Wiring board and manufacturing method thereof
A wiring board with a resin substrate and sintered metal particles, featuring voids for resin penetration, addresses adhesion and environmental issues in existing methods by enhancing adhesion and eliminating photolithography, ensuring flexibility and conductivity.
Patent Information
- Application Number
- JP2021567623
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-27
- Filing Date
- 2020-12-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Existing methods for forming metal wiring on flexible substrates, such as the subtractive, semi-additive, and additive methods, require a photolithography process, leading to high costs and environmental burdens due to waste liquid treatment, and the additive method faces issues with weak adhesion between the metal wiring and the substrate.
A wiring board is manufactured with a resin substrate and a sintered body of metal particles, featuring voids with openings towards the resin substrate, allowing resin penetration to enhance adhesion, and a manufacturing method that avoids photolithography by forming a sintered body and resin substrate without it.
The solution provides a wiring board with high adhesion between metal wiring and the insulating resin substrate, maintaining flexibility and conductivity while eliminating the need for photolithography, thus reducing costs and environmental impact.
Smart Images

Figure 0007586502000003 
Figure 0007586502000004 
Figure 0007586502000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a wiring board and a manufacturing method thereof. [Background technology]
[0002] A flexible wiring board has a substrate made of a flexible organic insulating film, on which metal wiring is formed.
[0003] There are three methods for forming metal wiring on a substrate: a subtractive method, a semi-additive method, and an additive method.
[0004] Specifically, in the subtractive method, a metal foil is attached to a substrate, and wiring is formed by a photolithography process. In the semi-additive method, a thin film that serves as a seed layer is deposited on the substrate by a sputtering method or the like, and then electrolytic plating is performed to form wiring (see, for example, Patent Documents 1 and 2). However, both the subtractive method and the semi-additive method require a photolithography process, resulting in a large number of steps. In addition, waste liquid treatment is required, which results in high costs and a heavy burden on the environment.
[0005] On the other hand, the additive method is a method of forming metal wiring by directly drawing the metal wiring on a substrate by inkjet or screen printing, and has the advantage of not requiring a photolithography process. However, when the metal wiring is simply formed directly on the substrate, the adhesion strength between the metal wiring and the substrate is weak, so there is a problem that the metal wiring is easily peeled off. Therefore, in order to increase the adhesion strength between the metal wiring and the substrate, a method is known in which a Ni-Cr alloy thin film is formed on the substrate in advance as an adhesion layer, and then the metal wiring is formed (for example, see Non-Patent Document 1). However, in this method, a photolithography process is required to etch the Ni-Cr alloy thin film of the adhesion layer into a wiring shape. Therefore, the method of forming the adhesion layer also has the problems of high cost and high environmental load, as with the subtractive method and the semi-additive method, since there are many steps and waste liquid treatment is required. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Unexamined Patent Publication No. 62-72200 [Patent Document 2] Japanese Patent Application Publication No. 5-136547 [Non-patent literature]
[0007] [Non-Patent Document 1] Y. Cao, J. Tian, and X. Hu, This Solid Films, Vol. 365(1), pp. 49-52 (2000) Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a wiring board that combines the flexibility derived from a resin substrate and the high electrical conductivity derived from metal wiring, while having high adhesion between the metal wiring and an insulating resin substrate, and to provide a method for manufacturing such a wiring board without using a photolithography process. [Means for solving the problem]
[0009] The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, they have found that a wiring board having a desired function can be obtained by providing a structure in which the sintered body has a plurality of voids and a part of the resin board enters through the opening of the void, and that such a wiring board can be manufactured by forming a sintered body of metal particles and a resin board, and have completed the present invention. Specifically, the present invention provides the following embodiments.
[0010] (1) A wiring board having a resin substrate and metal wiring, the metal wiring including a sintered body of metal particles, the sintered body having a plurality of voids with openings facing the resin substrate, and a portion of the resin substrate entering the voids from the openings. Wiring board.
[0011] (2) The wiring board according to (1) above, wherein the metal particles include at least one type selected from the group consisting of copper, silver, and nickel.
[0012] (3) The wiring board according to (1) or (2), wherein the proportion of the voids is 1 volume % or more and 30 volume % or less.
[0013] (4) The wiring board according to any one of (1) to (3), wherein the voids are partially connected to each other, and the portions of the resin substrate that have entered through the openings are partially connected to each other.
[0014] (5) The wiring board according to any one of (1) to (4), wherein a resin surface layer is formed on a surface of the sintered body opposite to a boundary surface in contact with the resin substrate.
[0015] (6) A method for producing a wiring board having a resin substrate and metal wiring including a sintered body of metal particles, the method comprising: a sintered body forming step of forming the sintered body on a sintering member; a coating step of coating a solution including a resin component onto the surface of the sintered body and around the sintered body on the sintering member; a curing step of curing the resin component to form a resin substrate; and a peeling step of peeling off the sintered body and the resin substrate from the sintering member.
[0016] (7) The method for producing a wiring board according to (6) above, wherein the solution contains a precursor material of a resin or a polymerizable monomer of a resin.
[0017] (8) A method for manufacturing a wiring board having a resin substrate and metal wiring including a sintered body of metal particles, the method comprising the steps of: preparing a resin substrate; and forming the sintered body on the resin substrate.
[0018] (9) A method for manufacturing a wiring board according to (8), comprising a step of applying a solution containing a resin component onto the resin substrate and curing the resin component to form an interfacial resin layer, and the sintered body forming step comprises forming the sintered body on the interfacial resin layer.
