Polycarbonate resin composition and optical lens using same
A polycarbonate resin composition with specific structural units and antioxidants addresses the imbalance in refractive index and Abbe number, enhancing heat resistance and moldability for optical lenses.
Patent Information
- Application Number
- JP2020571254
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-08
- Filing Date
- 2020-02-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-02-06
AI Technical Summary
Polycarbonate resins face challenges in balancing refractive index and Abbe number, leading to issues with chromatic aberration and large photoelastic constants, while also exhibiting poor heat resistance and moldability.
A polycarbonate resin composition comprising specific structural units derived from diol compounds and antioxidants, with precise copolymerization ratios, achieving a well-balanced refractive index and Abbe number, improved heat resistance, and enhanced molding properties.
The composition achieves a balanced refractive index and Abbe number, with good heat resistance and molding properties, suitable for optical lenses.
Smart Images

Figure 0007585790000023 
Figure 0007585790000001 
Figure 0007585790000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycarbonate resin composition having a well-balanced refractive index and Abbe number, and an optical lens using the same. [Background technology]
[0002] Polycarbonate resin (hereinafter sometimes referred to as "PC") is a polymer in which dihydric phenols are linked by carbonate esters, and among them, polycarbonate resin obtained from 2,2-bis(4-hydroxyphenyl)propane (commonly known as "bisphenol A") is used in many fields due to its excellent transparency, heat resistance, and mechanical properties such as impact resistance. In the optical field, such as various lenses and optical disks, its properties such as impact resistance, transparency, and low water absorption have attracted attention, and it occupies an important position as an optical material.
[0003] In particular, in the field of lenses, the thermoplastic resin PC has attracted attention due to its ease of production, and demand for it as an alternative to thermosetting resins such as CR-39 (diethylene glycol bisallyl carbonate), which have dominated plastic lenses up until now, has been increasing.
[0004] However, polycarbonate resins obtained by reacting bisphenol A with carbonate precursors such as phosgene and diphenyl carbonate have the disadvantages of being prone to chromatic aberration problems and a poor balance between the refractive index and Abbe number because they have a high refractive index but a low Abbe number, and also have the disadvantages of having a large photoelastic constant, which results in large birefringence in molded products.
[0005] In order to solve such drawbacks of polycarbonate resins, several copolymerized polycarbonate resins of aromatic dihydroxy compounds and aliphatic diols have been proposed (Patent Documents 1 to 5). These techniques have problems such as low refractive index and Abbe number, high photoelastic constant, high birefringence of molded products, insufficient moldability and heat resistance, and failure to obtain satisfactory molded products, and coloring. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 1-66234 [Patent Document 2] Japanese Patent Application Publication No. 10-120777 [Patent Document 3] Japanese Patent Application Publication No. 11-228683 [Patent Document 4] Japanese Patent Application Publication No. 11-349676 [Patent Document 5] JP 2000-63506 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to solve at least one of the above-mentioned problems in the prior art. Another object of the present invention is to provide a polycarbonate resin composition having a well-balanced refractive index and Abbe number, and an optical lens using the same. A further object of the present invention is to provide a polycarbonate resin composition having excellent heat resistance and molding cycle property, and an optical lens using the same. [Means for solving the problem]
[0008] As a result of extensive investigations, the present inventors have found that at least one of the above problems can be solved by using a combination of diol compounds having specific structures. That is, the present invention is as follows. <1> The present invention relates to a polymerizable composition comprising a constitutional unit represented by the following formula (1), a constitutional unit represented by the following formula (2), and a constitutional unit represented by the following general formula (3): It also contains antioxidants. Recarbonate resin composition And, (the constituent unit (mol) represented by the formula (1)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 8 to 32 mol %, (the constituent unit (mol) represented by the formula (2)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 28 to 52 mol %, (the constituent units (moles) represented by the general formula (3)) / (the constituent units (moles) represented by the formula (1)+the constituent units (moles) represented by the formula (2)+the constituent units (moles) represented by the general formula (3))×100 is 28 to 52 mol %, The antioxidant is selected from the group consisting of triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. the polycarbonate resin composition, wherein the polycarbonate resin is selected from the group consisting of N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane. It is. [ka] [ka] [ka] (In general formula (3), R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 20 carbon atoms which may contain a heterocyclic atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms; p, q, r, and s each independently represent an integer of 0 to 4; i represents an integer from 1 to 10, and ii represents an integer from 0 to 10. <2> The antioxidant is contained in the polycarbonate resin composition in an amount of 0.50% by mass or less. <1> The polycarbonate resin composition according to claim 1, <3> The antioxidant is contained in the polycarbonate resin composition in an amount of 0.10 to 0.40 mass %. <1> or <2> The polycarbonate resin composition according to claim 1, 。 <4 The polycarbonate resin composition according to claim 1, wherein the phenol content in the polycarbonate resin is 0.1 to 3000 ppm. <1> From < 3 1. The polycarbonate resin composition according to claim 1, < 5 The polycarbonate resin composition according to claim 1, wherein the content of the carbonic acid diester in the polycarbonate resin is 0.1 to 1000 ppm. <1> From < 4 1. The polycarbonate resin composition according to any one of claims 1 to 9. 。 <6 > The constitutional unit represented by the general formula (3) is [ka] The above <1> From < 5 10. The polycarbonate resin composition according to any one of claims 1 to 9. < 7 > The glass transition temperature (Tg) is 140°C to 200°C. <1> From < 6 1. The polycarbonate resin composition according to claim 1, < 8 > the refractive index (nD) is 1.565 to 1.600 and the Abbe number (v) is 26 to 32. <1> From < 7 1. The polycarbonate resin composition according to claim 1, < 9 > The refractive index (nD) and Abbe number (v) satisfy the following relationship: <1> From < 8 1. The polycarbonate resin composition according to claim 1, -0.0130v +1.9480 <nD<-0.0130v +1.9900 < 10 > The weight average molecular weight (Mw) of the above is 10,000 to 70,000. <1> From < 9 1. The polycarbonate resin composition according to claim 1, < 11 > Above <1> From < 10 An optical lens comprising the polycarbonate resin composition according to any one of claims 1 to 5. < 12 > The thickness is 0.01 to 30 mm. 11 >An optical lens as described in the above. Effect of the Invention
[0009] According to the present invention, a polycarbonate resin composition having a well-balanced refractive index and Abbe number can be obtained, and in particular, a polycarbonate resin composition having good heat resistance and molding cycle property can be obtained at a specific copolymerization ratio. The polycarbonate resin composition of the present invention is most suitable for optical lenses. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a graph showing the relationship between the Abbe number and the refractive index in the polycarbonate resin compositions obtained in the Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. <Polycarbonate resin composition> The polycarbonate resin composition of the present invention contains at least a polycarbonate resin containing a constitutional unit represented by the above formula (1), a constitutional unit represented by the above formula (2), and a constitutional unit represented by the above general formula (3). These constitutional units are derived from a diol compound represented by the following formula (1'), a diol compound represented by the following formula (2'), and a diol compound represented by the following general formula (3'), respectively.
[0012] [ka] Here, the diol compound represented by the above formula (1') is a diol compound called SPG (spiroglycol: 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane), and in the present invention, either a commercially available product or a synthesized product may be used.
[0013] [ka] Here, the diol compound represented by the above formula (2') is a diol compound called Bis-TMC (1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane), and in the present invention, either a commercially available product or a synthesized product may be used.
[0014] [ka] In general formula (3'), R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 20 carbon atoms which may contain a hetero ring atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms. 1 and R 2 each independently represents a hydrogen atom, a methyl group, an ethyl group, or a phenyl group; R 3 and R 4 each independently represents a hydrogen atom or a phenyl group. p, q, r and s each independently represent an integer of 0 to 4, and preferably, p and q represent 1, and r and s represent 0. "i" represents an integer of 1 to 10, preferably an integer of 1 to 4, and more preferably 2. ii represents an integer of 0 to 10, preferably an integer of 1 to 3, and more preferably 1.
[0015] In one embodiment of the present invention, the constitutional unit represented by the general formula (3) is [ka] When used as an optical lens, it is preferable that the refractive index and Abbe number are well balanced.
[0016] The above structural units are derived from BPEF (9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene) represented by the following structural formula and BPPEF (9,9-bis[4-(2-hydroxyethoxy)-3-phenylphenyl]fluorene) represented by the following structural formula, respectively, and in the present invention, either commercially available products or synthesized products may be used. [ka]
[0017] In one embodiment of the present invention, with respect to the proportion of the structural unit represented by formula (1), (structural unit (mol) represented by formula (1)) / (structural unit (mol) represented by formula (1)+structural unit (mol) represented by formula (2)+structural unit (mol) represented by general formula (3))×100 is preferably 8 to 32 mol%, more preferably 10 to 30 mol%, and particularly preferably 15 to 25 mol%. Furthermore, with regard to the proportion of the structural unit represented by the formula (2), (structural unit (mol) represented by the formula (2)) / (structural unit (mol) represented by the formula (1)+structural unit (mol) represented by the formula (2)+structural unit (mol) represented by the general formula (3))×100 is preferably 28 to 52 mol%, more preferably 30 to 48 mol%, and particularly preferably 33 to 42 mol%. Furthermore, with regard to the proportion of the structural unit represented by the general formula (3), (structural unit (mol) represented by the general formula (3)) / (structural unit (mol) represented by the formula (1)+structural unit (mol) represented by the formula (2)+structural unit (mol) represented by the general formula (3))×100 is preferably 28 to 52 mol%, more preferably 32 to 50 mol%, and particularly preferably 38 to 48 mol%. By adjusting the copolymerization ratio within the above range, it is possible to obtain a polycarbonate resin composition having good heat resistance and molding cycle property.
