Electrode assembly manufacturing method and electrode assembly manufacturing device

The method and apparatus address vapor interference in laser drying by incorporating vapor recovery and energy adjustment, enhancing drying efficiency and adhesion in electrode material processing.

JP7586136B2Active Publication Date: 2024-11-19TOYOTA JIDOSHA KK
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022080805
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-17
Publication Date
2024-11-19
Estimated Expiration
2042-05-17

AI Technical Summary

Technical Problem

Existing methods for drying electrode materials using laser heating face efficiency losses due to vapor interference, which obstructs laser irradiation.

Method used

A method and apparatus that involves conveying electrode materials through a system with laser irradiation positions and vapor recovery sections to recover vapor generated during drying, thereby preventing efficiency losses by maintaining clear laser paths and adjusting laser energy based on material thickness.

Benefits of technology

The method and apparatus effectively suppress drying efficiency losses by recovering vapor and adjusting laser energy, ensuring uniform drying and improved adhesion of electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586136000001
    Figure 0007586136000001
  • Figure 0007586136000002
    Figure 0007586136000002
  • Figure 0007586136000003
    Figure 0007586136000003
Patent Text Reader

Abstract

To provide an electrode body manufacturing method capable of suppressing decrease in drying efficiency when drying an electrode material using a laser.SOLUTION: An electrode body manufacturing method includes a conveyance step (S10) of conveying an electrode body 10 coated with an electrode material 1 by a conveyance unit 30, and a drying step (S30) of drying the electrode material 1 while conveying the electrode body 10 by the conveyance unit 30. The drying step (S30) includes an irradiation step (S31) of drying the electrode material 1 by irradiating the electrode material 1 with a laser when the electrode body 10 (electrode material 1) is conveyed to a position P1 (first position) in a transport direction (X direction) of the conveyance unit 30. The drying step (S30) includes a suction step (S32) of collecting vapor V generated due to laser irradiation on the electrode material 1 by a steam suction unit (steam recovery unit) provided at a position P2 (second position) adjacent to the position P1 in the conveyance direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an electrode assembly manufacturing method and an electrode assembly manufacturing apparatus. [Background technology]

[0002] Japanese Patent Laid-Open Publication No. 2000-353514 (Patent Document 1) discloses a coating line in which a paste material for an electrode active material is coated on one side of an electrode sheet unwound by a winding section using a surface coater. In the coating line, the paste material is dried in a drying chamber. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-353514 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, Patent Document 1 does not consider drying the paste material by laser heating in order to dry the applied paste material more efficiently. When drying the paste material by laser, the efficiency of drying by laser irradiation may decrease because steam evaporated from the paste material interferes with the laser irradiation. Therefore, it is desired to suppress the decrease in drying efficiency when drying the paste material (electrode material) by laser.

[0005] The present disclosure has been made to solve the above-mentioned problems, and its purpose is to provide an electrode body manufacturing method and an electrode body manufacturing apparatus that can suppress a decrease in drying efficiency when drying an electrode material with a laser. [Means for solving the problem]

[0006] An electrode body manufacturing method according to a first aspect of the present disclosure includes a conveying step of conveying an electrode body coated with at least one electrode material by a conveying unit, and a drying step of drying the electrode material while conveying the electrode body by the conveying unit. The drying step includes an irradiation step of drying the electrode material by irradiating the electrode material with a laser when the electrode body is conveyed to at least one first position in the conveying direction of the conveying unit, and a recovery step of recovering steam generated as a result of the electrode material being irradiated with the laser by a steam recovery unit provided at at least one second position adjacent to the first position in the conveying direction.

[0007] In the electrode assembly manufacturing method according to the first aspect of the present disclosure, as described above, the vapor recovery section provided at least one second position adjacent to the first position in the conveying direction recovers the vapor generated due to the laser irradiation of the electrode material. As a result, the amount of vapor at the first position can be reduced because the vapor generated at the first position is recovered by the vapor recovery section at the second position. As a result, the laser can be prevented from being blocked by the vapor, and therefore the efficiency of drying by the laser can be prevented from decreasing.

