Preform, resin container and manufacturing method thereof
The preform with a two-layer structure and optimized molding process addresses the haze issue in plastic bottles, enabling transparent containers with high recycled content and improved production efficiency.
Patent Information
- Application Number
- JP2021075978
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-12
- Filing Date
- 2023-06-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-06-12
AI Technical Summary
Conventional two-layer molding methods for plastic bottles result in increased haze, making it difficult to achieve sufficient transparency, especially when a high proportion of recycled materials is used, which hampers commercialization.
A preform with a two-layer structure comprising an inner layer of virgin material and an outer layer of recycled material, where the weight ratio of recycled material is 50% or more and the outer layer thickness is 1.5 times that of the inner layer, combined with a specific injection molding and cooling process to maintain transparency.
The method enables the production of transparent resin containers with a high recycling rate, achieving transparency comparable to those made from 30% recycled materials, while improving production efficiency and reducing whitening at the material interface.
Smart Images

Figure 0007586760000001 
Figure 0007586760000002 
Figure 0007586760000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a preform, a resin container, and a method for producing the same. [Background technology]
[0002] Patent Document 1 discloses a two-layer plastic bottle in which the inner layer is made of new plastic and the outer layer is made of recycled plastic. Patent Document 2 discloses a method for manufacturing a laminated resin molded product, which includes an outer layer molding step of molding a cylindrical outer layer material from recycled resin, and an inner layer molding step of laminating an inner layer material made of a cylindrical virgin resin that is thinner than the outer layer material on the inner side of the outer layer material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2002-103429 [Patent Document 2] Japanese Patent Publication No. 2002-104362 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, marine pollution caused by plastic waste has become a major issue, and efforts towards the 3Rs of plastics (reuse, reduce, recycle) have been gaining momentum internationally. A method has been developed for food / beverage / pharmaceutical bottles (food containers) in which a preform that has been injection molded with a two-layer structure, inner and outer, is blow molded, with virgin material used for the part that comes into contact with the contents (inner layer) and recycled material used for the part that does not come into contact with the contents (outer layer). However, with the conventional two-layer molding method, the bottles are prone to becoming hazy (turbid), making it difficult to manufacture bottles with sufficient transparency, and commercialization (practical use) has not progressed.
[0005] The present invention aims to provide a preform capable of forming a two-layer resin container having high transparency even when a large proportion of recycled material is used, a two-layer resin container having high transparency even when a large proportion of recycled material is used, and a method for manufacturing the same. [Means for solving the problem]
[0006] One aspect of the present invention that can solve the above problem is A preform having an opening, a body, and a bottom, the body and the bottom having a two-layer structure consisting of an inner layer made of a virgin material and an outer layer made of a recycled material, The weight ratio of the recycled material to the total weight of the preform is 50% by weight or more; a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more; The haze of the body of the container molded from the preform is 1.8% or less. It is a preform.
[0007] Another aspect of the present invention that can solve the above problem is A method for producing a preform comprising: an opening, a body portion, and a bottom portion, the body portion and the bottom portion having a two-layer structure composed of an inner layer made of a virgin material and an outer layer made of a recycled material, a first injection molding step of injecting the virgin material or the recycled material into a first mold to injection mold an inner layer material or an outer layer material; a second injection molding step of placing the inner layer material or the outer layer material molded in the first injection molding step in a second mold, and injecting the recycled material onto the outside of the inner layer material to injection mold an outer layer material, or injecting the virgin material onto the inside of the outer layer material to injection mold an inner layer material, This is a method for manufacturing a preform, in which the inner layer material and the outer layer material are molded so that the weight ratio of the recycled material to the total weight of the preform is 50 weight % or more, and the ratio of the thickness of the outer layer to the thickness of the inner layer in the body portion is 1.5 or more.
[0008] Another aspect of the present invention that can solve the above problem is A resin container having an opening, a body, and a bottom, the body and the bottom having a two-layer structure consisting of an inner layer made of a virgin material and an outer layer made of a recycled material, The weight ratio of the recycled material to the total weight of the resin container is 50% by weight or more, a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more; The haze of the body is 1.8% or less. The container is made of resin.
[0009] Another aspect of the present invention that can solve the above problem is an injection molding step of injection molding a preform having an opening, a body, and a bottom, the body and the bottom having a two-layer structure composed of an inner layer made of a virgin material and an outer layer made of a recycled material; A temperature control step of controlling the temperature of the preform; a blow molding step of blow molding the preform to form a resin container; A method for producing a resin container, comprising: The injection molding process includes: a first injection molding step of injecting the virgin material or the recycled material into a first mold to injection mold an inner layer material or an outer layer material; a second injection molding step of placing the inner layer material or the outer layer material molded in the first injection molding step in a second mold, and injecting the recycled material onto the outside of the inner layer material to injection mold an outer layer material, or injecting the virgin material onto the inside of the outer layer material to injection mold an inner layer material, This is a method for manufacturing a resin container, in which, in the injection molding process, the inner layer material and the outer layer material are molded so that the weight ratio of the recycled material to the total weight of the preform is 50 weight % or more, and the ratio of the thickness of the outer layer to the thickness of the inner layer in the body portion is 1.5 or more. Effect of the Invention
[0010] According to the present invention, it is possible to provide a preform capable of forming a two-layer resin container having high transparency even when a large proportion of recycled material is used, a two-layer resin container having high transparency even when a large proportion of recycled material is used, and a method for manufacturing the same. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a cross-sectional view showing a preform according to an embodiment. [Diagram 2] FIG. 1 is a cross-sectional view showing a resin container according to an embodiment. [Diagram 3] 4 is a flowchart showing a manufacturing process of a preform according to an embodiment. [Figure 4] FIG. 2 is a cross-sectional view showing an injection molding process for a preform according to an embodiment. [Diagram 5] FIG. 2 is a cross-sectional view showing one mode of cooling of a preform according to an embodiment. [Figure 6] 10 is a cross-sectional view showing another aspect of cooling the preform according to the embodiment. FIG. [Figure 7] 4 is a flowchart showing a manufacturing process of a resin container according to an embodiment. [Figure 8] 1 is a schematic diagram illustrating a resin container manufacturing apparatus according to an embodiment. [Figure 9] 10 is a flowchart showing a process for manufacturing a resin container according to a modified example of the embodiment. [Figure 10] 13 is a schematic diagram showing a resin container manufacturing device according to a modified example of the embodiment. FIG. [Figure 11] FIG. 11 is a cross-sectional view showing an aspect of injection molding of a preform according to a modified example of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that, for the sake of convenience of explanation, the dimensions of each component shown in the drawings may differ from the actual dimensions of each component.
