Galvanized steel sheets for automotive structural components
A Zn-Al-Mg-based plated steel sheet with optimized oxide layer compositions addresses corrosion resistance and lubricity issues, enhancing press formability for automotive structural members.
Patent Information
- Application Number
- JP2022575510
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-14
- Filing Date
- 2021-12-24
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2041-12-24
AI Technical Summary
Existing plated steel sheets for automobile structural members face challenges in achieving both excellent corrosion resistance and lubricity, with high manufacturing costs due to post-treatment processes and insufficient slidability from roughness improvements alone.
A Zn-Al-Mg-based plated steel sheet with controlled oxide layer compositions, specifically optimizing the ratios of Mg and Al oxides or hydroxides through XPS measurements, enhances lubricity and chemical conversion treatment properties.
The plated steel sheet achieves improved lubricity and chemical conversion treatment properties, suitable for press forming and automotive applications, while maintaining corrosion resistance.
Smart Images

Figure 0007587169000001 
Figure 0007587169000002 
Figure 0007587169000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a plated steel sheet for automobile structural members. This application claims priority based on Japanese Patent Application No. 2021-004012, filed on January 14, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, galvanized steel sheets have been used for automotive structural components from the viewpoint of rust prevention, and hot-dip galvanized steel sheets such as galvannealed steel sheets are mainly used in the Japanese domestic market. Galvannealed steel sheets are galvanized steel sheets that have been subjected to alloying heat treatment after hot-dip galvanization, and have improved weldability and corrosion resistance after painting by diffusing Fe from the steel sheet (base steel sheet) into the coating layer. However, further improvements in corrosion resistance, such as corrosion resistance after painting and red rust resistance, are required for hot-dip galvanized steel sheets.
[0003] Addition of Al to the coating layer containing Zn is one method for improving the corrosion resistance of hot-dip galvanized steel sheets. For example, hot-dip Al-Zn-coated steel sheets are widely used as highly corrosion-resistant coated steel sheets in the field of building materials. The coating layer of such hot-dip Al-Zn-coated steel sheets is formed from a dendritic α-(Zn,Al) phase (Al primary crystal part: α-(Zn,Al) phase that crystallizes as a primary crystal in the Al-Zn binary phase diagram, etc. It is not necessarily an Al-rich phase, but crystallizes as a solid solution of Zn and Al.) that is first crystallized from the molten state, and a structure (Zn / Al mixed phase structure) consisting of Zn phase and Al phase formed in the gaps of the dendritic Al primary crystal parts. Since the Al primary crystal parts are passivated and the Zn / Al mixed phase structure has a higher Zn concentration than the Al primary crystal parts, corrosion is concentrated in the Zn / Al mixed phase structure. As a result, corrosion progresses in a worm-eaten manner in the Zn / Al mixed phase structure, and the corrosion progression path becomes complex, making it difficult for corrosion to reach the underlying steel sheet. As a result, hot-dip Al-Zn coated steel sheets have superior corrosion resistance compared to hot-dip galvanized steel sheets with the same coating thickness. In order to improve corrosion resistance, studies are also being conducted on Zn-Al-Mg coated steel sheets, in which elements such as Mg are added to the Al-Zn coating.
[0004] On the other hand, plated steel sheets used in automobile structural members are required to have good workability. In particular, since press forming is performed without painting, lubrication between the die and the plated steel sheet is important. Therefore, steel sheets used in automobile structural members that undergo press forming are required to have excellent lubricity.
[0005] In response to such problems, Patent Document 1 discloses a method for forming a Zn alloy plating layer on the surface of a steel sheet, the Zn alloy plating layer containing 4 to 22 mass% Al, 1 to 5 mass% Mg, 0.1 mass% or less Ti, 0.5 mass% or less Si, with the remainder being Zn and unavoidable impurities, and then forming a base treatment layer thereon of a chromate film, a phosphate film, or a resin-based film containing a water-based resin, and then coating and drying the water-based resin with a water-based lubricating paint containing 5 to 50 mass% silica particles (b) and 1 to 40 mass% solid lubricant (c) relative to 100 mass% solid content of the water-based resin (a), to obtain a coating having a density of 0.2 to 5 g / m. 2The present invention discloses a lubricant-plated steel sheet having excellent workability, characterized in that the lubricant-plated steel sheet is formed with a coating weight of 1000g or more.
