Battery unit
The battery unit employs Zn-based plated steel with inorganic or resin films and a composite joint structure to enhance corrosion resistance, addressing both coolant and external exposure issues in water-cooled battery packs, ensuring effective cooling and durability.
Patent Information
- Application Number
- JP2023503661
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-25
- Filing Date
- 2022-02-07
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2042-02-07
AI Technical Summary
Existing battery packs in electric vehicles require improved corrosion resistance for both coolant and external environments, as current technologies do not adequately address the need for high corrosion resistance in water-cooled systems exposed to external conditions.
A battery unit design using a Zn-based plated steel plate with an inorganic or resin film containing Si-based or Zr-based components, and a composite joint structure with a sealer and spot welding, enhancing both coolant and external corrosion resistance.
The design significantly improves corrosion resistance against coolant and external environments, maintaining high thermal conductivity and cooling efficiency while preventing contamination and clogging.
Smart Images

Figure 0007587183000010 
Figure 0007587183000011 
Figure 0007587183000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery unit. This application claims priority based on Japanese Patent Application No. 2021-31920 filed in Japan on March 1, 2021, and Japanese Patent Application No. 2021-87651 filed in Japan on May 25, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] In the automotive field, the shift to EVs is progressing in order to reduce CO2 emissions. Among the components used in EVs, the battery packs that house the battery cells that serve as the power source must be provided with a cooling structure to prevent battery deterioration due to temperature rise. Until now, air-cooled cooling structures have been the mainstream, but in recent years, with the increase in battery capacity, there have been an increasing number of cases where water-cooled structures with high cooling capacity are being adopted (for example, Patent Documents 1 and 2). In water-cooled battery packs, a water coolant flow path through which cooling water flows is formed on the outside of the battery pack. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-107443 A [Patent Document 2] Patent No. 6125624 Summary of the Invention [Problem to be solved by the invention]
[0004] Here, since an organic component-containing LLC (long life coolant) aqueous solution flows as the coolant in the water coolant flow path, the members constituting the water coolant flow path are required to have high corrosion resistance against the coolant (coolant corrosion resistance). In addition, when the cooling structure (specifically, the water coolant flow path) is provided outside the battery pack, the battery pack and the cooling structure are placed on the bottom surface of the automobile and are exposed to the external environment. Therefore, the members constituting the battery pack and the cooling structure are required to have corrosion resistance (external corrosion resistance) equivalent to that of the chassis of an automobile. In other words, when the outer wall portion and the cooling structure of a water-cooled battery pack are to be made of iron, the iron members are required to have high coolant corrosion resistance and external corrosion resistance. However, no technology that satisfies such conditions has been proposed so far.
[0005] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a new and improved battery unit that can improve not only corrosion resistance against coolant (coolant corrosion resistance) but also corrosion resistance against the external environment (external corrosion resistance). [Means for solving the problem]
[0006] In order to solve the above problems, according to one aspect of the present invention, there is provided a battery unit having a battery pack that houses battery cells and a water coolant flow path formed on the outside of the bottom surface of the battery pack, the water coolant flow path being made of a Zn-based plated steel sheet, an inorganic coating or a resin coating being formed on the surface of the Zn-based plated steel sheet as a chemical conversion coating, and the inorganic coating contains a Si-based component or a Zr-based component as a main component. The bottom surface of the battery pack is flat. A battery unit is provided.
[0007] Here, the distance between the water coolant flow paths may be 40 mm or less.
[0008] The bottom surface of the battery pack may be made of an Al-plated steel sheet or a processed Al sheet, and the water coolant flow path may be in direct contact with the bottom surface of the battery pack.
[0009] The water coolant flow path may be joined to a flow path upper cover made of an Al-based plated steel plate or an Al plate, and the water coolant flow path may be joined to the bottom surface of the battery pack via the flow path upper cover.
[0010] The distance between the water coolant flow paths may be 10 mm or more and 40 mm or less.
[0011] The water coolant flow paths may be spaced apart from each other by 10 mm to 40 mm, and the bottom surface of the battery pack and the water coolant flow paths may be joined by a composite joining structure of a sealer and spot welding or a sealer and mechanical joining.
[0012] The inorganic coating may also contain at least one of a V component, a P component, and a Co component as a rust-preventive component.
[0013] The rust-preventive component may be at least one of vanadium oxide, phosphoric acid, and cobalt nitrate.
[0014] The inorganic coating or resin coating may be electrically conductive.
[0015] The inorganic coating may also be composed of a compound phase containing one or more of a Si-O bond, a Si-C bond, and a Si-OH bond.
[0016] The thickness of the inorganic coating may be more than 0 μm and not more than 1.5 μm.
[0017] The resin coating may also contain a resin, an anti-rust pigment, and a conductive pigment.
[0018] The resin film contains at least one of metal particles, intermetallic compound particles, conductive oxide particles, and conductive non-oxide ceramic particles as a conductive pigment, and the conductive pigment has a powder resistivity of 185×10 at 25° C. -6The material may have a resistivity of Ωcm or less and may contain at least one element selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, Fe, and W as a constituent element.
[0019] The resin film may contain a conductive pigment in a proportion of 1.0% by mass or more and 30% by mass or less.
[0020] The resin film may have an average thickness of 1.0 μm or more and 15 μm or less.
[0021] The Zn-based plated steel sheet may be a Zn-Al-Mg plated steel sheet, and an inorganic coating containing a Si-based component as a main component may be formed on the surface of the Zn-Al-Mg plated steel sheet.
[0022] The Zn-based plated steel sheet may be a Zn-Al plated steel sheet, and a resin film may be formed on the surface of the Zn-Al plated steel sheet. Effect of the Invention
[0023] According to the above-mentioned aspects of the present invention, it is possible to provide a new and improved battery unit that can improve not only corrosion resistance against coolant (coolant corrosion resistance) but also corrosion resistance against the external environment (external corrosion resistance). [Brief description of the drawings]
[0024] [Figure 1] 1 is a cross-sectional view showing an overview of a battery unit according to an embodiment of the present invention. [Diagram 2] 11 is a cross-sectional view showing another example of the battery unit according to the present embodiment. FIG. [Diagram 3] 11 is a cross-sectional view showing another example of the battery unit according to the present embodiment. FIG. [Figure 4] 11 is a cross-sectional view showing another example of the battery unit according to the present embodiment. FIG. [Diagram 5] 11 is a cross-sectional view showing another example of the battery unit according to the present embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings. A numerical range indicated by "to" means a range including the numerical values before and after "to" as the lower and upper limits. Numerical values indicated as "greater than" or "less than" are not included in the numerical range.
[0026] <1. Overall configuration of the battery unit> First, the overall configuration of a battery unit 1 according to this embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view (a cross-sectional view perpendicular to a bottom surface portion 10a of a battery pack 10) showing an overview of a battery unit 1 according to this embodiment.
[0027] The battery unit 1 according to this embodiment is provided on the outside (below) of the bottom surface of the vehicle. Therefore, the battery unit 1 is exposed to the external environment of the vehicle. Therefore, the battery unit 1 is required to have corrosion resistance (external corrosion resistance) comparable to that of the chassis of the vehicle. Furthermore, since an aqueous solution of LLC (long life coolant) containing organic components flows as a coolant in the water coolant flow path 25 of the battery unit 1, the members constituting the water coolant flow path 25 (the bottom surface portion 10a of the battery pack 10 and the cooling structure 20) are required to have high coolant corrosion resistance.
[0028] The battery unit 1 has a battery pack 10 that houses battery cells (not shown), and a cooling structure 20 provided on the outside (below) of a bottom surface portion 10a of the battery pack 10. The battery pack 10 has a housing portion and battery cells. The cross section of the housing portion is substantially rectangular, and is divided into a bottom surface portion 10a, a side surface portion 10b, and an upper surface portion 10c. Of course, the structure of the battery pack 10 is not limited to this example.
