Hot-pressed parts and hot-pressed steel plates
A controlled Al-Zn-based coating layer with Si, Sr, and Ca addresses the weldability and corrosion resistance issues in hot-pressed members, ensuring excellent performance in automotive applications.
Patent Information
- Application Number
- JP2023550703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-28
- Filing Date
- 2023-06-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-06-13
AI Technical Summary
Conventional hot-pressed members face challenges in achieving both high spot weldability and cut portion corrosion resistance due to issues such as FeAl-based alloy layer incompatibility with chemical conversion coatings, thick oxide layers, and liquid metal embrittlement cracking, which are not adequately addressed by existing Al, Zn, and Al-Zn-based plated steel sheets.
A specific composition of an Al-Zn-based coating layer with controlled amounts of Si, Sr, and Ca is introduced, which suppresses alloying and oxide formation, ensuring a metallic Zn phase remains, thereby enhancing spot weldability and corrosion resistance.
The proposed composition achieves both high spot weldability and cut portion corrosion resistance in hot-pressed members, meeting the requirements for automotive applications.
Smart Images

Figure 0007586336000001 
Figure 0007586336000002 
Figure 0007586336000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-pressed member, and more particularly to a hot-pressed member having excellent corrosion resistance at a cut portion after painting and excellent spot weldability. The present invention also relates to a steel sheet for hot-pressing. [Background technology]
[0002] In order to reduce the weight of automobiles and improve collision safety, the strength of steel sheets for automobiles is being increased. In recent years, cold-rolled steel sheets with a tensile strength of 1500 MPa have been developed and their application is being considered. However, as the strength of steel sheets increases, problems such as poor forming and springback in the press become an issue in terms of dimensional accuracy.
[0003] Therefore, the application of hot pressing technology, which forms steel sheets hot instead of cold, is increasing. Hot pressing is a forming method in which a steel sheet is heated to the austenite temperature range, press-formed while still at a high temperature, and then quenched by contact with a die. In hot pressing, press forming is performed in a state where formability is improved by heating, and the subsequent quenching increases strength, so that hot pressed members with excellent strength can be manufactured with high dimensional accuracy.
[0004] In view of this, steel sheets having coatings such as an Al-based plating layer, a Zn-based plating layer, and an Al-Zn-based plating layer on their surfaces have been proposed as hot-press steel sheets suitable for producing hot-press members (Patent Documents 1 to 5). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-049256 A [Patent Document 2] JP 2003-073774 A [Patent Document 3] JP 2005-113233 A [Patent Document 4] International Publication No. 2017 / 195269 [Patent Document 5] International Publication No. 2019 / 180853 Summary of the Invention [Problem to be solved by the invention]
[0006] The hot-pressed members obtained by hot-pressing the above-mentioned steel plate for hot pressing are mainly used for automobile parts, especially for frame structural members (inner plate frame) that require strength. However, in recent years, they have also been used as so-called quasi-exterior plate members, such as the members around the pillars that can be seen when the door is opened. For this reason, the hot-pressed members are required to be suitable for painting and have excellent corrosion resistance in the cut parts after painting.
[0007] In addition, since hot-pressed members are usually spot-welded before use, they are also required to have excellent spot weldability.
[0008] However, the conventional techniques proposed in Patent Documents 1 to 5 have not been able to satisfy all of the above requirements, as will be explained below.
[0009] For example, in the technology proposed in Patent Document 1, a hot-dip aluminum-plated steel sheet is used as a hot-press steel sheet to prevent scale formation and improve corrosion resistance. However, when an aluminum-plated steel sheet is hot-pressed, Fe diffuses from the base steel sheet to the surface layer of the aluminum plating layer, forming an FeAl-based alloy layer. Generally, a chemical conversion coating is formed on a hot-pressed member before electrocoating to ensure paintability, but since the FeAl-based alloy layer does not react with the chemical conversion solution, a chemical conversion coating cannot be formed. In addition, since the FeAl-based alloy layer does not have sacrificial corrosion protection, corrosion resistance such as corrosion resistance of cut parts is insufficient.
