Method for producing cement composition

By employing controlled mixing of carbonated water with cement to achieve a specific pH and incorporating aggregate, the method addresses the fluidity reduction issue in concrete production, enhancing both fluidity and carbon dioxide fixation.

JP7586733B2Active Publication Date: 2024-11-19TAIHEIYO CEMENT CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021030336
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-11-19
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Existing methods using water containing carbon dioxide, such as carbonated water, in concrete production face significant reductions in fluidity, and there is a need for a method to enhance fluidity while increasing the amount of carbon dioxide fixed in the concrete.

Method used

A method involving the use of carbonated water in specific proportions with cement, followed by controlled mixing steps to achieve a pH of 7.0 or more, and optionally incorporating aggregate, to produce a cement composition with improved fluidity and increased carbon dioxide fixation.

Benefits of technology

The method results in a cement composition with enhanced fluidity and greater carbon dioxide fixation, even when using carbonated water, by optimizing the mixing process and pH levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586733000001
    Figure 0007586733000001
  • Figure 0007586733000002
    Figure 0007586733000002
Patent Text Reader

Abstract

To provide a method, even when carbon dioxide-containing water is used, capable of producing a cement composition having excellent fluidity and stabilized with more carbon dioxide.SOLUTION: A method for producing a cement composition comprising cement and carbonic acid-containing water comprises: a first feed step in which carbonic acid-containing water is fed with cement by an amount of 1.2 to 20.0 mass% in the total amount (100 mass%) of the cement as a part of cement; a first mixing step in which, after the first feed step, the carbonic acid-containing water and a part of the cement are mixed to obtain a mixture with a pH of 7.0 or more; a second feed step in which the mixture obtained by the first mixing step is fed with the balance of the cement; and a second mixing step in which, after the second feed step, the mixture and the balance of the cement are mixed to obtain a cement composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a cement composition. [Background technology]

[0002] In recent years, reducing carbon dioxide emissions has become an important issue in order to prevent global warming. In relation to this, technology is being considered in which carbon dioxide captured from exhaust gases generated in cement manufacturing plants is fixed in concrete or the like. For example, Patent Document 1 describes a powder component, γ-C 2 The concrete mixture contains one or two of the following: S (symbol γ), steel slag powder (symbol B), and Portland cement (symbol C), and the total of γ and B in the total content of the above γ, B, and C is 25 to 95 mass %, and the water-cement ratio W / C is 80 to 250%. The concrete mixture is poured into a formwork, and after demolding, one or more holes are drilled in the solidified concrete to allow ventilation, and the solidified concrete is then cooled to room temperature. 2 By subjecting the material to carbonation curing in an atmosphere of CO2 concentration of 5 to 95%, a carbonation region is formed from the surface (excluding the surface inside the hole) to a depth of 20 mm or more (however, for parts with a thickness of less than 20 mm, the entire thickness of the material), and a carbonation region is also formed from the surface inside the hole. 2 A method for producing absorbent precast concrete is described, in which combustion exhaust gases emitted from factories and facilities can be used in the carbonation curing, thereby reducing the amount of carbon dioxide emissions.

[0003] Furthermore, as a method of mixing and fixing carbon dioxide gas into concrete, Patent Document 2 describes a method for mixing carbon dioxide gas into concrete, which is characterized by controlling and reducing the pressure of liquefied carbon dioxide gas pumped from a carbon dioxide gas storage facility to turn it into powdered dry ice, and then spraying this powdered dry ice into the concrete and mixing it therein. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-168436 A [Patent Document 2] Japanese Patent Application Publication No. 11-324324 Summary of the Invention [Problem to be solved by the invention]

[0005] When carbon dioxide-containing water such as carbonated water is used in the production of concrete or the like for the purpose of fixing carbon dioxide in the concrete or the like, there is a problem that the fluidity of the cement composition is significantly reduced. An object of the present invention is to provide a method for producing a cement composition that has excellent fluidity and in which a larger amount of carbon dioxide is fixed, even when water containing carbon dioxide is used. [Means for solving the problem]