[0008] In the electrode body manufacturing method according to the first aspect, the recovery step preferably includes recovering, by a vapor recovery unit, vapor generated from the electrode material while the electrode material is being irradiated with the laser. With this configuration, the vapor around the electrode material can be recovered during the laser irradiation, so that it is possible to easily prevent the vapor from blocking the laser irradiation of the electrode material.

[0009] In the electrode body manufacturing method according to the first aspect, the irradiation step is preferably a step of irradiating the electrode material with a laser at each of a plurality of first positions spaced apart from each other in the transport direction. The recovery step is a step of recovering steam by a steam recovery section disposed at each of a plurality of second positions located between adjacent first positions in the transport direction. With this configuration, the steam generated at each of the plurality of first positions can be recovered by the steam recovery section. As a result, it is possible to suppress a decrease in the drying efficiency by the laser at each of the plurality of first positions.

[0010] In the electrode body manufacturing method according to the first aspect, the electrode material preferably includes a first portion near an end on one side in the conveying direction, a second portion near an end on the other side in the conveying direction, and a third portion between the first portion and the second portion, and the irradiating step is a step of making the energy of the laser when at least one of the first portion and the second portion is located within the laser irradiation area and the third portion is located outside the irradiation area smaller than the energy of the laser when the third portion is located within the irradiation area. Here, when a liquid electrode material is applied to a surface, the thickness of the electrode material near the end (near the edge) is smaller than the thickness of the portion other than the near the end. Therefore, by adjusting the energy of the laser as described above, it is possible to prevent the relatively thin near the end from being excessively dried by the laser. Note that the near the end means a region including both the end itself and the portion near the end.

[0011] In the electrode body manufacturing method according to the first aspect, the irradiating step is preferably a step of irradiating the electrode material with the laser while aligning the laser irradiation area with the arrangement area of ​​the electrode material in the width direction of the conveying section perpendicular to the conveying direction. With this configuration, it is possible to prevent the laser from being irradiated to areas other than the electrode material.

[0012] In this case, the irradiation step is preferably a step of irradiating the electrode material with a laser in a state in which the energy of the laser corresponding to the vicinity of both ends in the width direction of the irradiation area is smaller than the energy of the laser corresponding to the center part in the width direction of the irradiation area. In this manner, it is possible to prevent the both ends, which have a relatively small thickness, from being excessively dried by the laser. Note that the vicinity of both ends means the areas including both the ends themselves and the parts near the both ends.

[0013] In the electrode body manufacturing method according to the first aspect, the irradiation step is preferably a step of heating the electrode material to 150° C. or more by a laser. Here, when the electrode material is heated to 150° C. or more, the fluorine component (adhesive component) in the electrode material tends to migrate from the adhesive surface between the electrode material and the foil portion (the member to which the electrode material is adhered) to the surface side of the electrode material. Therefore, by heating the electrode material to 150° C. steeply (in a short time) by the laser, the heating time is shortened, and the migration of the fluorine component can be suppressed.

[0014] In the electrode body manufacturing method according to the first aspect, the electrode body preferably includes a foil portion and a plurality of electrode materials arranged side by side along a predetermined direction on a surface of the foil portion, the conveying step is a step of conveying the electrode body such that the plurality of electrode materials are conveyed side by side along the conveying direction, and the irradiating step is a step of reducing the laser energy to zero when a portion of the foil portion between the electrode materials passes through an irradiation area of ​​the laser. With this configuration, the consumption of the laser energy can be suppressed by reducing the energy of the laser irradiated to the foil portion to zero.

[0015] An electrode body manufacturing apparatus according to a second aspect of the present disclosure includes a conveying section that conveys an electrode body coated with at least one electrode material, a laser irradiation section that dries the electrode material by irradiating the electrode material with a laser when the electrode body is conveyed to at least one first position in the conveying direction of the conveying section, and a vapor recovery section that is provided in at least one second position adjacent to the first position in the conveying direction and that recovers vapor generated as a result of the electrode material being irradiated with the laser.

