Welded joints
By controlling the Al concentration and phase ratio in the plating layer of plated steel sheets, the welded joint effectively suppresses LME cracking and improves corrosion resistance, addressing the limitations of existing methods in spot welding galvanized steel sheets.
Patent Information
- Application Number
- JP2023572419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-06
- Filing Date
- 2022-12-21
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2042-12-21
AI Technical Summary
Existing methods for suppressing Liquid Metal Embrittlement (LME) cracking in welded joints, particularly in spot welding of galvanized steel sheets, do not adequately consider the plating structure before welding, leading to insufficient resistance against LME cracking.
A welded joint design that includes plated steel sheets with a controlled Al concentration distribution in the plating layer, specifically within the range of 0.10% to 1.50% Al, and a controlled ratio of η phase to Γ phase in the plating layer, forming a structure that suppresses the intrusion of molten zinc during spot welding.
Significantly improves LME resistance and corrosion resistance of welded joints by reducing the penetration of molten zinc into the steel sheet, thereby enhancing the strength and durability of the welded joint.
Smart Images

Figure 0007587195000002 
Figure 0007587195000003 
Figure 0007587195000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a welded joint, and more particularly to a welded joint obtained by spot welding plated steel sheets. [Background technology]
[0002] Steel sheets used in automobiles and other applications require good weldability. Spot welding is mainly used in processes such as assembling automobile bodies and installing parts, but it is necessary to suppress liquid metal embrittlement (LME) cracking, especially when spot welding between galvanized steel sheets or between galvanized and non-galvanized steel sheets. This phenomenon occurs when zinc, which has been liquefied by the welding heat input, penetrates into the steel sheet along the grain boundaries, embrittling the steel sheet, and then tensile stress generated by welding acts on the embrittled part. If such LME cracking occurs in spot welding, the strength of the welded joint cannot be ensured, which may hinder the use of galvanized steel sheets.
[0003] In relation to this, Patent Document 1 teaches that such LME cracking can be dealt with by improving the spot welding method. More specifically, Patent Document 1 teaches that by continuing to hold the welding electrodes under pressure after the current between the welding electrodes is stopped (extending the post-weld hold time Ht) and adjusting the post-weld hold time Ht as a function of the total plate thickness t of the welded members, the molten zinc-based coating is solidified before the electrodes are released, and as a result, the molten zinc-based coating does not penetrate into the grain boundaries of the steel plate at locations with high welding residual stress, thereby suppressing cracking.
[0004] Patent Document 2 teaches that cracks can be prevented by controlling the plating structure in the vicinity of the spot welded portion after spot welding. More specifically, Patent Document 2 describes a spot welded component having a spot welded portion formed by sandwiching a sheet set of overlapping multiple steel sheets between a pair of electrodes and spot welding, in which at least one of the multiple steel sheets is a high-strength zinc-based plated steel sheet having a tensile strength of 780 MPa or more, and the Al content in the plating of the high-strength zinc-based plated steel sheet is 0.5 mass % or more, and the thermal shock region outside the corona bond end of the spot welded portion has a plating layer at the interface between the base steel sheet of the high-strength zinc-based plated steel sheet and the plating, the plating layer being an FeAl alloy layer having an average thickness of 0.3 μm or more and a zinc-based plating layer having an average thickness of 2.0 μm or more formed on the FeAl alloy layer. Furthermore, Patent Document 2 teaches that in order to suppress the penetration of Zn into the base steel sheet, it is important to set the Al content in the coating to 0.5 mass% or more, so that an FeAl alloy layer having a high melting point is formed at the interface between the steel sheet and the coating of the steel sheet by the heat input during welding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-047475 A [Patent Document 2] International Publication No. 2020 / 130079 Summary of the Invention [Problem to be solved by the invention]
[0006] Patent Documents 1 and 2 consider suppressing LME cracking in welded joints from the viewpoint of improving spot welding methods and controlling the plating structure in the vicinity of spot welds after spot welding. However, Patent Documents 1 and 2 do not necessarily consider sufficiently suppressing the occurrence of LME cracking in welded joints in relation to the plating structure of the plated steel sheet before spot welding. Therefore, the inventions described in these patent documents still have room for improvement in terms of improving LME resistance.