[0006] Patent Document 2 discloses a hot-dip galvanized steel sheet having a zinc plating layer containing 0.05-10 mass% Al, 0.01-5 mass% Mg as necessary, and the balance being Zn and unavoidable impurities, and characterized in that the plated steel sheet surface has a center line average roughness Ra of 0.5-1.5 μm, a PPI (the number of peaks having a size of 1.27 μm or more contained per inch (2.54 cm)) of 150-300, and a Pc (the number of peaks having a size of 0.5 μm or more contained per cm) of Pc≧PPI / 2.54+10. Patent Document 2 shows that sliding properties are improved by satisfying Pc≧PPI / 2.54+10. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 2004-338397 [Patent Document 2] Japanese Patent Publication No. 2003-13192 Summary of the Invention [Problem to be solved by the invention]
[0008] However, in Patent Document 1, a water-based lubricant coating must be applied and dried as a post-treatment after the plating process, which increases the manufacturing cost. In addition, in Patent Document 2, there is a problem that sufficient sliding properties cannot be obtained by only improving the roughness.
[0009] The present invention has been made in view of the above problems, and aims to provide a Zn-Al-Mg-plated steel sheet (a steel sheet provided with a plating containing Zn, Al, and Mg) having excellent corrosion resistance and excellent lubricity for use as an automobile structural member. [Means for solving the problem]
[0010] The present inventors have investigated methods for improving the lubricity of Zn-Al-Mg-plated steel sheets, and have found that the lubricity of a plating layer can be improved by increasing the proportion of Mg present in the plating layer as oxide [MgO] or hydroxide [Mg(OH)2]. In addition, they discovered that chemical conversion treatability can be improved by reducing the proportion of Al present in the plating layer in the form of oxide [Al2O3] or hydroxide [Al(OH)3].
[0011] The present invention has been made based on the above findings. The gist of the present invention is as follows. [1] A plated steel sheet for automobile structural members according to one embodiment of the present invention comprises a steel sheet, a plating layer formed on at least a part of a surface of the steel sheet, and an oxide layer formed on at least a part of the surface of the plating layer, wherein the plating layer contains, in mass%, Al: 0.5 to 35.0%, Mg: 0.5 to 15.0%, Si: 0 to 2.0%, Ca: 0 to 2.0%, Fe: 0 to 2.0%, La+Ce: 0 to 0.5% in total, Sb: 0 to 0.5%, Pb: 0 to 0.5%, Sr: 0 to 0.5%, Sn: 0 to 1.0%, Cu: 0 to 1.0%, A composition comprising Ti: 0-1.0%, Ni: 0-1.0%, Mn: 0-1.0%, Cr: 0-1.0%, Nb: 0-1.0%, Zr: 0-1.0%, Mo: 0-1.0%, Li: 0-1.0%, Ag: 0-1.0%, B: 0-0.5%, Y: 0-0.5%, and P: 0-0.5%, with the balance being Zn and impurities, wherein when the oxide layer is measured by XPS at a position 5.0 nm from the surface in the thickness direction, I is a ratio of the maximum detection intensity of Mg to the maximum detection intensity of an oxide or hydroxide of Mg. Mg / I MgOx is greater than or equal to 0.00 and less than or equal to 1.20. When the oxide layer is measured by XPS at a position of 5.0 nm from the surface in the thickness direction, I is a ratio of the maximum detection intensity of Al to the maximum detection intensity of the oxide or hydroxide of Al. Al / I AlOx is 0.77 or more . [2] In the plated steel sheet for automobile structural members according to the above [1], the chemical composition of the plated layer may contain, in mass%, Al: 6.0 to 30.0%, Mg: 3.0 to 11.0%. 。 [ 3 ]the above [1] or [2] The plated steel sheet for automobile structural members described in I Mg / I MgOx may be 0.00 or more and 0.80 or less. Effect of the Invention
