Steel material for hot stamp forming, hot stamp forming method, and hot stamp formed member

A steel alloy with controlled austenitization and quenching processes addresses the challenges of conventional hot stamp forming by enhancing toughness and fatigue resistance, achieving high strength and elongation without tempering, suitable for automotive components.

JP7586434B2Active Publication Date: 2024-11-19BENGANG STEEL PLATES CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021173301
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-07-08
Filing Date
2021-10-22
Publication Date
2024-11-19
Estimated Expiration
2036-09-08

AI Technical Summary

Technical Problem

Conventional high-strength steel materials used in hot stamp forming face challenges such as poor forming properties, low toughness, and susceptibility to fatigue cracking, requiring tempering heat treatments that complicate the process and increase costs.

Method used

A steel alloy composition with specific elements like C, Mn, V, and Nb, combined with controlled austenitization and quenching processes, produces a martensitic structure with refined austenite grains and fine carbide precipitates, enhancing toughness and fatigue resistance without the need for tempering.

Benefits of technology

The solution achieves yield strengths of 1300-1700 MPa, tensile strengths of 1800-2200 MPa, and elongations of 6-9%, with improved toughness and resistance to fatigue cracking, simplifying the manufacturing process by eliminating tempering steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586434000006
    Figure 0007586434000006
  • Figure 0007586434000007
    Figure 0007586434000007
  • Figure 0007586434000008
    Figure 0007586434000008
Patent Text Reader

Abstract

The present invention provides a steel material for hot stamp forming having an alloy composition that is advantageous for hot stamp forming, and further provides a simpler forming method that can produce a steel material or formed member that has high toughness and fatigue crack resistance after hot stamp forming without requiring heat treatment such as tempering. [Solution] A hot stamp-formed part is manufactured using a hot stamp-formed steel material containing C, Mn, V, Si, Al, Cr, Ti, Nb, B, Mo, Ni, Cu, and Fe in a specified weight ratio, and contains VC carbides and / or composite carbides of V with Ti and Nb in austenite grains with a specified grain size and volume fraction, and after tempering heat treatment, achieves a yield strength of 1350 MPa to 1800 MPa, a tensile strength of 1700 to 2150 MPa, and an elongation of 7 to 10%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel material for hot stamp forming with ultrafine grains, a hot stamp forming method, and a hot stamp formed part. [Background technology]

[0002] background In response to the urgent demand for global energy saving, emission reduction and green economy, the automobile industry is developing in the direction of weight reduction, but the light weight of automobiles does not sacrifice safety. On the contrary, the crash safety requirements for automobiles are becoming higher and higher. Nowadays, high-strength and ultra-high-strength steels for vehicles have attracted more and more attention in the automobile industry due to their high strength and light weight. Due to the high strength, cold stamp forming method is adopted, which reduces the forming characteristics, requires a large stamp forming force, and easily produces cracks. In addition, after forming, the rebound of the parts is large, which makes it almost impossible to guarantee their shape and dimensional accuracy.

[0003] Hot stamp forming technology originating from Europe is a new forming technology that solves the above-mentioned problems. This technology involves heating a blank to a fully austenitized state, then immediately transferring it to a die with a uniform cooling system for immediate stamp forming, and simultaneously performing a quenching process to obtain ultra-high strength steel parts with a uniform martensite structure. At high temperature, the material has good stamp formability and can be stamped into complex components, while eliminating rebound impact, so that the parts have high precision and good quality. At present, major automobile manufacturers in Europe and the United States have successfully applied this high strength steel hot stamp forming technology to the manufacture of automobile parts such as A-pillars, B-pillars, bumpers, roof frames, underbody frames, door crash prevention bars, etc. Due to the high strength and the presence of martensite structure, the performance of steel for hot stamp forming in automobile crash safety depends on its toughness, cold bending properties and resistance to fatigue cracks. At present, the steel for hot stamp forming widely used in the automotive industry is a structural alloy steel represented by 22MnB5, which has problems such as high austenitizing temperature (AC3 at about 850°C), low hardenability, low toughness after forming, limited cold bending properties, fatigue cracking, etc.