[0007] Therefore, an object of the present invention is to provide a welded joint that can suppress or reduce the occurrence of LME cracking during spot welding using a novel configuration. [Means for solving the problem]
[0008] The present inventors conducted a study focusing on the structure of the coating layer in a coated steel sheet used for a welded joint in order to suppress or reduce the occurrence of LME cracking when manufacturing a welded joint by spot welding. As a result, the present inventors found that by using a coated steel sheet having a coating layer in which the Al concentration distribution is appropriately controlled while containing a relatively small amount of Al, the coating layer structure in a portion where LME cracking is likely to occur during spot welding can be improved, and in connection with this, the LME resistance of the welded joint can be significantly improved, and thus completed the present invention.
[0009] The present invention which has achieved the above object is as follows. (1) Multiple overlapping steel plates; a nugget that joins the plurality of steel plates, and a spot weld having a pressure welded portion and a heat affected zone formed around the nugget; a separation portion located around the pressure-welded portion; A welded joint comprising: At least one of the plurality of steel sheets is a plated steel sheet comprising a base steel sheet and a plating layer formed on at least a surface of the base steel sheet that corresponds to an overlapping surface of the plurality of steel sheets, The plating layer in the separation portion outside the heat-affected zone has, in mass%, Al: 0.10 to 1.50%, and Fe: 0.01 to 2.00% and further comprising Mg: 0-1.500%, Si: 0 to 1.000%, Ni: 0 to 1.000%, Ca: 0-4.000%, Sb: 0 to 0.500%, Pb: 0~0.500%, Cu: 0-1.000%, Sn: 0~1.000%, Ti: 0 to 1.000%, Cr: 0~1.000%, Nb: 0 to 1.000%, Zr: 0 to 1.000%, Mn: 0 to 1.000%, Mo: 0~1.000%, Ag: 0~1.000%, Li: 0~1.000%, La: 0 to 0.500%, Ce: 0 to 0.500%, B: 0 to 0.500%, Y: 0 to 0.500%, P: 0 to 0.500%, and Sr: 0 to 0.500% Contains at least one of the following in total at 5.000% or less, The balance has a chemical composition consisting of Zn and impurities, A welded joint, characterized in that in the plating layer of the separation portion in a region 500 μm from the end of the pressure weld portion, the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase is 10 to 100%. (2) The welded joint described in (1) above, characterized in that the chemical composition contains, in mass%, Al: 0.30 to 1.50%, and in the plating layer of the separation portion in a region 500 μm from the end of the pressure weld portion, the ratio of the area fraction of the η phase to the total area fraction of the η phase and the Γ phase is 25 to 100%. (3) The welded joint described in (1) above, characterized in that the chemical composition contains, in mass%, Al: 0.30 to 1.50%, and in the plating layer of the separation portion in a region 500 μm from the end of the pressure weld, the ratio of the area fraction of the η phase to the total area fraction of the η phase and the Γ phase is 40 to 100%. (4) The welded joint according to any one of the above (1) to (3), characterized in that the plating layer is a hot-dip galvanized (GI) layer. (5) The welded joint according to any one of the above (1) to (4), wherein the plated steel sheet has a tensile strength of 780 MPa or more. Effect of the Invention
[0010] According to the present invention, it is possible to provide a welded joint capable of suppressing or reducing the occurrence of LME cracking during spot welding. [Brief description of the drawings]
[0011] [Figure 1] 1A and 1B are diagrams showing schematic cross sections of a welded joint according to an embodiment of the present invention, in which (a) is an overall view of the welded joint, and (b) is an enlarged view of the end of the pressure-welded portion and the separation portion immediately outside thereof. [Diagram 2] FIG. 1 shows the results of GDS analysis of plated steel sheets, where (a) shows the results of GDS analysis of an Al-containing plated steel sheet produced by a conventional method, and (b) shows the results of GDS analysis of a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Welded joints> A welded joint according to an embodiment of the present invention