Resistance spot welding method and manufacturing method for joint

A three-stage energization process for resistance spot welding improves joint strength and toughness in high-strength steel plates by regulating grain size and structure, addressing the challenge of maintaining strength with carbon contents above 0.3%.

JP7587150B2Active Publication Date: 2024-11-20NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021053809
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2021-03-26
Publication Date
2024-11-20
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing resistance spot welding methods struggle to maintain joint strength when using high-strength steel plates with carbon content exceeding 0.3%, as they result in decreased toughness and hardness in the weld zone.

Method used

A three-stage energization process is employed, involving a first energization, a non-energization period, a second energization, another non-energization period, and a final energization, with specific current and time parameters to regulate grain size and improve toughness, even with steel plates having carbon content between 0.30% and 0.70%.

Benefits of technology

This method significantly enhances joint strength and toughness, particularly in high-strength steel plates, by controlling grain size and structure through precise energization stages, resulting in improved cross-tensile strength and tensile shear strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587150000003
    Figure 0007587150000003
  • Figure 0007587150000004
    Figure 0007587150000004
  • Figure 0007587150000005
    Figure 0007587150000005
Patent Text Reader

Abstract

To provide a resistance-spot welding method and a joint manufacturing method which can substantially improve strength of a joint, even when using a plate set including steel plates whose carbon-contents are over 0.3%.SOLUTION: In the resistance-spot welding method and the joint manufacturing method, currents having a current value I1 (kA) are passed to a plate set in which carbon-contents of at least one steel plate are over 0.30% and 0.70% or less in terms of mass%, under the following condition, and the currents are not passed during time tc1 (ms) of 16 ms or more and 200 ms or less; currents having a current value I2 (kA) are passed during time t2 (ms), and the currents are not passed during time tc2 (ms); and currents having a current value I3 (kA) are passed during time t3 (ms): 0.6≤I2 / I1≤1.1, 50≤t2≤1000, 3.5×10-3×Ms2-3.3×Ms+1100<tc2≤9000, Ms(°C)=561-474×[C]-33×[Mn]-17×[Ni]-17×[Cr]-21×[Mo], 0.4≤I3 / I1≤1.0, 200≤t3.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a resistance spot welding method and a method for manufacturing a joint. [Background technology]

[0002] Spot welding is primarily used in processes such as assembling car bodies and attaching parts. In recent years, the automobile industry has been focusing on fuel efficiency and CO 2 There is an increasing demand for lighter vehicle bodies to reduce emissions and for higher vehicle body rigidity to improve collision safety. To meet these demands, there is an increasing need to use high-strength steel plates for vehicle bodies and parts. On the other hand, in order to achieve high strength steel plate, the carbon equivalent of the base material is large, and in spot welding, the weld is heated and then immediately cooled rapidly, so the weld becomes a martensite structure, and the hardness of the weld and the heat-affected zone increases and the toughness decreases.

[0003] As a method for improving the toughness of a spot weld and ensuring joint strength, a method of performing post-heating current application after main current application has been proposed. For example, as a spot welding method using two-stage current application, Patent Document 1 describes a method for spot welding high-strength steel sheets containing 0.15 mass % or more of carbon and having a tensile strength of 980 MPa or more by overlapping and spot welding, in which the spot welding process is divided into three steps: a first current application process for forming a nugget, a cooling process in which no current is applied following the first current application process, and a second current application process for softening the nugget following the cooling process. 1 , the current in the second current application step is I 2 Then, I 2 / I 1 is set to 0.5 to 0.8, and the cooling process time tc (sec) is set to tmin = 0.2 × H according to the steel plate thickness H (mm). 2 The range is 0.8×tmin or more and 2.5×tmin or less, calculated by the above formula. Also, the current application time t 2This spot welding method discloses a spot welding method in which (sec) is in the range of 0.7×tmin or more and 2.5×tmin or less, and welding is performed by increasing the electrode pressure after the cooling step compared to the electrode pressure up to the first current application step, thereby obtaining a spot welded joint.

[0004] In addition, Patent Document 2 describes a three-stage current spot welding method in which a sheet assembly of two or more overlapping steel sheets is sandwiched between a pair of electrodes and joined by applying current while applying pressure, and the current value I w (kA) is applied to the steel sheet, and then the post-tempering heat treatment process is performed by cooling the steel sheet for a cooling time t ct After cooling for 10 ms, the current I t (kA), and the current flow time t t (ms) of current is applied, 800≦t ct ...Equation (1) 0.5×I w ≦I t ≦I w ...Equation (2) 500≦t t ...Equation (3) At least one steel plate of the plate set is 0.08≦C≦0.3 (mass%), 0.1≦Si≦0.8 (mass%), 2.5≦Mn≦10.0 (mass%), P≦0.1 (mass%) and a balance consisting of Fe and unavoidable impurities. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2014 / 060848 [Patent Document 2] International Publication No. 2019 / 156073 Summary of the Invention [Problem to be solved by the invention]

[0006] Increasing the carbon content of the steel plate used for spot welding can increase the strength of the joint base material (steel plate). However, in the examples of Patent Document 1, steel plate with a C content of 0.22% or less is used, and it is desirable to use a steel plate with an even higher C content to manufacture a joint with high joint strength (toughness). Furthermore, Patent Document 2 requires the use of steel plates with a C content of 0.08 to 0.3%, and describes, as a comparative example, that when three-stage current is applied using steel plates with a C content of more than 0.3%, the joint strength decreases.