[0012] According to the above-mentioned aspect of the present invention, it is possible to provide a plated steel sheet for automobile structural members having a coating containing Zn, Al, and Mg (Zn-Al-Mg plated steel sheet) with excellent lubricity. Moreover, according to a preferred aspect of the present invention, it is possible to provide a plated steel sheet for automobile structural members having excellent chemical conversion treatability in addition to lubricity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A plated steel sheet for automobile structural members according to one embodiment of the present invention (the plated steel sheet according to this embodiment) has a steel sheet, a plated layer formed on at least a part of the surface of the steel sheet, and an oxide layer formed on at least a part of the surface of the plated layer. The plated steel sheet according to this embodiment has a chemical composition of the plated layer, in mass %, of Al: 0.5-35.0% (preferably 6.0-30.0%), Mg: 0.5-15.0% (preferably 3.0-11.0%), Si: 0-2.0%, Ca: 0-2.0%, Fe: 0-2.0%, La+Ce: 0-0.5% in total, Sb: 0-0.5%, Pb: 0-0.5%, Sr: 0-0.5%, and the like. 0.5%, Sn: 0-1.0%, Cu: 0-1.0%, Ti: 0-1.0%, Ni: 0-1.0%, Mn: 0-1.0%, Cr: 0-1.0%, Nb: 0-1.0%, Zr: 0-1.0%, Mo: 0-1.0%, Li: 0-1.0%, Ag: 0-1.0%, B: 0-0.5%, Y: 0-0.5%, and P: 0-0.5%, with the remainder being Zn and impurities. In addition, in the plated steel sheet according to the present embodiment, when the surface layer of the oxide layer (for example, at a position 5.0 nm from the surface in the thickness direction) is measured by XPS, the ratio of the maximum detection intensity of Mg to the maximum detection intensity of the oxide or hydroxide of Mg, I Mg / I MgOx is 0.00 or more and 1.20 or less (preferably 0.00 or more and 0.80 or less). In addition, the plated steel sheet according to the present embodiment preferably has a maximum detectable intensity (I AlOx ) for the maximum detectable intensity of Al (I Al ) is the ratio of I Al / I AlOx is greater than or equal to 0.77.
[0014] <Steel plate> In the plated steel sheet according to the present embodiment, the plating layer and the oxide layer are important. Therefore, the type of steel sheet (base steel sheet) is not particularly limited and may be determined according to the product to which it is applied and the required strength, sheet thickness, etc. For example, a hot-rolled steel sheet as described in JIS G3193:2008 or a cold-rolled steel sheet as described in JIS G3141:2017 can be used.
[0015] <Plating layer> The plated steel sheet according to this embodiment has a plating layer on at least a part of the surface of the steel sheet. The plating layer may be formed on one side or both sides of the steel sheet. The coating weight of the plating layer is 15 to 250 g / m per side. 2 is preferred.
[0016] [Chemical composition] The chemical composition of the plating layer of the plated steel sheet according to this embodiment will be described below. All percentages relating to the chemical composition below are by mass percent.
[0017] Al: 0.5 to 35.0% Al is an element effective for ensuring corrosion resistance after painting in a plating layer containing aluminum (Al), zinc (Zn) and magnesium (Mg). In order to fully obtain the above effect, the Al content is set to 0.5% or more. The Al content is preferably 1.0% or more, and more preferably 6.0% or more. On the other hand, if the Al content exceeds 35.0%, the corrosion resistance after painting and the corrosion resistance of the cut end surface of the plating layer are reduced. In addition, the generation of Al oxide increases, inhibiting the generation of MgO and Mg(OH)2 in the oxide layer. Therefore, the Al content is set to 35.0% or less. The Al content is preferably 30.0% or less.
[0018] Mg: 0.5-15.0% Mg is an element that has the effect of increasing the corrosion resistance of the plating layer. In order to fully obtain this effect, the Mg content is set to 0.5% or more. The Mg content is preferably 1.0% or more, and more preferably 3.0% or more. On the other hand, if the Mg content exceeds 15.0%, the corrosion resistance after painting is reduced, and the workability of the plating layer is reduced. In addition, Mg-based compounds are formed inside the plating layer, not near the surface, which inhibits the generation of MgO and Mg(OH)2 (oxide and hydroxide) near the surface. In addition, problems in production occur, such as an increase in the amount of dross generated in the plating bath. Therefore, the Mg content is set to 15.0% or less. The Mg content is preferably 11.0% or less.
