Ink and image forming method
The ink composition with specific organic solvents and polyoxyethylene ether compounds addresses discharge stability and scratch resistance issues on non-absorbent substrates, ensuring stable and durable image formation.
Patent Information
- Application Number
- JP2020204077
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Inkjet recording systems face challenges in achieving both discharge stability and scratch resistance, particularly when forming images on poorly absorbent substrates like coated paper or polymer films, with conventional techniques failing to adequately address both issues.
An ink composition comprising multiple organic solvents, including 1,2-propanediol and 1,2-hexanediol, combined with a polyoxyethylene ether compound, such as polyethylene glycol trimethyl nonyl ether, and optionally urethane and acrylic resins, to enhance ejection stability and scratch resistance.
The ink formulation effectively prevents beading on poorly absorbent substrates while maintaining continuous ejection stability and providing scratch resistance, ensuring high-quality image formation.
Smart Images

Figure 0007585750000003 
Figure 0007585750000004 
Figure 0007585750000005
Abstract
Description
[Technical field]
[0001] The present invention relates to inks and imaging methods. [Background technology]
[0002] Compared with other recording methods, the inkjet recording method has a simple process, is easy to achieve full color, and can obtain high-resolution images even with an apparatus having a simple configuration. Therefore, the inkjet recording method is spreading from personal use to office use, commercial printing, and industrial printing fields. In the field of commercial printing, in addition to plain paper, coated papers such as coated paper and art paper, and even polymer films for soft packaging such as PET and (OPP) polypropylene are used as recording media, and printed matter is handled as products such as postcards and packages. It is known that when an image is formed using a water-based ink on a poorly absorbent substrate such as coated paper or a polymer film, so-called beading is likely to occur.
[0003] Patent Document 1 listed below discloses an ink composition that contains at least a non-aqueous solvent such as a 1,2-alkanediol, which has a surface tension of 30 mN / m or less when dissolved in water to form a 10 wt % aqueous solution, and 0.1 wt % or more of an organic amine. Furthermore, Patent Document 2 listed below discloses an ink containing a plurality of pigments, a plurality of water-soluble resins, a surfactant, and a water-soluble organic solvent, in which the surfactant is a polyoxyethylene alkyl ether having an HLB value of 13.0 or more according to the Griffin method. Furthermore, the following Patent Document 3 proposes a technology for setting the viscoelasticity of ink at a concentrated state within a specific range, with the aim of providing an ink that can suppress beading without causing a decrease in image density or deterioration in ink ejection properties. Summary of the Invention [Problem to be solved by the invention]
[0004] In general, in order to reduce printing downtime and achieve high productivity, ejection stability is required in inkjet recording methods. In addition, ink is required to be scratch-resistant, but ink with scratch resistance is prone to adhesion to the recording head, which tends to result in poor ejection stability. For these reasons, achieving both ejection stability and scratch resistance is considered difficult in the industry. However, in the conventional techniques disclosed in the above Patent Documents 1 to 3, there is still room for improvement in terms of achieving both ejection stability and abrasion resistance.
[0005] Therefore, an object of the present invention is to provide an ink which is less likely to cause beading even when an image is formed on a poorly absorbent substrate such as coated paper or a polymer film, and which can achieve both continuous ejection stability and abrasion resistance. [Means for solving the problem]
[0006] The above problem is solved by the following configuration 1). 1) An ink containing a plurality of organic solvents, a pigment, and water, the organic solvents include 1,2-propanediol and 1,2-hexanediol; The ink further contains a polyoxyethylene ether compound. fruit, The polyoxyethylene ether compound is polyethylene glycol trimethylnonyl ether. ink. Effect of the Invention
[0007] According to the present invention, it is possible to provide an ink that is less likely to cause beading even when an image is formed on a poorly absorbent substrate such as coated paper or a polymer film, and that can achieve both continuous ejection stability and abrasion resistance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a perspective view illustrating an example of an inkjet recording apparatus. [Diagram 2]FIG. 2 is a perspective view illustrating an example of a main tank in the inkjet recording apparatus. [Diagram 3] 1A to 1C are diagrams illustrating a recording apparatus and a recording method that can be suitably applied to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described in further detail. The ink of the present invention contains a plurality of organic solvents, a pigment, and water, the plurality of organic solvents containing 1,2-propanediol and 1,2-hexanediol, and the ink further contains a polyoxyethylene ether compound.
[0010] By using a combination of these organic solvents and a polyoxyethylene ether compound, no beading occurs even when an image is formed on a poorly absorbent substrate such as coated paper or a polymer film, and high continuous ejection stability and abrasion resistance are obtained. 1,2-Hexanediol has a relatively low water retention capacity and easily volatilizes the water in the ink. Therefore, it quickly dries the water from ink droplets that land on a poorly absorbent substrate, and has the effect of preventing uneven distribution and aggregation of the pigment contained in the ink. At the same time, 1,2-Hexanediol itself has a high boiling point and is difficult to volatilize, so it also has the effect of preventing the flow, uneven distribution, and aggregation of the pigment. On the other hand, 1,2-propanediol has a relatively high water retention capacity, which helps prevent water from evaporating from the ink near the inkjet nozzle and causing the ink to dry out inside the nozzle, which can lead to abnormal ink ejection or nozzle clogging. The content of 1,2-hexanediol in the entire ink is preferably 5% by mass to 20% by mass, and more preferably 7% by mass to 13% by mass, which provides a further suppression effect on beading and makes it difficult for abnormal ejection to occur. The content of 1,2-propanediol in the ink is preferably 5% to 30% by mass, and more preferably 7% to 25% by mass, in order to achieve a further suppression of beading and to prevent ejection abnormalities.