[0029] The bottom surface portion 10a of the battery pack 10 faces and is in direct contact with a water coolant passage 25 described later. Therefore, the bottom surface portion 10a of the battery pack 10 is required to have corrosion resistance against the coolant (coolant corrosion resistance) in addition to external corrosion resistance. Therefore, in this embodiment, the bottom surface portion 10a of the battery pack 10 is made of a Zn-based plated steel sheet. The Zn-based plated steel sheet has high external corrosion resistance and coolant corrosion resistance. Therefore, the bottom surface portion 10a of the battery pack 10 has high external corrosion resistance and coolant corrosion resistance. The details of the Zn-based plated steel sheet will be described later.
[0030] The thickness of the Zn-plated steel sheet constituting the bottom surface portion 10a of the battery pack 10 is not particularly limited, but is preferably 0.2 to 1.2 mm, and more preferably 0.4 to 0.6 mm, for example. In this case, the bottom surface portion 10a of the battery pack 10 can be formed thin while maintaining the strength of the bottom surface portion 10a. Therefore, the distance between the coolant and the internal structure of the battery pack 10 can be narrowed, and the cooling efficiency of the battery pack 10 can be improved, and the cooling responsiveness of the battery pack 10 can be improved.
[0031] Although the material of the side surface portion 10b and the top surface portion 10c of the battery pack 10 is not particularly limited, it is preferable that they are also made of a Zn-based plated steel sheet similar to the bottom surface portion 10a. In particular, since the side surface portion 10b is exposed to the external environment, it is preferable that they are made of a Zn-based plated steel sheet similar to the bottom surface portion 10a. The top surface portion 10c and the side surface portion 10b are joined together via a sealer 10d. The top surface portion 10c is fixed to the bottom surface portion of the vehicle.
[0032] The cooling structure 20 is provided on the outside of the bottom surface of the battery pack 10, and has a plurality of flow path forming parts 21 and a plurality of joint parts 22. The flow path forming part 21 has a substantially rectangular cross section, and the inside is a space. This space serves as a water coolant flow path 25. The water coolant flow path 25 is in direct contact with the battery pack 10. Of course, the cross-sectional shape of the flow path forming part 21 is not limited to this example, and may be, for example, an arc shape as shown in FIG. 4, a trapezoidal shape as shown in FIG. 5, or other shapes. The water coolant flow path 25 extends in a direction perpendicular to the paper surface of FIG. 1 (for example, a direction parallel to or perpendicular to the longitudinal direction of the bottom surface part 10a of the battery pack 10), and is connected to a circulation path (not shown). Of course, the extension direction of the water coolant flow path 25 is not limited to this example, and may be, for example, curved on the bottom surface part 10a. For example, it may be U-shaped in a plan view. The coolant flows through this circulation path and the water coolant flow path 25. After being cooled in the circulation path, the cooling liquid flows through the water coolant flow path 25. The cooling liquid absorbs heat from the battery pack 10 while flowing through the water coolant flow path 25. The cooling liquid is then introduced into the circulation path again. That is, the cooling liquid repeatedly flows through the circulation path and the water coolant flow path 25, thereby repeatedly absorbing heat from the battery pack 10.
[0033] Therefore, the members constituting the water coolant passage 25, i.e., the cooling structure 20, are required to have not only the above-mentioned external corrosion resistance but also coolant corrosion resistance. Therefore, in this embodiment, the cooling structure 20 is made of a Zn-plated steel sheet. The Zn-plated steel sheet has high external corrosion resistance and coolant corrosion resistance. Therefore, the cooling structure 20 has high external corrosion resistance and coolant corrosion resistance. Furthermore, the Zn-plated steel sheet has a higher strength than an Al sheet of the same thickness. Here, the strength of the Zn-plated steel sheet is, for example, tensile strength, and can be measured by a tensile test in accordance with the provisions of JIS Z 2241. Although the Al sheet has high thermal conductivity, the Zn-plated steel sheet can be formed thin to achieve a thermal conductivity equivalent to that of the Al sheet. Therefore, in this embodiment, corrosion of the battery pack 10 and the cooling structure 20 by the coolant is suppressed, so that contamination (dissolution of components of the battery pack 10 or the cooling structure 20 into the coolant) that causes a decrease in thermal conductivity and clogging can be suppressed.
[0034] The interval between the water coolant flow paths 25, in other words, the distance w between the widthwise ends of the adjacent flow path forming parts 21, is not particularly limited, but is preferably 40 mm or less. In the example shown in FIG. 1, the cross-sectional shape of the flow path forming part 21 is substantially rectangular, so the distance w between the widthwise ends of the flow path forming part 21 can be rephrased as the distance between the side parts 21b of the flow path forming part 21. In the example shown in FIGS. 4 and 5, the boundary part between the flow path forming part 21 and the joint part 22 becomes the widthwise end of the flow path forming part 21. This allows the width of the water coolant flow path 25 to be widened, so that the contact area between the water coolant flow path 25 and the bottom part 10a, in other words, the contact area between the coolant and the battery pack 10, can be widened. When using the Zn-based plated steel sheet according to this embodiment, a particularly high cooling efficiency can be obtained by setting the interval between the water coolant flow paths 25 to 40 mm or less. Therefore, in this embodiment, the cooling efficiency of the battery pack 10 can be increased. The lower limit value of the interval between the water coolant flow paths 25 is not particularly limited, but is preferably 10 mm or more. By setting the distance between the water coolant flow paths 25 to 10 mm or more, joining by spot welding or mechanical joining means becomes possible, and it becomes easy to ensure the joining strength.
[0035] Furthermore, the ratio of the contact area between the water coolant channel 25 and the bottom surface portion 10a to the area of the bottom surface portion 10a is preferably 0.23 or more. This allows the contact area between the coolant and the battery pack 10 to be widened, and thus the cooling efficiency of the battery pack 10 to be improved. The upper limit is not particularly limited, but since it is preferable to ensure a certain degree of bonding strength between the bonding portion 22 and the bottom surface portion 10a, it may be about 0.80. From the perspective of the balance between the bonding strength and the cooling efficiency, the ratio is more preferably 0.23 to 0.71. In other words, the cooling performance of the cooling structure 20 improves as the ratio increases, but it is also preferable to consider the bonding strength with the battery pack 10. From this perspective, the ratio is preferably 0.23 to 0.71.
[0036] The height of the water coolant flow path 25, i.e., the distance h in the thickness direction of the battery unit 1 from the bottom surface portion 21a of the flow path forming portion 21 (the lower end portion 21a-1 of the flow path forming portion 21 in the example of FIG. 4) to the joint portion 22 adjacent to the flow path forming portion 21, is not particularly limited, but is preferably about 0.9 to 25.0 mm from the viewpoint of the cooling efficiency of the battery pack 10. On the other hand, from the viewpoint of the processability for forming the flow path, the upper limit of the distance h is preferably 8.0 mm. In other words, by setting the height of the water coolant flow path 25 to about 0.9 to 8.0 mm, it is possible to achieve both the cooling efficiency of the battery pack 10 and the processability for forming the flow path.
[0037] The joint 22 is a member for joining the cooling structure 20 to the battery pack 10, and is joined to the battery pack 10 via a spot weld 30. Of course, the method of joining the joint 22 to the battery pack 10 is not limited to this example. For example, the joint 22 may be joined to the battery pack 10 by a joining member such as a mechanical joint or a screw. Furthermore, as shown in FIG. 1, a sealer 35 may be used to protect the joint and improve the sealing. It is also possible to use the sealer 35 as an adhesive (that is, as an adhesive between the joint 22 and the battery pack 10). Here, examples of mechanical joining means (mechanical joining) include TOX (registered trademark) manufactured by Toxpressotechnik. Furthermore, a sealer is a coating-type organic material mainly composed of resin, which is applied to prevent the intrusion of liquids such as water (cooling liquid in the present invention) into gaps and leakage from gaps, and is also called a sealing agent. A commercially available sealer or sealing agent can be used. Furthermore, an adhesive may be used as long as it has a sealing function. The use of an adhesive is more preferable because it increases the strength of the joint. When a sealing agent having adhesive properties such as an adhesive is used, the joint strength can be secured without spot welding or mechanical joining, so it can be applied without spot welding or mechanical joining. In particular, depending on the type of plating of the steel plate constituting the battery pack 10 and the type of surface coating, the resistance during welding is large and the spot weldability is poor, so mechanical joining is preferable. In addition, the joint structure between the battery pack 10 and the cooling structure 20 is preferably a composite joint structure of a sealer and spot welding or a sealer and mechanical joining. This can increase the joint strength between the battery pack 10 and the cooling structure 20 while increasing the airtightness of the water coolant passage 25. In the example shown in Figures 1, 4, and 5, the joint structure between the battery pack 10 and the cooling structure 20 is a composite joint structure of a sealer and spot welding.