[0019] Si: 0 to 2.0% Si is an element that forms a compound with Mg and contributes to improving the post-painting corrosion resistance of the plating layer. In addition, Si is also an element that has the effect of suppressing the formation of an excessively thick alloy layer between the steel sheet and the plating layer when forming a plating layer on a steel sheet, thereby improving the adhesion between the steel sheet and the plating layer. Therefore, it may be contained. It is not necessarily required to contain Si, and the lower limit is 0%, but when obtaining the above effect, it is preferable that the Si content is 0.1% or more. On the other hand, if the Si content exceeds 2.0%, excessive Si crystallizes in the coating layer, the lamellar structure is not sufficiently formed, and the corrosion resistance after painting is reduced. In addition, the workability of the coating layer is reduced. Therefore, the Si content is set to 2.0% or less. The Si content is more preferably 1.5% or less.
[0020] Ca: 0-2.0% When Ca is contained in the coating layer, the amount of dross that is easily formed during coating operation decreases with an increase in the Mg content, improving coating manufacturability. Therefore, Ca may be contained. Ca does not necessarily have to be contained, and the lower limit is 0%, but to obtain the above effect, it is preferable that the Ca content be 0.1% or more. On the other hand, if the Ca content is excessive, the corrosion resistance after painting decreases. In addition, the corrosion resistance after painting of the flat part of the plating layer itself tends to deteriorate, and the corrosion resistance around the welded part may also deteriorate. Therefore, the Ca content is set to 2.0% or less. The Ca content is preferably 1.0% or less.
[0021] Fe: 0-2.0% When the plating layer is produced, Fe is mixed into the plating layer as an impurity from the steel sheet or the like that is the plating base material. It may be contained up to about 2.0%, but within this range, the adverse effect on the properties of the plated steel sheet according to the present embodiment is small. Therefore, the Fe content is preferably 2.0% or less. The Fe content is more preferably 1.5% or less, and further preferably 1.0% or less. On the other hand, as mentioned above, Fe is mixed into the plating layer as an impurity. Since it would be extremely costly to completely prevent the mixing of Fe, the Fe content may be set to 0.1% or more.
[0022] The chemical composition of the plating layer of the plated steel sheet according to this embodiment basically has the above-mentioned chemical composition, with the balance being Zn and impurities. However, the plating layer of the plated steel sheet according to the present embodiment may further contain, in place of a portion of Zn, for example, La, Ce, Sb, Pb, Cu, Sn, Ti, Sr, Ni, Mn, Cr, Nb, Zr, Mo, Li, Ag, B, Y, and P in the following ranges (whether intentionally added or contained as an impurity). These elements do not necessarily have to be contained, so the lower limit of the content is 0%. The total content of impurities is preferably 5.0% or less, and more preferably 3.0% or less.
[0023] La+Ce: 0-0.5% in total La and Ce are elements that contribute to improving the corrosion resistance of the plating layer. Therefore, one or both of La and Ce may be contained. It is not necessary to contain La and / or Ce, and the lower limit is 0%, but to obtain the above effect, it is preferable that the total content of La and Ce is 0.01% or more. On the other hand, if the total content of La and Ce exceeds 0.5%, the viscosity of the coating bath increases, making it difficult to prepare the coating bath itself, and it is not possible to produce a coated steel sheet with good coating properties. Therefore, the total content of La and Ce is set to 0.5% or less.
[0024] Sb: 0 to 0.5% Sr: 0-0.5% Pb: 0~0.5% When Sr, Sb, and Pb are contained in the plating layer, the appearance of the plating layer changes, spangles are formed, and an improvement in metallic luster is confirmed. Therefore, they may be contained. However, when the content of these elements exceeds 0.5%, various intermetallic compound phases are formed, and workability and corrosion resistance deteriorate. In addition, when the content of these elements is excessive, the viscosity of the plating bath increases, and the preparation of the plating bath itself often becomes difficult, making it impossible to produce a plated steel sheet with good plating properties. Therefore, the Sr content is set to 0.5% or less, the Sb content is set to 0.5% or less, and the Pb content is set to 0.5% or less.