includes a plurality of overlapping steel plates, a nugget that joins the plurality of steel plates, and a spot weld having a pressure welded portion and a heat affected zone formed around the nugget; a separation portion located around the pressure-welded portion; A welded joint comprising: At least one of the plurality of steel sheets is a plated steel sheet comprising a base steel sheet and a plating layer formed on at least a surface of the base steel sheet that corresponds to an overlapping surface of the plurality of steel sheets, The plating layer in the separation portion outside the heat-affected zone has, in mass%, Al: 0.10 to 1.50%, and Fe: 0.01 to 2.00% and further comprising Mg: 0-1.500%, Si: 0 to 1.000%, Ni: 0 to 1.000%, Ca: 0-4.000%, Sb: 0 to 0.500%, Pb: 0~0.500%, Cu: 0-1.000%, Sn: 0~1.000%, Ti: 0 to 1.000%, Cr: 0~1.000%, Nb: 0 to 1.000%, Zr: 0 to 1.000%, Mn: 0 to 1.000%, Mo: 0~1.000%, Ag: 0~1.000%, Li: 0~1.000%, La: 0 to 0.500%, Ce: 0 to 0.500%, B: 0 to 0.500%, Y: 0 to 0.500%, P: 0 to 0.500%, and Sr: 0 to 0.500% Contains at least one of the following in total at 5.000% or less, The balance has a chemical composition consisting of Zn and impurities, In the plating layer of the separation portion in a region 500 μm from the end of the pressure-welded portion, the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase is 10 to 100%.
[0013] As described above, in spot welding between galvanized steel sheets or between galvanized and non-galvanized steel sheets, it is necessary to suppress LME cracking. For example, when two or more steel sheets, including at least one galvanized steel sheet, are stacked and spot-welded to form a joint, LME cracking may occur inside a pressure-welded part (corona bond) formed on the outside of the weld metal (nugget) or immediately outside the pressure-welded part, for example, in a separation part (area where the steel sheets are not joined) located around the pressure-welded part. LME cracking occurs when zinc that has been liquefied by welding heat input during spot welding penetrates into the steel sheet along the grain boundaries and embrittles the steel sheet, and tensile stress generated by welding, for example, tensile stress generated by many factors such as the pressure applied by the electrodes, the expansion and contraction of the welded part, and springback when the electrodes are released, acts on the steel sheet. Therefore, in order to suppress or reduce the penetration of zinc into the steel sheet, the present inventors focused on the structure of the coating layer in the coated steel sheet and conducted a study from the viewpoint of making the structure of the coating layer more appropriate.
[0014] First, the inventors have found that adding a relatively small amount of aluminum (Al), i.e., 0.10 to 1.50 mass%, to a zinc (Zn)-based coating layer is effective from the viewpoint of suppressing or reducing the penetration of Zn into the steel sheet. When the amount of Al added is large, the composition of the coating layer approaches the Zn-Al eutectic composition, and the melting point of the coating layer decreases. For this reason, excessive addition of Al is likely to have a detrimental effect from the viewpoint of suppressing or reducing the penetration of molten Zn into the steel sheet and improving LME resistance. In particular, when Al is added in an amount significantly exceeding 1.50 mass%, the negative effect due to the excessive addition of Al becomes significant, and it is considered that the effect of suppressing LME cracking due to the addition of Al cannot be fully exhibited. In addition, the inventors have found that by using a plated steel sheet in which the Al concentration distribution in the plated layer is controlled so that the ratio of the Al concentration at the center of the plated layer to the Al concentration near the interface between the base steel sheet and the plated layer, more specifically the Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet, is 0.10 to 1.50, the plated structure in the separation area immediately outside the pressure welded area changes due to the heat effect during spot welding, etc., and the occurrence of LME cracks around the pressure welded area is significantly suppressed or reduced. This will be explained in more detail below with reference to the drawings.
