Polyphenylene sulfide resin composition for battery insulating member, and battery insulating member

A PPS resin composition combining polyphenylene sulfide with a crosslinked silicone elastomer addresses the issues of reduced flame retardancy and durability in existing PPS blends, ensuring safety and reliability in battery insulation materials by maintaining mechanical properties and insulation under high temperatures.

JP7586347B2Active Publication Date: 2024-11-19TORAY INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023571277
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-06-22
Filing Date
2023-11-09
Publication Date
2024-11-19
Estimated Expiration
2043-11-09

AI Technical Summary

Technical Problem

Existing polyphenylene sulfide (PPS) resin compositions for battery insulation materials face issues with reduced flame retardancy and long-term durability when blended with olefin elastomers or silicone compounds, leading to decreased safety and reliability in high-temperature environments, and inorganic powders compromise productivity.

Method used

A PPS resin composition is developed by blending polyphenylene sulfide resin with a silicone elastomer having a crosslinked structure, excluding thermoplastic elastomers, to achieve a balance of safety, long-term reliability, and productivity, with specific properties such as bending modulus, flame retardancy, and tensile elongation.

Benefits of technology

The composition exhibits excellent flame retardancy, long-term durability, and toughness, maintaining mechanical integrity and insulation properties under high temperatures, thus enhancing the safety and reliability of battery insulation members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586347000001
    Figure 0007586347000001
  • Figure 0007586347000002
    Figure 0007586347000002
  • Figure 0007586347000003
    Figure 0007586347000003
Patent Text Reader

Abstract

Provided is a polyphenylene sulfide resin composition for a battery insulation member, the resin composition being formed by blending (a) a polyphenylene sulfide resin and (b) a silicone elastomer having a cross-linked structure, wherein 0.1-15.0 parts by weight of the (b) silicone elastomer having a cross-linked structure is blended with 100 parts by weight of the (a) polyphenylene sulfide resin, and a test specimen obtained by injection molding the resin composition has a bending modulus of 3.1-3.6 GPa in a bending test in accordance with ISO178 (2010). According to the present invention, obtainable are: a polyphenylene sulfide resin composition for a battery insulation member; and a battery insulation member, which have excellent productivity, safety, and long-term reliability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyphenylene sulfide resin composition for battery insulating members, which has excellent productivity, safety, and long-term reliability, and to a battery insulating member. [Background technology]

[0002] As awareness of global environmental protection increases, 2 Electric vehicles, which can reduce emissions, and secondary batteries for home use, which are designed to efficiently utilize surplus electricity at night, are becoming more and more popular, and there is a demand for further efficiency improvements in storage batteries used in vehicles and stationary housing.

[0003] Polyphenylene sulfide (hereinafter sometimes abbreviated as PPS) resin is a super engineering plastic with a good balance of heat resistance, chemical resistance, flame retardancy, etc. Due to its cost advantage over other super engineering plastics, PPS resin is a highly versatile resin material second only to the five major engineering plastics, and is used in a wide range of applications such as automobiles, housing equipment, and electrical and electronic applications, and its application to various battery components is also being considered.

[0004] Patent Document 1 discloses a PPS resin composition containing an olefin-based elastomer, a type of thermoplastic elastomer, and a gasket for secondary batteries made of the same. By compounding the olefin-based elastomer, which is a material that is flexible relative to PPS resin, this PPS resin composition has been able to achieve improved resistance to moist heat and electrolyte, and improved compressive stress relaxation properties under a certain strain, and this PPS resin composition is applied to gaskets for secondary batteries.

[0005] Patent Document 2 discloses a PPS resin composition that is intended for use as an electrode insulating sealant for lithium batteries and the like, and that has excellent high-temperature compression creep properties and high weld strength imparted by adding silicone oil as a silane compound to the PPS resin.

[0006] In addition, in Patent Document 3, by adding inorganic powder carrying silicone oil as a silicone compound to PPS resin, it is possible to improve the moist heat resistance, electrolyte resistance, and compressive stress relaxation property under a certain strain, and this PPS resin composition is applied to gaskets for secondary batteries. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-29167 A [Patent Document 2] JP 2001-2920 A [Patent Document 3] JP 2011-29166 A Summary of the Invention [Problem to be solved by the invention]

[0008] Lithium-ion batteries and other storage batteries used in vehicles and stationary housing have a problem of deteriorating battery performance due to the heat effect in the usage environment. Therefore, in battery development, attention is being paid to the long-term reliability and degradation suppression of materials used in battery components from the viewpoint of lifetime management during long-term use of batteries. Specifically, it is expected that the long-term reliability of batteries will be improved by improving bleed-out resistance, physical property retention, and creep resistance during long-term high-temperature use. In addition, from the viewpoint of productivity of battery components, the toughness of the material is important to suppress damage to insulating materials during crimping in the battery manufacturing process. In addition, from the viewpoint of battery safety, it is expected that the flame retardancy of battery components will be improved.

[0009] However, the present inventors have evaluated the flame retardancy of a resin composition consisting of PPS resin and an olefin-based elastomer described in Patent Document 1, and found that the flame retardancy of the resin composition is significantly lower than that of the PPS resin alone. It is believed that the flame retardancy of the composition is reduced by blending an olefin-based elastomer, which has significantly inferior flame retardancy, while the PPS resin alone has high flame retardancy. In addition, the inventors have evaluated the toughness retention rate before and after long-term high-temperature treatment, and found that the retention rate is significantly reduced. While this composition has the advantages of flexibility and toughness, it does not exhibit the excellent flame retardancy and long-term high-temperature durability inherent to PPS resin, so that when used for battery applications, it has the problem of reduced safety and long-term reliability.

[0010] The present inventors have evaluated the long-term high-temperature durability of the PPS resin composition obtained by adding silicone oil to the PPS resin described in Patent Document 2, and found that, compared to the PPS resin alone, bleed-out components that are thought to be derived from the silicone oil components are generated on the surface of the molded article after processing. When this resin composition is applied to battery components, there is a concern that the generation of bleed-out components from the surface of the molded article will not only lead to a decrease in insulation properties but also to a decrease in the power generation efficiency of the battery, which is undesirable.

[0011] Furthermore, in the PPS resin composition described in Patent Document 3, in which a component in which silicone oil is supported on inorganic powder is added to the PPS resin, the addition of inorganic powder makes it impossible to achieve the toughness required for battery insulating materials, and undesirably leads to reduced productivity and long-term reliability of the battery materials.

[0012] Therefore, an object of the present invention is to obtain a polyphenylene sulfide resin composition for use in battery insulating members that combines excellent productivity, safety, and long-term reliability. [Means for solving the problem]

[0013] As a result of investigations to solve such problems, the present inventors have found that by blending (a) a polyphenylene sulfide resin and (b) a silicone elastomer having a crosslinked structure in a specific composition to obtain a polyphenylene sulfide resin composition having a flexural modulus of 3.1 GPa to 3.6 GPa, and using the composition for use as an insulating member for a battery, the resin composition has excellent productivity while also having properties of safety and long-term reliability. That is, the present invention has been made to solve at least a part of the above-mentioned problems, and can be carried out in the following forms. (1) A polyphenylene sulfide resin composition for use in battery insulating members, comprising (a) a polyphenylene sulfide resin and (b) a silicone elastomer having a crosslinked structure, the composition comprising 0.1 to 15.0 parts by weight of the silicone elastomer having a crosslinked structure per 100 parts by weight of the polyphenylene sulfide resin (a), the resin composition being injection molded into a test piece, which has a flexural modulus of 3.1 GPa or more and 3.6 GPa or less in a bending test in accordance with ISO178 (2010). (2) The polyphenylene sulfide resin composition for battery insulating members according to (1), wherein the resin composition is substantially free of (c) a thermoplastic elastomer. (3) The polyphenylene sulfide resin composition for battery insulating members according to (1) or (2), wherein, in a measurement according to the UL94 standard of a test piece obtained by injection molding the resin composition, the flame retardancy of the test piece having a thickness of 1.0 mmt or less is V-0. (4) The polyphenylene sulfide resin composition for battery insulating members according to any one of (1) to (3), wherein a test piece obtained by injection molding the resin composition has a tensile elongation at break of 8% or more in a tensile test according to ISO 527-1, 2 (2012). (5) The polyphenylene sulfide resin composition for battery insulating members according to any one of (1) to (4), wherein the (b) silicone elastomer having a crosslinked structure is a fine particle having an average primary particle diameter of 100 nm to 10 μm. (6) The polyphenylene sulfide resin composition for battery insulating members according to any one of (1) to (5), wherein the (b) silicone elastomer having a crosslinked structure has a Shore hardness A of 60 HS or less. (7) A polyphenylene sulfide resin composition for use in insulating members of a battery according to any one of (1) to (6), wherein the silicone elastomer having a crosslinked structure (b) contains 90% by weight or more of structural units derived from organopolysiloxane. (8) A battery insulating member, comprising the polyphenylene sulfide resin composition for battery insulating members according to any one of (1) to (7). Effect of the Invention

[0014] According to the present invention, it is possible to obtain a polyphenylene sulfide resin composition for battery insulating members, and a battery insulating member, which have excellent productivity, safety, and long-term reliability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described in detail.

