Pigment composition, its manufacturing method and use
The use of azo lake pigments formed with calcium and barium metal salts in pigment compositions addresses the issues of low laminate strength and transparency in gravure inks, resulting in enhanced ink layer properties for printed matter and packaging materials.
Patent Information
- Application Number
- JP2024050987
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Conventional pigment compositions used in gravure inks for laminate printing suffer from low laminate strength and decreased transparency due to rosin treatment, which affects the ink layer's properties during heating and drying.
A pigment composition comprising azo lake pigments formed through lake reactions with calcium and barium metal salts, with controlled azo dye content and particle size, and optionally including a surfactant, to enhance lamination strength and transparency.
The composition achieves an ink layer with improved lamination strength and transparency, suitable for producing high-quality printed matter and packaging materials.
Smart Images

Figure 0007586359000001 
Figure 0007586359000002 
Figure 0007586359000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pigment composition comprising an azo lake pigment. [Background technology]
[0002] Monoazo lake pigments obtained by coupling aromatic amines having a soluble group as the diazo component with 3-hydroxy-2-naphthalenecarboxylic acid, β-naphthol, etc. as the coupler component are widely used for coloring printing inks, paints, and plastics. Monoazo lake pigments are rosin-treated to make their color transparent and vivid and improve their dispersibility. Rosin treatment is a method in which an alkali salt solution of rosin (so-called rosin soap) is usually added to the coupler component or dye, and then a metal salt for the lake, such as calcium chloride, is added to precipitate the rosin on the surface of the pigment as an insoluble rosin lake metal salt.
[0003] Patent Document 1 discloses a monoazo lake pigment obtained by forming a lake from an azo dye by coupling a diazonium salt of an aromatic amine having a soluble group with a coupler component, and a coated monoazo lake pigment comprising rosin and a sulfosuccinate or a hydrolyzate thereof that coats the monoazo lake pigment. Patent Document 2 discloses a pigment composition in which rosin aluminum salt powder is added to the monoazo lake pigment. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 6-313120 [Patent Document 2] Patent Publication No. 07-278459 Summary of the Invention [Problem to be solved by the invention]
[0005] However, when using gravure inks using conventional pigment compositions for laminate printing, there was a problem that the laminate strength of the ink layer was low due to the influence of rosin treatment. Since rosin treatment contributes to accelerating the lake reaction of azo dyes, if monoazo lake pigments are not rosin treated, the azo dye remaining in the pigment composition will grow into azo dye particles when subsequently heated or dried, resulting in a problem of reduced transparency of the ink layer.
[0006] An object of the present invention is to provide a pigment composition capable of forming an ink layer having high laminate strength and good transparency. [Means for solving the problem]
[0007] <1> The pigment composition of the present invention comprises an azo lake pigment (B1) which is a lake product of an azo dye (A) with calcium, and an azo lake pigment (B2) which is a lake product of an azo dye (A) with barium, The content of the azo dye (A) in the pigment composition is from 0% by mass to 1% by mass. <2> The azo dye (A) is a compound represented by the following chemical formula (1) or (2): <1> A pigment composition. [ka] <3> The average primary particle size is 80 nm or more and 500 nm or less. <1> or <2> A pigment composition. <4> The rosin content in the pigment composition is 0% by mass or more and 10% by mass or less. <1> ~ <3> Any pigment composition. <5> In addition, surfactants are included <1> ~ <4> Any pigment composition. <6> <1> ~ <5> A method for producing the pigment composition according to any one of the above, comprising the steps of mixing a diazonium salt of an aromatic amine having a soluble group with a calcium metal salt and a barium metal salt, and then subjecting the mixture to a coupling reaction with a coupler component. <7> <1> ~ <5> A method for producing the pigment composition according to any one of the above, comprising the step of adding a calcium metal salt and a barium metal salt to the azo dye (A) and carrying out a lake reaction. <8> <1> ~ <5> A printing ink comprising any of the pigment compositions. <9> <8> A printed matter formed from the printing ink. <10> <9> Packaging material comprising the printed matter. Effect of the Invention
[0008] According to the present invention, it is possible to provide a pigment composition capable of forming an ink layer having high lamination strength and good transparency. The present invention also provides a printing ink, a printed matter, a packaging material, and a method for producing the pigment composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described in detail. The present invention is not limited to the following embodiments, and the present invention also includes embodiments that are implemented within the scope of the present invention. In this specification, "CI" means color index (CI).
[0010] The pigment composition of the present invention contains an azo lake pigment (B1) which is a lake product of an azo dye (A) with calcium, and an azo lake pigment (B2) which is a lake product of an azo dye (A) with barium, and the content of the azo dye (A) in the pigment composition is 0% by mass or more and 1% by mass or less.