[0025] Sn: 0-1.0% Sn is an element that increases the Mg dissolution rate in a plating layer that contains Zn, Al, and Mg. If the Mg dissolution rate increases, the corrosion resistance of the flat surface deteriorates. Therefore, the Sn content is set to 1.0% or less.
[0026] Cu: 0-1.0% Ti: 0-1.0% Ni: 0-1.0% Mn: 0-1.0% Cr: 0~1.0% Nb: 0-1.0% Zr: 0-1.0% Mo: 0-1.0% Li: 0 to 1.0% Ag: 0-1.0% B: 0 to 0.5% Y: 0 to 0.5% P: 0 to 0.5% These elements contribute to improving corrosion resistance. Therefore, they may be contained. On the other hand, if the content of these elements is excessive, the viscosity of the plating bath increases, which often makes it difficult to prepare the plating bath itself, and it is not possible to produce a plated steel sheet with good plating properties. Therefore, the content of each element is set to 1.0% or less.
[0027] The chemical composition of the plating layer is measured by the following method. First, an acid solution is obtained by peeling and dissolving the plating layer with an acid containing an inhibitor that suppresses corrosion of the base steel (steel sheet). The obtained acid solution is then measured by ICP analysis to obtain the chemical composition of the plating layer (if an alloy layer is formed between the plating layer and the steel sheet, the chemical composition will be the sum of the plating layer and the alloy layer, but since the alloy layer is thin, the effect is small). There are no particular restrictions on the type of acid, so long as it is an acid that can dissolve the plating layer. The chemical composition is measured as an average chemical composition.
[0028] [Organization] In the plated steel sheet according to the present embodiment, the plated structure is not particularly limited. According to the chemical composition of the plated layer of the plated steel sheet according to the present embodiment, the plated structure includes, for example, (Al-Zn) dendrites, a lamellar structure of an (Al-Zn) phase / MgZn2 phase, a lamellar structure of a Zn phase / MgZn2 phase, a ternary eutectic structure of Zn / Al / MgZn2, an MgZn2 phase, a dendrite or amorphous Zn phase, an Mg2Si phase, and / or other intermetallic compound phases.
[0029] <Oxide layer> The plated steel sheet according to the present embodiment has an oxide layer on at least a part of the surface of the plating layer. The oxide layer may be formed on one side or on both sides.
[0030] The present inventors have investigated methods for improving the lubricity of Zn-Al-Mg-plated steel sheets. As a result, they have found that the lubricity of a plating layer can be improved by increasing the proportion of Mg present in the plating layer as an oxide or hydroxide. Specifically, when the oxide layer was measured by XPS (X-ray photoelectron spectroscopy) at a position 5.0 nm from the surface in the thickness direction, the maximum detection intensity (I MgOx ) for Mg (metallic state) maximum detection intensity (I Mg ), I Mg / I MgOx It has been found that when the ratio is 0.00 or more and 1.20 or less, the lubricity is improved. The reason for this is unclear, but it is thought that the surface layer of the oxide layer that comes into contact with the mold, etc. Mg / I MgOx It is considered that the lubricity is improved by lowering the content of MgO (oxide of Mg) or by increasing the content of MgO (hydroxide of Mg) in the steel sheet, and that MgO or Mg(OH)2 functions as a lubricant. In terms of lubricity, both MgO and Mg(OH)2 are effective, but in the plated steel sheet according to the present embodiment, it is considered that MgO is the main component. Conventionally, MgO or Mg(OH)2 has been formed in relatively large amounts on the surface (or in a range significantly thinner than 5 nm from the surface). However, as a result of the inventors' investigations, it was found that it is important that the presence ratio of MgO (oxide of Mg) or Mg(OH)2 (hydroxide of Mg) is high at a position 5.0 nm from the surface in the thickness direction (a position obtained by removing 5.0 nm from the surface of the plating layer in the depth direction, as described later).
[0031] On the other hand, if Al2O3 (aluminum oxide) or Al(OH)3 (aluminum hydroxide) is excessively formed in the oxide layer, the chemical conversion treatability may be reduced. In order to ensure excellent chemical conversion treatability, the maximum detection intensity (I AlOx ) for the maximum detection intensity of Al (metallic state) (I Al ) is the ratio of I Al / I AlOx It is desirable that the ratio is 0.77 or more. There is no need to set an upper limit, but it is considered rare for the ratio to exceed 2.00.