[0016] In the electrode body manufacturing apparatus according to the second aspect of the present disclosure, as described above, the vapor recovery unit provided in at least one second position adjacent to the first position in the conveying direction recovers the vapor generated due to the laser irradiation of the electrode material. As a result, the amount of vapor at the first position can be reduced because the vapor generated at the first position is recovered by the vapor recovery unit at the second position. As a result, the laser can be prevented from being blocked by the vapor, and therefore an electrode body manufacturing apparatus capable of preventing a decrease in the drying efficiency by the laser can be provided. Effect of the Invention

[0017] According to the present disclosure, when drying an electrode material with a laser, a decrease in drying efficiency can be suppressed. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a diagram showing a configuration of an electrode assembly manufacturing apparatus according to an embodiment. [Diagram 2] FIG. 2 is a partially enlarged perspective view of FIG. [Diagram 3] 3A to 3C are a cross-sectional view taken along line III-III in FIG. 2 and a diagram showing the spatial distribution of laser energy. [Figure 4] 1A and 1B are diagrams showing a laser irradiation area and a spatial distribution of laser energy. [Diagram 5] FIG. 2 is a flow diagram showing a method for manufacturing an electrode assembly according to one embodiment. [Figure 6] FIG. 1 is a diagram showing the relationship between a laser irradiation area and laser energy in an electrode material. [Figure 7] FIG. 4 is a diagram showing a temperature change on the surface of an electrode material due to laser irradiation. [Figure 8] FIG. 13 is a diagram showing the distribution of fluorine components in an electrode material after laser irradiation. [Figure 9] FIG. 13 is a diagram showing the peel strength of an electrode material after laser irradiation and the peel strength after drying in a drying oven (Comparative Example). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are designated by the same reference characters and the description thereof will not be repeated.

[0020] In this specification, the X direction and the Y direction are examples of the "conveying direction" and the "width direction" of the present disclosure, respectively. The Z direction is a direction perpendicular to each of the X direction and the Y direction. The laser irradiation unit 40 described later irradiates the laser in the Z2 direction.

[0021] Fig. 1 is a diagram showing the configuration of an electrode body manufacturing apparatus 100 according to the present embodiment. In the electrode body manufacturing apparatus 100, an electrode material 1 (positive electrode material or negative electrode material) (see Fig. 2) is applied to a metal foil 2 (aluminum foil or copper foil) (see Fig. 2) to manufacture an electrode body 10 (see Fig. 2). A plurality of electrode materials 1 are arranged side by side on a surface 2a of the metal foil 2 along a predetermined direction (the left-right direction in Fig. 2). The electrode body 10 is used, for example, in an on-vehicle lithium-ion battery. The metal foil 2 is an example of a "foil portion" in the present disclosure.

[0022] (Electrode body manufacturing equipment) As shown in Fig. 1, the electrode body manufacturing apparatus 100 includes a coating unit 20, a conveying unit 30, a plurality of laser irradiation units 40, and a plurality of steam suction units 50. In the example shown in Fig. 1, the conveying unit 30 conveys the electrode body 10 to the X2 side. The conveying unit 30 conveys the electrode body 10 at a constant speed. The steam suction unit 50 is an example of a "steam recovery unit" in the present disclosure.

[0023] The coating unit 20 is configured to be able to discharge the liquid electrode material 1. The coating unit 20 coats (applies) the liquid electrode material 1 onto the surface 2a of the metal foil 2.

[0024] The conveying section 30 includes a first roll section 31, a second roll section 32, a winding section 33, and a belt section 34. Tension is applied to the belt section 34 by the first roll section 31 and the second roll section 32. The belt section 34 is also wound up by the winding section 33. As a result, the electrode body 10 (metal foil 2) placed on the belt section 34 is moved towards the winding section 33.

[0025] The first roll unit 31 is provided on the upstream side of the conveying unit 30. The second roll unit 32 is provided on the downstream side of the conveying unit 30 from the first roll unit 31. The coating unit 20 coats the metal foil 2 passing through the first roll unit 31 with the electrode material 1.

[0026] The multiple laser irradiation sections 40 are arranged at intervals from one another along the extension direction of the conveyance section 30 (belt section 34). The multiple laser irradiation sections 40 may be arranged at equal intervals from one another.