[0010] On the other hand, in the technology proposed in Patent Document 2, a Zn-based plated steel sheet is used as the steel sheet for hot pressing in order to ensure paint adhesion and corrosion resistance. However, when a Zn-based plated steel sheet is hot pressed, a thick oxide layer is formed on the surface of the plated layer, resulting in insufficient spot weldability. In addition, since Zn has a low melting point, liquid metal embrittlement (LME) cracking occurs when a steel sheet having a Zn-based plated layer is hot pressed, and sufficient fatigue resistance cannot be obtained.
[0011] Patent Document 3 proposes improving spot weldability by forming an oxide layer containing Mn on the surface of a Zn-based plated steel sheet. However, Patent Document 3 also uses a plated layer mainly composed of Zn, which results in insufficient fatigue resistance due to LME cracking.
[0012] Therefore, it has been proposed to use Al-Zn plated steel sheets instead of Al plated steel sheets, which have problems with chemical conversion treatability, and Zn plated steel sheets, which have the problem of LME cracking.
[0013] For example, Patent Document 4 proposes that an interface layer of a specific composition is formed at the interface between a base steel sheet and a plating layer by manufacturing a hot-pressed member using an Al-Zn-plated steel sheet. Patent Document 4 claims that providing the interface layer in the hot-pressed member can prevent LME cracking and improve fatigue resistance. However, this hot-pressed member still has insufficient spot weldability and cut corrosion resistance.
[0014] Patent Document 5 claims that by including Mg in an Al-Zn-plated steel sheet and forming a Mg oxide layer during hot pressing, a hot-pressed member can be obtained in which the Zn is not oxidized and the metal Zn phase remains in the coating layer, thereby achieving high corrosion resistance. However, in this hot-pressed member, the Mg oxide layer acts as an insulating film, and therefore sufficient spot weldability cannot be obtained.
[0015] Thus, even with technology using Al-Zn-plated steel sheets, it has not yet been possible to realize hot-pressed members that combine high levels of spot weldability and cut corrosion resistance.
[0016] The present invention has been made in consideration of the above-mentioned circumstances, and aims to achieve a high level of both cut corrosion resistance and spot weldability in a hot-pressed member having an Al-Zn-based coating layer that does not have the chemical conversion treatability problem of Al-plated steel sheets or the LME cracking problem of Zn-based plated steel sheets. [Means for solving the problem]
[0017] As a result of investigations conducted in order to solve the above problems, the present inventors have obtained the following findings.
[0018] (1) By adding a specific amount of Si to an Al-Zn-based plating layer, alloying during heating can be suppressed, and as a result, the spot weldability and cut corrosion resistance of hot-pressed members can be improved.
[0019] (2) When the Al-Zn-based coating layer contains a small amount of Sr or Ca, Sr and Ca are preferentially oxidized to form a surface barrier. As a result, the formation of an oxide layer is suppressed, and the spot weldability of hot-pressed parts is improved. In addition, the oxidation of Zn is suppressed, and it remains as a metallic Zn phase in the coating layer, improving corrosion resistance.
[0020] (3) Therefore, a hot-pressed member obtained using an Al-Zn-plated steel sheet containing specific amounts of Si and at least one of Sr and Ca has both excellent spot weldability and cut corrosion resistance.
[0021] The present invention has been completed based on the above findings, and the gist of the present invention is as follows.
[0022] 1. A steel plate; A coating layer disposed on at least one surface of the steel plate; and an oxide layer disposed on the coating layer, The coating layer comprises, in mass %, Zn: 25.0-55.0%, Si: 1.1-8.0%, Sr+Ca: 0.01-5.0%, and Fe: 55.0% or less; The balance is Al and unavoidable impurities, and A hot-pressed member comprising a metallic Zn phase in the coating layer.
[0023] 2. The hot-pressed member according to claim 1, wherein the oxide layer has a thickness of 0.3 μm or less.
[0024] 3. Steel plate; A hot press steel sheet having a plating layer disposed on at least one surface of the steel sheet, The plating layer comprises, in mass %, Zn: 30.0-70.0%, Si: 1.1-8.0%, Sr+Ca: 0.01 to 5.0%; The remainder of the composition of the steel sheet for hot pressing is Al and unavoidable impurities. Effect of the Invention
[0025] According to the present invention, it is possible to provide a hot-pressed member having both high levels of cut corrosion resistance and spot weldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present invention will be described. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited by the following description. In addition, the unit of content, "%", represents "mass %" unless otherwise specified.