[0032] I at 5.0 nm from the surface in the thickness direction of the oxide layer Mg / I MgOx , I Al / I AlOx The measurements are carried out using XPS. Specifically, the surface of the plating layer is scraped off by 5.0 nm (a range of 4.0 to 6.0 nm is acceptable) in the depth direction by argon sputtering or the like, and XPS measurement is performed at that position (a position with a depth of 5.0 nm (a range of 4.0 to 6.0 nm is acceptable)). For the XPS measurement, for example, a Quantera SXM type XPS analyzer manufactured by ULVAC-PHI, Inc. or an equivalent device is used, employing the following conditions. X-ray source: mono-Al Kα (1486.6eV) Vacuum degree: 9×10 -10 torr Ion species: Ar + Acceleration voltage: 4kV Rate: 22.7 nm / min (SiO2) As a result of the XPS measurement, the peaks in the energy range of 304 to 309 eV were considered to be peaks obtained from Mg oxide or Mg hydroxide, and the peaks in the energy range of 300 to 303 eV were considered to be peaks obtained from metallic Mg. The maximum detection intensity of each peak was measured, and the I Mg / I MgOx Calculate. I Al / I AlOx For the peaks in the energy range of 73.5 to 76.5 eV, the peaks were considered to be from Al oxide or Al hydroxide, and the peaks in the energy range of 72.0 to 73.4 eV were considered to be from metallic Al. From the maximum intensity of each peak, I Al / I AlOx Calculate.
[0033] The thickness of the oxide layer is not particularly limited, but is, for example, more than 5.0 nm and not more than 50.0 nm.
[0034] The thickness of the oxide layer is measured by the following method: XPS measurement is performed in the depth direction at a pitch of 1 to 3 nm from the surface of the plated steel sheet, and the depth at which the maximum oxygen intensity becomes 1 / 20 of the maximum intensity at the outermost surface is defined as the thickness of the oxide layer.
[0035] <Manufacturing method> Next, a preferred method for producing the plated steel sheet according to the present embodiment will be described. The plated steel sheet according to the present embodiment can obtain the effects as long as it has the above-mentioned characteristics regardless of the production method. However, the following method is preferable because it can be produced stably. Specifically, the steel sheet according to this embodiment can be produced by a production method including the following steps (I) to (III). (I) An annealing process for reducing and annealing a steel sheet; (II) A plating process in which a steel sheet is immersed in a plating bath containing Al, Mg, and Zn to produce a base sheet for plating; (III) A controlled cooling step of cooling the plated original sheet in a temperature range of from a bath temperature to 380°C at an average cooling rate of 10.0°C / sec or less in an inert gas atmosphere having a dew point of -10°C or higher, and cooling the plated original sheet in a temperature range of 380 to 100°C at an average cooling rate of 15°C / sec or more in an atmosphere having a dew point of -20°C or lower. Preferred conditions for each step will now be described.
[0036] [Annealing process] In the annealing process, prior to the plating process, reduction annealing is performed on a steel sheet (hot-rolled steel sheet or cold-rolled steel sheet) obtained by a known method. The annealing conditions may be known, for example, heating to 750 to 900°C in a 5% H2-N2 gas atmosphere with a dew point of -10°C or higher, and holding for 30 to 240 seconds.
[0037] [Plating process] In the plating step, the steel sheet is immersed in a plating bath to obtain a base sheet for plating. The plating bath preferably contains Al: 0.5 to 35.0%, Mg: 0.5 to 15.0%, Si: 0 to 2.0%, Ca: 0 to 2.0%, and the balance is Zn and impurities. The plating bath may further contain La, Ce, Fe, Sb, Pb, Cu, Sn, Ti, Sr, Ni, Mn, Cr, Nb, Li, and Ag as necessary. Since the composition of the plating bath can be estimated from the composition of the plating bath, the composition of the plating bath may be adjusted according to the chemical composition of the plating layer to be obtained.
