Anti-flowing-water double-liquid synchronous grouting material and preparation method thereof

By using the synergistic effect of specific components in the dual-liquid grouting material, the water erosion performance and settling time are improved, and the problem that the prior art is difficult to meet the strength and settling time requirements in the water-moving environment is solved, and high retention rate is achieved and suitable construction time, while reducing environmental pollution.

CN119059770AActive Publication Date: 2024-12-03CHINA RAILWAY SHISIJU GROUP CORP +4

Patent Information

Application Number
CN202411144803.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-03
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

It is difficult for existing dual-liquid grouting materials to meet the requirements of settling time and strength at the same time in a water-moving environment, and some materials are toxic, which may cause pollution to the environment.

Method used

The anti-moving dual-liquid synchronous grouting material with a volume ratio of 4 to 6 and liquid B is used. Liquid A includes cement, fly ash, fine sand and water reducer, and Liquid B includes polymer aluminum sulfate, aluminum oxide, Hydroxypropylmethylcellulose, calcium hydroxide, triethanolamine, fatty alcohol polyoxyethylene ether and polyacrylamide improve the material's water-resistant erosion performance and settling time through the synergistic effect of these components.

Benefits of technology

In a water-moving environment of 0.8m/s, the retention rate is higher than 65%, the initial settling time is 25~50s, and the final settling time is 70~140min. It not only meets the needs of fast condensation, but also ensures sufficient construction time. Small environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001920190000081
    Figure BDA0005001920190000081
Patent Text Reader

Abstract

The invention discloses an anti-flowing-water double-liquid synchronous grouting material and a preparation method thereof, and belongs to the technical field of grouting materials. The anti-flowing-water double-liquid synchronous grouting material provided by the invention comprises a liquid A and a liquid B in a volume ratio of (4-6): 1, and the liquid A comprises the following components in parts by weight: 18-22 parts of cement, 18-22 parts of fly ash, 35-45 parts of fine sand, 0.3-0.5 part of a water reducing agent and 35-45 parts of water; the liquid B is prepared from 4-7 parts of polyaluminum sulfate, 2-4 parts of aluminum oxide, 2-4 parts of hydroxypropyl methyl cellulose, 1-3 parts of calcium hydroxide, 0.3-0.7 part of triethanolamine, 0.3-0.6 part of fatty alcohol-polyoxyethylene ether, 0.8-1.2 parts of polyacrylamide and 95-105 parts of water, has good water washing resistance and proper setting time, can meet the requirements for rapid setting and hardening, can ensure sufficient construction time, and can be used for construction of the concrete. Good application prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grouting materials, and in particular to an anti-dynamic water double-liquid synchronous grouting material and a preparation method thereof. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Grouting is the use of pressure-feeding equipment to inject cementitious materials into underground cracks and cavities to diffuse, gel and solidify them, so as to achieve the purpose of filling cavities, reinforcing strata or preventing seepage and plugging leaks. Synchronous grouting behind the wall is an important element of modern shield construction. Due to the action of dissolution geology, a large number of pores, cracks, caves and even underground rivers are easily formed in the strata of springs or karst areas. Some of these water-rich areas even have dynamic water environments. When the shield advances to these areas, it will bring great difficulties to the synchronous grouting work.

[0004] Double liquid grouting is a new type of grouting scheme in which two different slurries enter the slurry mixing device through two grouting pressure units and two grouting pipes, and are mixed and then injected into the target formation. At present, many high-performance grouting materials with organic polymers as the main agent have been reported, but there are few studies on double liquid grouting materials for dynamic water conditions. It is difficult for existing double liquid grouting materials to meet many requirements in terms of setting time, strength, etc.; and some existing slurry ingredients contain toxic substances. If used in a water-rich environment, it is bound to have an impact on the environment. Therefore, it is particularly important to develop anti-dynamic water double liquid synchronous grouting materials with less environmental pollution, suitable setting time and high strength to solve the slurry problem of shield synchronous grouting. Summary of the invention

[0005] In view of this, the present invention provides a water-moving resistant two-liquid synchronous grouting material and a preparation method thereof, which solves the problem that the existing two-liquid grouting materials are difficult to meet the requirements of grouting materials under water-rich conditions. The water-moving resistant two-liquid synchronous grouting material provided by the present invention has a suitable setting time, can quickly set and harden in a dynamic water environment, and at the same time has good water scouring resistance and little impact on the environment.