[0011] The mechanism by which the pigment composition of the present invention can solve the problem is presumed to be as follows. According to an embodiment of the present invention, when a lake reaction is carried out using a calcium metal salt and a barium metal salt, the lake rate is improved and the amount of remaining azo dye is reduced compared to when a lake reaction is carried out using only a calcium metal salt. As a result, crystal growth of the pigment particles is suppressed and fine pigment particles are obtained. Due to the above-mentioned action, when the pigment composition of the present invention is used in, for example, a printing ink, a printed matter having improved printability (lamination strength) is obtained compared to a rosin-treated azo lake pigment.
[0012] <Azo Lake Pigments> The pigment composition of the present invention contains an azo lake pigment (B1) which is a lake product of an azo dye (A) with calcium, and an azo lake pigment (B2) which is a lake product of an azo dye (A) with barium.
[0013] <Azo dyes (A)> The azo dye (A) is a compound represented by the general formula (1). General formula (1) BN=NC Azo dyes (A) are compounds in which two aromatic rings are bonded by an azo group. The base component B-NH2 is diazotized to produce a diazo component (BN≡N + The compound of general formula (1) is obtained by reacting the azo dye (A) with a coupler component C. The azo dye (A) preferably has an acidic group, and examples of the acidic group include a sulfonic acid group and a carboxy group.
[0014] Examples of the base component B-NH2 include aromatic amine compounds. The aromatic amine compounds are preferably compounds having a soluble group, and examples of the soluble group include sulfonic acid groups and carboxy groups. Examples of the aromatic amines include 4-aminotoluene-3-sulfonic acid (p-toluidine-m-sulfonic acid: 4B acid), 4-amino-2-chlorotoluene-5-sulfonic acid (2B acid), 3-amino-6-chlorotoluene-4-sulfonic acid (C acid), and 2-aminonaphthalene-1-sulfonic acid (Tobias acid).
[0015] Examples of the coupler component C include 3-hydroxy-2-naphthalenecarboxylic acid, β-naphthol, and acetoacetanilide.
[0016] In the present invention, the coupler component and the aromatic amine component (base component) constituting the diazonium salt can be combined in any way. Suitable combinations of coupler components and base components include a compound represented by the following chemical formula (1) in which 4-amino-2-chlorotoluene-5-sulfonic acid and 3-hydroxy-2-naphthalenecarboxylic acid are combined, a compound represented by the following chemical formula (2) in which 4-aminotoluene-3-sulfonic acid and 3-hydroxy-2-naphthalenecarboxylic acid are combined, and a compound represented by the following chemical formula (3) in which 2-amino-5-chloro-4-methylbenzenesulfonic acid and 2-naphthol are combined. Among these, the compound represented by chemical formula (1) or chemical formula (2) is preferred from the viewpoint of hue.
[0017] [ka]
[0018] In the present invention, the polyvalent metal salt used in the lake reaction of the azo dye (A) is a divalent Ca salt or Ba salt, and more preferably a water-soluble salt thereof. Examples of the water-soluble salt include calcium chloride and barium chloride.
[0019] The azo dye shown in chemical formula (1) can be used in a lake reaction with barium to synthesize CI Pigment Red 48:1. Similarly, it can be used in a lake reaction with calcium to synthesize CI Pigment Red 48:2. The azo dye shown in chemical formula (2) can be used in a lake reaction with calcium to synthesize CI Pigment Red 57:1. Similarly, it can be used in a lake reaction with barium to synthesize CI Pigment Red 57:2. The azo dye shown in chemical formula (3) can be used in a lake reaction with barium to synthesize CI Pigment Red 53:1. Similarly, it can be used in a lake reaction with calcium to synthesize CI Pigment Red 53:2.
[0020] The mass ratio of the azo lake pigment (B1) to the azo lake pigment (B2) is preferably B1:B2=19:1 to 2:1, and more preferably 12:1 to 4:1.
[0021] <Method of producing pigment composition> The pigment composition of the present invention is preferably produced by a method including a step of mixing a diazonium salt of an aromatic amine having a soluble group with a calcium metal salt and a barium metal salt, and then carrying out a coupling reaction with a coupler component, or a method including a step of adding a calcium metal salt and a barium metal salt to an azo dye (A) and carrying out a lake reaction.
[0022] The method for producing the pigment composition will now be described in detail. In the present invention, the azo lake pigment can be synthesized by the following method. Examples of the synthesis of the azo lake pigment include Production Method 1, in which a metal salt is added to a diazo solution or a coupler solution in advance, and then an azo lake pigment is synthesized by a coupling reaction and a laking reaction, and Production Method 2, in which an azo dye is synthesized by reacting a diazo solution with a coupler solution, and then a metal salt is added and the azo dye is synthesized by a laking reaction. Among these, the above-mentioned method 1 is preferred. In addition, the above-mentioned method 2 is preferably a method in which a calcium metal salt is mixed first among the metal salts, and then a barium metal salt is mixed. This can further improve the laking reaction rate.