[0019] (10) The method for producing a wiring board according to (9), wherein the solution contains a precursor material of a resin or a polymerizable monomer of a resin. Effect of the Invention
[0020] According to the present invention, it is possible to provide a wiring board that has both flexibility derived from a resin substrate and high electrical conductivity derived from metal wiring, while improving adhesion between the metal wiring and the insulating resin substrate. Furthermore, according to the method for manufacturing a wiring board of the present invention, such a wiring board can be manufactured without using a photolithography process. [Brief description of the drawings]
[0021] [Figure 1] 1 is a schematic diagram showing a cross section of a wiring board according to an embodiment of the present invention; [Diagram 2] 1A and 1B are schematic diagrams for explaining a method for manufacturing a wiring board according to the present embodiment, in which (a) and (b) show a sintered body forming step, (c) shows a resin coating step, (d) shows a resin hardening step, and (e) shows a peeling step. [Figure 3A] 13 is a diagram showing scanning electron microscope photographs of cross sections of a resin substrate and a sintered body in a sample of Example 2. FIG. [Figure 3B] FIG. 3B is an enlarged view of the cross-sectional structure of the sintered body in FIG. 3A. [Figure 3C] FIG. 4 is a diagram showing the structure after binarization processing of FIG. 3B. [Figure 4] FIG. 11 is a diagram showing a cross section near the boundary between a resin substrate and a sintered body in a sample of Example 2. [Diagram 5] FIG. 13 is a diagram showing a resin surface layer of a sintered body in a sample of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Specific embodiments of the present invention will be described in detail below. The present invention is not limited to the following embodiments, and can be practiced with appropriate modifications within the scope of the object of the present invention.
[0023] 1. Wiring board Hereinafter, the wiring board according to this embodiment will be described in detail with reference to Fig. 1. Fig. 1 is a vertical cross-sectional view of a portion of the wiring board according to this embodiment that includes a sintered body.
[0024] The wiring board 1 according to the present embodiment is a wiring board having a resin substrate 2 and metal wiring, and the metal wiring includes a sintered body 3 of metal particles. The sintered body 3 has a plurality of voids 4a, 4b, 4c, and 4d. In this specification, the voids 4a, 4b, 4c, and 4d may be collectively referred to as voids 4. At least a part of the voids 4 has openings 41a, 41b, 41c, and 41d facing the resin substrate 2, and parts 21a, 21b, and 21c of the resin substrate 2 enter the voids 4 from the openings 41a, 41b, and 41c. As shown in FIG. 1, parts 21a, 21b, and 21c of the resin substrate are bent and enter the voids 4a, 4b, and 4c. By having such a form, the contact area between the insulating resin substrate and the sintered body is increased. Furthermore, when the sintered body and the resin substrate are peeled off, the resin that has entered the voids needs to deform, so that the peeling between the sintered body and the resin substrate is suppressed. Therefore, by providing the structure of this embodiment, it is possible to improve the adhesion between the sintered body and the resin substrate.
[0025] Moreover, it is preferable that the portions 21a, 21b of the resin substrate 2 that enter through the openings 41a, 41b are connected to each other within the gap 4. By providing such a connection structure, the contact area between the sintered body and the resin substrate increases. Furthermore, when the sintered body and the resin substrate are peeled off, the resin substrate that is connected within the gap needs to be cut, so that peeling between the sintered body and the resin substrate is suppressed. Therefore, by providing the structure of this embodiment, it is possible to increase the adhesion between the sintered body and the resin substrate.
[0026] The wiring board according to this embodiment may include a configuration in which an interfacial resin layer is interposed between the resin substrate and the sintered body.
[0027] [Porosity] Moreover, the sintered body preferably has a total void ratio of 1 volume % or more and 30 volume % or less. In this specification, the void ratio is referred to as "porosity." When the void ratio is 1 volume % or more, the resin substrate has openings through which a part of the resin substrate can enter. The ratio of voids with openings toward the resin substrate increases, making it easier for a part of the resin substrate to enter into the voids, and as a result, the adhesion between the resin substrate and the sintered body can be improved. Therefore, the void ratio is preferably 1 volume % or more, more preferably 7 volume % or more, and more preferably 10 volume % or more.
[0028] On the other hand, if the porosity exceeds 30% by volume, the sintered body may be broken, and the electrical conductivity of the sintered body may be reduced. From the viewpoint of increasing the breaking resistance and electrical conductivity of the sintered body, the porosity is preferably 30% by volume or less, more preferably 27% by volume or less, and even more preferably 25% by volume or less.
[0029] The "porosity", which is the ratio of voids according to this embodiment, is calculated as follows. That is, a cross section of a sintered body is observed with a scanning electron microscope, and the area of the interior bordered by the outer periphery of the cross section is obtained as the "total cross-sectional area", and the area of voids distributed within the interior is obtained as the "void area". The numerical values given by the following formula (1) are then averaged over 10 cross sections to obtain the porosity. Porosity (%)=(Void area / Total cross-sectional area)×100...Formula (1)
[0030] In addition, the porosity in this embodiment is calculated by selecting a region that does not include the ends of the sintered body (the surface of the sintered body and the interface with the resin substrate) in an image observed by a scanning electron microscope, under conditions where the image area of the selected region is in the range of 1 / 3 to 2 / 3 of the total cross-sectional area of the sintered body.
[0031] [Resin substrate] The resin substrate 2 is a substrate that mainly contains resin, and is used to form the wiring substrate 1 by forming a sintered body 3 of metal particles on this resin substrate 2.