[0016] (1)(a) Polyphenylene sulfide resin The polyphenylene sulfide resin (a) used in the present invention is a polymer having a repeating unit represented by the following structural formula:

[0017] [ka]

[0018] From the viewpoint of heat resistance, it is preferable for the polymer to contain 70 mol % or more, and more preferably 90 mol % or more, of the repeating unit represented by the above structural formula. In addition, about 30 mol % or less of the repeating units of the (a) PPS resin may be composed of repeating units having the following structure.

[0019] [ka]

[0020] A PPS copolymer partially having such a structure has a melting point lower than the general melting point of PPS, 280° C., and therefore such a resin composition is advantageous in terms of moldability.

[0021] There is no particular restriction on the weight average molecular weight of the (a) PPS resin used in the present invention, but in terms of obtaining better mechanical properties, the weight average molecular weight is preferably 30,000 to 150,000, more preferably 40,000 to 130,000, more preferably 45,000 to 110,000, and more preferably 50,000 to 90,000. If the weight average molecular weight is small, the mechanical properties of the PPS resin itself will decrease, and components will break during the crimping and fitting process during the manufacture of battery components, so 30,000 or more is preferable. Also, from the viewpoint of flame retardancy, if the weight average molecular weight is small, dripping will occur during flame retardancy testing and flame retardancy will decrease due to surface renewal (reappearance of combustible components on the surface due to dripping), so 30,000 or more is preferable. On the other hand, if the weight average molecular weight exceeds 150,000, the melt viscosity will increase significantly, which tends to be undesirable in molding processing. Also, in the present invention, a mixture of multiple (a) PPS resins with different weight average molecular weights may be used.

[0022] The weight average molecular weight in the present invention is a value calculated in terms of polystyrene using a gel permeation chromatography (GPC) manufactured by Senshu Scientific.

[0023] A method for producing the (a) PPS resin used in the present invention will be described below, but the method is not limited to the method described below as long as the (a) PPS resin having the above-mentioned properties can be obtained.

[0024] First, the polyhalogenated aromatic compound, sulfidizing agent, polymerization solvent, molecular weight regulator, polymerization aid and polymerization stabilizer used in the production method will be described.

[0025] [Polyhalogenated aromatic compounds] Polyhalogenated aromatic compounds refer to compounds having two or more halogen atoms in one molecule. Specific examples include polyhalogenated aromatic compounds such as p-dichlorobenzene, m-dichlorobenzene, o-dichlorobenzene, 1,3,5-trichlorobenzene, 1,2,4-trichlorobenzene, 1,2,4,5-tetrachlorobenzene, hexachlorobenzene, 2,5-dichlorotoluene, 2,5-dichloro-p-xylene, 1,4-dibromobenzene, 1,4-diiodobenzene, and 1-methoxy-2,5-dichlorobenzene, and p-dichlorobenzene is preferred. In addition, for the purpose of introducing carboxyl groups, it is also a preferred embodiment to use carboxyl group-containing dihalogenated aromatic compounds such as 2,4-dichlorobenzoic acid, 2,5-dichlorobenzoic acid, 2,6-dichlorobenzoic acid, and 3,5-dichlorobenzoic acid, and mixtures thereof, as copolymerization monomers. It is also possible to combine two or more different polyhalogenated aromatic compounds to form a copolymer, but it is preferable to use a p-dihalogenated aromatic compound as the main component.

[0026] The amount of the polyhalogenated aromatic compound used, in order to obtain a PPS resin (a) having a viscosity suitable for processing, can be, for example, in the range of 0.9 to 2.0 mol, preferably 0.95 to 1.5 mol, and more preferably 1.005 to 1.2 mol, per mol of the sulfidizing agent.

[0027] [Sulfidizing agent] The sulfidizing agent includes alkali metal sulfides, alkali metal hydrosulfides, and hydrogen sulfide.

[0028] Specific examples of alkali metal sulfides include lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, cesium sulfide, and mixtures of two or more of these, with sodium sulfide being preferred. These alkali metal sulfides can be used as hydrates or aqueous mixtures, or in the anhydrous form.

[0029] Specific examples of the alkali metal hydrosulfide include sodium hydrosulfide, potassium hydrosulfide, lithium hydrosulfide, rubidium hydrosulfide, cesium hydrosulfide, and mixtures of two or more of these, with sodium hydrosulfide being preferred. These alkali metal hydrosulfides can be used as hydrates or aqueous mixtures, or in the anhydrous form.

[0030] In addition, an alkali metal sulfide prepared in situ in the reaction system from an alkali metal hydrosulfide and an alkali metal hydroxide can also be used.Alkali metal sulfide can also be prepared from an alkali metal hydrosulfide and an alkali metal hydroxide, and then transferred to a polymerization tank for use.

[0031] Alternatively, an alkali metal sulfide prepared in situ in the reaction system from an alkali metal hydroxide such as lithium hydroxide or sodium hydroxide and hydrogen sulfide can be used.Alkaline metal sulfides can also be prepared from an alkali metal hydroxide such as lithium hydroxide or sodium hydroxide and hydrogen sulfide, and then transferred to a polymerization tank for use.

[0032] When a part of the sulfidizing agent is lost before the start of the polymerization reaction due to a dehydration operation or the like, the amount of the charged sulfidizing agent means the remaining amount obtained by subtracting the lost amount from the actual charged amount.

[0033] It is also possible to use an alkali metal hydroxide and / or an alkaline earth metal hydroxide together with the sulfidizing agent.Specific examples of the alkali metal hydroxide include, for example, sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide, and mixtures of two or more of these.Specific examples of the alkaline earth metal hydroxide include, for example, calcium hydroxide, strontium hydroxide, barium hydroxide, etc., and among these, sodium hydroxide is preferably used.

[0034] When an alkali metal hydrosulfide is used as the sulfidizing agent, it is particularly preferable to use an alkali metal hydroxide simultaneously. The amount of the alkali metal hydroxide used is, for example, in the range of 0.95 to 1.20 mol, preferably 1.00 to 1.15 mol, and more preferably 1.005 to 1.100 mol, per mol of the alkali metal hydrosulfide.

[0035] [Polymerization solvent] As the polymerization solvent, it is preferable to use an organic polar solvent. Specific examples include N-alkylpyrrolidones such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone, caprolactams such as N-methyl-ε-caprolactam, aprotic organic solvents such as 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide, N,N-dimethylformamide, hexamethylphosphoric triamide, dimethylsulfone, and tetramethylene sulfoxide, and mixtures thereof, all of which are preferably used because of their high reaction stability. Among these, N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) is particularly preferably used.

[0036] The amount of the organic polar solvent used is selected from the range of 2.0 to 10 moles, preferably 2.25 to 6.0 moles, and more preferably 2.5 to 5.5 moles, per mole of the sulfidizing agent.

[0037] [Molecular weight regulator] A monohalogen compound (which does not necessarily have to be an aromatic compound) can be used in combination with the polyhalogenated aromatic compound in order to form terminals in the resulting (a) PPS resin or to adjust the polymerization reaction or molecular weight.

[0038] [Polymerization aid] In order to obtain a (a) PPS resin having a relatively high degree of polymerization in a short time, it is also a preferred embodiment to use a polymerization aid. Here, the polymerization aid means a substance that has the effect of increasing the viscosity of the (a) PPS resin obtained. Specific examples of such polymerization aids include organic carboxylates, water, alkali metal chlorides, organic sulfonates, alkali metal sulfates, alkaline earth metal oxides, alkali metal phosphates, and alkaline earth metal phosphates. These can be used alone or in combination of two or more. Among them, organic carboxylates, water, and alkali metal chlorides are preferred, and alkali metal carboxylates are more preferred as organic carboxylates, and lithium chloride is more preferred as alkali metal chlorides.

[0039] The above alkali metal carboxylate has the general formula R(COOM) n (wherein R is an alkyl group, a cycloalkyl group, an aryl group, an alkylaryl group, or an arylalkyl group having 1 to 20 carbon atoms; M is an alkali metal selected from lithium, sodium, potassium, rubidium, and cesium; and n is an integer of 1 to 3). The alkali metal carboxylate can also be used as a hydrate, anhydride, or an aqueous solution. Specific examples of the alkali metal carboxylate include lithium acetate, sodium acetate, potassium acetate, sodium propionate, lithium valerate, sodium benzoate, sodium phenylacetate, potassium p-toluate, and mixtures thereof.

[0040] The alkali metal carboxylate may be formed by adding and reacting an organic acid with one or more compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates in approximately equal chemical equivalents. Among the above alkali metal carboxylates, lithium salts have high solubility in the reaction system and have a large auxiliary effect, but are expensive, while potassium, rubidium, and cesium salts are thought to have insufficient solubility in the reaction system, so sodium acetate, which is inexpensive and has moderate solubility in the polymerization system, is most preferably used.

[0041] When these alkali metal carboxylates are used as polymerization aids, the amount used is usually in the range of 0.01 mol to 2 mol per mol of the charged alkali metal sulfide. In terms of obtaining a higher degree of polymerization, the amount used is preferably in the range of 0.1 mol to 0.6 mol, and more preferably in the range of 0.2 mol to 0.5 mol.

[0042] When water is used as a polymerization aid, the amount added is usually in the range of 0.3 mol to 15 mol per mol of the charged alkali metal sulfide, and in terms of obtaining a higher degree of polymerization, the range of 0.6 mol to 10 mol is preferable, and the range of 1 mol to 5 mol is more preferable.