[0027] (1) Hot-pressed parts A hot-pressed member according to an embodiment of the present invention includes a steel plate, a coating layer disposed on at least one surface of the steel plate, and an oxide layer disposed on the coating layer. Each part will be described below.
[0028] [Steel plate] In the present invention, the above-mentioned problem is solved by controlling the component composition of the coating layer as described below, and then making the coating layer contain a metallic Zn phase. Therefore, the steel sheet is not particularly limited and any steel sheet can be used.
[0029] The hot-pressed member of the present invention is manufactured by hot pressing a steel plate for hot pressing as described later. Therefore, the steel plate can be said to be a steel plate formed by hot pressing. The steel plate may be either a cold-rolled steel plate or a hot-rolled steel plate.
[0030] From the viewpoint of using the hot-pressed member as an automobile member, etc., it is preferable that the hot-pressed member has high strength. In particular, in order to obtain a hot-pressed member having a strength of more than 1470 MPa, it is preferable to use a steel material having the following composition.
[0031] C: 0.20-0.35%, Si: 0.1 to 0.5%, Mn: 1.0-3.0%, P: 0.02% or less, S: 0.01% or less, Al: 0.1% or less, and N: Contains 0.01% or less, The balance consists of Fe and unavoidable impurities.
[0032] The effects and preferred contents of each element in the above-mentioned preferred composition will be described below.
[0033] C: 0.20-0.35% C is an element that improves strength by forming a structure such as martensite. From the viewpoint of obtaining a strength exceeding 1470 MPa, the C content is preferably 0.20% or more. On the other hand, if the C content exceeds 0.35%, the toughness of the spot welds deteriorates. Therefore, the C content is preferably 0.35% or less.
[0034] Silicon: 0.1 to 0.5% Silicon is an effective element for strengthening steel to obtain good material properties. In order to obtain the above effect, the silicon content is preferably 0.1% or more. On the other hand, if the silicon content exceeds 0.5%, ferrite is stabilized, and hardenability is reduced. Therefore, the silicon content is preferably 0.5% or less.
[0035] Mn: 1.0-3.0% Mn is an element that is effective in increasing the strength of steel. From the viewpoint of ensuring excellent mechanical properties and strength, the Mn content is preferably 1.0% or more. On the other hand, if the Mn content exceeds 3.0%, the amount of Mn that concentrates on the steel sheet surface during annealing increases, resulting in a decrease in coating adhesion. Therefore, the Mn content is preferably 3.0% or less.
[0036] P:0.02% or less If the P content is higher than 0.02%, local ductility is deteriorated due to grain boundary embrittlement caused by P segregation to the austenite grain boundaries during casting. As a result, the balance between the strength and ductility of the steel sheet is deteriorated. Therefore, from the viewpoint of improving the balance between the strength and ductility of the steel sheet, it is preferable that the P content is 0.02% or less. On the other hand, from the above viewpoint, the lower the P content, the better, so the lower limit of the P content is not particularly limited and may be 0%, but from the viewpoint of refining costs, it is preferable that the P content is 0.0005% or more.
[0037] S: 0.01% or less S becomes inclusions such as MnS, which causes deterioration of impact resistance and cracks along the metal flow of the weld. Therefore, it is desirable to reduce the S content as much as possible, and specifically, it is preferable to set it to 0.01% or less. From the viewpoint of ensuring good stretch flangeability, it is more preferable to set it to 0.005% or less. On the other hand, from the above viewpoint, the lower the S content, the better, so the lower limit of the S content is not particularly limited and may be 0%, but from the viewpoint of refining costs, it is preferable to set the S content to 0.0002% or more.
[0038] Al: 0.1% or less Al is an element that acts as a deoxidizer. However, if the Al content exceeds 0.1%, the hardenability decreases. Therefore, the Al content is preferably 0.1% or less. On the other hand, although there is no particular lower limit for the Al content, from the viewpoint of enhancing the effect as a deoxidizer, the Al content is preferably 0.01% or more.
[0039] N: 0.01% or less If the N content exceeds 0.01%, AlN is generated during heating before hot pressing, and hardenability is reduced. Therefore, the N content is preferably 0.01% or less. On the other hand, although there is no particular lower limit for the N content, from the viewpoint of refining costs, the N content is preferably 0.001% or more.