[0032] The resin constituting the resin substrate is not particularly limited, and may be a flexible resin such as polyimide, liquid crystal polymer, fluororesin, polyethylene terephthalate, or polyethylene naphthalate.
[0033] The resin substrate may contain, in addition to the resin, an antioxidant, a flame retardant, a filler made of inorganic particles, and the like, depending on the application of the wiring substrate.
[0034] The thickness of the resin substrate is not particularly limited. For example, if the thickness of the resin substrate is 5 μm or more, the substrate can be prevented from breaking due to bending or tensile deformation. Therefore, the thickness is preferably 5 μm or more, more preferably 10 μm or more, or 15 μm or more. On the other hand, if the thickness of the resin substrate is too large, the flexibility derived from the resin material decreases. Therefore, the thickness of the resin substrate is preferably 100 μm or less, more preferably 75 μm or less, or 50 μm or less.
[0035] Moreover, the resin substrate according to this embodiment includes a form in which an interface resin layer is provided on the boundary surface in contact with the sintered body.
[0036] [Sintered body] The sintered body in the wiring board according to this embodiment is composed of metal particles containing one or more types selected from the group consisting of copper, silver, and nickel, and functions as metal wiring for the conductive paths in the wiring board.
[0037] By using copper as the metal particles in the sintered body, it is possible to provide metal wiring exhibiting low electrical resistance at low cost. In addition, by using silver as the metal particles, the wiring does not oxidize even during high-temperature sintering. Furthermore, by using nickel as the metal particles, it is possible to suppress electromigration defects that occur under high current density load conditions.
[0038] The metal particles may be composed of a plurality of metal particles selected from the group consisting of copper, silver and nickel. In this case, the sintered body may be partially or entirely alloyed.
[0039] When voids are present inside the sintered body, there are parts with low mechanical strength. For example, there is a part called a "neck" where metal particles are sintered together to form a thin part. By selecting a flexible resin substrate for the wiring board, it can be used as a flexible circuit. When the wiring board is deformed in such an application, the force is concentrated at the neck, which makes it easy to cause localized damage.
[0040] Therefore, when the sintered body has a porous structure, it is preferable that the gaps of the porous structure contain a metal element having electrical conductivity, and in particular, it is preferable that the gaps contain a plating of the same metal element as the metal element constituting the sintered body. The metal element is preferably one or more selected from the group consisting of copper, silver, tin, and nickel. The presence of such a metal plating can disperse the force concentrated on the neck during deformation, improving durability against deformation such as bending and stretching. Furthermore, since the gaps are filled with the metal element having electrical conductivity, the electrical resistivity of the sintered body is reduced.
[0041] Depending on the type of metal element constituting the sintered body and the environment in which the wiring board is placed, the metal element in the sintered body may be oxidized inevitably. Therefore, as long as the electrical conductivity of the sintered body is ensured, for example, up to 20% or less of the metal atoms may be oxidized in terms of the number of atoms. In addition, the sintered body may contain various additives and unavoidable impurities other than copper, silver, tin, and nickel in an amount of about 30% by mass relative to the sintered body (100% by mass). The unavoidable impurities include the oxygen element in the oxide.
[0042] [Resin surface layer] The wiring board according to the present embodiment is preferably in a form including a resin surface layer on the surface located on the opposite side of the boundary surface in contact with the resin substrate in the sintered body. In this specification, the resin layer formed on the surface of the sintered body is referred to as a "resin surface layer". The sintered body has a plurality of voids distributed with a certain porosity or more. Therefore, in the process of manufacturing the wiring board according to the present embodiment on the sintering member, the resin of the resin substrate passes through the connected voids in the sintered body and spreads wet to the interface between the sintered body and the sintering member. As a result, a resin surface layer is formed on the surface of the sintered body located on the opposite side of the boundary surface in contact with the resin substrate. When used in an environment heated in the atmosphere, the surface of the sintered body is covered with the resin surface layer, so that oxidation of the surface is suppressed and the wiring board exhibits good durability, which is preferable.
[0043] 2. Manufacturing method of wiring board (1) Manufacturing Method Example 1 The method for manufacturing a wiring board according to this embodiment is a method for manufacturing a wiring board having a resin substrate and metal wiring including a sintered body of metal particles, and includes a sintered body formation step of forming the sintered body on a sintering member, a coating step of coating a solution including a resin component onto the surface of the sintered body and around the sintered body on the sintering member, a resin layer formation step of hardening the resin component to form a resin layer, and a peeling step of peeling the sintered body and the resin layer from the sintering member.
[0044] (2) Manufacturing Method Example 2 Another method for manufacturing the wiring board according to the present embodiment may be a method for manufacturing a wiring board having a resin substrate and metal wiring including a sintered body of metal particles, the method including the steps of: preparing a resin substrate; applying a solution including a resin component onto the resin substrate; curing the resin component to form a resin interface layer; and sintering the resin interface layer to form the sintered body.
[0045] A resin substrate made in advance into a film or plate shape is prepared, a metal-containing paste is applied onto the resin substrate, and a sintered body of metal particles is produced through a drying and firing process. At this time, the firing temperature of the metal-containing paste is a temperature that can prevent deterioration of the resin substrate due to heat, and for example, in the case of a polyimide substrate, it needs to be approximately 450°C or less.