[0006] In the first aspect, the present invention provides an anti-dynamic water double-liquid synchronous grouting material, which includes liquid A and liquid B in a volume ratio of (4-6):1. Calculated by weight, the liquid A includes 18-22 parts of cement, 18-22 parts of fly ash, 35-45 parts of fine sand, 0.3-0.5 parts of water reducer and 35-45 parts of water; the liquid B includes 4-7 parts of polyaluminum sulfate, 2-4 parts of alumina, 2-4 parts of hydroxypropyl methylcellulose, 1-3 parts of calcium hydroxide, 0.3-0.7 parts of triethanolamine, 0.3-0.6 parts of fatty alcohol polyoxyethylene ether, 0.8-1.2 parts of polyacrylamide and 95-105 parts of water.

[0007] Preferably, the volume ratio of liquid A to liquid B is 5:1.

[0008] Preferably, the liquid A comprises 20 parts of cement, 20 parts of fly ash, 20 parts of fine sand, 0.4 parts of water reducing agent and 40 parts of water.

[0009] Preferably, the B liquid includes 5-7 parts of polyaluminium sulfate, 3 parts of aluminium oxide, 3 parts of hydroxypropyl methylcellulose, 1-2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide and 100 parts of water.

[0010] Preferably, the cement is Portland cement.

[0011] Furthermore, the type of the silicate cement is P·I type.

[0012] Preferably, the fly ash is Class F, Grade I low-calcium fly ash, the CaO content of which is less than 10 wt% or the free CaO content is not more than 1 wt%.

[0013] Furthermore, the fineness of the fly ash meets the requirement that the residue on a 45 μm square hole sieve is no more than 12%.

[0014] Preferably, the fineness modulus of the fine sand is 2.2 to 1.6.

[0015] Preferably, the water reducer is an ether polycarboxylic acid water reducer.

[0016] In a second aspect, the present invention provides a method for preparing the above-mentioned anti-dynamic water two-liquid synchronous grouting material, comprising the following steps:

[0017] Weigh cement, fly ash, fine sand, water reducer and water in proportion and mix them evenly to obtain liquid A;

[0018] Weigh polyaluminium sulfate, aluminium oxide, hydroxypropyl methylcellulose, calcium hydroxide, triethanolamine, fatty alcohol polyoxyethylene ether, polyacrylamide and water in proportion, and mix them evenly to obtain solution B;

[0019] Before use, the liquid A and the liquid B are mixed in a volume ratio of (4-6):1 to obtain the product.

[0020] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0021] The anti-dynamic water double-liquid synchronous grouting material provided by the present invention uses traditional cement slurry as A liquid and a polymer solution containing polyacrylamide as B liquid. Polyacrylamide can promote the coagulation of the mixed slurry and greatly improve the water scouring resistance of the grouting material. A proper amount of fatty alcohol polyoxyethylene ether is used as an emulsifier to moderately slow down the coagulation rate and avoid the adverse effect of too fast coagulation rate on construction. Triethanolamine is used to increase the fluidity of the mixed slurry. Hydroxypropyl methylcellulose is used to improve the overall polymerization and improve the dynamic water retention rate. Polyaluminum sulfate, aluminum oxide and calcium hydroxide are used to accelerate the mixing progress of A and B liquids and increase the overall construction workability. The anti-dynamic water two-liquid synchronous grouting material of the present invention not only has good water scouring resistance through the synergistic effect of various components, and the dynamic water retention rate at 0.8 m / s is higher than 65%, but also has a suitable setting time, with an initial setting time of 25 to 50 seconds and a final setting time of 70 to 140 minutes, which can not only meet the requirements of rapid setting and hardening, but also ensure sufficient construction time; in addition, the components used in the present invention have little impact on the environment, and therefore have very good application prospects. DETAILED DESCRIPTION

[0022] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0023] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0024] There is no particular limitation on the purity of all raw materials in the present invention. The present invention preferably uses analytically pure materials or materials of conventional purity used in the field of grouting materials.

[0025] The invention provides an anti-dynamic water double-liquid synchronous grouting material, which comprises liquid A and liquid B in a volume ratio of (4-6):1. Calculated by weight, the liquid A comprises 18-22 parts of cement, 18-22 parts of fly ash, 35-45 parts of fine sand, 0.3-0.5 parts of water reducer and 35-45 parts of water, and the liquid B comprises 4-7 parts of polyaluminium sulfate, 2-4 parts of aluminium oxide, 2-4 parts of hydroxypropyl methylcellulose, 1-3 parts of calcium hydroxide, 0.3-0.7 parts of triethanolamine, 0.3-0.6 parts of fatty alcohol polyoxyethylene ether, 0.8-1.2 parts of polyacrylamide and 95-105 parts of water.