[0011] In addition, by using the polyoxyethylene ether compound in combination with the above-mentioned organic solvents, it is possible to achieve both suppression of beading and suppression of ejection abnormalities at a higher level. It is considered that this is because the solubility of the polyoxyethylene ether compound in the ink is sufficiently high, so that the polyoxyethylene ether compound is present on the outermost surface of the ink droplet at the moment it lands on the poorly absorbent substrate, and the spreading of the droplet can be promoted. In addition, it is considered that the polyoxyethylene ether compound is also present on the ink surface near the nozzle, which facilitates the formation of the ink meniscus, thereby improving the ejection stability. The content of the polyoxyethylene ether compound in the ink is preferably 0.05% to 2.0% by mass, and more preferably 0.5% to 1.5% by mass, in order to achieve a further suppression of beading and to prevent ejection abnormalities.
[0012] Polyoxyethylene ether compounds have the general formula RO(C2H4O) n In the general formula, R is an alkyl group, the preferred number of carbon atoms being 10 to 18. Furthermore, n is the number of repetitions, for example, 2 to 10. Among them, the polyoxyethylene ether compound in the present invention can be polyethylene glycol trimethylnonyl ether (Cas. No. 60828-78-6, (also known as poly(oxyethylene)=3,5-dimethyl-1-(2-methylpropyl)hexyl=ether)). By using this compound, the effect of the present invention is particularly enhanced. Commercially available polyethylene glycol trimethylnonyl ethers include Triton HW-1000 manufactured by Dow Chemical Japan, and Tergitol TMN6, TMN10, and TMN-3 manufactured by Sigma-Aldrich.
[0013] From the viewpoint of improving scratch resistance, it is preferable for the ink of the present invention to contain a urethane resin and / or an acrylic resin. These resins form a film on the recording medium, adhere to it, and fix the pigment in the ink. Although it depends on the application, it is generally preferable to use a urethane resin to improve abrasion resistance. However, urethane resins may have poor drying properties, and using them in combination with acrylic resins makes it easier to handle the ink and to improve adaptability to the type of recording medium. The urethane resin and / or acrylic resin is preferably in the form of resin particles, and more preferably in the form of a resin emulsion. Water-soluble resins tend to increase the viscosity of the ink and change its properties relative to temperature, but if they are in an emulsion state, it is easier to suppress changes in properties.
[0014] The resin can be obtained by mixing the resin particles in a resin emulsion state in which the resin particles are dispersed in water as a dispersion medium with materials such as a pigment and an organic solvent to obtain an ink. The resin particles to be used may be appropriately synthesized or may be a commercially available product.
[0015] As the urethane resin, polycarbonate urethane resin is preferable from the viewpoint of high abrasion resistance and fixing property. Examples of the polycarbonate urethane resin include Takelac WS-4000, W-6010, and W-6110 manufactured by Mitsui Chemicals, Inc. and U-coat series manufactured by Daiichi Kogyo Seiyaku Co., Ltd.
[0016] Examples of the acrylic resin include acrylic resin, vinyl acetate resin, styrene-butadiene resin, vinyl chloride resin, acrylic-styrene resin, butadiene resin, styrene resin, etc. These resins are preferably polymers having both hydrophilic and hydrophobic portions.
[0017] Examples of commercially available resin emulsions include Microgel E-1002, E-5002 (styrene-acrylic resin emulsions, manufactured by Nippon Paint Co., Ltd.), Boncoat 400, Boncoat 4001 (acrylic resin emulsions, manufactured by DIC Corporation), Boncoat 5454 (styrene-acrylic resin emulsion, manufactured by DIC Corporation), SAE-1014 (styrene-acrylic resin emulsion, manufactured by Zeon Corporation), and Saibinol SK-200 (acrylic resin emulsion, manufactured by Saiden Chemical Industry Co., Ltd.).
[0018] The volume average particle size of the resin particles is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining good fixing property and high image hardness, however, it is preferably from 10 nm to 1,000 nm, more preferably from 10 nm to 200 nm, and particularly preferably from 10 nm to 100 nm.
[0019] The content of the resin is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of high abrasion resistance and fixability, the content of the resin is preferably from 1% by mass to 30% by mass, and more preferably from 5% by mass to 20% by mass, based on the total amount of the ink.
[0020] In addition to the above-mentioned constituent materials, the ink of the present invention may also contain the following materials.