[0038] [Controlled cooling process] In the controlled cooling process, the original steel sheet after the plating process (pulled out of the plating bath) is cooled after adjusting the coating weight with wiping gas such as N2. In the cooling process, the steel sheet pulled out of the plating bath (which has a temperature equivalent to the plating bath temperature) is cooled to 100°C or less. In this process, the average cooling rate from the bath temperature to 380°C is 10.0°C / sec or less, and the atmosphere during cooling from the bath temperature to 380°C is an inert gas atmosphere with a dew point of -10°C or more (first cooling). In addition, the average cooling rate from 380 to 100°C is 15°C / sec or more, and the dew point of the atmosphere is -20°C or less (second cooling).
[0039] If the average cooling rate to 380°C exceeds 10.0°C / s, oxidation becomes insufficient, and the oxide layer is filled with I Mg / I MgOx becomes larger. In addition, when the dew point of the atmosphere is less than -10°C, the oxide of Al is formed preferentially over MgO and Mg(OH)2, and the oxide layer is filled with I. Mg / I MgOx The formation of an oxide of Al does not contribute to improving lubricity. In addition, in order to increase the ratio of the maximum detection intensity of Al to the maximum detection intensity of the oxide or hydroxide of Al and to improve the chemical conversion treatability, it is preferable to set the atmospheric dew point to 0°C or higher. Regarding the atmosphere, although the mechanism is not entirely clear, in the air, even if the dew point is -10°C or higher, the desired oxide layer cannot be obtained. Therefore, the atmosphere is an inert gas atmosphere. The inert gas atmosphere is, for example, an N2 atmosphere, an Ar atmosphere, or a He atmosphere. However, since the inert gas alone has a low dew point (it does not reach -20°C or higher), the dew point is controlled by introducing H2O gas.
[0040] If the average cooling rate from 380 to 100°C is less than 15°C / sec, oxidation proceeds excessively, oxides such as ZnO grow, and the oxide layer becomes thin. Mg / I MgOx becomes smaller. In addition, if the dew point of the atmosphere during cooling in this temperature range exceeds -20°C, oxidation proceeds excessively, oxides such as ZnO grow, and I Mg / I MgOx becomes smaller. The starting temperature for the second cooling is preferably 380°C (it is preferable to switch the cooling rate immediately after the completion of the first cooling), but the starting temperature for the second cooling may be in the range of 380 to 330°C as long as the average cooling rate up to 100°C is less than 15°C / sec.
[0041] According to the above-described manufacturing method, the plated steel sheet according to the present embodiment can be obtained. EXAMPLES
[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0043] A cold-rolled steel sheet (0.2%C-2.0%Si-2.3%Mn) having a thickness of 1.6 mm was prepared as the steel sheet to be annealed and plated. This steel sheet was cut into a size of 100 mm×200 mm (×sheet thickness), and then annealed and hot-dipped in succession using a batch-type hot-dip galvanizing test device. The annealing was performed in a furnace with an oxygen concentration of 20 ppm or less, in an atmosphere containing 5% H2 gas and the remainder N2, with a dew point of 0°C, at 860°C for 120 seconds. After annealing, the steel sheet was air-cooled with N2 gas, and when the steel sheet temperature reached bath temperature + 20°C, it was immersed in a plating bath having a bath temperature shown in Table 1A for approximately 3 seconds. The plated original sheet on which the plating layer was formed was cooled to room temperature so that the bath temperature was 380°C or less, and the average cooling rate from 380°C to 100°C and the atmosphere (atmospheric gas, dew point) were the conditions shown in Table 1B. The temperature of the steel sheet was measured using a thermocouple spot-welded to the center of the plated original sheet. The composition of the formed plating layer is shown in Table 1.
[0044] For the obtained plated steel sheet, the thickness of the oxide layer, the I Mg / I MgOx , and I Al / I AlOx was measured. The results are shown in Table 2.