[0038] The cooling structure 20 is manufactured by processing (for example, bending, drawing, etc.) one Zn-plated steel sheet. Therefore, the cooling structure 20 can be manufactured inexpensively and easily. That is, by forming the cooling structure 20 from a Zn-plated steel sheet, the cooling structure 20 can be manufactured with higher productivity than when the cooling structure of the battery pack is formed by a die casting method, a casting method, or the like as in the past. Here, the thickness of the Zn-plated steel sheet constituting the cooling structure 20 is not particularly limited, but is preferably 0.4 to 2.0 mm, for example, and more preferably 0.5 to 1.0 mm. In this case, the strength of the cooling structure 20 can be increased while the workability of the cooling structure 20 (the workability when manufacturing the cooling structure 20) can be improved. Of course, the manufacturing method of the cooling structure 20 is not limited to this example. For example, the cooling structure 20 may be manufactured by using a different Zn-plated steel sheet for each water coolant passage 25. In this example, each Zn-based plated steel sheet is processed (for example, bending, drawing, etc.) to form flow path forming portions 21 corresponding to each water coolant flow path 25, and these are then joined to the battery pack 10.
[0039] As described above, in this embodiment, the bottom portion 10a and cooling structure 20 of the battery pack 10, which are exposed to the external environment and coolant, are made of Zn-based plated steel plate, which has excellent external corrosion resistance and coolant corrosion resistance, thereby improving the external corrosion resistance and coolant corrosion resistance of the battery unit 1.
[0040] 2 and 3 show another example of the battery unit 1. In the example shown in FIG. 2, a flow path upper cover 26 is disposed between the cooling structure 20 and the battery pack 10. The flow path upper cover 26 is made of a Zn-based plated steel sheet. In the example shown in FIG. 3, a gap filler 40 is further disposed between the flow path upper cover 26 and the battery pack 10. In addition, in FIG. 2 and FIG. 3, the flow path upper cover 26 and the gap filler 40 are drawn apart from other members in order to clarify the positional relationship between the members, but in reality, the flow path upper cover 26, the gap filler 40, and other members are joined to each other. Due to some cause (such as an error in dimensional accuracy, a complex uneven shape being formed on the surface of the bottom surface portion 10a of the battery unit 1), it may be difficult to join the bottom surface portion 10a and the cooling structure 20 (here, the flow path upper cover 26) without any gaps. In such a case, the structure shown in FIG. 3 may be adopted. The gap filler 40 is generally a resin containing a pigment with high thermal conductivity, and the heat exchange efficiency can be improved by inserting the gap filler 40 between different substances. In this embodiment, the thermal conductivity of the gap filler 40 is preferably 3.5 W / m or more, and an example of the gap filler 40 is "SDP-3540-A" manufactured by Shin-Etsu Silicone Co., Ltd. The thickness of the gap filler is preferably 0.1 mm to 8.0 mm, and more preferably 0.5 mm to 3.0 mm. As described above, when connecting the battery pack 10 and the cooling structure 20, if a gap occurs between them due to variations in dimensional accuracy, the heat exchange performance can be improved by filling the gap with the thermally conductive gap filler 40 or the like. However, the thermal conductivity of the gap filler 40 is lower than that of a Zn-based plated steel sheet, and the thickness of the gap filler 40 is preferably 0.5 mm to 3.0 mm in order to fill the gap caused by variations in dimensional accuracy of the members.
[0041] 2 and 3, the bottom surface portion 10a does not necessarily have to be made of the above-mentioned metal material, because the bottom surface portion 10a does not come into contact with the coolant.
[0042] <2. Composition of Zn-based coated steel sheets> Next, an example of the Zn-based plated steel sheet constituting the battery pack 10 and the flow passage forming portion 21 will be described in detail.
[0043] The Zn-based plated steel sheet is a steel sheet on which a plating layer containing Zn is formed. The plating layer may be formed on only one side of the steel sheet, but is preferably formed on both sides. Examples of Zn-based plated steel sheets include zinc-plated steel sheets, zinc-nickel-plated steel sheets, zinc-iron-plated steel sheets, zinc-chromium-plated steel sheets, zinc-aluminum-plated steel sheets, zinc-titanium-plated steel sheets, zinc-magnesium-plated steel sheets, zinc-manganese-plated steel sheets, zinc-aluminum (Al)-magnesium (Mg)-plated steel sheets, and zinc-aluminum-magnesium-silicon-plated steel sheets. Furthermore, Zn-based plated steel sheets containing small amounts of different metal elements or impurities such as cobalt, molybdenum, tungsten, nickel, titanium, chromium, aluminum, manganese, iron, magnesium, lead, bismuth, antimony, tin, copper, cadmium, and arsenic in the plating layer, and Zn-based plated steel sheets in which inorganic substances such as silica, alumina, and titania are dispersed can also be used. Furthermore, the above plating can be combined with other types of plating, and for example, multi-layer plating can be applied by combining it with iron plating, iron-phosphorus plating, nickel plating, cobalt plating, etc. The plating method is not particularly limited, and any of the known methods such as electroplating, hot-dip plating, vapor deposition plating, dispersion plating, and vacuum plating can be used.
[0044] Furthermore, an inorganic coating or a resin coating is formed as a chemical conversion coating on the surface (which may be only one side, but preferably both sides) of the Zn-based plated steel sheet. The inorganic coating contains a Si-based component or a Zr-based component as a main component (for example, 50 mass% or more by mass). The inorganic coating may also contain an organic component.
[0045] The inorganic film or resin film is preferably conductive. In this case, the weldability or electrodeposition paintability of the Zn-plated steel sheet can be improved. Furthermore, the inorganic film is preferably composed of a compound phase containing one or more of Si-O bonds, Si-C bonds, and Si-OH bonds. In addition, it is preferable that the compound phase contains an acrylic resin, which will be described later. When these requirements are satisfied, the adhesion of the chemical conversion coating can be improved, so that the external corrosion resistance and coolant corrosion resistance of the processed part of the Zn-plated steel sheet can be improved. In addition, it is preferable that the inorganic film contains at least one of V, P, and Co components as a rust-preventive component. The rust-preventive component of the inorganic film is preferably one or more of vanadium oxide, phosphoric acid, and Co nitrate. In addition, the thickness of the inorganic film is preferably more than 0 μm and 1.5 μm or less. In this case, the conductivity or adhesion of the above-mentioned chemical conversion coating can be further improved.
[0046] The resin film preferably contains a resin, an anti-rust pigment, and a conductive pigment. The resin film further contains at least one of metal particles, intermetallic compound particles, conductive oxide particles, and conductive non-oxide ceramic particles as a conductive pigment, and the conductive pigment has a powder resistivity of 185×10 at 25° C. -6 It is preferable that the resin film has a resistivity of Ωcm or less and contains at least one constituent element selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, Fe, and W. Furthermore, it is preferable that the resin film contains a conductive pigment in a proportion of 1.0 mass % or more and 30 mass % or less. Furthermore, it is preferable that the average thickness of the resin film is 1.0 μm or more and 15 μm or less. Furthermore, it is preferable that the average particle size of the conductive pigment is 0.5 times or more and 1.5 times or less the average thickness of the resin film. When any one or more of these requirements are satisfied, the external corrosion resistance and coolant corrosion resistance of the Zn-based plated steel sheet can be further improved.
[0047] Examples of chemical conversion coatings are listed in, for example, Japanese Patent No. 4776458, Japanese Patent No. 5336002, Japanese Patent No. 6191806, Japanese Patent No. 6263278, International Publication No. 2020 / 202461, and Japanese Patent No. 4084702. Therefore, the chemical conversion coatings listed in these publications can be suitably used as the chemical conversion coating of this embodiment. Here, an overview of the chemical conversion coating will be described.