[0004] Chinese Patent No. 100370054 discloses high strength steel material for hot stamp forming coated with aluminum alloy. This patent document requires a strength of more than 1000 MPa, which is 1800 MPa when the carbon content is 0.35%, and reaches 1900-2100 MPa or more when the carbon content is more than 0.5, but the document does not mention its elongation and toughness. In fact, the material with alloy composition needs tempering heat treatment to achieve the strength value and has poor toughness, which cannot meet the elongation toughness requirement of more than 1800 MPa for hot stamp forming steel and components, and high carbon content is also disadvantageous for weldability.

[0005] China Patent Publication No. 101583486 discloses a method for producing a coating strip material and its hot stamped product. The preferred embodiment of this document states that heat treatment is required after hot stamping so that the mechanical properties can reach a yield strength of 1200 MPa and a tensile strength of more than 1500 MPa, but there is no quantitative mention of ductility. The document only suggests controlling the sulfur content to ensure ductility and avoid the propagation of cracks caused by the inclusion of sulfides (requiring the sulfur content to be less than 0.002 wt%), but it is difficult and expensive to control the sulfur content to less than 20 ppm in industry. Therefore, the problem of low ductility cannot be completely solved by controlling the sulfur element content. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Chinese Patent No. 100370054 [Patent Document 2] China Patent Application Publication No. 101583486 Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, in view of the above problems of the prior art, one of the objects of the present invention is to improve the shortcomings of conventional steel materials for hot stamp forming, hot stamp forming methods, and hot stamp formed parts, and to provide a steel material for hot stamp forming having an alloy composition that is more advantageous for the hot stamp forming method, and further, a simpler forming method that makes it possible to produce a steel material or formed part that has high toughness and fatigue crack resistance after hot stamp forming without requiring heat treatment such as tempering. [Means for solving the problem]

[0008] According to an embodiment of the present invention, there is provided a steel material for hot stamp forming, comprising the following components by weight: 0.27-0.40% C, 0.2-3.0% Mn, 0.11-0.4% V, 0-0.8% Si, 0-0.5% Al, 0-2% Cr, 0-0.15% Ti, 0-0.15% Nb, 0-0.004% B, less than 2% Mo, Ni, Cu in total, and other alloy elements beneficial for improving hardenability, and other impurities.

[0009] The hot stamp forming steel material of the present invention has a temperature range of 800 to 920°C during hot stamp forming treatment, and preferably has austenite grain boundaries during austenitization treatment. In the austenitization heat treatment of the hot stamp forming steel material of the present invention, the precipitate particle size of VC carbide and / or composite carbide of V and Ti, Nb in the austenite grain boundaries is preferably 1 to 80 nm. In the hot stamp forming treatment, the hot stamp forming steel material of the present invention precipitates a certain amount of VC carbide and / or composite carbide of V and Ti, Nb in the austenite crystals including the grain boundaries during cooling after austenitization, and the carbide particle size in the austenite crystals is 0.1 to 20 nm. The volume fraction of the VC carbide and / or composite carbide of V and Ti, Nb in the hot stamp forming steel material of the present invention is 0.1% or more.

[0010] The hot stamp forming steel material of the present invention can achieve a yield strength of 1300 MPa to 1700 MPa, a tensile strength of 1800 to 2200 MPa, and an elongation of 6 to 9% after hot stamp forming without tempering, and can achieve a yield strength of 1350 MPa to 1800 MPa, a tensile strength of 1700 to 2150 MPa, and an elongation of 7 to 10% after tempering heat treatment.

