Nonaqueous electrolyte and nonaqueous secondary battery

A non-aqueous electrolyte with acetonitrile and cyclic anion-containing lithium salt enhances lithium ion battery durability at high temperatures and low temperatures by preventing metal elution and delamination, ensuring stable performance.

JP7587020B2Active Publication Date: 2024-11-19ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023509344
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-30
Filing Date
2022-03-25
Publication Date
2024-11-19
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

Lithium ion batteries using acetonitrile-based electrolytes exhibit inferior high-temperature durability compared to those using carbonate solvents, with issues such as delamination between the positive electrode current collector and active material leading to increased electrical resistance.

Method used

A non-aqueous electrolyte containing acetonitrile with a specific cyclic anion-containing lithium salt and LiPF6, within defined concentration ranges, to enhance long-term high-temperature durability and low-temperature characteristics.

Benefits of technology

The electrolyte improves high-temperature durability by suppressing metal elution and physical delamination, maintaining excellent output characteristics and low-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587020000042
    Figure 0007587020000042
  • Figure 0007587020000043
    Figure 0007587020000043
  • Figure 0007587020000001
    Figure 0007587020000001
Patent Text Reader

Abstract

The present invention provides a nonaqueous electrolyte solution which contains a nonaqueous solvent and a lithium salt, wherein: the nonaqueous solvent contains acetonitrile in an amount of 3% by volume to 97% by volume relative to the total amount of the nonaqueous solvent; the lithium salt contains a cyclic anion-containing lithium salt that is represented by formula (1) (wherein Rf moieties may be the same as or different from each other, and each represents a fluorine atom or a perfluoro group having 4 or less carbon atoms); and the content of the cyclic anion-containing lithium salt that is represented by formula (1) is from 0.001 to 5 in terms of the molar ratio relative to the content of the acetonitrile.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nonaqueous electrolyte and a nonaqueous secondary battery. [Background technology]

[0002] Lithium ion batteries and other non-aqueous secondary batteries are characterized by their light weight, high energy and long life, and are widely used as power sources for various portable electronic devices. In recent years, non-aqueous electrolytes have been widely used for industrial applications, such as power tools, and for in-vehicle applications, such as electric vehicles and electric bicycles, and are also attracting attention in the field of power storage, such as residential power storage systems.

[0003] A typical example of a non-aqueous electrolyte for a lithium ion battery is a combination of a highly dielectric solvent such as a cyclic carbonate ester and a low viscosity solvent such as a chain carbonate ester. In addition, it is desirable to add an electrode protection additive such as vinylene carbonate to form a solid electrolyte interface (SEI) on the negative electrode surface and thereby suppress the reductive decomposition of the non-aqueous solvent.

[0004] In recent years, with the expansion of the large-scale power storage industry, mainly for electric vehicles, there is a strong demand for non-aqueous secondary batteries with higher energy density. As a non-aqueous solvent for lithium-ion batteries, nitrile-based solvents, which have an excellent balance between viscosity and dielectric constant, have been proposed as highly ion-conductive electrolytes. Among them, acetonitrile has high potential.

[0005] For example, in Patent Document 1, the formula LiN(SO 2 CF 3 ) 2 It is described that reversible lithium insertion / extraction to / from a graphite electrode is possible by using an electrolyte in which lithium bis(trifluoromethanesulfonyl)imide represented by the following formula is dissolved in acetonitrile to a concentration of 4.2 mol / L.

[0006] Patent Document 2 discloses a nonaqueous secondary battery that operates with a high-capacity electrode using an electrolyte solution that uses acetonitrile as a nonaqueous solvent, and also reports that the SEI is strengthened by adding multiple electrode protection additives.

[0007] Patent Document 3 reports that the use of a specific organic lithium salt strengthens the SEI, suppresses decomposition of the electrolyte, and provides excellent output characteristics.

[0008] Patent Document 4 reports that a non-aqueous electrolyte solution containing acetonitrile and a lithium-containing imide salt can effectively suppress the decrease in ion conductivity in the low temperature range, thereby obtaining excellent low-temperature characteristics.

[0009] Patent Document 5 reports that in a non-aqueous electrolyte solution containing acetonitrile, high-temperature durability can be improved by controlling the blending ratio of lithium salt. More specifically, Patent Document 5 reports that acetonitrile, a lithium-containing imide salt, and LiPF 6 Regarding non-aqueous electrolytes containing LiPF 6 A battery has been reported that prevents corrosion of the aluminum (Al) current collector by controlling the content of hydrogen fluoride (HF) to 0.01 mol / L or more and generating the amount of hydrogen fluoride (HF) necessary to form an aluminum passivation state.

[0010] On the other hand, studies are also being conducted to improve battery performance by using specific organic lithium salts in non-aqueous electrolyte solutions.

[0011] For example, Patent Documents 6 and 7 report that by combining a specific organic lithium salt with an ether-based solvent, it is possible to provide a non-aqueous electrolyte solution that is free from the risk of electrode corrosion and has both non-flammability and sufficient electrical conductivity for practical use.

[0012] Patent Document 8 reports that it is possible to provide a non-aqueous electrolyte solution that combines excellent non-flammability and cycle characteristics by combining a specific organic lithium salt with an ether-based solvent. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] International Publication No. 2013 / 146714 [Patent Document 2] International Publication No. 2013 / 062056 [Patent Document 3] International Publication No. 2012 / 057311 [Patent Document 4] International Publication No. 2018 / 169029 [Patent Document 5] International Publication No. 2020 / 262670 [Patent Document 6] International Publication No. 2009 / 133899 [Patent Document 7] International Publication No. 2010 / 110388 [Patent Document 8] International Publication No. 2011 / 052605 Summary of the Invention [Problem to be solved by the invention]

[0014] Furthermore, in the techniques described in Patent Documents 1 to 4, the lithium ion batteries using an acetonitrile-containing electrolyte solution are inferior in high-temperature durability to existing lithium ion batteries using an electrolyte solution containing a carbonate solvent.

[0015] The technology described in Patent Document 5 has been shown to have higher high-temperature durability than existing electrolytes in a long-term storage test at 85°C. However, the recovered capacity retention rate after storage at 85°C for 10 days is lower than that of existing carbonates, leaving room for improvement.

[0016] Furthermore, the techniques described in Patent Documents 6 to 8 have not been evaluated for high temperature durability.

[0017] As a result of disassembly and analysis of a battery by the present inventors, it was found that when a battery is stored for a long period of time in a high-temperature environment, peeling occurs between the positive electrode current collector and the positive electrode active material, and the electrical resistance at the peeling site increases and the high-temperature durability decreases. This phenomenon is a new problem not described in Patent Documents 1 to 8.

[0018] The present invention has been made in view of the above circumstances. An object of the present invention is to provide a non-aqueous electrolyte solution containing acetonitrile that can improve long-term high-temperature durability while exhibiting excellent output characteristics and low-temperature characteristics, and a non-aqueous secondary battery including the same. [Means for solving the problem]

[0019] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result have found that the above-mentioned problems can be solved by using a nonaqueous electrolyte or a nonaqueous secondary battery having the following composition, thereby completing the present invention. That is, the present invention is as follows: <1> A non-aqueous electrolyte solution containing a non-aqueous solvent and a lithium salt, The non-aqueous solvent contains acetonitrile in an amount of 3% by volume or more and 97% by volume or less based on the total amount of the non-aqueous solvent; and The lithium salt is represented by the following formula (1): [ka] {where, R f may be the same or different and each represents a fluorine atom or a perfluoro group having 4 or less carbon atoms. The lithium salt contains a cyclic anion represented by the formula: The nonaqueous electrolyte solution has a molar ratio of the content of the cyclic anion-containing lithium salt represented by the formula (1) to the content of the acetonitrile of 0.001 or more and 5 or less. <2> The cyclic anion-containing lithium salt represented by the formula (1) is represented by the following formulas (1-1) to (1-5): [ka] 2. The nonaqueous electrolyte solution according to item 1, comprising one or more cyclic anion-containing lithium salts represented by the formula: <3> 3. The nonaqueous electrolyte solution according to item 1 or 2, wherein the content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.08 or more and 0.79 or less in terms of a molar ratio relative to the content of the acetonitrile. <4> 4. The nonaqueous electrolyte solution according to any one of items 1 to 3, wherein the content of the acetonitrile is 10% by volume or more and 66% by volume or less with respect to the total amount of the nonaqueous solvent. <5> The lithium salt is LiPF 6 and Said LiPF 6 and the cyclic anion-containing lithium salt represented by the formula (1) are mixed to form LiPF 6 5. The nonaqueous electrolyte solution according to any one of items 1 to 4, wherein the cyclic anion-containing lithium salt is contained at a molar concentration such that: <6> The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The nonaqueous electrolyte solution according to item 5, wherein the molar ratio of the content of <7> Said LiPF 6 is less than 0.01 mol per 1 L of the nonaqueous solvent. <8> The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The nonaqueous electrolyte solution according to any one of items 5 to 7, wherein the molar ratio of the amount of the metal oxide to the amount of the cation exchange resin is 150 or less with respect to the content of the metal oxide. <9> The lithium salt is LiPF 6 5. The nonaqueous electrolyte solution according to any one of items 1 to 4, which does not contain <10> The nonaqueous electrolyte solution is a compound represented by the following formula (2): [ka] {where, R 1 , R 2 , and R 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a fluorine-substituted alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a fluorine-substituted alkoxy group having 1 to 4 carbon atoms, a phenyl group, a cyclohexyl group, a nitrile group, a nitro group, an amino group, an N,N'-dimethylamino group, or an N,N'-diethylamino group, and two or more of these substituents are hydrogen atoms. 10. The nonaqueous electrolyte solution according to any one of items 1 to 9, further comprising a nitrogen-containing cyclic compound represented by the following formula: <11> Item 11. The nonaqueous electrolyte solution according to item 10, wherein the content of the nitrogen-containing cyclic compound represented by the formula (2) is 0.0001 or more and 3 or less in terms of a molar ratio relative to the content of the cyclic anion-containing lithium salt represented by the formula (1). <12> Item 12. The nonaqueous electrolyte solution according to item 10 or 11, wherein the nitrogen-containing cyclic compound represented by formula (2) is one or more compounds selected from the group consisting of pyridine and 4-(tert-butyl)pyridine. <13> 13. The nonaqueous electrolyte solution according to any one of items 10 to 12, wherein the content of the nitrogen-containing cyclic compound represented by the formula (2) is 0.01% by mass or more and 10% by mass or less with respect to the total amount of the nonaqueous electrolyte solution. <14> The nonaqueous electrolyte solution is a compound represented by the following general formula (3): X-Si(OR 3 ) (3-m) R 4 m ...(3) {where, R 3 and R 4 represents an alkyl group which may be substituted with an aryl group, an alkoxysilyl group, or a halogen atom, or an aryl group which may be substituted with an alkyl group, an alkoxysilyl group, or a halogen atom, and X represents a group represented by the following formula (L1): [ka] (wherein k is an integer of 0 to 8, and * indicates the bonding site with Si), The following formula (L2): [ka] (wherein j is an integer of 0 to 8, and * indicates the bonding site with Si), The following formula (L3): [ka] (wherein h is an integer of 0 to 8, g is an integer of 0 or 1, and * indicates the bonding site to Si), and The following formula (L4) [ka] (In the formula, * indicates the bond site with Si) and m is an integer of 0 to 2}; The following general formula (4): [ka] {wherein each X independently represents at least one selected from the group consisting of groups represented by formulas (L1) to (L4), and d represents an integer of 0 to 10,000.} The following general formula (5): [ka] {where, R 5 each independently represents an aryl group or an alkyl group which may be substituted with a halogen atom, or an aryl group which may be substituted with an alkyl group or a halogen atom, y is an integer of 2 to 8, and X represents at least one selected from the group consisting of the groups represented by the formulas (L1) to (L4). The following general formula (6): X-Si(OR 3 'OR 3 ) (3-m) R 4 m ...(6) {where, R 3 , R 4 , X, and m are as defined in general formula (3), and R 3 ' is an aryl group, an alkoxysilyl group, or an alkylene group which may be substituted with a halogen atom; The following general formula (7): [ka] A compound represented by the formula (7): {in which R is each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 5 to 20 carbon atoms; X is O, S, or NH; Z is P, P=O, B, or Si; when Z is P or P=O, n1 is 1, n2 is an integer of 1 to 3, and n2+n3=3; when Z is B, n1 is 1, n2 is an integer of 1 to 3, and n2+n3=3; when Z is Si, n1 is 0, n2 is an integer of 1 to 4, and n2+n3=4.}, and The following general formula (8): [ka] 14. The nonaqueous electrolyte solution according to any one of items 1 to 13, further comprising a polymer compound containing a repeating unit represented by the following formula: {R in formula (8) has the same meaning as R in formula (7).}, and at least one silane compound selected from the group consisting of diphenyldialkoxysilanes. <15> Item 15. The nonaqueous electrolyte solution according to item 14, wherein the content of the silane compound is 0.0001 or more and 1.5 or less in terms of a molar ratio relative to the content of the cyclic anion-containing lithium salt represented by formula (1). <16> Item 16. The nonaqueous electrolyte solution according to item 14 or 15, wherein the silane-based compound is at least one selected from the group consisting of triethoxyvinylsilane, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) phosphite, tris(2,2,2-trifluoroethyl) phosphite, and diphenyldimethoxysilane. <17> 17. The non-aqueous electrolyte solution according to any one of items 14 to 16, wherein the content of the silane compound is 0.01% by mass or more and 10% by mass or less with respect to the total amount of the non-aqueous electrolyte solution. <18> 18. A non-aqueous secondary battery comprising: a positive electrode containing a positive electrode active material; a negative electrode containing a negative electrode active material; and the non-aqueous electrolyte solution according to any one of items 1 to 17. <19> The positive electrode active material includes a lithium phosphorus metal oxide having an olivine crystal structure containing iron (Fe) atoms, The non-aqueous electrolyte solution is The content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.9 or more in terms of molar ratio with respect to the total content of the lithium salts, The lithium salt is LiPF 6 Contains The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The molar ratio of the content of The content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.08 or more and 0.27 or less in terms of molar ratio with respect to the content of the acetonitrile; and Item 19. The nonaqueous secondary battery according to item 18, wherein the content of the acetonitrile is 30% by volume or more and 66% by volume or less with respect to the total amount of the nonaqueous solvent. <20> The positive electrode active material is represented by the following general formula (a t ): Li p Ni q Co r Mn s M t O u (a t ) {In the formula, M is at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba, and 0 < p < 1.3, 0 < q < 1.2, 0 < r < 1.2, 0 ≦ s < 0.5, 0 ≦ t < 0.3, 0.7 ≦ q + r + s + t ≦ 1.2, 1.8 < u < 2.2, and p is a value determined by the charge and discharge state of the battery.} comprising a lithium-containing metal oxide represented by The non-aqueous electrolyte contains the lithium salt LiPF 6 and The content of the cyclic anion-containing lithium salt represented by the formula (1) is 3 or more and 150 or less in molar ratio with respect to the content of the LiPF 6 and The content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.15 or more and 0.79 or less in molar ratio with respect to the content of the acetonitrile, and The content of the acetonitrile is 10% by volume or more and 50% by volume or less with respect to the total amount of the non-aqueous solvent. The non-aqueous secondary battery according to item 18. <21> The non-aqueous secondary battery includes a battery exterior, and the battery exterior contains aluminum in at least a part of the liquid contact layer on the positive electrode side with the non-aqueous electrolyte. The non-aqueous secondary battery according to any one of items 18 to 20. <22> In the battery exterior, at least a part of the contact portion on the positive electrode side with the non-aqueous electrolyte is made of iron or an iron alloy. The non-aqueous secondary battery according to any one of items 18 to 20. <23> The surface of the battery exterior made of iron or an iron alloy is not coated. The non-aqueous secondary battery according to item 22. <24> In the battery exterior, at least a part of the contact portion on the positive electrode side with the non-aqueous electrolyte is made of the iron alloy, and the iron alloy is stainless steel (SUS). The non-aqueous secondary battery according to item 22 or 23. <25> The potential of the positive electrode when fully charged is Li / Li + 25. The nonaqueous secondary battery according to any one of items 22 to 24, having a reference potential of 5.1 V or less. Effect of the Invention

[0020] According to the present invention, it is possible to provide a nonaqueous electrolyte solution that exhibits excellent output characteristics and low-temperature characteristics while improving long-term high-temperature durability, and a nonaqueous secondary battery including the same. [Brief description of the drawings]

[0021] [Figure 1] 1 is a plan view illustrating a schematic example of a nonaqueous secondary battery according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line AA of the nonaqueous secondary battery of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention. In this specification, a numerical range described using "~" includes the numerical values ​​described before and after it.

[0023] <1. Non-aqueous electrolyte> The non-aqueous electrolyte refers to an electrolyte containing 1% by mass or less of water relative to the total amount of the non-aqueous electrolyte. The non-aqueous electrolyte according to the present embodiment is preferably free of water as much as possible, but may contain a very small amount of water as long as it does not impede the solution of the problem of the present invention. The content of such water is 300 ppm by mass or less, preferably 200 ppm by mass or less, based on the total amount of the non-aqueous electrolyte. As long as the non-aqueous electrolyte has a configuration for achieving the solution of the problem of the present invention, the other components can be appropriately selected and applied from the constituent materials in the known non-aqueous electrolyte used in lithium ion batteries.

[0024] The non-aqueous electrolyte solution of the present embodiment can be produced by mixing a lithium salt and, if desired, various additives shown below (sometimes simply referred to as "additives" in this specification) with a non-aqueous solvent by any means. Note that the various additives are a general term for additives for protecting electrodes and other optional additives, and the contents thereof are as shown below.

[0025] Unless otherwise specified, the content of each compound in the non-aqueous solvent is specified in terms of volume % relative to the total amount of each component constituting the non-aqueous solvent for each component described in <2-1. Non-aqueous solvent> and the electrode protection additive described in <2-3. Additive for electrode protection>, the mixing ratio is specified in terms of the number of moles per 1 L of non-aqueous solvent for the lithium salt described in <2-2. Lithium salt>, and the mixing ratio is specified in terms of parts by mass when the lithium salt and the entire non-aqueous solvent are taken as 100 parts by mass for <2-4. Other optional additives>.

[0026] In the present embodiment, when the electrolyte solution contains a compound other than the compounds specifically shown in each of the items <2-1> to <2-4> below, if the compound is liquid at room temperature (25°C), it is treated as a non-aqueous solvent and the mixing ratio is expressed in volume % relative to the total amount of each component (including the compound) constituting the non-aqueous solvent. On the other hand, if the compound is solid at room temperature (25°C), the mixing ratio is expressed in parts by mass when the total amount of the lithium salt and the non-aqueous solvent is 100 parts by mass.

[0027] From the results of various verification experiments, the reason why lithium ion secondary batteries using a nonaqueous electrolyte solution containing acetonitrile have poor high-temperature durability is considered as follows. (1) The nitrile group of acetonitrile has a high metal coordination ability, so it forms a complex with the transition metal in the positive electrode active material, stabilizing it and promoting metal dissolution. Metal ions dissolved in the non-aqueous electrolyte are reduced and precipitated on the negative electrode side, damaging the SEI of the negative electrode. This promotes the reductive decomposition of the solvent at the negative electrode, increasing the irreversible capacity, and the reductively decomposed solvent accumulates on the negative electrode, increasing the internal resistance. This phenomenon is promoted at higher temperatures and for longer periods of time. (2) As a result of disassembly and analysis of a lithium-ion secondary battery using an electrolyte solution containing acetonitrile, it was found that physical peeling occurs between the positive electrode Al current collector and the positive electrode active material when the battery is stored for a long period of time in a high-temperature environment. It is presumed that the high-temperature durability is reduced due to an increase in electrical resistance at the peeled portion. These phenomena, which are supported by the results of the disassembly and analysis, are issues newly discovered by the present inventors and are not described at all in Patent Documents 1 to 8.

[0028] These phenomena are prominent in high-temperature environments exceeding 45° C., more prominent in high-temperature environments exceeding 60° C., and even more prominent in high-temperature environments exceeding 80° C. Moreover, such tendencies are prominent when the exposure time to high temperatures is 4 hours or more, more prominent when the exposure time is 100 hours or more, more prominent when the exposure time is 200 hours or more, more prominent when the exposure time is 300 hours or more, and even more prominent when the exposure time is 400 hours or more.

[0029] <2-1.Non-aqueous solvents> In the present embodiment, the term "non-aqueous solvent" refers to elements in the non-aqueous electrolyte excluding lithium salt and various additives. When the non-aqueous electrolyte contains an additive for protecting an electrode, the term "non-aqueous solvent" refers to elements in the non-aqueous electrolyte excluding lithium salt and additives other than the additive for protecting an electrode. Examples of non-aqueous solvents include alcohols such as methanol and ethanol; aprotic solvents, etc. Among them, aprotic solvents are preferred as non-aqueous solvents. The non-aqueous solvent may contain a solvent other than the aprotic solvent as long as it does not hinder the problem solving of the present invention.

[0030] The non-aqueous solvent related to the non-aqueous electrolyte of this embodiment contains acetonitrile as an aprotic solvent. The non-aqueous solvent contains acetonitrile, which improves the ionic conductivity of the non-aqueous electrolyte, thereby increasing the diffusibility of lithium ions in the battery. Therefore, even in a positive electrode in which the positive electrode active material layer is thickened to increase the amount of positive electrode active material filled, lithium ions can be well diffused to the area near the current collector where lithium ions are difficult to reach during high-load discharge. Therefore, it is possible to extract sufficient capacity even during high-load discharge, and a non-aqueous secondary battery with excellent load characteristics can be obtained.