[0023] The content of the unreacted azo dye (A) in the pigment composition is preferably 0% by mass or more and 1% by mass or less, more preferably 0.5% by mass or less. When the content of the unreacted azo dye (A) is within the above range, the growth of the pigment particles can be further suppressed, and therefore the transparency and color development can be further improved.
[0024] The average value of the major axis of the primary particles of the pigment composition of the present invention (hereinafter also referred to as "average primary particle diameter") is preferably 80 to 500 nm, more preferably 100 to 400 nm, and even more preferably 120 to 300 nm, from the viewpoint of color development and transparency of the coating film. Details of the method for measuring the major axis and minor axis of the primary particles and the method for calculating the average value are shown in the Examples.
[0025] The pigment composition of the present invention may contain rosin as long as the problem can be solved. The content of rosin in the non-volatile content of the pigment composition is preferably 0% by mass or more and 10% by mass or less, more preferably 7% by mass or less, even more preferably 3% by mass or less, and particularly preferably 1% by mass or less.
[0026] In the pigment composition of the present invention, the total number of moles of calcium and barium contained in the calcium metal salt and barium metal salt used is preferably 50 or more, more preferably 52.5 or more, relative to 100 moles of acidic groups contained in the azo dye (A). The molar ratio of calcium to barium contained in each metal salt is preferably 19:1 to 2:1, more preferably 12:1 to 4:1.
[0027] <Surfactant> The pigment composition of the present invention can contain a surfactant. This can reduce the aggregation of pigment particles. Examples of the surfactant include anionic surfactants and nonionic surfactants. Among these, anionic surfactants are preferred. Examples of the anionic surfactant include fatty acid salts, alkyl sulfate ester salts, alkylaryl sulfonates, alkyl naphthalene sulfonates, alkyl sulfates, dialkyl sulfosuccinates, alkyl phosphates, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkylaryl ether sulfates, naphthalene sulfonate-formaldehyde condensates, polyoxyethylene alkyl ether phosphates, and polyoxyethylene alkyl phosphate ester salts. Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, polyoxyethylene-polyoxypropylene block copolymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, and glycerin fatty acid esters. Surfactants can be used alone or in combination and can be added to the coupler solution or to the suspension after coupling.
[0028] <Printing ink> The printing ink of the present invention preferably contains the pigment composition, and further contains a binder resin and a liquid medium. The liquid medium is not particularly limited as long as it is a medium capable of dispersing the pigment composition. Examples of the liquid medium include organic solvents.
[0029] Examples of the binder resin include acrylic resin, polyester resin, styrene resin, styrene-maleic acid resin, maleic acid resin, vinyl chloride-vinyl acetate copolymer resin, polyurethane resin, polyamide resin, and cellulose-based resin.
[0030] Examples of the organic solvent include aromatic organic solvents such as toluene and xylene; ketone organic solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester organic solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, and isobutyl acetate; and alcohol organic solvents such as methanol, ethanol, 1-propanol (n-propanol), isopropanol, and n-butanol.
[0031] The binder resin and the liquid medium may be used alone or in combination of two or more.
[0032] The printing ink of the present invention may contain an appropriate selection of additives, such as pigment derivatives, extender pigments, dispersants, wetting agents, adhesion aids, silica particles, leveling agents, defoamers, antistatic agents, trapping agents, antiblocking agents, wax components, isocyanate-based curing agents, and silane coupling agents. Examples of the wax component include fatty acid amide wax and hydrocarbon wax, which improve the blocking resistance of the ink layer. Examples of the printing ink of the present invention include gravure ink, flexographic ink, inkjet ink, etc. Among these, gravure ink is preferred.
[0033] <Printed material> The printed matter of the present invention has an ink layer (printed layer) formed from a printing ink. The ink layer may be a solid coating, as long as it has a halftone or dot pattern. The printing ink used for the printed matter of the present invention is not limited as long as it can form an ink layer, and gravure ink is particularly preferred. The thickness of the ink layer is about 2 to 30 μm. Gravure ink is printed by the gravure printing method. In gravure printing, the gravure ink is diluted with a diluting solvent to a viscosity and concentration suitable for printing, and then supplied to the printing unit of the printing machine. The gravure ink is then printed on a substrate, and the volatile components are removed by drying, forming a printing layer to produce a printed product.
[0034] <Base material> Examples of the substrate include polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate, polycarbonate, and polylactic acid; polystyrene-based resins such as polystyrene, AS resin, and ABS resin; nylon, polyamide, polyvinyl chloride, polyvinylidene chloride, cellophane, paper, aluminum, and the like, or film-like substrates made of composite materials of these. Vapor-deposited substrates in which inorganic compounds such as silica, alumina, and aluminum are vapor-deposited onto polyethylene terephthalate or nylon film can also be used, and further, the vapor-deposited surface of the inorganic compound or the like may be coated with polyvinyl alcohol or the like, and further, a surface treatment such as a corona treatment may be performed. The thickness of the substrate is about 10 to 250 μm.