[0011] The steel material of the present invention includes a hot-rolled steel sheet, a hot-rolled pickled steel sheet, a cold-rolled steel sheet, or a steel sheet with a coating layer. The steel sheet with a coating layer is a zinc-coated steel sheet, which is a hot-rolled steel sheet or a cold-rolled steel sheet having a metallic zinc layer formed thereon, and the zinc-coated steel sheet includes at least one selected from hot-dip galvanizing, annealed galvanizing, galvanizing, and zinc-iron plating. The steel sheet with a coating layer is a hot-rolled steel sheet or a cold-rolled steel sheet having an aluminum-silicon layer formed thereon, or a steel sheet with an organic coating layer.

[0012] According to another embodiment of the present invention, there is provided a hot stamp forming method which may include the steps of:

[0013] (a) Steel austenitization treatment: This involves providing a hot stamp forming steel having the above-mentioned alloy composition or a preform member thereof, heating it to 800 to 920°C, and maintaining this temperature for 1 to 10,000 seconds, where the heating method in the treatment is, but not limited to, for example, Laura These may include furnaces, box furnaces, induction heating, and resistance heating.

[0014] (b) Steel Transfer: This involves transferring the above heated steel to a hot stamp forming die while ensuring that the steel has a temperature of 550° C. or higher during transfer to the die.

[0015] (c) Hot stamp forming: This involves setting a reasonable press tonnage according to the above-mentioned steel blank size with a stamping pressure of 1-40MPa, determining the residence time according to the thickness of the plate, which is usually controlled to 4-40 seconds so that the temperature of the part is less than 250°C when the die is opened, for example, a 1.2mm thick blank has a residence time of 5-15 seconds, and a 1.8mm thick blank has a residence time of 7-20 seconds, and controlling the die surface temperature to less than 200°C by the cooling system of the die, so that the steel in the die is rapidly cooled to less than 250°C at an average cooling rate of at least 10°C / s.

[0016] According to another embodiment of the present invention, there is further provided a method of tempering comprising the steps of:

[0017] (a) A step of obtaining a formed part by the hot stamp forming method of the present invention described above.

[0018] (b) The above coating During the process, the molded part is heated to 150-200°C and maintained at this temperature for 10-40 minutes, or the molded part is heated to 150-280°C at a heating rate of 0.001-100°C / sec and maintained at this temperature for 0.5-120 minutes, and then cooled by any method.

[0019] The hot stamp formed part formed by the hot stamp forming method of the present invention can be used for high strength automotive parts including, but not limited to, A-pillar, B-pillar, bumper, roof frame, underbody frame, door bumper bar of automobile.

[0020] After hot stamp forming or equivalent heat treatment, the steel of the present invention can achieve a yield strength of 1300MPa-1700MPa, a tensile strength of 1800-2200MPa and an elongation of 6-9% after direct hot stamp quenching (without tempering). After the tempering treatment of the present invention, it is preferably possible to reach 1500MPa-1900MPa-8% and 1600MPa-2100MPa-7%. These properties cannot be achieved by direct quenching (without tempering) of the compositions of the prior art. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 shows the prior austenite grain boundary morphology of the steel of the present invention after hot stamp forming. [Diagram 2] FIG. 2 shows the precipitate particle morphology and size of the steel material of the present invention after hot stamp forming. [Diagram 3] FIG. 3 shows a diagram of the hot stamp forming method of the preferred embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Detailed explanation The present invention will be described in more detail below with reference to examples. The following examples or experimental data are provided to illustrate the present invention, and those skilled in the art should recognize that the present invention is not limited to these examples or experimental data.

[0023] According to an embodiment of the present invention, there is provided a steel material for hot stamp forming, comprising the following components by weight: 0.27-0.40% C, 0.2-3.0% Mn, 0.11-0.4% V, 0-0.8% Si, 0-0.5% Al, 0-2% Cr, 0-0.15% Ti, 0-0.15% Nb, 0-0.004% B, less than 2% Mo, Ni, Cu in total, and other alloy elements beneficial for improving hardenability, and other impurities.