[0040] The above component composition may further include, optionally, Nb: 0.05% or less, Ti: 0.05% or less, B: 0.0002~0.0050%, Cr: 0.1-0.3%, and Sb: 0.003 to 0.03% The composition may contain at least one selected from the group consisting of:
[0041] Nb: 0.05% or less Nb is an effective component for strengthening steel, but if it is contained in excess, shape fixability decreases. Therefore, when Nb is contained, the Nb content is preferably 0.05% or less. On the other hand, the lower limit of the Nb content is not particularly limited and may be 0%, but from the viewpoint of the strength improvement effect, the Nb content is preferably 0.005% or more.
[0042] Ti: 0.05% or less Ti, like Nb, is an effective component for strengthening steel, but if it is contained in excess, shape fixability decreases. Therefore, when Ti is added, the Ti content is preferably 0.05% or less. On the other hand, the lower limit of the Ti content is not particularly limited and may be 0%, but from the viewpoint of the strength improvement effect, the Ti content is preferably 0.005% or more.
[0043] B: 0.0002~0.0050% B has the effect of suppressing the formation and growth of ferrite from the austenite grain boundaries. When B is added, the B content is preferably 0.0002% or more in order to obtain the above effect. On the other hand, excessive addition of B reduces formability. Therefore, when B is added, the B content is preferably 0.0050% or less.
[0044] Cr: 0.1-0.3% Cr is an element useful for strengthening steel and improving hardenability. When Cr is added, the Cr content is preferably 0.1% or more in order to obtain the above effect. On the other hand, since Cr is an expensive element, adding excessive Cr leads to a significant increase in cost. Therefore, when Cr is added, it is more preferable that the Cr content is 0.3% or less.
[0045] Sb: 0.003 to 0.03% Sb is an element that has the effect of suppressing decarburization of the surface layer of a steel sheet during hot pressing. When Sb is added, the Sb content is preferably 0.003% or more in order to obtain the above effect. On the other hand, when the Sb content exceeds 0.03%, the rolling load increases, and the productivity decreases. Therefore, when Sb is added, the Sb content is preferably 0.03% or less.
[0046] [Coating layer] The hot-pressed member of the present invention has a coating layer on at least one surface of the steel plate. The coating layer may be provided on only one surface of the steel plate, but is preferably provided on both surfaces.
[0047] The hot-pressed member of the present invention contains a metallic Zn phase in the coating layer. In a corrosive environment, this metallic Zn phase exerts a sacrificial anticorrosive effect, thereby obtaining high corrosion resistance. If Zn exists only in a solid solution state in the coating layer, the desired corrosion resistance cannot be obtained, so it is necessary for Zn to exist as a metallic Zn phase in the coating layer. The presence or absence of a metallic Zn phase in the coating layer can be evaluated by X-ray diffraction.
[0048] The coating layer has a composition containing at least one of Zn, Si, Sr and Ca, Fe in specific amounts, with the remainder being Al and unavoidable impurities. Each component will be described below.
[0049] Zn: 25.0-55.0% If the Zn content of the coating layer is less than 25.0%, the coating layer does not contain a metal Zn phase, and the desired corrosion resistance of the cut portion cannot be obtained. Therefore, the Zn content is set to 25.0% or more. If the Zn content is 30.0% or more, a larger amount of metal Zn phase is present in the coating layer, and the corrosion resistance of the cut portion is further improved. Therefore, the Zn content is preferably set to 30.0% or more. On the other hand, if the Zn content exceeds 55.0%, the amount of Zn oxide generated increases, and the desired spot weldability cannot be obtained. Therefore, the Zn content is set to 55.0% or less, preferably 50.0% or less.
[0050] Si: 1.1-8.0% Si is an element that has the effect of suppressing alloying of the plating layer in the plating process and the heat treatment process before hot pressing. Here, it is known that Zn in the plating layer is pushed out to the surface layer as Fe diffuses into the plating layer in the heat treatment process. In other words, if the alloying of the plating layer progresses excessively, Zn forms an oxide layer before Sr and Ca oxidize and form a surface barrier. As a result, the desired weldability cannot be obtained, and the Zn in the coating layer decreases, decreasing the corrosion resistance. Therefore, the Si content in the finally obtained coating layer is set to 1.1% or more, preferably 1.3% or more. On the other hand, if the Si content is excessive, the amount of Si-based oxides produced increases, resulting in impaired chemical conversion treatability and inferior corrosion resistance. Therefore, the Si content is set to 8.0% or less, preferably 4.0% or less.