[0048] The first example of the chemical conversion coating is an example of an inorganic coating, and is a chemical conversion coating containing an organosilicon compound (silane coupling agent) as the main component. The organosilicon compound is obtained by mixing a silane coupling agent (A) containing one amino group in the molecule and a silane coupling agent (B) containing one glycidyl group in the molecule in a solid content mass ratio [(A) / (B)] of 0.5 to 1.7. The organosilicon compound contains a group represented by the formula -SiR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 each independently represents an alkoxy group or a hydroxyl group, and at least one represents an alkoxy group), and one or more hydrophilic functional groups (b) selected from a hydroxyl group (different from those that may be contained in the functional group (a)) and an amino group, and has an average molecular weight of 1,000 to 10,000.
[0049] In the first example, the Zr-based component is contained in the chemical conversion coating as zirconium hydrofluoric acid. The V component is a vanadium compound, the P component is phosphoric acid, and the Co component is at least one selected from the group consisting of cobalt sulfate, cobalt nitrate, and cobalt carbonate. Examples of vanadium compounds include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxide, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3))2, vanadium acetylacetonate V(OC(=CH2)CH2COCH3))3, vanadium trichloride VCl3, and phosphorus vanadomolybdic acid. Also usable are pentavalent vanadium compounds reduced to tetravalent or divalent vanadium compounds by an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group.
[0050] The second example of the chemical conversion coating is an example of an inorganic coating, which is a chemical conversion coating containing an organosilicon compound (silane coupling agent) as a main component. The organosilicon compound has a cyclic siloxane structure in its structure. Here, the "cyclic siloxane bond" refers to a cyclic structure having a structure in which Si-O-Si bonds are continuous, and which is composed only of bonds between Si and O, with the number of Si-O repeats being 3 to 8.
[0051] The organosilicon compound is obtained by blending a silane coupling agent (A) containing at least one amino group in the molecule with a silane coupling agent (B) containing at least one glycidyl group in the molecule in a solid content mass ratio [(A) / (B)] of 0.5 to 1.7. The organosilicon compound (W) thus obtained contains a group represented by the formula -SiR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 each independently represents an alkoxy group or a hydroxyl group; R1 , R 2 and R 3 wherein at least one of the functional groups (a) represents an alkoxy group, and at least one hydrophilic functional group (b) selected from the group consisting of a hydroxyl group (when the functional group (a) contains a hydroxyl group, the functional group (b) is separate from the hydroxyl group) and an amino group, and the average molecular weight is preferably 1,000 to 10,000.
[0052] In the second example, the Zr-based component is contained in the chemical conversion coating as a zirconium compound. Examples of the zirconium compound include zirconium hydrofluoric acid, zirconium ammonium fluoride, zirconium sulfate, zirconium oxychloride, zirconium nitrate, and zirconium acetate. Among these, the zirconium compound is more preferably zirconium hydrofluoric acid. When zirconium hydrofluoric acid is used, better corrosion resistance and paintability can be obtained.
[0053] The V component is a vanadium compound, the P component is a phosphate compound, and the Co component is at least one selected from the group consisting of cobalt sulfate, cobalt nitrate, and cobalt carbonate, contained in the chemical conversion coating. Examples of vanadium compounds include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxide, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3)2, vanadium acetylacetonate V(OC(=CH2)CH2COCH3)3, vanadium trichloride VCl3, and phosphorus vanadomolybdic acid. Also usable is a compound obtained by reducing a pentavalent vanadium compound to a tetravalent or divalent vanadium compound using an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group.
[0054] Examples of the phosphate compound include phosphoric acid, ammonium phosphate, potassium phosphate, and sodium phosphate. Among these, the phosphate compound is preferably phosphoric acid. When phosphoric acid is used, better corrosion resistance can be obtained.
[0055] The third example of the chemical conversion coating is an example of an inorganic coating, and contains an acrylic resin, zirconium, vanadium, phosphorus, and cobalt. More specifically, the chemical conversion coating contains a particulate acrylic resin (resin particles) and an inhibitor phase. The acrylic resin is preferably a resin containing a polymer of an alkyl (meth)acrylate ester, and may be a polymer obtained by polymerizing only an alkyl (meth)acrylate ester, or may be a copolymer obtained by polymerizing an alkyl (meth)acrylate ester and another monomer. "(Meth)acrylic" means "acrylic" or "methacrylic". The inhibitor phase contains zirconium, vanadium, phosphorus, and cobalt. The zirconium forms a crosslinked structure with the acrylic resin.
[0056] The fourth example of the chemical conversion coating is an example of an inorganic coating, and includes a zirconium carbonate compound, an acrylic resin, a vanadium compound, a phosphorus compound, and a cobalt compound. Examples of the zirconium carbonate compound include zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate, and one or more of these can be used. Among these, zirconium carbonate and ammonium zirconium carbonate are preferred because of their excellent corrosion resistance.
[0057] The acrylic resin is a resin obtained by copolymerizing a monomer component containing at least styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (d4), wherein the amount of acrylonitrile (b4) is 20 to 38% by mass based on the solid content mass of all monomer components of the resin, and it is a water-soluble resin and an aqueous emulsion resin having a glass transition temperature of -12 to 15°C. That is, the acrylic resin exists in the form of resin particles in the chemical conversion treatment film.
[0058] Examples of the vanadium compound include divalent to tetravalent vanadium compounds. More specifically, for example, pentavalent vanadium compounds such as vanadium pentoxide (V2O5), metavanadic acid (HVO3), ammonium metavanadate, sodium metavanadate, and vanadium oxytrichloride (VOCl3) reduced to divalent to tetravalent with a reducing agent, vanadium trioxide (V2O3), vanadium dioxide (VO2), vanadyl sulfate (VOSO4), vanadyl oxalate [VO(COO)2], vanadium oxyacetylacetonate [VO(OC(CH3)=CHCOCH3))2], vanadium acetylacetonate [V(OC(CH3)=CHCOCH3))3], vanadium trichloride (VCl3), phosphovanadomolybdic acid {H 15-X [PV 12-x Mo x O 40 ·nH2O (6 < x < 12, n < 30)}, vanadium sulfate (VSO4·8H2O), vanadium dichloride (VCl2), vanadium compounds with an oxidation number of tetravalent to divalent such as vanadium monoxide (VO), etc. can be mentioned.
[0059] Examples of the phosphorus compound include inorganic acid anions having an acid group containing phosphorus and organic acid anions having an acid group containing phosphorus. Examples of the inorganic acid anions having an acid group containing phosphorus include inorganic acid anions in which at least one hydrogen of inorganic acids such as orthophosphoric acid, metaphosphoric acid, condensed phosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, tetraphosphoric acid, and hexametaphosphoric acid is free and salts thereof.
[0060] Examples of organic acid anions having an acid group containing phosphorus include organic acid anions having at least one free hydrogen atom, such as organic phosphonic acids such as 1-hydroxymethane-1,1-diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, 1-hydroxypropane-1,1-diphosphonic acid, 1-hydroxyethylene-1,1-diphosphonic acid, 2-hydroxyphosphonoacetic acid, aminotri(methylenephosphonic acid), ethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), hexamethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), diethylenetriamine-N,N,N',N'',N''-penta(methylenephosphonic acid), 2-phosphonic acid butane-1,2,4-tricarboxylic acid, inositol hexaphosphonic acid, and phytic acid, and organic phosphoric acid, and salts thereof.
[0061] Examples of the cobalt compound include cobalt sulfate, cobalt nitrate, and cobalt carbonate.
[0062] A fifth example of the chemical conversion coating is an example of a resin coating, and contains at least one of metal particles, intermetallic compound particles, conductive oxide particles, and conductive non-oxide ceramic particles as a conductive pigment. The conductive pigment has a powder resistivity of 185×10 at 25° C. -6 The material has a resistivity of Ωcm or less and contains at least one element selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, Fe, and W.