[0024] Although the martensite strength improves with increasing carbon content, high carbon content leads to the formation of twin martensite, which reduces the toughness of the material. Twin martensite must be tempered to prevent brittle fracture. The steel of the present invention has a specific composition of V element added to the alloy composition, which allows the full austenitization heating temperature range during hot stamp forming processing to be 800-920°C. According to the condition of the solubility product of VC precipitation, 0.11% or more V and 0.27% or more C are added to the material, so that there is a certain amount of VC and / or (V,Ti,Nb)C composite carbides at the austenite grain boundary during the austenitization process, and the austenite grains are effectively pinned by the second phase particles, thereby refining the previous austenite grains. Therefore, the precipitation of VC has an important effect on the control of the size of the previous austenite grains. According to a preferred embodiment of the present invention, the prior austenite grain size is 3-6 μm, and the grain refinement and strengthening can not only improve the yield strength but also increase the toughness. Figure 1 illustrates the prior austenite grain boundary morphology of the steel of the present invention after hot stamp forming.

[0025] If the achievement of tensile strength of 1800 MPa or more were to depend only on high carbon addition, the martensite formed would contain twinned martensite, which would result in poor toughness and would have ductile fracture only after tempering at 170°C for 20 minutes (usually used in automotive applications). coating After tempering at 170-200°C for 10-30 minutes, the yield strength of the material can increase by 50-100 MPa, the tensile strength can decrease by about 50 MPa, and the elongation can increase by more than 5%. In the prior art (e.g., material composition and properties published by Nippon Steel Corporation), Fe-0.31C-1.3Mn-Ti-B% has an elongation of about 3.5% at brittle fracture under a strength of 1700 MPa in the hot stamp formed state (quenched), and has a strength of 1785 MPa and an elongation of 7% after tempering at 170°C for 20 minutes. Not only does poor toughness before tempering increase the risk of fatigue cracks in the component, but also, coating By welding automotive components prior to processing, the poor toughness of the components in the hot stamped condition (without tempering) makes them prone to cracking during the weld assembly process.

[0026] According to the present invention, the steel alloy composition is added with 0.11% or more V and 0.27% or more C, and VC or (V,Ti,Nb)C with a volume fraction of 0.1% or more is further precipitated during the cooling treatment of 3-30 seconds after austenitization and before the quenching of the hot stamp forming die, and the tensile strength can be increased by 100MPa or more by the uniform fine second phase particles, and preferably, the precipitate particle size is 1-20nm, the average particle size is 4.5nm, and the volume fraction is about 0.22% (0.22% is calculated from the precipitation amount in the carbon replica sample due to the transformation from 2D to 3D, and the calculated volume fraction of Thermal-Cac is 0.28%), where the occurrence frequency of 1-10nm can reach 94.4%, and the precipitation strength strengthening can reach 240MPa by the precipitation strengthening mechanism. The precipitation of VC or (V,Ti)C consumes carbon in austenite and reduces its carbon content, thereby reducing the fraction of twin martensite formed in martensite after phase transformation, and therefore, based on the VC precipitation of the present invention, the toughness of martensite itself can be improved, and although the strength of martensite decreases due to the reduction of the carbon content therein, the strength of the material is increased by the VC precipitation strengthening and the fine grain strengthening of the previous austenite grains. Figure 2 illustrates the precipitate grain morphology and size of the steel of the present invention after hot stamp forming.

[0027] Furthermore, VC and H have high binding energy and are irreversible hydrogen traps, which can easily fix hydrogen atoms around them, thereby improving the fatigue crack resistance of materials induced by hydrogen (see: Harshad Kumar Dharamshi Hansraj BHADESHIA. “Prevention of Hydrogen Embrittlement in Steels”, ISIJ International, Vol. 56 (2016), No. 1, pp. 24-36).