[0015] FIG. 1 is a diagram showing a schematic cross section of a welded joint according to an embodiment of the present invention, in which (a) is an overall view of the welded joint, and (b) is an enlarged view of the end of the pressure welded part and the separation part immediately outside the end of the pressure welded part. First, referring to FIG. 1(a), the welded joint 1 according to the embodiment of the present invention includes two overlapping steel sheets 11, a nugget 12 that joins the steel sheets 11, a spot welded part 16 having a pressure welded part 13 and a heat-affected zone 15 formed around the nugget 12, and a separation part 17 located around the pressure welded part 13. In FIG. 1, a plated steel sheet having a plating layer mainly made of Zn and having an Al concentration distribution controlled within a predetermined range on both sides of the base steel sheet is used as the two steel sheets 11. In this regard, referring to FIG. 1(b), a plating layer 18 derived from the plating layer on the steel sheet 11 before spot welding is formed in the separation part 17 immediately outside the end 14 of the pressure welded part. According to an embodiment of the present invention, in the separation portion 17 in the heat-affected zone 15 located immediately outside the pressure-welded portion end portion 14, the structure of the initial plating layer changes due to the heat influence during spot welding, and a plating layer 18 having a relatively high ratio of η phase, more specifically, a plating layer 18 having an area ratio of η phase to the total area ratio of η phase and Γ phase of 10 to 100%, is formed. In the present invention, the η phase refers to a phase mainly composed of Zn and containing other elements such as Fe in a solid solution state, and more specifically, refers to a phase having a Zn concentration of 97 atomic % or more, an Fe concentration of 3 atomic % or less, and other elements of 3 atomic % or less, as measured by a scanning electron microscope with an electron probe microanalyzer (SEM-EPMA). Similarly, the Γ phase refers to a phase having a Zn concentration of 87 atomic % or more, an Fe concentration of 8 to 13 atomic %, and other impurities of 3 atomic % or less, as measured by a SEM-EPMA. Such a change in the structure of the plating layer is greatly influenced by the chemical composition and structure of the initial plating layer before spot welding. In Zn-based plating, the alloying of Zn in the plating layer progresses due to the heat input during welding, so the proportion of Γ phase generally becomes high and the proportion of η phase becomes relatively low.However, according to an embodiment of the present invention, compared to conventional spot welding of Zn-based plated steel sheet, a plating layer 18 having a relatively high proportion of η phase is formed in the separation portion 17 immediately outside the pressure welded portion 13, and in relation to this, the penetration of molten Zn into the steel sheet during spot welding is suppressed or reduced, and as a result, it is possible to significantly improve the LME resistance of the obtained welded joint.