[0007] An object of the present disclosure is to provide a resistance spot welding method and a method for manufacturing a joint that can significantly improve joint strength compared to resistance spot welding using a single current, even when using a sheet assembly including steel sheets with a carbon content of more than 0.3%. [Means for solving the problem]

[0008] The gist of the present disclosure to achieve the above object is as follows. <1> A sheet assembly consisting of two or more overlapping steel sheets, including at least one steel sheet with a C content of more than 0.30% and not more than 0.70% by mass, is sandwiched between a pair of electrodes in the thickness direction and pressure is applied while a current value I 1 A first current application step of applying current at (kA); After the first current application step, a time t of 16 ms or more and 200 ms or less c1 a first de-energization step of de-energizing the After the first de-energization step, the current value I satisfies the following formula (1): 2 (kA) and the time t that satisfies the following formula (2) 2 A second current application process in which current is applied for (ms); 0.6≦I 2 / I 1 ≦1.1 (1) 50≦t 2 ≦1000 (2) After the second current application step, a time t c2 A second de-energization step in which no current is applied for (ms); 3.5×10 -3 ×Ms 2 -3.3×Ms+1100 <t c2 ≦9000 (3) Ms(℃)=561-474×[C]-33×[Mn]-17×[Ni]-17×[Cr]-21×[Mo]...(4) After the second de-energization step, the current value I satisfies the following formula (5): 3 (kA) and the time t that satisfies the following formula (6) 3 A third current application process in which current is applied for (ms); 0.4≦I 3 / I 1 ≦1.0 (5) 200≦t 3 (6) A resistance spot welding method in which the above steps are performed continuously. Ms in the formula (3) means the Ms point calculated by substituting the mass% of each element contained in the steel plates constituting the sheet assembly into [element name] in the formula (4). However, when at least two steel plates constituting the sheet assembly have different compositions, the Ms point calculated for each steel plate by the formula (4) for all steel plates constituting the sheet assembly is multiplied by the sheet thickness ratio of each steel plate to the total thickness of the sheet assembly, and the weighted average Ms point is substituted into the formula (3). <2> Of the plate set, the at least one steel plate comprises, in mass%, P content less than 0.010% is <1> The resistance spot welding method according to claim 1 . <3> Of the plate set, the at least one steel plate comprises, in mass%, P content less than 0.010% S content is 0.0100% or less, is <1> The resistance spot welding method according to claim 1 . <4> Of the plate set, the at least one steel plate comprises, in mass%, Si content is more than 0.10%, P content less than 0.010% S content is 0.0100% or less, is <1> The resistance spot welding method according to claim 1 . <5> Of the plate set, the at least one steel plate comprises, in mass%, Si content is more than 0.10%, Mn content is 15.00% or less, P content less than 0.010% S content is 0.0100% or less, is <1> The resistance spot welding method according to claim 1 . <6> <1> ~ <5> 13. A method for manufacturing a joint using the resistance spot welding method according to claim 12. Effect of the Invention

[0009] According to the present disclosure, there is provided a resistance spot welding method and a method for manufacturing a joint that can significantly improve joint strength compared to resistance spot welding using a single current, even when using a sheet assembly including steel sheets with a carbon content of more than 0.3%. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a diagram showing the relationship between the spot welding conditions applied to overlapping steel plates and the CTS (cross tensile strength) of a joint. [Diagram 2] These are SEM-EBSD analysis images of the area near the nugget after spot welding. (A) is a single current only, and (B) is a case where a second current was applied after a single current. [Diagram 3] FIG. 4 is a diagram illustrating an example of current and time in each step of the resistance spot welding method according to the present disclosure. [Figure 4] FIG. 1 is a schematic diagram showing an example of a nugget and a heat affected zone (HAZ) formed when resistance spot welding is performed on a sheet assembly in which two steel sheets are overlapped. [Diagram 5]FIG. 1 is a diagram comparing CTS when spot welding is performed by single current while changing the carbon content of steel sheets (single current CTS) with CTS when spot welding is performed by current (three-stage current) according to the present disclosure. [Figure 6] FIG. 7 is a processed view of FIG. 5, showing the rate of increase in CTS when spot welding is performed by energization according to the present disclosure (three-stage energization) relative to CTS when spot welding is performed by single energization (single-energy CTS). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment that is an example of the present disclosure will be described. In this disclosure, the "%" display of the content of each element means "mass %." In this disclosure, a numerical range expressed using "~" means a range that includes the numerical values ​​written before and after "~" as the lower and upper limits, unless otherwise specified. In addition, when the numerical values ​​written before and after "~" are followed by "more than" or "less than," the numerical range does not include these numerical values ​​as the lower or upper limit. In the numerical ranges described in stages in this disclosure, the upper or lower limit of a certain numerical range may be replaced by the upper or lower limit of another numerical range described in stages, or may be replaced by a value shown in the examples. In addition, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.