[0051] Sr+Ca: 0.01-5.0% Sr and Ca are elements that have the effect of improving weldability by suppressing the formation of an oxide layer. That is, Sr and Ca are preferentially oxidized to form a surface barrier, and as a result, the formation of an oxide layer is suppressed and weldability is improved. Furthermore, by suppressing the formation of an oxide layer, Zn contained in the coating layer is not oxidized and remains in the coating layer, thereby improving corrosion resistance. Therefore, in the present invention, it is important that the coating layer contains one or both of Sr and Ca. However, if the total content of Sr and Ca is less than 0.01%, the desired effect cannot be obtained. Therefore, the total content of Sr and Ca is set to 0.01% or more, preferably 0.1% or more. On the other hand, if the content of Sr and Ca is excessive, the oxides of Sr and Ca themselves are excessively generated, resulting in deterioration of spot weldability. Therefore, the total content of Sr and Ca is set to 5.0% or less, preferably 1.0% or less. In the present invention, the total content of Sr and Ca is represented as "Sr+Ca".
[0052] Fe:55.0% or less Since Fe diffuses from the steel sheet to the plating layer due to heating before hot pressing, Fe is inevitably contained in the coating layer of the hot pressed member. However, as the Fe content increases, the solid solubility limit of Zn in the coating layer decreases, so Zn concentrates on the surface layer of the coating layer. As a result, Zn oxide is excessively formed, and weldability deteriorates. Therefore, the Fe content is set to 55.0% or less, preferably 50.0% or less. On the other hand, the lower limit of the Fe content is not particularly limited, but when manufactured under general conditions, the Fe content may be 20.0% or more.
[0053] The component composition of the coating layer can be measured by SEM (scanning electron microscope)-EDX (energy dispersive X-ray analysis).
[0054] The coating weight of the coating layer is not particularly limited, but from the viewpoint of corrosion resistance, the coating weight is set to 60 g / m per one side of the steel sheet. 2 On the other hand, from the viewpoint of production costs, the coating amount is preferably 400 g / m per one side of the steel sheet. 2 The coating layer adhesion amount can be determined by dissolving and removing the coating layer from the surface of the hot-pressed part using an acid solution, and subtracting the weight of the hot-pressed part after removal from the weight of the hot-pressed part before removal. An inhibitor that inhibits dissolution of the base steel sheet is added to the acid solution.
[0055] [Oxide layer] When a steel sheet for hot pressing is subjected to hot pressing, Fe in the base steel diffuses into the plating layer to form the above-mentioned coating layer, and at the same time, the components in the plating layer combine with oxygen present in the heating atmosphere to form an oxide layer on the surface of the coating layer.
[0056] The thickness of the oxide layer is not particularly limited. However, since the oxide layer is insulating, if the oxide layer is excessively thick, the spot weldability may be reduced. Therefore, from the viewpoint of further improving the spot weldability, it is preferable to set the thickness of the oxide layer to 0.6 μm or less. In addition, if the thickness of the oxide layer is sufficiently thin, the oxide layer can be destroyed by the pressure of the electrode during spot welding, so that the spot weldability is further improved. From the above viewpoint, it is more preferable to set the thickness of the oxide layer to 0.3 μm or less. On the other hand, from the viewpoint of spot weldability, the thinner the oxide layer, the better, so the lower limit of the thickness of the oxide layer is not particularly limited and may be 0 μm.
[0057] The thickness of the oxide layer can be measured by observing the cross section of the hot-pressed member using a SEM.
[0058] (2) Steel sheets for hot pressing A steel sheet for hot press use in one embodiment of the present invention comprises a steel sheet and a plating layer disposed on at least one surface of the steel sheet.
[0059] [Steel plate] The steel plate is not particularly limited and any steel plate can be used. The steel plate may be either a cold-rolled steel plate or a hot-rolled steel plate. The composition of the steel plate is not particularly limited, but it is preferable to use a steel plate having the composition described in the description of the hot-pressed member.