[0018] The polycarbonate resin used in the polycarbonate resin composition of the present invention may be a ternary resin prepared using, as monomers, the diol compound represented by the above formula (1'), the diol compound represented by the above formula (2'), and the diol compound represented by the above general formula (3'), or may contain other diol compounds other than these diol compounds. Examples of such other diol compounds include [ka] 4,4'-biphenyldiol, bis(4-hydroxyphenyl)methane, bis(2-hydroxyphenyl)methane, 2,4'-dihydroxydiphenylmethane, bis(4-hydroxyphenyl)ether, bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis(2-hydroxyphenyl)sulfone, bis(4-hydroxy-3-methylphenyl)sulfone, bis(4-hydroxyphenyl)sulfoxide, bis(4-hydroxyphenyl)sulfide, bis(4-hydroxyphenyl)ketone, 1,1 -Bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-methylphenyl)ethane, bis(4-hydroxy-3-methylphenyl)methane, 2,2-bis(4-hydroxy-3-t-butylphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)cycloundecane, 1,1-bis(4-hydroxyphenyl)cyclododecane, 2,2-bis(4-hydroxy-3-allylphenyl)propane, 3,3,5-trimethyl-1,1-bis(4-hydroxyphenyl)cyclohexane, α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethyldiphenyl random copolymer siloxane, α,ω-bis[3-(o-hydroxyphenyl)propyl]polydimethyldiphenyl random copolymer siloxane )propyl]polydimethylsiloxane, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol, 1,3-adamantanediol, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1-bis(4-hydroxyphenyl)-2-methylpropane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 1,1-bis(4-hydroxyphenyl)decane, 1,3-Bis(4-hydroxyphenyl)-5,7-dimethyladamantane, 2,2-bis(4-(2-hydroxyethoxy)phenyl)propane, 4,4-bis(2-hydroxyethoxy)biphenyl, 2,2'-(1,4-phenylene)bis(ethan-1-ol), 2,2'-(1,4-phenylene)bis(methane-1-ol), 2,2'-(1,4-phenylenebis(oxy))bis(ethan-1-ol), 1,1-bis(4-hydroxyphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-methylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-phenylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-t-butylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-sec-butylphenyl)cyclododecane, 1,1-bis(4-hydroxyphenyl)cyclododecane, Examples of the diol compound include, but are not limited to, 1,1-bis(4-hydroxy-3-allylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)cyclododecane, 1,1-bis(4-hydroxy-3-fluorophenyl)cyclododecane, 1,1-bis(4-hydroxy-3-chlorophenyl)cyclododecane, 1,1-bis(4-hydroxy-3-bromophenyl)cyclododecane, 7-ethyl-1,1-bis(4-hydroxyphenyl)cyclododecane, 5,6-dimethyl-1,1-bis(4-hydroxyphenyl)cyclododecane, pentacyclopentadecanedimethanol, 1,4-cyclohexanedimethanol, 1,3-adamantanedimethanol, decalin-2,6-dimethanol, tricyclodecane, dimethanolfluorene glycol, fluorene diethanol, and isosorbide. The other diol compound is preferably 2,2-bis(4-hydroxyphenyl)propane. The amount of the other diol compound added can be appropriately adjusted within a range that does not impair the effects of the present invention.
[0019] In one embodiment of the present invention, the polycarbonate resin composition may contain any of a random copolymer structure, a block copolymer structure, and an alternating copolymer structure.
[0020] In one embodiment of the present invention, the polystyrene-equivalent weight average molecular weight (Mw) of the polycarbonate resin composition may be preferably 10,000 to 70,000. The polystyrene-equivalent weight average molecular weight (Mw) of the polycarbonate resin composition is more preferably 20,000 to 50,000, and particularly preferably 30,000 to 45,000. If the polystyrene-equivalent weight average molecular weight (Mw) of the polycarbonate resin composition is within the above range, it is possible to prevent the molded body from becoming brittle, to prevent the melt viscosity from becoming excessively high, to facilitate removal of the resin after production, and to improve the flowability, to facilitate injection molding in a molten state.
[0021] In another embodiment of the present invention, the polycarbonate resin composition can be used for the production of an optical lens by blending the polycarbonate resin with other resins, such as, but not limited to, polyester carbonate, polyamide, polyacetal, modified polyphenylene ether, polyester (e.g., polyethylene terephthalate, polybutylene terephthalate), etc.
[0022] (Other Ingredients) In one embodiment of the present invention, the polycarbonate resin composition may contain antioxidants and mold release agents as additives.
[0023] Antioxidants include triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane.
[0024] The content of the antioxidant in the polycarbonate resin composition is preferably 0.50% by mass or less, more preferably 0.05 to 0.40% by mass, even more preferably 0.05 to 0.20% by mass or 0.10 to 0.40% by mass, and particularly preferably 0.20 to 0.40% by mass.