[0012] The present inventors have intensively studied a method for improving joint strength (cross tensile strength: CTS) when resistance spot welding is performed even when the C content of the steel sheet exceeds 0.30 mass%. FIG. 1 shows the relationship between the CTS of a joint in which two types of steel sheets, each having a C content of 0.34% and a P content of 0.015% (normal P material) and 0.0007% (ultra-low P material), are stacked together and resistance spot welded. The components other than the C and P contents are common to both steel sheets, namely S: 0.0008%, Si: 0.25%, and Mn: 1.25%. In addition, "single current" means that resistance spot welding was performed by one current to form a nugget in the sheet assembly, and "temper current" means that after a single current was performed to form a nugget in the sheet assembly, a post-current (temper current) equivalent to an annealing treatment to soften the nugget was performed (two-stage current). The three-stage current passing means that after a single current passing for forming a nugget, a current passing with a current value greater than that of the temper current passing was performed, and then the temper current passing was performed.

[0013] Both the single current joint and the temper current joint were made of normal P material and extremely low P material. The three-stage current joint used normal P material, but the CTS far exceeded that of extremely low P material when temper current was applied. Since the extremely low P material has a high CTS even without current application after segregation relaxation, the inventors speculated that the improvement in CTS by the three-stage current application cannot be explained only by the effect of segregation relaxation and tempering by temper current application. Therefore, in order to investigate the effect of the second stage of current passing in the three-stage current passing, the inventors cut the steel sheet after spot welding perpendicular to the sheet thickness, polished it, and observed the metal structure.

[0014] Figure 2 shows images of a nugget and its vicinity after spot welding, analyzed using SEM-EBSD. (A) shows the result when only a single current was applied, and (B) shows the result when a second current was applied for 0.1 seconds after the single current (no tempering current was applied). In (B), grain order can be seen near the edge of the nugget (near the fusion boundary) that is not seen much in (A). This is thought to be due to a change in the grain shape caused by the grains being heated again after solidification, undergoing δ transformation, and then cooled again and undergoing γ transformation, and it is believed that this grain order improves toughness and CTS.

[0015] Generally, the higher the C content, the higher the tensile strength of the steel sheet, but the toughness of the welded part decreases, resulting in a decrease in joint strength. However, the present inventors considered that not only segregation mitigation but also grain regulating is important for steel sheets with a C content of more than 0.30%. They also discovered that even for sheet assemblies including steel sheets with a C content of more than 0.30% and 0.70% or less, by performing a three-stage current application process that combines a current application process for forming a nugget under specific conditions, a current application process for grain regulating, and a current application process for tempering, the toughness of the part (near the nugget boundary within the nugget) where the most stress in the peeling direction is applied in the CTS test can be improved, and the joint strength can be significantly improved.

[0016] That is, the resistance spot welding method according to the present disclosure includes: A sheet assembly consisting of two or more overlapping steel sheets, including at least one steel sheet with a C content of more than 0.30% and not more than 0.70% by mass, is sandwiched between a pair of electrodes in the thickness direction and pressure is applied while a current value I 1 A first current application step of applying current at (kA); After the first current application step, a time t of 16 ms or more and 200 ms or less c1 a first de-energization step of de-energizing the After the first de-energization step, the current value I satisfies the following formula (1): 2 (kA) and the time t that satisfies the following formula (2) 2 A second current application process in which current is applied for (ms); 0.6≦I 2 / I 1 ≦1.1 (1) 50≦t2 ≦1000 (2) After the second current application step, a time t c2 A second de-energization step in which no current is applied for (ms); 3.5×10 -3 ×Ms 2 -3.3×Ms+1100 <t c2 ≦9000 (3) Ms(℃)=561-474×[C]-33×[Mn]-17×[Ni]-17×[Cr]-21×[Mo]...(4) After the second de-energization step, the current value I satisfies the following formula (5): 3 (kA) and the time t that satisfies the following formula (6) 3 A third current application process in which current is applied for (ms); 0.4≦I 3 / I 1 ≦1.0 (5) 200≦t 3 (6) This is done continuously. Ms in the formula (3) means the Ms point calculated by substituting the mass% of each element contained in the steel plates constituting the sheet assembly into [element name] in the formula (4). However, when at least two steel plates constituting the sheet assembly have different compositions, the Ms point calculated for each steel plate by the formula (4) for all steel plates constituting the sheet assembly is multiplied by the sheet thickness ratio of each steel plate to the total thickness of the sheet assembly, and the weighted average Ms point is substituted into the formula (3).