[0028] After hot stamp forming or equivalent heat treatment, the steel of the present invention can achieve tensile strength of 1800-2200 MPa, yield strength of 1300 MPa-1700 MPa, and elongation of 6-9% after direct hot stamp quenching without tempering. Preferably, it can reach 1400 MPa-1900 MPa-8% and 1450 MPa-2100 MPa-7%, which are not achievable by prior art alloy compositions when directly quenched (without tempering). coating Even if the function of tempering can be realized by processing, tempering heat treatment must be performed after hot stamp forming to meet the welding requirements that some brittle fractures do not occur during the welding process, whereas the main advantage of the present invention is that the process step of tempering heat treatment is eliminated, thereby simplifying the forming process.

[0029] A specific method for producing the steel material for hot stamp forming of the present invention is as follows.

[0030] (1) Smelting process using a vacuum induction furnace or converter furnace to produce smelting products in strict accordance with the above composition.

[0031] (2) A heat treatment in which the smelted steel blank is heated to a temperature of 1100-1260°C and maintained at this temperature for 30-600 minutes.

[0032] (3) A hot rolling process in which the steel blank is rolled at a temperature less than 1200°C, and the final rolling temperature is controlled to 800°C or higher to obtain a hot-rolled steel material.

[0033] (4) crimping the hot-rolled steel at a temperature range below 750°C, where the structure is mainly ferrite and pearlite. According to actual needs, the hot-rolled steel can be further pickled to obtain hot-rolled pickled steel.

[0034] Moreover, the above manufacturing method may further include one or more of the following steps.

[0035] (5) The hot-rolled steel material can be pickled and cold-rolled to obtain a cold-rolled steel material.

[0036] (6) After the cold-rolled steel material is annealed, a cold-rolled annealed plate can be produced.

[0037] (7) The surface of the cold-rolled steel material can be subjected to a coating treatment to obtain a coated steel material.

[0038] (8) The surface of the hot-rolled pickled steel material can be subjected to a coating treatment to obtain a coated steel material.

[0039] 3 illustrates a hot stamp forming process diagram of a preferred embodiment of the present invention. According to a preferred embodiment of the present invention, the hot stamp forming process of the present invention can include the following processes:

[0040] (a) Steel austenitization treatment: This involves providing any kind of hot stamp forming steel or its preform according to the first aspect of the present invention, heating it to 800-920°C, and maintaining this temperature for 1-10000 seconds, where the heating method in the treatment can be, but is not limited to, for example: Laura These may include furnaces, box furnaces, induction heating, and resistance heating.

[0041] (b) Steel Transfer: for example, this typically involves transferring the heated steel to a hot stamp forming die using, but not limited to, a manipulator or robot, while the steel has a temperature of 550° C. or higher during transfer to the die;

[0042] (c) Hot stamp forming: This involves setting a reasonable press tonnage according to the above-mentioned steel blank size with a stamping pressure of 1-40MPa, controlling the dwell time according to the thickness of the plate to be 4-40 seconds so that the temperature of the part is less than 250℃ when the die is opened, for example, a dwell time of 5-15 seconds for a 1.2mm-thick blank, and a dwell time of 7-20 seconds for a 1.8mm-thick blank, and controlling the die surface temperature to less than 200℃ by the die rapid cooling system, so that the steel in the die is rapidly cooled to less than 250℃ at an average cooling rate of at least 10℃ / sec.

[0043] The following are exemplary experimental data of the steel material of the present invention. It will be obvious to those skilled in the art that these data are merely exemplary, and the specific components and manufacturing methods of the present invention are not limited thereto.

[0044] [Table 1]

[0045] [Table 2]

[0046] [Table 3]

[0047] [Table 4]

[0048] [Table 5]

[0049] Although the preferred embodiments of the present invention have been described above, it should be understood by those skilled in the art that any possible variations or substitutions without departing from the concept of the present invention fall within the protection scope of the present invention.