[0006] As a result of intensive research into solving the above-mentioned problems, the present inventors have found that the above-mentioned objects can be achieved by a method for producing a cement composition including the steps of: supplying a portion of cement, that is, 1.2 to 20.0 mass% of the total amount of cement (100 mass%), to carbon dioxide-containing water; mixing the carbon dioxide-containing water with the portion of the cement to obtain a mixture having a pH of 7.0 or higher; supplying the remainder of the cement to the mixture; and mixing the mixture with the remainder of the cement to obtain a cement composition, and have completed the present invention. That is, the present invention provides the following [1] to [3]. [1] A method for producing a cement composition containing cement and carbon dioxide-containing water, comprising: a first supplying step of supplying a portion of the cement, i.e., 1.2 to 20.0 mass% of the total amount (100 mass%) of the cement, to the carbon dioxide-containing water; a first mixing step of mixing the carbon dioxide-containing water and a portion of the cement after the first supplying step to obtain a mixture having a pH of 7.0 or higher; a second supplying step of supplying the remainder of the cement to the mixture obtained in the first mixing step; and a second mixing step of mixing the mixture and the remainder of the cement after the second supplying step to obtain a cement composition. [2] The method for mixing a cement composition according to [1], wherein the cement composition contains aggregate, and the aggregate is further mixed in at least one of the first mixing step and the second mixing step. [3] The method for producing a cement composition according to the above [1] or [2], wherein the mixture obtained in the first mixing step has a pH of 7.0 to 11.5. Effect of the Invention

[0007] According to the method for producing a cement composition of the present invention, even when water containing carbon dioxide is used, a cement composition having excellent fluidity and in which a larger amount of carbon dioxide is fixed can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The method for producing a cement composition of the present invention is a method for producing a cement composition containing cement and carbon dioxide-containing water, and includes a first supplying step of supplying a part of the cement, that is, 1.2 to 20.0 mass% of the total amount (100 mass%) of the cement, to the carbon dioxide-containing water, a first mixing step of mixing the carbon dioxide-containing water and the part of the cement after the first supplying step to obtain a mixture having a pH of 7.0 or higher, a second supplying step of supplying the remainder of the cement to the mixture obtained in the first mixing step, and a second mixing step of mixing the mixture and the remainder of the cement after the second supplying step to obtain a cement composition. Each step will be explained in detail below.

[0009] [First supply process] This step is a step of supplying cement, which is a part of the cement contained in the cement composition produced by the production method of the present invention, in an amount of 1.2 to 20.0 mass% of the total amount (100 mass%) of the cement, to carbon dioxide-containing water. In this specification, the term "carbonated water" refers to water containing carbon dioxide gas (gaseous carbon dioxide). Specific examples include carbonated water, carbon dioxide bubble-free water, water saturated with dry ice, and carbon dioxide fine bubble water having bubbles containing carbon dioxide gas (e.g., carbon dioxide microbubble water, carbon dioxide ultrafine bubble water, etc.). Carbonated water can be obtained, for example, by blowing carbon dioxide gas into water under high pressure. Water containing dissolved carbon dioxide without bubbles can be obtained, for example, by blowing carbon dioxide into water under normal pressure. The carbon dioxide gas or the carbon dioxide gas used as a raw material for dry ice may be a gas obtained by separating and recovering carbon dioxide from exhaust gas generated in cement production, etc. By using such a gas, it is possible to reduce the amount of carbon dioxide emitted in cement production, etc.

[0010] Fine bubble water is water that contains air bubbles, and in which the proportion of air bubbles having a particle size of less than 100 μm is 50 vol% or more of the total volume (100 vol%) of the air bubbles. Examples of carbon dioxide fine bubble water containing bubbles containing carbon dioxide gas include carbon dioxide ultrafine bubble water in which the proportion of bubbles with a particle size of less than 1 μm is 50% or more by volume of the total bubble volume (100% by volume), and carbon dioxide microbubble water in which the proportion of bubbles with a particle size of 1 μm or more and less than 100 μm is 50% or more by volume of the total bubble volume (100% by volume). The gas constituting the bubbles contains carbon dioxide gas. The content of carbon dioxide gas in the gas constituting the bubbles is preferably 5% by volume or more, more preferably 20% by volume or more, and particularly preferably 40% by volume or more. If the content is 5% by volume or more, the amount of carbon dioxide fixed in the cement composition can be increased. As the gas constituting the bubbles, exhaust gas generated in cement production or the like, or gas obtained by separating and recovering carbon dioxide from the exhaust gas, or the like, may be used. By using the exhaust gas or gas obtained by separating and recovering carbon dioxide from the exhaust gas, or the like, the amount of carbon dioxide emitted in cement production or the like can be reduced.

[0011] The amount of carbon dioxide gas in the carbon dioxide-containing water is preferably 500 to 10,000 mg / L, more preferably 1,000 to 9,000 mg / L, further preferably 1,500 to 8,000 mg / L, and particularly preferably 3,000 to 7,000 mg / L. If the concentration is 500 mg / L or more, the amount of carbon dioxide fixed in the cement composition can be increased. If the amount is 10,000 mg / L or less, the pH value when mixing the cement composition does not become excessively low, and the fluidity of the cement composition can be prevented from decreasing. The amount of carbonated water may be a general amount of water in cement compositions such as paste, mortar, and concrete, for example, an amount such that the mass ratio of carbonated water to cement (carbonated water / cement) is 0.2 to 0.6.