[0031] Furthermore, the non-aqueous solvent contains acetonitrile, which can improve the rapid charging characteristics of the non-aqueous secondary battery. In constant current (CC)-constant voltage (CV) charging of a non-aqueous secondary battery, the capacity per unit time during the CC charging period is greater than the charge capacity per unit time during the CV charging period. When acetonitrile is used as the non-aqueous solvent of the non-aqueous electrolyte, the range in which CC charging is possible can be expanded (CC charging time can be extended) and the charging current can also be increased, so that the time from the start of charging to fully charging the non-aqueous secondary battery can be significantly shortened.

[0032] In addition, acetonitrile is easily electrochemically reduced and decomposed, so when acetonitrile is used, it is preferable to use another solvent (e.g., an aprotic solvent other than acetonitrile) together with acetonitrile as a non-aqueous solvent and / or to add an additive for protecting an electrode for forming a protective film on the electrode.

[0033] The content of acetonitrile is 3% by volume or more and 97% by volume or less based on the total amount of the non-aqueous solvent. The content of acetonitrile is more preferably 5% by volume or more, 10% by volume or more, 20% by volume or more, or 30% by volume or more based on the total amount of the non-aqueous solvent, and more preferably 35% by volume or more. This value is more preferably 85% by volume or less, 66% by volume or less, and more preferably 60% by volume or less. When the content of acetonitrile is 3% by volume or more based on the total amount of the non-aqueous solvent, the ion conductivity increases, and high output characteristics and excellent low-temperature characteristics tend to be exhibited, and furthermore, the dissolution of the lithium salt can be promoted. When the content of acetonitrile is 97% by volume or less based on the total amount of the non-aqueous solvent, the elution of the transition metal caused by the coordination of acetonitrile with the transition metal in the positive electrode active material is suppressed, and physical peeling between the positive electrode Al current collector and the positive electrode active material is suppressed, and excellent high-temperature durability tends to be exhibited. Since the additive described below suppresses an increase in the internal resistance of the battery, when the content of acetonitrile in the non-aqueous solvent is within the above range, the high-temperature cycle characteristics and other battery characteristics tend to be improved while maintaining the excellent performance of acetonitrile.

[0034] The preferred range of the acetonitrile content varies depending on the type of positive electrode active material used in combination.

[0035] Examples of aprotic solvents other than acetonitrile include cyclic carbonates, fluoroethylene carbonate, lactones, organic compounds having sulfur atoms, chain carbonates, cyclic ethers, mononitriles other than acetonitrile, alkoxy group-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, and compounds in which some or all of the H atoms of the aprotic solvents are substituted with halogen atoms.

[0036] Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, trans-2,3-butylene carbonate, cis-2,3-butylene carbonate, 1,2-pentylene carbonate, trans-2,3-pentylene carbonate, cis-2,3-pentylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinylethylene carbonate;

[0037] Fluoroethylene carbonates include, for example, 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one;

[0038] Lactones include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone;

[0039] Examples of organic compounds having sulfur atoms include ethylene sulfite, propylene sulfite, butylene sulfite, pentene sulfite, sulfolane, 3-sulfolene, 3-methyl sulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propene 1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite;

[0040] Examples of chain carbonates include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, and ethyl propyl carbonate;

[0041] Cyclic ethers include, for example, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane;

[0042] Examples of mononitriles other than acetonitrile include propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile;

[0043] Alkoxy group-substituted nitriles include, for example, methoxyacetonitrile and 3-methoxypropionitrile;

[0044] Dinitriles include, for example, malononitrile, succinonitrile, glutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, and 2,4-dimethylglutaronitrile;

[0045] Cyclic nitriles include, for example, benzonitrile;

[0046] Examples of short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl hydroangelate, methyl caproate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl hydroangelate, ethyl caproate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl hydroangelate, propyl caproate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, isopropyl valerate, and isopropyl pivalate. propyl, isopropyl hydroangelate, isopropyl caproate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl pivalate, butyl hydroangelate, butyl caproate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl pivalate, isobutyl hydroangelate, isobutyl caproate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl pivalate, tert-butyl hydroangelate, and tert-butyl caproate;

[0047] Chain ethers include, for example, dimethoxyethane, diethyl ether, 1,3-dioxolane, diglyme, triglyme, and tetraglyme;

[0048] Examples of fluorinated ethers include R f aa -OR bb {where, R f aa is an alkyl group containing a fluorine atom, R bb is an organic group which may contain a fluorine atom};

[0049] Ketones, for example, acetone, methyl ethyl ketone, and methyl isobutyl ketone;

[0050] Examples of the aprotic solvent compound in which some or all of the H atoms have been substituted with halogen atoms include compounds in which the halogen atoms are fluorine; The following can be mentioned.

[0051] Here, examples of the fluorinated chain carbonate include methyl trifluoroethyl carbonate, trifluorodimethyl carbonate, trifluorodiethyl carbonate, trifluoroethyl methyl carbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, methyl 2,2,3,3-tetrafluoropropyl carbonate, etc. The above-mentioned fluorinated chain carbonate is represented by the following general formula: R cc -OC(O)OR dd {where, R cc and R dd is CH 3 , C.H. 2 CH 3 , C.H. 2 CH 2 CH 3 , CH(CH 3 ) 2 , and C.H. 2 R f ee and R is at least one selected from the group consisting of f ee is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is substituted with at least one fluorine atom, and R cc and / or R dd contains at least one fluorine atom} It can be expressed as:

[0052] Examples of fluorinated short-chain fatty acid esters include fluorinated short-chain fatty acid esters such as 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, and 2,2,3,3-tetrafluoropropyl acetate. Fluorinated short-chain fatty acid esters are represented by the following general formula: R ff -C(O)OR gg {where, R ff is CH 3 , C.H. 2 CH 3 ,CH 2 CH 2 CH 3 , CH(CH 3 ) 2 , C.F. 3 CF 2 H, CFH 2 , C.F. 2 R f hh , CFHR f hh , and C.H. 2 R f ii and R is at least one selected from the group consisting of gg is CH 3 , C.H. 2 CH 3 , C.H. 2 CH 2 CH 3 , CH(CH 3 ) 2 , and C.H. 2 R f ii and R is at least one selected from the group consisting of f hh is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom may be substituted with at least one fluorine atom, and R f ii is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is substituted with at least one fluorine atom, and R ff and / or R gg contains at least one fluorine atom, and R ff CF 2 If H, then R gg CH 3(not

[0053] In the present embodiment, the aprotic solvent other than acetonitrile may be used alone or in combination of two or more kinds.

[0054] In the present embodiment, the non-aqueous solvent is preferably used in combination with acetonitrile and one or more of a cyclic carbonate and a chain carbonate from the viewpoint of improving the stability of the non-aqueous electrolyte. From this viewpoint, the non-aqueous solvent in the present embodiment is more preferably used in combination with acetonitrile and a cyclic carbonate, and more preferably used in combination with acetonitrile and both a cyclic carbonate and a chain carbonate.

[0055] When a cyclic carbonate is used with acetonitrile, it is particularly preferred that such cyclic carbonate comprises ethylene carbonate, vinylene carbonate, and / or fluoroethylene carbonate.

[0056] <2-2. Lithium salts> (Lithium salts containing cyclic anions) The nonaqueous electrolyte according to this embodiment is The following general formula (1): [ka] {where, R f may be the same or different and each represents a fluorine atom or a perfluoro group having 4 or less carbon atoms. The lithium salt contains a cyclic anion represented by the formula:

[0057] In a non-aqueous electrolyte solution containing acetonitrile, the use of a cyclic anion-containing lithium salt represented by formula (1) improves long-term high-temperature durability. The mechanism is presumed to be as follows.

[0058] The cyclic anion-containing lithium salt represented by formula (1) (hereinafter also referred to as compound (1)) dissociates into lithium ions and cyclic anions in a non-aqueous electrolyte solution containing acetonitrile. The cyclic anion electrically interacts with acetonitrile, weakening the metal coordination ability of the nitrile group of acetonitrile. This makes it possible to suppress metal elution caused by acetonitrile forming a complex with a transition metal in the positive electrode active material at high temperatures, and to suppress the migration of the metal complex to the negative electrode. Therefore, deterioration of the negative electrode SEI due to reductive precipitation of the metal complex at the negative electrode is suppressed, and long-term high-temperature durability is improved.

[0059] In addition, the decomposition products produced by the reductive decomposition of cyclic anions at the negative electrode accumulate on the negative electrode and act as SEI, improving the durability of the negative electrode SEI against reductive precipitation of metal complexes at the negative electrode and suppressing the reductive decomposition of the solvent at the negative electrode.

[0060] In addition, by using the cyclic anion-containing lithium salt represented by formula (1) in a non-aqueous electrolyte solution containing acetonitrile, the physical peeling phenomenon between the positive electrode Al current collector and the positive electrode active material can be suppressed. This peeling phenomenon is presumably caused by the following mechanism. The imide anions of various lithium-containing imide salts in the non-aqueous electrolyte solution coordinate with the Al on the surface of the positive electrode Al current collector to form a stable Al-imide complex. This Al-imide complex is easily dissolved in acetonitrile, which has high polarity, so its dissolution is promoted in the non-aqueous electrolyte solution containing acetonitrile. As a result, the surface of the Al current collector is scraped off, causing physical peeling between the positive electrode Al current collector and the positive electrode active material. From the results of analytical simulations of the behavior of various lithium-containing imide salts and lithium salts containing cyclic anions in acetonitrile, LiN(SO 2 F) 2 and LiN(SO 2 CF 3It was found that compared to chain-like lithium-containing imide salts such as ), lithium ions and the nitrogen atom of the imide anion in cyclic anion-containing lithium salts are less likely to dissociate. From this result, it was found that in cyclic anion-containing lithium salts, lithium remains close to the nitrogen atom of the imide anion derived from the lithium salt, making it difficult for the nitrogen atom of the imide anion to coordinate with the aluminum on the surface of the positive electrode aluminum current collector, suppressing the formation of an aluminum-imide complex. It is presumed that as a result, physical peeling between the positive electrode aluminum current collector and the positive electrode active material is suppressed.

[0061] The detailed results of the analytical simulation are shown below.

[0062] (Molecular dynamics simulation of non-aqueous electrolyte consisting of Li salt and acetonitrile solvent) A solution model of LiX and acetonitrile solvent was created (X = CTFSI, TFSI, FSI, represented by the structural formula below), and the motion of solution molecules was simulated. The existence probability distribution (radial distribution function) of the distance between the Li ion and the nitrogen atom (derived from the imide anion X) was analyzed, and the dissociation state of the Li salt was evaluated. As a result, it was found that the Li ion and nitrogen atom are less likely to dissociate in CTFSI than in TFSI and FSI, and the Li ion remains closer to the nitrogen atom of the imide anion. [ka] Next, we focused on specific Li salts in the solution model and analyzed the movement of Li ions in more detail. As a result, we found that in TFSI and FSI, Li ions move from near the nitrogen atom of the imide anion to near the oxygen atom. On the other hand, in CTFSI, the movement of Li ions is difficult, and the Li ions continue to remain near the nitrogen atom of the imide anion. In TFSI and FSI, it is thought that the Li ions move from near the nitrogen atom to near the oxygen atom due to intramolecular rotation. On the other hand, in the cyclic CTFSI, the degree of freedom of intramolecular rotation is small, so it is thought that the movement of Li ions from near the nitrogen atom to near the oxygen atom is difficult.

[0063] Detailed conditions for the motion simulation are shown below. (Common conditions) The simulation was performed using Materials Studio 2019. COMPASSII was used as the force field. The atomic charges were assigned values ​​by the COMPASSII force field parameters. The Ewald method was used to calculate the electrostatic interactions. The cutoff radius r of the Van der Waals interactions was c is c = 9.5 Å. The temperature was controlled by Nose-Hoover Langevin dynamics, and the pressure was controlled by Berendsen's method. (i. Creation of solution model) The solution model was created using the Amorphous Cell module in Materials studio 2019. Three-dimensional periodic boundary conditions were imposed on the solution model, and the unit cell was set to contain 570 acetonitrile molecules and 30 LiX molecules (X = CTFSI, TFSI, FSI). The initial structure had a density of 0.5 g / cm. 3 Created with. (ii. Structural relaxation of the solution model) The Forcite module of Materials studio 2019 was used to simulate the solution model. After optimizing the initial structure, structural relaxation was performed by annealing calculations followed by MD simulations in the NPT ensemble (constant particle number, pressure, and temperature). Annealing consisted of five cycles of heating and cooling in the temperature range of 300K to 500K, with a total simulation time of 500ps and a time step of 1fs. The NPT simulation was performed at a temperature of 298K and a pressure of 1013hPa, with a total simulation time of 500ps and a time step of 1.0fs. (iii. Simulation for data acquisition) The NPT simulation for data acquisition was performed for 500 ps under the same conditions as above. For the obtained structure trajectory, the radial distribution function between the Li ion and the nitrogen atom of the imide anion was calculated.

[0064] R in formula (1) fRegarding the above, the perfluoro group having 4 or less carbon atoms may be, for example, a perfluoroalkyl group having 1 to 4 carbon atoms. Specific examples of the compound (1) include compounds represented by the following formulas (1-1) to (1-5) (hereinafter also referred to as compounds (1-1) to (1-5), respectively). In the formula (1), one or more fluorine atoms may be substituted with a perfluoroalkyl group having 4 or less carbon atoms. When a fluorine atom is substituted with a perfluoroalkyl group, the number of fluorine atoms substituted with the perfluoroalkyl group is preferably 2 or less, more preferably 1. The number of carbon atoms in the perfluoroalkyl group is preferably 2 or less, and the perfluoroalkyl group is preferably a trifluoromethyl group. The cyclic anion-containing lithium salt represented by the formula (1) is preferably a compound represented by the compounds (1-1) to (1-5), more preferably a compound represented by the compounds (1-1) to (1-3), and even more preferably a compound represented by the compound (1-2). [ka]

[0065] As a result of further investigation, it was found that in an electrolyte solution containing acetonitrile, the cyclic anion-containing lithium salt represented by formula (1) has a significantly improved high-temperature durability compared to the case where the cyclic anion-containing lithium salt represented by the following formula (9) is used. From the results of various verification experiments, the reason for this is considered to be as follows: [ka] In the lithium salt containing a 6-membered ring cyclic anion represented by formula (9), the bond between the fluorine atom and the carbon atom in the difluoromethylene group that is not adjacent to the sulfonyl group is weak, so that the fluorine anion is eliminated by reduction at the negative electrode during charging. The eliminated fluorine anion is easily stabilized in a non-aqueous electrolyte containing highly polar acetonitrile, so that the above-mentioned elimination reaction continues to proceed, resulting in a decrease in high-temperature durability. On the other hand, compound (1) does not eliminate fluorine anion during charging as compared to compound (9), so that the high-temperature durability does not decrease. In particular, in the lithium salt containing a 5-membered ring cyclic anion represented by formula (1-2), the bond between the fluorine atom and the carbon atom in the two difluoromethylene groups is strong, so that the fluorine anion is not eliminated during charging, so that the high-temperature durability does not decrease.

[0066] In addition, as the molecular weight of the lithium salt increases, the weight of the lithium salt required to prepare a non-aqueous electrolyte solution containing a certain molar concentration of lithium ions increases, and the viscosity of the non-aqueous electrolyte solution increases, tending to reduce output characteristics. Therefore, by using compound (1), which has a smaller number of atoms constituting the ring compared to formula (9), particularly the cyclic anion-containing lithium salt represented by formula (1-2), excellent output characteristics can be achieved.

[0067] The content of the cyclic anion-containing lithium salt represented by formula (1) is preferably 0.1 mol or more, more preferably 0.5 mol or more, and even more preferably 0.8 mol or more, per 1 L of non-aqueous solvent. When it is within the above range, the ionic conductivity increases, and high output characteristics tend to be exhibited. In addition, the content of the cyclic anion-containing lithium salt represented by formula (1) is preferably less than 3 mol, more preferably 2.5 mol or less, and even more preferably 1.5 mol or less, per 1 L of non-aqueous solvent. When the content of the cyclic anion-containing lithium salt represented by formula (1) is within the above range, the ionic conductivity of the non-aqueous electrolyte increases, and the high output characteristics of the battery can be exhibited, and the decrease in ionic conductivity due to the increase in viscosity of the non-aqueous electrolyte at low temperatures tends to be suppressed, and the high temperature cycle characteristics and other characteristics of the battery tend to be further improved while maintaining the excellent performance of the non-aqueous electrolyte.

[0068] In order to improve the volumetric energy density of the nonaqueous secondary battery, the weight of the positive electrode active material layer contained in the positive electrode is set to 24 to 200 mg / cm. 2 When the content of the cyclic anion-containing lithium salt represented by formula (1) is adjusted to the range, the content is preferably 1 mol or more, more preferably 1.2 mol or more, even more preferably 1.5 mol or more, and particularly preferably 2 mol or more. When the content of the cyclic anion-containing lithium salt represented by formula (1) is within the above-mentioned range, quick ion conduction is possible even in the deep part of the positive electrode away from the positive electrode-electrolyte interface, and there is a tendency that the volumetric energy density can be improved while maintaining a balance with the output performance in the nonaqueous secondary battery.

[0069] In the non-aqueous electrolyte, the content of the cyclic anion-containing lithium salt represented by formula (1) relative to the content of acetonitrile is 0.001 or more and 5 or less in molar ratio. From the viewpoint of suppressing the elution of the positive electrode metal by acetonitrile at high temperatures and suppressing the decomposition of the solvent at the negative electrode, the molar ratio of the content of the cyclic anion-containing lithium salt to the content of acetonitrile is preferably 0.001 or more, more preferably 0.01 or more, more preferably 0.08 or more, and even more preferably 0.1 or more. When the molar ratio of the content of the cyclic anion-containing lithium salt to the content of acetonitrile is within the above-mentioned range, the elution of the positive electrode metal by acetonitrile at high temperatures and the physical peeling between the positive electrode Al current collector and the positive electrode active material are effectively suppressed, and the decomposition of the solvent at the negative electrode is suppressed, thereby obtaining excellent high-temperature durability.

[0070] The content of the cyclic anion-containing lithium salt in the electrolyte can be measured using, for example, perfluorobenzene as an internal standard. 19 One example is a method that combines the measurement of the cyclic anion content by F-NMR and the measurement of the lithium ion content by ion chromatography.

[0071] In addition, from the viewpoint of suppressing the decrease in ion conductivity associated with the increase in viscosity of the non-aqueous electrolyte, the molar ratio of the content of the cyclic anion-containing lithium salt to the content of acetonitrile is preferably 5 or less, more preferably 1 or less, more preferably 0.79 or less, more preferably 0.5 or less, and even more preferably 0.27 or less. When the molar ratio of the content of the cyclic anion-containing lithium salt to the content of acetonitrile is within the above-mentioned range, the decrease in ion conductivity at room temperature and low temperature ranges such as low temperatures of -10°C or -40°C can be effectively suppressed, and excellent output characteristics and low temperature characteristics can be obtained.

[0072] The preferred range of the content of the cyclic anion-containing lithium salt represented by formula (1) relative to the content of acetonitrile varies depending on the type of positive electrode active material used in combination.

[0073] In addition, the saturation concentration of the cyclic anion-containing lithium salt represented by formula (1) in acetonitrile is LiPF 6 Since the saturation concentration is higher than that of LiPF 6 From the viewpoint of suppressing association and precipitation of the lithium salt and acetonitrile at low temperatures, it is preferable to use a lithium salt having a molar concentration of LiPF 6 The molar ratio of the content of the cyclic anion-containing lithium salt to the content of LiPF is preferably 3 or more, more preferably greater than 10, more preferably 15 or more, even more preferably 20 or more, and particularly preferably 25 or more. 6 When the molar ratio of the content of the cyclic anion-containing lithium salt to the content of the cyclic anion-containing lithium salt is within the above-mentioned range, the decrease in ionic conductivity at low temperatures such as -10°C or -40°C can be effectively suppressed, and excellent low-temperature characteristics can be obtained.

[0074] In addition, in the electrolyte containing acetonitrile, excess LiPF 6 On the other hand, the cyclic anion-containing lithium salt suppresses the deterioration of battery performance at high temperatures by a mechanism that is presumed to be the above-mentioned effect of suppressing the elution of the positive electrode metal or contribution to the negative electrode SEI. Therefore, LiPF 6 By controlling the molar ratio of the content of the cyclic anion-containing lithium salt to the content of within the above range, it is possible to more effectively improve long-term high-temperature durability.

[0075] In addition, in non-aqueous electrolytes, LiPF 6 The molar ratio of the content of the cyclic anion-containing lithium salt to the content of LiPF is preferably 150 or less. 6 When the molar ratio of the content of the cyclic anion-containing lithium salt to the content of LiPF is within the above-mentioned range, the organic component derived from the cyclic anion-containing lithium salt and the LiPF 6By forming a negative electrode SEI with an excellent balance of inorganic components derived from the lithium ion, it becomes easier to insert and remove lithium ions at room temperature and low temperatures, and the capacity deterioration and resistance increase due to the contraction of the negative electrode SEI at low temperatures are suppressed, thereby improving output performance and low-temperature performance.

[0076] Depending on the type of positive electrode active material used, LiPF 6 The preferred range of the molar ratio of the content of the cyclic anion-containing lithium salt to the content of the cyclic anion-containing lithium salt varies.

[0077] The lithium salt in the present embodiment may further include, in addition to the cyclic anion-containing lithium salt, one or more selected from a lithium-containing imide salt, a fluorine-containing inorganic lithium salt, an organic lithium salt, and other lithium salts.

[0078] The method for measuring the content of the lithium salt in this embodiment is the same as the method for measuring the content of the cyclic anion-containing lithium salt described above.

[0079] (LiPF 6 ) The nonaqueous electrolyte of this embodiment contains LiPF as a lithium salt. 6 The non-aqueous electrolyte solution of this embodiment may further contain LiPF 6 The content of is preferably less than 0.5 mol, more preferably less than 0.1 mol, and even more preferably less than 0.01 mol, per 1 L of the non-aqueous solvent.