[0063] Examples of intermetallic compounds include ferrosilicon and ferromanganese. Examples of conductive oxide particles include materials that have conductivity by doping impurities into the crystal lattice of the oxide (doped conductive oxides) or oxides whose surfaces are modified with conductive materials. The former can be generally known metal oxides doped with one or more metal elements selected from Al, Nb, Ga, Sn, etc. (e.g., Al-doped zinc oxide, Nb-doped zinc oxide, Ga-doped zinc oxide, Sn-doped zinc oxide, etc.). The latter can be generally known zinc oxide or silica modified with SnO2, which has conductivity in the oxide. The conductive oxide is preferably a doped conductive oxide, and the doped conductive oxide is preferably Al-doped zinc oxide.
[0064] The conductive non-oxide ceramic particles are composed of ceramics made of elements or compounds that do not contain oxygen. Examples of the conductive non-oxide ceramic particles include boride ceramics, carbide ceramics, nitride ceramics, and silicide ceramics. In addition, boride ceramics, carbide ceramics, nitride ceramics, and silicide ceramics are non-oxide ceramics that have boron (B), carbon (C), nitrogen (N), and silicon (Si) as major non-metallic constituent elements, respectively, and these generally known non-oxide ceramics that contain one or more selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, and W can be used. Furthermore, the non-oxide ceramic particles are more preferably the non-oxide ceramics exemplified below in terms of the presence or absence of industrial products, stable distribution in domestic and overseas markets, price, electrical resistivity, and the like. For example, particles of Mo2B, MoB, MoB2, Mo2B5, NbB2, VB, VB2, W2B5, ZrB2, Mo2C, V2C, VC, WC, W2C, ZrC, Mo2N, VN, ZrN, Mo3Si, Mo5Si3, MoSi2, NbSi2, Ni2Si, Ta2Si, TaSi2, TiSi, TiSi2, V5Si3, VSi2, W3Si, WSi2, ZrSi, ZrSi2, CrB, CrB2, Cr3C2, Cr2N, CrSi, and particles of a mixture of two or more selected from these are more preferred.
[0065] The sixth example of the chemical conversion coating is an example of a resin coating, which contains a resin having a urethane bond and conductive particles (conductive pigments). The resin having a urethane bond is an organic resin obtained from a film-forming resin raw material that contains (a) a polyester polyol having at least three functional groups, and (b) a blocked product of an organic polyisocyanate or a blocked product of a prepolymer having NCO groups at its terminals, which is obtained by reacting an organic polyisocyanate with an active hydrogen compound.
[0066] (a) The polyester polyol having a functionality of at least 3 can be obtained by esterifying a dicarboxylic acid, a glycol, and a polyol having at least 3 OH groups.
[0067] Examples of dicarboxylic acids used in the production of polyester polyols include aliphatic dicarboxylic acids such as succinic acid, succinic anhydride, adipic acid, azelaic acid, sebacic acid, dodecanoic diacid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, and dimer acid; and aromatic and alicyclic dicarboxylic acids such as phthalic acid, phthalic anhydride, isophthalic acid, isophthalic acid dimethyl ester, terephthalic acid, terephthalic acid dimethyl ester, 2,6-naphthalenedicarboxylic acid, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, cyclohexanedicarboxylic acid, cyclohexanedicarboxylic acid dimethyl ester, methylhexahydrophthalic anhydride, himic anhydride, and methyl himic anhydride.
[0068] Examples of glycols include ethylene glycol, diethylene glycol, propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, dipropylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, neopentyl glycol ester of hydroxydivalanic acid, triethylene glycol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,4-diethyl-1,5-pentanediol, polycaprolactone diol, polypropylene glycol, Examples of the polyphenols include aliphatic polyphenols such as glycol, polytetramethylene ether glycol, polycarbonate diol, 2-n-butyl-2-ethyl-1,3-propanediol, and 2,2-diethyl-1,3-propanediol; and aliphatic or aromatic polyphenols such as cyclohexanedimethanol, cyclohexanediol, 2-methyl-1,1-cyclohexanedimethanol, xylylene glycol, bishydroxyethyl terephthalate, 1,4-bis(2-hydroxyethoxy)benzene, hydrogenated bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A.
[0069] Examples of polyols having at least three OH groups include glycerin, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, pentaerythritol, diglycerin, and ethylene oxide adducts, propionate adducts, and ε-caprolactone adducts using these polyols as initiators.
[0070] Examples of the blocked compounds of (b) include compounds having at least two NCO groups, such as aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, dodecamethylene diisocyanate, and 2,6-diisocyanatomethyl caproate. and other isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylhexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,2-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, 1,3-bis(isocyanatomethyl)cyclohexane, Cycloalkylene diisocyanates such as (methyl)cyclohexane and trans-cyclohexane-1,4-diisocyanate, and diisocyanates such as m-xylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, aromatic diisocyanates such as isocyanate, for example, ω,ω'-diisocyanato-1,3-dimethylbenzene, ω,ω'-diisocyanato-1,4-dimethylbenzene, ω,ω'-diisocyanato-1,4-diethylbenzene, α,α,α',α'-tetramethylmetaxylylenediisocyanate, and aromatic aliphatic diisocyanates such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, ω-isocyanatoethyl-2,Examples of such blocked products include triisocyanates such as 6-diisocyanatocaproate, tetraisocyanates such as 4,4'-diphenylmethylmethane-2,2',5,5'-tetraisocyanate, and derivatives of isocyanate compounds such as dimers, trimers, biuret, allophanates, carbodiimides, polymethylene polyphenyl polyisocyanates (crude MDI, c-MDI, polymeric MDI), and crude TDI, as well as blocked products of prepolymers having NCO groups at their ends obtained by reacting these with active hydrogen compounds.
[0071] The conductive particles are corrosion-resistant particles that are alloys or compounds containing 50% or more by mass of Si, or composites thereof. The conductive particles are preferably ferrosilicon. Anti-rust pigments may be added to the chemical conversion coating. Examples of the anti-rust pigments include known anti-rust pigments such as hexavalent chromates, such as strontium chromate and calcium chromate. When it is desired to avoid using hexavalent chromium compounds as anti-rust agents, it is possible to use those that release one or more of silicate ions, phosphate ions, and vanadate ions.
[0072] Of course, examples of the chemical conversion coating of this embodiment are not limited to those mentioned above, and for example, the chemical conversion coatings given in the examples described below can also be suitably used.
[0073] The method for forming the above-mentioned chemical conversion coating is not particularly limited, and a chemical conversion solution (coating solution) corresponding to each of the above compositions may be applied to a Zn-based plated steel sheet by a known method, followed by baking and drying. An example of a preferred combination of a Zn-based plated steel sheet and a chemical conversion coating is a combination of a Zn-Al-Mg plated steel sheet and an inorganic coating containing a Si-based component as a main component. Another example is a combination of a Zn-Al plated steel sheet and a resin coating. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples. Note that the examples described below are merely examples of the present invention and are not intended to limit the present invention.
[0075] <Material preparation> A steel having the steel composition shown in Table 1 (the balance being iron and impurities) as an extra-low carbon steel with excellent workability was hot-rolled, pickled, and cold-rolled to prepare a cold-rolled steel sheet with a thickness of 0.6 mm.
[0076] [Table 1]
[0077] Furthermore, the cold-rolled steel sheet was annealed under conditions where the maximum sheet temperature reached was 820°C using a continuous hot-dip plating apparatus capable of annealing, and then hot-dip galvanized to prepare a hot-dip galvanized steel sheet. Here, the gas atmosphere in the annealing furnace in the annealing process was an N2 atmosphere containing 1.0% by volume of H2. Four types of plating bath components in the plating process were used: Zn-0.2% by mass Al (hereinafter also referred to as "GI"), Zn-0.09% by mass Al (hereinafter also referred to as "GA"), Zn-6% by mass Al-3% by mass Mg (hereinafter also referred to as "Zn-Al-Mg"), and Zn-11% by mass Al-3% by mass Mg-0.2% by mass Si (hereinafter also referred to as "Zn-Al-Mg-Si").