[0027] Each of the multiple laser irradiation units 40 is provided so as to be able to irradiate a laser toward the belt unit 34. Each of the multiple laser irradiation units 40 irradiates the electrode material 1 with a laser when the electrode body 10 (electrode material 1) is transported to position P1 in the X direction. Therefore, the electrode material 1 is repeatedly irradiated with a laser. As a result, the liquid electrode material 1 is dried by the heat of the laser. Note that position P1 corresponds to the position of the irradiation region R to which the laser of each of the multiple laser irradiation units 40 is irradiated.

[0028] Each of the multiple steam suction units 50 is provided at a position P2 adjacent to the position P1 in the X direction. The most upstream steam suction unit 50 of the multiple steam suction units 50 is provided upstream (X1 side) of the most upstream position P1. The most downstream steam suction unit 50 of the multiple steam suction units 50 is provided downstream (X2 side) of the most downstream position P1. The multiple steam suction units 50 other than the above two steam suction units 50 are each arranged one by one between adjacent positions P1 (laser irradiation units 40).

[0029] Each of the multiple vapor suction units 50 sucks in vapor V (see FIG. 2) generated due to laser irradiation of the electrode material 1 at the adjacent position P1. The vapor V is a gas containing water vapor and other gases. The distance between positions P1 and P2 is a distance that allows the vapor suction unit 50 to suck in the vapor V (with a suction force).

[0030] Each of the steam suction units 50 includes a suction port 51 for steam V and a flow pipe 52 for steam V. The flow pipe 52 allows the steam V introduced from the suction port 51 to flow. The width W1 of the suction port 51 in the X direction gradually increases toward the conveying unit 30 side (Z2 side). Specifically, the suction port 51 has a cone shape that widens toward the conveying unit 30 side. In other words, the suction port 51 has a shape that narrows toward the opposite side (Z1 side) from the conveying unit 30. This makes it easier for the steam V generated at the adjacent position P1 to be sucked through the suction port 51. The suction port 51 and the conveying unit 30 (belt unit 34) are spaced apart from each other by a predetermined distance D in the Z direction.

[0031] 3, the laser irradiation region R coincides with the arrangement region of the electrode material 1 in the Y direction. In other words, the position in the Y direction of the end R1 on the Y1 side of the laser irradiation region R coincides with the position in the Y direction of the end 1a on the Y1 side of the electrode material 1. Also, the position in the Y direction of the end R2 on the Y2 side of the laser irradiation region R coincides with the position in the Y direction of the end 1b on the Y2 side of the electrode material 1. Therefore, the width W2 in the Y direction of the laser irradiation region R is equal to the width W3 in the Y direction of the electrode material 1.

[0032] Furthermore, in the Y direction, the thickness t of the electrode material 1 in the Z direction is not uniform. Specifically, the thickness t of the electrode material 1 near both ends (1a, 1b) is smaller than the thickness t of the central portion 1c of the electrode material 1 in the Y direction. Specifically, in a cross-sectional view along the Y direction (cross-sectional view of FIG. 3), the cross-section of the electrode material 1 has a mountain-like shape with a flat center.

[0033] Here, the laser energy corresponding to the vicinities of both ends (R1, R2) in the Y direction of the laser irradiation region R is smaller than the laser energy corresponding to the center R3 in the Y direction of the irradiation region R. Specifically, in a graph showing the relationship between the position in the Y direction and the amount of laser energy as shown in Fig. 3, the waveform of the laser energy is a mountain-shaped waveform with a flat center so as to correspond to the cross-sectional shape of the electrode material 1 in the Y direction.

[0034] 4, the laser energy corresponding to the vicinity of both ends (R4, R5) in the X direction of the laser irradiation region R is smaller than the laser energy corresponding to the center R6 in the X direction of the irradiation region R. Specifically, in the graph showing the relationship between the position in the X direction and the amount of laser energy as shown in FIG. 4, the waveform of the laser energy is a mountain-shaped waveform corresponding to the cross-sectional shape (not shown) of the electrode material 1 along the X direction. The waveform of the laser energy may also be a triangular or square waveform.