[0013] First, a preform 10 according to an embodiment will be described with reference to FIG. 1. FIG. 1 is a cross-sectional view of the preform 10. The preform 10 is a cylindrical resin molded product having an opening 12, a neck 14 connected to the opening 12, a body 16 connected to the neck 14, and a bottom 18 connected to the body 16. The body 16 and the bottom 18 have a two-layer structure consisting of an inner layer 22 and an outer layer 24. The inner layer 22 is made of virgin material, which is an unused resin material. The outer layer 24 is made of recycled material prepared by recycling used resin material. The virgin material and the recycled material are made of a thermoplastic resin (crystalline plastic) having transparency in an amorphous state, for example, polyethylene terephthalate (PET) resin as a base material. The preform 10 is used to mold a resin container 30 described later.
[0014] The weight ratio of the recycled material to the total weight of the preform 10 is 50% by weight or more. From the viewpoint of the recycling rate of the resin material, the weight ratio is preferably 60% by weight or more, and from the viewpoint of the transparency of the molded container, the weight ratio is preferably 70% by weight or less. The ratio of the thickness th2 of the outer layer 24 to the thickness th1 of the inner layer 22 in the body portion 16 is 1.5 or more. From the viewpoint of the transparency of the molded container, the ratio is preferably 3.0 or less.
[0015] Gate marks 22a, 24a formed by injection molding are present in the inner layer 22 and the outer layer 24 at the bottom 18 of the preform 10. The height he1 of the gate mark 22a of the inner layer 22 is smaller than the thickness th3 of the outer layer 24 at the bottom 18.
[0016] Next, a container 30 according to an embodiment will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view of the container 30. The container 30 is a bottle-shaped resin container obtained by blow molding the preform 10. The container 30 has a neck portion 14 connected to the opening 12, a body portion 36 connected to the neck portion 14, and a bottom portion 38 connected to the body portion 36. As with the preform 10, the body portion 36 and the bottom portion 38 have a two-layer structure consisting of an inner layer 42 made of virgin material and an outer layer 44 made of recycled material.
[0017] The weight ratio of the recycled material to the total weight of the container 30 and the ratio of the thickness th12 of the outer layer 44 to the thickness th11 of the inner layer 42 in the body portion 36 are similar to the weight ratio of the recycled material to the total weight of the preform 10 and the ratio of the thickness th2 of the outer layer 24 to the thickness th1 of the inner layer 22 in the body portion 16, respectively, and therefore will not be explained here.
[0018] The haze of the body 36 of the container 30 is 1.8% or less, more preferably 1.4% or less, and even more preferably 1.0% or less. Although not particularly limited, the lower limit of the haze may be 0.1%. The haze here refers to the average value of measurements taken at 10 selected locations on the body 36. The haze is measured using a haze meter (cloudiness measuring device) in accordance with "Determination of haze for plastic transparent materials (JIS K 7136:2000)". The container 30 is a two-layered resin container that has high transparency even when a large proportion of recycled materials is used, and can achieve a high recycling rate of plastic materials while being highly practical.
[0019] Next, a method for producing the preform 10 will be described with reference to Fig. 3 to Fig. 6. Fig. 3 is a diagram showing the steps for producing the preform 10. Fig. 4 is a diagram showing the injection molding of the preform 10. Figs. 5 and 6 are diagrams showing the cooling of the preform 10 after injection molding.
[0020] As shown in FIG. 3, the manufacturing method of the preform 10 of this embodiment includes an inner layer material molding step S1 and an outer layer material molding step S2, which are two-stage injection molding steps. Here, each step will be described with reference to FIG. 4. In the inner layer material molding step S1, a virgin material is injected through a first gate 58 into a cavity formed by a first mold 50 composed of a first cavity mold 52, a first injection core mold 54, and a neck mold 56. The first mold 50 includes a first hot runner mold 59. The first hot runner mold 59 has a valve pin 59a that can move toward the first gate 58 in a flow path through which a resin material in a molten state (for example, a state melted at about 255°C for PET resin) flows. That is, the first gate 58 in the first mold 50 is configured as a valve gate. When the filling of the virgin material into the cavity is completed, the first mold 50 is kept clamped for a predetermined time and then opened to mold the inner layer material 60. The first cavity mold 52 and the first injection core mold 54 are provided with a circuit (medium flow hole or medium flow groove) through which a cooling medium (fluid) for cooling the inner layer material 60 flows, and the temperature of the cooling medium is appropriately set, for example, within the range of approximately 5°C to approximately 20°C.
[0021] The molded inner layer material 60 is raised together with the first injection core mold 54 and the neck mold 56 and separated from the first cavity mold 52. The first injection core mold 54 is further raised and separated from the inner layer material 60. The inner layer material 60 is then rotated together with the neck mold 56 by a rotating means (not shown) while held by the neck mold 56, and placed above the second cavity mold 72. In the outer layer material molding step S2, the neck mold 56 that holds the inner layer material 60 is clamped to the second injection core mold 55 and the second cavity mold 72, so that the inner layer material 60 is accommodated in the second mold 70 that is composed of the second cavity mold 72, the second injection core mold 55, and the neck mold 56. The molten recycled material is then injected through the second gate 78 into the cavity formed by the second mold 70, outside the inner layer material 60. The second mold 70 includes a second hot runner mold 79. The second hot runner mold 79 may have a valve pin that can move toward the second gate 78 in the flow path through which the resin material flows. That is, the second gate 78 in the second mold 70 may be configured as a valve gate. When the filling of the cavity with the recycled material is completed, the second mold 70 is clamped for a predetermined time, and then opened to mold the preform 10 composed of the outer layer material 80 and the inner layer material 60. In this embodiment, the inner layer material molding step S1 of the next preform 10 is performed during the outer layer material molding step S2 of the previous preform 10. In addition, the second cavity mold 72 and the second injection core mold 55 are also provided with a circuit through which a cooling medium flows to cool the outer layer material 80 and the inner layer material 60, and the cooling medium is appropriately set within a range of, for example, about 5°C to about 20°C. The temperature of the cooling medium, i.e., the cooling strength, may be different between the first mold 50 and the second mold 70 (for example, the temperature of the cooling medium of the second mold 70 is set lower than that of the first mold 50). Furthermore, in the second mold 70, the cooling strength may be different between the second cavity mold 72 and the second injection core mold 55 (for example, the temperature of the cooling medium of the second cavity mold 72 is set lower than that of the second injection core mold 55).