[0078] In addition, in the hot-dip galvanizing using a hot-dip galvanizing bath of Zn-0.09 mass% Al plating (GA), alloying hot-dip galvanizing was performed by the following process. That is, the steel sheet was immersed in the hot-dip galvanizing bath. Next, while the steel sheet was pulled out of the plating bath, N2 gas was sprayed from a slit nozzle to perform gas wiping, and the coating weight was adjusted. Next, the steel sheet was alloyed by heating it to a sheet temperature of 480°C using an induction heater, and Fe in the steel sheet was diffused into the plating layer.
[0079] The coating weight of the plated steel sheet is 45 g / m2 for GA per side of the steel sheet. 2 , 60g / m for plating other than GA 2For comparison, cold-rolled steel sheets that were not plated but only annealed in a continuous annealing line were also prepared.
[0080] Next, the surface of the plated steel sheet prepared in the above process was coated with a chemical conversion solution (film treatment solution) using a roll coater as necessary. The amount of chemical conversion solution applied (i.e., the film thickness of the chemical conversion film) was adjusted by adjusting the rotation speed of the roll coater and the pressure between the rolls (generally called nip pressure). In this way, a chemical conversion film with a specified film thickness was formed on the plated steel sheet.
[0081] Here, when the chemical conversion coating is an inorganic coating, the chemical conversion coating solution was applied and then dried in a hot air oven under conditions where the ultimate sheet temperature was 80°C. When the chemical conversion coating is a resin coating, before the chemical conversion coating solution was applied to the plated steel sheet, the plated steel sheet was coated with Palcoat E200, a chemical conversion coating made by Nippon Parkerizing Co., Ltd., using a roll coater as a pretreatment to enhance adhesion to the plated steel sheet, and then dried in a hot air oven under conditions where the ultimate sheet temperature was 80°C. Thereafter, the chemical conversion coating solution was applied to a predetermined film thickness using a roll coater, and then dried in a hot air oven under conditions where the ultimate sheet temperature was 200°C. The chemical conversion coating was applied to both sides of the plated steel sheet. The film thickness after the coating and drying of each coating was measured by embedding the coated steel sheet in resin and polishing it so that the vertical cross section could be observed, and observing it with a scanning electron microscope. The magnification of the observation with the scanning electron microscope was appropriately selected optimally according to the film thickness of the coating.
[0082] In addition, in the samples where the inorganic film was created with a thickness exceeding 1.5 μm after coating and drying, cracks occurred in the film or the film came off, and it was not possible to obtain a uniformly formed film in any of the treatment solutions, so it was determined that it is difficult to produce an inorganic film with a thickness exceeding 1.5 μm. Details of the steel sheets created by coating various plated steel sheets with films are shown in Tables 5A to 5E.
[0083] <How to make inorganic conversion treatment solution> An inorganic conversion treatment liquid (chemical conversion treatment liquid for forming an inorganic coating) was prepared by the following process. That is, an aqueous solution containing 10 g / L of γ-aminopropyltriethoxysilane was prepared as an inorganic conversion treatment liquid mainly composed of a Si-based component. Furthermore, 1.3 g / L of vanadium oxide, 0.7 g / L of phosphoric acid, and 0.5 g / L of Co nitrate were added to the prepared γ-aminopropyltriethoxysilane aqueous solution as required to prepare an inorganic conversion treatment liquid.
[0084] Furthermore, an aqueous solution containing 3.0 g / L of ammonium zirconium carbonate was prepared as an inorganic conversion treatment solution mainly composed of Zr-based components. Furthermore, 1.3 g / L of vanadium oxide, 0.7 g / L of phosphoric acid, and 0.5 g / L of Co nitrate were added to the prepared aqueous solution of ammonium zirconium carbonate as required to prepare an inorganic conversion treatment solution. Details of the inorganic conversion treatment solution prepared are shown in Table 2.
[0085] [Table 2]
[0086] The following method was used to confirm whether the inorganic coating contained Si-O bonds or the like. That is, the prepared inorganic conversion treatment solution was applied to any of the plated steel sheets prepared above using a wire bar, and dried under conditions that resulted in a sheet temperature of 80°C. In this way, an inorganic coating was formed on the plated steel sheet. Next, the coating surface was measured using an IRT-5200 manufactured by JASCO Corporation, and it was determined whether the inorganic coating contained one or more of Si-O bonds, Si-C bonds, and Si-OH bonds based on the assignment of observed peaks derived from resin components in the infrared absorption spectrum of the obtained inorganic coating. Specifically, the inorganic conversion treatment solution was applied to any of the plated steel sheets prepared above using a wire bar, and dried under conditions that resulted in a sheet temperature of 80°C. In this way, an inorganic coating was formed on the plated steel sheet. Next, the coating surface was measured using an IRT-5200 manufactured by JASCO Corporation, and it was determined whether the inorganic coating contained one or more of Si-O bonds, Si-C bonds, and Si-OH bonds based on the assignment of observed peaks derived from resin components in the infrared absorption spectrum of the obtained inorganic coating. -1 Near, 1080~1020cm -1 Near, 500~300cm -1 Near, 900~700cm -1 When a peak was observed in at least one of the vicinity, it was judged that the inorganic coating contained one or more of the Si-O bond, the Si-C bond, and the Si-OH bond. The judgment results are shown in Table 2.
[0087] <How to prepare resin-based chemical conversion treatment solution> A resin-based chemical conversion treatment liquid (chemical conversion treatment liquid for forming a resin film) was prepared in the following steps. That is, a polyester resin "Vylon(R) 300" manufactured by Toyobo Co., Ltd. was dissolved in cyclohexanone as a solvent at 30 mass %, and 20 mass parts of solid content of melamine resin "CYMEL(R) 303" manufactured by Allnex Co., Ltd. was added to 100 mass parts of solid content of this solution and mixed. In addition, 5 mass % of hardening catalyst "CYCAT(R) 600" manufactured by Allnex Co., Ltd. was added to the total solid content of the prepared mixture and mixed. In this way, a base treatment liquid for obtaining a resin film was prepared.
[0088] Next, the particles shown below were mixed into the prepared base treatment liquid to prepare a resin-based chemical conversion treatment liquid. The amount of particles added was adjusted by the following method. That is, the solid mass ratio (mass ratio to solids other than particles) of the particles added to the base treatment liquid in the resin film was obtained, and the volume ratio was calculated from the specific gravity of the solids in the resin film and the specific gravity of the particles. Next, the amount of particles added was adjusted so that the calculated volume ratio became the volume ratio shown in Table 3. The specific gravity was used from the catalog value or literature value of each substance. Details of the resin-based treatment liquid are shown in Table 3.
[0089] [Table 3]
[0090] Vanadium boride: "VB2-O" manufactured by Japan New Metals Co., Ltd. was sieved to obtain an average particle size of 3.1 μm. Hereinafter, this is also referred to as "VB2". The average particle size was calculated based on the mass percentage of each particle size fraction. Al-doped zinc oxide: Conductive zinc oxide (Al-doped ZnO) "23-K" manufactured by Haktech, with a primary particle size of 120 to 250 nm (catalog value) was used. Hereinafter, this is also referred to as "Al-ZnO". Metallic zinc: Reagent zinc particles were classified using a sieve to have an average particle size of 10 μm. Hereinafter, this will be referred to as "Zn." Ferrosilicon: Ferrosilicon manufactured by Marubeni Tetsugen Co., Ltd. was crushed into fine particles using a grinder and classified using a sieve to obtain an average particle size of 3.5 μm. Hereinafter, this is also referred to as "Fe-Si." Ferromanganese: Ferro-silicon manufactured by Marubeni Tetsugen Co., Ltd. was crushed into fine particles using a grinder and classified using a sieve to obtain an average particle size of 3.5 μm. Hereinafter, this is also referred to as "Fe-Mn." Zirconium boride: "ZrB2-O" manufactured by Japan New Metals Co., Ltd. was classified with a sieve to have an average particle size of 2 μm. Hereinafter, this will be referred to as "ZrB2". Molybdenum silicide: "MoSi2-F" manufactured by Nippon Shinkinzoku Co., Ltd. was classified with a sieve to obtain an average particle size of 3.5 μm. Hereinafter, this will be referred to as "MoSi2". Chromium boride: "CrB2-O" manufactured by Nippon Shinkinzoku Co., Ltd. was classified with a sieve to have an average particle size of 5 μm. Hereinafter, this will be referred to as "CrB2". Tungsten silicide: "B2-O" manufactured by Japan New Metals Co., Ltd. was classified with a sieve to have an average particle size of 2 μm. Hereinafter, this will be referred to as "WSi2". Nickel: Nickel powder was used as a reagent, which was sieved to have an average particle size of 5 μm. Hereinafter, this will be referred to as "Ni." Conductive titanium oxide: Ishihara Sangyo Kaisha's Sn-doped titanium oxide "ET-500W" with an average particle size of 2 to 3 μm (catalog value) was used. Hereinafter, this will be referred to as "conductive Ti." Alumina: Showa Denko Co., Ltd. fine alumina "A-42-2" with an average particle size (median particle size distribution diameter) of 4.7 μm (catalog value) was used. Hereinafter, this will also be referred to as "alumina". Titanium oxide: Ishihara Sangyo Kaisha's "Tipaque" (R) CR-95" with an average particle size of 0.28 μm (catalog value) was used. Hereinafter, this will also be referred to as "TiO2". Aluminum nitride: Tokuyama Corporation's aluminum nitride powder for filler, particle size 1 μm (catalog value), was used. Hereinafter, this will be referred to as "AlN".