[0025] The release agent is preferably one that is composed of 90% by weight or more of an ester of alcohol and fatty acid. Specific examples of the ester of alcohol and fatty acid include ester of monohydric alcohol and fatty acid, and partial or full ester of polyhydric alcohol and fatty acid. The ester of monohydric alcohol and fatty acid is preferably an ester of monohydric alcohol having 1 to 20 carbon atoms and saturated fatty acid having 10 to 30 carbon atoms. In addition, the partial or full ester of polyhydric alcohol and fatty acid is preferably a partial or full ester of polyhydric alcohol having 1 to 25 carbon atoms and saturated fatty acid having 10 to 30 carbon atoms.
[0026] Specifically, examples of esters of monohydric alcohols and saturated fatty acids include stearyl stearate, palmityl palmitate, butyl stearate, methyl laurate, isopropyl palmitate, etc. Examples of partial or complete esters of polyhydric alcohols and saturated fatty acids include complete or partial esters of dipentaerythritol, such as stearic acid monoglyceride, stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearic acid monosorbitate, behenic acid monoglyceride, capric acid monoglyceride, lauric acid monoglyceride, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propylene glycol monostearate, biphenyl biphenate, sorbitan monostearate, 2-ethylhexyl stearate, and dipentaerythritol hexastearate.
[0027] The content of the release agent in the polycarbonate resin composition is preferably 0.50% by mass or less, more preferably 0.01 to 0.10% by mass, even more preferably 0.02 to 0.05% by mass, and particularly preferably 0.03 to 0.05% by mass.
[0028] Further, the polycarbonate resin composition of the present invention may contain other additives such as a processing stabilizer, an ultraviolet absorber, a flow modifier, a crystal nucleating agent, a reinforcing agent, a dye, an antistatic agent, a bluing agent, and an antibacterial agent.
[0029] (impurities) The polycarbonate resin of the present invention may contain impurities such as phenol generated during production, and diols and diester carbonates which are monomers remaining unreacted. The phenol content in the polycarbonate resin is preferably 0.1 to 3000 ppm, more preferably 0.1 to 2000 ppm, and particularly preferably 1 to 1000 ppm, 1 to 800 ppm, 1 to 500 ppm, or 1 to 300 ppm. The diol content in the polycarbonate resin is preferably 0.1 to 5000 ppm, more preferably 1 to 3000 ppm, even more preferably 1 to 1000 ppm, and particularly preferably 1 to 500 ppm. The diester carbonate content in the polycarbonate resin is preferably 0.1 to 1000 ppm, more preferably 0.1 to 500 ppm, and particularly preferably 1 to 100 ppm. By adjusting the amount of phenol and carbonic acid diester contained in the polycarbonate resin, it is possible to obtain a resin having properties according to the purpose. The amount of phenol and carbonic acid diester can be appropriately adjusted by changing the polycondensation conditions and the apparatus. It can also be adjusted by the conditions of the extrusion process after polycondensation.
[0030] If the content of phenol or carbonic acid diester exceeds the above range, problems may occur such as a decrease in strength of the obtained resin molded body, generation of odor, etc. On the other hand, if the content of phenol or carbonic acid diester is below the above range, there is a risk of a decrease in plasticity when the resin is melted.
[0031] <Method for producing polycarbonate resin composition> In one embodiment of the present invention, the polycarbonate resin can be produced according to the method described in WO2018 / 016516. Specifically, the polycarbonate resin can be produced by reacting the diol compound represented by the formula (1'), the diol compound represented by the formula (2'), and the diol compound represented by the general formula (3') with a carbonate precursor such as a carbonic acid diester in the presence or absence of a basic compound catalyst and / or an ester exchange catalyst under heating and under normal or reduced pressure by a melt polycondensation method. The method for producing the polycarbonate resin composition of the present invention is not limited to the above-mentioned method.
[0032] <Physical properties of polycarbonate resin composition> (A) Refractive index (nD) In one embodiment of the present invention, the polycarbonate resin composition has a refractive index of preferably 1.565 to 1.600, more preferably 1.585 to 1.600, and particularly preferably 1.585 to 1.590 at a wavelength of 587.6 nm and 23° C. The polycarbonate resin composition of the present invention has a high refractive index and is suitable as an optical lens material. The refractive index can be measured using an Abbe refractometer in accordance with JIS-K-7142:2014.
[0033] (B) Abbe number (ν) In one embodiment of the present invention, the polycarbonate resin composition has an Abbe number at 23° C. of preferably 26 to 32, more preferably 27 to 31, and particularly preferably 28 to 30. The Abbe number can be measured using an Abbe refractometer and calculated by the method described in the examples described later. In one embodiment of the present invention, it is preferable that the refractive index (nD) and Abbe number (v) of the polycarbonate resin composition satisfy the following relationship. -0.0130v +1.9480 <nD<-0.0130v +1.9900 It is more preferable that the refractive index (nD) and the Abbe number (v) satisfy the following relational expression: -0.0130v +1.9480 <nD<-0.0065v +1.7785 By satisfying such a relational expression, a well-balanced relationship between the refractive index and the Abbe number is obtained, which is preferable.