[0043] Of course, two or more of these polymerization aids can be used in combination. For example, when an alkali metal carboxylate and water are used in combination, a higher molecular weight can be achieved with a smaller amount of each.

[0044] The timing of addition of these polymerization aids is not particularly specified, and they may be added at any time during the pre-step, at the start of polymerization, or during the polymerization, as described below, or may be added in several portions, but when an alkali metal carboxylate is used as the polymerization aid, it is more preferable to add it at the start of the pre-step or at the start of polymerization, because it is easy to add it. When water is used as the polymerization aid, it is effective to add it during the polymerization reaction after the polyhalogenated aromatic compound is charged.

[0045] [Polymerization stabilizer] A polymerization stabilizer can be used to stabilize the polymerization reaction system and prevent side reactions. The polymerization stabilizer contributes to the stabilization of the polymerization reaction system and suppresses undesirable side reactions. One of the indicators of side reactions is the generation of thiophenol, and the addition of a polymerization stabilizer can suppress the generation of thiophenol. Specific examples of polymerization stabilizers include compounds such as alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, and alkaline earth metal carbonates. Among them, alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, and lithium hydroxide are preferred. The above-mentioned alkali metal carboxylates also act as polymerization stabilizers. In addition, when an alkali metal hydrosulfide is used as a sulfidizing agent, it is particularly preferable to use an alkali metal hydroxide at the same time, as mentioned above, but an alkali metal hydroxide that is in excess of the sulfidizing agent can also serve as a polymerization stabilizer.

[0046] These polymerization stabilizers can be used alone or in combination of two or more. The polymerization stabilizer is preferably used in a ratio of usually 0.02 to 0.2 mol, preferably 0.03 to 0.1 mol, more preferably 0.04 to 0.09 mol, per mol of the charged alkali metal sulfide. If this ratio is too small, the stabilizing effect is insufficient, and conversely, if it is too large, it is economically disadvantageous and the polymer yield tends to decrease.

[0047] The timing of adding the polymerization stabilizer is not particularly specified, and it may be added at any time during the pre-step described below, at the start of polymerization, or during the polymerization, or may be added in several divided portions. However, it is more preferable to add it simultaneously at the start of the pre-step or at the start of polymerization from the viewpoint of ease.

[0048] Next, a preferred method for producing the PPS resin (a) used in the present invention will be specifically described in order, including a pre-process, a polymerization reaction process, a recovery process, and a post-treatment process, although the method is not limited to this method.

[0049] [Pre-process] (a) In the production process for PPS resin, the sulfidizing agent is usually used in the form of a hydrate. It is preferable to heat a mixture containing an organic polar solvent and a sulfidizing agent and remove excess water from the system before adding a polyhalogenated aromatic compound.

[0050] As described above, the sulfidizing agent may be prepared in situ in the reaction system from an alkali metal hydrosulfide and an alkali metal hydroxide, or in a tank separate from the polymerization tank. There is no particular restriction on this method, but a preferable method is to add an alkali metal hydrosulfide and an alkali metal hydroxide to an organic polar solvent in an inert gas atmosphere at room temperature to 150°C, preferably from room temperature to 100°C, and then heat the mixture to at least 150°C or higher, preferably 180 to 260°C, under normal pressure or reduced pressure, to distill off water. A polymerization aid may be added at this stage. Toluene or the like may be added to promote the distillation of water.

[0051] In the polymerization reaction, the amount of water in the polymerization system is preferably 0.3 mol to 10.0 mol per 1 mol of the charged sulfidizing agent. Here, the amount of water in the polymerization system is the amount of water charged to the polymerization system minus the amount of water removed from the polymerization system. The charged water may be in any form such as water, an aqueous solution, or crystal water.

[0052] [Polymerization reaction process] (a) PPS resin is produced by reacting a sulfidizing agent with a polyhalogenated aromatic compound in an organic polar solvent at a temperature range of 200° C. or higher and lower than 290° C.

[0053] When starting the polymerization reaction process, the organic polar solvent, the sulfidizing agent, and the polyhalogenated aromatic compound are mixed, desirably in an inert gas atmosphere, at a temperature range of room temperature to 240° C., preferably 100° C. to 230° C. A polymerization aid may be added at this stage. The order of charging these raw materials may be random, or they may be charged simultaneously.

[0054] The mixture is usually heated to a temperature in the range of 200° C. to less than 290° C. There are no particular limitations on the heating rate, but a rate of 0.01 to 5° C. / min is usually selected, and a range of 0.1 to 3° C. / min is more preferable.

[0055] In general, the temperature is finally raised to 250 to less than 290° C., and the reaction is carried out at that temperature for usually 0.25 to 50 hours, preferably 0.5 to 20 hours.

[0056] In order to obtain a higher degree of polymerization, it is effective to react at 200° C. to 260° C. for a certain period of time before the final temperature is reached, and then to raise the temperature to 270° C. to less than 290° C. In this case, the reaction time at 200° C. to 260° C. is usually selected within the range of 0.25 hours to 20 hours, and preferably 0.25 hours to 10 hours.

[0057] In order to obtain a polymer with a higher degree of polymerization, it may be effective to carry out the polymerization in multiple stages. When carrying out the polymerization in multiple stages, it is effective to carry out the polymerization when the conversion rate of the polyhalogenated aromatic compound in the system at 245°C reaches 40 mol% or more, preferably 60 mol%.

[0058] The conversion rate of polyhalogenated aromatic compounds (abbreviated as PHA here) is a value calculated by the following formula: The amount of remaining PHA can usually be determined by gas chromatography.

[0059] (A) When a polyhalogenated aromatic compound is added in excess of an alkali metal sulfide in terms of molar ratio Conversion rate=[charged amount of PHA (mol)−remaining amount of PHA (mol)] / [charged amount of PHA (mol)−excess amount of PHA (mol)].

[0060] (B) Cases other than (A) above Conversion rate=[charged amount of PHA (mol)−remaining amount of PHA (mol)] / [charged amount of PHA (mol)].

[0061] [Recovery process] In the (a) PPS resin manufacturing method, after the polymerization is completed, solid matter is recovered from the polymerization reaction product containing the polymer, the solvent, etc. As for the recovery method, it is essential to adopt a method of recovering the particulate polymer by slowly cooling after the polymerization reaction is completed. The cooling speed is not particularly limited, but is usually about 0.1°C / min to 3°C / min. It is not necessary to slowly cool at the same speed throughout the entire cooling process, and a method of slowly cooling at a speed of 0.1 to 1°C / min until the polymer particles crystallize and precipitate, and then at a speed of 1°C / min or more may be adopted.

[0062] [Post-processing process] The (a) PPS resin may be produced through the above-mentioned polymerization and recovery steps, and then may be subjected to acid treatment, hot water treatment, washing with an organic solvent, or treatment with an alkali metal or alkaline earth metal.

[0063] The acid treatment is carried out as follows: There are no particular limitations on the acid used in the acid treatment of the (a) PPS resin so long as it does not have the effect of decomposing the (a) PPS resin, and examples of the acid include acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, silicic acid, carbonic acid, and propylic acid, and among these, acetic acid and hydrochloric acid are more preferably used, but acids such as nitric acid that decompose and deteriorate the (a) PPS resin are undesirable.

[0064] The acid treatment may be carried out by immersing the PPS resin (a) in an acid or an aqueous solution of an acid, and may be carried out with appropriate stirring or heating, if necessary. For example, when acetic acid is used, a sufficient effect can be obtained by immersing the PPS resin powder in an aqueous solution of pH 4 heated to 80 to 200°C and stirring for 30 minutes. The pH after the treatment may be 4 or higher, for example, about pH 4 to 8. The PPS resin (a) that has been subjected to the acid treatment is preferably washed several times with water or warm water to remove the remaining acid or salt. The water used for washing is preferably distilled water or deionized water, so as not to impair the effect of the preferable chemical modification of the PPS resin (a) by the acid treatment.

[0065] The hot water treatment is carried out as follows: When the (a) PPS resin is subjected to hot water treatment, the temperature of the hot water is preferably 100° C. or higher, more preferably 120° C. or higher, still more preferably 150° C. or higher, and particularly preferably 170° C. or higher. If the temperature is less than 100° C., the desired chemical modification effect of the (a) PPS resin is small, which is not preferred.

[0066] In order to achieve the desired chemical modification effect of the (a) PPS resin by hot water washing, it is preferable that the water used is distilled water or deionized water. There are no particular limitations on the procedure for the hot water treatment, and it can be carried out by adding a specified amount of (a) PPS resin to a specified amount of water, heating and stirring in a pressure vessel, or by continuously carrying out hot water treatment. The ratio of (a) PPS resin to water is preferably higher, but a bath ratio of 200 g or less of (a) PPS resin to 1 liter of water is usually selected.

[0067] In addition, since decomposition of the terminal groups is undesirable, it is desirable to carry out the treatment in an inert atmosphere to avoid this. Furthermore, after the hot water treatment, the (a) PPS resin is preferably washed several times with warm water to remove any remaining components.