[0080] In addition, LiPF in the nonaqueous electrolyte of this embodiment 6 The content is preferably 0.01 millimol or more per 1 L of the non-aqueous solvent.

[0081] LiPF 6It is known that LiPF undergoes thermal decomposition at high temperatures to generate acid components. In particular, this tendency is prominent in a high-temperature environment exceeding 60°C, and even more prominent in a high-temperature environment exceeding 80°C. In addition, this tendency is prominent when the time of exposure to high temperatures is 4 hours or more, more prominent when it is 100 hours or more, more prominent when it is 200 hours or more, more prominent when it is 300 hours or more, and even more prominent when it is 400 hours or more. 6 When the content is within the above range, the LiPF 6 The generation of acid components due to the thermal decomposition reaction of acetonitrile can be suppressed. In addition, hydrogen is removed from the α-position of acetonitrile, which results in the formation of PF 6 The amount of hydrogen fluoride (HF) generated from the anions can also be reduced. If the amount of HF generated in the electrolyte is large, not only will metal components be eluted from the battery components, causing corrosion of the components, but complex cations formed from the eluted metal ions and acetonitrile will be generated, accelerating battery deterioration. In particular, this tendency is prominent in a high-temperature environment exceeding 45°C, more prominent in a high-temperature environment exceeding 60°C, and even more prominent in a high-temperature environment exceeding 80°C. In addition, this tendency is prominent when the time of exposure to high temperatures is 4 hours or more, more prominent when it is 100 hours or more, more prominent when it is 200 hours or more, more prominent when it is 300 hours or more, and even more prominent when it is 400 hours or more. However, LiPF 6 When the content of is within the above range, even if it is exposed to a high temperature exceeding 45°C for more than 4 hours, hydrogen is abstracted from the α-position of acetonitrile to form PF 6 The amount of HF generated from the anions can also be reduced, suppressing the progression of such deterioration, and as a result, the deterioration of battery performance caused by corrosion of the positive electrode active material layer or the positive electrode current collector, or the deterioration reaction of the electrolyte can be kept to a minimum.

[0082] For example, acetonitrile, a lithium-containing imide salt, and LiPF 6Regarding non-aqueous electrolytes containing LiPF 6 In contrast to controlling the content of 0.01 mol / L or more, acetonitrile, a cyclic anion-containing lithium salt represented by formula (1), and LiPF 6 For non-aqueous electrolytes containing LiPF 6 The inventors' investigations have revealed that even when the content of is controlled to less than 0.01 mol / L, corrosion of the aluminum (Al) current collector can be avoided. The mechanism behind this is presumed to be as follows: The cyclic anion-containing lithium salt represented by formula (1) dissociates into lithium ions and cyclic anions in an acetonitrile-containing electrolyte. The cyclic anion electrically interacts with acetonitrile, weakening the metal coordination ability of the nitrile group of acetonitrile. This can suppress metal elution that occurs when acetonitrile forms a complex with the Al ions of the positive electrode current collector at high temperatures.

[0083] LiPF 6 When the content of LiPF is less than 0.01 mol / L, the LiPF 6 This suppresses the generation of acid components due to the thermal decomposition reaction of , and also removes hydrogen from the α-position of acetonitrile, resulting in the formation of PF 6 The amount of HF generated from the anions can also be reduced, and as a result, deterioration of battery performance caused by corrosion of the positive electrode active material layer or the positive electrode current collector, or deterioration reactions of the electrolyte can be kept to a minimum.

[0084] In another embodiment, the nonaqueous electrolyte of the present embodiment contains LiPF as a lithium salt. 6 It is preferable that the lithium salt does not contain LiPF 6 "Containing" refers to the case where the amount is less than 0.01 millimol per liter of the non-aqueous solvent, or where the amount is not detected by the measurement method described above.

[0085] The non-aqueous electrolyte is LiPF 6When the battery does not contain the lithium salt, it can have long-term high-temperature durability even when exposed to high temperatures exceeding 45° C. for 4 hours or more. This is believed to be because the deterioration of battery performance caused by the corrosion of the positive electrode active material layer derived from the lithium salt, the positive electrode current collector, or the deterioration reaction of the electrolyte is minimized.

[0086] (Lithium-containing imide salt) Specific examples of lithium-containing imide salts include LiN(SO 2 F) 2 , and LiN(SO 2 CF 3 ) 2 It is preferable that the composition contains at least one of the following:

[0087] When acetonitrile is included in the non-aqueous solvent, the saturation concentration of the lithium-containing imide salt in acetonitrile is LiPF 6 Since the saturation concentration is higher than that of LiPF 6 It is preferable to contain the lithium-containing imide salt at a molar concentration of ≦lithium-containing imide salt, since it is possible to suppress association and precipitation of the lithium salt and acetonitrile at low temperatures. In addition, it is preferable that the content of the lithium-containing imide salt is 0.5 mol or more and 3.0 mol or less per 1 L of the non-aqueous solvent, from the viewpoint of ensuring the amount of ions supplied to the non-aqueous electrolyte according to this embodiment.

[0088] LiN(SO 2 F) 2 , and LiN(SO 2 CF 3 ) 2 According to the acetonitrile-containing nonaqueous electrolyte solution containing at least one of the above, it is possible to effectively suppress the decrease in ion conductivity in a low temperature range such as −10° C. or −30° C., and obtain excellent low-temperature characteristics. In this embodiment, by limiting the content of the lithium-containing imide salt in this way, it is also possible to more effectively suppress the increase in resistance during high-temperature heating.

[0089] (Fluorine-containing inorganic lithium salt) The lithium salt used in the nonaqueous electrolyte of this embodiment is LiPF 6Other fluorine-containing inorganic lithium salts may be included, for example, LiBF 4 , LiAsF 6 , Li 2 SiF 6 , LiSbF 6 , Li 2 B 12 F b H 12-b [wherein b is an integer of 0 to 3]. Here, "inorganic lithium salt" refers to a lithium salt that does not contain a carbon atom in the anion and is soluble in acetonitrile. Also, "fluorine-containing inorganic lithium salt" refers to a lithium salt that does not contain a carbon atom in the anion and contains a fluorine atom in the anion and is soluble in acetonitrile. Fluorine-containing inorganic lithium salts are excellent in that they form a passive film on the surface of the aluminum foil that is the positive electrode current collector, and suppress corrosion of the positive electrode current collector. These fluorine-containing inorganic lithium salts are used alone or in combination of two or more. As the fluorine-containing inorganic lithium salt, a compound that is a double salt of LiF and a Lewis acid is preferred, and among them, it is more preferred to use a fluorine-containing inorganic lithium salt having a phosphorus atom, since it is easy to release free fluorine atoms. When a fluorine-containing inorganic lithium salt having a boron atom is used as the fluorine-containing inorganic lithium salt, it is preferred because it is easy to capture excess free acid components that may cause battery deterioration, and from this viewpoint, LiBF 4 is particularly preferred.

[0090] The content of the fluorine-containing inorganic lithium salt in the lithium salt used in the non-aqueous electrolyte of this embodiment is preferably 0.01 mol or more, more preferably 0.1 mol or more, and even more preferably 0.25 mol or more, relative to 1 L of the non-aqueous solvent. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range, the ion conductivity increases, and there is a tendency for high-output characteristics to be exhibited. In addition, this content is preferably less than 2.8 mol, more preferably less than 1.5 mol, and even more preferably less than 1 mol, relative to 1 L of the non-aqueous solvent. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range, there is a tendency for the ion conductivity to increase, high-output characteristics to be exhibited, and the decrease in ion conductivity associated with an increase in viscosity at low temperatures to be suppressed, and there is a tendency for the high-temperature cycle characteristics and other battery characteristics to be further improved while maintaining the excellent performance of the non-aqueous electrolyte.

[0091] (Organic Lithium Salts) The lithium salt in this embodiment may include an organic lithium salt. The term "organic lithium salt" refers to a lithium salt other than a lithium-containing imide salt that contains a carbon atom in the anion and is soluble in acetonitrile.

[0092] As the organic lithium salt, an organic lithium salt having an oxalic acid group can be mentioned. A specific example of the organic lithium salt having an oxalic acid group is LiB(C 2 O 4 ) 2 , LiBF 2 (C 2 O 4 ), LiPF 4 (C 2 O 4 ), and LiPF 2 (C 2 O 4 ) 2 Among them, LiB(C 2 O 4 ) 2 and LiBF 2 (C 2 O 4It is preferable to use at least one lithium salt selected from the lithium salts represented by the formula (I) and (II). It is more preferable to use one or more of these together with a fluorine-containing inorganic lithium salt. This organic lithium salt having an oxalic acid group may be added to a non-aqueous electrolyte solution or may be contained in a negative electrode (negative electrode active material layer).

[0093] In the present embodiment, the amount of the organic lithium salt added to the non-aqueous electrolyte is preferably 0.005 mol or more, more preferably 0.01 mol or more, even more preferably 0.02 mol or more, and particularly preferably 0.05 mol or more, per 1 L of non-aqueous solvent, in order to better ensure the effect of its use. However, if the amount of the organic lithium salt having an oxalic acid group in the non-aqueous electrolyte is too large, it may precipitate. Therefore, the amount of the organic lithium salt having an oxalic acid group added to the non-aqueous electrolyte is preferably less than 1.0 mol, more preferably less than 0.5 mol, and even more preferably less than 0.2 mol, per 1 L of non-aqueous solvent.

[0094] It is known that the organic lithium salt having an oxalic acid group is poorly soluble in organic solvents with low polarity, particularly in chain carbonates. The content of the organic lithium salt in the non-aqueous electrolyte according to this embodiment may be, for example, 0.01 mol or more and 0.5 mol or less per 1 L of non-aqueous solvent.

[0095] In addition, the organic lithium salt having an oxalic acid group may contain a small amount of lithium oxalate, and when mixed as a non-aqueous electrolyte solution, it may react with a small amount of water contained in other raw materials to generate new white precipitation of lithium oxalate. Therefore, it is preferable to suppress the content of lithium oxalate in the non-aqueous electrolyte solution according to this embodiment to a range of 500 ppm or less.

[0096] (Other lithium salts) The lithium salt in the present embodiment may contain other lithium salts in addition to those mentioned above.

[0097] Other specific examples of lithium salts include, for example, LiClO 4 , LiAlO 4 , LiAlCl 4 , LiB 10 Cl 10 , chloroborane Li, and other inorganic lithium salts that do not contain a fluorine atom in the anion; LiCF 3 SO 3 , LiCF 3 CO 2 , Li 2 C 2 F 4 (SO 3 ) 2 , LiC(CF 3 SO 2 ) 3 , LiCnF (2n+1) SO 3 {where n≧2}, lower aliphatic carboxylic acid Li, tetraphenylborate Li, LiB(C 3 O 4 H 2 ) 2 etc. organic lithium salts; LiPF 5 (CF 3 ) and other LiPFs n (C p F 2p+1 ) 6-n

[0033] (wherein n is an integer of 1 to 5, and p is an integer of 1 to 8); LiBF 3 (CF 3 ) and other LiBFs q (C s F 2s+1 ) 4-q (wherein q is an integer of 1 to 3, and s is an integer of 1 to 8); Lithium salts combined with multivalent anions; The following formula (XXa): LiC(SO 2 R jj )(SO 2 R kk )(SO 2 R ll ) (XXa) {where, R jj, R kk , and R ll may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms. The following formula (XXb): LiN(SO 2 OR mm )(SO 2 OR nn ) (XXb) {where, R mm , and R nn may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.}, and The following formula (XXc): LiN(SO 2 R oo )(SO 2 OR pp ) (XXc) {where, R oo , and R pp may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.} One or more of these can be used together with the fluorine-containing inorganic lithium salt.

[0098] The amount of the other lithium salt added to the non-aqueous electrolyte solution may be appropriately set within the range of, for example, 0.01 mol or more and 0.5 mol or less per 1 L of the non-aqueous solvent.

[0099] <2-3. Additives for electrode protection> The non-aqueous electrolyte according to the present embodiment may contain an additive for protecting the electrodes (electrode protection additive). The electrode protection additive may substantially overlap with a substance that serves as a solvent for dissolving the lithium salt (i.e., the above-mentioned non-aqueous solvent). The electrode protection additive is preferably a substance that contributes to improving the performance of the non-aqueous electrolyte and the non-aqueous secondary battery, but also includes a substance that is not directly involved in the electrochemical reaction.

[0100] Specific examples of the electrode protection additive include, for example, Fluoroethylene carbonates represented by 4-fluoro-1,3-dioxolan-2-one, 4,4-difluoro-1,3-dioxolan-2-one, cis-4,5-difluoro-1,3-dioxolan-2-one, trans-4,5-difluoro-1,3-dioxolan-2-one, 4,4,5-trifluoro-1,3-dioxolan-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolan-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolan-2-one; unsaturated bond-containing cyclic carbonates, such as vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinylethylene carbonate; Lactones represented by γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone; Cyclic ethers, such as 1,4-dioxane; Cyclic sulfur compounds represented by ethylene sulfite, propylene sulfite, butylene sulfite, pentene sulfite, sulfolane, 3-sulfolene, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propene 1,3-sultone, and tetramethylene sulfoxide; These may be used alone or in combination of two or more.

[0101] The content of the electrode protection additive in the nonaqueous electrolyte solution is preferably 0.1 to 30 volume %, more preferably 0.3 to 15 volume %, even more preferably 0.4 to 8 volume %, and particularly preferably 0.5 to 4 volume %, relative to the total amount of the nonaqueous solvent.

[0102] In this embodiment, the greater the content of the electrode protection additive, the more the deterioration of the non-aqueous electrolyte solution is suppressed. However, the smaller the content of the electrode protection additive, the more the high-output characteristics of the non-aqueous secondary battery in a low-temperature environment are improved. Therefore, by adjusting the content of the electrode protection additive within the above range, it is possible to exhibit excellent performance based on the high ionic conductivity of the electrolyte solution without impairing the basic function of the non-aqueous secondary battery, and by preparing the non-aqueous electrolyte solution with such a composition, it is possible to further improve the cycle performance of the non-aqueous secondary battery, the high-output performance in a low-temperature environment, and other battery characteristics.

[0103] Acetonitrile is easily electrochemically decomposed by reduction. Therefore, the non-aqueous solvent containing acetonitrile preferably contains one or more cyclic aprotic polar solvents, more preferably one or more unsaturated bond-containing cyclic carbonates, as an electrode protection additive for forming a protective film on the negative electrode.

[0104] As the unsaturated bond-containing cyclic carbonate, vinylene carbonate is preferred, and the content of vinylene carbonate in the non-aqueous electrolyte is preferably 0.1% by volume or more and 4% by volume or less, more preferably 0.2% by volume or more and less than 3% by volume, and even more preferably 0.5% by volume or more and less than 2.5% by volume. This makes it possible to more effectively improve low-temperature durability and provide a secondary battery with excellent low-temperature performance.

[0105] Vinylene carbonate as an additive for electrode protection suppresses the reductive decomposition reaction of acetonitrile on the surface of the negative electrode, while excessive film formation leads to a decrease in low-temperature performance. Therefore, by adjusting the amount of vinylene carbonate added within the above range, the interface (film) resistance can be kept low, and cycle deterioration at low temperatures can be suppressed.

[0106] (acid anhydride) The non-aqueous secondary battery according to this embodiment is stabilized by forming an SEI on the negative electrode surface as a result of a part of the non-aqueous electrolyte being decomposed during the initial charge. In order to more effectively strengthen this SEI, an acid anhydride can be added to the non-aqueous electrolyte, the battery material, or the non-aqueous secondary battery. When acetonitrile is included as the non-aqueous solvent, the strength of the SEI tends to decrease with increasing temperature, but the addition of an acid anhydride promotes the strengthening of the SEI. Therefore, by using such an acid anhydride, it is possible to effectively suppress the increase in internal resistance over time due to thermal history.

[0107] Specific examples of acid anhydrides include chain acid anhydrides such as acetic anhydride, propionic anhydride, and benzoic anhydride; cyclic acid anhydrides such as malonic anhydride, succinic anhydride, glutaric anhydride, maleic anhydride, phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, 2,3-naphthalene dicarboxylic anhydride, and naphthalene-1,4,5,8-tetracarboxylic dianhydride; and mixed acid anhydrides having a structure in which different types of acids, such as two different types of carboxylic acids or a carboxylic acid and a sulfonic acid, are dehydrated and condensed. These may be used alone or in combination of two or more types.

[0108] Since it is preferable that the non-aqueous secondary battery according to this embodiment strengthens the SEI before the reductive decomposition of the non-aqueous solvent, it is preferable that the acid anhydride contains at least one cyclic acid anhydride that acts early during the first charge. These cyclic acid anhydrides may contain only one type or multiple types. Or, it may contain a cyclic acid anhydride other than these cyclic acid anhydrides. In addition, it is preferable that the cyclic acid anhydride contains at least one type of succinic anhydride, maleic anhydride, and phthalic anhydride.

[0109] A non-aqueous electrolyte solution containing at least one of succinic anhydride, maleic anhydride, and phthalic anhydride can form a strong SEI on the negative electrode and more effectively suppress the increase in resistance during high-temperature heating. In particular, it is preferable to contain succinic anhydride. This makes it possible to more effectively form a strong SEI on the negative electrode while suppressing side reactions.

[0110] When the nonaqueous electrolyte solution according to the present embodiment contains an acid anhydride, the content thereof is preferably in the range of 0.01 parts by mass or more and 10 parts by mass or less, more preferably 0.05 parts by mass or more and 1 part by mass or less, and even more preferably 0.1 parts by mass or more and 0.5 parts by mass or less, per 100 parts by mass of the nonaqueous electrolyte solution.

[0111] The acid anhydride is preferably contained in the non-aqueous electrolyte. On the other hand, since it is sufficient that the acid anhydride can act in the non-aqueous secondary battery, at least one battery member selected from the group consisting of the positive electrode, the negative electrode, and the separator may contain the acid anhydride. As a method for containing the acid anhydride in the battery member, for example, the acid anhydride may be contained in the battery member during the preparation of the battery member, or the acid anhydride may be impregnated into the battery member by a post-treatment represented by coating, immersion, or spray drying of the battery member.

[0112] (Nitrogen-containing cyclic compound) The electrolyte solution according to the present embodiment contains, in addition to a non-aqueous solvent and a lithium salt, an additive represented by the following formula (2): [ka] {where, R 1 , R 2 , and R 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a fluorine-substituted alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a fluorine-substituted alkoxy group having 1 to 4 carbon atoms, a phenyl group, a cyclohexyl group, a nitrile group, a nitro group, an amino group, an N,N'-dimethylamino group, or an N,N'-diethylamino group, and two or more of these substituents are hydrogen atoms. The compound may further contain a compound represented by the following formula (nitrogen-containing cyclic compound):

[0113] In this embodiment, it has been found that by using acetonitrile as a nonaqueous solvent, a cyclic anion-containing lithium salt represented by the above formula (1) as a lithium salt, and a nitrogen-containing cyclic compound represented by the above formula (2) in combination, the durability of a nonaqueous electrolyte or a nonaqueous secondary battery can be improved in a high temperature environment, for example, at 85°C, 90°C, or above 90°C.

[0114] Specific examples of the nitrogen-containing cyclic compound include pyridine, 2-methylpyridine, 3-methylpyridine, 4-methylpyridine, 2-ethylpyridine, 3-ethylpyridine, 4-ethylpyridine, 2-(n-propyl)pyridine, 3-(n-propyl)pyridine, 4-(n-propyl)pyridine, 2-isopropylpyridine, 3-isopropylpyridine, 4-isopropylpyridine, 2-(n-butyl)pyridine, 3-(n-butyl)pyridine, 4-(n-butyl)pyridine, 2-(1-methylpropyl)pyridine, 3-(1-methylpropyl)pyridine, )pyridine, 4-(1-methylpropyl)pyridine, 2-(2-methylpropyl)pyridine, 3-(2-methylpropyl)pyridine, 4-(2-methylpropyl)pyridine, 2-(tert-butyl)pyridine, 3-(tert-butyl)pyridine, 4-(tert-butyl)pyridine, 2-trifluoromethylpyridine, 3-trifluoromethylpyridine, 4-trifluoromethylpyridine, 2-(2,2,2-trifluoroethyl)pyridine, 3-(2,2,2-trifluoroethyl)pyridine, 4-(2,2,2-trifluoroethyl )pyridine, 2-(pentafluoroethyl)pyridine, 3-(pentafluoroethyl)pyridine, 4-(pentafluoroethyl)pyridine, 2-methoxypyridine, 3-methoxypyridine, 4-methoxypyridine, 2-ethoxypyridine, 3-ethoxypyridine, 4-ethoxypyridine, 2-(n-propoxy)pyridine, 3-(n-propoxy)pyridine, 4-(n-propoxy)pyridine, 2-isopropoxypyridine, 3-isopropoxypyridine, 4-isopropoxypyridine, 2-(n-butoxy)pyridine, 3-(n-butoxy )pyridine, 4-(n-butoxy)pyridine, 2-(1-methylpropoxy)pyridine, 3-(1-methylpropoxy)pyridine, 4-(1-methylpropoxy)pyridine, 2-(2-methylpropoxy)pyridine, 3-(2-methylpropoxy)pyridine, 4-(2-methylpropoxy)pyridine, 2-trifluoromethoxypyridine, 3-trifluoromethoxypyridine, 4-trifluoromethoxypyridine, 2-(2,2,2-trifluoroethoxy)pyridine, 3-(2,2,2-trifluoroethoxy)pyridine, 4-(2,2,2-trifluoroethoxy)pyridine, 2-phenylpyridine, 3-phenylpyridine, 4-phenylpyridine, 2-cyclohexylpyridine, 3-cyclohexylpyridine, 4-cyclohexylpyridine, 2-cyanopyridine, 3-cyanopyridine, 4-cyanopyridine, 2-aminopyridine, 3-aminopyridine, 4-aminopyridine, 2-(N,N'-dimethylamino)pyridine, 3-(N,N'-dimethylamino)pyridine, 4-(N,N'-dimethylamino)pyridine, 2-(N,N'-diethylamino)pyridine, 3-(N,N'-diethylamino)pyridine, and 4-(N,N'-diethylamino)pyridine. These may be used alone or in combination of two or more. Among these, from the viewpoint of further improving the high-temperature durability of the nonaqueous electrolyte or the nonaqueous secondary battery, the nitrogen-containing cyclic compound is preferably one or more compounds selected from the group consisting of pyridine and 4-(tert-butyl)pyridine.