[0034] (C) Glass transition temperature (Tg) In one embodiment of the present invention, the glass transition temperature (Tg) of the polycarbonate resin composition is preferably 140 to 200°C, more preferably 145 to 160°C, and particularly preferably 150 to 160°C. If the glass transition temperature (Tg) of the polycarbonate resin composition is within the above range, it is convenient for injection molding. If the Tg is lower than 140°C, the use temperature range becomes narrow, which is not preferable. If the Tg exceeds 200°C, the melting temperature of the resin becomes high, which is not preferable because decomposition or coloring of the resin is likely to occur. If the glass transition temperature of the resin is too high, the difference between the mold temperature and the resin glass transition temperature becomes large in a general-purpose mold temperature regulator. Therefore, in applications where strict surface accuracy is required for the product, it is difficult and not preferable to use a resin with a too high glass transition temperature.
[0035] (D) Other characteristics The polycarbonate resin composition of the present invention has high moist heat resistance. The moist heat resistance can be evaluated by performing a "PCT test" (pressure cooker test) on an optical molded article obtained using the polycarbonate resin composition and measuring the total light transmittance of the optical molded article after the test. The PCT test can be performed by holding an injection molded article having a diameter of 50 mm and a thickness of 3 mm obtained by the method described in the following examples under conditions of 120°C, 0.2 MPa, 100% RH, and 20 hours. The polycarbonate resin composition of the present invention has a total light transmittance of preferably 60% or more, more preferably 70% or more, even more preferably 75% or more, and particularly preferably 80% or more after the PCT test. If the total light transmittance is 60% or more, it can be said that the composition has high moist heat resistance compared to conventional polycarbonate resins. The total light transmittance can be measured by the method described in the following examples.
[0036] The b value of the polycarbonate resin composition of the present invention is preferably 5 or less. The smaller the b value, the weaker the yellowness and the better the hue. The b value can be measured by the method described in the following examples.
[0037] The amount of residual phenol contained in the polycarbonate resin composition of the present invention is preferably 500 ppm or less, more preferably 300 ppm or less, further preferably 150 ppm or less, and particularly preferably 50 ppm or less. Incidentally, it is considered that the inclusion of some residual phenol has the advantages of increasing thermoplasticity and providing an antibacterial effect.
[0038] The amount of residual diphenyl carbonate (DPC) contained in the polycarbonate resin composition of the present invention is preferably 200 ppm or less, more preferably 150 ppm or less, further preferably 100 ppm or less, and particularly preferably 50 ppm or less. Incidentally, it is considered that the inclusion of some residual diphenyl carbonate (DPC) has the advantage of preventing hydrolysis during melt molding.
[0039] <Optical lenses> The optical lens of the present invention can be obtained by injection molding the polycarbonate resin composition of the present invention described above into a lens shape using an injection molding machine or an injection compression molding machine. In one embodiment of the present invention, the optical lens can be produced according to the method described in WO2018 / 016516. The molding conditions for injection molding are not particularly limited, but the molding temperature is preferably 180 to 300°C, more preferably 180 to 290°C. The injection pressure is preferably 50 to 1700 kg / cm. 2 It is.
[0040] In order to prevent foreign matter from being mixed into the optical lens as much as possible, the molding environment must naturally be a low-dust environment, preferably class 1000 or less, and more preferably class 100 or less.
[0041] The optical lens of the present invention is preferably used in the form of an aspherical lens as necessary. Since an aspherical lens can substantially eliminate spherical aberration with a single lens, it is not necessary to remove spherical aberration by combining a plurality of spherical lenses, and it is possible to reduce weight and production costs. Therefore, among optical lenses, the aspherical lens is particularly useful as a camera lens. The astigmatism of the aspherical lens is preferably 0 to 15 mλ, and more preferably 0 to 10 mλ.
[0042] The thickness of the optical lens of the present invention can be set in a wide range depending on the application and is not particularly limited, but is preferably 0.01 to 30 mm, more preferably 0.1 to 15 mm. A coating layer such as an antireflection layer or a hard coat layer may be provided on the surface of the optical lens of the present invention as necessary. The antireflection layer may be a single layer or a multilayer, and may be an organic or inorganic material, but is preferably an inorganic material. Specifically, examples of the antireflection layer include oxides or fluorides such as silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, cerium oxide, magnesium oxide, and magnesium fluoride. Among these, silicon oxide and zirconium oxide are more preferable, and a combination of silicon oxide and zirconium oxide is even more preferable. In addition, the antireflection layer is not particularly limited with respect to the combination of single layer / multilayer, or the combination of their components and thicknesses, but is preferably a two-layer or three-layer structure, and particularly preferably a three-layer structure. The antireflection layer as a whole is preferably formed to a thickness of 0.00017 to 3.3% of the thickness of the optical lens, specifically 0.05 to 3 μm, and particularly preferably 1 to 2 μm. EXAMPLES
[0043] The present invention will be described below using examples, but the present invention is not limited to these examples in any way.