[0017] Fig. 3 shows an example of current and time in each step of the resistance spot welding method according to the present disclosure. The resistance spot welding method according to the present disclosure uses a sheet assembly in which two or more steel sheets are overlapped, including at least one steel sheet having a C content, in mass%, of more than 0.30% and not more than 0.70%, and performs a first current-flow step, a first non-current-flow step, a second current-flow step, a second non-current-flow step, and a third current-flow step consecutively, i.e., without any other steps in between, as shown in Fig. 3. Each step will be specifically described below.

[0018] [First energization process] First, in the first current application step, a sheet assembly in which two or more steel sheets including at least one steel sheet having a C content of more than 0.30% and not more than 0.70% by mass is sandwiched between a pair of electrodes in the sheet thickness direction and pressurized with a current value I 1 (kA) is applied.

[0019] In the first current application process, the current value I is set so that a nugget is formed by spot welding to join all the steel plates that make up the plate assembly. 1 (kA) and current application time t 1 It is preferable to set the time (ms) so as to weld the steel sheets. Fig. 4 shows an example of a nugget formed when the first current application step is performed on a sheet pair of overlapping two steel sheets. As shown in Fig. 4, current is applied between the electrodes 2A and 2B while the electrodes 2A and 2B are pressed against each other so as to sandwich the sheet pair of overlapping steel sheets 1A and 1B in the sheet thickness direction. As a result, a nugget 13 and a heat-affected zone (so-called HAZ) 14 are formed in the current-passing portion between the steel sheets 1A and 1B, and the two steel sheets are welded together. Current value I in the first current application process 1 is the current value at which the desired nugget diameter is obtained, and the thinnest steel plate in the sheet assembly is t (mm). The current application time t 1 The current may be 10t-5 to 10t+50 cycles (50Hz), for example. From the viewpoint of joint strength and avoiding the occurrence of expulsion, it is preferable to aim for a nugget diameter of 4√t or more. The nugget diameter is more preferably 5√t or more. In order to form such a nugget diameter of 5√t or more without causing expulsion, it is preferable to set an upslope of 1 cycle to 80 cycles (50Hz) before the first current application process. In addition, before the first current application process, pre-current application may be performed for 2 to 80 cycles at a current value lower than that of the first current application process. When performing upslope current application, the current value at the end of the upslope is set to the current value I 1 (kA), and the current application time of the first current application process is t 1 (ms) does not include the time taken for the upslope. The pressure of the electrodes 2A, 2B against the sheet assembly is, for example, 2000 to 8000 N so as to suppress the occurrence of expulsion and stably obtain nuggets. The pressure may be constant or may be changed during welding.

[0020] In the resistance spot welding method according to the present disclosure, at least one of the steel sheets constituting the sheet assembly may have a C content, in mass%, of more than 0.30% and 0.70% or less. Examples of such steel sheets include cold-rolled steel sheets, hot-rolled steel sheets, and hot-stamped steel sheets. In particular, hot-stamped steel sheets with a high C content are preferable. The surface of the steel sheet may be unplated, zinc-plated, or aluminum-plated. The number of steel sheets constituting the sheet assembly is not particularly limited as long as it is two or more, and may be selected according to the application of the joint to be manufactured. Hereinafter, a steel sheet having a C content of more than 0.30% and 0.70% or less in a sheet assembly according to the present disclosure (hereinafter, may be simply referred to as a "steel sheet") will be described.

[0021] C: More than 0.30% and less than 0.70% C is an element that improves the hardenability of steel and contributes to improving strength. When spot welding is performed by stacking only steel sheets with a C content of 0.3% or less, it is possible to ensure joint strength without applying the resistance spot welding method according to the present disclosure. Therefore, in the resistance spot welding method according to the present disclosure, the C content of at least one steel sheet is set to be more than 0.30%. It is preferably 0.31% or more, more preferably 0.33% or more, and even more preferably 0.35% or more. However, if the C content exceeds 0.70%, the toughness is too low and even if the resistance spot welding method according to the present disclosure is applied, only a low CTS can still be obtained, so the C content is set to 0.70% or less. The C content is preferably 0.55% or less, and more preferably 0.48% or less.

[0022] FIG. 5 is a graph comparing the CTS when the carbon content of steel sheets was changed and spot welded by single current (single current CTS) with the CTS when spot welded under the following conditions (normal condition CTS of the present invention). 1st energization process / I 1:6800A,t 1 :500ms 1st non-current process / t c1 :70ms 2nd energization process / I 2 :5800A,t 2 :250ms 2nd non-current process / t c2 :700ms 3rd energization process / I 3 :4000A,t 3 :1300ms

[0023] FIG. 6 is a graph showing the rate of increase, calculated by the following formula, of CTS when spot welding is performed by current application according to the present disclosure (invention normal condition CTS) relative to CTS when spot welding is performed by single current application (single current CTS). Rise rate [%] = [(normal condition CTS of the present invention - single current CTS) / single current CTS] x 100 [%]

[0024] As shown in Figures 5 and 6, when the C content is 0.3% or less, the improvement in CTS is small (Figure 6), but when it exceeds 0.70%, the CTS is quite low to begin with (Figure 5). Therefore, by performing three-stage current application under specific conditions on sheet assemblies including steel sheets with a C content of more than 0.3% to 0.7%, it is possible to significantly improve the CTS.

