group. , inkjet ink set.
2. The anionic resin and the cationic resin have the urethane skeleton. Item 2. The inkjet ink set according to item 1.
3. The urethane skeleton is selected from polycarbonate, polyether, and polyester. The ink-jet ink set according to claim 1 or 2, comprising one or more of the following: to.
4. The ink-jet ink set according to any one of claims 1 to 3 is used. A recording method comprising the steps of: The anionic ink is ejected from an inkjet head and deposited on a recording medium. an anionic ink deposition step; The cationic ink is discharged from the inkjet head and applied to the recording medium. and a cationic ink attaching step of attaching the cationic ink to the ink. The area on the recording medium to which the anionic ink is applied and the area on which the cationic ink is applied are A recording method in which the area on the recording medium to which the ink is applied overlaps in part or in whole. 。
Citation Information
Patent Citations
Ink jet cartridge set and ink jet print system
JP1999342635A
Printing liquid set and ink-jet ink set
JP1999343440A
Ink set, recording therewith, and recording apparatus provided with such ink set
JP2000007964A
Ink jet recording method and ink jet recording ink set utilizing the same
JP2002347338A
Ink set
JP2004285348A