[0044] <Refractive index (nD)> The refractive index (nD) of a 0.1 mm thick film made of the polycarbonate resin obtained below was measured using an Abbe refractometer at a wavelength of 587.6 nm and at 23° C. according to the method of JIS-K-7142:2014. The 0.1 mm film was obtained by press molding.
[0045] <Abbe number (ν)> The refractive indexes of a 0.1 mm thick film made of the polycarbonate resin obtained below at wavelengths of 486 nm, 587.6 nm, and 656 nm at 23° C. were measured using an Abbe refractometer, and the Abbe number (ν) was calculated using the following formula: The 0.1 mm film was obtained by press molding. ν=(nD-1) / (nF-nC) nD: Refractive index at a wavelength of 587.6 nm nC: Refractive index at a wavelength of 656 nm nF: Refractive index at a wavelength of 486 nm
[0046] <Glass transition temperature (Tg)> The glass transition temperature (Tg) was measured by differential scanning calorimetry (DSC) under the following specific conditions: Equipment: Hitachi High-Tech Science DSC7000X Sample size: 5mg Atmosphere: Nitrogen gas atmosphere Temperature rise condition: 10℃ / min
[0047] <Weight average molecular weight (Mw)> The weight average molecular weight (Mw) in terms of polystyrene was calculated from a calibration curve of a standard polystyrene prepared in advance. That is, a calibration curve was prepared using a standard polystyrene ("PStQuick MP-M" manufactured by Tosoh Corporation) with a known molecular weight (molecular weight distribution = 1), and the elution time and molecular weight value of each peak from the measured standard polystyrene were plotted, and a cubic approximation was performed to obtain a calibration curve. Mw was calculated from the following formula. Mw = Σ(Wi × Mi) ÷ Σ(Wi) Here, i represents the i-th division point when dividing the molecular weight M, Wi represents the i-th weight, and Mi represents the i-th molecular weight. The molecular weight M represents the polystyrene molecular weight value at the same elution time on the calibration curve. The GPC device used was a Tosoh Corporation HLC-8320GPC, with one TSKguardcolumn SuperMPHZ-M as the guard column and three TSKgel SuperMultiporeHZ-M connected in series as the analytical column. Other conditions were as follows. Solvent: HPLC grade tetrahydrofuran Injection volume: 10μL Sample concentration: 0.2 w / v% HPLC grade chloroform solution Solvent flow rate: 0.35ml / min Measurement temperature: 40℃ Detector: RI
[0048] <Heat resistance test> The polycarbonate resin obtained below was vacuum dried at 120°C for 4 hours, and then injection molded using an injection molding machine (FANUC ROBOSHOT α-S30iA) at a cylinder temperature of 270°C and a mold temperature of Tg-10°C to obtain a plate. The plate was then heated at Tg-20°C for 4 hours and allowed to stand at 25°C for 24 hours, after which a disk-shaped plate test piece with a diameter of 50.00 mm and a thickness of 3 mm was obtained. The disk-shaped plate test piece was allowed to stand at 125°C for 1000 hours under air, and the diameter of the test piece was measured. Heat resistance was evaluated according to the following criteria. Heat resistance A: Disk-shaped plate diameter 49.9 mm to 50.00 mm Heat resistance B: Disc-shaped plate diameter 49.8 mm or more and less than 49.9 mm Heat resistance C: Disc-shaped plate diameter less than 49.8 mm
[0049] <Molding cycle test> The polycarbonate resin obtained below was vacuum dried at 120°C for 4 hours, and then injection molded using an injection molding machine (FANUC ROBOSHOT α-S30iA) at a cylinder temperature of 270°C and a mold temperature of Tg-10°C. The molding cycle and the obtained molded products were visually checked for cracks and sticking to the mold. The molding cycle was evaluated according to the following criteria. Molding cycle A: Molding cycle of 20 seconds is possible. Molded products do not crack or stick to the mold. Molding cycle B: With a molding cycle of 20 seconds, the molded product cracks or sticks to the mold. A molding cycle of 30 seconds is possible. Molding cycle C: Molding is not possible with a molding cycle of 20 seconds. Even with a molding cycle of 30 seconds, the molded product cracks and sticks to the mold.
[0050] <Measurement of phenol (PhOH) and diphenyl carbonate (DPC) content in polycarbonate resin> 0.5 g of the polycarbonate resin obtained below was dissolved in 50 mL of tetrahydrofuran (THF) to prepare a sample solution. A calibration curve for phenol and diphenyl carbonate was prepared from pure products obtained by distilling commercially available phenol and diphenyl carbonate as standards for phenol and diphenyl carbonate, and 2 μL of the sample solution was quantified by LC-MS under the following measurement conditions. The detection limit under these measurement conditions is 0.01 ppm (mass ratio). LC-MS measurement conditions: Measuring device (LC part): Agilent Infinity 1260 LC System Column: ZORBAX Eclipse XDB-18, and guard cartridge Mobile phase: A: 0.01mol / L-ammonium acetate solution B: 0.01 mol / L ammonium acetate in methanol C:THF Mobile phase gradient program: As shown in Table 1 below, the mixture of A to C above was used as the mobile phase, and the mobile phase was flowed through the column for 30 minutes while switching the composition of the mobile phase when the time shown in the "Time (min)" column elapsed.