[0060] [Plating layer] The steel sheet for hot press use of the present invention has a plating layer on at least one surface of the steel sheet. The plating layer may be provided on only one surface of the steel sheet, but is preferably provided on both surfaces.
[0061] In order for the composition of the coating layer after hot pressing to satisfy the above-mentioned conditions, the plating layer of the steel sheet for hot pressing needs to have the following component composition. Zn: 30.0-70.0%, Si: 1.1 to 8.0%, and Sr+Ca: 0.01-5.0% The balance is Al and unavoidable impurities.
[0062] Here, the Zn content of the plating layer is preferably 35.0% or more. Meanwhile, the Zn content is preferably 65.0% or less. Furthermore, the Si content of the plating layer is preferably 1.3% or more. Meanwhile, the Si content is preferably 4.0% or less. Furthermore, the Sr+Ca content of the plating layer is preferably 0.1% or more. Meanwhile, the Sr+Ca content is preferably 1.0% or less.
[0063] That is, the plating layer is Zn: 35.0-65.0%, Si: 1.3-4.0%, and Sr+Ca: 0.1-1.0% It is preferable that the balance of the composition be Al and unavoidable impurities.
[0064] As in the composition of the coating layer, the total content of Sr and Ca in the composition of the plating layer is represented as "Sr+Ca."
[0065] The component composition of the plating layer can be measured by SEM (scanning electron microscope)-EDX (energy dispersive X-ray analysis).
[0066] The plating layer is not particularly limited and may be formed by any method, but is preferably formed by a hot-dip plating method, in other words, the plating layer is preferably a hot-dip plating layer.
[0067] The coating weight of the plating layer is not particularly limited, but from the viewpoint of corrosion resistance, the coating weight is set to 30 g / m per one side of the steel sheet. 2 On the other hand, from the viewpoint of production costs, the coating amount is preferably 200 g / m per one side of the steel sheet. 2The coating weight of the plating layer can be determined by dissolving and removing the plating layer from the surface of the steel sheet for hot press use using an acid solution, and subtracting the weight of the steel sheet for hot press use after removal from the weight of the steel sheet for hot press use before removal. An inhibitor that inhibits dissolution of the base steel sheet is added to the acid solution.
[0068] (3) Manufacturing method of hot-pressed parts Next, a preferred method for producing the hot-pressed member of the present invention will be described.
[0069] The hot-pressed member of the present invention can be produced by hot-pressing a steel plate for hot press that satisfies the above conditions.
[0070] The method of hot pressing is not particularly limited, and can be performed according to a conventional method. Typically, the steel sheet for hot pressing is heated to a predetermined heating temperature (heat treatment step), and then the steel sheet for hot pressing heated in the heat treatment step is hot pressed (hot pressing step). Preferred hot pressing conditions are described below.
[0071] [Heat treatment] In the heat treatment process, the hot press steel sheet is heated to a heating temperature of the Ac3 transformation point or higher and 980°C or lower. By setting the heating temperature to the Ac3 transformation point or higher, the structure of the steel sheet can be austenitized. The austenite becomes a hard phase such as a martensite phase by subsequent quenching during hot pressing, and as a result, the hot press member can be made high-strength. If the heating temperature is lower than the Ac3 transformation point, the austenite fraction in the heated steel sheet decreases, so that the volume fraction of martensite becomes insufficient after hot pressing, and sufficient tensile strength cannot be ensured. On the other hand, if the heating temperature is higher than 980°C, the alloying of the plating layer may proceed excessively, resulting in an excessive Fe content in the coating layer, and even if the Fe content is not excessive, the oxidation of Zn proceeds excessively, making it impossible to retain the metal Zn phase in the coating layer. Therefore, a hot press member that satisfies the conditions of the present invention cannot be obtained. In addition, if the heating temperature is higher than 980°C, a thick oxide layer is formed, and further, the crystal grain size becomes excessively coarse, resulting in a decrease in bending crushability.