[0091] The powder resistivity of the particles in Table 3 was determined as the resistance value when each powder was compressed at 10 MPa at 25°C using a powder resistivity measurement system MCP-PD51 manufactured by Mitsubishi Chemical Analytech Co., Ltd.
[0092] <Evaluation of the created metal plate> (0. Strength rating) The strength of the prepared Zn-plated steel sheets, etc. was evaluated by a tensile test in accordance with the provisions of JIS Z 2241. As a result, the strength of all the Zn-plated steel sheets, etc. was 270 MPa or more. Next, an Al sheet (A6063) having a thickness similar to that of the Zn-plated steel sheets, etc. was prepared, and the strength of this Al sheet was evaluated in the same manner as above, and was found to be 200 MPa or less. Therefore, it was confirmed that the Zn-plated steel sheets, etc. have high strength.
[0093] (1. Evaluation of coolant resistance) The coolant resistance was investigated when the prepared Zn-plated steel sheets, etc. were used in the cooling structure (cooling device) of a battery unit. Specifically, the prepared Zn-plated steel sheets, etc. were processed by Erichsen to produce a cup-shaped cylindrical product with a diameter of 50 mm and a drawing height of 40 mm. 30 mL of coolant was added to the inside of this cylindrical product, and then the product was sealed with a lid. The coolant used was an aqueous solution of Nissan Motor's long-life coolant liquid diluted with water to 30% by mass. These were left in a thermostatic bath at 90°C for 1000 hours to promote the deterioration of the steel sheet in the coolant-immersed area. In addition, assuming the deterioration of the coolant liquid, a similar test was also conducted using a deteriorated liquid in which 800 ppm of formic acid was added to a 30% by mass aqueous solution of the long-life coolant liquid. After the test, the coolant immersed in the cylindrical product was removed and the cylindrical product was dried, and the corrosion state of the coolant-immersed area was observed, and the coolant resistance was evaluated according to the following criteria. The results are shown in Tables 5A to 5E. 5 points: No change in appearance 4 points: Black discoloration or white rust spots have appeared. 3 points: White rust has occurred, but the area of the part immersed in the coolant where the white rust has occurred is less than 20% of the total area immersed in the coolant. 2 points: White rust occurrence rate is 20% or more but less than 80%. 1 point: White rust occurrence is 80% or more, or red rust has occurred.
[0094] (2. Corrosion resistance test) A corrosion resistance test was carried out to evaluate the corrosion resistance of the battery unit (including the cooling structure) at the portion exposed to the outside air. Since electrodeposition coating is generally applied to the portion exposed to the outside air, in the present invention, the corrosion resistance after electrodeposition coating was evaluated.
[0095] Specifically, the prepared steel plate was cut into pieces measuring 70 mm wide x 150 mm long, and the pieces were degreased, surface-conditioned, and zinc phosphate-treated, and then electrocoated. Specifically, the pieces were degreased by immersing them in a degreaser "Fine Cleaner E6408" manufactured by Nippon Parkerizing Co., Ltd. for 5 minutes at 60°C. The degreased pieces were surface-conditioned by immersing them in "Preparen X" manufactured by Nippon Parkerizing Co., Ltd. for 5 minutes at 40°C. Thereafter, the pieces were immersed in a zinc phosphate conversion agent "Palbond L3065" manufactured by Nippon Parkerizing Co., Ltd. for 3 minutes at 35°C to perform zinc phosphate treatment. The pieces after the zinc phosphate treatment were washed with water and dried in an oven at 150°C. Then, the pieces were electrocoated with an electrocoating paint "Power Float 1200" manufactured by Nippon Paint Co., Ltd. at a thickness of 15 μm per side, and baked in an oven at 170°C for 20 minutes. The electrocoated steel pieces prepared by the above steps were cut with a cutter knife to prepare test pieces.
[0096] A cyclic corrosion test (CCT) was conducted using the prepared test pieces. The CCT mode was conducted in accordance with the automotive industry standard JASO-M609. The surface with cut scratches in the electrocoating film was used as the evaluation surface, and the test piece was placed in a testing machine so that salt water was sprayed on the evaluation surface, and a cyclic corrosion test was conducted.
[0097] The test was carried out for 120 cycles (1 cycle lasting 8 hours), and the state of corrosion from the cut portion was observed and the corrosion resistance was evaluated according to the following criteria. The results are shown in Tables 5A to 5E. 5 points: The paint film bulge width from the cut part is within 15 mm and there is no red rust. 4 points: The paint film bulge width from the cut part is more than 15mm but not more than 20mm, and there is no red rust. 3 points: The paint film bulge width from the cut part is more than 20 mm, and there is no red rust. 2 points: A small amount of red rust was observed at the cut area. 1 point: Red rust has appeared on the entire cut surface
[0098] <Evaluation of cooling characteristics in a battery unit> (1. Creating a battery unit) The battery unit 1 shown in FIG. 3 was produced using the prepared Zn-plated steel sheet and the like. Specifically, the flat plate material that was only cut was used as the case top cover (top surface portion 10c) and the flow path top cover 26. Separately prepared Zn-plated steel sheet and the like were subjected to square cylinder deep drawing by a press machine, and the flange portion was cut after processing to produce the other parts (bottom surface portion 10a and side surface portion 10b) of the battery pack 10. In addition, the bottom surface portion 10a of the battery pack 10 was processed to have a width of 315 mm and a length of 2000 mm. During processing, rust-preventive oil was applied to the Zn-plated steel sheet and the like, and the oil was removed by alkaline degreasing after processing. The punch shoulder R, die shoulder R, and corner R of the square cylinder shape were all 20 mm. The cooling structure 20 was also produced by pressing. Each R in the cooling structure 20 was set to 10 mm, and the number of flow paths, the flow path width, and the distance between the flow paths were produced to the values shown in Table 4.
[0099] [Table 4]
[0100] Next, the sealer 35 was applied to the joint 22 of the cooling structure 20 as shown in FIG. 3, and the cooling structure 20 and the flow path upper cover 26 were overlapped. Next, the joint 22 and the flow path upper cover 26 were joined by spot welding. Hereinafter, spot welding is also referred to as "SW". In some levels, instead of spot welding, the joint 22 and the flow path upper cover 26 were joined using a mechanical joining method "TOX" (registered trademark) manufactured by Toxpressotechnik. In addition, in cases where the interval between the water coolant flow paths 25 was narrow, less than 10 mm, and the welding tip for spot welding could not be inserted and welding could not be performed, the two were bonded together using only a sealer. In addition, in cases where the resin film coated on the plated steel sheet had a thickness of more than 15 μm, the film did not conduct and welding was difficult, so the two were bonded together using TOX and a sealer. Next, the cooling structure 20 was left at room temperature for two weeks to harden the sealer. The sealer used was "Sealant 45N" manufactured by Shin-Etsu Silicone Co., Ltd.