[0035] <Packaging materials> The packaging material of the present invention includes the printed matter. For example, the packaging material may be configured by sequentially laminating a printed matter, an adhesive layer, and a sealant base material. Examples of the packaging material include packaging bodies having various shapes, such as four-sided sealed packages, three-sided sealed packages, pillow packages, stick bags, gusset bags, square bottom bags, standing pouches, deep-draw containers, vacuum packages, skin packs, zipper bags, spout pouches, twist packages, wrap packages, shrink packages, labels, liquid paper packs, and paper trays, that can store the packaged items. Note that the packaging material of the present specification is not limited to the above uses as long as it can store the contents.
[0036] Examples of items packaged in the packaging materials include food products (e.g., rice, confectionery, seasonings, edible oils and fats, cooked foods, etc.), beverages (e.g., alcoholic beverages, soft drinks, mineral water, etc.), daily necessities (e.g., medicines, cosmetics, stationery, etc.), electronic components, etc. EXAMPLES
[0037] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, unless otherwise specified, "parts" means parts by mass, and "%" means % by mass.
[0038] [Particle size measurement] The average primary particle diameter of the pigment compositions of the Examples and Comparative Examples was determined by the following method through observation with a transmission electron microscope (TEM). For 50 primary particles of the pigment composition randomly selected from multiple photographs taken at a magnification of 10,000 times using a transmission electron microscope, a rectangle with the smallest area circumscribing the image of the particle was drawn, and the length of the long side of the rectangle was taken as the long diameter, and the average long diameter was calculated. The average long diameter was rounded off to the nearest 1 digit to obtain the average primary particle diameter, which is shown in Table 1.
[0039] [Production Example 1] - Manufacturing of binder resin solution BD1 170 parts of a polyester polyol obtained from adipic acid and neopentyl glycol having a number average molecular weight of 2,000 (hereinafter referred to as "NPG / AA"), 30 parts of polyethylene glycol (hereinafter referred to as "PEG") having a number average molecular weight of 1,000, 58.8 parts of isophorone diisocyanate (hereinafter referred to as "IPDI"), and 64.7 parts of ethyl acetate were reacted with stirring under a nitrogen stream at 80°C for 4 hours to obtain a solution of a terminal isocyanate prepolymer. Next, the obtained terminal isocyanate prepolymer solution was gradually added at 40°C to a mixture obtained by mixing and stirring 25.8 parts of isophoronediamine (hereinafter "IPDA"), 2.0 parts of iminobispropylamine (hereinafter "IBPA"), 1.5 parts of 2-ethanolamine (hereinafter "2EtAm"), and 607.4 parts of a mixed solvent of ethyl acetate / isopropanol (hereinafter "IPA") = 70 / 30, and then reacted at 80°C for 1 hour to obtain a binder resin solution BD1 having a non-volatile content of 30%, an amine value of 11.1 mgKOH / g, a hydroxyl value of 4.8 mgKOH / g, and a weight average molecular weight of 40,000.
[0040] Example 1 Production of pigment composition (1) 380 parts of 4-aminotoluene-3-sulfonic acid was added as a base component to 1,700 parts of water and stirred, after which 308 parts of 35% hydrochloric acid was added for acid precipitation, and 1,100 parts of ice was added to lower the liquid temperature to 0°C. Next, 650 parts of a 35% aqueous calcium chloride solution and 42 parts of barium chloride dihydrate were added and stirred for 10 minutes. Further, 350 parts of a 40% aqueous sodium nitrite solution were added, and water was added so that the total amount became 7,000 parts, and the mixture was stirred at 0° C. for 60 minutes to obtain a diazo solution. In a separate vessel, 3,000 parts of water, 380 parts of 3-hydroxy-2-naphthalene carboxylic acid as a coupler component, and 700 parts of 25% aqueous sodium hydroxide solution were added and stirred to dissolve. 5,000 parts of water and 26 parts of roto oil (manufactured by Taiko Yushi Kagaku Kogyo Co., Ltd., alkyl sulfate ester salt) as an anionic surfactant were added and heated to 35°C, and water was added to make the total amount 11,200 parts, to obtain a coupler solution. The diazo solution was transferred to the coupler solution over 30 minutes, and the mixture was stirred for an additional 60 minutes to carry out coupling, thereby obtaining a suspension of an azo pigment composition. The suspension was heated to 80°C over 90 minutes and then cooled to 70°C to obtain a slurry containing pigment composition (1). The slurry was filtered through a Nutsche filter and washed with 18,200 parts of water to obtain a wet cake. The wet cake was dried in a dryer at 80°C for 24 hours, pulverized, and passed through a 80-mesh wire screen to obtain 935 parts of pigment composition (1).
[0041] Example 2 Production of pigment composition (2) The same procedure as in Example 1 was repeated, except that 587 parts of 35% calcium chloride and 90 parts of barium chloride dihydrate were used, to obtain 952 parts of pigment composition (2).