[0072] The Ac3 transformation point can be calculated by the following formula (1). Ac3 transformation point (℃) = 881-206C + 53Si-15Mn-20Ni-1Cr-27Cu + 41Mo…(1) In formula (1), the element symbols represent the content (mass%) of each element. The content of elements that are not contained is set to 0 in the calculation. For example, if Ni, Cu, and Mo are not contained, the following formula (2) can be used. Ac3 transformation point (℃) = 881-206C + 53Si-15Mn-1Cr…(2) In the formula (2), the element symbols represent the content (mass%) of each element. The content of elements that are not contained is calculated as 0.
[0073] In the heat treatment process, the steel sheet may be heated to the heating temperature and then held at the heating temperature. The holding time at the heating temperature is not particularly limited, but if the holding time is longer than 5 minutes, the alloying of the plating layer proceeds excessively, the Fe content of the coating layer becomes excessive, and the hot press member satisfying the conditions of the present invention may not be obtained, and in addition, the thickness of the oxide layer becomes excessive. Therefore, the holding time is preferably 5 minutes or less. On the other hand, since the holding is an optional process, the holding time may be 0 seconds. However, from the viewpoint of homogeneously austenitizing the base steel sheet, the holding time is preferably 10 seconds or more.
[0074] The method of heating the steel sheet for hot pressing in the heat treatment step is not particularly limited, and any method can be used. The heating can be performed, for example, by heating in a heating furnace, electric heating, induction heating, high-frequency heating, flame heating, etc. As the heating furnace, any heating furnace can be used, such as an electric furnace or a gas furnace.
[0075] [Hot press] After the above heating, the hot press steel plate is hot pressed to obtain a hot press member. In the hot press, cooling is performed using a mold or a coolant such as water at the same time as or immediately after processing. In the present invention, the hot press conditions are not particularly limited. For example, pressing can be performed at a general hot press temperature range of 600 to 800°C. EXAMPLES
[0076] In order to confirm the effects of the present invention, a steel plate for hot press use and a hot press member using the steel plate for hot press use were produced, and the properties thereof were evaluated.
[0077] ·Steel plates for hot pressing A plating layer was formed on the surface of a steel sheet by the following procedure to obtain a steel sheet for hot pressing. Specifically, a plating layer was formed on both sides of a steel sheet with a thickness of 1.4 mm by a continuous hot-dip plating facility. As the steel sheet, a cold-rolled steel sheet was used having a composition containing C: 0.24%, Si: 0.25%, Mn: 1.3%, P: 0.01%, S: 0.002%, Al: 0.03%, N: 0.005%, Cr: 0.16%, Ti: 0.03%, B: 0.002%, and Sb: 0.008%, with the balance being Fe and unavoidable impurities. The Ac3 transformation point of the cold-rolled steel sheet is 825°C. The temperature of the plating bath is 600°C, and the coating weight of the plating layer is 100 g / m2 per side of the steel sheet. 2 , i.e. 200 g / m2 on both sides 2 It was decided.
[0078] (Composition of plating layer) The component composition of the obtained plating layer was measured by area analysis using SEM (scanning electron microscope)-EDX (energy dispersive X-ray analysis). In the SEM-EDX analysis, a JEOL SEM (JSM-7200F) and a Thermo Fisher EDX detector (UltraDry) were used, and the analysis was performed at an acceleration voltage of 15.0 kV. The results are shown in Tables 1 and 2.
[0079] Hot press parts Next, the obtained steel sheets for hot pressing were each subjected to hot pressing under the conditions shown in Tables 3 and 4 to obtain hot pressed members. Specifically, the steel sheets for hot pressing were first cut into a size of 70 mm x 150 mm and subjected to heat treatment in an electric furnace. The heating temperature and the holding time at the heating temperature in the heat treatment were as shown in Tables 3 and 4. Next, the steel sheets for hot pressing were taken out of the electric furnace and hot pressed using a flat die. The forming start temperature was 700°C.
[0080] Next, the presence or absence of a metallic Zn phase, the component composition of the coating layer, and the thickness of the oxide layer were evaluated for each of the obtained hot-pressed members by the following procedures. The measurement results are shown in Tables 3 and 4.
[0081] (metallic Zn phase) The presence or absence of a metallic Zn phase in the coating layer was determined by X-ray diffraction. The analysis was performed using a SmartLab manufactured by Rigaku Corporation, with X-ray used: Cu-Kα, tube voltage: 40 kV, tube current: 30 mA, and scanning speed: 4° / min.