[0035] The width W4 of the laser irradiation area R in the X direction is smaller than the width W2 of the irradiation area R in the Y direction (see FIG. 3). The irradiation area R is fixed and does not move. The width W5 of the electrode material 1 in the X direction (see FIG. 2) is larger than the width W3 of the electrode material 1 in the Y direction (see FIG. 2).

[0036] (Electrode body manufacturing method) Next, a method for manufacturing the electrode assembly 10 using the electrode assembly manufacturing apparatus 100 will be described with reference to FIGS.

[0037] First, in step S10 shown in FIG. 5, the metal foil 2 is placed on the conveying section 30 (belt section 34), and the metal foil 2 is conveyed by the conveying section 30 (conveyance starts).

[0038] Next, in step S20, a plurality of electrode materials 1 are applied by the coating unit 20 (see FIG. 1) onto the surface 2a of the metal foil 2 being transported by the transport unit 30. At this time, the plurality of electrode materials 1 are arranged on the surface 2a at intervals from one another. As a result, the plurality of electrode materials 1 are transported side by side along the X direction on the surface 2a of the metal foil 2.

[0039] Next, in step S30, the electrode material 1 is dried while the electrode body 10 is transported by the transport unit 30. Specifically, in step S30, a drying process (step S31) is performed in which the electrode material 1 is dried by irradiating a laser onto the electrode body 1 (electrode material 1) when the electrode body 10 (electrode material 1) is transported to each of the multiple positions P1. Furthermore, in step S30, a suction process (step S32) is also performed in which the steam V is sucked by the steam suction units 50 provided at multiple positions P2 adjacent to the position P1 in the X direction. The suction process is an example of the "recovery process" of the present disclosure.

[0040] In the suction step (S32), while the electrode material 1 is being irradiated with a laser, the vapor V generated from the electrode material 1 is sucked by the vapor suction unit 50. That is, the period during which the irradiation step (S31) is performed and the period during which the suction step (S32) is performed overlap with each other. Note that the suction of the vapor V by the vapor suction unit 50 is not performed intermittently but is performed continuously.

[0041] 6, in the irradiation step (S31), the laser irradiation unit 40 irradiates the laser intermittently. Specifically, when a portion 2b of the metal foil 2 between the electrode materials 1 passes through a laser irradiation region R (see FIG. 2), the laser energy is set to 0. Then, the laser is output (the laser energy is set to be greater than 0) only when the electrode material 1 passes through the laser irradiation region R.

[0042] Here, the electrode material 1 includes a first portion 1e near the end 1d on the X1 side. The electrode material 1 also includes a second portion 1g near the end 1f on the X2 side. The electrode material 1 also includes a third portion 1h between the first portion 1e and the second portion 1g. The third portion 1h is adjacent to each of the first portion 1e and the second portion 1g in the X direction. The width W4 of the first portion 1e in the X direction is equal to the width W5 of the second portion 1g in the X direction. The width W6 of the third portion 1h in the X direction is larger (for example, 10 times or more) than the width W4 and the width W5.

[0043] In the irradiation process (S31), the energy of the laser when the first portion 1e or the second portion 1g is located within the laser irradiation region R and the third portion 1h is located outside the irradiation region R is made smaller than the energy of the laser when the third portion 1h is located within the irradiation region R.

[0044] Specifically, the laser energy is set to 0 when the first portion 1e or the second portion 1g is located within the laser irradiation region R and the third portion 1h is located outside the irradiation region R. In this case, the laser energy may be set to a value greater than 0.

[0045] Moreover, when the third portion 1h is located within the irradiation region R, the laser energy is made greater than 0. In detail, when a portion 1i of the third portion 1h, which is a part of the third portion 1h on the second portion 1g side, passes through the irradiation region R, the laser energy is increased from 0 to E. When a portion 1j of the third portion 1h, which is a part of the third portion 1h on the first portion 1e side, passes through the irradiation region R, the laser energy is reduced from E to 0. When a portion 1k of the third portion 1h between the portions 1i and 1j passes through the irradiation region R, the laser energy is fixed at E. In the example shown in FIG. 6, the laser energy is increased (reduced) linearly (linearly), but may be increased (reduced) quadratically.