[0021] <Organic solvent> The organic solvent used in the present invention is not particularly limited, and any water-soluble organic solvent can be used. Examples of the organic solvent include polyhydric alcohols, ethers such as polyhydric alcohol alkyl ethers and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds. Specific examples of the water-soluble organic solvent include ethylene glycol, diethylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 2,4-pentanediol, and 1,5-pentanediol. polyhydric alcohols such as 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol; ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, and diethylene glycol mono Examples of the alkyl ether include polyhydric alcohol alkyl ethers such as methyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether; nitrogen-containing heterocyclic compounds such as 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone; amides such as formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide; amines such as monoethanolamine, diethanolamine, and triethylamine; sulfur-containing compounds such as dimethyl sulfoxide, sulfolane, and thiodiethanol; propylene carbonate; and ethylene carbonate. It is preferable to use an organic solvent having a boiling point of 250° C. or less, since this not only functions as a wetting agent but also provides good drying properties. The content of the organic solvent in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, the content is preferably from 10% by mass to 60% by mass, and more preferably from 20% by mass to 60% by mass.
[0022] The water content in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of the drying property and ejection reliability of the ink, however, it is preferably from 10% to 90% by mass, and more preferably from 20% to 60% by mass.
[0023] The pigment may be an inorganic pigment or an organic pigment. These may be used alone or in combination of two or more. Mixed crystals may also be used. Examples of pigments that can be used include black pigments, yellow pigments, magenta pigments, cyan pigments, white pigments, green pigments, orange pigments, glossy pigments such as gold and silver pigments, and metallic pigments. As inorganic pigments, titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, as well as carbon black produced by known methods such as the contact method, furnace method, and thermal method can be used. As organic pigments, azo pigments, polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), dye chelates (e.g., basic dye chelates, acid dye chelates, etc.), nitro pigments, nitroso pigments, aniline black, etc. can be used. Among these pigments, those having good affinity with the solvent are preferably used. In addition, resin hollow particles and inorganic hollow particles can also be used. Specific examples of pigments for black colors include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black; metals such as copper, iron (CI Pigment Black 11), and titanium oxide; and organic pigments such as aniline black (CI Pigment Black 1). In addition, for color, CI Pigment Yellow 1, 3, 12, 13, 14, 17, 24, 34, 35, 37, 42 (yellow iron oxide), 53, 55, 74, 81, 83, 95, 97, 98, 100, 101, 104, 108, 109, 110, 117, 120, 138, 150, 153, 155, 180, 185, 213, CI Pigment Yellow Range 5, 13, 16, 17, 36, 43, 51, CI Pigment Red 1, 2, 3, 5, 17, 22, 23, 31, 38, 48:2, 48:2 (Permanent Red 2B (Ca)), 48:3, 48:4, 49:1, 52:2, 53:1, 57:1 (Brilliant Carmine 6B), 60:1, 63:1, 63:2, 64:1, 81, 83, 88 , 101 (red oxide), 104, 105, 106, 108 (cadmium red), 112, 114, 122 (quinacridone magenta), 123, 146, 149, 166, 168, 170, 172, 177, 178, 179, 184, 185, 190, 193, 202, 207, 208, 209, 213, 219, 224, 254, 264, CI Pigment Violet 1 (Rhodamine Lake), 3, 5:1, 16, 19, 23, 38; CI Pigment Blue 1, 2, 15 (Phthalocyanine Blue), 15:1, 15:2, 15:3, 15:4 (Phthalocyanine Blue), 16, 17:1, 56, 60, 63; CI Pigment Green 1, 4, 7, 8, 10, 17, 18, 36, etc. If necessary, a dye may be added. The dye is not particularly limited, and acid dyes, direct dyes, reactive dyes, and basic dyes can be used. One type of dye may be used alone, or two or more types may be used in combination. Examples of the dyes include CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 173, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Directed Black 19, 38, 51, 71, 154, 168, 171, 195, and CI Reactive Red. 14, 32, 55, 79, 249, and CI Reactive Black 3, 4, and 35.
[0024] The content of the coloring material in the ink is preferably from 0.1% to 15% by mass, and more preferably from 1% to 10% by mass, from the viewpoints of improving image density, good fixing property and ejection stability.
[0025] Methods for dispersing a pigment to obtain an ink include a method of introducing a hydrophilic functional group into the pigment to make it a self-dispersing pigment, a method of dispersing the pigment by coating the surface of the pigment with a resin, and a method of dispersing the pigment using a dispersant. As a method for introducing a hydrophilic functional group into a pigment to make it a self-dispersing pigment, for example, a method in which a functional group such as a sulfone group or a carboxyl group is added to a pigment (e.g., carbon) to make it dispersible in water can be mentioned. As a method for dispersing a pigment by coating its surface with a resin, there is a method in which the pigment is encapsulated in a microcapsule to make it dispersible in water. This can be called a resin-coated pigment. In this case, it is not necessary for all of the pigments blended in the ink to be coated with a resin, and uncoated or partially coated pigments may be dispersed in the ink as long as the effect of the present invention is not impaired. Examples of the method for dispersing using a dispersant include a method for dispersing using a known low molecular weight dispersant or a polymeric dispersant, typified by a surfactant. As the dispersant, for example, anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. can be used depending on the pigment. RT-100 (nonionic surfactant) manufactured by Takemoto Oil Co., Ltd. and sodium naphthalenesulfonate formalin condensate can also be suitably used as dispersants. The dispersants may be used alone or in combination of two or more.