[0025] The balance other than C may be Fe and impurities, or may contain optional components instead of a portion of Fe. The impurities are, for example, components contained in raw materials such as ores and scraps, or components mixed in during the manufacturing process, and refer to components that are not intentionally contained in the steel sheet. The following describes the preferred contents of components other than C and Fe. The components described below are impurities or optional components, and the lower limit may be 0% or may exceed 0%.

[0026] P: Less than 0.010% P is an impurity and an element that causes embrittlement. If the P content is 0.010% or more, it becomes difficult to obtain sufficient joint strength, so the upper limit is preferably set to less than 0.010%, and more preferably to 0.009% or less. It should be noted that the lower the P content, the more preferable it is, but the lower the P content, the higher the deP cost. According to the resistance spot welding method of the present disclosure, even when a steel sheet with a normal P content is used, as shown in Fig. 1, it is possible to improve the CTS to a level equal to or higher than when a steel sheet with an extremely low P content is used, a nugget is formed by energizing, and then tempering is performed. Therefore, it is not necessary to significantly lower the P content of the steel sheet, and the lower limit of the P content may be 0.0005%.

[0027] S: 0.0100% or less Like P, S is an impurity and an element that causes embrittlement. S also forms coarse MnS in steel, which reduces the workability of steel and also reduces joint strength. If the S content exceeds 0.0100%, it is difficult to obtain the required joint strength, and the workability of steel decreases, so it is preferable to keep the S content at 0.0100% or less. In addition, the lower the S content, the more preferable it is. From the same viewpoint as for P, the lower limit of the S content in the steel sheet may be 0.0003%.

[0028] Si: over 0.10% Silicon is an element that increases the strength of steel through solid solution strengthening. If the silicon content is 0.10% or less, the strength of the joint decreases, so the lower limit is preferably set to more than 0.10%, and more preferably to more than 0.80%. On the other hand, if the Si content is too high, the workability and the joint strength decrease, so the upper limit may be set to 3.5% or 3.0%.

[0029] Mn: 15.00% or less Mn is an element that increases the strength of steel. If the Mn content exceeds 15.00%, the workability and joint strength are deteriorated, so the upper limit is preferably set to 15.00%. In order to ensure a good balance between the strength, workability, and joint strength of the steel plate, the Mn content is more preferably 0.5 to 7.5%. The Mn content is further preferably 1.0 to 2.5%.

[0030] Al: 3.00% or less Al is an element that has a deoxidizing effect, stabilizes ferrite, and inhibits the precipitation of cementite. Al is added for deoxidation and to control the steel structure, but Al is easily oxidized. If the Al content exceeds 3.00%, the amount of inclusions increases, reducing the workability and the strength of the joint, so it is preferable to set the Al content at 3.00% or less. In terms of ensuring workability, a more preferable upper limit is 1.2%.

[0031] N: 0.0100% or less N is an element that increases the strength of steel plate, but it also forms coarse nitrides in steel, which deteriorates the formability of the steel. If the N content exceeds 0.0100%, the deterioration of the formability of the steel and the decrease in joint strength become significant, so it is desirable to keep the N content at 0.0100% or less. From the viewpoint of increasing the cleanliness of the steel sheet, N may be 0%. From the viewpoint of reducing the production cost of N, the lower limit may be 0.0001%.

[0032] Ti: 0.30% or less Ti is an element that forms precipitates and makes the steel sheet structure fine-grained, and may be contained. In order to obtain the effect of containing Ti, it is preferable that the content is 0.001% or more. More preferably, it is 0.01% or more. On the other hand, if it is contained excessively, not only the manufacturability is reduced, cracks are generated during processing, but also the joint strength is reduced, so that the upper limit is preferably set to 0.30%, and more preferably 0.20% or less.

[0033] Nb: 0.30% or less Nb is an element that forms fine carbonitrides and suppresses the coarsening of crystal grains, and may be contained. In order to obtain the effect of containing Nb, it is preferable to contain 0.001% or more, and more preferably 0.01% or more. If contained excessively, it not only impairs toughness and makes manufacturing difficult, but also causes a decrease in joint strength, so the upper limit is preferably set to 0.30%, and more preferably 0.20% or less.

[0034] V: 0.30% or less V is an element that forms fine carbonitrides and suppresses the coarsening of crystal grains, and may be contained. In order to obtain the effect of containing it, it is preferable that it is contained in an amount of 0.001% or more, and more preferably 0.03% or more. If it is contained in an excessive amount, it not only impairs toughness and makes manufacturing difficult, but also causes a decrease in joint strength, so the upper limit is preferably set to 0.30%, and more preferably 0.25% or less.

[0035] Cr:5.00% or less Mo: 2.00% or less Cr and Mo are elements that contribute to improving the strength of steel, and may be contained. In order to obtain the effect of containing them, it is preferable that each of them is contained in an amount of 0.001% or more. More preferably, it is contained in an amount of 0.05% or more. However, if the Cr content exceeds 5.00% or the Mo content exceeds 2.00%, not only may problems occur during pickling or hot working, but also joint strength may decrease, so the upper limit of the Cr content is preferably set to 5.00% and the upper limit of the Mo content is preferably set to 2.00%.