[0042] Example 3 Production of pigment composition (3) In the same manner as in Example 1, except that the amounts of 35% calcium chloride and barium chloride dihydrate were changed to 469 parts and 181 parts, respectively, 985 parts of pigment composition (3) were obtained.
[0043] Example 4 Production of pigment composition (4) The same procedure as in Example 1 was carried out except that 26 parts of turmeric oil was not added, to obtain 909 parts of pigment composition (4).
[0044] Example 5 Production of pigment composition (5) The same procedure as in Example 1 was carried out up to the step of obtaining a suspension of an azo pigment composition, and the obtained suspension was heated to 60°C over 60 minutes to obtain a slurry containing a pigment composition (5). This slurry was filtered through a Nutsche filter and washed with 18,200 parts of water to obtain a wet cake. This wet cake was dried in a dryer at 80°C for 24 hours, pulverized, and passed through a 80-mesh wire screen to obtain 935 parts of pigment composition (5).
[0045] Example 6 Production of pigment composition (6) The procedure was the same as in Example 1 up to the step of obtaining a suspension of the azo pigment composition, and then the suspension of the azo pigment composition was heated to 90°C over 90 minutes, and then cooled to 70°C to obtain a slurry containing the pigment composition (6). This slurry was filtered through a Nutsche filter and washed with 18,200 parts of water to obtain a wet cake. This wet cake was dried in a dryer at 80°C for 24 hours, pulverized, and passed through a 80-mesh wire screen to obtain 935 parts of the pigment composition (6).
[0046] Example 7 Production of pigment composition (7) In Example 1, no rotenone oil was added during the preparation of the coupler solution, and 116 parts of Diplosin K-25 (manufactured by Toho Chemical Industry Co., Ltd.) was added as rosin to the suspension of the azo pigment composition and stirred for 10 minutes. The temperature was then raised to 80°C over 90 minutes, and then cooled to 70°C to obtain a slurry containing the pigment composition (7). The slurry was filtered through a Nutsche filter and washed with 18,200 parts of water to obtain a wet cake. The wet cake was dried in a dryer at 80°C for 24 hours, pulverized, and passed through a 80-mesh wire screen to obtain 934 parts of the pigment composition (7).
[0047] Example 8 Production of pigment composition (8) In the same manner as in Example 7, except that Diplodin K-25 (manufactured by Toho Chemical Industry Co., Ltd.) was changed to 270 parts, 970 parts of pigment composition (8) was obtained.
[0048] Example 9 Production of pigment composition (9) 495 parts of sodium 4-amino-2-chlorotoluene-5-sulfonate was added to 1,700 parts of water and stirred, after which 308 parts of 35% hydrochloric acid was added for acid precipitation, and 1,100 parts of ice was added to bring the liquid temperature to 0° C. Further, 350 parts of a 40% aqueous sodium nitrite solution was added, and water was added so that the total amount became 7,000 parts, followed by stirring at 0° C. for 60 minutes to obtain a diazo solution.
[0049] In a separate vessel, 3,000 parts of water, 380 parts of 3-hydroxy-2-naphthalenecarboxylic acid, and 700 parts of 25% aqueous sodium hydroxide solution were added and stirred to dissolve. 4,500 parts of water were added to adjust the temperature to 15°C, and water was added so that the total amount became 11,200 parts, to obtain a coupler solution.
[0050] The diazo solution was transferred to the coupler solution over 30 minutes, and the mixture was stirred for an additional 60 minutes to effect coupling, thereby obtaining a suspension of an azo dye.
[0051] The suspension was heated to 50°C, 650 parts of 35% calcium chloride was added and stirred for 10 minutes, and 42 parts of barium chloride dihydrate was added and stirred for 10 minutes. The suspension was further heated to 90°C over 60 minutes, and then cooled to 70°C. 37 parts of PELLEX OT-P (Kao Corporation, sodium dialkyl sulfosuccinate) was added and stirred for 10 minutes to obtain a slurry containing pigment composition (9). The slurry was filtered through a Nutsche filter and washed with 18,200 parts of water to obtain a wet cake. The wet cake was dried in a dryer at 80°C for 24 hours, pulverized, and passed through an 80-mesh wire screen to obtain 971 parts of pigment composition (9).
[0052] Example 10 Production of pigment composition (10) In Example 9, the azo dye suspension was heated to 65° C. instead of 50° C., and the rest was similarly carried out to obtain 971 parts of a pigment composition (10).
[0053] Example 11 Production of pigment composition (11) In Example 9, the azo dye suspension was heated to 80° C. instead of 50° C., and the rest was similarly carried out to obtain 971 parts of a pigment composition (11).