[0026] <Pigment dispersion> It is possible to obtain ink by mixing a pigment with materials such as water or an organic solvent, or it is also possible to manufacture ink by mixing a pigment with other materials such as water and a dispersant to prepare a pigment dispersion, and then mixing the resulting mixture with materials such as water or an organic solvent. The pigment dispersion is obtained by mixing and dispersing water, a pigment, a pigment dispersant, and other components as required, and adjusting the particle size. Dispersion is preferably performed using a dispersing machine. The particle size of the pigment in the pigment dispersion is not particularly limited, but the maximum frequency in terms of the maximum number is preferably 20 nm or more and 500 nm or less, more preferably 20 nm or more and 150 nm or less, in order to improve the dispersion stability of the pigment and the image quality such as ejection stability and image density. The particle size of the pigment can be measured using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac Bell Co., Ltd.). The content of the pigment in the pigment dispersion is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of obtaining good ejection stability and increasing image density, the content is preferably 0.1% by mass or more and 50% by mass or less, and more preferably 0.1% by mass or more and 30% by mass or less. It is preferable that the pigment dispersion is degassed, if necessary, by filtering coarse particles using a filter, a centrifugal separator, or the like.
[0027] The volume average particle size of the resin particles is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of obtaining good fixing property and high image hardness, however, it is preferably from 10 nm to 1,000 nm, more preferably from 10 nm to 200 nm, and particularly preferably from 10 nm to 100 nm. The volume average particle size can be measured, for example, using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac-Bell Co., Ltd.).
[0028] The resin content is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of fixation property and storage stability of the ink, however, the resin content is preferably from 1% by mass to 30% by mass, and more preferably from 5% by mass to 20% by mass, of the total amount of the ink.
[0029] The particle size of the solid content in the ink is not particularly limited and can be appropriately selected depending on the purpose, but in terms of improving image quality such as ejection stability and image density, the maximum frequency in terms of maximum number is preferably 20 nm or more and 1000 nm or less, more preferably 20 nm or more and 150 nm or less. The solid content includes resin particles, pigment particles, etc. The particle size can be measured using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac Bell Co., Ltd.).
[0030] <Additives> If necessary, surfactants, antifoaming agents, antiseptics, antifungals, rust inhibitors, pH adjusters, etc. may be added to the ink.
[0031] In the present invention, a surfactant may be used in combination, if necessary. <Surfactant> As the surfactant, any of silicone-based surfactants, fluorine-based surfactants, amphoteric surfactants, nonionic surfactants, and anionic surfactants can be used. Silicone surfactants are not particularly limited and can be appropriately selected according to purpose.Among them, those that do not decompose even at high pH are preferred, such as side chain modified polydimethylsiloxane, both end modified polydimethylsiloxane, one end modified polydimethylsiloxane, side chain both end modified polydimethylsiloxane, etc., and those having polyoxyethylene group or polyoxyethylene polyoxypropylene group as modified group are particularly preferred because they show good properties as aqueous surfactants.In addition, polyether modified silicone surfactants can also be used as the silicone surfactant, such as a compound in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylsiloxane. As the fluorosurfactant, for example, perfluoroalkyl sulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain are particularly preferred because they have low foaming properties. As the perfluoroalkyl sulfonic acid compounds, for example, perfluoroalkyl sulfonic acid, perfluoroalkyl sulfonate, etc. are included. As the perfluoroalkyl carboxylic acid compounds, for example, perfluoroalkyl carboxylic acid, perfluoroalkyl carboxylate, etc. are included. As the polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain, for example, sulfate ester salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups on the side chains, salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups on the side chains, etc. are included. As counter ions of the salts in these fluorosurfactants, Li, Na, K, NH4, NH3CH2CH2OH, NH2(CH2CH2OH)2, NH(CH2CH2OH)3, etc. are included. Examples of amphoteric surfactants include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine. Examples of nonionic surfactants include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and ethylene oxide adducts of acetylene alcohol. Examples of the anionic surfactant include polyoxyethylene alkyl ether acetates, dodecylbenzene sulfonates, laurates, and salts of polyoxyethylene alkyl ether sulfates. These may be used alone or in combination of two or more.