[0036] Cu:2.00% or less Ni: 10.00% or less Cu and Ni are elements that contribute to improving the strength of steel, and may be contained. In order to obtain the effect of containing them, it is preferable that each of them is contained at 0.001% or more. More preferably, it is contained at 0.10% or more. However, if the Cu content exceeds 2.00% and the Ni content exceeds 10.00%, not only may problems occur during pickling and hot working, but also joint strength may decrease, so the upper limit of the Cu content is preferably set to 2.00% and the upper limit of the Ni content is preferably set to 10.00%.

[0037] Ca:0.0030% or less REM: 0.050% or less Mg: 0.05% or less Zr: 0.05% or less Ca, REM (rare earth metal), Mg, and Zr are elements that refine oxides after deoxidation and sulfides present in hot-rolled steel sheets, and contribute to improving formability, and may be contained. However, if the Ca content exceeds 0.0030%, the REM content exceeds 0.050%, and each of the Mg and Zr contents exceeds 0.05%, the workability of the steel decreases. Therefore, it is preferable to set the upper limit of the Ca content to 0.0030%, the upper limit of the REM content to 0.050%, and the upper limit of each of the Mg and Zr contents to 0.05%. In order to obtain the effects of each of these elements, it is preferable that the Ca content be 0.0005% or more, the REM content be 0.001% or more, the Mg content be 0.001% or more, and the Zr content be 0.001% or more.

[0038] In addition, "REM" is a general term for 17 elements in total, including Sc, Y, and lanthanides, and the REM content refers to the total content of one or more REM elements. REM is generally contained in misch metal. For this reason, for example, REM may be contained in the form of misch metal so that the total REM content falls within the above range.

[0039] B: 0.0200% or less B is an element that segregates at grain boundaries to increase grain boundary strength, and may be contained. In order to obtain the effect of containing B, it is preferable that B is contained in an amount of 0.0001% or more, and more preferably 0.0008% or more. On the other hand, if it is contained in an excessive amount, it not only impairs toughness and makes manufacturing difficult, but also causes a decrease in joint strength, so that the upper limit is preferably set to 0.0200%, and more preferably 0.010% or less.

[0040] In the resistance spot welding method according to the present disclosure, at least one of the steel plates in a sheet set in which two or more steel plates are overlapped has a C content, by mass%, of more than 0.30% and not more than 0.70%, and preferably a steel plate having a composition within the above-mentioned range is used by selecting desired elements from the elements described above. As steel sheet components, C: More than 0.30%~0.70%, Si: more than 0.10%, Mn: 15.00% or less, P: less than 0.010%, S: 0.0100% or less, Al: 3.00% or less, and N: 0.0100% or less, including The balance of the steel sheet may be iron (Fe) and impurities. The steel sheet having the above composition contains, instead of a part of the iron (Fe), Ti: 0.30% or less, Nb: 0.30% or less, V: 0.30% or less, Cr:5.00% or less, Mo: 2.00% or less Cu: 2.00% or less, Ni: 10.00% or less, Ca: 0.0030% or less, REM: 0.050% or less, Mg: 0.05% or less, Zr: 0.05% or less, and B: 0.0200% or less It may contain one or more elements from the group consisting of: The C content of all of the steel plates constituting the sheet assembly may be more than 0.30% and 0.70% or less, or the C content of some of the steel plates in the sheet assembly may be 0.30% or less or more than 0.70%.

[0041] The thickness of the steel plates constituting the plate assembly is not particularly limited, but may be, for example, 0.5 to 3.5 mm. The total thickness t of the plate assembly is not particularly limited, but may be, for example, 1.5 to 8.0 mm.

[0042] [1st non-current process] Time t of 16ms or more and 200ms or less after the first energization process c1 is assumed to be unpowered. No-power time t c1 If the de-energization time t is less than 16 ms, the nugget edge may not solidify before the second current application process. c1 If the time exceeds 200 ms, there is a risk that the edge of the nugget will solidify excessively before the second current application process. In order to avoid the second current application process when the nugget edge is insufficiently or excessively solidified and to appropriately solidify the nugget edge, the current-free time t c1 is set to 16 ms or more and 200 ms or less, preferably 25 ms or more and 160 ms or less, and more preferably 30 ms or more and 150 ms or less.

[0043] [Second energization process] The second current passing step is an important step that the inventors discovered can improve the CTS even if the C content of the steel sheet exceeds 0.3%. This step has the effect of regulating the grain size of the crystal grains near the fusion boundary in the nugget and improving the toughness of the part where the stress applied in the peeling direction is the highest in the CTS test. After the first de-energization step, the current value I satisfies the following formula (1). 2 (kA) and the time t that satisfies the following formula (2) 2 Power is applied in (ms). 0.6≦I 2 / I 1 ≦1.1 (1) 50≦t 2 ≦1000 (2) In the second current application process, the current value (I 1 ) to the ratio (I 2 / I 1 ) and current application time (t 2 ) are energized under the conditions that satisfy the above formulas (1) and (2), respectively. The second current application process corresponds to a grain control heat treatment, and the current value I2 (kA) and time t 2 By passing an electric current at (ms), the crystal grains of the nugget change, improving the joint strength. I 2 / I 1 is 0.75~1.05, t 2 is preferably 200 to 600.