[0016] In FIG. 1, for ease of understanding, a welded joint in which only two steel sheets 11 are overlapped and both steel sheets 11 have a plating layer formed thereon has been described. However, the welded joint according to the embodiment of the present invention is not necessarily limited to such a welded joint, and may include various welded joints in which a plating layer 18 having a predetermined amount of η phase is formed in a separation portion 17 in a heat-affected zone 15. For example, in a welded joint in which two steel sheets 11 are spot-welded as shown in FIG. 1, only one of the steel sheets 11 may be a plated steel sheet. In this case, it is sufficient that the plating layer 18 is present in the separation portion 17 immediately outside the pressure-welded portion 13 on at least the surface corresponding to the overlapping surface among the two surfaces of the plated steel sheet, and naturally the plating layer 18 and / or an initial plating layer related to the plating layer 18 may be present on both surfaces. For example, when an initial plating layer related to the plating layer 18 is present on the surface of the electrode side, i.e., the opposite side to the overlapping surface side of the steel sheet, the structure of the plating layer also changes during spot welding in the region in the heat-affected zone (for example, the contact portion between the electrode and the steel sheet and its periphery), and a plating layer 18 having a relatively high ratio of η phase is formed in the initial plating layer on the electrode side. This makes it possible to further improve LME resistance compared to when the plating layer 18 is simply present only on the surface corresponding to the overlapping surface of the steel sheet. Similarly, in the case of a welded joint made of three or more steel sheets, various welded joints in which a plating layer 18 having a predetermined amount of η phase is formed in the separation portion 17 in the heat-affected zone 15 may be included. For example, in a welded joint in which three steel sheets 11 are spot-welded, the plating layer 18 may be present in the separation portion 17 immediately outside the pressure-welded portion 13 on at least the surface corresponding to the overlapping surface of one or more of the three steel sheets 11. For example, when only the middle steel sheet 11 of three overlapping steel sheets 11 is a plated steel sheet, the plating layer 18 may be present only in the separation portion 17 immediately outside the pressure-welded portion 13 on one of the two surfaces of the plated steel sheet, or the plating layer 18 may be present in the separation portion 17 immediately outside the pressure-welded portion 13 on both surfaces. For example, the plating layer 18 may be present only in the separation portion 17 immediately outside the pressure-welded portion 13 of some of the steel sheets 11, and another Zn-based plating layer may be present in the separation portion 17 immediately outside the pressure-welded portion 13 of the other steel sheets 11.Such an embodiment is also included in the present invention. In this case, compared with the case of a welded joint in which the plating layer 18 is present in the separation portion 17 immediately outside the pressure-welded portion 13 of all the steel sheets 11, the risk of LME cracking is increased on the surface where another Zn-based plating layer is present, and therefore the strength of the joint may be somewhat reduced, but the specific number and arrangement of the steel sheets 11 on which the plating layer 18 having a predetermined amount of η phase is formed in the welded joint may be appropriately determined in consideration of the desired joint strength, etc.
[0017] Next, a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention will be described. FIG. 2 shows the results of analysis by GDS of plated steel sheet, in which FIG. 2(a) shows the results of analysis by GDS of an Al-containing plated steel sheet manufactured by a conventional method, and FIG. 2(b) shows the results of analysis by GDS of a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention. First, referring to FIG. 2(a), in an Al-containing plated steel sheet in which 0.20% Al is contained in a Zn-based plating layer by a conventional method, the Al concentration gradually increases as the depth from the depth position of 0 μm corresponding to the plating surface increases, and it can be seen that the Al concentration has a relatively high peak near the interface between the base steel sheet and the plating layer, that is, near the plating layer position where the Fe concentration is 50% of that of the base steel sheet. This peak in Al concentration suggests that an Fe-Al barrier layer containing an alloy of Fe and Al is formed at the interface between the base steel sheet and the plating layer. As is clear from the relatively high peak of the Al concentration, in aluminium-containing coated steel sheets manufactured by conventional methods, a larger amount of Al in the coating layer is consumed in the formation of the Fe-Al barrier layer, resulting in the formation of a relatively thick Fe-Al barrier layer. Therefore, in Fig. 2(a), it can be seen that the Al concentration decreases significantly from near the interface between the base steel sheet and the coating layer toward the coating surface, and then becomes an almost constant, very low value, and that the Al concentration is a low value of about 0.1% at the center of the coating layer, which corresponds to the midpoint between the coating surface and the coating layer position where the Fe concentration is 50% of that of the base steel sheet.