[0115] When a compound that is a double salt of LiF and a Lewis acid is used as the fluorine-containing inorganic lithium salt, it is desirable that there is no steric hindrance around the nitrogen atom in the nitrogen-containing cyclic compound. 1 is preferably a hydrogen atom, and R 1 and R 2 It is more preferable that both of R in the above formula (2) are hydrogen atoms. 1 and R 2 When both are hydrogen atoms, in view of the electronic effect on the unshared electron pair present on the nitrogen atom, R in the above formula (2) 3is particularly preferably a hydrogen atom or a tert-butyl group. The electrolyte solution of this embodiment contains the nitrogen-containing cyclic compound represented by the above formula (2) as an additive, and in the non-aqueous electrolyte solution containing acetonitrile and a fluorine-containing inorganic lithium salt, which has an excellent balance between viscosity and relative dielectric constant, the generation of a complex cation consisting of a transition metal and acetonitrile is suppressed, excellent load characteristics are exhibited, and self-discharge during high-temperature storage can be suppressed. The content of the nitrogen-containing cyclic compound in the electrolyte solution of this embodiment is not particularly limited, but is preferably 0.01 to 10 mass%, more preferably 0.02 to 5 mass%, and even more preferably 0.05 to 3 mass%, based on the total amount of the electrolyte solution.

[0116] In the non-aqueous electrolyte, the content of the nitrogen-containing cyclic compound represented by the above formula (2) relative to the content of the cyclic anion-containing lithium salt represented by the above formula (1) is preferably 0.0001 or more and 3 or less in molar ratio. From the viewpoint of maximizing the effects of both compounds, that is, weakening the coordination ability of the nitrile group of acetonitrile by the effect of the cyclic anion-containing lithium salt, while suppressing the generation of a complex cation consisting of a transition metal and acetonitrile by the effect of the nitrogen-containing cyclic compound represented by the above formula (2), for example, a pyridine-based compound, in the non-aqueous electrolyte, the content of the nitrogen-containing cyclic compound represented by the above formula (2) relative to the content of the cyclic anion-containing lithium salt represented by the formula (1) is preferably 0.0001 or more in molar ratio, more preferably 0.001 or more, and even more preferably 0.01 or more, and this molar ratio is preferably 3 or less, more preferably 1 or less, and even more preferably 0.1 or less. When this molar ratio is in the above range, deterioration of the negative electrode SEI due to reduction precipitation of the metal complex at the negative electrode is suppressed, and long-term high-temperature durability is improved.

[0117] The content of the nitrogen-containing cyclic compound represented by formula (2) is preferably 0.01% by mass or more and 10% by mass or less, more preferably 0.02% by mass or more and 5% by mass or less, and even more preferably 0.05% by mass or more and 1% by mass or less, based on the total amount of the non-aqueous electrolyte. From the viewpoint of the long-term high-temperature durability of the non-aqueous electrolyte or the non-aqueous secondary battery, the nitrogen-containing cyclic compound represented by formula (2) is preferably contained in an amount of 0.01% by mass or more based on the total amount of the non-aqueous electrolyte. From the viewpoint of the output performance of the non-aqueous secondary battery in a low-temperature environment, the nitrogen-containing cyclic compound represented by formula (2) is preferably contained in an amount of 10% by mass or less based on the total amount of the non-aqueous electrolyte.

[0118] In this embodiment, by adjusting the content of the nitrogen-containing cyclic compound within the above-mentioned range, the reaction on the electrode surface can be suppressed without impairing the basic functions of the nonaqueous secondary battery, and therefore the increase in internal resistance accompanying charging and discharging can be reduced.

[0119] In addition, by preparing an electrolyte solution having the above-mentioned composition, the cycle performance of the nonaqueous secondary battery, high output performance in a low temperature environment, and all of the other battery characteristics tend to be further improved.

[0120] (Silane compounds) The electrolyte solution according to this embodiment contains, in addition to a non-aqueous solvent and a lithium salt, an additive represented by the following general formula (3): X-Si(OR 3 ) (3-m) R 4 m ...(3) {where, R 3 and R 4 represents an alkyl group which may be substituted with an aryl group, an alkoxysilyl group, or a halogen atom, or an aryl group which may be substituted with an alkyl group, an alkoxysilyl group, or a halogen atom, and X represents a group represented by the following formula (L1): [ka] (wherein k is an integer of 0 to 8, and * indicates the bonding site with Si), The following formula (L2): [ka] (wherein j is an integer of 0 to 8, and * indicates the bonding site with Si), The following formula (L3): [ka] (wherein h is an integer of 0 to 8, g is an integer of 0 or 1, and * indicates the bonding site to Si), and The following formula (L4): [ka] (In the formula, * indicates the bond site with Si) and m is an integer of 0 to 2}; The following general formula (4): [ka] {wherein each X independently represents at least one selected from the group consisting of groups represented by formulas (L1) to (L4), and d represents an integer of 0 to 10,000.} The following general formula (5): [ka] {where, R 5 each independently represents an aryl group or an alkyl group which may be substituted with a halogen atom, or an aryl group which may be substituted with an alkyl group or a halogen atom, y is an integer of 2 to 8, and X represents at least one selected from the group consisting of the groups represented by the formulas (L1) to (L4). The following general formula (6): X-Si(OR 3 'OR 3 ) (3-m) R 4 m ...(6) {where, R3 , R 4 , X, and m are as defined in general formula (3), and R 3 ' is an aryl group, an alkoxysilyl group, or an alkylene group which may be substituted with a halogen atom; The following formula (7): [ka] A compound represented by the formula (7): {in which R is each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 5 to 20 carbon atoms; X is O, S, or NH; Z is P, P=O, B, or Si; when Z is P or P=O, n1 is 1, n2 is an integer of 1 to 3, and n2+n3=3; when Z is B, n1 is 1, n2 is an integer of 1 to 3, and n2+n3=3; when Z is Si, n1 is 0, n2 is an integer of 1 to 4, and n2+n3=4.}, and The following formula (8): [ka] {R in formula (8) has the same meaning as R in formula (7).}, and at least one silane compound selected from the group consisting of diphenyldialkoxysilanes.

[0121] In this embodiment, it has been found that by using acetonitrile as a nonaqueous solvent, a cyclic anion-containing lithium salt represented by the above formula (1) as a lithium salt, and the above silane-based compound in combination, the durability of a nonaqueous electrolyte or a nonaqueous secondary battery can be improved in a high-temperature environment, for example, at 85°C, 90°C, or above 90°C.

[0122] The compounds represented by the general formulas (3) to (8) and diphenyldialkoxysilane have the effect of suppressing active sites (active sites of the positive electrode active material) that cause oxidative deterioration of the nonaqueous electrolyte. By using such compounds, it is possible to provide a nonaqueous electrolyte and a nonaqueous secondary battery that exhibit excellent load characteristics and can suppress various deterioration phenomena that occur when stored at high temperatures or when charging and discharging cycles are repeated. In addition, the hydrogen fluoride (HF) trapping effect of the diphenyldialkoxysilane suppresses deterioration of the positive electrode active material with a high nickel (Ni) ratio, and LiPF 6 PF included in 5 It is also possible to suppress the decomposition of the acetonitrile solvent, which reduces the Lewis acid catalytic activity of the catalyst and contributes to high ionic conductivity.

[0123] Specific examples of the compounds represented by the general formulas (3) to (6) include triethoxyvinylsilane, allyltriethoxysilane, triethoxy(3-glycidyloxypropyl)silane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, allyltris(trimethylsilyloxy)silane, 1,3-divinyltetramethyldisiloxane, 1,1,1,3,5,5,5-heptamethyl-3-(3-glycidyloxypropyl)trisiloxane, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisiloxane, allyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, [8-( glycidyloxy)-n-octyl]trimethoxysilane, trimethoxy(4-vinylphenyl)silane, trimethoxy(7-octen-1-yl)silane, vinyltrimethoxysilane, vinyltris(2-methoxyethoxy)silane, diethoxymethylvinylsilane, diethoxy(3-glycidyloxypropyl)methylsilane, dimethoxymethylvinylsilane, 3-glycidyloxypropyl(dimethoxy)methylsilane, vinyl group-terminated dimethylpolysiloxane, allyl group-terminated dimethylpolysiloxane, epoxy group-terminated dimethylpolysiloxane, glycidyl group-terminated dimethylpolysiloxane, cycloepoxy group-terminated dimethylpolysiloxane, alkylcycloepoxy group-terminated dimethylpolysiloxane, and the like.

[0124] R in the above formula (7) is preferably a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, more preferably an unsubstituted alkyl group having 1 to 20 carbon atoms, or an alkyl group having 1 to 20 carbon atoms substituted with a halogen atom, still more preferably an alkyl group having 1 to 6 or 1 to 4 carbon atoms, or a fluoroalkyl group having 1 to 6 or 1 to 4 carbon atoms, and particularly preferably a methyl group or a 2,2,2-trifluoroethyl group. X is preferably an oxygen atom.

[0125] Specific examples of the compound in which Z is P in the above formula (7) include mono(trimethylsilyl) phosphite, tris(trimethylsilyl) phosphite, and tris(2,2,2-trifluoroethyl) phosphite. A specific example of the compound where Z is P=O is tris(trimethylsilyl) phosphate. Specific examples of the compound in which Z is B include tris(trimethylsilyl)borate and tris(2,2,2-trifluoroethylsilyl)borate. A specific example of the compound in which Z is Si is tris(trimethylsilyl)silane.

[0126] A specific example of a polymer compound containing a repeating unit represented by the above formula (8) is polytrimethylsilyl phosphate.

[0127] Diphenyldialkoxysilane can act as an additive for protecting electrodes when a non-aqueous electrolyte is used in a non-aqueous secondary battery. Specific examples of diphenyldialkoxysilane include diphenyldimethoxysilane, diphenyldiethoxysilane, diphenyldipropoxysilane, and diphenyldibutoxysilane. These are used alone or in combination of two or more. Among them, diphenyldimethoxysilane, which has the smallest molecular weight, is more preferable because it increases the number of moles per unit weight.

[0128] These may be used alone or in combination of two or more. Among the silane-based compounds listed above, from the viewpoint of further improving the high-temperature durability of the nonaqueous electrolyte or nonaqueous secondary battery, the compound represented by the above formula (3), tris(trimethylsilyl) phosphate, tris(trimethylsilyl) phosphite, tris(2,2,2-trifluoroethyl) phosphite, and diphenyldialkoxysilane are preferred, and triethoxyvinylsilane and diphenyldimethoxysilane are more preferred.

[0129] In the non-aqueous electrolyte, the content of the silane-based compound relative to the content of the cyclic anion-containing lithium salt represented by formula (1) is preferably 0.0001 or more and 1.5 or less in molar ratio. From the viewpoint of maximizing the effects of both compounds, that is, weakening the coordination ability of the nitrile group of acetonitrile by the effect of the cyclic anion-containing lithium salt, while suppressing the active site (active site of the positive electrode active material) that oxidizes and deteriorates the non-aqueous electrolyte by the effect of the silane-based compound, in the non-aqueous electrolyte, the content of the silane-based compound relative to the content of the cyclic anion-containing lithium salt represented by formula (1) is preferably 0.0001 or more in molar ratio, more preferably 0.001 or more, and even more preferably 0.01 or more, and this molar ratio is preferably 1.5 or less, more preferably 0.5 or less, and even more preferably 0.1 or less. When the molar ratio of the content of the silane-based compound to the content of the cyclic anion-containing lithium salt represented by formula (1) is within the above-mentioned range, deterioration of the negative electrode SEI due to reductive precipitation of the metal complex at the negative electrode is suppressed, and long-term high-temperature durability is improved.

[0130] The content of the silane compound selected from the group consisting of the compounds represented by the general formulas (3) to (8) and diphenyldialkoxysilane is preferably 0.01% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, and even more preferably 0.075% by mass to 3% by mass, based on the total amount of the nonaqueous electrolyte (i.e., 100% by mass of the nonaqueous electrolyte). By being in this range, it is possible to effectively suppress active sites of the positive electrode active material that cause oxidative deterioration of the nonaqueous electrolyte while keeping the internal resistance of the nonaqueous secondary battery low.

[0131] <2-4. Other optional additives> In this embodiment, for the purpose of improving the charge / discharge cycle characteristics, high-temperature storage property, and safety (e.g., prevention of overcharging) of the nonaqueous secondary battery, optional additives (additives other than the acid anhydride and the additive for protecting the electrodes) may be appropriately contained in the nonaqueous electrolyte solution.

[0132] Optional additives include, for example, sulfonic acid esters, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, phosphate esters [ethyl diethyl phosphonoacetate (EDPA); (C 2 H 5 O) 2 (P=O)-CH 2 (C=O)OC 2 H 5 , tris(trifluoroethyl) phosphate (TFEP); (CF 3 CH 2 O) 3 P=O, triphenyl phosphate (TPP); (C 6 H 5 O) 3 P=O, triaryl phosphate; (CH 2 =CHCH 2 O) 3 In particular, phosphoric acid esters have the effect of suppressing side reactions during storage, and are effective as optional additives.

[0133] When the non-aqueous electrolyte according to the present embodiment contains other optional additives, the content of the additives is preferably in the range of 0.01% by mass to 10% by mass, more preferably 0.02% by mass to 5% by mass, and even more preferably 0.05 to 3% by mass, based on the total amount of the non-aqueous electrolyte. By adjusting the content of the other optional additives within the above range, there is a tendency that it is possible to add even better battery characteristics without impairing the basic functions of the non-aqueous secondary battery.

[0134] <3.Non-aqueous secondary battery> The nonaqueous electrolyte solution of the present embodiment can be used in a nonaqueous secondary battery. The nonaqueous secondary battery according to this embodiment is not particularly limited, but is configured by housing a positive electrode, a negative electrode, a separator, and a nonaqueous electrolyte solution in a suitable battery exterior.

[0135] Specifically, the nonaqueous secondary battery according to this embodiment may be a nonaqueous secondary battery 100 shown in Figures 1 and 2. Here, Figure 1 is a plan view that shows a schematic diagram of the nonaqueous secondary battery, and Figure 2 is a cross-sectional view taken along line AA in Figure 1.

[0136] The nonaqueous secondary battery 100 shown in FIG. 1 and FIG. 2 is composed of a pouch-type cell. The nonaqueous secondary battery 100 accommodates a laminated electrode body formed by laminating a positive electrode 150 and a negative electrode 160 with a separator 170 interposed therebetween, and a nonaqueous electrolyte (not shown) in a space 120 of a battery exterior 110. The battery exterior 110 is composed of, for example, an aluminum laminate film, and is sealed by heat-sealing the upper and lower films at the outer periphery of the space formed by the two aluminum laminate films. The laminate formed by laminating the positive electrode 150, the separator 170, and the negative electrode 160 in this order is impregnated with a nonaqueous electrolyte. However, in FIG. 2, in order to avoid the drawing becoming complicated, the layers constituting the battery exterior 110 and the layers of the positive electrode 150 and the negative electrode 160 are not shown separately.

[0137] The aluminum laminate film constituting the battery exterior 110 is preferably made of aluminum foil coated on both sides with a polyolefin resin.

[0138] The positive electrode 150 is connected to the positive electrode lead body 130 within the nonaqueous secondary battery 100. Although not shown, the negative electrode 160 is also connected to the negative electrode lead body 140 within the nonaqueous secondary battery 100. One end of each of the positive electrode lead body 130 and the negative electrode lead body 140 is drawn out to the outside of the battery exterior 110 so that they can be connected to an external device, and the ionomer portions of these are heat-fused to one side of the battery exterior 110.

[0139] 1 and 2, the positive electrode 150 and the negative electrode 160 each have one laminated electrode body, but the number of laminated positive electrodes 150 and negative electrodes 160 can be appropriately increased depending on the capacity design. In the case of a laminated electrode body having a plurality of positive electrodes 150 and negative electrodes 160, the tabs of the same electrode may be joined by welding or the like and then joined to a single lead body by welding or the like and taken out of the battery. The tabs of the same electrode may be formed from an exposed portion of a current collector, or may be formed by welding a metal piece to the exposed portion of a current collector, or the like.

[0140] The positive electrode 150 is composed of a positive electrode current collector and a positive electrode active material layer, and the negative electrode 160 is composed of a negative electrode current collector and a negative electrode active material layer.

[0141] The positive electrode active material layer contains a positive electrode active material, and the negative electrode active material layer contains a negative electrode active material.

[0142] The positive electrode 150 and the negative electrode 160 are arranged such that the positive electrode active material layer and the negative electrode active material layer face each other with the separator 170 interposed therebetween. Hereinafter, each element constituting the nonaqueous secondary battery according to this embodiment will be described in order.

[0143] <4. Positive electrode> The positive electrode 150 is composed of a positive electrode active material layer made of a positive electrode mixture, and a positive electrode current collector. The positive electrode mixture contains a positive electrode active material, and optionally contains a conductive assistant and a binder.

[0144] The positive electrode active material layer contains a material capable of absorbing and releasing lithium ions as a positive electrode active material, which can provide a high voltage and a high energy density.

[0145] The positive electrode active material may be, for example, a positive electrode active material containing at least one transition metal element selected from the group consisting of Ni, Mn, and Co, and may be represented by the following general formula (a t ): Li p Ni q Co r Mns M t O u ·····(a t ) {Wherein, M is at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba, and 0 < p < 1.3, 0 < q < 1.2, 0 < r < 1.2, 0 ≦ s < 0.5, 0 ≦ t < 0.3, 0.7 ≦ q + r + s + t ≦ 1.2, 1.8 < u < 2.2, and p is a value determined by the charge and discharge state of the battery.} At least one Li-containing metal oxide selected from lithium (Li)-containing metal oxides represented by the formula is preferable.

[0146] Specific examples of the positive electrode active material include, for example, lithium cobalt oxide represented by LiCoO 2 ; lithium manganese oxide represented by LiMnO 2 , LiMn 2 O 4 , and Li 2 Mn 2 O 4 ; lithium nickel oxide represented by LiNiO 2 ; lithium-containing composite metal oxides represented by LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , LiNi 0.5 Co 0.2 Mn 0.3 O 2 , LiNi 0.8 Co 0.2 O 2 ; Li z MO 2 (wherein, M represents two or more metal elements selected from the group consisting of Ni, Mn, Al, and Mg, and z represents a number greater than 0.9 and less than 1.2), and the like.

[0147] In particular, the general formula (a t) When the Ni content ratio q of the Li-containing metal oxide represented by is 0.5 < q < 1.2, it is preferable because both the reduction in the amount of the rare metal Co used and the increase in the high energy density can be achieved. As such a positive electrode active material, for example, LiNi 0.6 Co 0.2 Mn 0.2 O 2 , LiNi 0.75 Co 0.15 Mn 0.15 O 2 , LiNi 0.8 Co 0.1 Mn 0.1 O 2 , LiNi 0.85 Co 0.075 Mn 0.075 O 2 , LiNi 0.8 Co 0.15 Al 0.05 O 2 , LiNi 0.81 Co 0.1 Al 0.09 O 2 , LiNi 0.85 Co 0.1 Al 0.05 O 2 , and lithium-containing composite metal oxides typified by the like can be mentioned.

[0148] On the other hand, as the Ni content ratio of the Li-containing metal oxide increases, deterioration tends to progress at a low voltage. In the layered rock salt type positive electrode active material represented by the general formula (a t ), active points that oxidatively deteriorate the electrolytic solution essentially exist. These active points may consume the electrode protection additive unintentionally.

[0149] In addition, these additive decomposition products incorporated and deposited on the positive electrode side not only become a factor for increasing the internal resistance of the non-aqueous secondary battery, but also accelerate the deterioration of the lithium salt. In particular, when LiPF 6 is included as the lithium salt, it is considered that HF is generated due to deterioration and the elution of transition metals is promoted. In a non-aqueous electrolytic solution containing acetonitrile as the non-aqueous solvent, a complex of a metal cation and acetonitrile is formed, and the deterioration of the battery is accelerated.

[0150] Furthermore, the deterioration of the electrode protection additive or lithium salt makes the protection of the negative electrode surface, which was the original purpose, insufficient. In particular, in a non-aqueous electrolyte solution containing acetonitrile as a non-aqueous solvent, if the protection of the negative electrode surface is insufficient, the reductive decomposition of acetonitrile proceeds, and the battery performance rapidly deteriorates, which is a fatal problem.

[0151] In order to deactivate the active sites that essentially cause the oxidation deterioration of the non-aqueous electrolyte, it is important to control the Jahn-Teller distortion or to have a component that acts as a neutralizer. Therefore, it is preferable that the positive electrode active material contains at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba.

[0152] For the same reason, it is preferable that the surface of the positive electrode active material is coated with a compound containing at least one metal element selected from the group consisting of Zr, Ti, Al, and Nb. It is more preferable that the surface of the positive electrode active material is coated with an oxide containing at least one metal element selected from the group consisting of Zr, Ti, Al, and Nb. Furthermore, it is preferable that the surface of the positive electrode active material is coated with an oxide containing at least one metal element selected from the group consisting of ZrO 2 , TiO 2 , Al 2 O 3 , NbO 3 , and LiNbO 2 It is particularly preferable that the carbon nanotube is coated with at least one oxide selected from the group consisting of the following, since this does not inhibit the permeation of lithium ions.