[0050] Other embodiments (1) The present invention relates to The following ingredients by weight: 0.27~0.40% C, 0.2-3.0% Mn, 0.11 to 0.4% V, 0-0.8% Si, 0-0.5% Al, 0-2% Cr, 0~0.15% Ti, 0-0.15% Nb, 0~0.004% B, Less than 2% in total of Mo, Ni, Cu, and In one embodiment, the steel material for hot stamp forming is characterized by containing unavoidable impurities.

[0051] (2) The present invention may be a steel material for hot stamp forming according to (1), characterized in that the steel material for hot stamp forming has a heating temperature range of 800 to 920°C during hot stamp forming treatment, and has VC carbides and / or composite carbides of V and Ti and Nb at austenitic grain boundaries during austenitization treatment.

[0052] The present invention may be a steel material for hot stamp forming according to (2), characterized in that during the austenitizing treatment of the steel material for hot stamp forming, the precipitate particle size of VC carbides and / or composite carbides of V and Ti and Nb at the austenite grain boundaries is 1 to 80 nm.

[0053] The present invention may be a steel material for hot stamp forming according to any one of (1) to (3), characterized in that in the hot stamp forming process, during a cooling treatment after the austenitizing treatment, a certain amount of carbides of VC and / or composite carbides of V and Ti and Nb are precipitated in austenite crystals including grain boundaries, and the carbide particle size of the austenite crystals is 0.1 to 20 nm.

[0054] The present invention may be a steel material for hot stamp forming according to any one of (1) to (3), characterized in that a volume fraction of the VC carbide and / or composite carbide of V with Ti and Nb in the steel material for hot stamp forming is 0.1% or more.

[0055] The present invention may be the steel material for hot stamp forming according to any one of (1) to (3), characterized in that after the hot stamp forming, the steel material for hot stamp forming achieves a yield strength of 1300 MPa to 1700 MPa, a tensile strength of 1800 to 2200 MPa, and an elongation of 6 to 9% without tempering, and after tempering heat treatment, a yield strength of 1350 MPa to 1800 MPa, a tensile strength of 1700 to 2150 MPa, and an elongation of 7 to 10%.

[0056] The present invention may be the steel sheet according to any one of (1) to (3), characterized in that the steel material includes a hot-rolled steel sheet, a hot-rolled pickled steel sheet, a cold-rolled steel sheet, or a steel sheet provided with a coating layer.

[0057] The present invention may be a zinc-coated steel sheet, in which the steel sheet having a coating layer is a hot-rolled steel sheet or a cold-rolled steel sheet having a metallic zinc layer formed thereon, and wherein the zinc-coated steel sheet may be the steel sheet described in (7) characterized in that it includes at least one selected from hot-dip galvanizing, galvanizing annealing, galvanizing, and zinc-iron plating.

[0058] The present invention may be the steel sheet according to (7), characterized in that the steel sheet having a coating layer is a hot-rolled steel sheet or a cold-rolled steel sheet having an aluminum-silicon layer formed thereon, or a steel sheet having an organic coating layer.

[0059] The present invention relates to the following process: (a) a steel material austenitizing treatment, which comprises providing a steel material for hot stamp forming according to any one of (1) to (9) or a preform member thereof, heating it to 800 to 920°C, and maintaining this temperature for 1 to 10,000 seconds; (b) transferring the heated steel to a hot stamp forming die while the steel has a temperature of 550° C. or more during transfer to the die; (c) hot stamp forming, comprising: setting a stamping pressure of 1 to 40 MPa, setting a reasonable press tonnage according to a size of the steel blank, determining a residence time according to a thickness of the plate, which is controlled to be 4 to 40 seconds, and controlling a die surface temperature to less than 200°C by a cooling system of the die, thereby rapidly cooling the steel material in the die to less than 250°C at an average cooling rate of at least 10°C / second.