[0032] The silicone surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the silicone surfactant include side-chain modified polydimethylsiloxane, both-end modified polydimethylsiloxane, one-end modified polydimethylsiloxane, and both-end side-chain modified polydimethylsiloxane. Polyether-modified silicone surfactants having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modifying group are particularly preferred because they exhibit good properties as an aqueous surfactant. Such surfactants may be appropriately synthesized or commercially available products, such as those available from BYK-Chemie Co., Ltd., Shin-Etsu Chemical Co., Ltd., Dow Corning Toray Silicone Co., Ltd., Nippon Emulsion Co., Ltd., and Kyoeisha Chemical Co., Ltd. As the polyether-modified silicone surfactant, commercially available products can be used, such as KF-618, KF-642, KF-643 (Shin-Etsu Chemical Co., Ltd.), EMALEX-SS-5602, SS-1906EX (Nihon Emulsion Co., Ltd.), FZ-2105, FZ-2118, FZ-2154, FZ-2161, FZ-2162, FZ-2163, FZ-2164 (Dow Corning Toray Silicone Co., Ltd.), BYK-33, BYK-387 (BYK-Chemie Co., Ltd.), TSF4440, TSF4452, TSF4453 (Toshiba Silicon Co., Ltd.), and the like.
[0033] The fluorine-based surfactant is preferably a compound having 2 to 16 fluorine-substituted carbon atoms, and more preferably a compound having 4 to 16 fluorine-substituted carbon atoms. As the fluorine-based surfactant, commercially available products may be used. Examples of such commercially available products include Surflon S-111, S-112, S-113, S-121, S-131, S-132, S-141, and S-145 (all manufactured by Asahi Glass Co., Ltd.); Fullard FC-93, FC-95, FC-98, FC-129, FC-135, FC-170C, FC-430, and FC-431 (all manufactured by Sumitomo 3M Limited); Megafa F-470, F-1405, F-474 (all manufactured by Dainippon Ink & Chemicals, Inc.); Zonyl TBS, FSP, FSA, FSN-100, FSN, FSO-100, FSO, FS-300, UR, Capstone FS-30, FS-31, FS-3100, FS-34, FS-35 (all manufactured by Chemours); FT-110, FT- 250, FT-251, FT-400S, FT-150, FT-400SW (all manufactured by NEOS Co., Ltd.), Polyfox PF-136A, PF-156A, PF-151N, PF-154, PF-159 (manufactured by OMNOVA Co., Ltd.), Unidyne DSN-403N (manufactured by Daikin Industries, Ltd.), and the like. Among these, FS-3100, FS-34, FS-300 manufactured by Chemours Co., Ltd., FT-110, FT-250, FT-251, FT-400S, FT-150, FT-400SW manufactured by NEOS Co., Ltd., Polyfox PF-151N manufactured by OMNOVA Co., Ltd., and Unidyne DSN-403N manufactured by Daikin Industries, Ltd. are particularly preferred from the viewpoint of excellent print quality, particularly color development, penetration into paper, wettability, and uniform dyeing.
[0034] <Antifoaming agent> The defoaming agent is not particularly limited, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, and fatty acid ester-based defoaming agents. These may be used alone or in combination of two or more. Among these, silicone-based defoaming agents are preferred because of their excellent foam breaking effect.
[0035] <Preservative and fungicide> The antiseptic and antifungal agent is not particularly limited, and examples thereof include 1,2-benzisothiazolin-3-one.
[0036] <Rust inhibitor> There are no particular restrictions on the rust inhibitor, and examples thereof include acid sulfite and sodium thiosulfate.
[0037] <pH adjuster> There are no particular restrictions on the pH adjuster as long as it can adjust the pH to 7 or higher, and examples thereof include amines such as diethanolamine and triethanolamine.
[0038] There are no particular restrictions on the physical properties of the ink, and it can be appropriately selected according to the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are within the following ranges. The viscosity of the ink at 25°C is preferably 5 mPa·s or more and 30 mPa·s or less, more preferably 5 mPa·s or more and 25 mPa·s or less, from the viewpoints of improving the printing density and the quality of characters and obtaining good ejection properties. Here, for example, a rotational viscometer (RE-80L manufactured by Toki Sangyo Co., Ltd.) can be used to measure the viscosity. The measurement conditions are as follows: at 25°C, with a standard cone rotor (1°34’×R24), a sample liquid volume of 1.2 mL, a rotation speed of 50 rpm, and it can be measured in 3 minutes. The surface tension of the ink is preferably 35 mN / m or less, more preferably 32 mN / m or less at 25°C, from the viewpoints of the ink being preferably leveled on the recording medium and shortening the drying time of the ink. The pH of the ink is preferably 7 to 12, more preferably 8 to 11, from the viewpoint of preventing corrosion of the metal members in contact with the liquid.
[0039] The image forming method of the present invention is a method of forming an image using ink by an inkjet method on a recording medium, and is a method of forming an image using the ink of the present invention as the ink after applying a treatment liquid containing at least a flocculant on the recording medium.
[0040] <Treatment liquid> The treatment liquid contains a flocculant, an organic solvent, and water, and may contain a surfactant, an antifoaming agent, a pH adjuster, an antiseptic and antifungal agent, a rust inhibitor, etc. as necessary. The organic solvent, surfactant, defoamer, pH adjuster, antiseptic / fungal agent, and rust inhibitor may be the same as those used in ink, and other materials used in known treatment liquids may be used. The type of the flocculant is not particularly limited, and examples thereof include water-soluble cationic polymers, acids, and polyvalent metal salts.