[0026] The above-mentioned anti-dynamic water double-liquid synchronous grouting material of the present invention uses traditional cement slurry as liquid A and a polymer solution containing polyacrylamide as liquid B. Polyacrylamide can promote the coagulation of the mixed slurry and greatly improve the water scouring resistance of the grouting material. The present invention also adds fatty alcohol polyoxyethylene ether, which as an emulsifier can prevent the construction inconvenience caused by the excessive coagulation speed of polyacrylamide. In the present invention, hydroxypropyl methylcellulose is a macromolecule, which can improve the overall polymerization of the material, thereby further improving the anti-dynamic water scouring performance and making the material have a higher dynamic water retention rate. In the present invention, polyaluminum sulfate, aluminum oxide and calcium hydroxide can jointly accelerate the mixing progress of liquid A and liquid B and increase the overall construction and workability; triethanolamine can improve the coagulation performance of the slurry, and increase the fluidity and filling density.

[0027] The anti-dynamic water two-liquid synchronous grouting material of the present invention not only has good water scouring resistance through the synergistic effect of various components, but also has a retention rate higher than 65% even in a dynamic water environment of 0.8 m / s; it also has a suitable setting time, with an initial setting time of 25 to 50 seconds and a final setting time of 70 to 140 minutes, which can not only meet the requirements of rapid setting and hardening, but also ensure sufficient construction time; in addition, the various components used in the present invention have little impact on the environment, so it is a green anti-dynamic water two-liquid synchronous grouting material with significant economic and environmental benefits.

[0028] In the present invention, the volume ratio of the liquid A to the liquid B is preferably 5: 1. The volume ratio of the two will affect the coagulation time of the material after the two slurries are mixed.

[0029] In the present invention, the liquid A includes 20 parts of cement, 20 parts of fly ash, 20 parts of fine sand, 0.4 parts of water reducer and 40 parts of water; the liquid B includes 5-7 parts of polyaluminium sulfate, 3 parts of alumina, 3 parts of hydroxypropyl methylcellulose, 1-2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide and 100 parts of water.

[0030] The present invention has no particular limitation on the cement, and any type and brand of cement known to those skilled in the art may be used. Those skilled in the art may select and adjust the cement according to actual application conditions, product requirements and quality requirements. The cement of the present invention is preferably silicate cement, and its model is preferably P·I type.

[0031] In the present invention, the fly ash is Class F, Class I low-calcium fly ash, whose CaO content is less than 10wt% or free CaO content is not more than 1wt%. High-calcium fly ash contains a large amount of free calcium oxide, which can easily cause poor volume stability and other consequences if used improperly. Low-calcium fly ash can ensure the stability and uniformity of the slurry. Furthermore, the fineness of the fly ash meets the requirement that the sieve residue of a 45μm square hole sieve is not more than 12%.

[0032] The present invention does not impose any special restrictions on the type of fine sand, and fine sand commonly used in the art can be used. The fineness modulus of the fine sand of the present invention is preferably 2.2 to 1.6.

[0033] In the present invention, the water reducer is preferably an ether polycarboxylic acid water reducer, which can improve the fluidity of liquid A and effectively reduce the required amount of cement.

[0034] The present invention also provides a method for preparing the above-mentioned anti-dynamic water double-liquid synchronous grouting material, comprising the following steps:

[0035] Weigh cement, fly ash, fine sand, water reducer and water in proportion and mix them evenly to obtain liquid A;

[0036] Weigh polyaluminium sulfate, aluminium oxide, hydroxypropyl methylcellulose, calcium hydroxide, triethanolamine, fatty alcohol polyoxyethylene ether, polyacrylamide and water in proportion, and mix them evenly to obtain solution B;

[0037] Before use, the liquid A and the liquid B are mixed in a volume ratio of (4-6):1 to obtain the product.

[0038] The present invention does not impose any special restrictions on the step of mixing uniformly to obtain liquid A, and a mixing method well known in the art can be used. In the present invention, preferably, cement, fly ash and fine sand are first dry-mixed and uniformly mixed, and then the aqueous solution of the water reducing agent is added and stirred uniformly. The present invention does not impose any special restrictions on the speed and time of stirring in this step, as long as the materials are stirred uniformly.