[0068] When washing with an organic solvent, the procedure is as follows. The organic solvent used for washing the (a) PPS resin is not particularly limited as long as it does not have the action of decomposing the (a) PPS resin, and examples thereof include nitrogen-containing polar solvents such as N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, 1,3-dimethylimidazolidinone, hexamethylphosphoramide, and piperazinones, sulfoxide-sulfone solvents such as dimethylsulfoxide, dimethylsulfone, and sulfolane, ketone solvents such as acetone, methyl ethyl ketone, diethyl ketone, and acetophenone, dimethyl ether, dipropyl ether, dioxane, and tetrahydrofuran. Examples of the organic solvent include ether solvents such as hydrofuran, halogen-based solvents such as chloroform, methylene chloride, trichloroethylene, ethylene dichloride, perchloroethylene, monochloroethane, dichloroethane, tetrachloroethane, perchloroethane, and chlorobenzene, alcohol-phenol solvents such as methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, and polypropylene glycol, and aromatic hydrocarbon solvents such as benzene, toluene, and xylene. Among these organic solvents, N-methyl-2-pyrrolidone, acetone, dimethylformamide, and chloroform are particularly preferred. These organic solvents are used alone or in combination of two or more.

[0069] The method of washing with an organic solvent includes immersing the (a) PPS resin in the organic solvent, and stirring or heating can be performed as necessary. There is no particular restriction on the washing temperature when washing the (a) PPS resin with an organic solvent, and any temperature between room temperature and about 300°C can be selected. The higher the washing temperature, the higher the washing efficiency tends to be, but usually a washing temperature between room temperature and 150°C is sufficient to obtain the desired effect. Washing can also be performed under pressure in a pressure vessel at a temperature above the boiling point of the organic solvent. There is also no particular restriction on the washing time. Although it depends on the washing conditions, in the case of batch washing, washing for 5 minutes or more usually obtains the desired effect. Continuous washing is also possible.

[0070] Examples of the method of alkali metal or alkaline earth metal treatment include a method of adding an alkali metal salt or alkaline earth metal salt before, during, or after the previous step, a method of adding an alkali metal salt or alkaline earth metal salt into a polymerization vessel before, during, or after the polymerization step, or a method of adding an alkali metal salt or alkaline earth metal salt at the beginning, middle, or end of the washing step. The easiest method among them is a method of adding an alkali metal salt or alkaline earth metal salt after removing residual oligomers and residual salts by washing with an organic solvent or washing with warm or hot water. The alkali metal or alkaline earth metal is preferably introduced into PPS in the form of an alkali metal ion or alkaline earth metal ion such as an acetate, hydroxide, or carbonate. It is also preferable to remove excess alkali metal salt or alkaline earth metal salt by washing with warm water or the like. The concentration of the alkali metal ion or alkaline earth metal ion when introducing the alkali metal or alkaline earth metal is preferably 0.001 mmol or more per 1 g of PPS, and more preferably 0.01 mmol or more. The temperature is preferably 50° C. or higher, more preferably 75° C. or higher, and particularly preferably 90° C. or higher. There is no particular upper limit to the temperature, but from the viewpoint of operability, it is usually preferably 280° C. or lower. The bath ratio (weight of cleaning solution relative to the weight of dry PPS) is preferably 0.5 or higher, more preferably 3 or higher, and even more preferably 5 or higher.

[0071] In the present invention, from the viewpoint of obtaining a polyphenylene sulfide resin composition excellent in retention stability, a method in which residual oligomers and residual salts are removed by repeatedly washing with an organic solvent and with warm water of about 80° C. or the above-mentioned hot water several times, and then the method in which the resin is treated with an acid, an alkali metal salt, or an alkaline earth metal salt is treated is preferred, and in particular a method in which the resin is treated with an alkali metal salt or an alkaline earth metal salt is more preferred.

[0072] In addition, the (a) PPS resin can also be used after being polymerized by a thermal oxidative crosslinking treatment in which heating is performed in an oxygen atmosphere after polymerization or by heating with the addition of a crosslinking agent such as a peroxide, thereby increasing the molecular weight.

[0073] When dry heat treatment is performed for the purpose of increasing the molecular weight by thermal oxidation crosslinking, the temperature is preferably 160 to 260°C, more preferably 170 to 250°C. The oxygen concentration is desirably 5% by volume or more, more desirably 8% by volume or more. There is no particular upper limit to the oxygen concentration, but the limit is about 50% by volume. The treatment time is preferably 0.5 to 100 hours, more preferably 1 to 50 hours, and even more preferably 2 to 25 hours. The heat treatment device may be a normal hot air dryer, or a rotary or stirring blade-equipped heating device, but in the case of efficient and more uniform treatment, it is more preferable to use a rotary or stirring blade-equipped heating device.

[0074] Dry heat treatment can also be performed to suppress thermal oxidative crosslinking and remove volatiles. The temperature is preferably 130 to 250°C, more preferably 160 to 250°C. In this case, the oxygen concentration is preferably less than 5% by volume, and even less than 2% by volume. The treatment time is preferably 0.5 to 50 hours, more preferably 1 to 20 hours, and even more preferably 1 to 10 hours. The heat treatment device may be a normal hot air dryer, or a rotary or stirring blade-equipped heating device, but in the case of efficient and more uniform treatment, it is more preferable to use a rotary or stirring blade-equipped heating device.

[0075] In the (a) PPS resin of the present invention, functional groups such as carboxyl groups and amino groups may be introduced into the PPS resin terminals or side chains from the viewpoint of improving the reactivity with the (b) silicone elastomer having a crosslinked structure and other additives. A preferred embodiment of the functional group amount is 25 to 400 μmol / g, more preferably 25 to 250 μmol / g, more preferably 30 to 150 μmol / g, and even more preferably 30 to 80 μmol / g. By making the functional group amount 25 μmol / g or more, reactivity with the (b) silicone elastomer having a crosslinked structure and other additives can be obtained, which is preferable. On the other hand, by making the functional group amount of the PPS resin 400 μmol / g or less, the decrease in processability and the decrease in flame retardancy and chemical resistance due to the increase in the amount of volatile components can be suppressed, which is preferable.

[0076] Examples of methods for introducing functional groups such as carboxyl groups and amino groups into the (a) PPS resin include a method of copolymerizing a polyhalogenated aromatic compound containing a carboxyl group or an amino group with a sulfidizing agent, and a method of adding a compound containing a carboxyl group or an amino group, such as maleic anhydride or sorbic acid, and reacting it with the (a) PPS resin while melt-kneading. The type of functional group is preferably a carboxyl group or an amino group.

[0077] (2)(b) Silicone elastomer having a cross-linked structure Blending the (b) silicone elastomer having a crosslinked structure with the PPS resin composition according to an embodiment of the present invention is essential for achieving a polyphenylene sulfide resin composition for battery insulating members that combines excellent productivity, safety, and long-term reliability.

[0078] The silicone elastomer having a crosslinked structure (b) has a main chain structure of organopolysiloxane and a molecular structure in which the organopolysiloxane molecules are bonded by crosslinking. The degree of polymerization of the silicone elastomer having a crosslinked structure is preferably 100 or more, and the weight average molecular weight is preferably 10,000 or more. Note that silicone oil and uncrosslinked silicone gum do not have a crosslinked structure, and therefore are not included in the silicone elastomer having a crosslinked structure (b).

[0079] Examples of methods for introducing a crosslinked structure include peroxide crosslinking, condensation reaction crosslinking, addition reaction crosslinking, and ultraviolet crosslinking. Examples of peroxide crosslinking include a method in which an alkyl group or vinyl group of a silicone polymer is reacted with an organic peroxide such as an alkyl peroxide or an acyl peroxide to form a crosslink. Examples of condensation reaction crosslinking include a condensation reaction caused by a reaction between a silanol group of a silicone polymer and a crosslinking agent, and representative examples of crosslinking agents include dealcohol type, deacetic acid type, deoxime type, deamidation type, dehydroxylamine type, and deacetone type. In addition, in order to promote the reaction, it is preferable to use a tin compound, a titanium compound, a metal fatty salt, or an amino group-containing compound as a catalyst. Examples of addition reaction crosslinking include a hydrosilylation reaction between a multiple bond such as a vinyl group of a silicone elastomer and a Si-H group. In this case, it is preferable to use a transition metal compound, especially a platinum compound, as a catalyst.

[0080] The silicone elastomer having a crosslinked structure (b) may have a copolymer component in a part of its molecular structure.Specific examples include copolymers of an organopolysiloxane component with one or more copolymer components selected from polyolefins (polyethylene, polypropylene, polybutylene, etc.), polycarbonates, polyamides, polybutylene terephthalates, polyester elastomers, polystyrenes, polyetherimides, polyketones, liquid crystal polymers, polyether ketones, polyether ether ketones, polyacrylates (polymethyl methacrylate, etc.), etc., and the silicone elastomer having a crosslinked structure (b) preferably has 90% by weight or more of the constitutional unit derived from the organopolysiloxane.

[0081] Examples of composites that contain organopolysiloxane as a constituent unit include core-shell rubbers in which silicone elastomer particles are covered with an acrylic component (silicone acrylic core-shell rubbers) and composite powders in which silicone elastomer is covered with a silicone resin. From the standpoint of flame retardancy and long-term durability, however, it is preferable that the organopolysiloxane is 90% by weight or more.

[0082] (b) The silicone elastomer having a crosslinked structure preferably has one or more hydrocarbon groups in its structure selected from alkyl groups having 1 to 8 carbon atoms (e.g., methyl, ethyl, propyl, butyl, 2-ethylbutyl, octyl), cycloalkyl groups having 3 to 8 carbon atoms (e.g., cyclohexyl, cyclopentyl), alkenyl groups having 2 to 8 carbon atoms (e.g., vinyl, propenyl, butenyl, heptenyl, hexenyl, allyl), and aryl groups (e.g., phenyl, tolyl, xylyl, naphthyl, diphenyl), and among these, it is preferable that the silicone elastomer has a methyl group, a phenyl group, or a vinyl group.