[0022] In the inner layer material molding step S1 and the outer layer material molding step S2, the inner layer material 60 and the outer layer material 80 are molded using a first mold 50 and a second mold 70 designed so that the weight ratio of the recycled material (outer layer material 80) to the total weight of the preform 10 is 50% by weight or more, and the ratio of the thickness of the outer layer 24 (outer layer material 80) to the thickness of the inner layer 22 (inner layer material 60) in the body portion 16 of the preform is 1.5 or more. Here, the length le1 of the first gate 58 in the first mold 50 is smaller than the thickness th3 of the outer layer 24 (outer layer material 80) in the bottom portion 18 of the preform 10.
[0023] In the manufacturing method of the preform 10 of this embodiment, if a cooling step S3 for cooling the preform is included after the outer layer material molding step S2, the cooling time of the injection molding step can be shortened, which is preferable from the viewpoint of production efficiency (FIG. 3). Note that the cooling step S3 here does not include a step of cooling the preform 10 in the second mold 70 by maintaining the clamping of the second mold 70. Here, the aspect of the cooling step S3 will be described with reference to FIGS. 5 and 6.
[0024] FIG. 5 is a diagram showing one embodiment of the cooling step S3. In the cooling step S3 shown in FIG. 5, the preform 10 released from the second mold 70 is accommodated in the third cavity mold 100, and the air introduction member 110 is abutted against the preform 10 in an airtight manner. The air introduction member 110 is composed of a rod member 112 that is hollow and has an air circulation hole therein, and a fitting core (blow core member) 114. The rod member 112 is accommodated inside the fitting core 114 so as to be movable up and down. The tip of the rod member 112 is provided with an inward circulation port 116 that can blow or suck air. The temperature of the air is appropriately set within a range of, for example, about 0°C to about 20°C (room temperature) depending on the thickness of the preform 10 and the container 30. The fitting core 114 is configured so that when the air introduction member 110 is inserted into the preform 10 (airtightly abutted against the preform 10), it fits (comes in close contact with) the neck portion 14. This can prevent air inside the preform 10 from leaking from the neck portion 14 to the outside of the fitting core 114. The gap between the rod member 112 and the fitting core 114 is an air flow path for supplying and discharging air to and from the preform 10. The gap formed between the tip of the fitting core 114 and the rod member 112 constitutes an outer flow port 118 that can eject or suck air. The inner flow port 116 and the outer flow port 118 can be an air supply port and an exhaust port, respectively. For example, the preform 10 is cooled by sending air into the inside of the preform 10 from the air supply port of the air introduction member 110 and discharging the air to the outside of the preform 10 from the exhaust port of the air introduction member 110. The third cavity mold 100 is also provided with a circuit for a cooling medium to cool the outer layer material 80, and the fluid medium is appropriately set within a range of, for example, about 5°C to about 80°C, more preferably 10°C to 70°C, and even more preferably 20°C to 65°C.
[0025] Fig. 6 is a diagram showing another aspect of the cooling step S3. In the cooling step S3 shown in Fig. 6, the preform 10 released from the second mold 70 is accommodated in the fourth cavity mold 120, and the preform 10 is sandwiched between the fourth cavity mold 120 and a core mold 130 configured to be movable up and down, thereby cooling the preform 10. Note that the fourth cavity mold 120 and the core mold 130 are also provided with a circuit through which a cooling medium flows, the temperature of which is set within a range of, for example, about 5°C to about 80°C, more preferably 10°C to 70°C, and even more preferably 20°C to 65°C.
[0026] Next, a method for manufacturing the container 30 will be described with reference to Fig. 4 to Fig. 7. Fig. 7 is a diagram showing the steps of manufacturing the container 30. As shown in Fig. 7, the method for manufacturing the container 30 of this embodiment includes an injection molding step S11 of injection molding the preform 10, a temperature adjustment step S12 of adjusting the temperature of the preform 10, and a blow molding step S13 of blow molding the preform 10 to form the container 30.
[0027] First, the injection molding step S11 will be described. The injection molding step S11 includes the inner layer material molding step S1 and the outer layer material molding step S2 described in the manufacturing method of the preform 10. In the injection molding step S11, as described in the inner layer material molding step S1 and the outer layer material molding step S2 of the preform 10, the inner layer material 60 and the outer layer material 80 are molded so that the weight ratio of the recycled material (outer layer material 80) to the total weight of the preform 10 is 50% by weight or more, and the ratio of the thickness of the outer layer 24 (outer layer material 80) to the thickness of the inner layer 22 (inner layer material 60) in the body part 16 of the preform is 1.5 or more. The first mold 50 used in the inner layer material molding step S1, the second mold 70 used in the outer layer material molding step S2, and other aspects adopted in the injection molding step S11 are the same as those described in the manufacturing method of the preform 10 (FIG. 4), so the description will be omitted.
[0028] Next, the temperature control step S12 will be described. The temperature control step S12 is a step of adjusting the temperature of the injection-molded preform 10 to a temperature range suitable for blow molding. In the temperature control step S12, the temperature of the preform 10 is controlled using a temperature control pod, a temperature control core, an infrared heater, or the like. In the temperature control step S12, the temperature of the preform 10 may be controlled while cooling the preform by adopting the aspect (FIGS. 5 and 6) described in the cooling step S3 of the manufacturing method of the preform 10. When the temperature control step S12 is the aspect described in the cooling step S3 of the manufacturing method of the preform 10, the production efficiency of the container 30 is improved, which is preferable. In particular, when the preform 10 and the container 30 are continuously manufactured in a hot parison-type resin container manufacturing device shown in FIG. 8 described later, the production efficiency of the container 30 is improved, which is preferable. In addition, when the injection molding and blow molding of a two-layer preform are continuously performed by the hot parison-type blow molding method, the boundary portion between the inner layer 22 and the outer layer 24 is insufficiently cooled (slowly cooled), and the haze is likely to become large. However, if the aspect explained in the cooling step S3 (FIGS. 5 and 6) is adopted in the temperature adjustment step S12, it is possible to improve the cooling efficiency of the boundary portion while maintaining the amount of heat required for blow molding, and to reduce haze in the container 30. When the cooling step S3 is adopted in the temperature adjustment step S12, the temperature of the cooling medium flowing through the third cavity mold 100, the fourth cavity mold 120, and the core mold 130 is appropriately set within a wider range, for example, from about 10°C to about 65°C.