[0039] The present invention does not impose any special restrictions on the step of mixing uniformly to obtain liquid B, and a mixing method well known in the art can be used. The present invention preferably comprises dry-mixing polyaluminum sulfate, aluminum oxide, and calcium hydroxide, and then adding an aqueous solution containing fatty alcohol polyoxyethylene ether, polyacrylamide, and hydroxypropyl methylcellulose, and stirring uniformly to obtain the liquid B. The present invention does not impose any special restrictions on the speed and time of stirring in this step, and only needs to satisfy the requirement of stirring the materials uniformly.

[0040] The present invention does not impose any special restrictions on the step of mixing liquid A and liquid B, and the mixing step of the double-liquid grouting material commonly used in the art can be used. The present invention preferably allows liquid A and liquid B to enter the slurry mixing device through two grouting pressure units and two grouting pipes respectively, and then inject them into the target formation after mixing. The grouting material of the present invention needs to be grouted immediately after mixing to avoid clogging of the grouting pipe due to slurry coagulation.

[0041] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0042] In the following examples, the silicate cement is of P·I type, the fly ash is of Class F I low-calcium fly ash, the fineness modulus of the fine sand is 2.2 to 1.6, and the water reducer is an ether polycarboxylic acid water reducer.

[0043] Example 1

[0044] The present embodiment provides an anti-dynamic water two-liquid synchronous grouting material, which is composed of liquid A and liquid B. By weight, liquid A: 20 parts of silicate cement, 20 parts of fly ash, 40 parts of fine sand, 0.4 parts of water reducer, and 40 parts of water; liquid B: 5 parts of polyaluminum sulfate, 3 parts of alumina, 3 parts of hydroxypropyl methylcellulose, 2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide, and 100 parts of water.

[0045] Weigh cement, fly ash, fine sand, water reducer and water in proportion, first dry-mix the cement, fly ash and fine sand, then add the water solution of the water reducer and stir evenly to obtain Liquid A.

[0046] Weigh polyaluminum sulfate, aluminum oxide, hydroxypropyl methylcellulose, calcium hydroxide, triethanolamine, fatty alcohol polyoxyethylene ether, polyacrylamide and water in proportion. First, dry-mix the polyaluminum sulfate, aluminum oxide and calcium hydroxide, and then add the aqueous solution containing fatty alcohol polyoxyethylene ether, polyacrylamide and hydroxypropyl methylcellulose. Stir well to obtain liquid B.

[0047] Mix solution A and solution B in a volume ratio of 5:1.

[0048] Example 2

[0049] The difference between this embodiment and embodiment 1 is that the composition of liquid B is different. Liquid B in this embodiment is: 7 parts of polyaluminum sulfate, 3 parts of aluminum oxide, 3 parts of hydroxypropyl methylcellulose, 2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide, and 100 parts of water.

[0050] Example 3

[0051] The difference between this embodiment and embodiment 1 is that the composition of liquid B is different. Liquid B in this embodiment is: 5 parts of polyaluminum sulfate, 3 parts of aluminum oxide, 3 parts of hydroxypropyl methylcellulose, 1 part of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide, and 100 parts of water.

[0052] Comparative Example 1

[0053] Compared with Example 1, the difference between this comparative example and Example 1 is that the composition of liquid B is different, and this comparative example does not contain polyacrylamide and fatty alcohol polyoxyethylene ether. Liquid B of this comparative example is: 5 parts of polyaluminum sulfate, 3 parts of aluminum oxide, 3 parts of hydroxypropyl methylcellulose, 2 parts of calcium hydroxide, 0.5 parts of triethanolamine, and 100 parts of water.

[0054] Comparative Example 2

[0055] Compared with Example 1, the difference between this comparative example and Example 1 is that the composition of liquid B is different, and this comparative example does not contain fatty alcohol polyoxyethylene ether. Liquid B of this comparative example is: 5 parts of polyaluminum sulfate, 3 parts of aluminum oxide, 3 parts of hydroxypropyl methylcellulose, 2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 1 part of polyacrylamide, and 100 parts of water.

[0056] Comparative Example 3

[0057] Compared with Example 1, the difference between this comparative example and Example 1 is that the composition of liquid B is different, and this comparative example does not contain hydroxypropyl methylcellulose. Liquid B of this comparative example is: 5 parts of polyaluminum sulfate, 3 parts of aluminum oxide, 2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide, and 100 parts of water.

[0058] The setting time and the dynamic water retention rate at different flow rates (0.4 m / s and 0.8 m / s) were measured for Examples 1 to 3 and Comparative Examples 1 to 3. The results are shown in Table 1.