[0083] From the viewpoint of improving compatibility with PPS resins, it is preferable that the organopolysiloxane structure contains one or more functional groups selected from alkoxyl groups having 1 to 8 carbon atoms (e.g., methoxy, ethoxy, propoxy, butoxy), amino, epoxy, carbinol, methacryl, ether, mercapto, carboxyl, phenol, silanol, acrylic, carboxylic anhydride, polyether, aralkyl, fluoroalkyl, long-chain alkyl, higher fatty acid ester, higher fatty acid amide, etc. at the molecular chain end or molecular chain side chain. Among these, it is preferable to contain an alkoxyl group, amino, epoxy, methacryl, mercapto, carboxyl, or acrylic group, and alkoxyl, epoxy, or methacryl group is particularly preferable.

[0084] (b) The shape of the silicone elastomer having a crosslinked structure is not limited, but examples thereof include pellets, bulk, powder, powder aggregates, and flakes. From the viewpoints of handleability, processability, and dispersibility, pellets, powder, powder aggregates, and flakes are preferred.

[0085] When the shape of the silicone elastomer having a crosslinked structure is a fine particle, the average primary particle diameter (number average primary particle diameter) is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, from the viewpoints of dispersibility, flame retardancy, and toughness of the PPS resin composition. If the average primary particle diameter exceeds 10 μm, it is not preferable because it becomes the starting point of cracks and leads to a decrease in mechanical properties. On the other hand, the lower limit is preferably 100 nm or more from the viewpoint of productivity. The average primary particle diameter of the silicone elastomer having a crosslinked structure (b) can be calculated by randomly specifying the diameter of 100 particles from a scanning electron microscope photograph and calculating the arithmetic average. In the above photograph, if the shape is not a perfect circle, i.e., if it is an ellipse, the maximum diameter of the particle is taken as the particle diameter. Representative methods for obtaining a silicone elastomer having a crosslinked structure in the shape of fine particles include a method of dissolving the silicone elastomer in a soluble solvent and then precipitating it, a method of forming an emulsion using an emulsifier and then recovering it, and a method of mechanically crushing and pulverizing a silicone elastomer having a crosslinked structure in pellets or bulk form.

[0086] The blending amount of the silicone elastomer having a crosslinked structure (b) used in the present invention must be 0.1 parts by weight or more and 15.0 parts by weight or less relative to 100 parts by weight of the PPS resin (a), preferably 0.5 parts by weight or more and 12.0 parts by weight or less, and more preferably 1 part by weight or more and 10.0 parts by weight or less. If the blending amount of the silicone elastomer having a crosslinked structure exceeds 15.0 parts by weight relative to 100 parts by weight of the PPS resin, the PPS resin composition becomes too flexible, and creep deformation occurs as a battery insulating member, leading to a decrease in long-term reliability. On the other hand, if the silicone elastomer having a crosslinked structure (b) is less than 0.1 parts by weight relative to 100 parts by weight of the PPS resin, sufficient flexibility, toughness, and flame retardancy of the resin composition cannot be obtained, which is not preferable from the viewpoint of productivity and long-term reliability as a battery insulating member.

[0087] It is also possible to use two or more types of silicone elastomers having crosslinked structures in combination.

[0088] (b) The Shore hardness A of the silicone elastomer having a crosslinked structure is preferably 60 HS or less, more preferably 50 HS or less, and even more preferably 45 HS or less. By making the Shore hardness A of the silicone elastomer having a crosslinked structure 60 HS or less, it is possible to obtain the desired flame retardancy and toughness as an insulating material, which is preferable. On the other hand, although there is no particular lower limit, a significantly small Shore hardness means that it is equivalent to silicone oil, and shows bleed-out during long-term high-temperature use, so that it is substantially preferable that it is 10 HS or more.

[0089] (3)(c) Thermoplastic elastomer The PPS resin composition according to the embodiment of the present invention preferably does not substantially contain (c) thermoplastic elastomer. Here, "substantially does not contain (c) thermoplastic elastomer" means that the blending amount of (c) thermoplastic elastomer is 0.5 parts by weight or less per 100 parts by weight of PPS resin, more preferably 0.3 parts by weight or less per 100 parts by weight of PPS resin, and even more preferably 0.1 parts by weight or less per 100 parts by weight of PPS resin. Most preferably, the PPS resin composition does not contain (c) thermoplastic elastomer. Thermoplastic elastomers are materials that plasticize at high temperatures and exhibit rubber-like elasticity at room temperature. When a thermoplastic elastomer is added to a PPS resin composition, the mechanical properties of the battery insulating material are reduced and degraded components are eluted into the electrolyte due to thermal degradation associated with the low long-term high-temperature durability of the thermoplastic elastomer, leading to a decrease in long-term reliability. In addition, the flame retardancy of the battery insulating material is reduced due to the low flame retardancy of the thermoplastic elastomer itself, so the PPS resin composition according to the embodiment of the present invention does not substantially contain (c) thermoplastic elastomer. In addition, silicone elastomers are thermosetting elastomers and are therefore different from (c) thermoplastic elastomers.

[0090] Specific examples of the thermoplastic elastomer include olefin-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and styrene-based thermoplastic elastomers. Examples of the olefin-based thermoplastic elastomers include ethylene-butene copolymers, ethylene-propylene copolymers, ethylene-hexene copolymers, ethylene-octene copolymers, ethylene-vinyl acetate copolymers, ethylene-methyl acrylate copolymers, ethylene-ethyl acrylate copolymers, ethylene-glycidyl methacrylate copolymers, ethylene-butyl acrylate copolymers, ethylene-methyl acrylate copolymers, ethylene-styrene copolymers, ethylene-methyl acrylate-glycidyl methacrylate copolymers, ethylene-ethyl acrylate-glycidyl methacrylate copolymers, and ethylene-vinyl acetate-glycidyl methacrylate copolymers.

[0091] (4)(d) Other additives To the PPS resin composition according to an embodiment of the present invention, resins other than (a) the PPS resin and (b) the silicone elastomer having a crosslinked structure may be added as long as the effects of the present invention are not impaired. Specific examples of such resins include polyamide, polybutylene terephthalate, polyethylene terephthalate, polyetherimide, polyetherimide-siloxane copolymer, polyketone, liquid crystal polymer, polyether ketone, polyether ether ketone, fluororesin (polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene-hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), and polychlorotrifluoroethylene (PCTFE), but are not limited thereto. The amount of such resins added is preferably less than 10 parts by weight, more preferably less than 5 parts by weight, and more preferably less than 3 parts by weight, relative to 100 parts by weight of PPS resin. The lower limit is preferably 0 parts by weight, i.e., does not include these resins.

[0092] The PPS resin composition according to the embodiment of the present invention can be added with the following compounds for the purpose of modification. Plasticizers such as polyalkylene oxide oligomer compounds, thioether compounds, ester compounds, and organic phosphorus compounds, crystal nucleating agents such as organic phosphorus compounds and polyether ether ketones, montanic acid waxes, metal soaps such as lithium stearate and aluminum stearate, release agents such as ethylenediamine-stearic acid-sebacic acid polycondensates, water, lubricants, ultraviolet inhibitors, coloring inhibitors, colorants, foaming agents, phosphorus-based flame retardants, halogen-based flame retardants, and inorganic flame retardants can be blended. If the amount of any of the above compounds to be added exceeds 10 parts by weight per 100 parts by weight of the total PPS resin composition, the inherent properties of the PPS resin composition of the present invention are impaired, which is not preferable, and it is preferable to add 5 parts by weight or less, more preferably 1 part by weight or less.

[0093] In the present invention, an organic silane compound or an epoxy resin can be added to the PPS resin composition for the purpose of increasing the toughness of the PPS resin composition.

[0094] Specific examples of the organic silane compound are preferably organic silane compounds having at least one functional group selected from an isocyanate group, an epoxy group, an amino group, a hydroxyl group, a mercapto group, a ureido group, and an alkoxy group.Specific examples include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-phenylaminomethyltrimethoxysilane, N-phenylaminopropyl Preferred examples of such silane include γ-ureidopropyltrimethoxysilane, dimethoxymethyl-3-piperazinopropylsilane, 3-piperazinopropyltrimethoxysilane, 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-isocyanatopropylmethyldimethoxysilane, 3-isocyanatopropylmethyldiethoxysilane, 3-isocyanatopropylethyldimethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptomethyldimethoxysilane, and γ-ureidopropyltrimethoxysilane.

[0095] Among the above-mentioned organic silane compounds, 3-isocyanatopropyltriethoxysilane, 3-aminopropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane are preferred from the viewpoints of reactivity and ease of handling.

[0096] These alkoxy organic silane compounds can be used alone or in the form of a mixture of two or more kinds.

[0097] The amount of the organosilane compound used in the present invention is preferably 0.01 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, and more preferably 0.3 to 3 parts by weight, relative to 100 parts by weight of the PPS resin. By setting the amount of the organosilane compound to 10 parts by weight or less, it is preferable that the flame retardancy of the resulting PPS resin composition can be maintained. When the amount of the organosilane compound is 0.01 parts by weight or more, the reaction between PPS and the organosilane compound becomes sufficient, and excellent toughness can be exhibited, which is preferable.