[0153] The above general formula (a t When at least one Li-containing metal oxide selected from the lithium (Li)-containing metal oxides represented by the formula (1) and (2), LiPF 6 The molar ratio of the content of the cyclic anion-containing lithium salt to the content of LiPF is preferably 3 or more and 150 or less. 6When the molar ratio of the content of the cyclic anion-containing lithium salt to the content of the [substance not specified in the original] is within the above range, when a Li-containing metal oxide containing Ni is used as the positive electrode, while suppressing the elution of the positive electrode metal, the organic component derived from the cyclic anion-containing lithium salt and the inorganic component derived from LiPF 6 By forming a negative electrode SEI with an excellent balance between the inorganic components derived from [substance not specified in the original], excellent high-temperature durability can be obtained, and excellent output characteristics and low-temperature characteristics can be obtained.

[0154] In the case of using at least one Li-containing metal oxide selected from the lithium (Li)-containing metal oxides represented by the above general formula (a t ), when the Ni content ratio q of the Li-containing metal oxide represented by the general formula (a t ) is q ≤ 0.5, the content of acetonitrile is preferably 10% by volume or more and preferably 49% by volume or less with respect to the total amount of the non-aqueous solvent. Further, when the Ni content ratio q of the Li-containing metal oxide represented by the general formula (a t ) is 0.5 < q < 1.2, the content of acetonitrile is preferably 10% by volume or more and preferably 35% by volume or less with respect to the total amount of the non-aqueous solvent. When the content of acetonitrile is within the above range, when a Li-containing metal oxide containing Ni is used as the positive electrode, while increasing the ionic conductivity, the elution of the transition metal caused by the coordination of acetonitrile to the transition metal in the positive electrode active material is suppressed, and the physical separation between the positive electrode Al current collector and the positive electrode active material is suppressed, and excellent output characteristics and low-temperature characteristics can be obtained, and excellent high-temperature durability can be obtained.

[0155] In the case of using at least one Li-containing metal oxide selected from the lithium (Li)-containing metal oxides represented by the above general formula (a t ), when the general formula (a t) When the Ni content ratio q of the Li-containing metal oxide represented by is q ≤ 0.5, the content of the cyclic anion-containing lithium salt represented by formula (1) with respect to the content of acetonitrile is preferably 0.06 or more, more preferably 0.075 or more, still more preferably 0.1 or more, still more preferably 0.15 or more, preferably 0.79 or less, preferably 0.75 or less, more preferably 0.5 or less, and still more preferably 0.25 or less in terms of molar ratio. When within the above range, when using a Li-containing metal oxide containing Ni as the positive electrode, by effectively suppressing the elution of the positive electrode metal by acetonitrile at high temperature and the physical separation between the positive electrode Al current collector and the positive electrode active material, excellent high-temperature durability can be obtained, and excellent output characteristics and low-temperature characteristics can be obtained. Also, general formula (a t ) When the Ni content ratio q of the Li-containing metal oxide represented by is 0.5 < q < 1.2, the content of the cyclic anion-containing lithium salt represented by formula (1) with respect to the content of acetonitrile is preferably 0.1 or more, more preferably 0.15 or more, still more preferably 0.17 or more, preferably 1.5 or less, more preferably 0.5 or less, and still more preferably 0.4 or less in terms of molar ratio. When within the above range, even when using a Li-containing metal oxide with a high Ni content ratio and prone to positive electrode metal elution at high temperature as the positive electrode, by effectively suppressing the elution of the positive electrode metal by acetonitrile at high temperature and the physical separation between the positive electrode Al current collector and the positive electrode active material, excellent high-temperature durability can be obtained, and excellent output characteristics and low-temperature characteristics can be obtained.

[0156] In the non-aqueous secondary battery according to this embodiment, it is preferable to use a lithium iron metal oxide having an olivine crystal structure containing iron (Fe) atoms, and the following formula (Xba): Li w M II PO 4 (Xba) {In the formula, M IIrepresents one or more transition metal elements including at least one transition metal element including Fe, and the value of w is determined depending on the charge / discharge state of the battery and represents a number from 0.05 to 1.10. It is more preferable to use a lithium phosphorus metal oxide having an olivine structure represented by the formula: In order to stabilize the structure, these lithium-containing metal oxides may be those in which a part of the transition metal element is replaced with Al, Mg, or other transition metal element, those in which these metal elements are contained in the crystal grain boundaries, those in which a part of the oxygen atoms is replaced with fluorine atoms, or those in which at least a part of the surface of the positive electrode active material is coated with another positive electrode active material, or the like.

[0157] Examples of the positive electrode active material include metal phosphate oxides containing lithium and a transition metal element, and metal silicate oxides containing lithium and a transition metal element. From the viewpoint of obtaining a higher voltage, the lithium-containing metal oxide is preferably a metal phosphate oxide containing lithium and at least one transition metal element selected from the group consisting of Co, Ni, Mn, Fe, Cu, Zn, Cr, V, and Ti, and from the viewpoint of the lithium phosphorus metal oxide represented by the above formula (Xba), a metal phosphate oxide containing Li and Fe is more preferable.

[0158] As a lithium phosphorus metal oxide different from the lithium phosphorus metal oxide represented by the above formula (Xba), Li v M I D 2 (Xa) In the formula, D represents a chalcogen element, and M I represents one or more transition metal elements including at least one transition metal element, and the value of v is determined depending on the charge / discharge state of the battery and represents a number from 0.05 to 1.10. A compound represented by the following formula may also be used.

[0159] When a lithium phosphorus metal oxide having an olivine structure represented by the formula (Xba) is used, the content of acetonitrile is preferably 30% by volume or more and preferably 66% by volume or less with respect to the total amount of the non-aqueous solvent. When the content of acetonitrile is within the above range, even when a lithium phosphorus metal oxide having excellent stability of the positive electrode crystal structure and relatively little positive electrode metal elution at high temperatures is used for the positive electrode, the ion conductivity is increased while suppressing the elution of transition metals caused by the coordination of acetonitrile with the transition metals in the positive electrode active material, and physical peeling between the positive electrode Al current collector and the positive electrode active material is suppressed, and excellent output characteristics and low-temperature characteristics can be obtained, as well as excellent high-temperature durability.

[0160] When using a lithium phosphorus metal oxide having an olivine structure represented by the above formula (Xba), the content of the cyclic anion-containing lithium salt represented by formula (1) relative to the content of acetonitrile is preferably 0.05 or more in molar ratio, more preferably 0.075 or more, more preferably 0.08 or more, even more preferably 0.1 or more, preferably 0.4 or less, more preferably 0.3 or less, more preferably 0.27 or less, and even more preferably 0.2 or less. When the molar ratio of the content of the cyclic anion-containing lithium salt relative to the content of acetonitrile is within the above range, even when a lithium phosphorus metal oxide having excellent stability of the positive electrode crystal structure and relatively little positive electrode metal elution at high temperatures is used for the positive electrode, the positive electrode metal elution by acetonitrile at high temperatures and physical peeling between the positive electrode Al current collector and the positive electrode active material can be effectively suppressed, thereby obtaining excellent high-temperature durability, as well as excellent output characteristics and low-temperature characteristics.

[0161] When a lithium phosphorus metal oxide having an olivine structure represented by the above formula (Xba) is used, LiPF 6 The molar ratio of the content of the cyclic anion-containing lithium salt to the content of LiPF is preferably 3 or more and 150 or less. 6When the molar ratio of the content of the cyclic anion-containing lithium salt to the content of LiPF is within the above-mentioned range, the stability of the positive electrode crystal structure is excellent, and even when a lithium phosphorus metal oxide, which is relatively unlikely to cause positive electrode metal elution at high temperatures, is used for the positive electrode, the positive electrode metal elution can be suppressed while the organic component derived from the cyclic anion-containing lithium salt and the LiPF 6 By forming a negative electrode SEI having an excellent balance of inorganic components derived from the cathode, it is possible to obtain excellent high-temperature durability, as well as excellent output characteristics and low-temperature characteristics.

[0162] In the present embodiment, the positive electrode active material may be the lithium-containing metal oxide alone, or may be used in combination with other positive electrode active materials. Examples of other positive electrode active materials include metal oxides or metal chalcogenides having a tunnel structure and a layer structure; sulfur; and conductive polymers. Examples of metal oxides or metal chalcogenides having a tunnel structure and a layer structure include MnO 2 , FeO 2 , FeS 2 , V 2 O 5 , V 6 O 13 , TiO 2 , TiS 2 , MoS 2 , and NbSe 2 Examples of the conductive polymer include oxides, sulfides, and selenides of metals other than lithium, such as those represented by the following formula: Examples of the conductive polymer include conductive polymers represented by polyaniline, polythiophene, polyacetylene, and polypyrrole.

[0163] The above-mentioned other positive electrode active materials may be used alone or in combination of two or more. The positive electrode active material layer preferably contains at least one transition metal element selected from Ni, Mn, and Co, because it is capable of reversibly and stably absorbing and releasing lithium ions and achieving a high energy density.

[0164] When a lithium-containing metal oxide and another positive electrode active material are used in combination as a positive electrode active material, the ratio of the two materials is preferably 80 mass% or more, and more preferably 85 mass% or more, of the lithium-containing metal oxide relative to the total positive electrode active material.

[0165] The positive electrode active material layer is formed by dispersing a positive electrode mixture, which is a mixture of a positive electrode active material and, if necessary, a conductive assistant and a binder, in a solvent to form a positive electrode mixture-containing slurry, which is applied to a positive electrode current collector, drying (solvent removal), and pressing if necessary. As such a solvent, a known one can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be used.

[0166] Examples of the conductive assistant include graphite, carbon black such as acetylene black and ketjen black, and carbon fiber. The content of the conductive assistant is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, per 100 parts by mass of the positive electrode active material.

[0167] If the content of the conductive assistant is too high, the volume energy density decreases, but if the content is too low, the formation of the electron conduction path becomes insufficient. In particular, since the electron conductivity of the positive electrode active material layer is lower than that of the negative electrode active material layer, if the amount of the conductive assistant is insufficient, it becomes impossible to obtain a predetermined battery capacity when the nonaqueous secondary battery is discharged or charged at a high current value. Therefore, in applications requiring high output and / or rapid charging, it is preferable to increase the content of the conductive assistant to a range in which the reaction based on the transfer of electrons is not rate-determining.

[0168] Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, carboxymethyl cellulose, styrene butadiene rubber, and fluororubber. The content of the binder is preferably 6 parts by mass or less, and more preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the positive electrode active material.

[0169] The positive electrode current collector is made of a metal foil such as aluminum foil, nickel foil, stainless steel foil, etc. The positive electrode current collector may have a carbon coating on the surface, or may be processed into a mesh shape. The thickness of the positive electrode current collector is preferably 5 to 40 μm, more preferably 7 to 35 μm, and further preferably 9 to 30 μm.

[0170] The weight per surface of the positive electrode, excluding the positive electrode current collector, is set to 15 mg / cm from the viewpoint of improving the volumetric energy density of the non-aqueous secondary battery. 2 It is preferable that the concentration is 17.5 mg / cm or more. 2 More preferably, it is 24 mg / cm or more. 2 The weight per surface of the positive electrode excluding the positive electrode current collector is more preferably 200 mg / cm2 or more. 2 It is preferable that the concentration is less than 100 mg / cm 2 More preferably, it is 60 mg / cm or less. 2 By limiting the basis weight per one side of the positive electrode excluding the positive electrode current collector to the above range, it is possible to provide a nonaqueous secondary battery that achieves high output performance even in the case where an electrode active material layer with a high volumetric energy density is designed.

[0171] Here, the basis weight is the weight per unit area of ​​the electrode when forming an electrode active material layer on one side of the current collector. 2 When electrode active material layers are formed on both sides of a current collector, the mass of the electrode active material is calculated based on the electrode area of ​​each side (1 cm2). 2 If a large amount of electrode active material is applied to the electrode current collector, the amount of electrode active material per unit volume of the battery will be relatively greater than other battery materials that are not related to battery capacity, such as the current collector foil and separator, resulting in a high capacity battery. When an electrode active material layer is formed on one surface of a current collector, the coating weight can be calculated by the following formula (12). Weight [mg / cm 2 ] = (electrode mass [mg] - electrode current collector mass [mg]) ÷ electrode area [cm2 ] ·····(12)

[0172] <5. Negative electrode> The negative electrode 160 is composed of a negative electrode active material layer made of a negative electrode mixture and a negative electrode current collector. The negative electrode 160 can function as a negative electrode of a non-aqueous secondary battery.

[0173] The negative electrode mixture contains a negative electrode active material, and optionally contains a conductive assistant and a binder.

[0174] Examples of the negative electrode active material include amorphous carbon (hard carbon, soft carbon), graphite (artificial graphite, natural graphite), pyrolytic carbon, coke, glassy carbon, a fired body of an organic polymer compound, mesocarbon microbeads, carbon fiber, activated carbon, carbon colloid, and carbon materials such as carbon black, metallic lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon alloys, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. The negative electrode active material can be used alone or in combination of two or more.

[0175] As the negative electrode active material of this embodiment, it is preferable to use graphite or a compound containing one or more elements selected from the group consisting of Ti, V, Sn, Cr, Mn, Fe, Co, Ni, Zn, Al, Si, and B.

[0176] The negative electrode active material layer uses lithium ions as the negative electrode active material at 0.4V vs. Li / Li in order to increase the battery voltage. + It is preferable that the hydrogen-containing gas contains a material capable of absorbing at a potential lower than the hydrogen potential.

[0177] The negative electrode active material layer is formed by dispersing a negative electrode mixture, which is a mixture of a negative electrode active material and, if necessary, a conductive assistant and a binder, in a solvent to form a negative electrode mixture-containing slurry, which is applied to a negative electrode current collector, drying (solvent removal), and pressing if necessary. As such a solvent, a known one can be used, and examples thereof include N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc.

[0178] Examples of the conductive assistant include carbon black, such as acetylene black and ketjen black, carbon fiber, and graphite. The content of the conductive assistant is preferably 20 parts by mass or less, and more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the negative electrode active material.

[0179] Examples of the binder include carboxymethyl cellulose, PVDF, PTFE, polyacrylic acid, and fluororubber. Also included are diene rubbers such as styrene-butadiene rubber. The content of the binder is preferably 10 parts by mass or less, more preferably 0.5 to 6 parts by mass, based on 100 parts by mass of the negative electrode active material.

[0180] The negative electrode current collector is made of a metal foil such as copper foil, nickel foil, stainless steel foil, etc. The surface of the negative electrode current collector may be carbon-coated or processed into a mesh shape. The thickness of the negative electrode current collector is preferably 5 to 40 μm, more preferably 6 to 35 μm, and further preferably 7 to 30 μm.

[0181] <6. Separator> In the present embodiment, the nonaqueous secondary battery 100 preferably includes a separator 170 between the positive electrode 150 and the negative electrode 160 from the viewpoint of preventing short circuits between the positive electrode 150 and the negative electrode 160 and providing safety such as shutdown. The separator 170 is preferably an insulating thin film having high ion permeability and excellent mechanical strength. Examples of the separator 170 include woven fabric, nonwoven fabric, and synthetic resin microporous membrane, and among these, synthetic resin microporous membrane is preferable.

[0182] As the synthetic resin microporous film, for example, a microporous film containing polyethylene or polypropylene as a main component, or a polyolefin-based microporous film such as a microporous film containing both of these polyolefins is preferably used. As the nonwoven fabric, for example, a porous film made of a heat-resistant resin such as glass, ceramic, polyolefin, polyester, polyamide, liquid crystal polyester, or aramid can be used.

[0183] Separator 170 may be configured as a single layer or multiple layers of one type of microporous film, or may be configured as a stack of two or more types of microporous films. Separator 170 may be configured as a single layer or multiple layers of a mixed resin material obtained by melting and kneading two or more types of resin materials.

[0184] For the purpose of providing functions, inorganic particles may be present on the surface or inside of the separator, or other organic layers may be further coated or laminated. The separator may also include a crosslinked structure. In order to improve the safety performance of the nonaqueous secondary battery, these techniques may be combined as necessary.

[0185] By using such a separator 170, it is possible to realize good input / output characteristics and low self-discharge characteristics required for lithium ion batteries for high power applications. The thickness of the separator is preferably 1 μm or more from the viewpoint of separator strength, and is preferably 500 μm or less from the viewpoint of permeability, more preferably 5 μm to 30 μm, and even more preferably 10 μm to 25 μm. In addition, when emphasis is placed on short circuit resistance performance, the thickness of the separator is more preferably 15 μm to 20 μm, but when emphasis is placed on high energy density, the thickness is more preferably 10 μm to less than 15 μm. The porosity of the separator is preferably 30% to 90%, more preferably 35% to 80%, and even more preferably 40% to 70% from the viewpoint of following the rapid movement of lithium ions at high power. In addition, when priority is given to improving output performance while ensuring safety, 50% or more and 70% or less is particularly preferable, and when emphasis is placed on both short circuit resistance and output performance, 40% or more and less than 50% is particularly preferable. The air permeability of the separator is set to 1 sec / 100 cm from the viewpoint of the balance between the thickness and porosity of the separator. 3 More than 400 seconds / 100cm 3 Less than 100 seconds / 100 cm is preferable. 3 More than 350 / 100cm 3 It is more preferable that the air permeability is 150 sec / 100 cm. 3 More than 350 seconds / 100cm 3 The following is particularly preferable. If you prioritize improving output performance while ensuring safety, 100 / 100cm 3 seconds or more 150 seconds / 100cm 3is particularly preferably less than 10 mS / cm. On the other hand, when a non-aqueous electrolyte with low ionic conductivity is combined with a separator within the above range, the lithium ion migration rate is not determined by the structure of the separator, but by the high ionic conductivity of the electrolyte, and the expected input / output characteristics tend not to be obtained. Therefore, the ionic conductivity of the non-aqueous electrolyte at 25°C is preferably 10 mS / cm or more, more preferably 15 mS / cm or more, and even more preferably 20 mS / cm or more. However, the thickness, air permeability and porosity of the separator, and the ionic conductivity of the non-aqueous electrolyte are not limited to the above examples.

[0186] <7. Battery exterior> The battery exterior 110 of the nonaqueous secondary battery 100 in this embodiment may be, for example, a battery can (not shown) or a laminate film exterior. The battery can may be, for example, a metal can made of steel, stainless steel (SUS), aluminum, clad material, or the like, and may be rectangular, rectangular tube, cylindrical, elliptical, flat, coin, or button-shaped. The laminate film exterior may be, for example, a laminate film made of a three-layer structure of heat-melting resin / metal film / resin.

[0187] The laminate film exterior body can be used as an exterior body by stacking two sheets with the heat-melting resin side facing inward, or by folding the laminate film exterior body so that the heat-melting resin side faces inward, and sealing the ends by heat sealing. When using a laminate film exterior body, the positive electrode lead body 130 (or a lead tab connected to the positive electrode terminal and the positive electrode terminal) may be connected to the positive electrode current collector, and the negative electrode lead body 140 (or a lead tab connected to the negative electrode terminal and the negative electrode terminal) may be connected to the negative electrode current collector. In this case, the laminate film exterior body may be sealed with the ends of the positive electrode lead body 130 and the negative electrode lead body 140 (or the lead tabs connected to the positive electrode terminal and the negative electrode terminal, respectively) pulled out to the outside of the exterior body.

[0188] In the present embodiment, the battery exterior of the nonaqueous secondary battery preferably contains aluminum in at least a part of the liquid-contacting layer on the positive electrode side with the nonaqueous electrolyte. By using such a battery exterior, it is possible to minimize corrosion deterioration of the battery exterior and improve the high-temperature durability and cycle characteristics of the battery. The liquid-contacting layer may be made of the same material as the main body, i.e., the liquid-contacting layer of the main body, or may be a layer formed by coating the main body with another material.

[0189] The aluminum contained in the liquid contact layer may be present in a portion of the liquid contact layer with the nonaqueous electrolyte, or may be present in the entire liquid contact layer. However, in order to minimize corrosion deterioration of the battery exterior and maximize improvement in the cycle characteristics of the battery, it is more preferable that the entire liquid contact layer is aluminum.

[0190] In addition, the battery exterior of the nonaqueous secondary battery in this embodiment may be one in which the main body is made of a metal other than aluminum, and at least a part of the liquid contact layer with the nonaqueous electrolyte contains aluminum. The liquid contact layer containing aluminum can be provided by plating, cladding, or the like. More preferably, it is made of aluminum cladding. A cladding is a material in which two or more different metals are bonded together, and is generally considered to be one in which the boundary surface between the different metals is diffusion bonded (has an alloy layer). The cladding can be produced by pressing or explosive welding.

[0191] In the case of a coin-type nonaqueous secondary battery, the battery exterior preferably contains aluminum in at least a part of the liquid contact layer on the positive electrode side, and more preferably has at least a part of the liquid contact layer on the positive electrode side clad with aluminum.

[0192] When the main metal layer of the battery exterior is made of a metal other than aluminum, the main metal is not particularly limited, but from the viewpoint of preventing corrosion of the outside of the container, it is preferable to use austenitic stainless steels such as SUS304, SUS316, and SUS316L, austenitic-ferritic stainless steels such as SUS329J1 and SUS329J3L, ferritic stainless steels such as SUS405 and SUS430, and martensitic stainless steels such as SUS403 and SUS410.

[0193] In addition, in the battery exterior body in this embodiment, at least a part of the contact portion with the nonaqueous electrolyte on the positive electrode side may be made of iron or an iron alloy. By making the battery exterior body of iron or an iron alloy, a battery having excellent impact resistance and safety can be provided. The battery exterior body and the positive electrode current collector may be separate or may be integrated. In addition, the battery exterior 110 of the nonaqueous secondary battery 100 in this embodiment may be, for example, a battery exterior of either a battery can (not shown) or a laminate film exterior body. As the battery can, for example, a metal can such as a square, rectangular tube, cylindrical, elliptical, flat, coin, or button type made of steel, stainless steel (SUS), or clad material can be used. As the laminate film exterior body, for example, a laminate film made of a three-layer structure of a heat-melting resin / metal film / resin can be used.