[0046] The width W7 of the portion 1i in the X direction is equal to the width W8 of the portion 1j in the X direction. Therefore, the time required to increase the laser energy and the time required to decrease the laser energy are equal to each other.

[0047] In the irradiation step (S31), the electrode material 1 is heated to 150° C. or higher by the laser, as shown in FIG. 7. Specifically, the surface temperature of the electrode material 1 reaches 150° C. or higher (for example, about 155° C.) within a few seconds from the start of the laser irradiation. The surface temperature of the electrode material 1 rises and falls repeatedly in short cycles (for example, about 0.1 second cycles), gradually rising over the above few seconds. The surface temperature of the electrode material 1 repeatedly rises and falls in short cycles due to the alternating cooling caused by the suction of the steam V by the steam suction unit 50 and heating caused by the laser irradiation.

[0048] (Evaluation Results) FIG. 8 is a diagram showing the distribution of fluorine components on the surface of the electrode material 1 (opposite the bonding surface between the electrode material 1 and the metal foil 2) (left side of FIG. 8) and the distribution of fluorine components on the bonding surface between the electrode material 1 and the metal foil 2 (right side of FIG. 8). In FIG. 8, the hatched portion indicates the area where the fluorine components are present. As shown in FIG. 8, it was confirmed that the distribution of the fluorine components does not vary significantly (is uniform) for each part of the electrode material 1. Therefore, it was confirmed that the excessive decrease in the adhesion between the electrode material 1 and the metal foil 2 due to the excessive decrease in the amount of fluorine components on the bonding surface between the electrode material 1 and the metal foil 2 was suppressed. In addition, it was confirmed that the excessive bias of the fluorine components on the surface side of the electrode material 1 was suppressed, and therefore the electrical resistance between the above surface and the layer laminated on the above surface was suppressed from becoming excessively large.

[0049] FIG. 9 is a diagram showing the peel strength of the electrode material 1 for each laser scanning speed (0.2 m / s, 0.3 m / s, and 0.5 m / s) and the peel strength (comparative example) when the electrode material 1 is dried in a drying oven. The scanning speed corresponds to the conveying speed of the conveying section 30 in the above embodiment. It was confirmed that the peel strength at each scanning speed was greater than the peel strength in the drying oven. It was also confirmed that the peel strength was greatest when the laser scanning speed was 0.5 m / s, which was the highest. The peel strength means the adhesive strength of the electrode material 1 to the metal foil 2.

[0050] As described above, in this embodiment, the drying step (S30) includes an irradiation step (S31) of drying the electrode material 1 by irradiating the electrode material 1 with a laser when the electrode body 10 (electrode material 1) is transported to position P1, and a suction step (S32) of suctioning the steam V by the steam suction unit 50 provided at position P2. As a result, the steam V generated at position P1 is sucked toward position P2, so that it is possible to prevent the steam V from accumulating at position P1. As a result, it is possible to prevent the steam V from interfering with the laser irradiation of the electrode material 1.

[0051] Furthermore, when a laser is used to dry (heat) the electrode material 1, the temperature of the tool (in this case, the laser irradiation unit 40) itself does not rise, unlike when a heater or the like is used. This eliminates the need to provide a mechanism for cooling the tool (for example, a water-cooling mechanism or an air-cooling mechanism), making it possible to simplify the configuration of the device (facility) and reduce the number of parts.

[0052] Furthermore, when an infrared heater is used to dry the electrode material 1, the infrared heater outputs infrared rays having a wavelength that can be measured by a pyrosensor, making it impossible to measure the temperature of the electrode material 1. In contrast, when a laser is used, the infrared rays described above are not output, making it possible to measure the temperature of the electrode material 1. This allows feedback control based on the measured temperature, making it possible to precisely adjust the temperature of the electrode material 1.

[0053] In the above embodiment, the electrode material 1 is irradiated with a laser at a plurality of positions P1, and the vapor suction unit 50 is provided at a plurality of positions P2, but the present disclosure is not limited to this. The laser may be irradiated at one position P1, and the vapor suction unit 50 may be provided at one position P2 adjacent to the one position P1.