[0041] The flocculant is contained in the treatment liquid in an amount of, for example, 10 to 30% by mass.
[0042] <Post-processing solution> The post-treatment liquid is not particularly limited as long as it can form a transparent layer. The post-treatment liquid is obtained by selecting and mixing organic solvents, water, resins, surfactants, defoamers, pH adjusters, antiseptics, antifungals, rust inhibitors, etc. as necessary. The post-treatment liquid may be applied to the entire recording area formed on the recording medium, or may be applied only to the area where the ink image is formed.
[0043] <Treatment liquid application step and treatment liquid application means> The treatment liquid application step is a step of applying the treatment liquid of the present invention onto the recording medium, and is carried out by a treatment liquid application device. When applying the treatment liquid, if the substrate is a non-permeable substrate such as polyethylene terephthalate (PET), the substrate surface may be subjected to corona treatment using a conductive roller or plasma. Corona treatment generally improves the hydrophilicity of organic materials and improves the wettability and coating uniformity of aqueous liquids. The method of applying the treatment liquid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include an inkjet method, a blade coating method, a gravure coating method, a gravure offset coating method, a bar coating method, a roll coating method, a spray coating method, a knife coating method, an air knife coating method, a comma coating method, a U comma coating method, an AKKU coating method, a smoothing coating method, a microgravure coating method, a reverse roll coating method, a four-roll coating method, a five-roll coating method, a dip coating method, a curtain coating method, a slide coating method, a die coating method, etc. Among these, the roll coating method and the spray coating method are preferred.
[0044] The recording medium to which the treatment liquid has been applied may be subjected to a heating step of heating the recording medium to dry the treatment liquid, if necessary, but the heating step may not be performed. The heating step is a step of heating the printed material by a known heating means such as a roll heater, a drum heater, or hot air, to dry the treatment liquid applied to the printed material.
[0045] <Ink application process and ink application means> The ink application step is a step of applying the ink of the present invention, and is carried out by an ink application means. In the present invention, for example, an inkjet method can be used.
[0046] <Recording device and recording method> The ink of the present invention can be suitably used in various recording devices using the ink jet recording method, such as printers, facsimile machines, copying machines, printer / fax / copier combination machines, and three-dimensional modeling devices. In the present invention, the recording apparatus and recording method refer to an apparatus capable of ejecting ink, various treatment liquids, etc. onto a recording medium, and a method of recording using the apparatus. The recording medium refers to an object onto which ink or various treatment liquids can be attached even temporarily. This recording device can include not only a head portion that ejects ink, but also means related to feeding, transporting, and discharging the recording medium, as well as other devices called pre-processing devices and post-processing devices. The recording apparatus and the recording method may have a heating means used in the heating step and a drying means used in the drying step. The heating means and the drying means include, for example, a means for heating and drying the printed surface and the back surface of the recording medium. The heating means and the drying means are not particularly limited, but for example, a hot air heater and an infrared heater can be used. Heating and drying can be performed before, during, or after printing. In addition, the recording device and recording method are not limited to those that visualize meaningful images such as characters and figures with ink. For example, those that form patterns such as geometric designs and those that create three-dimensional images are also included. Furthermore, unless otherwise specified, the recording apparatus includes both a serial type apparatus in which the ejection head moves and a line type apparatus in which the ejection head does not move. Furthermore, this recording device includes not only desktop types, but also wide-width recording devices capable of printing on A0-sized recording media, and continuous-feed printers that can use continuous paper wound into a roll as a recording medium. An example of a recording device will be described with reference to Figs. 1 and 2. Fig. 1 is a perspective view of the device. Fig. 2 is a perspective view of a main tank. An image forming device 400 as an example of a recording device is a serial type image forming device. A mechanism unit 420 is provided inside an exterior 401 of the image forming device 400. Each ink storage unit 411 of the main tanks 410 (410k, 410c, 410m, 410y) for each color of black (K), cyan (C), magenta (M), and yellow (Y) is formed of a packaging material such as an aluminum laminate film. The ink storage unit 411 is stored in a storage container case 414 made of plastic, for example. As a result, the main tanks 410 are used as ink cartridges of each color. On the other hand, a cartridge holder 404 is provided at the back side of the opening when the cover 401c of the apparatus body is opened. A main tank 410 is detachably attached to the cartridge holder 404. As a result, each ink outlet 413 of the main tank 410 communicates with an ejection head 434 for each color via a supply tube 436 for each color, and ink can be ejected from the ejection head 434 to a recording medium.
[0047] This recording apparatus can include not only a portion that ejects ink, but also devices called pre-processing devices and post-processing devices. As an embodiment of the pre-treatment device and post-treatment device, a liquid storage section having a pre-treatment liquid and a liquid ejection head, similar to the case of inks such as black (K), cyan (C), magenta (M), and yellow (Y), and the like, are added, and the pre-treatment liquid and the post-treatment liquid are ejected by an inkjet recording method. As another embodiment of the pre-treatment device and the post-treatment device, there is an embodiment in which a pre-treatment device and a post-treatment device using a method other than the inkjet recording method, for example, a blade coating method, a roll coating method, or a spray coating method, are provided.