[0046] The manufacturing method may also include a step of applying a solution containing a resin component onto the resin substrate, curing the resin component, and forming an interface resin layer, and the sintering step may include forming the sintered body on the interface resin layer. In order to increase the adhesion between the resin substrate and the sintered body, a resin precursor or a resin solution is applied onto the resin substrate, and an interface resin layer is formed through a predetermined heat treatment step. Thereafter, a metal-containing paste may be applied onto the interface resin layer, and a sintered body of metal particles may be produced through a drying and firing step. For example, a polyamic acid can be used as the resin precursor. For example, a polyimide varnish can be used as the resin solution.
[0047] According to the above-mentioned "(1) Manufacturing Method Example 1" and "(2) Manufacturing Method Example 2" manufacturing methods for a wiring board, a wiring board having the characteristics described in "1. Wiring board" can be obtained. That is, a wiring board having a resin substrate and metal wiring, the metal wiring including a sintered body of metal particles, the sintered body having a plurality of voids with openings facing the resin substrate, and a portion of the resin substrate entering the voids from the openings can be obtained.
[0048] The method for manufacturing a wiring board according to this embodiment will be described below with reference to Fig. 2. Fig. 2 is a schematic diagram for explaining the manufacturing method. The following description will be based on the above-mentioned "Embodiment 1 of the manufacturing method". The manufacturing method according to the present invention is not limited to embodiment 1. The above-mentioned "Embodiment 2 of the manufacturing method" can also provide a wiring board having the characteristics of the present invention.
[0049] [Sintered body formation process] The sintered body forming step according to this embodiment is shown in Figure 2 (a) and (b). The sintered body forming step is a step of forming a sintered body 6 of metal particles on a sintering member 5. The metal particles preferably contain one or more types selected from the group consisting of copper, silver, and nickel.
[0050] An example of a method for forming the sintered body 6 on the sintering member 5 will be described below. The manufacturing method according to the present invention is not limited to the following specific example. Any known or unknown example can be adopted as long as it does not impair the effects of the present invention.
[0051] (Sintering materials) It is preferable to select a sintering member such that the metal-containing paste containing metal particles applied onto the sintering member, the dried product thereof, and the sintered body formed by sintering the same will adhere to a certain degree and will not easily peel off in subsequent processes.
[0052] The material and type of the sintering member are preferably a material that does not react with metal when the metal-containing paste is sintered at high temperature. For example, an inorganic substrate made of an inorganic material can be used, and any of a carbide substrate, a nitride substrate, and an oxide substrate can be used. Specifically, examples of the inorganic material include silicon carbide (SiC), silicon nitride (Si3N4), boron nitride (BN), silicate glass (SiO2), magnesia (MgO), alumina (Al2O3), mullite (Al2O3+SiO2), and silicon (Si). Furthermore, metals such as molybdenum and tungsten that can be molded into a sheet and do not react with the metal in the paste can be used. Magnesia (MgO) or silicate glass (SiO2) are preferable in terms of good releasability when peeling off the wiring board made of the sintered body and the resin substrate from the sintering member.
[0053] A graphite substrate may also be used as the sintering member. When a graphite substrate is used as the sintering member, graphite particles may adhere to the resin layer of the wiring board, and depending on the application of the wiring board, the function of the resin layer (e.g., electrical insulation) may be impaired. In such a case, the surface of the sintering member may be coated with an insulator such as a carbide, nitride, or oxide.
[0054] As shown in this example, the surface of the sintering member may be modified or coated in consideration of the adhesion with the metal-containing paste, its dried product, and the sintered body, and the use of the resulting wiring board. The modification or coating may be either organic or inorganic.
[0055] The average roughness (Ra) of the surface of the sintering member is preferably 25 μm or less. By making the average roughness (Ra) 25 μm or less, the smoothness of the surface of the resin layer formed on the surface of the sintering member can be ensured, and the occurrence of starting points for fracture due to tensile deformation or bending deformation of the resin layer can be prevented.
[0056] (Metal-containing paste) The metal-containing paste is used to form a sintered body of a metal containing one or more selected from the group consisting of copper, silver, and nickel. Specifically, the metal-containing paste contains, for example, at least metal particles or metal oxide particles, a binder resin, and a solvent.
[0057] (Metal particles or metal oxide particles) The metal particles may contain a metal element other than copper, silver, or nickel. The content of the metal element other than copper, silver, and nickel is preferably 30 mass% or less, and may be 20 mass% or less, in terms of metal, relative to all the metal elements contained in the metal sintered body, regardless of the state.
[0058] The content of glass components such as glass frit in the metal-containing paste is not particularly limited. It is preferable that the content of glass components in the metal-containing paste is 5% by mass or less, and more preferably 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less, in terms of metal, regardless of the state of all metal elements contained in the metal-containing paste. If the content of glass components in the metal-containing paste exceeds 5% by mass, the glass components react excessively with the sintering member in the sintering process in which the sintered body is formed by the metal-containing paste. Therefore, when the resin layer is peeled off from the sintering member, the sintered body may remain on the surface of the sintering member, which is not preferable. In addition, by making the content of glass components 0.5% by mass or less, or 0.1% by mass or less, it is possible to suppress an increase in the electrical resistivity of the sintered body.
[0059] The average particle size of metal particles or metal oxide particles (D 50 The average particle diameter (D 50 The average particle diameter (D 50 By making the average particle diameter (D) 0.1 μm or more, it is possible to prevent the occurrence of disconnections due to the influence of surface irregularities of the sintering member 5, impairing the function of the wiring, and to prevent the opening of voids having a size as small as the particle diameter, making it difficult for a part of the resin substrate to enter. 50 By setting the average particle diameter (D 50 ) refers to the 50% volume particle size, and refers to the particle size measured by laser diffraction method.