[0029] Next, the blow molding step S13 will be described. In the blow molding step S13, the preform 10 is placed in a blow cavity mold. Next, the preform 10 is optionally stretched by a stretch rod while blow air is introduced from a blow core mold to inflate the preform 10 to the shape of the container 30, thereby producing the container 30. After that, the container 30 is released from the mold. Through the above procedure, the container is produced.
[0030] Here, referring to FIG. 8, a manufacturing apparatus 150 for the container 30 of this embodiment will be described. FIG. 8 is a functional block diagram of the manufacturing apparatus 150 for the container 30. The manufacturing apparatus 150 includes an injection molding section 152 for manufacturing the preform 10, a temperature adjustment section 154 for adjusting the temperature of the manufactured preform 10, a blow molding section (one example of a blow device) 156 for blowing the preform 10 to manufacture the container 30, and a removal section 158 for removing the manufactured container 30. The preform 10 and the container 30 are transported in the manufacturing apparatus 150 by a transport means (not shown) in the order of the injection molding section 152, the temperature adjustment section 154, the blow molding section 156, and the removal section 158. As the configurations of the injection molding section 152, the temperature adjustment section 154, and the blow molding section 156, the configurations of ... The manufacturing apparatus 150 is a hot parison type resin container manufacturing apparatus, and continuously carries out the manufacture of the preforms 10 and the containers 30.
[0031] Meanwhile, as 3R plastic initiatives are gaining momentum internationally, various recycling efforts are being made in the area of PET containers, with the ultimate goal of "bottle to bottle." For example, PET bottles for detergents and toners (non-food containers) are often manufactured using flakes obtained by crushing used PET bottles, or blends of recycled pellets and virgin materials. On the other hand, PET bottles for food, beverages and medicines (food containers) are manufactured using virgin materials, with almost no recycled materials being used. This is because these types of PET bottles require high safety in terms of hygiene. Therefore, a method has been developed in which a preform that has been injection molded with an inner and outer two-layer structure is blow molded, and the part that comes into contact with the contents (inner layer) is made of virgin materials, and the part that does not come into contact with the contents (outer layer) is made of recycled materials.
[0032] However, the conventional two-layer molding method tends to result in a large amount of bottle haze (turbidity), making it difficult to manufacture bottles with sufficient transparency, and commercialization (practical use) has not progressed. Even when using blended materials, the usage ratio (weight ratio) of recycled pellet material is limited to about 30% by weight at most, taking into account the transparency of the bottle, and further improvement was necessary.
[0033] The preform 10 having the above configuration can form a two-layered resin container 30 that has high transparency even if it uses a large proportion of recycled material. Specifically, it can form a resin container that has the same transparency as a container formed from a two-layered preform made of a blend material containing 30% by weight of recycled pellet material.
[0034] In addition, the height he1 of the gate mark 22a of the preform 10 is smaller than the thickness th3 of the outer layer 24 at the bottom 18, so that the virgin material can be prevented from melting and mixing with the recycled material when the recycled material is injected. This makes it possible to provide a preform 10 that can prevent whitening at the bottom 18 of the preform 10 and can form a two-layered resin container 30 with high transparency.
[0035] In addition, recycled materials are more likely to crystallize than virgin materials, and are therefore more likely to whiten. In order to suppress the whitening of recycled materials, an inner layer material 60 made of virgin material was first molded, and then an outer layer material 80 made of recycled material was molded. When the recycled material was injected, the virgin material was reheated to a temperature range where it is likely to crystallize (for example, about 150°C for PET resin) and slowly cooled, and it was found that whitening (crystallization) was likely to occur at the boundary surface between the virgin material and the recycled material. Therefore, by lowering the weight ratio of the virgin material to the total weight of the preform 10 and reducing the thickness of the inner layer 22 relative to the outer layer 24, the cooling efficiency of the inner layer 22 by the first mold 50 and the second mold 70 (second injection core mold 55) was increased, and whitening at the boundary surface between the virgin material and the recycled material was successfully suppressed. That is, according to the above-mentioned method for manufacturing preform 10, an inner layer material 60 made of virgin material is molded, and then an outer layer material 80 made of recycled material is molded, and the inner layer material 60 and the outer layer material 80 are molded so that the weight ratio of the recycled material to the total weight of preform 10 is 50 weight % or more, and the ratio of the thickness th2 of the outer layer 24 to the thickness th1 of the inner layer 22 in the body 16 is 1.5 or more, thereby providing a preform 10 that can form a two-layered resin container 30 that has high transparency even when the proportion of recycled material used is large.
[0036] In addition, in the above-mentioned manufacturing method of the preform 10, the length le1 of the first gate 58 through which the virgin material is injected is smaller than the thickness th3 of the outer layer 24 at the bottom 18, so that the height he1 of the gate mark 22a formed in the inner layer material 60 is small, and it is possible to prevent the virgin material from melting and mixing with the recycled material when the recycled material is injected. This makes it possible to prevent whitening due to crystallization or the like at the bottom 18 of the preform 10, and it is possible to provide a preform 10 that can form a two-layered resin container 30 with high transparency.
[0037] In addition, in the above-mentioned method for manufacturing the preform 10, by providing a cooling step S3 for cooling the preform 10 after the outer layer material molding step S2, it is possible to shorten the cooling time of the preform 10 during injection molding. This allows molding of the next preform 10 to be started while the preform 10 is being cooled, thereby improving production efficiency.
[0038] Furthermore, by cooling the preform 10 by supplying and exhausting air in the cooling step S3 of the above-mentioned manufacturing method of the preform 10, the cooling of the preform 10 can be accelerated, improving the production efficiency of the preform 10 while providing a preform 10 that can form a two-layered resin container 30 with excellent transparency.
[0039] Furthermore, by sandwiching the preform 10 between the fourth cavity mold 120 and the core mold 130 in the cooling step S3 of the manufacturing method of the preform 10 described above, the cooling of the preform 10 can be accelerated, improving the production efficiency of the preform 10 while providing a preform 10 that can be used to form a two-layered resin container 30 with excellent transparency.