[0048] FIG. 3 is a diagram for explaining a recording apparatus and a recording method that can be suitably applied to the present invention. The recording apparatus shown in FIG. 3 includes a treatment liquid application device 2 that applies a treatment liquid, an ink ejection head 3 that ejects black ink (K), cyan ink (C), magenta ink (M), and yellow ink (Y), and a drying device 5. and a conveyor belt 6 for conveying a printing medium (recording medium) 1. The recording method includes a treatment liquid application step of applying a treatment liquid to the substrate 1, an ink application step of applying ink to the substrate 1 using an ink ejection head 3 to form a printed portion 7, and a drying step of drying the substrate 1 after the ink has been applied. The recording apparatus and the recording method may have a heating means used in the heating step and a drying means used in the drying step. The heating means and the drying means include, for example, a means for heating and drying the printed surface or the back surface of the printed material. The heating means and the drying means are not particularly limited, but for example, a hot air heater or an infrared heater can be used. Heating and drying can be performed before, during, or after printing. In addition, the recording device and recording method are not limited to those that visualize meaningful images such as characters and figures with ink. For example, those that form patterns such as geometric designs and those that create three-dimensional images are also included. Furthermore, unless otherwise specified, the recording apparatus includes both a serial type apparatus in which the ejection head moves and a line type apparatus in which the ejection head does not move. Furthermore, this recording device includes not only desktop types, but also wide-width recording devices that can print on A0-sized substrates, and continuous-feed printers that can use continuous paper wound into a roll as the substrate.
[0049] Examples of the poorly absorbent substrate include a polypropylene film, a polyethylene terephthalate film, and a nylon film. Examples of the polypropylene film include P-2002, P-2161, and P-4166 manufactured by Toyobo Co., Ltd., PA-20, PA-30, and PA-20W manufactured by Suntox Co., Ltd., and FOA, FOS, and FOR manufactured by Futamura Chemical Co., Ltd. Examples of the polyethylene terephthalate film include E-5100 and E-5102 manufactured by Toyobo Co., Ltd., P60 and P375 manufactured by Toray Industries, and G2, G2P2, K and SL manufactured by Teijin DuPont Films. Examples of the nylon film include Harden Film N-1100, N-1102, and N-1200 manufactured by Toyobo Co., Ltd., and ON, NX, MS, and NK manufactured by Unitika Co., Ltd. Other examples include coated paper, such as OK-TOP Coat made by Oji Paper Co., Ltd. and colored liner for corrugated paper. EXAMPLES
[0050] Examples of the present invention will be described below, but the present invention is not limited to these examples. Unless otherwise specified, the preparation and evaluation of the examples and comparative examples were carried out under conditions of 25°C and a relative humidity of 60%. In addition, "parts" means parts by mass.
[0051] (Pigment Dispersion Preparation Example 1) <Preparation of Dispersant-Dispersed Black Pigment Dispersion> A mixture of 100 g of carbon black (Black Pearls 1000) manufactured by Cabot Corporation, 15 g of sodium naphthalenesulfonate formalin condensate (Paionin A-45-PN, manufactured by Takemoto Oil Co., Ltd.), and 280 g of ion-exchanged water was premixed and then dispersed in a Dyno Mill (manufactured by Shinmaru Enterprises Corporation) using zirconia beads with a diameter of 0.3 mm at a rotation speed of 10 m / sec and a liquid temperature of 10°C for 30 minutes to obtain a pigment dispersion. Next, the obtained pigment dispersion and zirconia beads were separated and filtered through a membrane filter (cellulose acetate type) with an average pore size of 0.8 μm. Thereafter, the water content was adjusted so that the solid content concentration was 20 mass %, and a dispersant-dispersed black pigment dispersion was obtained.
[0052] Ink was prepared according to the recipe (mass %) shown in the following Table 1. The ink was prepared by putting the raw materials into a 1 L beaker, thoroughly stirring, and then filtering through a filter.
[0053] [Table 1]
[0054] Ink materials: The polyoxyethylene ether compound used was Triton HW-1000 (polyethylene glycol trimethyl nonyl ether) manufactured by Dow Chemical Japan. Other surfactants used were Surfynol 440 (acetylene glycol surfactant) manufactured by Nissin Chemical Industry Co., Ltd. and BYK-345 (polysiloxane surfactant) manufactured by BYK. The urethane resin particles used were Takelac WS-6021 (solid content 30.0% by mass, manufactured by Mitsui Chemicals, Inc.) or Superflex 460S (solid content 38% by mass, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.). The acrylic resin particles used were Boncoat 400 (solid content 38.0% by mass, manufactured by DIC Corporation) or Tocryl W463 (solid content 45% by mass, manufactured by Toyochem Co., Ltd.). The values for the pigment dispersion and resin particles in Table 1 correspond to the solid content.