[0082] (Component composition of coating layer) The component composition of the coating layer was measured by area analysis using SEM-EDX. The SEM-EDX analysis was performed using a JEOL SEM (JSM-7200F) and a Thermo Fisher EDX detector (UltraDry) at an acceleration voltage of 15.0 kV.
[0083] (Oxide layer thickness) A test piece for cross-sectional observation was taken from the flat part of the top surface of the hot-pressed part, and the thickness of the oxide layer was measured by cross-sectional observation. Specifically, the cross section of the surface of the hot-pressed part was observed at a magnification of 500 times using an SEM, and the thickness of the oxide layer was measured at 20 random locations, and the average value was taken as the oxide layer thickness.
[0084] Next, the spot weldability and cut corrosion resistance of each of the hot-pressed members obtained were evaluated by the following procedure. The measurement results are shown in Tables 3 and 4.
[0085] (Spot weldability) Two test pieces taken from the obtained hot pressed members were stacked together and subjected to resistance spot welding. For the resistance spot welding, an AC spot welding machine was used equipped with a DR type electrode (chromium copper) with a curved tip diameter of 6 mm and a curved tip curvature radius (tip R) of 40 mm. The shape of the test piece was a rectangular shape of 30 × 50 mm, and the pressure was 3.5 kN. Resistance spot welding was performed by changing the current value from 4 kA to the current value at which dust was generated, and the nugget diameter was 4t 1 / 2 The optimum current range was determined as the range from the current value at which the welded joint was 1.0 mm (t = plate thickness) to the current value at which dust was generated. The wider the optimum current range, the better the spot weldability. Here, it was determined that an optimum current range of 1.0 kA or more was sufficient.
[0086] (Corrosion resistance of cut parts) A test piece for evaluating corrosion resistance was prepared by subjecting a test piece taken from the hot pressed member to a phosphoric acid-based conversion treatment and an electrocoating. A cross-cut scratch (angle 60°) of 80 mm in length and 160 mm in total was made in the center of the test piece for evaluating corrosion resistance, and then the test piece was subjected to a corrosion test (SAE-J2334). Based on the occurrence of red rust after 30 cycles, the corrosion resistance of the cut part was evaluated according to the following criteria. Score 4: No red rust on cut areas Score 3: The length of the cut scratch where red rust has occurred is less than 2 mm Grade 2: The length of the cut scratch where red rust has occurred is 2mm or more but less than 4mm Score 1: The length of the cut scratch where red rust has occurred is 4 mm or more Here, a rating of 3 or more was deemed to indicate sufficient cut corrosion resistance.
[0087] As can be seen from the results shown in Tables 3 and 4, the hot-pressed members satisfying the conditions of the present invention had both excellent spot weldability and corrosion resistance at the cut portions.
[0088] [Table 1]
[0089]
Table 2
[0090]
Table 3
[0091]
Table 4
Claims
1. A steel plate, A coating layer disposed on at least one surface of the steel plate; and an oxide layer disposed on the coating layer, The coating layer comprises, in mass %, Zn: 25.0 to 55.0%, Si: 1.1-8.0%, Sr: 0.01 to 5.0%, and Fe: 55.0% or less; The balance is Al and unavoidable impurities, and A hot-pressed member comprising a metallic Zn phase in the coating layer.
2. 2. The hot pressed part of claim 1, wherein the oxide layer has a thickness of 0.3 μm or less.
3. A steel plate, A hot press steel sheet having a plating layer disposed on at least one surface of the steel sheet, The plating layer comprises, in mass %, Zn: 30.0-70.0%, Si: 1.1-8.0%, Sr: 0.01 to 5.0%; The balance of the composition of the steel sheet for hot pressing is Al and unavoidable impurities.
Citation Information
Patent Citations
High-strength aluminum-plated steel sheet with superior weldability and corrosion resistance after coating for automobile, and automotive member using it
JP2003049256A
Plated steel sheet for hot press
JP2003073774A
Zn-BASED PLATED STEEL FOR HOT PRESS
JP2005113233A
Plated steel sheet for hot press, method for manufacturing hot-pressed member using the same, and hot-pressed member
JP2012112010A
JPP7156573B