Table 1
Table 2
[0051] <Total light transmittance after PCT test> The polycarbonate resin obtained below was vacuum dried at 120 °C for 4 hours, and then injection molded by an injection molding machine (FANUC ROBOSHOT α-S30iA) at a cylinder temperature of 270 °C and a mold temperature of Tg - 10 °C to obtain a disc-shaped test plate piece with a diameter of 50 mm and a thickness of 3 mm. The PCT test was performed by holding the obtained plate piece with a diameter of 50 mm and a thickness of 3 mm under the conditions of 120 °C, 0.2 Mpa, 100% RH, and 20 hours. The total light transmittance after this PCT test was measured with a turbidimeter (MODEL 1001DP, manufactured by Nippon Denshoku Industries Co., Ltd.) according to the old JIS K7105.
[0052] The polycarbonate resin obtained below was vacuum dried at 120°C for 4 hours, and then injection molded using an injection molding machine (FANUC ROBOSHOT α-S30iA) at a cylinder temperature of 270°C and a mold temperature of Tg-10°C to obtain a disk-shaped test plate piece with a diameter of 50 mm and a thickness of 3 mm. Using the obtained plate piece, the b value was measured using a Nippon Denshoku Industries Co., Ltd. SE2000 spectrophotometer in accordance with the old JIS K7105. The smaller the b value, the weaker the yellowness and the better the hue.
[0053] Example 1 The raw materials were 0.30 mol of SPG (spiroglycol: 3,9-bis(1,1-dimethyl-2-hydroxyethyl)-2,4,8,10-tetraoxaspiro[5.5]undecane) represented by the following structural formula, 0.41 mol of Bis-TMC (1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane) represented by the following structural formula, 0.29 mol of BPEF (9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene) represented by the following structural formula, 1.15 mol of DPC (diphenyl carbonate), and 1×10 sodium hydrogen carbonate. -5 mol was placed in a 2L reactor equipped with a stirrer and a distillation device, and heated to 180 ° C under a nitrogen atmosphere of 760 mmHg. 10 minutes after the start of heating, the complete dissolution of the raw materials was confirmed, and stirring was continued for another 110 minutes under the same conditions. Then, the degree of vacuum was adjusted to 200 mmHg, and the temperature was raised to 200 ° C at a rate of 60 ° C / hr. At this time, the start of distillation of by-produced phenol was confirmed. Then, the reaction was carried out by holding at 200 ° C for 20 minutes. The temperature was further raised to 230 ° C at a rate of 75 ° C / hr, and 10 minutes after the end of the temperature rise, the degree of vacuum was reduced to 1 mmHg or less over 1 hour while maintaining the temperature. Then, the temperature was raised to 245 ° C at a rate of 60 ° C / hr, and stirring was continued for another 30 minutes. After the reaction was completed, nitrogen was introduced into the reactor to return it to normal pressure, and the produced polycarbonate resin was taken out. The phenol (PhOH) content in the obtained polycarbonate resin was 100 ppm (mass ratio), and the DPC content was 100 ppm (mass ratio). The physical properties of the obtained resin are summarized in Table 3 below.
[0054] [ka]
[0055] (Examples 2 to 7, Comparative Examples 1 to 4) A polycarbonate resin was obtained in the same manner as in Example 1, except that the dihydroxy compound used as the raw material was changed to the dihydroxy compound (mol) shown in the following Table 3. The physical properties of the obtained resin are summarized in the following Table 3.