[0060] The content of the metal particles or metal oxide particles is not particularly limited, but is preferably 80% by mass or more and 95% by mass or less with respect to 100% by mass of the metal-containing paste.
[0061] (binder resin) The binder resin to be mixed in the metal-containing paste is not particularly limited as long as it is a resin material that is decomposed by sintering. Examples include cellulose resins such as methyl cellulose, ethyl cellulose, and carboxymethyl cellulose, acrylic resins, butyral resins, alkyd resins, epoxy resins, and phenolic resins. Cellulosic resins that tend to react with oxygen and carbon monoxide and disappear easily from the paste are preferred. Of the cellulose resins, ethyl cellulose is preferred.
[0062] The content of the binder resin is not particularly limited. For example, it is preferably 0.1% by mass or more and 5% by mass or less with respect to 100% by mass of the metal-containing paste. If the binder resin remains in the sintered body, it increases the electrical resistivity. When sintering is performed in the atmosphere, the binder resin reacts with oxygen in the atmosphere and burns, thereby reducing the amount of binder resin remaining in the sintered body and reducing the electrical resistivity of the sintered body. Therefore, the content of the binder resin is preferably 5% by mass or less. By having the content of the binder resin be 5% by mass or less, it is possible to suppress the binder resin component from remaining in the sintered body and to make the effect on the electrical resistivity of the sintered body negligible. On the other hand, by having the binder resin in the metal-containing paste be 0.1% by mass or more, it is possible to increase the viscosity of the metal-containing paste and improve the coatability or printability of the paste. Therefore, the content of the binder resin is preferably 0.1% by mass or more.
[0063] (solvent) The solvent contained in the metal-containing paste is not particularly limited as long as it has an appropriate boiling point, vapor pressure, and viscosity. For example, hydrocarbon solvents, chlorinated hydrocarbon solvents, cyclic ether solvents, amide solvents, sulfoxide solvents, ketone solvents, alcohol compounds, polyhydric alcohol ester solvents, polyhydric alcohol ether solvents, terpene solvents, and mixtures thereof can be mentioned. Among these, texanol, butyl carbitol, butyl carbitol acetate, terpineol, and the like, which have a boiling point of about 200°C, are preferred.
[0064] The content of the solvent contained in the metal-containing paste is not particularly limited. For example, it is preferably 2% by mass or more and 25% by mass or less with respect to 100% by mass of the metal-containing paste. By making the content of the solvent 25% by mass or less, the viscosity of the metal-containing paste is reduced, and it is possible to suppress the metal-containing paste from expanding beyond the desired print shape. On the other hand, by making the content of the solvent 2% by mass or more, it is possible to improve the printability of the metal-containing paste.
[0065] In the present embodiment, the term "organic vehicle" refers to a liquid in which a binder resin, a solvent, and other organic substances added as necessary are all mixed. As the organic vehicle, one prepared by mixing a binder resin and a solvent can usually be used. Furthermore, a metal salt and a polyol may be mixed into the organic vehicle.
[0066] The method for producing the metal-containing paste is not particularly limited. For example, the binder resin and the solvent described above are mixed, and metal particles are added and kneaded using a device such as a planetary mixer. If necessary, a three-roll mill can be used to improve the dispersibility of the metal particles.
[0067] A metal-containing paste is applied or printed onto the sintering member to form a predetermined shape of wiring, electrodes, etc. Specific examples of the application or printing method include screen printing, dispenser printing, gravure printing, offset printing, and inkjet printing.
[0068] (Sintering) After the metal-containing paste is applied or printed on the member to be sintered, the member to be sintered is heated at a temperature of 600° C. or more and 800° C. or less to obtain a sintered body.
[0069] Sintering may be performed in one stage under a nitrogen atmosphere or a reducing atmosphere, or in two stages, first under an oxidizing atmosphere and then under a reducing atmosphere. When heating is performed in two stages, the heating temperatures in both stages are 600°C or higher and 800°C or lower.
[0070] The gas atmosphere when heating is performed in two stages will be described below.
[0071] The oxidizing gas in the oxidizing atmosphere may be, for example, oxygen or air. In addition, a mixture of the oxidizing gas and a gas other than the oxidizing gas may be used. The gas other than the oxidizing gas may be an inert gas (for example, nitrogen gas or argon gas).
[0072] The concentration of oxygen in the oxidizing atmosphere is not particularly limited. In terms of oxygen partial pressure, it is preferably 50 Pa or more, more preferably 60 Pa or more or 70 Pa or more. 5 When these oxygen partial pressures are converted into a volumetric concentration, the oxygen partial pressure is preferably 500 ppm or more, more preferably 600 ppm or more, or even more preferably 700 ppm or more.
[0073] By setting the oxygen concentration at 500 ppm or more, the binder resin in the metal-containing paste can be sufficiently burned and eliminated. On the other hand, if the concentration of the oxidizing gas exceeds 8000 ppm, there is a risk that a rapid reaction will occur only near the surface of the metal-containing paste. In order to sufficiently sinter the inside of the sintered body, it is preferable that the oxygen gas concentration is 8000 ppm or less.
[0074] The reducing gas may be hydrogen, carbon monoxide, formic acid, ammonia, etc. In addition, the gas other than the reducing gas may be an inert gas, such as nitrogen gas or argon gas.