[0055] The treatment solution was obtained by the following procedure. 70 parts of pure water and 20 parts of 1,2-propanediol were placed in a beaker, and 10 parts of magnesium sulfate (manufactured by Naikai Salt Industry Co., Ltd., product name: magnesium sulfate) was gradually added while stirring. After the entire solution was dissolved, the mixture was stirred for a further 30 minutes and then filtered to obtain a treated liquid.
[0056] Evaluation method The obtained ink was filled into a printing device shown in FIG. 3, and the black ink was ejected onto a recording medium to print five solid images of 3 cm square, followed by thorough drying in an air oven at 70°C.
[0057] The following recording media were used: Plain paper My Paper (manufactured by Ricoh Co., Ltd.) Glossy paper OK-TOP manufactured by Oji Paper Co., Ltd. PET Lumirror T60 (thickness 25μm) manufactured by Toray Industries, Inc.
[0058] The treatment liquid was applied at a rate of 10 g / mm on the recording medium shown in Table 2 below. 2 After the treatment liquid was applied by roller and dried, ink was discharged onto the area where the treatment liquid had been applied using the printing device shown in FIG. 3 under the above-mentioned conditions. The obtained solid image was visually observed and evaluated for beading based on the following evaluation criteria, with a score of 3 or higher being a practically usable level. [Evaluation Criteria] 5: No beading observed 4: Some beading is observed, but this does not affect practical use. 3: Beading is observed, but does not affect practical use. 2: Beading is clearly observed, causing problems in practical use. 1: Severe beading is observed, causing problems in practical use.
[0059] Next, the solid image was rubbed 50 times or more with a dry cotton cloth (Kanakin No. 3) with a weight of 400 g. The solid image after rubbing was visually observed and the rub resistance was evaluated based on the following evaluation criteria. A rating of 4 or higher is a practically usable level. [Evaluation Criteria] 5: No scratches observed even after 50 or more rubs 4: After rubbing 50 times, some scratches are observed, but this does not affect the image brightness and is not a problem for practical use. 3: After 50 rubs, scratches are observed, image brightness decreases slightly, and problems occur in practical use. 2: If rubbed 20 to 50 times, scratches are observed, image brightness decreases, and problems occur in practical use. 1: Scratches are observed when rubbed less than 20 times, and image brightness decreases, causing problems in practical use.
[0060] Using an inkjet printer (IPSiO GXe5500 manufactured by Ricoh Co., Ltd.), 100 sheets of A4-sized full-page solid images were continuously printed in glossy paper clean mode, and the printed images were visually observed to judge the "ejection stability" based on the following evaluation criteria. [Evaluation Criteria] A: The image does not change until 100 sheets are taken. B: Lines and unevenness appear in the image between 50 and 100 sheets. C: Streaks and unevenness appear in the image before 50 sheets are printed. A and B are levels suitable for practical use.
[0061] The evaluation results are shown in Table 2.
[0062] [Table 2]
[0063] From the results of the Examples and Comparative Examples, it is apparent that the present invention provides an ink and an image forming method that are excellent in beading, abrasion resistance, and ejection stability. [Explanation of symbols]
[0064] 1 Printing material 2 Processing liquid application device 3 Ink ejection head 5 Drying equipment 6 Conveyor belt 7 Printed part 400 Image forming device 401 Exterior of image forming device 401c Device body cover 404 Cartridge Holder 410 Main Tank 410k, 410c, 410m, 410y Main tanks for black (K), cyan (C), magenta (M), and yellow (Y) 411 Ink storage unit 413 Ink outlet 414 Storage container case 420 Mechanism Department 434 Discharge Head 436 Supply Tube [Prior art documents] [Patent documents]
[0065] [Patent Document 1] JP 2005-194500 A [Patent Document 2] JP 2012-72359 A [Patent Document 3] JP 2017-165961 A
Claims
1. An ink comprising a plurality of organic solvents, a pigment and water, the organic solvents include 1,2-propanediol and 1,2-hexanediol; The ink further comprises a polyoxyethylene ether compound, The ink, wherein the polyoxyethylene ether compound is polyethylene glycol trimethylnonyl ether.
2. The ink according to claim 1 , further comprising a urethane resin and / or an acrylic resin.
3. 3. The ink according to claim 2, wherein the urethane resin and / or the acrylic resin is in the form of resin particles.
4. A method for forming an image on a recording medium using ink by an inkjet method, comprising the steps of: An image forming method, comprising the steps of: applying a treatment liquid containing at least a flocculant onto the recording medium; and forming an image using the ink according to any one of claims 1 to 3 as the ink.
Citation Information
Patent Citations
Inkjet recording pigment ink and inkjet recording method
JP2004203903A
Ink composition imparting glossy feeling and method for evaluating glossy feeling
JP2005194500A
Ink-jet recording ink, recording method, print, and ink-jet recording apparatus
JP2005272847A
Inkjet recording ink
JP2008231219A
Ink, inkjet recording method, ink cartridge, recording unit and inkjet recording apparatus
JP2010121034A