[0054] The configurations described in the above embodiment and the various modified examples may be implemented in any combination.

[0055] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is defined by the claims, not by the description of the embodiments described above, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0056] 1 electrode material, 1d, 1f end (end of electrode material), 1e first portion, 1g second portion, 1h third portion, 2 metal foil (foil portion), 2a surface (surface of metal foil), 2b portion (metal foil portion), 10 electrode body, 30 transport portion, 40 laser irradiation portion, 50 steam suction portion (steam recovery portion), 100 electrode body manufacturing device, P1 position (first position), P2 position (second position), R irradiation area, R1, R2 end (end of irradiation area), R3 center (center of irradiation area), V steam, X direction (transport direction), Y direction (width direction).

Claims

1. a conveying step of conveying the electrode body coated with at least one electrode material by a conveying unit; A drying process of drying the electrode material while transporting the electrode body by the transport unit, The drying step includes: an irradiation step of drying the electrode material by irradiating the electrode material with a laser when the electrode body is transported to at least one first position in a transport direction of the transport section; a recovery process for recovering vapor generated due to the laser being irradiated onto the electrode material by a vapor recovery section provided at at least one second position adjacent to the first position in the transport direction.

2. The electrode body manufacturing method according to claim 1 , wherein the recovery step includes recovering the vapor generated from the electrode material by the vapor recovery section while the electrode material is being irradiated with the laser.

3. the irradiation step is a step of irradiating the electrode material with the laser at each of a plurality of first positions spaced apart from each other in the transport direction; 3. The electrode body manufacturing method according to claim 1, wherein the recovery process is a process of recovering the vapor by the vapor recovery section disposed at each of a plurality of the second positions located between the first positions adjacent to each other in the transport direction.

4. the electrode material includes a first portion near an end portion on one side in the transport direction, a second portion near an end portion on the other side in the transport direction, and a third portion between the first portion and the second portion, 3. The electrode body manufacturing method according to claim 1 or 2, wherein the irradiation process is a process of making the energy of the laser smaller when at least one of the first portion and the second portion is located within an irradiation area of ​​the laser and the third portion is located outside the irradiation area than the energy of the laser when the third portion is located within the irradiation area.

5. 3. The electrode body manufacturing method according to claim 1, wherein the irradiation process is a process of irradiating the electrode material with the laser while aligning the irradiation area of ​​the laser with an arrangement area of ​​the electrode material in a width direction of the conveying section perpendicular to the conveying direction.

6. 6. The electrode body manufacturing method according to claim 5, wherein the irradiation process is a process of irradiating the electrode material with the laser in a state in which the energy of the laser corresponding to the vicinity of both ends in the width direction of the irradiation area is smaller than the energy of the laser corresponding to the center part in the width direction of the irradiation area.

7. 3. The electrode body manufacturing method according to claim 1, wherein the irradiating step is a step of heating the electrode material to 150 degrees or more by the laser.

8. the electrode body includes a foil portion and a plurality of the electrode materials arranged side by side along a predetermined direction on a surface of the foil portion; the conveying step is a step of conveying the electrode body such that the plurality of electrode materials are conveyed side by side along the conveying direction, 3. The electrode body manufacturing method according to claim 1, wherein the irradiation step is a step of setting energy of the laser to zero when a portion of the foil portion between the electrode materials passes through an area irradiated with the laser.

9. A conveying unit that conveys an electrode body coated with at least one electrode material; a laser irradiation unit that irradiates the electrode material with a laser to dry the electrode material when the electrode body is transported to at least one first position in a transport direction of the transport unit; a vapor recovery section provided in at least one second position adjacent to the first position in the transport direction, which recovers vapor generated due to the electrode material being irradiated with the laser.

Citation Information

Patent Citations

  • Manufacture of battery sheet electrode

    JP2000353514A

  • Laser drying method and apparatus therefor

    JP2005342658A

  • Method and device for drying dried object

    JP2006138499A

  • Drying device, and method for manufacturing electrode for secondary battery using the same

    JP2012097917A

  • Drying device and heat treatment system

    JP2012202600A