[0075] The concentration of the reducing gas is not particularly limited. 5 When the reducing gas concentration is less than 0.5% by volume, the reduction of metal oxides such as copper, silver, and nickel in the sintered body is not sufficiently carried out and the metal oxides remain, so that the metal wiring after firing may have a high electrical resistivity.
[0076] When a paste containing metal particles is used, sintering may be performed under a nitrogen atmosphere, or when a paste containing metal oxide particles is used, sintering may be performed under a reducing atmosphere. In either case, the sintering temperature is preferably 600° C. or higher and 850° C. or lower.
[0077] [Coating process] The coating step according to this embodiment is shown in (c) of Fig. 2. The coating step is a step of coating the surface of the sintered body 6 and the periphery of the sintered body 6 on the member for sintering 5 with a solution 7 containing a resin component.
[0078] The resin component in the coating step according to the present embodiment may be a precursor of the resin or a polymerizable monomer of the resin. A resin or a precursor thereof that is cured by a drying process for removing the solvent or a further process may be used.
[0079] The polymerizable monomer is not particularly limited as long as it is a monomer of a resin that is cured by polymerization or further treatment, and examples thereof include monomers of flexible resins such as polyimide, liquid crystal polymer, fluororesin, polyethylene terephthalate, and polyethylene naphthalate.
[0080] Moreover, the term "precursor material" of a resin refers to a material that can be cured by some kind of treatment to obtain a flexible resin. An example of the precursor material is polyamic acid when polyimide is used as the resin. This polyamic acid is a material that changes to polyimide by imidization treatment, and can be said to be a precursor material of polyimide. Note that the precursor material according to this embodiment also includes a monomer that is polymerized and then cured by some kind of treatment.
[0081] The solvent is not particularly limited. It can be appropriately selected in consideration of the solubility of the resin component, the viscosity according to the coating method, etc. For example, in the case of polyimide resin, N-methylpyrrolidone can be used as the solvent.
[0082] The viscosity of the solution containing the resin component is not particularly limited. For example, it is preferably 0.5 Pa·s or more, more preferably 2 Pa·s or more. On the other hand, it is preferably 50 Pa·s or less, more preferably 25 Pa·s or less. When the viscosity of the solution is 0.5 Pa·s or more and 50 Pa·s, parts of the resin substrate can enter the voids of the sintered body. Furthermore, when the viscosity of the solution is 2 Pa·s or more and 25 Pa·s or less, the parts of the resin substrate that have entered the voids of the sintered body can be connected to each other, and high adhesion strength and high breaking elongation can be obtained.
[0083] The coating method is not particularly limited, and for example, a slit coater, a bar coater, a spin coater, or the like can be used.
[0084] As described above, the solution containing the resin component is applied onto the sintering member, and then dried. The drying method is not particularly limited, and for example, drying at room temperature and atmospheric pressure may be performed, or at least one of heating and decompression may be performed.
[0085] The thickness of the resin component-containing layer after drying is almost equal to the thickness of the resin substrate. The thickness of the resin component-containing layer after drying is not particularly limited. For example, it is preferably 5 μm or more, more preferably 10 μm or more, or 15 μm or more. On the other hand, it is preferably 100 μm or less, more preferably 75 μm or less, or 50 μm or less. By having a thickness of 5 m or more after drying, it is possible to prevent the substrate from breaking due to bending or tensile deformation. On the other hand, by having a thickness of 100 m or less after drying, it is possible to impart excellent flexibility.
[0086] [Curing process] The curing step according to this embodiment is shown in Fig. 2(d). The curing step is a step of converting a resin component, such as a precursor substance or a polymerizable monomer, contained in the applied or printed resin component-containing solution into a resin, and forming a resin substrate layer 8 in a cured state of the resin.
[0087] The curing method is not particularly limited, and may be heating or using various catalysts depending on the chemical species of each monomer. For example, when a polyamic acid is used as a precursor material to form a polyamide as a resin, a dehydration reaction by heating may be used.
[0088] In the method for manufacturing a wiring board according to the present embodiment, in the curing step, the resin of the resin substrate passes through the connected voids in the sintered body and spreads to the interface between the sintered body and the sintering member, forming a resin surface layer on the surface of the sintered body located on the opposite side to the interface in contact with the resin substrate.
[0089] [Peeling process] 2(e) shows the peeling step according to this embodiment. The peeling step is a step of peeling the sintered body 6 and the resin layer 8 from the sintering member 5. For example, the sintered body 6 and the resin layer 8 can be peeled off from the sintering member 5 by gripping an end of the resin layer 8 and pulling it in the peeling direction. EXAMPLES
[0090] The present invention will be further described below with reference to examples, but the present invention is not limited to these examples.
[0091] [Examples 1 to 4, Comparative Examples 1 to 2] (Sample preparation) A magnesia plate was used as the sintering member. A copper paste was printed on the surface of the sintering member by screen printing. The copper paste used contained 80% by mass of spherical particles with an average particle size of 1 μm and 20% by mass of a vehicle consisting of a mixture of a binder resin and a solvent. The printed copper paste was dried in the air at 100°C, then heat-treated in a nitrogen atmosphere to be sintered, and then cooled to room temperature. As shown in Table 1, the heat treatment temperature was appropriately changed in the range of 600°C to 850°C, and the heat treatment time was appropriately changed in the range of 30 minutes to 60 minutes, thereby obtaining sintered bodies with different porosities in Examples 1 to 4 and Comparative Examples 1 to 2. The approximate dimensions of the copper wiring of the obtained sintered bodies were a line width of 200 μm, a height of 13 μm, and a length of 6 cm.