[0194] In this embodiment, the surface of the battery exterior body made of iron or iron alloy may not be coated. Since the increase in energy density of a non-aqueous secondary battery increases the risk of battery ignition, further safety measures are required. Therefore, from the viewpoint of impact resistance, it is a useful method to use a battery exterior made of iron or iron alloy with high strength instead of a lightweight aluminum battery exterior.

[0195] Furthermore, since iron and iron alloys are less expensive than aluminum, when a large number of batteries are installed in an electric vehicle or the like, significant cost reductions are possible by using battery exteriors made of iron or iron alloys.

[0196] The inventors have found that in a lithium ion battery using an acetonitrile-containing electrolyte, if the material of the battery exterior body including at least a part of the contact portion with the non-aqueous electrolyte on the positive electrode side is iron or an iron alloy, the metal component of the battery exterior body corrodes during charging, causing overcharging. This phenomenon is a problem newly discovered by the inventors, and is not described at all in Patent Documents 1 to 8.

[0197] By using the cyclic anion-containing lithium salt represented by formula (1) in a non-aqueous electrolyte solution containing acetonitrile, overcharging caused by corrosion of the battery exterior body made of iron or iron alloy can be suppressed. The mechanism is presumed to be as follows: The cyclic anion-containing lithium salt represented by formula (1) dissociates into lithium ions and cyclic anions in a non-aqueous electrolyte containing acetonitrile. The cyclic anion electrically interacts with acetonitrile, weakening the metal coordination ability of the nitrile group of acetonitrile. This suppresses metal dissolution caused by acetonitrile forming a complex with a transition metal in iron or an iron alloy, and suppresses the migration of the metal complex to the negative electrode. Therefore, overcharging due to continuous reduction precipitation of the metal complex at the negative electrode can be suppressed.

[0198] When the material of the battery exterior is stainless steel (SUS), from the viewpoint of preventing corrosion inside or outside the container, it is preferable to use austenitic stainless steels such as SUS304, SUS316, and SUS316L, austenitic-ferritic stainless steels such as SUS329J1 and SUS329J3L, ferritic stainless steels such as SUS405 and SUS430, and martensitic stainless steels such as SUS403 and SUS410.

[0199] <8. How to make a battery> The nonaqueous secondary battery 100 in this embodiment is produced by a known method using the above-mentioned nonaqueous electrolyte, a positive electrode 150 having a positive electrode active material layer on one or both sides of a current collector, a negative electrode 160 having a negative electrode active material layer on one or both sides of a current collector, a battery exterior 110, and, if necessary, a separator 170.

[0200] First, a laminate is formed consisting of the positive electrode 150, the negative electrode 160, and, if necessary, the separator 170. For example, possible modes include a mode in which the long positive electrode 150 and the negative electrode 160 are wound in a stacked state with the long separator interposed between the positive electrode 150 and the negative electrode 160 to form a laminate with a wound structure; a mode in which the positive electrode sheets and the negative electrode sheets obtained by cutting the positive electrode 150 and the negative electrode 160 into a plurality of sheets having a certain area and shape are alternately stacked with a separator sheet between to form a laminate with a laminate structure; a mode in which a long separator is folded zigzag and a positive electrode body sheet and a negative electrode body sheet are alternately inserted between the zigzag folded separators to form a laminate with a laminate structure; and the like.

[0201] Next, the above-mentioned laminate is housed in a battery exterior 110 (battery case), the electrolyte solution according to this embodiment is poured into the battery case, and the laminate is immersed in the electrolyte solution and sealed, thereby producing the nonaqueous secondary battery of this embodiment. Alternatively, a gelled electrolyte membrane is produced in advance by impregnating a substrate made of a polymer material with the electrolyte solution, and a laminate having a laminated structure is formed using a sheet-like positive electrode 150, a negative electrode 160, and an electrolyte membrane, and a separator 170 as necessary, and then the laminate is housed in the battery exterior 110 to produce the nonaqueous secondary battery 100.

[0202] In addition, if the arrangement of the electrodes is designed so that there is a portion where the outer peripheral edge of the negative electrode active material layer overlaps with the outer peripheral edge of the positive electrode active material layer, or there is a portion where the width is too small in the non-facing portion of the negative electrode active material layer, the position of the electrodes may be shifted during battery assembly, which may deteriorate the charge-discharge cycle characteristics of the non-aqueous secondary battery. Therefore, it is preferable that the electrode positions of the electrode body used in the non-aqueous secondary battery are fixed in advance by tapes such as polyimide tape, polyphenylene sulfide tape, and polypropylene (PP) tape, adhesives, etc.

[0203] In this embodiment, due to the high ionic conductivity of acetonitrile, lithium ions released from the positive electrode during the initial charge of the non-aqueous secondary battery may diffuse throughout the negative electrode. In non-aqueous secondary batteries, the area of ​​the negative electrode active material layer is generally made larger than that of the positive electrode active material layer. However, if lithium ions diffuse and are absorbed to a portion of the negative electrode active material layer that does not face the positive electrode active material layer, the lithium ions will not be released during the initial discharge and will remain in the negative electrode. Therefore, the contribution of the lithium ions that are not released becomes the irreversible capacity. For these reasons, in non-aqueous secondary batteries using a non-aqueous electrolyte containing acetonitrile, the initial charge / discharge efficiency may be low.

[0204] On the other hand, if the area of ​​the positive electrode active material layer is larger than that of the negative electrode active material layer or they are the same, current tends to concentrate at the edge portions of the negative electrode active material layer during charging, making lithium dendrites more likely to form.

[0205] Although there is no particular restriction on the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer face each other, for the reasons described above, it is preferably greater than 1.0 and less than 1.1, more preferably greater than 1.002 and less than 1.09, even more preferably greater than 1.005 and less than 1.08, and particularly preferably greater than 1.01 and less than 1.08. In a nonaqueous secondary battery using a nonaqueous electrolyte solution containing acetonitrile, the initial charge / discharge efficiency can be improved by reducing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer face each other.

[0206] Reducing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer face each other means limiting the ratio of the area of ​​the portion of the negative electrode active material layer that does not face the positive electrode active material layer. This makes it possible to reduce as much as possible the amount of lithium ions absorbed in the portion of the negative electrode active material layer that does not face the positive electrode active material layer among the lithium ions released from the positive electrode during the initial charge (i.e., the amount of lithium ions that are not released from the negative electrode during the initial discharge and become irreversible capacity). Therefore, by designing the ratio of the area of ​​the entire negative electrode active material layer to the area of ​​the portion where the positive electrode active material layer and the negative electrode active material layer face each other within the above range, it is possible to improve the load characteristics of the battery by using acetonitrile, increase the initial charge / discharge efficiency of the battery, and further suppress the generation of lithium dendrites.

[0207] The non-aqueous secondary battery 100 in this embodiment can function as a battery by initial charging, but is stabilized by decomposing a part of the electrolyte during initial charging. There is no particular limitation on the method of initial charging, but the initial charging is preferably performed at 0.001 to 0.3 C, more preferably at 0.002 to 0.25 C, and even more preferably at 0.003 to 0.2 C. Initial charging via constant voltage charging also gives favorable results. By setting the voltage range in which the lithium salt is involved in the electrochemical reaction to be long, a stable and strong negative electrode SEI is formed on the electrode surface, suppressing an increase in internal resistance, and providing a good effect on members other than the negative electrode 160, such as the positive electrode 150 and the separator 170, without the reaction product being firmly fixed only to the negative electrode 160. For this reason, it is very effective to perform the initial charging in consideration of the electrochemical reaction of the lithium salt dissolved in the non-aqueous electrolyte.

[0208] The nonaqueous secondary battery 100 in this embodiment can also be used as a battery pack in which a plurality of nonaqueous secondary batteries 100 are connected in series or in parallel. From the viewpoint of managing the charge / discharge state of the battery pack, when the positive electrode active material represented by the above formula (Xba) is used in the positive electrode, the operating voltage range per battery is preferably 1.5 to 4.0 V, and particularly preferably 2.0 to 3.8 V.

[0209] In addition, the general formula (a t When a positive electrode active material represented by the formula (1) is used, the operating voltage range per battery is preferably 2 to 5V, more preferably 2.5 to 5V, and particularly preferably 2.75V to 5V. EXAMPLES

[0210] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0211] (1) Preparation of non-aqueous electrolyte Various non-aqueous solvents were mixed in an inert atmosphere to obtain a predetermined concentration. Furthermore, various lithium salts were added to obtain a predetermined concentration to prepare non-aqueous electrolyte solutions (S01) to (S13), (S20), (S22) to (S36), and (S40). Furthermore, these non-aqueous electrolyte solutions were used as mother electrolyte solutions, and various additives were added to the mother electrolyte solution in a predetermined amount by mass to 100 parts by mass to prepare non-aqueous electrolyte solutions (S14) to (S19), (S21), and (S37) to (S39). The compositions of these non-aqueous electrolyte solutions are shown in Table 1.

[0212] The abbreviations for the non-aqueous solvents, lithium salts, and various additives in Table 1 have the following meanings. (Non-aqueous solvent) AN: Acetonitrile EMC: Ethyl methyl carbonate EC: Ethylene carbonate ES: Ethylene sulfite VC: Vinylene carbonate (Lithium salts) (1-2): A compound represented by the above formula (1-2) (9): A compound represented by the above formula (9) LiFSI: Lithium bis(fluorosulfonyl)imide (LiN(SO 2 F) 2 ) LiPF 6 : Lithium hexafluorophosphate (Various additives) Py: Pyridine TMSPi: Tris(trimethylsilyl) phosphite DPDMS: diphenyldimethoxysilane TEVS: Triethoxyvinylsilane SN: Succinonitrile

[0213] [Table 1]

[0214] (2) Fabrication of a small non-aqueous secondary battery with an Fe-based positive electrode (2-1) Preparation of positive electrode (P1) Lithium iron phosphate (LiFePO) with an olivine structure was used as the positive electrode active material. 4 ) was mixed with carbon black powder as a conductive assistant and polyvinylidene fluoride (PVDF) as a binder in a mass ratio of 89:3:8 to obtain a positive electrode mixture.

[0215] The obtained positive electrode mixture was mixed with N-methyl-2-pyrrolidone as a solvent to prepare a positive electrode mixture-containing slurry. The positive electrode mixture-containing slurry was applied to one side of an aluminum foil having a thickness of 20 μm to serve as a positive electrode current collector in an amount of 11.0 mg / cm. 2 The positive electrode active material layer was then dried and removed using a roll press until the density of the layer became 1.8 g / cm. 3 The positive electrode (P1) was obtained by rolling the positive electrode active material layer and the positive electrode current collector.

[0216] (2-2) Preparation of negative electrode (N1) Graphite powder as the negative electrode active material, carbon black powder as a conductive assistant, and polyvinylidene fluoride (PVDF) as a binder were mixed in a solid content mass ratio of 90:3:7 to obtain a negative electrode mixture.

[0217] Water was added as a solvent to the obtained negative electrode mixture so that the solid content was 45 mass % and further mixed to prepare a negative electrode mixture-containing slurry. The negative electrode mixture-containing slurry was applied to one side of a copper foil having a thickness of 8 μm and a width of 280 mm as a negative electrode current collector using a three-roll transfer coater while adjusting the basis weight of the negative electrode mixture-containing slurry so as to have a coating width of 240 to 250 mm, a coating length of 125 mm, and an uncoated length of 20 mm, and the solvent was dried and removed in a hot air drying oven. The obtained electrode roll was trimmed and cut on both sides and dried under reduced pressure at 80 ° C for 12 hours. Thereafter, the density of the negative electrode active material layer was adjusted to 1.3 g / cm by roll pressing. 3 The negative electrode (N1) was obtained by rolling the negative electrode active material layer and the negative electrode current collector so that the coating weight excluding the negative electrode current collector was 5.4 mg / cm. 2 It was.

[0218] (2-3) Assembly of a small non-aqueous secondary battery with an Fe-based positive electrode The positive electrode (P1) obtained as described above was punched out into a disk shape having a diameter of 15.958 mm, and the negative electrode (N1) obtained as described above was punched out into a disk shape having a diameter of 16.156 mm. The disks were then sandwiched between a polyethylene microporous membrane separator (film thickness 21 μm, air permeability 285 s / 100 cm 3 A laminate was obtained by laminating the laminate on both sides of a laminate (porosity 41%). The laminate was inserted into a disk-shaped battery case made of SUS. Next, 200 μL of non-aqueous electrolyte (S01 to S22) was poured into the battery case, and the laminate was immersed in the non-aqueous electrolyte. The battery case was then sealed and held at 25° C. for 12 hours to allow the non-aqueous electrolyte to fully penetrate the laminate, thereby obtaining a small non-aqueous secondary battery.

[0219] (3) Evaluation of small non-aqueous secondary batteries with Fe-based positive electrodes The small non-aqueous secondary batteries obtained as described above were first subjected to an initial charge / discharge treatment and initial charge / discharge capacity measurement according to the procedure in (3-1) below. Next, each small non-aqueous secondary battery was evaluated according to the procedure in (3-2) below. In another evaluation, after the procedure in (3-1) below, an output test was performed according to the procedure in (3-3) or (3-4) below. The charging and discharging were performed using a charging and discharging device ACD-M01A (product name) manufactured by Asuka Electronics Co., Ltd. and a programmable thermostatic chamber IN804 (product name) manufactured by Yamato Scientific Co., Ltd.

[0220] In this specification, 1C means the current value at which a fully charged battery is expected to be discharged completely within one hour when discharged at a constant current.

[0221] Specifically, in a small non-aqueous secondary battery, 1C means a current value at which a battery is discharged from a fully charged state of 3.5 V to 2.0 V at a constant current, with the discharge expected to be completed in one hour. The small non-aqueous secondary battery assembled according to the procedure in (2-3) above is a 3 mAh class cell, with the battery voltage in a fully charged state set to 3.5 V and the current value equivalent to 1 C set to 3.0 mA. Hereinafter, unless otherwise specified, the notation of current value and voltage will be omitted for convenience.

[0222] (3-1) Initial charge / discharge process The ambient temperature of the small non-aqueous secondary battery was set to 25°C, and the battery was charged at a constant current equivalent to 0.1C until it reached a fully charged state, i.e., 3.5V, and then charged at a constant voltage for 1.5 hours. The battery was then discharged to 2.0V at a constant current equivalent to 0.1C. The initial efficiency was calculated by dividing the discharge capacity at this time by the charge capacity. The discharge capacity at this time was also taken as the initial capacity. Thereafter, in order to stably form the negative electrode SEI, the same charge and discharge as above was performed once.

[0223] The initial efficiency indicates the ratio of the initial discharge capacity to the initial charge capacity, but is generally lower than the charge / discharge efficiency from the second time onwards. This is because Li ions are used during the initial charge to form the negative electrode SEI. This results in fewer Li ions being able to be discharged. Here, there is no problem if the initial efficiency is 84% ​​or higher.

[0224] (3-2) 85℃ 100 hours and 200 hours fully charged storage test The small non-aqueous secondary battery that had been subjected to the initial charge / discharge treatment according to the method described in (3-1) above was charged at a constant current equivalent to 1C at an ambient temperature of 25°C, and the battery was charged to a fully charged state, i.e., 3.5V, and then charged at a constant voltage for 1.5 hours. Next, the small non-aqueous secondary battery was stored in a thermostatic chamber at 85°C for 100 hours. After that, the ambient temperature was returned to 25°C, and the battery was discharged to 2.0V at a current value equivalent to 0.1C. The remaining discharge capacity at this time was taken as the remaining discharge capacity after 100 hours. The remaining capacity retention rate was calculated based on the following formula as the measured value of the 85°C 100-hour fully charged storage test. In addition, when measuring a commercially available battery, the initial charge / discharge treatment is performed according to the procedure of (3-1) to measure the initial capacity, and then the remaining discharge capacity is measured according to the procedure of (3-2) to calculate the remaining capacity retention rate. Residual capacity maintenance rate after 100 hours = (Residual discharge capacity after 100 hours / Initial capacity) x 100[%]

[0225] After that, the small non-aqueous secondary battery was charged at a constant current equivalent to 1C to reach a fully charged state of 3.5V, and then charged at a constant voltage for 1.5 hours. Next, this small non-aqueous secondary battery was stored in a thermostatic chamber at 85°C for 100 hours. After that, the ambient temperature was returned to 25°C, and the battery was discharged to 2.0V at a current value equivalent to 0.1C. The remaining discharge capacity at this time was taken as the remaining discharge capacity after 200 hours. The remaining capacity retention rate was calculated based on the following formula as the measured value of the 85°C 200-hour fully charged storage test. Residual capacity maintenance rate after 200 hours = (Residual discharge capacity after 200 hours / Initial capacity) x 100[%]

[0226] The remaining capacity retention rate is an index of the degree of self-discharge in a storage test at 85°C in a full charge. The larger this value, the smaller the self-discharge at high temperatures and the more current that can be used. The remaining capacity retention rate after 100 hours is preferably 35% or more, more preferably 45% or more, even more preferably 55% or more, and particularly preferably 60% or more. The remaining capacity retention rate after 200 hours is preferably 12% or more, more preferably 20% or more, even more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more.

[0227] The results of the 85°C fully charged storage tests for 100 hours and 200 hours are shown in Table 2.

[0228] (3-3) -40℃ Output Test The battery that had been subjected to the initial charge / discharge treatment according to the method described in (3-1) above was charged at a constant current of 3 mA, which corresponds to 1 C, to 3.5 V, and then charged at a constant voltage of 3.5 V for a total of 1.5 hours. Then, it was discharged to 2.0 V at a current value of 0.3 mA, which corresponds to 0.1 C. Next, the battery was set at an ambient temperature of 25 ° C., charged at a constant current of 3 mA, which corresponds to 1 C, to 3.5 V, and then charged at a constant voltage of 3.5 V for a total of 1.5 hours. Then, the battery was set at an ambient temperature of -40 ° C., and discharged to 2.0 V at a current value of 3 mA, which corresponds to 1 C, to calculate the capacity retention rate below. 1C capacity retention rate = (Capacity at 1C discharge at -40℃ / Capacity at 0.1C discharge at 25℃) x 100 [%]

[0229] The 1C capacity retention rate is an index of output performance at -40°C. The larger this value is, the smaller the internal resistance of the nonaqueous secondary battery at low temperatures, and the more current can be used. In particular, there is increasing demand for nonaqueous secondary batteries containing Fe-based positive electrodes as auxiliary batteries for electric vehicles, and high low-temperature performance is required for stable operation even in cold regions. The 1C capacity retention rate is preferably 10% or more, and more preferably 30% or more. The results of the -40°C output test are shown in Table 2.

[0230] (3-4) 25℃ Output Test The battery that had been initially charged and discharged by the method described in (3-1) above was charged at a constant current of 3 mA, equivalent to 1 C, to 3.5 V, and then charged at a constant voltage of 3.5 V for a total of 1.5 hours. It was then discharged to 2.0 V at a current value of 0.3 mA, equivalent to 0.1 C. Next, the same charge and discharge as above was performed, except that the current value during constant current discharge was changed to 60 mA, equivalent to 20 C, and the capacity retention rate was calculated as follows. 20C capacity retention rate = (capacity when discharging at 20C / capacity when discharging at 0.1C) x 100 [%]

[0231] Here, we discuss the interpretation of each test.

[0232] The 20C capacity retention rate is an index of output performance at 25°C. The larger this value is, the smaller the internal resistance of the nonaqueous secondary battery is, and the more current can be used. In particular, there is an increasing demand for nonaqueous secondary batteries containing an Fe-based positive electrode in high-output applications such as electric tools, and high output performance is required. The 20C capacity retention rate is preferably 30% or more, and more preferably 60% or more. The results of the 25°C output test are shown in Table 2.

[0233] [Table 2]

[0234] As shown in Table 2, the initial efficiency was equal to or higher than the preferred value in Examples 1 to 18. On the other hand, Comparative Example 4 showed an initial efficiency of less than 84%.

[0235] As shown in Table 2, in Examples 1 to 18, the remaining capacity retention rates after the 100-hour fully charged storage test and the 200-hour fully charged storage test were equal to or higher than the preferred values. On the other hand, in Comparative Examples 1 and 4, the remaining capacity retention rates after 100 hours were less than 35%, and the remaining capacity retention rates after 200 hours were less than 12%.

[0236] Furthermore, in Examples 1 to 18, the 1C capacity retention rate in the −40° C. output test was equal to or higher than the preferred value, whereas in Comparative Examples 2 and 3, the 1C capacity retention rate was less than 10%.

[0237] Furthermore, in Examples 1 to 18, the 20C capacity retention rate in the 25° C. output test was greater than or equal to a preferable value, whereas in Comparative Examples 2 and 3, the 20C capacity retention rate was less than 30%.

[0238] Comparing Example 1 and Comparative Example 1, by replacing the lithium salt LiFSI with the compound represented by the above formula (1-2), the remaining capacity retention rate after 100 hours and 200 hours was improved. This is thought to be because the use of a lithium salt containing a cyclic anion suppresses the positive electrode metal elution and physical peeling between the positive electrode Al current collector and the positive electrode active material, which are issues with an acetonitrile-containing electrolyte, and the decomposition product of the cyclic anion acts as a negative electrode SEI component.

[0239] In addition, when Examples 1 to 3 are compared, the cyclic anion-containing lithium salt / LiPF 6 As the molar ratio of LiPF increases, the remaining capacity retention rate after 100 hours and 200 hours improves. This is because the amount of LiPF, which causes a decrease in battery performance at high temperatures in an acetonitrile-containing electrolyte, is reduced. 6 It is speculated that this is because by reducing the amount of lithium salt containing a cyclic anion, which can suppress the elution of positive electrode metal and physical peeling between the positive electrode Al current collector and the positive electrode active material in an acetonitrile-containing electrolyte, and by increasing the amount of lithium salt containing a cyclic anion, which can suppress the deterioration of battery performance at high temperatures by contributing to the negative electrode SEI, it is possible to more effectively suppress the deterioration of battery performance at high temperatures.