[0098] Specific examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, brominated epoxy resins, special skeleton bifunctional epoxy resins having a biphenyl skeleton or a naphthalene skeleton, glycidyl ether type epoxy resins such as multifunctional epoxy resins such as cresol novolac type, trisphenol methane type, and dicyclopentadiene type, glycidyl amine type epoxy resins such as aromatic amine type and aminophenol type, and glycidyl ester type epoxy resins such as hydrophthalic acid type and dimer acid type. The amount of such epoxy resins to be added is preferably 0.1 to 5 parts by weight, particularly preferably 0.2 to 3 parts by weight, based on 100 parts by weight of the total PPS resin composition.

[0099] Although not an essential component, inorganic fillers can be blended and used in the PPS resin composition according to the embodiment of the present invention within the scope that does not impair the effects of the present invention. Specific examples of such inorganic fillers include fibrous fillers such as glass fibers, carbon fibers, carbon nanotubes, carbon nanohorns, potassium titanate whiskers, zinc oxide whiskers, calcium carbonate whiskers, wollastonite whiskers, aluminum borate whiskers, aramid fibers, alumina fibers, silicon carbide fibers, ceramic fibers, asbestos fibers, gypsum fibers, and metal fibers, as well as fullerenes, talc, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, bentonite, asbestos, alumina silicate, and the like. Examples of inorganic fillers include silicates such as silicate oxide, silicon oxide, magnesium oxide, alumina, zirconium oxide, titanium oxide, iron oxide, and other metal compounds, carbonates such as calcium carbonate, magnesium carbonate, and dolomite, sulfates such as calcium sulfate and barium sulfate, and non-fibrous fillers such as glass beads, glass flakes, glass powder, ceramic beads, boron nitride, silicon carbide, carbon black, and graphite. Among these, glass fibers, calcium carbonate, and carbon black are preferred, and calcium carbonate and carbon black are particularly preferred from the viewpoint of corrosion prevention and lubricant effects. These inorganic fillers may be hollow, and two or more types may be used in combination. These inorganic fillers may be pretreated with coupling agents such as isocyanate compounds, organic silane compounds, organic titanate compounds, organic borane compounds, and epoxy compounds before use.

[0100] The amount of the inorganic filler is selected to be less than 10 parts by weight, preferably less than 5 parts by weight, more preferably less than 3 parts by weight, and even more preferably 1 part by weight or less, relative to 100 parts by weight of the total PPS resin composition. There is no particular lower limit, but 0.0001 parts by weight or more is preferred. While the incorporation of an inorganic filler is effective in improving the strength of the material, an incorporation of more than 10 parts by weight is not preferred because it reduces toughness.

[0101] (5) Method for producing resin composition The method for producing the PPS resin composition according to the embodiment of the present invention includes production in a molten state and production in a solution state, but from the viewpoint of simplicity, production in a molten state is preferably used. For production in a molten state, melt kneading using an extruder or melt kneading using a kneader can be used, but from the viewpoint of productivity, melt kneading using an extruder that can be continuously produced is preferably used. For melt kneading using an extruder, at least one extruder such as a single screw extruder, a twin screw extruder, a multi-screw extruder such as a four-screw extruder, or a twin-screw single screw composite extruder can be used, but from the viewpoint of kneading property, reactivity, and productivity improvement, a multi-screw extruder such as a twin screw extruder or a four-screw extruder can be preferably used, and melt kneading using a twin screw extruder is most preferable.

[0102] A more specific method of melt kneading is not necessarily limited to this, but it is preferable to use a twin-screw extruder having an L / D (L: screw length, D: screw diameter) of 10 or more, preferably 20 or more, and having two or more kneading sections, preferably three or more. There is no particular upper limit to L / D, but 60 or less is preferable from the viewpoint of economic efficiency. There is also no particular upper limit to the number of kneading sections, but 10 or less is preferable from the viewpoint of productivity. The ratio of the kneading section to the entire screw length is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more, from the viewpoint of dispersibility of the silicone elastomer having a crosslinked structure (b) in the PPS resin. On the other hand, the upper limit of the ratio of the kneading section to the entire screw length is preferably 40% or less, from the viewpoint of preventing deterioration of the resin due to the generation of excessive shear heat during kneading.

[0103] The screw rotation speed is preferably 150 to 1000 rpm, more preferably 300 to 1000 rpm, and even more preferably 350 to 800 rpm. When the screw rotation speed exceeds 150 rpm, the kneading force is sufficient, so that the aggregation of the silicone elastomer having a crosslinked structure (b) is suppressed, leading to the development of the desired toughness. When the screw rotation speed exceeds 1000 rpm, deterioration of the resin and additives occurs due to excessive shear heat generation during kneading, leading to a decrease in toughness, a decrease in mold fouling, the generation of burrs due to a decrease in melt viscosity, and a decrease in the long-term reliability of the battery insulating member due to decomposition products, which is not preferable.

[0104] Specifically, the preferred range of the cylinder temperature (°C) is 280 to 400°C, more preferably 280 to 360°C, and even more preferably 280 to 330°C.

[0105] The order of mixing the raw materials when melt-kneading is not particularly limited, and any of the following methods may be used: a method in which all the raw materials are mixed and then melt-kneaded by the above-mentioned method; a method in which a portion of the raw materials are mixed and then melt-kneaded by the above-mentioned method, and then the remaining raw materials are mixed and melt-kneaded; or a method in which a portion of the raw materials are mixed and then the remaining raw materials are mixed using a side feeder while being melt-kneaded by a twin-screw extruder.

[0106] (6) PPS resin composition The PPS resin composition of the present invention must have a flexural modulus (in accordance with ISO178 (2010), bending speed 2 mm / min, 23°C) of 3.1 GPa or more and 3.6 GPa or less, which is one of the physical properties indicating the flexibility of the material. It is preferable that it is 3.2 GPa or more and 3.6 GPa or less. The PPS resin composition for battery insulating members is required to have flexibility from the viewpoint of suppressing breakage in the insulating member manufacturing process, and high rigidity from the viewpoint of creep deformation during long-term use. Since these contradictory performances are required, it is essential that the flexural modulus of the resin composition is 3.1 GPa or more and 3.6 GPa or less. The method for obtaining a PPS resin composition having such characteristics is not particularly limited, but for example, the blending amount of (b) silicone elastomer having a crosslinked structure relative to 100 parts by weight of (a) polyphenylene sulfide resin is 0.1 to 15.0 parts by weight of the resin composition.

[0107] The PPS resin composition of the present invention preferably has a flame retardancy of V-0 measured on a test piece having a thickness of 1.0 mmt or less, and more preferably has a flame retardancy of V-0 measured on a test piece having a thickness of 0.7 mmt or less, in a measurement according to the UL94 standard, which is an index of the flame retardancy of a material. Having such flame retardancy means that it is possible to achieve a thinner molded product and a lighter molded product while having excellent flame retardancy, and this not only contributes to reducing human and economic losses due to fires, but also contributes to energy saving effects due to the lighter weight, so that it can be suitably used as an insulating member for automobile batteries such as electric vehicles. The method for obtaining a PPS resin composition having such characteristics is not particularly limited, but examples thereof include a blending amount of (b) silicone elastomer having a crosslinked structure relative to 100 parts by weight of (a) polyphenylene sulfide resin of 0.1 to 15.0 parts by weight, a silicone elastomer having a fine particle crosslinked structure with a particle size of 100 nm to 10 μm, and a silicone elastomer having a crosslinked structure with a Shore hardness A of 60 HS or less. Although the flame retardant mechanism is unclear, it was found that when silicone elastomers with a crosslinked structure and particle size and hardness within the above ranges are used, the flame retardant performance is improved compared to when silicone elastomers outside the ranges are used. This is presumably due to the difference in the formation of a flame retardant layer derived from the silicone elastomer during combustion.

[0108] The PPS resin composition of the present invention has a tensile breaking elongation (dumbbell test piece (ISO527-2-1A), tensile speed of 50 mm / min, 23°C, (compliant with ISO527-1,2 (2012))) which is one of the physical properties indicating the toughness of a material, of preferably 8% or more, more preferably 10% or more, even more preferably 12% or more, and particularly preferably 14% or more. From the viewpoint of preventing breakage of battery insulating members during actual use, it is desirable for the resin composition to have a tensile breaking elongation of 8% or more. From the viewpoint of preventing breakage of members during actual use and long-term reliability, the higher the tensile breaking elongation, the more preferable it is, and although there is no particular upper limit, it can be exemplified as being substantially 500% or less. The method for obtaining a PPS resin composition having such properties is not particularly limited, but examples thereof include a method in which the blending amount of (b) silicone elastomer having a crosslinked structure per 100 parts by weight of (a) polyphenylene sulfide resin is 0.1 to 15.0 parts by weight, a method in which a silicone elastomer having a crosslinked structure in the form of fine particles with a particle size of 100 nm to 10 μm is used, and a method in which an organosilane compound and an epoxy resin are used in combination.