[0040] In addition, according to the above-mentioned manufacturing method of the container 30, the inner layer material 60 of the preform 10 is molded, and then the outer layer material 80 of the preform 10 is molded so that the weight ratio of the recycled material to the total weight of the preform 10 is 50% by weight or more, and the ratio of the thickness th2 of the outer layer 24 to the thickness th1 of the inner layer 22 in the body 16 is 1.5 or more, thereby providing a two-layered container 30 having high transparency even if the ratio of the recycled material is large. In addition, in the conventional hot parison type two-layer molding method, the haze of the container tends to be large, and it is difficult to manufacture a bottle with sufficient transparency, and commercialization (practical use) has not progressed. According to the above-mentioned method, particularly in the hot parison type two-layer molding method, a two-layered container 30 having high transparency can be provided even if the ratio of the recycled material is large.
[0041] Furthermore, by performing the injection molding step S11 and the temperature control step S12 in the manufacturing method of the above-mentioned container 30 in the manner described in the manufacturing method of the preform 10, a resin container having a two-layer structure with better transparency can be formed, and the cycle time for molding the container can be shortened, thereby improving production efficiency.
[0042] In the above embodiment, the outer layer material molding step S2 is performed after the inner layer material molding step S1, but the present invention is not limited to this embodiment. Fig. 9 is a flow chart showing the manufacturing process of a resin container according to a modified example of the above embodiment. As shown in Fig. 9, a resin container may be manufactured by performing the first injection molding step S31, the first temperature adjustment step S32, the second injection molding step S33, the second temperature adjustment step S34, and the blow molding step S35 in this order. When molding a preform, the first injection molding step S31, the first temperature adjustment step S32, the second injection molding step S33, and the second temperature adjustment step S34 may be performed in this order.
[0043] In this modified example, the first injection molding step S31 is a step of molding either the inner layer material or the outer layer material of the preform, and the second injection molding step S33 is a step of molding either the inner layer material or the outer layer material of the preform that is not molded in the first injection molding step S31 to mold the preform. The first temperature adjustment step S32 is a step of adjusting the temperature of the inner layer material or the outer layer material of the preform molded in the first injection molding step S31. The first temperature adjustment step S32 may be a step of cooling the inner layer material or the outer layer material of the preform. In the first temperature control step S32 between the first injection molding step S31 and the second injection molding step S33, the inner layer material or the outer layer material of the preform molded first is post-cooled (particularly, the surface on which the resin material is laminated in the second injection molding step S33 is post-cooled), thereby reducing the haze of the two-layer preform (reduction of haze by suppressing whitening at the boundary surface between the inner layer material and the outer layer material) and shortening the molding cycle. The second temperature control step S34 is a step of adjusting the temperature of the preform molded in the second injection molding step S33. The second temperature control step S34 may be a step of cooling the preform. The blow molding step S35 is a step of blow molding the preform whose temperature has been controlled in the second temperature control step S34 to obtain a resin container.
[0044] FIG. 10 is a schematic diagram showing a resin container manufacturing apparatus 350 according to a modified example of the embodiment. As shown in FIG. 10, the manufacturing apparatus 350 is a six-station manufacturing apparatus including a first injection molding section 352 including a first injection device 362, a first temperature control section 354, a second injection molding section 353 including a second injection device 363, a second temperature control section 355, a blow molding section 356, and a removal section 358. In the manufacturing apparatus 350, the preform and the resin container are transported in the direction of the arrow shown in the figure by a transport device 370 including a rotating disk or the like, and are molded according to the manufacturing process described above. As a specific aspect of each station, those of the above-mentioned embodiment can be appropriately adopted.
[0045] In the above embodiment, a two-step injection molding process is described in which the outer layer material molding process S2 is carried out after the inner layer material molding process S1, but a process in which the outer layer material is molded first and then the inner layer material can be adopted. A modified example of this embodiment will be described below with reference to Fig. 11. Fig. 11 is a cross-sectional view showing the injection molding of a preform 210 according to a modified example of the above embodiment.
[0046] Below, this modified example will be described based on a manufacturing apparatus that molds preform 210 and molds a resin container from preform 210. The manufacturing apparatus according to this modified example is similar to manufacturing apparatus 150 and manufacturing apparatus 350 described in the above-mentioned embodiment and modified examples, except for a different configuration of the injection molding unit. The injection molding unit of the manufacturing apparatus of this modified example includes a first mold 250 that molds outer layer material 280, and a second mold 270 that molds inner layer material 260 inside outer layer material 280 (see FIG. 11).
[0047] The first mold 250 includes a first cavity mold 252, a first injection core mold 254, and a neck mold 256. The first mold 250 is configured to form an outer layer material 280 by pouring recycled material into a cavity formed by clamping these molds. The recycled material is supplied from a first hot runner mold 259 and poured into the cavity through a first gate 258.
[0048] The first hot runner mold 259 has a valve pin 259a that is movable toward the first gate 258 in a flow path through which the recycled material flows. The valve pin 259a is configured to move through the first gate 258 to a position close to the first injection core mold 254 after the recycled material has been filled into the cavity. As a result, a thin film portion 281 that is thinner in the center of the bottom of the outer layer material 280 than in the peripheral portion is formed.
[0049] The second mold 270 includes a second cavity mold 272, a second injection core mold 255, and a neck mold 256. The neck mold 256 is a common neck mold that moves to the position of the second mold 270 while holding the outer layer material 280 molded by the first mold 250. The diameter of the core of the second injection core mold 255 is smaller than the diameter of the core of the first injection core mold 254 by the thickness of the layer of the inner layer material 260. In addition, the size (diameter) of the recess in the top view of the second cavity mold 272 and the size (diameter) of the recess in the top view of the first cavity mold 252 are formed to be the same diameter. The second mold 270 is configured to form the inner layer material 260 inside the outer layer material 280 molded by the first mold 250 by pouring virgin material into the cavity formed by clamping these molds.
[0050] Virgin material is supplied from a second hot runner mold 279 and poured into the cavity via a second gate 278. The virgin material is poured into the cavity as a thin film portion 281 formed on the outer layer material 280 is broken by the flow of the virgin material. An opening 282 is formed in the bottom 218 of the preform 210 (the bottom of the outer layer material 280) as a result of the thin film portion 281 of the outer layer material 280 being broken. The virgin material poured into the cavity fills the cavity via the opening 282.
[0051] In this modification, a two-stage injection molding process is adopted in which an outer layer material molding process for forming an outer layer material 280 is performed by the above-mentioned first mold 250, and then an inner layer material molding process for molding an inner layer material 260 inside the outer layer material 280 by the second mold 270 is performed. In this modification, the preform 210 is molded so that the weight ratio of the recycled material to the total weight of the preform 210 molded by the two-stage injection molding process and the ratio of the thickness of the outer layer to the thickness of the inner layer in the body are similar to those of the above-mentioned embodiment. Also, in this modification, a container is molded so that the haze of the body of the container molded from the preform 210 is similar to those of the above-mentioned embodiment.