[0092] For each sample of Examples 1 to 4 and Comparative Examples 1 to 2, a polyimide varnish (Ube Industries' product "UPIA") with a viscosity of 10 Pa·s was applied to the surface of the sintering member having a sintered body (copper wiring) by adjusting the amount of solvent. Next, a heat treatment was performed at 280°C for 10 minutes in a nitrogen atmosphere, and then at 350°C for 30 minutes to harden the polyimide varnish and form a film-like polyimide resin substrate. The thickness of the resin substrate was 25 μm at the center in contact with the sintered body and 31 μm at the end. After cooling to room temperature, the laminate consisting of the copper sintered body and the polyimide resin substrate was peeled off from the sintering member. Then, the obtained laminate was subjected to ion beam processing using a cross-section polisher (IB-19530CP manufactured by JEOL Ltd.) to obtain a flat cross section.
[0093] (Cross-section observation) The obtained laminate consisting of the copper sintered body and the polyimide resin substrate had a size of about 20 mm x about 15 mm. The copper wiring was cut vertically near the center in the longitudinal direction to obtain a sample for cross-sectional observation. The cross-sectional structure of the laminate was observed using a field emission scanning electron microscope (hereinafter abbreviated as "SEM"). The cross-sectional structure observed for the sample of Example 2 is shown in FIG. 3A. This is the part where the upper side of the copper sintered body 11 was in contact with the sintering member. It was confirmed that the entire copper sintered body was embedded in the resin substrate 12. The image portion including only the copper wiring region surrounded by the dotted frame in FIG. 3A was cut out (FIG. 3B). Then, the image was binarized using image analysis software (Image J) to obtain a black and white image as shown in FIG. 3C. The area ratio of the black part in FIG. 3C was calculated using Image J to obtain the void ratio (%).
[0094] In calculating the porosity, ten locations were arbitrarily selected from the cross-sectional structure of the sample, the porosity of each was determined, and the average value was regarded as the porosity of the sintered body in this example.
[0095] FIG. 4 is an enlarged view of the vicinity of the boundary between the copper sintered body 11 and the resin substrate 12 in FIG. 3A. The dotted line shown on the boundary 16 in FIG. 4 is a line drawn along the outer periphery of the cross section of the copper sintered body, and indicates the boundary between the copper sintered body and the resin substrate. The area located inside this boundary line and not having the copper sintered part corresponds to the void of the copper sintered body. In addition, this SEM image was visually observed, and when resin was present inside the boundary 16, it was determined that the resin had entered the void. For example, the inside of the void 13 and the void 14 present near the boundary 16 in FIG. 4 had openings 9, 10 toward the resin substrate 12, and a part of the resin of the resin substrate had entered the voids 13, 14. Furthermore, the voids 13 and 14 were connected inside the copper sintered body, and the resin 15 that had entered each void was also connected.
[0096] In this specification, when a part of the resin of the resin board is infiltrated into the voids of the copper sintered body, the wiring board is said to have "resin infiltration." Also, when the resin that has infiltrated into multiple voids in the sintered body is connected to each other, the wiring board is said to have "resin continuity."
[0097] (Measurement of electrical resistivity) The electrical resistivity of the sample of Example 2 was measured using a DC four-probe method with a probe spacing of 1 mm.
[0098] (Evaluation of Adhesion) A sample was prepared for evaluating adhesion. Copper paste was applied to a 10 mm square area on a magnesia substrate, and then sintered to obtain a flat copper sintered body. A polyimide varnish with a viscosity of 15 Pa·s was then applied, heat-treated, cooled to room temperature, and peeled off from the sintering member. A tape test was performed according to ASTM D 3359-79 using a sample in which the obtained copper sintered body and resin substrate were laminated, and the area of the peeled part of the copper sintered body peeled off from the resin substrate was measured to obtain the area ratio (%), and the adhesion between the copper sintered body and the resin substrate was evaluated. The adhesion was evaluated on a six-point scale from 0 to 5 according to the area ratio (%) of the peeled part as shown below. 5 is the highest adhesion strength and 0 is the lowest adhesion strength. 5:0 4: More than 0% and less than 5% 3: 5% to less than 15% 2: 15% to less than 35% 135% or more but less than 65% 0:65% or more
[0099] (Measurement of breaking elongation) In addition, a tensile test was performed in the longitudinal direction of the copper sintered body to measure the change in electrical resistance with increasing elongation strain. As a result, the electrical resistance increased by 40% compared to the initial value when the elongation strain was 18%. When the elongation strain was further increased, the electrical resistance increased rapidly, and the breakage of the copper sintered body was confirmed. In this example, the elongation strain (%) at which a rapid increase in electrical resistance was observed was defined as the "breakage elongation".
[0100] The results of these evaluations are shown in Table 1. Desirable results are an electrical resistivity of 4 μΩ·cm or less, an adhesion rating of 3 or more, and an elongation at break of 8% or more. More desirable results are an electrical resistivity of 3 μΩ·cm or less, an adhesion rating of 5, and an elongation at break of 13% or more.