[0057] [Table 3] The present invention also includes the following aspects. <1> The polycarbonate resin composition includes a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), and a structural unit represented by the following general formula (3), and further contains an antioxidant. [ka] [ka] [ka] (In general formula (3), R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 20 carbon atoms which may contain a heterocyclic atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms; p, q, r, and s each independently represent an integer of 0 to 4; i represents an integer from 1 to 10, and ii represents an integer from 0 to 10. <2> The antioxidant is contained in the polycarbonate resin composition in an amount of 0.50% by mass or less. <1> The polycarbonate resin composition according to claim 1, <3> The antioxidant is contained in the polycarbonate resin composition in an amount of 0.10 to 0.40 mass %. <1> or <2> The polycarbonate resin composition according to claim 1, <4> The antioxidant is selected from the group consisting of triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl- 4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane, <1> from <3> The polycarbonate resin composition according to any one of claims 1 to 5, <5> The polycarbonate resin composition has a phenol content of 0.1 to 3000 ppm. <1> from <4> The polycarbonate resin composition according to any one of claims 1 to 5, <6> The polycarbonate resin composition has a carbonic acid diester content of 0.1 to 1000 ppm. <1> from <5> The polycarbonate resin composition according to any one of claims 1 to 5, <7> (the constituent unit (mol) represented by the formula (1)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 8 to 32 mol %. <1> from <6> The polycarbonate resin composition according to any one of claims 1 to 5, <8> (the constituent unit (mol) represented by the formula (2)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 28 to 52 mol %. <1> from <7> The polycarbonate resin composition according to any one of claims 1 to 5, <9> (the constituent unit (mol) represented by the general formula (3)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 28 to 52 mol %. <1> from <8> The polycarbonate resin composition according to any one of claims 1 to 5, <10> The constitutional unit represented by the general formula (3) is [ka] The above <1> from <9> The polycarbonate resin composition according to any one of claims 1 to 5, <11> The glass transition temperature (Tg) is 140°C to 200°C. <1> from <10> The polycarbonate resin composition according to any one of claims 1 to 5, <12> The refractive index (nD) is 1.565 to 1.600 and the Abbe number (v) is 26 to 32. <1> from <11> The polycarbonate resin composition according to any one of claims 1 to 5, <13> The refractive index (nD) and Abbe number (v) satisfy the following relationship: <1> from <12> The polycarbonate resin composition according to any one of claims 1 to 5, -0.0130v +1.9480 <nD<-0.0130v +1.9900 <14> The weight average molecular weight (Mw) of the above is 10,000 to 70,000. <1> from <13> The polycarbonate resin composition according to any one of claims 1 to 5, <15> the above <1> from <14> An optical lens comprising the polycarbonate resin composition according to any one of claims 1 to 5. <16> The thickness is 0.01 to 30 mm. <15> 1 is an optical lens according to the present invention.
Claims
1. A polycarbonate resin composition comprising a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), and a structural unit represented by the following general formula (3), and further containing an antioxidant: (the constituent unit (mol) represented by the formula (1)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 8 to 32 mol %, (the constituent unit (mol) represented by the formula (2)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 28 to 52 mol %, (the constituent unit (mol) represented by the general formula (3)) / (the constituent unit (mol) represented by the formula (1)+the constituent unit (mol) represented by the formula (2)+the constituent unit (mol) represented by the general formula (3))×100 is 28 to 52 mol %, The antioxidant is selected from the group consisting of triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, benzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate and 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane. 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 (In general formula (3), R 1 ~R 4 each independently represents a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 20 carbon atoms which may contain a heterocyclic atom selected from an oxygen atom, a nitrogen atom, and a sulfur atom, an alkenyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aralkyl group having 7 to 17 carbon atoms; p, q, r, and s each independently represent an integer of 0 to 4; i represents an integer from 1 to 10, and ii represents an integer from 0 to 10.
2. The polycarbonate resin composition according to claim 1 , wherein the antioxidant is contained in the polycarbonate resin composition in an amount of 0.50 mass % or less.
3. 3. The polycarbonate resin composition according to claim 1, wherein the antioxidant is contained in an amount of 0.10 to 0.40 mass % in the polycarbonate resin composition.
4. 4. The polycarbonate resin composition according to claim 1, wherein the phenol content in the polycarbonate resin contained in the polycarbonate resin composition is 0.1 to 3000 ppm.
5. 5. The polycarbonate resin composition according to claim 1, wherein the content of the carbonic acid diester in the polycarbonate resin contained in the polycarbonate resin composition is 0.1 to 1000 ppm.
6. The constitutional unit represented by the general formula (3) is 【Chemistry 4】 The polycarbonate resin composition according to any one of claims 1 to 5,
7. The polycarbonate resin composition according to any one of claims 1 to 6, having a glass transition temperature (Tg) of 140°C to 200°C.
8. 8. The polycarbonate resin composition according to claim 1, having a refractive index (nD) of 1.565 to 1.600 and an Abbe number (v) of 26 to 32.
9. The polycarbonate resin composition according to any one of claims 1 to 8, wherein the refractive index (nD) and the Abbe number (v) satisfy the following relationship: -0.0130v +1.9480<nD<-0.0130v +1.9900
10. The polycarbonate resin composition according to any one of claims 1 to 9, having a weight average molecular weight (Mw) of 10,000 to 70,000.
11. An optical lens comprising the polycarbonate resin composition according to any one of claims 1 to 10.
12. The optical lens according to claim 11, having a thickness of 0.01 to 30 mm.
Citation Information
Patent Citations
Aromatic-aliphatic polycarbonate copolymer
JP1989066234A
New polycarbonate resin
JP1998120777A
New copolymerized polycarbonate resin and its production
JP1999228683A
Aromatic-aliphatic copolymerized polycarbonate resin
JP1999349676A
Aromatic-aliphatic copolymer polycarbonate
JP2000063506A