[0052] In addition, in this modification, unlike the method of performing the outer layer material molding step S2 after the inner layer material molding step S1 (see FIG. 7), no gate marks are formed on the outer layer material 280 (recycled material) that is first molded in the first injection molding step. Therefore, the possibility of the virgin material and the recycled material melting and mixing in the bottom region of the preform 210 is further reduced, and whitening (crystallization, etc.) of the bottom can be more reliably suppressed. In addition, the injection amount of the inner layer material 260 (virgin material) injected in the second injection molding step is smaller than the injection amount of the outer layer material 280 (recycled material) injected in the first injection molding step, and the degree of reheating of the outer layer material 280 molded first is also reduced. Therefore, the phenomenon of whitening (crystallization) at the boundary surface between the virgin material and the recycled material is less likely to occur. As a result, in this modification, the preform 210 that can form a two-layered resin container with high transparency can be more easily manufactured and provided.
[0053] It is preferable to carry out this modified example by the manufacturing method of FIG. 9 or the manufacturing apparatus 350 of FIG. 10. This is because the thick outer layer material 280 of the preform 210 made of recycled material can be cooled in the first injection molding step S31 (first mold 250) and can be additionally cooled (post-cooled) in the first temperature adjustment step S32 (first temperature adjustment unit 354). This allows the thick outer layer material 280 of the preform 210 to be sufficiently cooled and the temperature to be reduced, so that the temperature rise (reheating) of the outer layer material 280 due to the injection of virgin material in the second injection molding step S33 (second mold 270) can be suppressed. Therefore, the whitening of the preform 210 can be further reduced, and a container with a lower haze value can be manufactured. EXAMPLES
[0054] Examples of the present embodiment will be described below. Note that the technical scope of the present invention is not limited to these examples. The technical scope of the present invention is defined by the scope of the claims or equivalents thereto.
[0055] Using the manufacturing apparatus 150 described in this embodiment, however, by changing the resin material used in the injection molding of the preform, manufacturing tests were carried out for resin containers having the two-layer structure of Examples 1, 2, and 3.
[0056] The container of Example 1 was molded from a preform having an inner layer made of virgin PET material (BK-2180, manufactured by Mitsubishi Chemical Corporation) and an outer layer made of recycled PET material (LCG-1810, manufactured by Pet One, Mexico) with the structure shown in Figure 1. The weight ratio of the virgin material to the total weight was 38%, and the weight ratio of the recycled material to the total weight was 62%. The thickness of the inner layer in the body of the preform was 1.8 mm, and the thickness of the outer layer was 2.98 mm.
[0057] The container of Example 2 was molded from a preform having an inner layer and an outer layer made of a blend of virgin and recycled materials (a mixture of BK-2180 manufactured by Mitsubishi Chemical and LCG-1810 manufactured by Pet One, Mexico), with the proportion of recycled material in the total weight being 30%. The weight ratio of the virgin material to the total weight was 70%. The thickness of the inner layer in the body of the preform was 1.8 mm, and the thickness of the outer layer was 2.98 mm.
[0058] The container of Example 3 was molded from a preform having an inner layer and an outer layer made of recycled material (Pet One, Mexico, LCG-1810) and the structure shown in Figure 1. The thickness of the inner layer in the body of the preform was 1.8 mm, and the thickness of the outer layer was 2.98 mm.
[0059] The haze in the body of the container of Examples 1 to 3 was measured using a haze meter (NDH-300, manufactured by Nippon Denshoku Industries Co., Ltd.). The average values calculated from the values measured by selecting 10 arbitrary points on the body of the container of Examples 1 to 3 were 1.74%, 1.75%, and 2.69%, respectively. In addition, when the thickness of the body is converted to 0.5 mm, the haze values of Examples 1 to 3 are 1.36%, 1.49%, and 2.13%, respectively. It was found that the containers of Examples 1 and 2 had lower haze and better transparency than the container of Example 3, which used only recycled materials. In addition, although the container of Example 1 had a higher ratio of recycled materials than the container of Example 2, it showed the same haze value, and it was found to be a container with excellent transparency while having a high recycling rate.
[0060] The present invention is not limited to the above-described embodiment, and can be freely modified, improved, etc. as appropriate. The material, shape, size, numerical value, form, number, location, etc. of each component in the above-described embodiment are arbitrary and not limited as long as the present invention can be achieved.
[0061] For example, in the above embodiment, the virgin material and the recycled material are described as having PET resin as the base material, but materials having PE resin, PP resin, etc. as the base material may also be used. However, in the embodiment of the present invention, PET resin is preferred.
[0062] Below, aspects extracted from the above-described embodiment and its modifications will be listed. [1] A preform having an opening, a body, and a bottom, the body and the bottom having a two-layer structure consisting of an inner layer made of a virgin material and an outer layer made of a recycled material, The weight ratio of the recycled material to the total weight of the preform is 50% by weight or more; a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more; The haze of the body of the container molded from the preform is 1.8% or less. Preform. [2] The preform according to [1], wherein a height of a gate mark of the inner layer at the bottom is smaller than a thickness of the outer layer at the bottom. [3] A method for producing a preform comprising: an opening, a body portion, and a bottom portion, the body portion and the bottom portion having a two-layer structure composed of an inner layer made of a virgin material and an outer layer made of a recycled material, a first injection molding step of injecting the virgin material or the recycled material into a first mold to injection mold an inner layer material or an outer layer material; a second injection molding step of placing the inner layer material or the outer layer material molded in the first injection molding step in a second mold, and injecting the recycled material onto the outside of the inner layer material to injection mold an outer layer material, or injecting the virgin material onto the inside of the outer layer material to injection mold an inner layer material, A method for manufacturing a preform, comprising molding the inner layer material and the outer layer material so that a weight ratio of the recycled material to a total weight of the preform is 50 weight % or more, and a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more. [4] the first injection molding step is an inner layer material molding step of injecting the virgin material into the first mold to injection mold an inner layer material, The second injection molding step is an outer layer material molding step of placing an inner layer material in the second mold and injecting the recycled material on the outside of the inner layer material to injection mold an outer layer material. A method for producing a preform according to [3]. [5] The method for manufacturing a preform described in [4], wherein the length of a gate in the first mold through which the virgin material is injected is smaller than the thickness of the outer layer at the bottom of the preform. [6] the first injection molding step is an outer layer material molding step of injecting the recycled material into the first mold to injection mold an outer layer material, The second injection molding step is an inner layer material molding step of placing an outer layer material in the second mold and injecting the virgin material into the inner side of the outer layer material to injection mold an inner layer material. A method for producing a preform according to [3]. [7] A cooling step of cooling the preform after the second injection molding step is included. A method for producing a preform according to any one of [3] to [6]. [8] In the cooling step, The preform is placed in a cavity mold; An air introducing member is abutted against the preform in an airtight manner; The preform is cooled by sending air into the inside of the preform from the air blowing port of the air introduction member and discharging the air to the outside of the preform from the exhaust port of the air introduction member. A method for producing a preform according to [7]. [9] In the cooling step, the preform is cooled by sandwiching the preform between a cavity mold and a core mold. A method for producing a preform according to [7].