[0054] Example 12 Production of pigment composition (12) Pigment composition (12) was obtained in the same manner as in Example 1, except that 450 parts of 2-amino-5-chloro-4-methylbenzenesulfonic acid was added instead of 380 parts of 4-aminotoluene-3-sulfonic acid, 335 parts of 35% calcium chloride aqueous solution was changed from 650 parts to 335 parts, and 14 parts of barium chloride dihydrate was changed from 42 parts to 14 parts, 291 parts of 2-naphthol was added instead of 380 parts of 3-hydroxy-2-naphthalenecarboxylic acid, and 26 parts of Demol N (sodium salt of naphthalenesulfonic acid formalin condensate manufactured by Kao Corporation) was added as a surfactant instead of 26 parts of turpentine oil.
[0055] (Example 13) Production of pigment composition (13) 380 parts of 4-aminotoluene-3-sulfonic acid was added to 1,700 parts of water and stirred, after which 308 parts of 35% hydrochloric acid was added for acid precipitation, and 1,100 parts of ice was added to bring the liquid temperature to 0° C. Further, 350 parts of a 40% aqueous sodium nitrite solution was added, and water was added so that the total amount became 7,000 parts, followed by stirring at 0° C. for 60 minutes to obtain a diazo solution.
[0056] In a separate vessel, 3,000 parts of water, 380 parts of 3-hydroxy-2-naphthalenecarboxylic acid, and 700 parts of 25% aqueous sodium hydroxide solution were added and stirred to dissolve. 4,500 parts of water and 26 parts of turmeric oil were added and heated to 15°C, and water was added to make the total amount 11,200 parts, to obtain a coupler solution.
[0057] The diazo solution was transferred to the coupler solution over 30 minutes, and the mixture was stirred for a further 60 minutes to obtain a suspension of the azo dye.
[0058] 650 parts of 35% calcium chloride was added to this suspension and stirred for 10 minutes, and 42 parts of barium chloride was added and stirred for 10 minutes. The suspension was then heated to 80°C over 90 minutes and then cooled to 70°C to obtain a slurry containing pigment composition (13). The slurry was filtered through a Nutsche filter and washed with 18,200 parts of water to obtain a wet cake. The wet cake was dried in a dryer at 80°C for 24 hours, pulverized, and passed through a 80-mesh wire screen to obtain 935 parts of pigment composition (13).
[0059] Example 14 Production of pigment composition (14) In Example 9, 37 parts of PELLEX OT-P were replaced with 26 parts of turmeric oil, and the same procedure was repeated to obtain 971 parts of pigment composition (14).
[0060] Comparative Example 1 Production of pigment composition (15) In the same manner as in Example 1, except that 650 parts of 35% calcium chloride was not added and 42 parts of barium chloride dihydrate was changed to 542 parts, 1,087 parts of pigment composition (15) was obtained.
[0061] Comparative Example 2 Production of pigment composition (16) In the same manner as in Example 14, except that 650 parts of 35% calcium chloride was not added and 42 parts of barium chloride dihydrate was changed to 542 parts, 1,185 parts of pigment composition (16) was obtained.
[0062] Comparative Example 3 Production of pigment composition (17) In the same manner as in Comparative Example 1, except that 542 parts of barium chloride dihydrate was changed to 704 parts of a 35% aqueous calcium chloride solution, 920 parts of a pigment composition (17) was obtained.
[0063] Comparative Example 4 Production of pigment composition (18) In the same manner as in Comparative Example 2, except that 542 parts of barium chloride dihydrate was changed to 704 parts of a 35% aqueous calcium chloride solution, 953 parts of pigment composition (18) was obtained.
[0064] Comparative Example 5 Production of pigment composition (19) In Comparative Example 3, 1,028 parts of pigment composition (19) was obtained in the same manner except that no fungus oil was added when preparing the coupler solution, and 568 parts of Diplodin K-25 (manufactured by Toho Chemical Industry Co., Ltd.) was added to the suspension of the azo pigment composition after coupling and stirred for 10 minutes.
[0065] Comparative Example 6 Production of pigment composition (20) In Comparative Example 4, 1,066 parts of pigment composition (20) was obtained in the same manner except that no fungus oil was added when preparing the coupler solution, and 589 parts of Diplodin K-25 (manufactured by Toho Chemical Industry Co., Ltd.) was added to the suspension of the azo pigment composition after coupling and stirred for 10 minutes.