[0018] In contrast, referring to FIG. 2(b), it can be seen that in the plated steel sheet of FIG. 2(b), the Al concentration near the interface between the base steel sheet and the plated layer is very low compared to that in FIG. 2(a), even though the plated layer has the same Al content as that in FIG. 2(a). Therefore, in the plated steel sheet of FIG. 2(b), a thinner Fe-Al barrier layer is formed compared to that in FIG. 2(a). In relation to this, in FIG. 2(b), even when moving from the vicinity of the interface between the base steel sheet and the plated layer toward the plated surface side, the Al concentration in the plated layer does not decrease significantly, but decreases relatively slowly, and then becomes almost constant, and the Al concentration in the center of the plated layer exceeds about 0.2%, which is a very high value that is about twice as high as that in FIG. 2(a). From the analysis results by GDS in FIG. 2(a) and (b), it is considered that in the plated steel sheet of FIG. 2(b), most of the Al in the plated layer is not consumed in the formation of the Fe-Al barrier layer, but exists as an Al phase in the plated layer other than the Fe-Al barrier layer, for example in a solid solution state. Based on the results of the GDS analysis of these plated steel sheets and the fact that a welded joint obtained by spot welding the plated steel sheet of Fig. 2(b) experimentally showed higher LME resistance than a welded joint obtained by spot welding the plated steel sheet of Fig. 2(a), the inventors conducted further studies, assuming that the Al phase present in the plated layer other than the Fe-Al barrier layer plays a very important role in suppressing or reducing the penetration of molten Zn into the steel sheet during spot welding. As a result, the inventors found that the effect of adding Al to the plated layer can be fully exhibited by controlling the total amount of Al added to a relatively low amount of 1.50 mass% or less to suppress deterioration of LME resistance due to a decrease in the melting point of the plated layer, while controlling the ratio of "Al concentration at the center of the plated layer" to "Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet" within the range of 0.10 to 1.50 when the plated layer is measured by GDS.Furthermore, the present inventors have found that by using such a plated steel sheet, the structure of the initial plating layer changes during spot welding in the separation portion in the heat-affected zone immediately outside the pressure welded portion, more specifically, in the separation portion in the region 500 μm from the end of the pressure welded portion, forming a plating layer in which the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase is 10 to 100%, and in connection with this, the penetration of molten Zn into the steel sheet during spot welding can be significantly suppressed or reduced. In addition to such an improvement in LME resistance, the present inventors have found that the corrosion resistance of the welded portion can also be significantly improved by relatively increasing the ratio of the η phase mainly composed of Zn in the plating layer of the welded portion.
[0019] Without intending to be bound by any particular theory, it is believed that in the welded joint according to the embodiment of the present invention, Al in the initial coating layer acts as follows to suppress or reduce the penetration of Zn, which has been liquefied by the welding heat input during spot welding, into the steel sheet along the grain boundaries. To explain in more detail, first, the Fe-Al barrier layer formed at the interface between the base steel sheet and the coating layer in the coated steel sheet is relatively brittle, and is therefore believed to be relatively easily broken by the stress applied to the steel sheet due to the pressure applied by the electrode during spot welding. The Zn melted during spot welding comes into direct contact with the base steel sheet due to the breakage of the Fe-Al barrier layer, and therefore the risk of the molten Zn penetrating into the steel sheet along the grain boundaries increases. However, when a coated steel sheet having a coating layer having an Al concentration distribution as shown in FIG. 2 is used, Al, which is relatively abundant in the portions of the coating layer other than the Fe-Al barrier layer, comes into direct contact with the base steel sheet together with Zn due to the breakage of the Fe-Al barrier layer. In this case, it is considered that Al in the coating layer reacts with Fe in the base steel sheet due to the heat input during spot welding to form a new Fe-Al barrier layer, and as a result, the broken Fe-Al barrier layer is repaired. That is, since there is a lot of Al in the coating layer other than the Fe-Al barrier layer, even if Zn comes into direct contact with the base steel sheet due to the breakage of the Fe-Al barrier layer during spot welding, a new Fe-Al barrier layer is immediately formed at the breakage part by the Al present in the immediate vicinity. Therefore, the frequency and time of direct contact of molten Zn with the base steel sheet is reduced, and the alloying of Zn in the coating layer is suppressed or the alloying reaction is delayed even by the heat input during spot welding, and a coating layer with a relatively high ratio of η phase is formed in the area immediately outside the pressure welded part compared to the case of conventional spot welding of Zn-based coated steel sheets. In addition, in relation to the formation of such a new Fe-Al barrier layer, it is considered that the penetration of molten Zn into the steel sheet during spot welding can be significantly suppressed or reduced, and therefore it is possible to reliably suppress or reduce the occurrence of LME cracking. Conventionally, plated steel sheets in which Al is added to a Zn-based plating layer have been known.However, by keeping the Al content of the entire plating layer relatively low in consideration of the decrease in the melting point of the plating layer, while increasing the Al content in the plating layer other than the Fe-Al barrier layer, it is possible to change the plating structure of the plated steel sheet in the separation portion immediately outside the pressure welded portion to a structure having a relatively high proportion of the η phase, and in connection with this, it is possible to suppress or reduce the penetration of molten Zn into the steel sheet during spot welding, and further to improve the corrosion resistance of the welded portion. This fact was not previously known, and has now been revealed for the first time by the present inventors.