[0060] The present invention relates to a heating method in the treatment (a): Laura The hot stamp forming method may be the method according to (10), characterized in that it includes a heating furnace, a box-type heating furnace, induction heating, or resistance heating.

[0061] The present invention relates to a method for producing a method for manufacturing a semiconductor device comprising the steps of: (a) a step of obtaining a formed part by the hot stamp forming method according to any one of (1) to (10); (b) coating The tempering method may be characterized by including a step of heating the formed member to 150 to 200°C and maintaining this temperature for 10 to 40 minutes, or heating the formed member to 150 to 280°C at a heating rate of 0.001 to 100°C / sec and maintaining this temperature for 0.5 to 120 minutes, and then cooling it by any method.

[0062] The present invention can be a hot stamp-formed member that is produced from the steel material described in any of (1) to (6) by using the hot stamp forming method described in (10) or (11), and that achieves the following properties: a yield strength of 1300 MPa to 1700 MPa, a tensile strength of 1800 to 2200 MPa, and an elongation of 6 to 9%.

[0063] The present invention may be a hot stamp formed member according to (13), which is treated by the tempering method according to (12) and has properties of a yield strength of 1300 MPa to 1800 MPa, a tensile strength of 1700 to 2150 MPa, and an elongation of 7 to 10%.

[0064] The present invention may be the hot stamp formed member according to (13) or (14), which can be used for high strength automobile components including A-pillars, B-pillars, bumpers, roof frames, underbody frames, and door bumper bars.

Claims

1. The following ingredients by weight: 0.27-0.40% C; 0.2 to 3.0% Mn, 0.11 to 0.4% V, 0.16 to 0.8% Si; 0 to 0.5% Al, 0-2% Cr, 0 to 0.15% Ti, 0-0.15% Nb, 0 to 0.004% B, and Contains less than 2% Mo, Ni, and Cu in total; a steel austenitizing treatment, the treatment comprising heating a hot stamp forming steel material, the balance of which is Fe and unavoidable impurities; a hot stamp forming process including hot stamp forming the steel material for hot stamp forming heated in the steel material austenitizing treatment to obtain a primary formed body; A hot stamp formed member produced by a method including a tempering treatment including subjecting the primary formed body to a tempering heat treatment, The hot stamp forming steel material includes a hot-rolled steel sheet, a hot-rolled pickled steel sheet, a cold-rolled steel sheet, a hot-rolled steel sheet or a cold-rolled steel sheet on which an aluminum-silicon layer is formed, or a steel sheet having an organic coating layer; Precipitating VC carbides and / or composite carbides of V, Ti, and Nb in prior austenite grains and at prior austenite grain boundaries; The sum of the volume fraction of the VC carbide and the volume fraction of the composite carbide of V, Ti, and Nb is greater than 0.1%, The particle size of the VC carbide and / or the composite carbide of V with Ti and Nb in the prior austenite grains is 0.1 to 20 nm, A hot stamp formed part achieving a yield strength of 1350 MPa to 1800 MPa, a tensile strength of 1700 to 2150 MPa, and an elongation of 7 to 10%.

2. A hot stamp formed member as described in claim 1, characterized in that the precipitate particle size of the VC carbide and / or the composite carbide of V with Ti and Nb at the prior austenite grain boundary is 1 to 80 nm.

3. 2. The hot stamped formed part according to claim 1, which can be used for automotive high strength components, including A-pillar, B-pillar, bumper, roof frame, underbody frame, and door bumper bar of an automobile.

Citation Information

Patent Citations

  • High-strength alloyed aluminum-system plated steel sheet and high-strength automotive part excellent in heat resistance and after-painting corrosion resistance

    CN100370054C

  • Coated steel strips, methods of making the same, methods of using the same, stamping blanks prepared from the same, stamped products prepared from the same, and articles of manufacture which contain s

    CN101583486A

  • JP1974027236A

  • Automobile member and its production method

    JP2006183139A

  • High-strength steel material and its production method

    JP2007291464A