[0066] Details of the pigment compositions prepared in Examples 1 to 14 and Comparative Examples 1 to 6 are shown in Table 1. [Table 1]
[0067] Calculation of azo dyes in pigment compositions For the pigment compositions (1) to (20) obtained in Examples 1 to 14 and Comparative Examples 1 to 6, the content of the azo dye remaining in each pigment composition was determined by the following method using liquid chromatography in accordance with the method described below. (extraction method) Preparation of standard samples 6.0 mg of pigment composition (1), (9), or (12) was completely dissolved in 30 ml of dimethylformamide (DMF), and filtered through a 0.2 μm filter to prepare a measurement sample. Furthermore, samples were also prepared by diluting the three obtained measurement samples 10 times, 20 times, and 30 times. Preparation of test samples 300 mg of pigment composition (1), 30 ml of water, and 75 g of 0.3 mm zirconia beads were placed in a 75 cc mayonnaise bottle and dispersed for 2 hours at a vibration frequency of 172 rpm using a paint shaker (SK450 manufactured by Fast & Fluid Co., Ltd.). The resulting dispersion was centrifuged for 30 minutes at a rotation frequency of 9500 rpm using a centrifuge Cectrifuge 5810 (manufactured by Eppendorf Co., Ltd.). The supernatant after centrifugation was filtered through a 0.2 μm filter to prepare a measurement sample. Measurement samples were also prepared for pigment compositions (2) to (20) in the same manner. (analytical method) The azo dye in the measurement sample was quantified using liquid chromatography (LC-MS) under the following conditions. The same quantitative analysis was repeated twice, and the average value was calculated and converted into the content in the pigment composition. Equipment: Liquid chromatography Xevo TQD (Waters) Column: Symmetry C18 180mm x 2.1mm 5μm (Waters) Temperature: 35℃ Flow rate: 0.4ml / min Injection volume of measurement sample: 10μL Column: Symmetry C18, particle size 5 μm, column length 2.1 × 150 mm Detector: 996PDA Wavelength: 520nm Eluent: (A) 50 mM ammonium acetate aqueous solution / DMF = 7 / 1, (B) DMF
[0068] [Table 2]
[0069] Preparation of calibration curves: The mass-to-volume ratio concentration mg / L of pigment compositions (1), (9), and (12) in the standard sample was plotted on the horizontal axis, and the peak area value corresponding to the azo dye obtained from the measurement by LC-MS was plotted on the vertical axis to prepare calibration curves for each. From the calibration curves and the peak area value corresponding to the azo dye in the test sample, the amount of dye component of the corresponding CINo was calculated. That is, the amount of dye component in pigment compositions (1) to (8), (13), and comparative examples (1), (3), and (5) was calculated using the calibration curve for the standard sample (R57) in which pigment composition (1) was dissolved, the amount of dye component in pigment compositions (9) to (11), (14), and comparative examples (2), (4), and (6) was calculated using the calibration curve for the standard sample (R48) in which pigment composition (9) was dissolved, and the amount of dye component in pigment composition (12) was calculated using the calibration curve for the same sample. Table 3 shows the number of the pigment composition in the standard sample corresponding to each pigment composition and the mass % of the residual azo dye in each sample.
[0070] [Table 3]
[0071] [Example 101] Preparation of solvent-based gravure ink for lamination (1) 30 parts of the pigment composition (1) obtained in Example 1, 30 parts of binder resin solution BD1 (non-volatile content 30%), 5.0 parts of vinyl chloride-vinyl acetate copolymer resin (Nissin Chemical Industry Co., Ltd. Solvine TAO vinyl chloride:vinyl acetate:vinyl alcohol = 91:2:7 (mass ratio) (non-volatile content 30% ethyl acetate solution)), and 29 parts of n-propyl acetate / IPA = 70 / 30 solution were mixed and dispersed with an Eiger mill for 20 minutes. Then, while stirring with a disperser, 3.0 parts of ethylene glycol monomethyl ether and 3.0 parts of water were mixed to obtain a solvent-based lamination gravure ink (1).
[0072] [Examples 102 to 114, Comparative Examples 101 to 106] Preparation of solvent-based gravure inks for lamination (2)-(20) Except for changing the pigment composition as shown in Table 4, the same procedure as in Example 101 was carried out to obtain solvent-based gravure inks for lamination (2) to (20).
[0073] [Table 4]
[0074] [Example 201] - Creation of printed matter (1) The obtained solvent-based lamination gravure ink (1) was diluted with a mixed solvent (methyl ethyl ketone: n-propyl acetate: IPA = 40: 40: 20) to a viscosity of 16 seconds (25 ° C, Zahn cup No. 3), and printed on the corona discharge treated surface of a 12 μm thick corona discharge treated polyester (PET) film (Toyobo Co., Ltd. E-5100) at a printing speed of 150 m / min using a Helio 175 line gradation plate (press type, 100% to 3% gradation pattern) to obtain a printed matter (1). The printing conditions were a temperature of 32 ° C, a humidity of 80%, and a printing distance of 4000 m.
[0075] [Examples 202 to 214, Comparative Examples 201 to 206] - Creation of printed matter (2) to (20) Printed matters (2) to (20) were obtained in the same manner as in Example 201, except that the solvent-based laminating gravure ink was changed as shown in Table 5.
[0076] ·Transparency The printed matter (1) to (20) were visually observed and evaluated for transparency according to the following criteria. The results are shown in Table 5. The standard printed matter was (17). Prints with evaluation results of "◎" or "○" were usable. : Extremely higher transparency than the reference print. ○: Higher transparency than the reference print. △: Transparency is equivalent to that of the reference print. X: Less transparent than the reference print.