[0109] From the viewpoint of long-term durability as a battery insulating member, the PPS resin composition of the present invention is preferably excellent in bleed-out resistance. The generation of bleed-out components from the surface of a molded article is undesirable because it leads not only to a decrease in insulation but also to a decrease in the power generation efficiency of the battery. The bleed-out resistance can be evaluated by the following method. A dumbbell test piece (ISO527-2-1A) obtained by injection molding is placed in a gear oven set at 180°C, treated for 250 hours, and then cooled at room temperature for 24 hours or more, and the bleed-out resistance is evaluated based on the presence or absence of bleed-out components on the surface. The method for obtaining a PPS resin composition having such characteristics is not particularly limited, but may be to select and use a silicone elastomer having a crosslinked structure instead of a non-crosslinked silicone oil.

[0110] From the viewpoint of long-term durability as a battery insulating member, the PPS resin composition of the present invention preferably has an elongation retention rate of 50% or more before and after long-term durability treatment, more preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. The higher the elongation retention rate of the resin composition before and after long-term durability treatment, the more preferable it is, and there is no particular upper limit, but since the practical upper limit is 100%, it is preferable that it is 100% or less. The evaluation of the elongation retention rate before and after long-term durability treatment can be performed by the following method. A dumbbell test piece (ISO527-2-1A) obtained by injection molding is placed in a gear oven set at 180°C, treated for 250 hours, and then allowed to cool at room temperature for 24 hours or more. Then, a tensile breaking elongation measurement (based on ISO527-1,2 (2012)) is performed under conditions of a tensile speed of 50 mm / min and 23°C, and the change rate when the elongation before the long-term durability treatment is taken as 100% is calculated as the retention rate. The method for obtaining a PPS resin composition having such properties is not particularly limited, but an example thereof is that the content of (b) silicone elastomer having a crosslinked structure is 0.1 to 15.0 parts by weight relative to 100 parts by weight of (a) polyphenylene sulfide resin, and the composition does not contain a thermoplastic elastomer.

[0111] The PPS resin composition of the present invention preferably has a low tensile creep displacement in a high-temperature environment. If a battery insulating member is formed from a material with a large tensile creep displacement in a high-temperature environment, deformation occurs during long-term use, the sealing property of the electrolyte is reduced, and this is undesirable from the viewpoint of safety. The amount of tensile creep displacement is preferably 4.0% or less, more preferably 3.7% or less, even more preferably 3.5% or less, and even more preferably 3.0% or less. The amount of tensile creep displacement of the resin composition is preferably as close to 0% as possible, and there is no particular lower limit, but since the actual lower limit is 0%, it is preferable that it is 0% or more. The evaluation of the tensile creep displacement can be performed by the following method. A dumbbell test piece (ASTM No. 4, thickness 1.6 mm) obtained by injection molding is treated under conditions of 80°C, 20 MPa, and 100 hours using a tensile creep tester with a chuck distance of 64 mm, and the amount of displacement is evaluated. The method for obtaining a PPS resin composition having such properties is not particularly limited, but an example of this is to control the flexural modulus of the resin composition to be in the range of 3.1 GPa or more and 3.6 GPa or less by mixing 0.1 to 15.0 parts by weight of (b) a silicone elastomer having a crosslinked structure with respect to 100 parts by weight of (a) a polyphenylene sulfide resin.

[0112] The PPS resin composition of the present invention preferably has excellent fluidity when melted. Resin compositions with poor fluidity are undesirable because they are difficult to mold into thin-walled battery insulating components. The fluidity can be measured using melt viscosity as an index, and the melt viscosity of the PPS resin composition of the present invention was measured using a capillograph under the conditions of 320°C, orifice length L (mm) / orifice diameter D (mm) = 10 at a shear rate of 1216 s -1The value in the above is adopted. The melt viscosity is preferably 250 Pa·s or less, more preferably 200 Pa·s or less, and even more preferably 160 Pa·s or less. From the viewpoint of suppressing burrs during molding, the melt viscosity is preferably 80 Pa·s or more, more preferably 90 Pa·s or more, and even more preferably 100 Pa·s or more. The method for obtaining a PPS resin composition having such characteristics is not particularly limited, but examples thereof include a method in which the PPS resin composition is substantially free of (c) thermoplastic elastomer, a method in which (a) PPS resin having a weight average molecular weight of 30,000 to 150,000 is used, 0.01 to 10 parts by weight of an organic silane compound is blended with 100 parts by weight of the PPS resin, and 0.1 to 5 parts by weight of an epoxy resin is blended with 100 parts by weight of the PPS resin composition.

[0113] Generally, when a resin composition has excellent fluidity, the flame retardancy of the resin composition tends to be low in a combustion test according to the UL94 standard. This is thought to be because dripping occurs during the combustion test, and the dripping causes flammable components to reappear on the surface, causing the combustion to continue. On the other hand, the PPS resin composition for battery insulating members of the present invention can exhibit excellent fluidity required for molding and processing battery insulating members, while also exhibiting flame retardancy in thin-walled molded products.

[0114] (7) Battery insulating materials The battery insulating member made of the PPS resin composition of the present invention refers to an insulating member for primary or secondary batteries, and is used to prevent internal and external short circuits in primary or secondary batteries. Examples of primary or secondary batteries include primary batteries such as alkaline manganese dry batteries, galvanic batteries, nickel-based primary batteries, lithium batteries, manganese dry batteries, mercury batteries, and all-solid-state batteries, and secondary batteries such as lead-acid batteries, lithium-air batteries, lithium-ion secondary batteries, lithium-ion polymer secondary batteries, lithium iron phosphate batteries, lithium-sulfur batteries, nickel-cadmium storage batteries, nickel-hydrogen rechargeable batteries, nickel-lithium batteries, nickel-zinc batteries, and all-solid-state batteries.

[0115] Examples of battery insulating members include insulating plates, gaskets, terminal holders, cases, insulating rings, insulating tubes, wire coatings, bus bar coatings, etc. Battery insulating members made of the PPS resin composition of the present invention have excellent toughness, which reduces the risk of breakage during the crimping process, and also have excellent long-term reliability, so that they are preferably applied to insulating plates, gaskets, terminal holders, and cases, which are important safety members of batteries.

[0116] The battery insulating member of the present invention can be molded by various molding techniques such as injection molding, extrusion molding, compression molding, blow molding, and injection compression molding, among which injection molding is preferred from the standpoint of productivity. EXAMPLES

[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto.

[0118] In the examples and comparative examples, the following were used as (a) a PPS resin, (b) a silicone elastomer having a crosslinked structure, (c) a thermoplastic elastomer, and (d) other additives.

[0119] [(a)PPS resin (a-1)] [Reference example 1 PPS resin (a-1)] In an autoclave equipped with a stirrer, 8267.37g (70.00 mol) of 47.5% sodium hydrosulfide, 2923.88g (70.17 mol) of 96% sodium hydroxide, 11434.50g (115.50 mol) of N-methyl-2-pyrrolidone (NMP), 1894.20g (23.10 mol) of sodium acetate, and 10500g of ion-exchanged water were charged, and the mixture was gradually heated to 230°C over about 3 hours while passing nitrogen through it at normal pressure. After distilling out 14780.1g of water and 280g of NMP, the reaction vessel was cooled to 160°C. The amount of water remaining in the system per mole of charged alkali metal sulfide was 1.06 mol, including the water consumed in the hydrolysis of NMP. The amount of hydrogen sulfide scattered was 0.017 mol per mole of charged alkali metal sulfide.

[0120] Next, 10420g (70.89 mol) of p-dichlorobenzene and 9078.30g (91.70 mol) of NMP were added, and the reaction vessel was sealed under nitrogen gas. While stirring at 240 rpm, the temperature was raised to 240°C at a rate of 0.6°C / min, and after reacting at 240°C for 40 minutes, the temperature was raised to 275°C at a rate of 0.8°C / min. Then, 2394g (133 mol) of ion-exchanged water was pressed into the autoclave while cooling to 250°C at a rate of 1.3°C / min. Then, it was cooled to 200°C at a rate of 1.0°C / min, and then quenched to near room temperature.

[0121] The contents were taken out and diluted with 26300g of NMP, the solvent and solids were filtered through a sieve (80 mesh), and the obtained particles were washed with 31900g of NMP and filtered. This was washed and filtered several times with 56000g of ion-exchanged water, and then washed and filtered with 70000g of 0.05% by weight acetic acid aqueous solution. After washing and filtering with 70000g of ion-exchanged water, the obtained hydrous PPS particles were dried with hot air at 80°C and dried under reduced pressure at 120°C. The obtained PPS resin (a-1) had a weight average molecular weight of 73000, a melting point of 280°C, and a carboxyl group amount of 35μmol / g.

[0122] [(b) Silicone elastomer having a crosslinked structure (b-1, b-2, b-3)] b-1: Silicone elastomer with cross-linked structure (Dowsil "EP5500" manufactured by Dow Toray), Shore hardness A: 30HS, polyorganosiloxane content: 90% or more, average primary particle diameter 3μm b-2: Silicone elastomer with cross-linked structure (Dowsil "EP2600" manufactured by Dow Toray), Shore hardness A: 50HS, polyorganosiloxane content: 90% or more, average primary particle diameter 2μm b-3: Silicone elastomer with cross-linked structure (Dowsil "EP2720" manufactured by Dow Toray), Shore hardness A: 70HS, polyorganosiloxane content: 90% or more, average primary particle size 2μm, methacryloxy group-containing

[0123] [(c) Thermoplastic elastomer (c-1)] c-1: Ethylene-glycidyl methacrylate copolymer (Sumitomo Chemical Co., Ltd. olefin resin, Bondfast ETX-6, melting point 105°C, MFR: 3g / 10min (190°C, 21.2N load)), reactive functional group content: 6% by weight

[0124] [(d) Other additives (d-1, d-2, d-3)] d-1: Silicone powder (Dowsil "Trefil F-202" manufactured by Dow Toray, a powder in which 60% by mass of silicone oil (viscosity (25°C): 60,000cs (62,000mPa s)) is supported on inorganic powder (silica)) d-2: Silicone oil (Dowsil "SH200" manufactured by Dow Toray, viscosity (25°C): 60,000cs (62,000mPa·s)) d-3: 3-isocyanatepropyltriethoxysilane (Shin-Etsu Silicone Co., Ltd. "KBE9007N")

[0125] In the following examples, material properties were evaluated by the following methods.