[0240] In addition, when Examples 1 to 3 are compared, LiPF 6 As the amount of LiPF is reduced, the remaining capacity retention rate after 100 hours and 200 hours is improved. 6 The generation of acid components due to the thermal decomposition of acetonitrile is suppressed, and hydrogen is removed from the α-position of acetonitrile to form PF6 It is presumed that this is because the amount of HF generated from the anions could also be reduced, resulting in minimizing the deterioration of battery performance due to corrosion of the positive electrode active material layer and the positive electrode current collector, or deterioration reactions of the electrolyte.

[0241] In addition, when Example 1 is compared with Comparative Example 4, by replacing the lithium salt with the compound represented by the above formula (1-2) instead of the compound represented by the above formula (9), the remaining capacity retention rate after 100 hours and 200 hours is improved. This is believed to be because the decomposition of the cyclic anion is suppressed by using a lithium salt containing a cyclic anion having a 5-membered ring instead of a 6-membered ring.

[0242] In addition, when Examples 2 and 3 are compared with Example 1, the content of the cyclic anion-containing lithium salt is LiPF 6 The remaining capacity retention rate after 100 hours was 50% or more, and the remaining capacity retention rate after 200 hours was 30% or more. This is because the LiPF 6 It is speculated that this is because by reducing the amount of lithium salt containing a cyclic anion, which can suppress the elution of positive electrode metal and physical peeling between the positive electrode Al current collector and the positive electrode active material in an acetonitrile-containing electrolyte, and by increasing the amount of lithium salt containing a cyclic anion, which can suppress the deterioration of battery performance at high temperatures by contributing to the negative electrode SEI, it is possible to more effectively suppress the deterioration of battery performance at high temperatures.

[0243] In addition, when comparing Example 2 and Example 3, the content of the cyclic anion-containing lithium salt is LiPF 6 The content of LiPF was within the range of 150 or less, and the 1C capacity retention rate in the -40°C output test was 30% or more, and the 20C capacity retention rate in the 25°C output test was 60% or more. This is because the organic component derived from the cyclic anion-containing lithium salt and the LiPF 6It is speculated that by forming a negative electrode SEI with an excellent balance of inorganic components derived from the lithium ion, the insertion and removal of lithium ions at room temperature and low temperature is facilitated, and the capacity degradation due to the contraction of the negative electrode SEI at low temperatures is suppressed.

[0244] In addition, when comparing Example 2 and Example 6, when the acetonitrile content was within the range of 30% or more, the 1C capacity retention rate in the -40°C output test was 30% or more, and the 20C capacity retention rate in the 25°C output test was 60% or more. This is presumably due to the increased ionic conductivity of the non-aqueous electrolyte.

[0245] In addition, when Examples 13 and 14 are compared with Example 12, the inclusion of a nitrogen-containing cyclic compound as an additive improves the remaining capacity retention rate after 100 hours and 200 hours. This is believed to be due to the suppression of the generation of complex cations consisting of transition metals and acetonitrile.

[0246] In addition, when Examples 15 to 18 are compared with Example 12, the inclusion of a silane-based compound as an additive improves the remaining capacity retention rate after 100 hours and 200 hours. This is believed to be due to the suppression of active sites (active sites of the positive electrode active material) that cause the oxidative deterioration of the non-aqueous electrolyte.

[0247] Furthermore, when comparing Example 2 with Examples 6 to 7, the content of the cyclic anion-containing lithium salt was within a range of 0.27 or less in molar ratio relative to the content of acetonitrile, and thus the 1C capacity retention rate in the -40°C output test was 30% or more, and the 20C capacity retention rate in the 25°C output test was 60% or more. This is presumably because the decrease in ion conductivity at room temperature and low temperature was effectively suppressed.

[0248] (4) Fabrication of a small non-aqueous secondary battery with a Ni-based positive electrode (4-1) Preparation of Ni-based positive electrode (4-1-1) Preparation of Ni-based positive electrode (P2) The positive electrode active material is a composite oxide of lithium, nickel, manganese and cobalt (LiNi 0.8 Mn 0.1 Co 0.1 O 2 ) was mixed with carbon black powder as a conductive assistant and polyvinylidene fluoride (PVDF) as a binder in a mass ratio of 94:3:3 to obtain a positive electrode mixture.

[0249] The obtained positive electrode mixture was mixed with N-methyl-2-pyrrolidone as a solvent to prepare a positive electrode mixture-containing slurry. The positive electrode mixture-containing slurry was applied to one side of an aluminum foil having a thickness of 20 μm to serve as a positive electrode current collector in an amount of 8.4 mg / cm. 2 The positive electrode active material layer was then coated while adjusting the density so that the density became 2.7 g / cm. 3 The positive electrode (P2) was obtained by rolling the positive electrode active material layer and the positive electrode current collector.

[0250] (4-1-2) Preparation of Ni-based positive electrode (P3) The positive electrode active material is a composite oxide of lithium, nickel, manganese and cobalt (LiNi 0.5 Mn 0.3 Co 0.2 O 2 ) was mixed with carbon black powder as a conductive assistant and polyvinylidene fluoride (PVDF) as a binder in a mass ratio of 94:3:3 to obtain a positive electrode mixture.

[0251] The obtained positive electrode mixture was mixed with N-methyl-2-pyrrolidone as a solvent to prepare a positive electrode mixture-containing slurry. The positive electrode mixture-containing slurry was applied to one side of an aluminum foil having a thickness of 20 μm to serve as a positive electrode current collector in an amount of 10.2 mg / cm. 2 The positive electrode active material layer was then coated while adjusting the density so that the density became 2.8 g / cm. 3 The positive electrode (P3) was obtained by rolling the positive electrode active material layer and the positive electrode current collector.

[0252] (4-1-3) Preparation of Ni-based positive electrode (P4) The positive electrode active material is a composite oxide of lithium, nickel, manganese and cobalt (LiNi 0.33 Mn 0.33 Co 0.33 O 2 ) was mixed with carbon black powder as a conductive assistant and polyvinylidene fluoride (PVDF) as a binder in a mass ratio of 94:3:3 to obtain a positive electrode mixture.

[0253] The obtained positive electrode mixture was mixed with N-methyl-2-pyrrolidone as a solvent to prepare a positive electrode mixture-containing slurry. The positive electrode mixture-containing slurry was applied to one side of an aluminum foil having a thickness of 20 μm to serve as a positive electrode current collector in an amount of 11.4 mg / cm. 2 The positive electrode active material layer was then coated while adjusting the density so that the density became 2.7 g / cm. 3 The positive electrode (P4) was obtained by rolling the positive electrode active material layer and the positive electrode current collector.

[0254] (4-2) Preparation of negative electrode (N1) A negative electrode (N1) was prepared in the same manner as in (2-2).

[0255] (4-3) Assembly of small non-aqueous secondary batteries containing Ni-based positive electrodes The positive electrodes (P2 to P4) obtained as described above were punched out into disks with a diameter of 15.958 mm, and the negative electrodes (N1) obtained as described above were punched out into disks with a diameter of 16.156 mm. These were then sandwiched between a polyethylene microporous membrane separator (film thickness 21 μm, air permeability 285 s / 100 cm 3 A laminate was obtained by laminating the laminate on both sides of a laminate (41% porosity, 41%). The laminate was inserted into a disk-shaped battery case made of SUS. Next, 200 μL of non-aqueous electrolyte (S07, S10, S20, S23 to S36) was poured into the battery case, and the laminate was immersed in the non-aqueous electrolyte. The battery case was then sealed and held at 25° C. for 12 hours, allowing the non-aqueous electrolyte to fully penetrate the laminate, thereby obtaining a small non-aqueous secondary battery.

[0256] (5) Evaluation of small non-aqueous secondary batteries containing Ni-based positive electrodes The small non-aqueous secondary batteries obtained as described above were first subjected to an initial charge / discharge treatment and an initial charge / discharge capacity measurement according to the procedure (5-1) below. Next, each small non-aqueous secondary battery was evaluated according to the procedure (5-2) below. In another evaluation, after the procedure (5-1) below, an output test was performed according to the procedure (5-3) or (5-4) below. The charge / discharge was performed using a charge / discharge device ACD-M01A (product name) manufactured by Asuka Electronics Co., Ltd. and a programmable thermostatic chamber IN804 (product name) manufactured by Yamato Scientific Co., Ltd.

[0257] In this specification, 1C means the current value at which a fully charged battery is expected to be discharged completely within one hour when discharged at a constant current.

[0258] Specifically, in a small non-aqueous secondary battery, 1C means a current value at which a battery is discharged from a fully charged state of 4.2 V to 3.0 V at a constant current, with the discharge expected to be completed in one hour. The small non-aqueous secondary battery assembled according to the procedure in (4-3) above is a 3 mAh class cell, with the battery voltage in a fully charged state set to 4.2 V and the current value equivalent to 1 C set to 3.0 mA. Hereinafter, unless otherwise specified, the notation of current value and voltage will be omitted for convenience.

[0259] (5-1) Initial charge / discharge process The ambient temperature of the small non-aqueous secondary battery was set to 25°C, and the battery was charged at a constant current equivalent to 0.1C until it reached a fully charged state, i.e., 4.2V, and then charged at a constant voltage for 1.5 hours. The battery was then discharged to 3.0V at a constant current equivalent to 0.1C. The initial efficiency was calculated by dividing the discharge capacity at this time by the charge capacity. The discharge capacity at this time was also taken as the initial capacity. Thereafter, in order to stably form the negative electrode SEI, the same charge and discharge as above was performed twice.

[0260] (5-2) 50℃ cycle test The small non-aqueous secondary battery that had been subjected to the initial charge / discharge treatment according to the method described in (5-1) above was charged at an ambient temperature of 50°C at a constant current of 1.5mA equivalent to 0.5C until the battery voltage reached 4.2V, and then charged at a constant voltage of 4.2V for 1.5 hours. The battery was then discharged at a constant current of 1.5mA equivalent to 0.5C until the battery voltage reached 3.0V. This process of charging and discharging once each constituted one cycle, and 100 cycles of charging and discharging were performed. The 50°C cycle capacity retention rate was calculated based on the following formula. 50℃ cycle capacity retention rate = (discharge capacity at 100th cycle in 50℃ cycle test / discharge capacity at 1st cycle in 50℃ cycle test) × 100[%]

[0261] The initial efficiency indicates the ratio of the initial discharge capacity to the initial charge capacity, but is generally lower than the charge / discharge efficiency from the second time onwards. This is because Li ions are used during the initial charge to form the negative electrode SEI. This results in fewer Li ions being able to be discharged. Here, there is no problem if the initial efficiency is 84% ​​or higher.

[0262] The 50°C cycle capacity retention rate is an index of battery deterioration due to repeated use. The higher this value, the less capacity loss due to repeated use, and the more suitable the battery is for long-term use. In addition, the 50°C cycle capacity retention can be used as an index of the degree of self-discharge at high temperatures. The larger this value is, the smaller the self-discharge at high temperatures will be, and the more current the battery can be used for. Therefore, it is desirable that the 50° C. cycle capacity retention rate be 80% or more.

[0263] The evaluation results obtained are shown in Table 3.

[0264] (5-3) -40℃ Output Test The battery that had been subjected to the initial charge / discharge treatment according to the method described in (5-1) above was charged at a constant current of 3 mA, which corresponds to 1 C, to 4.2 V, and then charged at a constant voltage of 4.2 V for a total of 1.5 hours. Then, it was discharged to 3.0 V at a current value of 0.3 mA, which corresponds to 0.1 C. Next, the battery was set at an ambient temperature of 25 ° C., charged at a constant current of 3 mA, which corresponds to 1 C, to 4.2 V, and then charged at a constant voltage of 4.2 V for a total of 1.5 hours. Then, the battery was set at an ambient temperature of -40 ° C., and discharged to 3.0 V at a current value of 3 mA, which corresponds to 1 C, to calculate the capacity retention rate below. 1C capacity retention rate = (Capacity at 1C discharge at -40℃ / Capacity at 0.1C discharge at 25℃) x 100 [%]

[0265] The 1C capacity retention rate is an index of output performance at -40°C. The larger this value is, the smaller the internal resistance of the nonaqueous secondary battery at low temperatures is, and the more current can be used. In a nonaqueous secondary battery containing a Ni-based positive electrode, the 1C capacity retention rate is preferably 5% or more, and more preferably 10% or more. The results of the -40°C output test are shown in Table 3.

[0266] (5-4) 25℃ Output Test The battery that had been initially charged and discharged by the method described in (5-1) above was charged at a constant current of 3 mA, equivalent to 1 C, to 4.2 V, and then charged at a constant voltage of 4.2 V for a total of 1.5 hours. It was then discharged to 3.0 V at a current value of 0.3 mA, equivalent to 0.1 C. Next, the same charge and discharge as above was performed, except that the current value during constant current discharge was changed to 60 mA, equivalent to 20 C, and the capacity retention rate was calculated as follows. 20C capacity retention rate = (capacity when discharging at 20C / capacity when discharging at 0.1C) x 100 [%]

[0267] The 20C capacity retention rate is an index of output performance at 25°C. The larger this value is, the smaller the internal resistance of the nonaqueous secondary battery is, and the more current can be used. In a nonaqueous secondary battery containing a Ni-based positive electrode, the 20C capacity retention rate is preferably 10% or more, and more preferably 20% or more. The results of the 25°C output test are shown in Table 3.

[0268] [Table 3]

[0269] As shown in Table 3, in Examples 19 to 31, the initial efficiency was equal to or higher than the preferable value.

[0270] Furthermore, in Examples 19 to 31, the 50° C. cycle capacity retention in the 50° C. cycle test was greater than or equal to a preferable value, whereas in Comparative Examples 5 to 7, the 50° C. cycle capacity retention was less than 80%.

[0271] Furthermore, in Examples 19 to 31, the 1C capacity retention rate in the −40° C. output test was equal to or higher than the preferred value, whereas in Comparative Example 8, the 1C capacity retention rate was less than 5%.

[0272] Furthermore, in Examples 19 to 31, the 20C capacity retention rate in the output test at 25° C. was equal to or higher than the preferred value, whereas in Comparative Example 8, the 20C capacity retention rate was less than 10%.

[0273] Comparing Example 19 with Comparative Example 6, by replacing the lithium salt LiFSI with the compound represented by the above formula (1-2), the 50°C cycle capacity retention rate was 80% or more. This is thought to be because the use of a lithium salt containing a cyclic anion suppresses the positive electrode metal elution and physical peeling between the positive electrode Al current collector and the positive electrode active material, which are issues with an acetonitrile-containing electrolyte, and the decomposition product of the cyclic anion acts as a negative electrode SEI component.

[0274] In addition, when Examples 19 to 21 are compared, LiPF 6 As the amount of LiPF is reduced, the 50°C cycle capacity retention rate is improved. 6 The generation of acid components due to the thermal decomposition of acetonitrile is suppressed, and hydrogen is removed from the α-position of acetonitrile to form PF 6 It is presumed that this is because the amount of HF generated from the anions could also be reduced, resulting in minimizing the deterioration of battery performance due to corrosion of the positive electrode active material layer and the positive electrode current collector, or deterioration reactions of the electrolyte.

[0275] In addition, when comparing Example 20 and Example 21, the content of the cyclic anion-containing lithium salt is LiPF 6 The content of LiPF was within the range of 150 or less, and the 1C capacity retention rate in the -40°C output test was 10% or more, and the 20C capacity retention rate in the 25°C output test was 20% or more. This is because the organic component derived from the cyclic anion-containing lithium salt and the LiPF 6 It is speculated that by forming a negative electrode SEI with an excellent balance of inorganic components derived from the lithium ion, the insertion and removal of lithium ions at room temperature and low temperature is facilitated, and the capacity degradation due to the contraction of the negative electrode SEI at low temperatures is suppressed.

[0276] Furthermore, when comparing Example 20 and Example 25, the content of the cyclic anion-containing lithium salt was within a range of 0.79 or less in molar ratio relative to the content of acetonitrile, and thus the 1C capacity retention rate in the -40°C output test was 10% or more, and the 20C capacity retention rate in the 25°C output test was 20% or more. This is presumably because the decrease in ion conductivity at room temperature and low temperature was effectively suppressed.

[0277] (6) Preparation of small non-aqueous secondary batteries for 90°C storage tests (6-1) Preparation of positive electrode (P1) A positive electrode (P1) was prepared in the same manner as in (2-1).

[0278] (6-2) Preparation of negative electrode (N1) A negative electrode (N1) was prepared in the same manner as in (2-2).

[0279] (6-3) Assembly of small non-aqueous secondary batteries for evaluation at 90°C The positive electrode (P1) obtained as described above was punched out into a disk shape having a diameter of 15.958 mm, and the negative electrode (N1) obtained as described above was punched out into a disk shape having a diameter of 16.156 mm. The disks were then sandwiched between a polyethylene microporous membrane separator (film thickness 21 μm, air permeability 285 s / 100 cm 3 A laminate was obtained by stacking the positive electrode current collector on both sides of a non-aqueous electrolyte (S20, S36, S37) (porosity 41%). The laminate was inserted into a disk-shaped battery case made of SUS. Next, 200 μL of non-aqueous electrolyte (S20, S36, S37) was poured into the battery case, and the laminate was immersed in the non-aqueous electrolyte. After that, the positive electrode current collector was pressed with an aluminum plunger, and the battery case was sealed and held at 25° C. for 12 hours, allowing the non-aqueous electrolyte to fully penetrate the laminate, and a small non-aqueous secondary battery was obtained.

[0280] (7) Evaluation of small non-aqueous secondary batteries for 90°C storage tests The small non-aqueous secondary batteries obtained as described above in (6-3) were first subjected to an initial charge / discharge treatment and an initial charge / discharge capacity measurement according to the procedure described below in (7-1). Next, each small non-aqueous secondary battery was evaluated according to the procedure described below in (7-2). The charge / discharge was performed using a charge / discharge device ACD-M01A (product name) manufactured by Asuka Electronics Co., Ltd. and a programmable thermostatic chamber IN804 (product name) manufactured by Yamato Scientific Co., Ltd.

[0281] In this specification, 1C means the current value at which a fully charged battery is expected to be discharged completely within one hour when discharged at a constant current.

[0282] Specifically, in a small non-aqueous secondary battery, 1C means a current value at which a battery is discharged from a fully charged state of 3.5 V to 2.0 V at a constant current, with the discharge expected to be completed in one hour. The small non-aqueous secondary battery assembled according to the procedure in (6-3) above is a 3 mAh class cell, the battery voltage in a fully charged state is set to 3.5 V, and the current value equivalent to 1 C is set to 3.0 mA. Hereinafter, unless otherwise specified, the notation of current value and voltage will be omitted for convenience.

[0283] (7-1) Initial charge / discharge process The ambient temperature of the small non-aqueous secondary battery was set to 25°C, and the battery was charged at a constant current equivalent to 0.1C until it reached 3.5V, after which it was charged at a constant voltage for 1.5 hours. The battery was then discharged to 2.0V at a constant current equivalent to 0.1C. The initial efficiency was calculated by dividing the discharge capacity at this time by the charge capacity. The discharge capacity at this time was also taken as the initial capacity.

[0284] (7-2) 90℃ 4-hour fully charged storage test The small non-aqueous secondary battery that had been subjected to the initial charge / discharge treatment according to the method described in (7-1) above was charged at a constant current equivalent to 1C at an ambient temperature of 25°C until it reached 3.5V, after which it was charged at a constant voltage for 1.5 hours. Next, this small non-aqueous secondary battery was stored in a thermostatic chamber at 90°C for 4 hours. After that, the ambient temperature was returned to 25°C, and the battery was discharged to 2.0V at a current value equivalent to 0.1C. The remaining discharge capacity at this time was taken as the remaining discharge capacity after 4 hours. The remaining capacity retention rate was calculated based on the following formula as the measured value of the 90°C 4-hour full charge storage test. Residual capacity maintenance rate after 4 hours = (Residual discharge capacity after 4 hours / Initial capacity) x 100[%]

[0285] The remaining capacity retention rate is an index of the degree of self-discharge in a 90°C fully charged storage test. The larger this value is, the smaller the self-discharge at high temperatures is, and the more current can be used. The remaining capacity retention rate after 4 hours of storage is preferably 85% or more, and more preferably 90% or more, and was evaluated according to the following criteria. A: 85% or more B: 75% or more but less than 85% C: Less than 75%

[0286] The results of a 90°C, 4-hour fully charged storage test are shown in Table 4.

[0287] [Table 4]

[0288] (8) Fabrication of small non-aqueous secondary batteries for evaluation at 100°C (8-1) Preparation of positive electrode (P1) A positive electrode (P1) was prepared in the same manner as in (2-1).

[0289] (8-2) Preparation of negative electrode (N1) A negative electrode (N1) was prepared in the same manner as in (2-2).

[0290] (8-3) Assembly of small non-aqueous secondary batteries The positive electrode (P1) obtained as described above was punched out into a disk shape having a diameter of 15.958 mm, and the negative electrode (N1) obtained as described above was punched out into a disk shape having a diameter of 16.156 mm. The disks were then sandwiched between a polyethylene microporous membrane separator (film thickness 21 μm, air permeability 285 s / 100 cm 3 A laminate was obtained by laminating the positive electrode collector on both sides of a non-aqueous electrolyte (S20, S36, S38, S39) (porosity 41%). The laminate was inserted into a disk-shaped battery case made of SUS. Next, 200 μL of non-aqueous electrolyte (S20, S36, S38, S39) was poured into the battery case, and the laminate was immersed in the non-aqueous electrolyte. After that, the positive electrode collector was pressed with an aluminum plunger, and the battery case was sealed and held at 25° C. for 12 hours, allowing the non-aqueous electrolyte to fully penetrate the laminate, and a small non-aqueous secondary battery was obtained.