[10] a first cooling step of cooling the inner layer material or the outer layer material after the first injection molding step; A second cooling step of cooling the preform after the second injection molding step is included. A method for producing a preform according to any one of [3] to [6].
[11] In the first cooling step and the second cooling step, The preform is placed in a cavity mold; An air introducing member is abutted against the preform in an airtight manner; The preform is cooled by sending air into the inside of the preform from the air blowing port of the air introduction member and discharging the air to the outside of the preform from the exhaust port of the air introduction member. A method for producing a preform according to
[10] .
[12] In the first cooling step and the second cooling step, the preform is cooled by sandwiching the preform between a cavity mold and a core mold. A method for producing a preform according to
[10] .
[13] A resin container having an opening, a body, and a bottom, the body and the bottom having a two-layer structure consisting of an inner layer made of a virgin material and an outer layer made of a recycled material, The weight ratio of the recycled material to the total weight of the resin container is 50% by weight or more, a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more; The haze of the body is 1.8% or less. Plastic container.
[14] an injection molding step of injection molding a preform having an opening, a body, and a bottom, the body and the bottom having a two-layer structure composed of an inner layer made of a virgin material and an outer layer made of a recycled material; A temperature control step of controlling the temperature of the preform; a blow molding step of blow molding the preform to form a resin container; A method for producing a resin container, comprising: The injection molding process includes: a first injection molding step of injecting the virgin material or the recycled material into a first mold to injection mold an inner layer material or an outer layer material; a second injection molding step of placing the inner layer material or the outer layer material molded in the first injection molding step in a second mold, and injecting the recycled material onto the outside of the inner layer material to injection mold an outer layer material, or injecting the virgin material onto the inside of the outer layer material to injection mold an inner layer material, A method for manufacturing a resin container, wherein in the injection molding process, the inner layer material and the outer layer material are molded so that the weight ratio of the recycled material to the total weight of the preform is 50 weight % or more, and the ratio of the thickness of the outer layer to the thickness of the inner layer in the body portion is 1.5 or more.
[15] the first injection molding step is an inner layer material molding step of injecting the virgin material into the first mold to injection mold an inner layer material, The second injection molding step is an outer layer material molding step of placing an inner layer material in the second mold and injecting the recycled material on the outside of the inner layer material to injection mold an outer layer material. A method for manufacturing a resin container according to
[14] .
[16] The method for manufacturing a resin container described in
[15] , wherein the length of the gate in the first mold through which the virgin material is injected is smaller than the thickness of the outer layer at the bottom of the preform.
[17] the first injection molding step is an outer layer material molding step of injecting the recycled material into the first mold to injection mold an outer layer material, The second injection molding step is an inner layer material molding step of placing an outer layer material in the second mold and injecting the virgin material into the inner side of the outer layer material to injection mold an inner layer material. A method for manufacturing a resin container according to
[14] .
[18] In the temperature control step, the preform molded in the injection molding step is cooled. A method for manufacturing a resin container according to any one of
[14] to
[17] .
[19] In the temperature control step, The preform is placed in a cavity mold; An air introducing member is abutted against the preform in an airtight manner; The preform is cooled by sending air into the inside of the preform from the air blowing port of the air introduction member and discharging the air to the outside of the preform from the exhaust port of the air introduction member. A method for producing a resin container according to
[18] .
[20] In the temperature control step, the preform is cooled by sandwiching the preform between a cavity mold and a core mold. A method for producing a resin container according to
[18] . [twenty one] the temperature control step includes a first temperature control step and a second temperature control step, the first temperature control step is a step of cooling the inner layer material or the outer layer material after the first injection molding step, The second temperature control step is a step of cooling the preform after the second injection molding step. A method for manufacturing a resin container according to any one of
[14] to
[17] . [twenty two] In the first cooling step and the second cooling step, The preform is placed in a cavity mold; An air introducing member is abutted against the preform in an airtight manner; The preform is cooled by sending air into the inside of the preform from the air blowing port of the air introduction member and discharging the air to the outside of the preform from the exhaust port of the air introduction member. A method for manufacturing a resin container according to
[21] . [twenty three] In the first cooling step and the second cooling step, the preform is cooled by sandwiching the preform between a cavity mold and a core mold. A method for manufacturing a resin container according to
[21] .
[0063] This application is based on a Japanese patent application (Patent Application No. 2019-109558) filed on June 12, 2019, the entirety of which is incorporated by reference. In addition, all references cited herein are incorporated in their entirety. [Explanation of symbols]
[0064] 10,210: preform, 12: opening, 14: neck, 16: body, 18,218: bottom, 22: inner layer, 24: outer layer, 22a, 24a: gate marks, 30: container, 36: body, 38: bottom, 42: inner layer, 44: outer layer, 50,250: first mold, 52,252: first cavity mold, 54,254: first injection core mold, 55,255: second injection core mold, 56,256: neck mold, 58,258: first gate, 59,259: first hot runner mold, 59a,259a: valve pin, 60,260: inner layer material, 70,270: second mold, 72,2 72: second cavity mold, 78, 278: second gate, 79, 279: second hot runner mold, 80, 280: outer layer material, 282: opening, 100: third cavity mold, 110: air introduction member, 120: fourth cavity mold, 130: core mold, 150, 350: manufacturing device, 152: injection molding section, 154: temperature control section, 156, 356: blow molding section, 158, 358: removal section, 352: first injection molding section, 353: second injection molding section, 354: first temperature control section, 355: second temperature control section, 362: first injection device, 363: second injection device, 370: conveying device
Claims
1. A method for producing a preform, comprising: an opening, a body, and a bottom, the body and the bottom having a two-layer structure composed of an inner layer made of a virgin material that is an unused resin material, and an outer layer made of a recycled material prepared by recycling used resin material, a first injection molding step of injecting the recycled material into a first mold to injection mold an outer layer material; a second injection molding step of placing the outer layer material molded in the first injection molding step in a second mold and injecting the virgin material into the inner side of the outer layer material to injection mold an inner layer material, In the first injection molding step, a thin film portion is formed on the outer layer material, The thin film portion is formed thinner than the outer layer material around the thin film portion, In the second injection molding step, the virgin material is poured into the cavity by breaking the thin film portion due to the flow of the virgin material, In the injection molding process, the preform is configured to mold the inner layer material and the outer layer material so that the weight ratio of the recycled material to the total weight of the preform is 50% by weight or more, and the ratio of the thickness of the outer layer to the thickness of the inner layer in the body portion is 1.5 or more. A method for manufacturing a preform.