[0059] Table 1 Setting time and dynamic water retention rate of double liquid grouting materials of Examples 1 to 3 and Comparative Examples 1 to 3

[0060]

[0061] The proportions of Example 1, Example 2 and Example 3 have suitable coagulation time and high dynamic water retention rate. By comparing Example 1 with Comparative Example 1 and Comparative Example 2, it can be seen that polyacrylamide has a significant effect on coagulation time and dynamic water retention rate; while fatty alcohol polyoxyethylene ether will affect the coagulation time. When fatty alcohol polyoxyethylene ether suspending agent is not added, coagulation will be premature, which is not conducive to on-site construction. From the comparison of Example 1 and Comparative Example 3, it can be seen that if hydroxypropyl methylcellulose is not added, the anti-dynamic water scouring ability of the slurry is significantly reduced.

[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A water-resistant dual-liquid synchronous grouting material, characterized in that: The invention comprises liquid A and liquid B in a volume ratio of (4-6):

1. In parts by weight, the liquid A comprises 18-22 parts of cement, 18-22 parts of fly ash, 35-45 parts of fine sand, 0.3-0.5 parts of water reducing agent and 35-45 parts of water; the liquid B comprises 4-7 parts of polyaluminium sulfate, 2-4 parts of aluminium oxide, 2-4 parts of hydroxypropyl methylcellulose, 1-3 parts of calcium hydroxide, 0.3-0.7 parts of triethanolamine, 0.3-0.6 parts of fatty alcohol polyoxyethylene ether, 0.8-1.2 parts of polyacrylamide and 95-105 parts of water.

2. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The volume ratio of liquid A to liquid B is 5:

1.

3. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The liquid A includes 20 parts of cement, 20 parts of fly ash, 20 parts of fine sand, 0.4 parts of water reducing agent and 40 parts of water.

4. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The B liquid includes 5-7 parts of polyaluminium sulfate, 3 parts of aluminium oxide, 3 parts of hydroxypropyl methylcellulose, 1-2 parts of calcium hydroxide, 0.5 parts of triethanolamine, 0.5 parts of fatty alcohol polyoxyethylene ether, 1 part of polyacrylamide and 100 parts of water.

5. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The cement is silicate cement.

6. The anti-dynamic water double-liquid synchronous grouting material according to claim 5, characterized in that: The type of the silicate cement is P·I type.

7. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The fly ash is Class F, Grade I low-calcium fly ash, and its CaO content is less than 10wt% or its free CaO content is not more than 1wt%.

8. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The fineness of the fly ash meets the requirement that the residue on a 45 μm square sieve is no more than 12%.

9. The anti-dynamic water double-liquid synchronous grouting material according to claim 1, characterized in that: The fineness modulus of the fine sand is 2.2-1.6; the water reducer is an ether polycarboxylic acid water reducer.

10. The method for preparing the anti-dynamic water double-liquid synchronous grouting material according to any one of claims 1 to 9, characterized in that: The steps include: Weigh cement, fly ash, fine sand, water reducer and water in proportion and mix them evenly to obtain liquid A; Weigh polyaluminium sulfate, aluminium oxide, hydroxypropyl methylcellulose, calcium hydroxide, triethanolamine, fatty alcohol polyoxyethylene ether, polyacrylamide and water in proportion, and mix them evenly to obtain solution B; Before use, the liquid A and the liquid B are mixed in a volume ratio of (4-6):1 to obtain the product.

Citation Information

Patent Citations

  • High-waterproofness synchronous grouting slurry for submarine shield tunnels

    CN107827422A

  • Peaceability regulator for machine-made sand concrete

    CN114315219A

  • Chloride ion permeation resistant fluoride-free alkali-free liquid accelerator and preparation method thereof

    CN115057650A

  • Dispersion-resistant and high-impermeability grouting material under flowing water condition as well as preparation method and application thereof

    CN115504747A

  • Shield synchronous double-liquid grouting material and preparation method thereof

    CN116768574A

Cited By

  • Dispersion-resistant solid waste grouting filling material as well as preparation method and application thereof

    CN121225963A

  • Self-repairing synchronous grouting material and preparation method thereof

    CN121342431A

  • Underwater anti-dispersion quick-setting polymer two-component grouting material

    CN122380760A

  • Underwater anti-dispersion quick-setting polymer two-component grouting material

    CN122380760B

  • An anti-water-washing grouting material for slurry shield spoil disposal and a preparation method thereof

    CN122771683A