[0044] [Second non-current process] After the second current application step, a time t that satisfies the following formula (3) and the following formula (4) c2 (ms) is when no current is applied. 3.5×10 -3 ×Ms 2 -3.3×Ms+1100 <t c2 ≦9000 (3) Ms(℃)=561-474×[C]-33×[Mn]-17×[Ni]-17×[Cr]-21×[Mo]...(4) Ms in formula (3) means the Ms point calculated by substituting the mass% of each element contained in the steel plates constituting the sheet assembly into [element name] in formula (4). However, when at least two steel plates constituting the sheet assembly have different compositions, the plate thickness is taken into consideration, and the weighted average Ms point of the value obtained by multiplying the Ms point calculated for each steel plate by formula (4) for all steel plates constituting the sheet assembly by the plate thickness ratio of each steel plate to the total thickness (total thickness) of the sheet assembly is substituted into formula (3). Note that, for elements in formula (4) that are not contained in the steel plates, zero is substituted.

[0045] For example, when spot welding a sheet assembly in which three steel sheets, α, β, and γ, each having a different composition, are overlapped, the Ms point (℃) calculated from the composition of each steel sheet using formula (4) is α , Ms. β , Ms. γ , the thickness of each steel plate (mm) is t α , t β , t γ If the total thickness of the plate assembly is t, the weighted average Ms point (Ms ave ) is calculated as follows: Ms ave =Msα ×(t α / t)+Ms β ×(t β / t)+Ms γ ×(t γ / t)

[0046] In the second non-energizing process, the temperature of the entire weld needs to be lowered below the Ms point in order to temper the nugget and HAZ in the next third current application process. Therefore, the required time varies depending on the composition of the steel. The Ms point was calculated using the above formula (4) to determine the time required for the temperature of the entire weld to be lowered below the Ms point, and the result was 3.5 x 10 -3 ×Ms 2 -3.3×Ms+1100 <t c2 It is necessary to do so. However, the second de-energized time t c2 If the second de-energization time t exceeds 9000 ms, the fatigue strength in cross tension may decrease. c2 Although there is a third current application process following the second current application process, it is considered that strong residual stress remains in the welded part. c2 must be less than or equal to 9000ms.

[0047] [Third energization process] After the second de-energization step, the current value I satisfies the following formula (5). 3 (kA) and the time t that satisfies the following formula (6) 3 Power is applied in (ms). 0.4≦I 3 / I 1 ≦1.0 (5) 200≦t 3 (6) The third current application process corresponds to tempering heat treatment, and the current value I 3 and current flow time t 3 The current value (I 3 ) the current value of the first current application process (I 1 ) to the ratio (I 3 / I 1 ) and current application time (t 3) satisfying the formula (5) and the formula (6), respectively, the toughness can be improved. If the current application time in the third current application step is too long, productivity will decrease, so it is preferable to set the current application time to 5000 ms or less. A downslope may be provided after the third current application step. The downslope further improves the properties of the weld by reducing cracks due to liquid metal embrittlement, reducing blowholes, and suppressing delayed fracture. When downslope current application is performed, the current value at the start of the downslope is set to the current value I in the third current application step. 3 (kA), and the current application time of the third current application process is t 3 (ms) does not include downslope time. After the third current application step, it is preferable to provide a so-called holding time during which pressure is applied but no current is applied in order to prevent cracking due to liquid metal embrittlement. The holding time is preferably 5 cycles (50 Hz) or more.

[0048] By performing resistance spot welding consisting of the above-mentioned steps on a sheet assembly in which two or more steel sheets are overlapped, including at least one steel sheet with a C content of more than 0.30% and 0.70% or less, the CTS can be significantly improved compared to when resistance spot welding is performed with a single current. In addition, with the sheet assembly described above, a TSS (tensile shear strength) that matches the nugget hardness may not be obtained with a single current. According to the present invention, the TSS can also be improved by improving the toughness of the weld. Furthermore, the delayed fracture resistance of the spot weld can also be improved by improving the toughness and softening the weld. The field of application of the resistance spot welding method according to the present disclosure is not particularly limited, but it is believed to be particularly effective in processes such as vehicle body assembly and part installation. EXAMPLES

[0049] Hereinafter, the resistance spot welding method and the method for manufacturing a joint according to the present disclosure will be described with reference to examples. However, the resistance spot welding method and the method for manufacturing a joint according to the present disclosure are not limited to these examples.