[0012] The above cement is not particularly limited, and examples thereof include various Portland cements such as ordinary Portland cement, high-early-strength Portland cement, moderate-heat Portland cement, and low-heat Portland cement, mixed cements such as blast-furnace cement and fly ash cement, and ecocement, etc. These may be used alone or in combination of two or more.

[0013] In this step, the amount of the part of cement supplied to the carbon dioxide-containing water is 1.2 to 20.0 mass% of the total amount of cement contained in the cement composition (100 mass%), preferably 1.3 to 18.0 mass%, more preferably 1.4 to 16.0 mass%, even more preferably 1.8 to 12.0 mass%, and particularly preferably 2.5 to 8.0 mass%. If the amount is less than 1.2 mass%, the pH of the mixture obtained in the first mixing step may be less than 7.0, and the effect of improving the fluidity of the cement composition is reduced compared to the case where the entire amount of cement is mixed with the carbon dioxide-containing water. If the amount exceeds 20.0 mass%, the fluidity and strength development of the cement composition are reduced. In this process, the method of supplying a portion of the cement to the carbon dioxide-containing water is not particularly limited. For example, the carbon dioxide-containing water may be introduced into a mixer or the like, and then a portion of the cement may be introduced, or the carbon dioxide-containing water and a portion of the cement may be introduced into the mixer or the like simultaneously.

[0014] [First mixing process] This step is a step provided after the first supplying step, in which the carbonated water and a part of the cement are mixed to obtain a mixture having a pH of 7.0 or more. The pH of the mixture obtained by mixing the carbonated water and a part of the cement is 7.0 or more, preferably 7.2 to 11.5, more preferably 7.6 to 11.3, further preferably 8.5 to 11.0, and particularly preferably 9.0 to 10.7. If the pH is less than 7.0, the effect of improving the fluidity of the cement composition is reduced compared to the case where the entire amount of the cement is mixed with the carbonated water. The mixing is preferably carried out for 5 seconds or more, more preferably 8 to 30 seconds, and particularly preferably 10 to 20 seconds, after a portion of the cement is supplied to the carbonated water in the previous step. By carrying out the mixing for 5 seconds or more, the fluidity of the cement composition can be further improved.

[0015] [Second supply process] This step is a step of supplying the remainder of the cement to the mixture obtained in the previous step. The remainder of the cement is the amount of cement obtained by subtracting the amount of cement used in the first supply step from the total amount of cement contained in the cement composition produced by the production method of the present invention. [Second mixing process] This step is a step provided after the second supplying step, and is a step of producing a cement composition by mixing the mixture obtained in the first mixing step with the remainder of the cement.

[0016] The cement composition to be produced in the present invention may be a paste containing no aggregate, or may be a mortar or concrete containing aggregate. The aggregate contained in the cement composition may be fine aggregate alone or a combination of fine and coarse aggregates. In addition, any of natural aggregates, artificial aggregates, and recycled aggregates may be used. The fine aggregate is not particularly limited, and examples thereof include river sand, mountain sand, land sand, sea sand, crushed sand, silica sand, slag fine aggregate, lightweight fine aggregate, and mixtures thereof. The coarse aggregate is not particularly limited, and examples thereof include river gravel, mountain gravel, land gravel, sea gravel, crushed stone, slag coarse aggregate, lightweight coarse aggregate, and mixtures thereof. The amount of aggregate to be mixed (the total amount when fine aggregate and coarse aggregate are used in combination) is not particularly limited, and may be a general amount used in mortar or concrete.

[0017] When the cement composition contains aggregate, the aggregate may be mixed with other materials in at least one of the first mixing step and the second mixing step. For example, when the aggregate is mixed in the first mixing step, the carbon dioxide-containing water, a part of the cement, and the aggregate are mixed. The method of mixing each material is not particularly limited, and the carbon dioxide-containing water and a part of the cement may be mixed, and then the aggregate may be added and mixed, or the carbon dioxide-containing water, a part of the cement, and the aggregate may be mixed simultaneously. In the case where aggregate is mixed in the second mixing step, the mixture obtained in the first mixing step, the remaining part of the cement, and the aggregate are mixed. The method of mixing each material is not particularly limited, and the mixture and the remaining part of the cement may be mixed, and then the aggregate may be added and mixed, or the mixture, the remaining part of the cement, and the aggregate may be mixed simultaneously. Alternatively, the aggregate may be mixed in two separate steps, a first mixing step and a second mixing step. Among these, from the viewpoint of ease of production, etc., a method in which, in the second mixing step, the mixture is mixed with the remainder of the cement, and then aggregate is added and mixed is preferred.