[0101] Next, "SDP-3540-A" manufactured by Shin-Etsu Silicone Co., Ltd. was applied to the entire outer surface of the flow path upper cover 26, and the bottom surface portion 10a of the battery pack 10 was attached thereon as shown in FIG. 3, and the gap filler 40 was hardened by leaving it at room temperature for one week. The battery unit 1 shown in FIG. 3 was manufactured by the above process. The battery unit 1 shown in FIG. 1 and FIG. 2 was also manufactured. Specifically, the battery pack 10 was directly joined to the flow path upper cover 26 as shown in FIG. 2. At this time, the flow path upper cover 26 and the battery pack 10 were joined with screws. Also, the sealer 35 was applied to the cooling structure 20 as shown in FIG. 1, and the cooling structure 20 and the battery pack 10 were overlapped. Next, the joint portion 22 and the battery pack 10 were joined by spot welding. Note that in the case where the interval between the water coolant flow paths 25 was narrow, less than 10 mm, and the welding tip for spot welding could not be inserted and welding could not be performed, the two were bonded together using only the sealer.
[0102] Next, rubber heaters were laid on the inside bottom surface of the battery pack 10 as a substitute for heat-generating battery cells, and the case was covered with a lid. When the lid was closed, a sealer 10d was applied to the case flange to seal it. The sealer used was "Sealant 45N" manufactured by Shin-Etsu Silicone Co., Ltd. The metal materials constituting the battery pack 10 and the cooling structure 20 were the same. That is, the battery pack 10, the flow path lid 26, and the cooling structure 20 constituting one battery unit 1 were manufactured from the same metal material.
[0103] (2. Battery unit cooling characteristic evaluation test) The battery unit 1 was heated by passing a current through the rubber heater of the battery unit 1. Here, the current value at which the surface temperature of the rubber heater becomes 50°C was searched in advance, and the current value was passed through the rubber heater as a fixed value. Next, the coolant was passed through the water coolant flow path 25. The coolant was an aqueous solution obtained by diluting PITWORK's long-life coolant liquid with water to 30% by mass. In addition, a hose, a pump, and a chiller were attached to the ends of the flow paths on both sides of the cooling structure 20 to form a circulation path, and the coolant was circulated within this circulation path. Here, the chiller was controlled so that the temperature of the coolant was 25 to 30°C. Then, the temperature of the surface of the rubber heater in the case directly above the middle part between the cooling flow paths one hour after the start of the cooling water circulation was measured, and the case where the temperature was 8°C or more lower than when the cooling water was not circulating was evaluated as ◎, the case where the temperature drop was less than 8°C and 5°C or more was evaluated as ◯, the case where the temperature drop was less than 5°C and 2°C or more was evaluated as △, and the case where the temperature drop was less than 2°C was evaluated as ×. The cooling characteristic evaluation test of the battery unit 1 was carried out in an air-conditioned room kept at 25° C. The results are shown in Tables 5A to 5E.
[0104] [Table 5A]
[0105] [Table 5B]
[0106] [Table 5C]
[0107] [Table 5D]
[0108] [Table 5E]
[0109] As shown in Tables 5A to 5E, in the examples of the present invention that satisfy the requirements of this embodiment, excellent results were obtained not only in corrosion resistance against the coolant (coolant corrosion resistance) but also in corrosion resistance against the external environment (external corrosion resistance). Furthermore, in most of the examples of the present invention, high evaluation results were obtained for cooling efficiency. Examples of the examples of the present invention include those in which the plating layer is Zn-Al-Mg, those in which the distance between the water coolant flow paths is 40 mm or less, those in which the inorganic coating contains a rust-preventive component, those in which the resin coating is 1.0 to 15 μm thick, those in which the resin coating contains a conductive pigment, and those in which the powder resistivity of the conductive pigment is 185×10 -6 Particularly excellent results were obtained for those with a resistance of Ωcm or less. Therefore, it was found that the battery unit 1 according to this embodiment has excellent corrosion resistance not only against the coolant (coolant corrosion resistance) but also against the external environment (external corrosion resistance).
[0110] In contrast, in comparative examples that do not satisfy the requirements of this embodiment, i.e., those that are not coated with a chemical conversion coating or are not plated, poor results were obtained in either coolant corrosion resistance or external corrosion resistance (or both).
[0111] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. [Explanation of symbols]
[0112] 1 Battery unit 10 Battery Pack 10a Bottom part 10b Side part 10c Top part 20 Cooling structure 21 Flow path forming section 22 Joint 25 Water cooling medium channel 30 Spot welds
Claims
1. A battery unit having a battery pack that houses battery cells and a water coolant passage formed on an outer side of a bottom surface of the battery pack, The water coolant flow path is made of a Zn-based plated steel sheet, The zinc-based plated steel sheet has a surface on which an inorganic coating or a resin coating is formed as a chemical conversion coating, The inorganic coating contains a Si-based component or a Zr-based component as a main component, A battery unit, characterized in that the bottom surface of the battery pack is flat.
2. 2. The battery unit according to claim 1, wherein the water coolant passages are spaced apart from one another by a distance of 40 mm or less.
3. 3. The battery unit according to claim 1, wherein a bottom surface of the battery pack is made of a material processed from the Zn-based plated steel sheet, and the water coolant flow path is in direct contact with the bottom surface of the battery pack.
4. 3. The battery unit described in claim 1 or 2, characterized in that the water coolant flow path is joined to a flow path upper cover made of the Zn-based plated steel plate, and the water coolant flow path is joined to a bottom surface of the battery pack via the flow path upper cover.
5. The battery unit according to any one of claims 1 to 4, wherein the water coolant passages are spaced apart from one another by a distance of 10 mm to 40 mm.
6. The distance between the water coolant flow paths is 10 mm or more and 40 mm or less, The battery unit according to any one of claims 1 to 5, characterized in that the joint between the bottom surface of the battery pack and the water coolant flow path is a composite joint structure of a sealer and spot welding or a sealer and mechanical joining.
7. The battery unit according to any one of claims 1 to 6, wherein the inorganic coating contains at least one of a V component, a P component, and a Co component as an anti-rust component.
8. 8. The battery unit according to claim 7, wherein the rust-preventing component is at least one of vanadium oxide, phosphoric acid, and cobalt nitrate.
9. 9. The battery unit according to claim 1, wherein the inorganic coating or the resin coating has electrical conductivity.
10. The battery unit according to any one of claims 1 to 9, wherein the inorganic coating is composed of a compound phase containing at least one of a Si-O bond, a Si-C bond, and a Si-OH bond.
11. The battery unit according to any one of claims 1 to 10, wherein the inorganic coating has a thickness of more than 0 µm and not more than 1.5 µm.
12. The battery unit according to any one of claims 1 to 6, wherein the resin coating contains a resin, an anti-rust pigment, and a conductive pigment.
13. The resin coating contains, as the conductive pigment, at least one of metal particles, intermetallic compound particles, conductive oxide particles, and conductive non-oxide ceramic particles; The conductive pigment has a powder resistivity of 185×10 at 25° C. -6 The battery unit according to claim 12, characterized in that it has a resistivity of Ωcm or less and contains at least one element selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, Fe and W as a constituent element.
14. The battery unit according to claim 12 or 13, wherein the resin film contains the conductive pigment in a proportion of 1.0 mass % or more and 30 mass % or less.
15. The battery unit according to any one of claims 12 to 14, wherein the resin film has an average thickness of 1.0 µm or more and 15 µm or less.
16. The Zn-based plated steel sheet is a Zn-Al-Mg plated steel sheet, The battery unit according to any one of claims 1 to 11, characterized in that an inorganic coating containing a Si-based component as a main component is formed on a surface of the Zn-Al-Mg plated steel sheet.
17. The Zn-based plated steel sheet is a Zn-Al plated steel sheet, The battery unit according to any one of claims 1 to 6 and 12 to 15, wherein a resin film is formed on a surface of the Zn-Al plated steel sheet.
Citation Information
Patent Citations
Separator
JP1986025624A
Painted metallic material, which is excellent in corrosion resistance of formed part and can be welded
JP2004042622A
Battery unit
JP2014157756A
Power storage device
JP2014186865A