[0101] [Table 1]
[0102] [Examples 5 to 8, Comparative Examples 3 to 4] In Examples 5 to 8 and Comparative Examples 3 to 4, samples were prepared under the same conditions as in Example 2, except that a copper sintered body with a porosity of 28% was obtained by firing at 650°C for 30 minutes, and the viscosity of the polyimide varnish was changed in the range of 0.6 to 63 Pa·s. The viscosity of the polyimide varnish was changed by adjusting the content of N-methylpyrrolidone (NMP) contained in the varnish (expressed as mass% relative to the varnish). The obtained samples were evaluated for the penetration of the resin into the voids, the continuity of the resin in the voids, the adhesion, and the breaking elongation. The results are shown in Table 2. Desirable results are an adhesion rating of 3 or more and a breaking elongation of 8% or more. More desirable results are an adhesion rating of 5 and a breaking elongation of 13% or more.
[0103] [Table 2]
[0104] (Durability evaluation) [Example 9] A plurality of samples of the copper sintered body were prepared in the same manner as in Example 2, and the cross-sectional structure of the copper sintered body was observed by SEM. FIG. 5 is an enlarged view of the surface area located on the opposite side of the boundary surface 16 where the copper sintered body 11 contacts the resin substrate. A resin surface layer 17 was formed on the surface of the sintered body, and the thickness of the resin surface layer 17 was about 0.8 μm. These samples were subjected to heat treatment at 200 ° C., 250 ° C. and 300 ° C. in the atmosphere for 10 minutes, and then cooled, and the surface of the copper sintered body was visually observed. No discoloration was observed on the surface of the copper sintered body before and after the heat treatment, and surface oxidation was suppressed. In this respect, it was confirmed that the wiring board according to the present invention has good durability against the usage environment.
[0105] The copper sintered body of Example 9 has a plurality of voids distributed therein with a porosity similar to that of Example 2. Therefore, it is presumed that when the polyimide varnish is heated and cured, the resin of the resin substrate wets and spreads through the interconnected voids in the copper sintered body to the interface between the copper sintered body and the sintering member, forming a resin surface layer of the sintered body.
[0106] [Comparative Example 5] A plurality of samples of sintered copper bodies were prepared in the same manner as in Comparative Example 1, and the cross-sectional structure near the surface of the sintered copper bodies was observed by SEM in the same manner as in Example 9. The copper bodies were then subjected to heat treatment, and the surfaces of the sintered copper bodies were visually observed. As a result, no resin surface layer was observed on the surface of the sintered copper bodies. Furthermore, the surfaces of the sintered copper bodies after the heat treatments at 200°C, 250°C, and 300°C all turned black-gray, and the surfaces were oxidized.
[0107] In the copper sintered body of Comparative Example 5, the sintering process proceeds more than in Example 9, and therefore the distribution ratio of voids is small, similar to Comparative Example 1. Therefore, it is presumed that this copper sintered body does not have connected voids large enough to allow the resin of the resin substrate to pass through, and thus the resin surface layer is not formed. [Explanation of symbols]
[0108] 1. Wiring board 2 Resin substrate 21a, 21b, 21c Part of resin substrate 3. Sintered body 4,4a,4b,4c,4d void 41a,41b,41c,41d opening 5 Sintering materials 6 Sintered body 7 solution 8 Resin substrate layer 9,10 Opening 11 Copper sintered body 12 Resin substrate 13,14 void 15 Resin 16 Boundary (dotted line) 17 Resin surface layer
Claims
1. A wiring board having a resin substrate and metal wiring, the metal wiring includes a sintered body of metal particles, the sintered body has a plurality of voids each having an opening portion facing the resin substrate, a portion of the resin substrate extends into the gap through the opening, A wiring board, wherein a resin surface layer covers a surface of the sintered body located on the opposite side to a boundary surface in contact with the resin substrate.
2. The wiring board according to claim 1 , wherein the metal particles include at least one type selected from the group consisting of copper, silver, and nickel.
3. 3. The wiring board according to claim 1, wherein the ratio of the voids is 1% by volume or more and 30% by volume or less.
4. The wiring board according to claim 1 , wherein the voids are partially connected to each other, and the portions of the resin substrate that have entered through the openings are connected to each other.
5. A wiring board as described in claim 1 or 2, containing a conductive metal element in the voids of the sintered body.
6. A method for manufacturing a wiring board according to any one of claims 1 to 5, comprising: a sintered body forming step of forming the sintered body on a sintering member; a coating step of coating a solution containing a resin component on the surface of the sintered body and around the sintered body on the sintering member; a curing step of curing the resin component to form a resin substrate; a peeling step of peeling the sintered body and the resin substrate from the sintering member; A method for manufacturing a wiring board comprising the steps of:
7. The method for manufacturing a wiring board according to claim 6 , wherein the solution contains a precursor material of a resin or a polymerizable monomer of a resin.
8. A method for manufacturing a wiring board according to any one of claims 1 to 5, comprising the steps of: preparing a resin substrate; a sintered body forming step of forming the sintered body on the resin substrate; A method for manufacturing a wiring board comprising the steps of:
9. 9. The method for manufacturing a wiring board according to claim 8, further comprising the steps of: applying a solution containing a resin component onto the resin substrate; and curing the resin component to form an interfacial resin layer; and the sintered body forming step comprises forming the sintered body on the interfacial resin layer.
10. The method for manufacturing a wiring board according to claim 9 , wherein the solution contains a precursor material of a resin or a polymerizable monomer of a resin.
Citation Information
Patent Citations
Printed circuit board with flexible resistance layer
JP1987072200A
Method of manufacturing flexible printed wiring board
JP1993136547A
Conductor film pattern and its forming method, wiring board, and electronic apparatus
JP2004281658A
Pattern-shaped body and manufacturing method thereof
JP2005322834A
Conductive substrate
JP2016110690A