2. The thin film portion is formed as a recess formed by being pressed from the outer surface of the outer layer material. A method for producing the preform according to claim 1.
3. The amount of the virgin material injected in the second injection molding process is smaller than the amount of the recycled material injected in the first injection molding process, thereby reducing the degree of reheating of the recycled material. A method for producing the preform according to claim 1 or 2.
4. an injection molding step of injection molding a preform having an opening, a body, and a bottom, the body and the bottom having a two-layer structure composed of an inner layer made of a virgin material and an outer layer made of a recycled material; A temperature control step of controlling the temperature of the preform; a blow molding step of blow molding the preform to form a resin container; A method for producing a resin container by a hot parison method, comprising: The injection molding process includes: a first injection molding step of injecting the recycled material into a first mold to injection mold an outer layer material; a second injection molding step of housing the outer layer material molded in the first injection molding step in a second mold and injecting the virgin material into the inner side of the outer layer material to injection mold an inner layer material, In the first injection molding step, a thin film portion is formed on the outer layer material, The thin film portion is formed thinner than the outer layer material around the thin film portion, In the second injection molding step, the virgin material is poured into the cavity by breaking the thin film portion due to the flow of the virgin material, In the injection molding process, the preform is configured to mold the inner layer material and the outer layer material so that the weight ratio of the recycled material to the total weight of the preform is 50% by weight or more, and the ratio of the thickness of the outer layer to the thickness of the inner layer in the body portion is 1.5 or more. A method for manufacturing a resin container.
5. The thin film portion is formed as a recess formed by being pressed from the outer surface of the outer layer material. The method for producing the resin container according to claim 4.
6. and producing the resin container by a hot parison method. The method for producing a resin container according to claim 4 or 5.
7. The amount of the virgin material injected in the second injection molding process is smaller than the amount of the recycled material injected in the first injection molding process, thereby reducing the degree of reheating of the recycled material. A method for producing a resin container according to any one of claims 4 to 6.
8. A manufacturing apparatus for manufacturing a preform, the preform comprising an opening, a body, and a bottom, the body and the bottom having a two-layer structure composed of an inner layer made of a virgin material and an outer layer made of a recycled material, a first injection molding section including a first mold and configured to injection mold an outer layer material by injecting the recycled material from a first hot runner mold into the first mold; a second injection molding section including a second mold for accommodating the outer layer material molded in the first injection molding section, and for injection molding an inner layer material by injecting the virgin material from a second hot runner mold into the inside of the outer layer material; Equipped with In the first injection molding section, a thin film section is formed in the outer layer material, The thin film portion is formed thinner than the outer layer material around the thin film portion, In the second injection molding section, the virgin material is injected so as to break the thin film section and is poured into the cavity, The preform is configured to mold the inner layer material and the outer layer material so that a weight ratio of the recycled material to a total weight of the preform is 50% by weight or more, and a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more. An apparatus for manufacturing the preform.
9. the first hot runner mold includes a pin movable toward the outer layer material; After the recycled material is injected from a first hot runner mold into the first mold, the pin moves toward the outer layer material, whereby the outer layer material is pressed against an outer surface thereof to form the concave thin film portion. An apparatus for manufacturing a preform according to claim 8.
10. The injection amount of the virgin material injected in the second injection molding section is smaller than the injection amount of the recycled material injected in the first injection molding section, thereby reducing the degree of reheating of the recycled material. An apparatus for manufacturing a preform according to claim 8 or 9.
11. A manufacturing apparatus for manufacturing a resin container from a preform having a two-layer structure including an opening, a body, and a bottom, the body and the bottom being composed of an inner layer made of a virgin material and an outer layer made of a recycled material, a first injection molding section including a first mold and configured to injection mold an outer layer material by injecting the recycled material from a first hot runner mold into the first mold; a second injection molding section including a second mold for accommodating the outer layer material molded in the first injection molding section, and for injection molding an inner layer material by injecting the virgin material from a second hot runner mold into the inside of the outer layer material; a blow molding section for blow molding the preform into a resin container; Equipped with In the first injection molding section, a thin film section is formed in the outer layer material, The thin film portion is formed thinner than the outer layer material around the thin film portion, In the second injection molding section, the virgin material is injected so as to break the thin film section and is poured into the cavity, The preform is configured to mold the inner layer material and the outer layer material so that a weight ratio of the recycled material to a total weight of the preform is 50% by weight or more, and a ratio of a thickness of the outer layer to a thickness of the inner layer in the body portion is 1.5 or more. Plastic container manufacturing equipment.
12. the first hot runner mold includes a pin movable toward the outer layer material; After the recycled material is injected from a first hot runner mold into the first mold, the pin moves toward the outer layer material, whereby the outer layer material is pressed against an outer surface thereof to form the concave thin film portion. The resin container manufacturing apparatus according to claim 11.
13. The resin container is manufactured by a hot parison method. The resin container manufacturing apparatus according to claim 11 or 12.
14. The injection amount of the virgin material injected in the second injection molding section is smaller than the injection amount of the recycled material injected in the first injection molding section, thereby reducing the degree of reheating of the recycled material. The resin container manufacturing apparatus according to any one of claims 11 to 13.
Citation Information
Patent Citations
Polyethylene naphthalate for bottle
JP1995258394A
Multilayer preform with recovery polyester resin layer, manufacture of the preform, and multilayer container molded from the preform
JP1999090975A
Plastic bottle
JP2002103429A
Laminated resin bottle and manufacturing method for laminated resin molded product
JP2002104362A
Preform and biaxially stretched container produced by using preform
JP2004148616A