[0077] Color development The printed matter (1) to (20) were visually observed and the color development was evaluated according to the following criteria. The results are shown in Table 5. The standard printed matter was (17). If the evaluation result was "◎" or "○", it was usable. ◎: The color development is much higher than that of the reference print. ○: Higher color development than the reference print. △: Color development is equivalent to the reference print. X: Lower color development than the standard print [Table 5]
[0078] [Example 301] - Preparation of packaging materials (1) For the obtained printed matter (1), a polyether urethane laminating adhesive (TM 320 / CAT13B manufactured by Toyo Morton Co., Ltd.) was further diluted with an ethyl acetate solution having a non-volatile content of 30% by weight, and the coating amount after drying was 2.0 g / m 2 This was then laminated with aluminum-deposited unoriented polypropylene (VMCP2203, film thickness 25 μm, manufactured by Toray Advanced Film Co., Ltd.) and dry laminated at 50°C to obtain packaging material (1). Evaluation was performed after aging the packaging material at 50°C for 48 hours.
[0079] [Examples 302 to 314, Comparative Examples 301 to 306] - Preparation of packaging materials (2) to (20) Packaging materials (2) to (20) were obtained in the same manner as in Example 301, except that the printed matter was changed as shown in Table 6. The evaluation was carried out after the packaging materials were kept at 50° C. for 48 hours.
[0080] <Evaluation of Laminate Strength> The printed portion of the obtained packaging materials (1) to (20) was cut to a width of 15 mm, and the peel strength (lamination strength) was measured at a peel speed of 300 mm / min in an atmosphere of 20°C and 65% humidity using an Intesco 201 universal tensile tester. The practical level is 0.7 N / 15 mm or more. The results are shown in Table 6. If the evaluation result is "◎", "○", or "△", the material can be used. Even if the evaluation of the laminate strength is within the usable range, if the evaluation of the transparency and color development shown in Table 5 is outside the usable range, the material cannot be used. ◎ Lamination strength is 1.0N / 15mm or more. ○···Laminate strength is 0.85N / 15mm or more and less than 1.0N / 15mm. △···Laminate strength is 0.7N / 15mm or more and less than 0.85N / 15mm. X... The laminate strength is less than 0.7N / 15mm.
[0081] <Boiling retort test> The packaging materials (1) to (20) obtained in Examples 301 to 314 and Comparative Examples 301 to 306 were made into pouches measuring 120 mm x 120 mm, and 70 g of a pseudo food containing vinegar, salad oil, and meat sauce in a weight ratio of 1:1:1 was filled and sealed. The pouches were subjected to steam retort sterilization at 135°C for 30 minutes, and the degree of peeling of the ink layer was evaluated on a three-point scale. The results are shown in Table 6. If the evaluation results are "◎" or "○", the product can be used. Even if the product is within the usable range in the boiling retort property test, it cannot be used if it is outside the usable range in the transparency and color development evaluation shown in Table 5. ⊚: No peeling at all. ○: There is a very small amount of small blister-like peeling. ×: Large and small peeling is observed over the entire surface.
[0082] [Table 6]
Claims
1. 1. A pigment composition comprising: The present invention includes an azo lake pigment (B1) which is a lake product of the azo dye (A) with calcium, and an azo lake pigment (B2) which is a lake product of the azo dye (A) with barium, The content of the azo dye (A) in the pigment composition is 0% by mass or more and 1% by mass or less, the molar ratio of the azo lake pigment (B1) to the azo lake pigment (B2) is B1:B2=19:1 to 4:1; A pigment composition, wherein the azo dye (A) is a compound represented by the following chemical formula (1) or (2): 【Chemistry 1】
2. The pigment composition according to claim 1 , wherein the average primary particle size is from 80 nm to 500 nm.
3. The pigment composition according to claim 1 , wherein the rosin content in the pigment composition is from 0% by mass to 10% by mass.
4. The pigment composition of claim 1 further comprising a surfactant.
5. A method for producing the pigment composition according to any one of claims 1 to 4, comprising the steps of mixing a diazonium salt of an aromatic amine having a solubilizing group with a calcium metal salt and a barium metal salt, and then subjecting the mixture to a coupling reaction with a coupler component.
6. A method for producing the pigment composition according to any one of claims 1 to 4, comprising the step of adding a calcium metal salt and a barium metal salt to the azo dye (A) and carrying out a lake reaction.
7. A printing ink comprising the pigment composition according to any one of claims 1 to 4.
8. A printed matter having an ink layer formed from the printing ink according to claim 7.
9. A packaging material comprising the printed matter according to claim 8.
Citation Information
Patent Citations
Improved azo lake pigments
JP1976116827A
Mixed crystal composed of raked azo dye
JP1988090572A
Monoazo lake pigment, its production, and pigment dispersion
JP1994313120A
Monoazo lake pigment composition and gravure ink
JP1995278459A
Pigment composition based on CI Pigment Yellow 191
JP2010519356A