[0126] [Bending test] The PPS resin composition pellets of the present invention were dried at 130°C for 3 hours using a hot air dryer, and then fed to a Sumitomo Heavy Industries injection molding machine (SE-75DUZ) set at a cylinder temperature of 320°C and a mold temperature of 145°C. Using a mold with a type A1 test piece shape specified in ISO 20753 (2008), injection molding was performed under conditions where the average speed of the molten resin passing through the cross-sectional area of ​​the central parallel part was 400±50 mm / s to obtain a test piece. The central parallel part of this test piece was cut out to obtain a type B2 test piece. This test piece was conditioned for 16 hours under conditions of 23°C and 50% relative humidity, and then the flexural modulus was measured in accordance with the ISO 178 (2010) method under conditions of a span of 64 mm and a test speed of 2 mm / min.

[0127] [Tensile test] Type A1 test pieces obtained under the same molding conditions as the bending test were conditioned for 16 hours at 23°C and 50% relative humidity, after which the tensile elongation (and strain) at break was measured in accordance with ISO 527-1, 2 (2012) at a chuck distance of 114 mm and a test speed of 50 mm / min.

[0128] [Flame retardancy test] The PPS resin composition pellets of the present invention were dried at 130°C for 3 hours using a hot air dryer, and then fed into a Sumitomo Heavy Industries injection molding machine (SE-75DUZ) with a cylinder temperature of 320°C and a mold temperature of 150°C to obtain a test piece for evaluating flame retardancy. The flame retardancy of the test piece was evaluated according to the evaluation criteria set forth in the UL94 vertical test. Flame retardancy is ranked in the order of V-0>V-1>V-2. If the V-2 standard was not met, it was indicated as out. The thicknesses of the test pieces used were 1.0mmt and 0.7mmt.

[0129] [Bleed-out resistance] Type A1 test pieces obtained under the same molding conditions as those for the bending test were conditioned for 16 hours at 23°C and 50% relative humidity, then placed in a Geer oven set at 180°C and treated for 250 hours, then left to cool at room temperature for at least 24 hours, after which the bleed-out resistance was evaluated from the surface condition. Specifically, the level at which discoloration different from the base PPS resin composition was visually observed on the surface after heat treatment was judged to be poor (bad) in bleed-out resistance, and the level at which no discoloration was observed was judged to be good (good).

[0130] [Elongation retention rate before and after long-term durability treatment] Type A1 test pieces obtained under the same molding conditions as the bending test were conditioned for 16 hours at 23°C and 50% relative humidity, then placed in a Geer oven set at 180°C and treated for 250 hours, and then allowed to cool at room temperature for at least 24 hours, after which the tensile breaking elongation was measured and evaluated under the same conditions as the tensile test. The rate of change in elongation after the long-term durability treatment, when the elongation before the long-term durability treatment was taken as 100%, was calculated as the elongation retention rate.

[0131] [Tensile creep displacement] The PPS resin composition pellets of the present invention were dried at 130°C for 3 hours using a hot air dryer, and then fed into a Sumitomo Heavy Industries injection molding machine (SE-75DUZ) set at a cylinder temperature of 300°C and a mold temperature of 150°C to obtain dumbbell test pieces with a parallel part width of 6 mm and a thickness of 1.6 mm. The amount of displacement after treatment for 100 hours was evaluated using a tensile creep tester under conditions of chuck distance of 64 mm, 80°C, 20 MPa, and 100 hours.

[0132] [Melt Viscosity] The PPS resin composition pellets of the present invention were measured using a Capillograph 1B manufactured by Toyo Seiki Co., Ltd. under the conditions of 320°C, orifice length L (mm) / orifice diameter D (mm) = 10. Shear rate: 1216 s -1 The values ​​in were adopted.

[0133] [Examples 1 to 8, Comparative Examples 1 to 6] PPS resin, silicone elastomer having a crosslinked structure, thermoplastic elastomer, and other additives were dry blended according to the composition shown in Table 1, and then fed into a Japan Steel Works TEX30α twin screw extruder (L / D=30, two kneading sections) and melt-kneaded. Kneading was performed at a temperature of 300°C and a rotation speed of 300 rpm. After pelletizing with a strand cutter, the pellets were dried at 130°C for 3 hours and then subjected to injection molding. The evaluation results are shown in Table 1.

[0134] [Table 1]

[0135] The results of the above-mentioned Examples and Comparative Examples will be compared and explained.

[0136] In Examples 1 to 8, the PPS resin composition contains (a) PPS resin and (b) silicone elastomer having a crosslinked structure in a specific composition, and thus, excellent toughness represented by tensile elongation at break and flame retardancy are achieved, as well as bleed-out resistance, elongation retention rate before and after long-term durability treatment, and tensile creep properties. Comparing Examples 6 to 8, which have different Shore hardness of silicone elastomer having a crosslinked structure, Example 6, which has a low Shore hardness, is more flame retardant than Examples 7 and 8.

[0137] In Comparative Example 1, since it does not contain a silicone elastomer having a crosslinked structure, the tensile elongation at break, which is an index of toughness, is low, and the elongation retention rate before and after long-term durability treatment is also significantly inferior, compared to Examples 1 to 8. A PPS resin composition having both the flame retardancy and toughness required for battery insulating materials cannot be obtained. The flexural modulus is also high, and the flexibility required for battery insulating materials is not satisfied.

[0138] In Comparative Examples 2 and 3, a silicone compound that does not fall under component (b) was added, as compared with Example 2. In Comparative Example 2, the addition of the compound significantly reduced the tensile elongation at break and the flame retardancy. It is presumed that the toughness was reduced because inorganic silicone powder was used. On the other hand, in Comparative Example 3, in which silicone oil was used, although the toughness and flame retardancy before the heat treatment were excellent, bleed-out components presumably derived from the silicone oil were generated on the surface of the molded product due to the heat treatment, and the elongation retention rate after the heat treatment was also low, indicating that the compound is not suitable for use as a battery insulating material used in a long-term high-temperature environment.

[0139] In comparison with Examples 1 to 8, Comparative Example 4 contains a large amount of silicone elastomer having a crosslinked structure, and therefore is inferior in flame retardancy, long-term durability, and creep displacement.

[0140] Comparative Examples 5 and 6 are at the same level as Comparative Example 4 in which a thermoplastic elastomer was blended, but are inferior in flame retardancy, long-term durability, and creep displacement. It is presumed that the poor flame retardancy and long-term durability of the thermoplastic elastomer caused the deterioration of the physical properties of the resin composition.

Claims

1. A polyphenylene sulfide resin composition for use in a battery insulating member, comprising: (a) a polyphenylene sulfide resin; and (b) a silicone elastomer having a crosslinked structure, the silicone elastomer having a crosslinked structure being blended in an amount of 0.1 to 15.0 parts by weight per 100 parts by weight of the polyphenylene sulfide resin (a), the silicone elastomer having a crosslinked structure (b) having a Shore hardness A of 45 HS or less, and a flexural modulus of elasticity of 3.1 GPa or more and 3.6 GPa or less in a bending test in accordance with ISO 178 (2010) obtained by injection molding the resin composition, the resin composition being substantially free of a thermoplastic elastomer (c).

2. 2. The polyphenylene sulfide resin composition for battery insulating members according to claim 1, wherein a test piece obtained by injection molding the resin composition has a flame retardancy of V-0 as measured according to the UL94 standard on a test piece having a thickness of 1.0 mmt or less.

3. 2. The polyphenylene sulfide resin composition for battery insulating members according to claim 1, wherein a test piece obtained by injection molding the resin composition has a tensile elongation at break of 8% or more in a tensile test according to ISO 527-1, 2 (2012).

4. 2. The polyphenylene sulfide resin composition for battery insulating members according to claim 1, wherein the silicone elastomer having a crosslinked structure (b) is a fine particle having an average primary particle diameter of 100 nm to 10 μm.

5. 2. The polyphenylene sulfide resin composition for battery insulating members according to claim 1, wherein the silicone elastomer having a crosslinked structure (b) has a constitutional unit derived from an organopolysiloxane of 90% by weight or more.

6. A battery insulating member comprising the polyphenylene sulfide resin composition for battery insulating members according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Polyarylene sulfide resin composition

    JP2001002920A

  • Resin composition for gasket, manufacturing method therefor, and gasket for secondary battery

    JP2011029166A

  • Resin composition for gasket, manufacturing method therefor, and gasket for secondary battery

    JP2011029167A

  • Flat battery and tire pressure detecting device equipped with it

    JP2011187401A

  • Polyarylene sulfide composition containing a silane coupling agent and a silicone elastomer

    JP2015523416A