[0045] [Table 1A]
[0046] [Table 1B]
[0047] [Table 2]
[0048] [Lubricity] The obtained plated steel sheets were also subjected to a ball-on-disk test as follows to evaluate their lubricity. In this test, a 5 mm diameter SUS ball was pressed against the sample with a load P of 30 N, and the sample was rotated with a rotation radius of 10 mm and a rotation speed of 1 rpm while the load P was applied, and the load F in the direction perpendicular to the SUS ball was measured. The dynamic friction coefficient was calculated by dividing F by P when the sliding distance reached 200 mm. The dynamic friction coefficient was evaluated as follows, with AA or A being judged to have excellent lubricity. AA: Dynamic friction coefficient 0.2 or less A: Dynamic friction coefficient: over 0.2 to 0.4 B: Dynamic friction coefficient over 0.4
[0049] [Chemical conversion treatment] Furthermore, the chemical conversion treatability of the obtained plated steel sheets was evaluated in the following manner. A sample of 50 x 100 mm (x sheet thickness) was taken from the resulting plated steel sheet, and this sample was treated with zinc phosphate in accordance with the SD5350 system (standard manufactured by Nippon Paint Industrial Coating Co., Ltd.) to form a chemical conversion coating. The surface of the plated steel sheet on which the chemical conversion coating was formed was observed using an SEM to measure the percentage of incompleteness (area %) of the chemical conversion coating. In this case, the percentage of incompleteness was defined as the area ratio of the area where the steel sheet was exposed in the SEM observation field. Chemical treatability was evaluated based on the percentage of incompleteness as follows: AA: No schedule A: Less than 5%
[0050] As can be seen from Tables 1A, 1B, and 2, the invention examples Nos. 2 to 8, 10 to 13, 19 to 22, 24, and 26 to 30 have excellent lubricity. Ox Nos. 3 to 8, 10 to 13, 19 to 22, 24, 26, 28, and 29, which had large values, also had excellent chemical treatability. In contrast, in the comparative examples Nos. 1, 9, 14-18, 23, 25, 31, and 32, at least one of the chemical composition of the plating layer or the bath temperature of 380°C or the cooling condition of 380°C to 100°C was outside the preferred range, and the I Mg / I MgOx became larger and the lubricity decreased. [Industrial Applicability]
[0051] According to the present invention, it is possible to provide a Zn-Al-Mg-plated steel sheet having excellent lubricity. This steel sheet has improved press formability and can be suitably applied to automobile structural members.
Claims
1. A steel plate, A plating layer formed on at least a part of a surface of the steel sheet; an oxide layer formed on at least a portion of the surface of the plating layer; having The plating layer comprises, in mass %, Al: 0.5-35.0%, Mg: 0.5-15.0%, Si: 0-2.0%, Ca: 0-2.0%, Fe: 0-2.0%, La+Ce: 0 to 0.5% in total, Sb: 0 to 0.5%, Pb: 0 to 0.5%, Sr: 0 to 0.5%, Sn: 0 to 1.0%, Cu: 0 to 1.0%, Ti: 0 to 1.0%, Ni: 0-1.0%, Mn: 0 to 1.0%, Cr: 0-1.0%, Nb: 0 to 1.0%, Zr: 0 to 1.0%, Mo: 0 to 1.0%, Li: 0 to 1.0%, Ag: 0-1.0%, B: 0 to 0.5%, Y: 0 to 0.5%, and P: 0 to 0.5%, and the balance being Zn and impurities, When the oxide layer was measured by XPS at a position 5.0 nm from the surface in the thickness direction, the ratio of the maximum detection intensity of Mg to the maximum detection intensity of Mg oxide or hydroxide was I Mg / I MgOx is equal to or greater than 0.00 and equal to or less than 1.20, When the oxide layer is measured by XPS at a position 5.0 nm from the surface in the thickness direction, I Al / I AlOx , which is the ratio of the maximum detected intensity of Al to the maximum detected intensity of an oxide or hydroxide of Al, is 0.77 or more. Galvanized steel sheet for automotive structural components.
2. The chemical composition of the plating layer is, in mass%, Al: 6.0-30.0%, Mg: 3.0 to 11.0%, The plated steel sheet for automobile structural members according to claim 1, comprising:
3. I Mg / I MgOx is 0.00 or more and 0.80 or less; The plated steel sheet for automobile structural members according to claim 1 or 2.
Citation Information
Patent Citations
Glass fiber used for strengthening cement and like
JP1977053090A
Hot-dip galvanized steel sheet superior in formability
JP2003013192A
Non-removable coating type lubricated plated steel sheet excellent in workability