[0018] The cement composition may contain other materials as necessary. Examples of other materials that may be contained as necessary include various admixtures such as AE agents, water reducing agents, AE water reducing agents, high performance water reducing agents, and high performance AE water reducing agents, as well as various admixtures such as fly ash, silica fume, and ground granulated blast furnace slag. The method of mixing the other materials is not particularly limited, but it is preferable that the various admixtures are mixed in the second mixing step from the viewpoint of not affecting the pH of the mixture obtained in the first mixing step. EXAMPLES

[0019] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Materials used] (1) Cement: ordinary Portland cement, manufactured by Taiheiyo Cement Corporation (2) Water; Carbonated water (carbon dioxide content: 6,000 mg / liter) (3) Fine aggregate: mountain sand (4) AE water reducing agent; product name "Master Polyhede 15SR" manufactured by Pozzolith Corporation

[0020] [Examples 1 to 6] Cement (part of cement) in an amount shown in Table 1 in 100% by mass of cement used and carbonated water mixed with an AE water reducing agent in advance were simultaneously charged into the mixer, and mixed for 10 seconds to obtain a mixture with a pH value shown in Table 1 (indicated as "after adding part of cement" in Table 1). The pH of the carbonated water before adding part of the cement was 4.7. Next, the remainder of the cement (cement in an amount obtained by subtracting the ratio shown in Table 1 from 100% by mass of cement) was charged into the mixture in the mixer, and mixed for 30 seconds to obtain a mixture. Next, fine aggregate was charged into the mixture in the mixer and mixed for 30 seconds, after which the kneaded material attached to the inner wall of the mixer was scraped off, and the mixture was mixed for another 60 seconds to produce mortar (the above-mentioned mortar production method is indicated as kneading method "II" in Table 1). The above mixing was performed in an environment of 20°C. The amounts of each material mixed were such that the mass ratio of carbonated water to cement (carbonated water / cement) was 0.5, and the mass ratio of fine aggregate to cement (fine aggregate / cement) was 2.44. The amount of AE water reducer mixed was 1.0 part by mass per 100 parts by mass of cement.

[0021] The 15-stroke flow value of the resulting mortar immediately after mixing, 30 minutes after mixing, and 60 minutes after mixing, as well as the mortar compressive strength at 1 day, 7 days, and 28 days were measured in accordance with JIS R 5201:2015 (Physical testing methods for cement). The mass of carbon dioxide fixed in the mortar was determined as the mass per ton of cement contained in the mortar by thermogravimetry-differential thermal analysis (TG-DTA). Specifically, from the measurement results of thermogravimetry-differential thermal analysis (TG-DTA), the decrease in mass in the endothermic peak range of about 550 to 800°C was determined to be due to decarbonation of calcium carbonate contained in the mortar, and the amount of carbon dioxide was calculated from the amount of the decrease.

[0022] [Comparative Example 1] The entire amount of cement and water previously mixed with an AE water reducing agent were simultaneously poured into the mixer and mixed for 30 seconds. Next, fine aggregate was poured into the mixture in the mixer and mixed for 30 seconds, after which the kneaded material adhering to the inner wall of the mixer was scraped off and further mixed for 60 seconds to produce mortar (in Table 1, the above-mentioned mortar production method is shown as kneading method "I"). The pH of the water before the cement was poured was 8.0, and the above mixing was carried out in an environment of 20°C. The amounts of each material mixed were such that the mass ratio of water to cement (water / cement) was 0.5 and the mass ratio of fine aggregate to cement (fine aggregate / cement) was 2.44. The amount of AE water reducer mixed was 1.0 part by mass per 100 parts by mass of cement. The 15-pile flow value and other properties of the resulting mortar were measured in the same manner as in Example 1.

[0023] [Comparative Example 2] A mortar was produced in the same manner as in Comparative Example 1, except that carbonated water was used instead of water. The 15-pile flow value and other properties of the resulting mortar were measured in the same manner as in Example 1. [Comparative Example 3] Mortar was produced in the same manner as in Example 1, except that as part of the cement, cement was used in an amount corresponding to the proportion shown in Table 1, and as the remainder of the cement, cement was used in an amount obtained by subtracting the proportion shown in Table 1 from 100% by mass of cement. The 15-pile flow value and other properties of the resulting mortar were measured in the same manner as in Example 1.