[0020] Hereinafter, each component of the welded joint according to the embodiment of the present invention will be described in more detail. In the following description, the unit of content of each element, "%", means "mass%" unless otherwise specified. In addition, in this specification, "~" indicating a numerical range is used to mean that the numerical values before and after it are included as the lower limit and upper limit unless otherwise specified.
[0021] [Plated steel sheet] In a welded joint according to an embodiment of the present invention, at least one of the overlapping steel sheets is a plated steel sheet comprising a base steel sheet and a plating layer formed on at least a surface of the base steel sheet that corresponds to the overlapping surfaces of the steel sheets. The plating layer of this plated steel sheet has the following chemical composition in a separation area outside the heat-affected zone, which is the same as the initial chemical composition before spot welding.
[0022] [Chemical composition of plating layer] [Al: 0.10-1.50%] Al is an element effective in suppressing the penetration of molten Zn into the steel sheet along the grain boundaries. In order to fully obtain such an effect, the Al content is set to 0.10% or more. The Al content may be 0.12% or more, 0.15% or more, 0.18% or more, 0.20% or more, 0.25% or more, 0.30% or more, 0.35% or more, 0.40% or more, more than 0.50%, 0.52% or more, 0.55% or more, more than 0.60%, 0.62% or more, 0.65% or more, or 0.70% or more. On the other hand, if Al is contained excessively, the composition of the coating layer approaches the Zn-Al eutectic composition, so that the melting point of the coating layer decreases. For this reason, Zn in the coating layer becomes more likely to melt during spot welding, which may promote LME cracking. Therefore, the Al content is set to 1.50% or less. The Al content may be 1.45% or less, 1.40% or less, 1.30% or less, 1.20% or less, 1.10% or less, 1.00% or less, 0.90% or less, or 0.80% or less.
[0023] [Fe: 0.01-2.00%] Fe is an element that is inevitably contained in the coating layer, for example, by dissolving from the base steel sheet into the coating bath or by reacting with Al during coating to form an Fe-Al barrier layer at the interface between the base steel sheet and the coating layer. For this reason, in the embodiment of the present invention, the Fe content in the coating layer is 0.01% or more. The Fe content may be 0.04% or more, 0.05% or more, 0.10% or more, 0.15% or more, 0.20% or more, 0.25% or more, 0.30% or more, 0.40% or more, or 0.50% or more. On the other hand, if the Fe content in the coating layer is too high, Al in the coating layer may combine with Fe, or a large amount of Al may be consumed to form the Fe-Al barrier layer. As a result, the effect of adding Al, that is, the effect of adding Al, that is, the effect of suppressing or reducing direct contact between molten Zn and the base steel sheet during spot welding by Al in the coating layer, suppressing alloying of Zn in the coating layer, and suppressing or reducing the occurrence of LME cracking, may not be fully exhibited. Therefore, the Fe content is set to 2.00% or less. The Fe content may be 1.80% or less, 1.60% or less, 1.50% or less, 1.30% or less, 1.20% or less, 1.00% or less, 0.90% or less, 0.80% or less, 0.70% or less, or 0.60% or less.