[0291] (9) Evaluation of small non-aqueous secondary batteries for 100°C evaluation The small non-aqueous secondary batteries obtained as described above in (8-3) were first subjected to an initial charge / discharge treatment and an initial charge / discharge capacity measurement according to the procedure described below in (9-1). Next, each small non-aqueous secondary battery was evaluated according to the procedure described below in (9-2). The charge / discharge was performed using a charge / discharge device ACD-M01A (product name) manufactured by Asuka Electronics Co., Ltd. and a programmable thermostatic chamber IN804 (product name) manufactured by Yamato Scientific Co., Ltd.

[0292] In this specification, 1C means the current value at which a fully charged battery is expected to be discharged completely within one hour when discharged at a constant current.

[0293] Specifically, in a small non-aqueous secondary battery, 1C means a current value at which a battery is discharged from a fully charged state of 3.5 V to 2.0 V at a constant current, with the discharge expected to be completed in one hour.

[0294] The small nonaqueous secondary battery assembled according to the procedure in (8-3) above is a 3 mAh class cell, the battery voltage in a fully charged state is set to 3.5 V, and the current value equivalent to 1 C is set to 3.0 mA. Hereinafter, unless otherwise specified, the notation of current value and voltage will be omitted for convenience.

[0295] (9-1) Initial charge / discharge process The ambient temperature of the small non-aqueous secondary battery was set to 25°C, and the battery was charged at a constant current equivalent to 0.1C until it reached 3.5V, after which it was charged at a constant voltage for 1.5 hours. The battery was then discharged to 2.0V at a constant current equivalent to 0.1C. The initial efficiency was calculated by dividing the discharge capacity at this time by the charge capacity. The discharge capacity at this time was also taken as the initial capacity.

[0296] (9-2) 100℃ 4-hour fully charged storage test The small non-aqueous secondary battery that had been subjected to the initial charge / discharge treatment according to the method described in (9-1) above was charged at a constant current equivalent to 1C at an ambient temperature of 25°C until it reached a fully charged state, i.e., 3.5V, and then charged at a constant voltage for 1.5 hours. Next, this small non-aqueous secondary battery was stored in a thermostatic chamber at 100°C for 4 hours. After that, the ambient temperature was returned to 25°C, and the battery was discharged to 2.0V at a current value equivalent to 0.1C. The remaining discharge capacity at this time was taken as the remaining discharge capacity after 4 hours. The remaining capacity retention rate was calculated based on the following formula as the measured value of the 100°C 4-hour fully charged storage test. Residual capacity maintenance rate after 4 hours = (Residual discharge capacity after 4 hours / Initial capacity) x 100[%]

[0297] The remaining capacity retention rate is an index of the degree of self-discharge in a 100°C fully charged storage test. The larger this value is, the smaller the self-discharge at high temperatures is, and the more current can be used. The remaining capacity retention rate after 4 hours of storage is preferably 85% or more, and more preferably 90% or more, and was evaluated according to the following criteria. A: 85% or more B: 75% or more but less than 85% C: Less than 75%

[0298] The results of a 100°C, 4-hour fully charged storage test are shown in Table 5.

[0299] [Table 5]

[0300] (10) Fabrication of coin-type non-aqueous secondary batteries (10-1) Preparation of positive electrode (P5) The positive electrode active material is a composite oxide of lithium, nickel, manganese and cobalt (LiNi 0.8 Mn 0.1 Co 0.1 O 2 ) was mixed with carbon black powder as a conductive assistant and polyvinylidene fluoride (PVDF) as a binder in a mass ratio of 94:3:3 to obtain a positive electrode mixture.

[0301] The obtained positive electrode mixture was mixed with N-methyl-2-pyrrolidone as a solvent to prepare a positive electrode mixture-containing slurry. The positive electrode mixture-containing slurry was applied to one side of an aluminum foil having a thickness of 20 μm to serve as a positive electrode current collector in an amount of 16.6 mg / cm. 2 The positive electrode active material layer was then coated while adjusting the density so that the density became 2.91 g / cm. 3 The positive electrode (P5) was obtained by rolling the positive electrode active material layer and the positive electrode current collector.

[0302] (10-2) Preparation of negative electrode (N2) A negative electrode mixture was obtained by mixing graphite powder as a negative electrode active material, carbon black powder as a conductive assistant, and polyvinylidene fluoride (PVDF) as a binder in a mass ratio of 90:3:7.

[0303] The obtained negative electrode mixture was mixed with water as a solvent to prepare a negative electrode mixture-containing slurry. The slurry was applied to one side of a copper foil having a thickness of 8 μm to be used as a negative electrode current collector in an amount of 10.3 mg / cm2. 2 The negative electrode active material layer was then coated while adjusting the density so that the density became 1.36 g / cm. 3 The negative electrode (N2) was obtained by rolling the negative electrode active material layer and the negative electrode current collector.

[0304] (10-3) Assembly of coin-type non-aqueous secondary batteries A polypropylene gasket was set in a CR2032 type battery case (SUS304), and the positive electrode (P5) obtained as described above was punched into a disk shape with a diameter of 15.958 mm and set in the center with the positive electrode active material layer facing up. A glass fiber filter paper (GA-100, manufactured by Advantec Co., Ltd.) punched into a disk shape with a diameter of 16.156 mm was set on top of it, and 150 μL of non-aqueous electrolyte (S33, S34, S40) was poured, and then the negative electrode (N2) obtained as described above was punched into a disk shape with a diameter of 16.156 mm and set with the negative electrode active material layer facing down. After setting the spacer and spring, the battery cap was fitted and crimped with a crimping machine. The overflowing electrolyte was wiped off with a rag. The laminate was kept at 25 ° C for 12 hours, and the non-aqueous electrolyte was thoroughly absorbed into the laminate to obtain a coin-type non-aqueous secondary battery.

[0305] (11) Evaluation of coin-type non-aqueous secondary batteries The coin-type non-aqueous secondary battery obtained as described above in (10-3) was first subjected to an initial charge-discharge treatment and an initial charge-discharge capacity measurement according to the procedure described below in (11-1). The charge-discharge was performed using a charge-discharge device ACD-M01A (product name) manufactured by Asuka Electronics Co., Ltd. and a programmable thermostatic chamber IN804 (product name) manufactured by Yamato Scientific Co., Ltd.

[0306] Here, 1C means the current value at which a fully charged battery is expected to be discharged at a constant current to complete discharging in one hour. In the evaluation of (11-1) below, specifically, 1C means the current value at which a fully charged battery of 4.2V is discharged at a constant current to 3.0V to complete discharging in one hour.

[0307] The small non-aqueous secondary battery assembled according to the above procedure (10-3) is a 6 mAh class cell, the battery voltage in a fully charged state is set to 4.2 V, and the current value equivalent to 1 C is set to 6.0 mA. Hereinafter, unless otherwise specified, the notation of current value and voltage will be omitted for convenience.

[0308] (11-1) Initial charge / discharge process The ambient temperature of the coin-type non-aqueous secondary battery was set to 25°C, and it was charged at a constant current of 0.15mA, which corresponds to 0.025C, until it reached 3.1V, and then it was charged at a constant voltage of 3.1V for 1.5 hours. After a 3-hour pause, the battery was charged at a constant current of 0.3mA, which corresponds to 0.05C, until it reached 4.2V, and then it was charged at a constant voltage of 4.2V for 1.5 hours. The battery was then discharged to 3.0V at a constant current of 0.9mA, which corresponds to 0.15C. The initial efficiency was calculated by dividing the discharge capacity at this time by the charge capacity.

[0309] In addition, for coin-type nonaqueous secondary batteries prepared in exactly the same manner as in (10-3) above, except that the battery case was changed to SUS304 / aluminum clad to prevent corrosion of the battery exterior, the initial charge capacity was 7.20 mAh. Therefore, nonaqueous secondary batteries that showed an initial charge capacity of 1.1 times this capacity (7.92 mAh) or more were determined to have been overcharged, and no discharge treatment was performed.

[0310] (12) Analysis of metal elution after the first charge / discharge The coin-type non-aqueous secondary battery after the initial charge and discharge treatment in (11-1) above was disassembled, and the negative electrode was taken out and placed in a Teflon (registered trademark) decomposition container, and 3 mL of 68% nitric acid and 5 mL of 98% nitric acid were added and subjected to thermal decomposition at 220°C for 45 minutes (first stage reaction) using microwaves (output: 1000 W). Then, 2 mL of 68% nitric acid was added again and thermal decomposition was performed at 230°C for 40 minutes (second stage reaction) using microwaves (output: 1000 W) to make the total amount about 100 g with ultrapure water. This sample was subjected to ICP emission spectroscopy (ICP emission spectroscopy analyzer: SPS3520UV-DD (manufactured by SII Corporation)) to calculate the amount of eluted metal per negative electrode.

[0311] The elements selected for measurement were Fe, Ni, Mo, Co, and Mn, which are contained in SUS304, a component of the battery exterior.

[0312] Here, we discuss the interpretation of each test.

[0313] The initial efficiency indicates the ratio of the initial discharge capacity to the initial charge capacity, and is generally lower than the charge / discharge efficiency from the second time onwards. This is because Li ions are used during the initial charge to form the negative electrode SEI. This results in fewer Li ions being able to be discharged. Here, the initial efficiency is preferably 80% or more, more preferably 84% or more.

[0314] The amount of metal eluted from the negative electrode is an index of the amount of metal eluted from the metal exterior body during the initial charge and discharge. If this value is large, the battery performance tends to deteriorate due to overcharging or damage to the SEI of the negative electrode caused by continuous reduction and precipitation of metal ions eluted from the battery exterior body on the negative electrode side.

[0315] Table 6 shows the results of the initial charge / discharge test and the subsequent analysis of the amount of metal elution.

[0316] [Table 6]

[0317] As shown in Table 6, the initial charge-discharge efficiency was equal to or higher than the preferred value in Examples 35 and 36. On the other hand, in Comparative Example 13, overcharging occurred, so that no subsequent discharge treatment was performed.

[0318] In addition, since the amount of metal eluted from the negative electrode in Comparative Example 13 was greater than in Examples 35 and 36, it is presumed that overcharging was caused by metal ions eluted from the battery outer casing being continuously reduced and precipitated on the negative electrode side.

[0319] Next, comparing Examples 35 and 36, Example 35 has a higher initial efficiency than Example 36. This is because LiPF 6 The amount of cyclic anion-containing lithium salt / LiPF 6 It is speculated that the increase in the molar ratio of the cations in the cations in the negative electrode suppressed the deterioration of battery performance by suppressing the elution of the metal from the battery exterior or by contributing to the negative electrode SEI.

[0320] In addition, the amount of metal eluted from the negative electrode in Example 35 is smaller than that in Example 36. This is because LiPF 6 The amount of cyclic anion-containing lithium salt / LiPF 6 It is speculated that the increase in the molar ratio of the negative electrode suppressed the deterioration of battery performance due to overcharging or damage to the negative electrode SEI. [Industrial Applicability]

[0321] Since the nonaqueous electrolyte within the scope of the constituent requirements of the present invention can be used in batteries that require both excellent output characteristics, low-temperature characteristics, and high-temperature durability, the nonaqueous secondary battery using the nonaqueous electrolyte of the present invention is expected to be used as, for example, a rechargeable battery for portable devices such as mobile phones, portable audio devices, personal computers, and IC (Integrated Circuit) tags; a rechargeable battery for automobiles such as hybrid automobiles, plug-in hybrid automobiles, and electric automobiles; a low-voltage power source such as a 12V class power source, a 24V class power source, and a 48V class power source; a residential power storage system, an IoT device, etc. In addition, the nonaqueous secondary battery using the nonaqueous electrolyte of the present invention can also be used in cold regions and outdoor applications in summer. [Explanation of symbols]

[0322] 100 Nonaqueous secondary battery 110 Battery housing 120 Space in battery housing 130 Positive electrode lead body 140 Negative electrode lead body 150 positive electrode 160 negative electrode 170 Separator

Claims

1. A non-aqueous electrolyte solution containing a non-aqueous solvent and a lithium salt, The non-aqueous solvent contains acetonitrile in an amount of 3% by volume or more and 97% by volume or less based on the total amount of the non-aqueous solvent; and The lithium salt is represented by the following formula (1): 【Chemistry 1】 {In the formula, R f may be the same or different and each represents a fluorine atom or a perfluoro group having 4 or less carbon atoms. The lithium salt contains a cyclic anion represented by the formula: The nonaqueous electrolyte solution has a molar ratio of the cyclic anion-containing lithium salt represented by the formula (1) to the acetonitrile content of 0.001 to 5.

2. The cyclic anion-containing lithium salt represented by the formula (1) is represented by the following formulas (1-1) to (1-5): 【Chemistry 2】 The non-aqueous electrolyte solution according to claim 1 , comprising at least one cyclic anion-containing lithium salt represented by the formula:

3. 3. The nonaqueous electrolyte solution according to claim 1, wherein the content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.08 or more and 0.79 or less in terms of a molar ratio relative to the content of the acetonitrile.

4. The nonaqueous electrolyte solution according to any one of claims 1 to 3, wherein the content of the acetonitrile is 10% by volume or more and 66% by volume or less with respect to the total amount of the nonaqueous solvent.

5. The lithium salt is LiPF 6 and The LiPF 6 and the cyclic anion-containing lithium salt represented by the formula (1) are mixed to form LiPF 6 The nonaqueous electrolyte solution according to any one of claims 1 to 4, wherein the lithium salt is contained at a molar concentration of ≦cyclic anion-containing lithium salt.

6. The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The nonaqueous electrolyte solution according to claim 5 , wherein the molar ratio of the content of

7. The LiPF 6 The non-aqueous electrolyte solution according to claim 5 or 6, wherein the content of is less than 0.01 mol per 1 L of the non-aqueous solvent.

8. The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The nonaqueous electrolyte solution according to any one of claims 5 to 7, wherein the molar ratio of the content of

9. The lithium salt is LiPF 6 The non-aqueous electrolyte solution according to any one of claims 1 to 4, which does not contain

10. The nonaqueous electrolyte solution is a compound represented by the following formula (2): 【Chemistry 3】 {In the formula, R 1 , R 2 , and R 3 are each independently a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a fluorine-substituted alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a fluorine-substituted alkoxy group having 1 to 4 carbon atoms, a phenyl group, a cyclohexyl group, a nitrile group, a nitro group, an amino group, an N,N'-dimethylamino group, or an N,N'-diethylamino group, and two or more of these substituents are hydrogen atoms. The non-aqueous electrolyte solution according to any one of claims 1 to 9, further comprising a nitrogen-containing cyclic compound represented by the formula:

11. The nonaqueous electrolyte solution according to claim 10, wherein the content of the nitrogen-containing cyclic compound represented by the formula (2) is 0.0001 or more and 3 or less in terms of a molar ratio relative to the content of the cyclic anion-containing lithium salt represented by the formula (1).

12. The nonaqueous electrolyte solution according to claim 10 or 11, wherein the nitrogen-containing cyclic compound represented by formula (2) is one or more compounds selected from the group consisting of pyridine and 4-(tert-butyl)pyridine.

13. The content of the nitrogen-containing cyclic compound represented by the formula (2) is 0.01 mass% or more and 10 mass% or less with respect to the total amount of the nonaqueous electrolyte solution. The nonaqueous electrolyte solution according to any one of claims 10 to 12.

14. The nonaqueous electrolyte solution is a compound represented by the following general formula (3): X-Si(OR 3 ) (3-m) R 4 m ・・・・・(3) {In the formula, R 3 and R 4 represents an alkyl group which may be substituted with an aryl group, an alkoxysilyl group, or a halogen atom, or an aryl group which may be substituted with an alkyl group, an alkoxysilyl group, or a halogen atom, and X represents a group represented by the following formula (L1): 【Chemistry 4】 (wherein k is an integer from 0 to 8, and * indicates the point of attachment to Si). The following formula (L2): 【Chemistry 5】 (wherein j is an integer from 0 to 8, and * indicates the point of attachment to Si). The following formula (L3): 【Chemistry 6】 (wherein h is an integer of 0 to 8, g is an integer of 0 or 1, and * indicates the point of attachment to Si), and The following formula (L4): 【Chemistry 7】 (In the formula, * indicates the bond site with Si) and m is an integer of 0 to 2}, The following general formula (4): 【Chemistry 8】 {wherein each X independently represents at least one selected from the group consisting of groups represented by formulas (L1) to (L4), and d represents an integer of 0 to 10,000.} The following general formula (5): 【Chemistry 9】 {In the formula, R 5 each independently represents an aryl group or an alkyl group which may be substituted with a halogen atom, or an aryl group which may be substituted with an alkyl group or a halogen atom, y is an integer of 2 to 8, and X represents at least one selected from the group consisting of the groups represented by the formulas (L1) to (L4) above. The following general formula (6): X-Si(OR 3 'OR 3 ) (3-m) R 4 m ・・・・・(6) {In the formula, R 3 , R 4 , X, and m are as defined in general formula (3), and R 3 ' represents an aryl group, an alkoxysilyl group, or an alkylene group which may be substituted with a halogen atom}, The following general formula (7): 【Chemistry 10】 Compounds represented by formula (7): {in which R is each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 5 to 20 carbon atoms; X is O, S, or NH; Z is P, P=O, B, or Si; when Z is P or P=O, n1 is 1, n2 is an integer of 1 to 3, and n2+n3=3; when Z is B, n1 is 1, n2 is an integer of 1 to 3, and n2+n3=3; when Z is Si, n1 is 0, n2 is an integer of 1 to 4, and n2+n3=4.}; and The following general formula (8): 【Chemistry 11】 The nonaqueous electrolyte solution according to any one of claims 1 to 13, further comprising a polymer compound containing a repeating unit represented by the formula (8): {R in formula (8) has the same meaning as R in formula (7).}, and at least one silane compound selected from the group consisting of diphenyldialkoxysilanes.

15. The nonaqueous electrolyte solution according to claim 14, wherein the content of the silane-based compound is in a molar ratio of 0.0001 to 1.5 with respect to the content of the cyclic anion-containing lithium salt represented by formula (1).

16. The nonaqueous electrolyte solution according to claim 14 or 15, wherein the silane-based compound is at least one selected from the group consisting of triethoxyvinylsilane, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) phosphite, tris(2,2,2-trifluoroethyl) phosphite, and diphenyldimethoxysilane.

17. The non-aqueous electrolyte solution according to any one of claims 14 to 16, wherein the content of the silane-based compound is 0.01% by mass or more and 10% by mass or less with respect to the total amount of the non-aqueous electrolyte solution.

18. A non-aqueous secondary battery comprising a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, and the non-aqueous electrolyte solution according to any one of claims 1 to 17.

19. The positive electrode active material includes a lithium phosphorus metal oxide having an olivine crystal structure containing iron (Fe) atoms, The non-aqueous electrolyte solution is the content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.9 or more in terms of molar ratio with respect to the total content of the lithium salts, The lithium salt is LiPF 6 Contains The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The molar ratio of the content of The content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.08 or more and 0.27 or less in terms of molar ratio with respect to the content of the acetonitrile; and 19. The nonaqueous secondary battery according to claim 18, wherein the content of the acetonitrile is 30% by volume or more and 66% by volume or less with respect to the total amount of the nonaqueous solvent.

20. The positive electrode active material is represented by the following general formula (a t ): Li p Ni q Co r Mn s M t O u ・・・・・(a t ) {In the formula, M is at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba, and is in the ranges of 0<p<1.3, 0<q<1.2, 0<r<1.2, 0≦s<0.5, 0≦t<0.3, 0.7≦q+r+s+t≦1.2, 1.8<u<2.2, and p is a value determined by the charge / discharge state of the battery.} The lithium-containing metal oxide is represented by The non-aqueous electrolyte solution is The lithium salt is LiPF 6 Contains The content of the cyclic anion-containing lithium salt represented by the formula (1) is 6 The molar ratio of the content of The content of the cyclic anion-containing lithium salt represented by the formula (1) is 0.15 or more and 0.79 or less in terms of molar ratio with respect to the content of the acetonitrile; and 19. The nonaqueous secondary battery according to claim 18, wherein the content of the acetonitrile is 10% by volume or more and 50% by volume or less with respect to the total amount of the nonaqueous solvent.

21. The nonaqueous secondary battery according to any one of claims 18 to 20, wherein the nonaqueous secondary battery includes a battery exterior, and the battery exterior contains aluminum in at least a part of a liquid-contacting layer with the nonaqueous electrolyte on the positive electrode side.

22. The nonaqueous secondary battery according to any one of claims 18 to 20, wherein the nonaqueous secondary battery has a battery exterior, and at least a portion of the battery exterior that is in contact with the nonaqueous electrolyte on the positive electrode side is made of iron or an iron alloy.

23. 23. The non-aqueous secondary battery of claim 22, wherein the surface of the battery exterior made of iron or an iron alloy is uncoated.

24. 24. The nonaqueous secondary battery according to claim 22 or 23, wherein at least a portion of the battery exterior that is in contact with the nonaqueous electrolyte on the positive electrode side is made of the iron alloy, and the iron alloy is stainless steel (SUS).

25. The potential of the positive electrode when fully charged is Li / Li + The nonaqueous secondary battery according to any one of claims 22 to 24, having a reference potential of 5.1 V or less.

Citation Information

Patent Citations

  • Batteries containing bis(perfluoroalkylsulfonyl)imide salts and cyclic perfluoroalkylenedisulfonylimide salts

    JP1999512563A

  • Electrolyte and battery

    JP2007250191A

  • Secondary cell nonaqueous electrolyte and secondary cell

    WO2009133899A1

  • Electrolyte solution for electrical energy storage devices, and electrical energy storage device

    WO2010110388A1

  • Nonaqueous electrolyte solution for secondary battery, and secondary battery

    WO2011052605A1