[0024] For each of Examples 1 to 6 and Comparative Examples 1 to 3, the 15-shot flow value, the mortar compressive strength at ages of 1 day, 7 days, and 28 days, and the amount of carbon dioxide absorbed from the carbonated water and fixed in the mortar are shown in Table 2. In Examples 1 to 6 and Comparative Examples 1 to 3, the amount of carbon dioxide calculated from the TG-DTA measurements includes that derived from calcium carbonate of limestone contained in cement, which is a raw material for mortar. Since the type and amount of cement used in Examples 1 to 6 and Comparative Examples 1 to 3 are the same, the amount of carbon dioxide absorbed from the carbonated water and fixed in the mortar can be calculated by subtracting the amount of carbon dioxide in Comparative Example 1 (all of which is derived from the limestone contained in the cement, and the mass of carbon dioxide per ton of cement is 35.4 kg at an age of 1 day, 35.0 kg at an age of 7 days, and 35.3 kg at an age of 28 days) from the amount of carbon dioxide in each of Examples 1 to 6 and Comparative Examples 2 to 3.

[0025] [Table 1]

[0026] [Table 2]

[0027] From Table 2, comparing Comparative Example 1 with Comparative Example 2 (which was the same as Comparative Example 1 except that carbonated water was used instead of water), it can be seen that the 15-shot flow value of Comparative Example 2 (immediately: 178 mm, after 30 minutes: 163 mm, after 60 minutes: 159 mm) is smaller than the 15-shot flow value of Comparative Example 1 (immediately: 232 mm, after 30 minutes: 210 mm, after 60 minutes: 204 mm), and that when carbonated water is used instead of water, the fluidity of the cement composition decreases. On the other hand, in Examples 1 to 6, the 15-attach flow values ​​of the mortar (immediately: 195 to 230 mm, after 30 minutes: 187 to 216 mm, after 60 minutes: 175 to 199 mm) are larger than the 15-attach flow values ​​(immediately: 178 to 180 mm, after 30 minutes: 163 to 170 mm, after 60 minutes: 159 to 162 mm) of Comparative Example 2 (a mortar produced by kneading method "I" using carbonated water) and Comparative Example 3 (a mortar produced by kneading method "II" similarly to Examples 1 to 3, except that 1.0 mass% of cement was used as part of the cement and the pH after mixing part of the cement with carbonated water was 6.7). This shows that the manufacturing method of the present invention can improve the fluidity of the cement composition, even though carbonated water is used. It is also clear that in Examples 1 to 6, the mass of carbon dioxide per ton of cement that was taken from the carbonated water and fixed in the mortar (1 day: 18.9 to 20.7 kg / ton, 7 days: 19.9 to 21.3 kg / ton, 28 days: 19.6 to 20.3 kg / ton) is greater than the mass of carbon dioxide per ton of cement that was taken from the carbonated water and fixed in the mortar in Comparative Examples 2 and 3 (1 day: 12.7 to 14.9 kg / ton, 7 days: 13.4 to 15.6 kg / ton, 28 days: 12.8 to 14.5 kg / ton).

Claims

1. A method for producing a cement composition comprising cement and carbon dioxide-containing water, comprising: A first supply step of supplying a part of the cement, that is, a cement amount of 1.2 to 20.0 mass% of the total amount (100 mass%) of the cement, to the carbon dioxide-containing water; a first mixing step of mixing the carbon dioxide-containing water and a part of the cement after the first supply step to obtain a mixture having a pH of 7.0 or more; a second supplying step of supplying the remainder of the cement to the mixture obtained in the first mixing step; a second mixing step of mixing the mixture with the remainder of the cement after the second supplying step to obtain a cement composition; A method for producing a cement composition comprising the steps of:

2. The cement composition comprises aggregate, 2. The method for mixing a cement composition according to claim 1, wherein the aggregate is further mixed in at least one of the first mixing step and the second mixing step.

3. The method for producing a cement composition according to claim 1 or 2, wherein the mixture obtained in the first mixing step has a pH of 7.0 to 11.5.

Citation Information

Patent Citations

  • Method and device for mixing carbon dioxide with concrete

    JP1999324324A

  • Special mineral water for manufacturing heat resistant, fire resistant and reinforced concrete and its manufacturing method

    JP2006298737A

  • Concrete kneading material, co2 absorption precast concrete and method of producing the same

    JP2011168436A

  • Water for concrete production, and method for producing the same

    JP2014213479A

  • Ready mixed concrete

    JP2016002747A