[0050] Steel sheets having the compositions shown in Table 1 were prepared, and resistance spot welding was performed under the conditions shown in Table 2 (sheet assembly, pressure, current conditions, etc.). In Table 1, even if P, S, and N were not intentionally added, the composition analysis was performed. Moreover, notations using inequality signs such as "<0.0002%" mean that the value is below the lower analytical limit. For other elements, if they are not intentionally added, "-" is entered and composition analysis was not performed. The balance is Fe and impurities. Moreover, in Table 1, values ​​for which the C content of the steel plate is 0.30% or less or exceeds 0.70% are underlined. Note that although steel plate r and steel plate s have a C content of 0.30% or less, they were prepared for use in the sheet assembly of the invention example in which they are combined with steel plates with a C content of more than 0.30% and 0.70% or less, and are not underlined.

[0051] The underlines in Table 2 mean that the requirements of this disclosure are not met. -3 ×Ms 2 -3.3×Ms+1100" and "single current CTS" refers to the value calculated by the first current (I 1 ,t 1 ) only. The rate of increase was compared with this single-current CTS, and anything exceeding 10% was judged to have an effect of improving joint strength. Rise rate [%] = [(CTS under the current conditions disclosed herein - CTS with single current) / CTS with single current] × 100 In addition to the conditions shown in Table 2, in No. 43, an up-slope current was applied for 500 ms before the first current step, and in No. 44, a pre-current was applied with a current of 6.7 kA and a current time of 500 ms before the first current step.

[0052] [Table 1]

[0053] [Table 2]

[0054] In Nos. 1, 3 to 6, 8 to 19, and 32 to 44, resistance spot welding satisfying the conditions disclosed herein was performed on sheet assemblies in which the C content of at least one steel sheet was greater than 0.30% and less than 0.70% by mass, and in all cases the increase in CTS exceeded 10% compared to when resistance spot welding was performed using a single current. On the other hand, in Nos. 2, 7, and 20 to 31, which do not satisfy the conditions of the present disclosure, the increase rate of CTS was less than 10% compared to when resistance spot welding was performed with a single current, and in some cases the CTS actually decreased. [Explanation of symbols]

[0055] 1A, 1B steel plate 2A, 2B electrode 13. Nugget 14 Heat Affected Zone (HAZ)

Claims

1. A plate assembly in which two or more steel plates including at least one steel plate having a C content of more than 0.30% and not more than 0.70% by mass is sandwiched between a pair of electrodes in the plate thickness direction and pressurized with a current value I 1 a first current application step of applying a current at (kA) to form a nugget; After the first current application step, a time t of 16 ms or more and 200 ms or less c1 a first de-energization step of de-energizing the After the first de-energization step, a current value I satisfies the following formula (1): 2 (kA) and the time t that satisfies the following formula (2) 2 A second current application step of applying current for (ms); 0.6≦I 2 / I 1 ≦1.1 ・・・(1) 50≦t 2 ≦1000 ・・・(2) After the second current application step, a time t c2 A second de-energization step in which no current is applied for (ms); 3.5×10 -3 ×Ms 2 -3.3×Ms+1100<t c2 ≦9000 ・・・(3) Ms(℃)=561-474×[C]-33×[Mn]-17×[Ni]-17×[Cr]-21×[Mo]...(4) After the second de-energization step, the current value I satisfies the following formula (5): 3 (kA) and the time t that satisfies the following formula (6) 3 A third current application step of applying current for (ms); 0.4≦I 3 / I 1 ≦1.0 ・・・(5) 200≦t 3 ・・・(6) A resistance spot welding method in which the above steps are performed continuously. The Ms in the formula (3) means the Ms point calculated by substituting the mass% of each element contained in the steel plates constituting the plate assembly into [name of element] in the formula (4). However, when at least two steel plates constituting the plate assembly have different compositions, the Ms point calculated for each steel plate by the formula (4) for all steel plates constituting the plate assembly is multiplied by the plate thickness ratio of each steel plate to the total thickness of the plate assembly, and the weighted average Ms point is substituted into the formula (3).

2. Of the plate set, the at least one steel plate comprises, in mass%, The P content is less than 0.010%.

2. The resistance spot welding method of claim 1.

3. Of the plate set, the at least one steel plate comprises, in mass%, P content is less than 0.010%; S content is 0.0100% or less, is 2. The resistance spot welding method of claim 1.

4. Of the plate set, the at least one steel plate comprises, in mass%, The Si content is more than 0.10%, P content is less than 0.010%; S content is 0.0100% or less, is 2. The resistance spot welding method of claim 1.

5. Of the plate set, the at least one steel plate comprises, in mass%, The Si content is more than 0.10%, Mn content is 15.00% or less, P content is less than 0.010%; S content is 0.0100% or less, is 2. The resistance spot welding method of claim 1.

6. A method for manufacturing a joint using the resistance spot welding method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • After treating method for spot welding

    JP1995068388A

  • Welding method and welded structure

    JP2016055337A

  • Spot welding method

    JP2016068142A

  • Treatment methods using adenovirus

    WO2014060848A2

  • Method for resistance spot welding, and method for producing resistance-spot-welded joint

    WO2019156073A1