[0024] The basic chemical composition of the plating layer is as described above. In addition, the plating layer may optionally contain Mg: 0-1.500%, Si: 0-1.000%, Ni: 0-1.000%, Ca: 0-4.000%, Sb: 0-0.500%, Pb: 0-0.500%, Cu: 0-1.000%, Sn: 0-1.000%, Ti: 0-1.000%, Cr: 0-1.000%, Nb: 0-1.000% , Zr: 0-1.000%, Mn: 0-1.000%, Mo: 0-1.000%, Ag: 0-1.000%, Li: 0-1.000%, La: 0-0.500%, Ce: 0-0.500%, B: 0-0.500%, Y: 0-0.500%, P: 0-0.500%, and Sr: 0-0.500% may be contained. From the viewpoint of fully exerting the action and function of the above basic components constituting the plating layer, especially Al, the total amount of these optional elements is 5.000% or less. The total amount of the optional elements may be 4.500% or less, 4.000% or less, 3.500% or less, 3.000% or less, 2.500% or less, 2.000% or less, 1.500% or less, or 1.000% or less. These optional elements are described in detail below.
[0025] [Mg:0~1.500%] Mg is an element effective in improving the corrosion resistance of the plating layer. The Mg content may be 0%, but in order to obtain such an effect, the Mg content is preferably 0.001% or more. The Mg content may be 0.010% or more, 0.050% or more, or 0.100% or more. On the other hand, if Mg is contained excessively, a large amount of MgZn-based compounds, which are brittle compounds, may be generated in the plating layer, which may cause a decrease in workability. Therefore, the Mg content is preferably 1.500% or less. The Mg content may be 1.200% or less, 1.000% or less, 0.800% or less, or 0.500% or less.
[0026] [Si:0~1.000%] Si is an element effective for improving the corrosion resistance of the plating layer. The Si content may be 0%, but Si may be contained in the plating layer in an amount of 0.0001% or more, or 0.001% or more, as necessary. On the other hand, if Si is contained excessively, the plating adhesion of the plating layer may decrease. Therefore, the Si content is preferably 1.000% or less. The Si content may be 0.800% or less, 0.500% or less, 0.100% or less, or 0.050% or less.
[0027] [Ni:0~1.000%] Ni is an element effective for improving the corrosion resistance of the plating layer. The Ni content may be 0%, but in order to obtain such an effect, the Ni content is preferably 0.001% or more. The Ni content may be 0.005% or more, 0.010% or more, or 0.020% or more. On the other hand, excessive Ni content may form a large amount of intermetallic compounds, which may reduce the corrosion resistance. Therefore, the Ni content is preferably 1.000% or less. The Ni content may be 0.800% or less, 0.600% or less, or 0.400% or less.
[0028] [Ca: 0-4.000%] Ca is an element effective in ensuring wettability of the plating bath. The Ca content may be 0%, but in order to obtain such an effect, the Ca content is preferably 0.001% or more. The Ca content may be 0.010% or more, 0.100% or more, or 1.000% or more. On the other hand, if Ca is contained excessively, a large amount of hard intermetallic compounds are formed in the plating layer, making the plating layer brittle and reducing the adhesion to the steel sheet. Therefore, the Ca content is preferably 4.000% or less. The Ca content may be 3.000% or less, 2.000% or less, or 1.500% or less.
[0029] [Sb:0~0.500%, Pb:0~0.500%, Cu:0~1.000%, Sn:0~1.000%, Ti:0~1.000%, Cr:0~1.000%, Nb:0~1.000%, Zr:0~1.000%, Mn:0~1.000 %, Mo:0~1.000%, Ag:0~1.000%, Li:0~1.000%, La:0~0.500%, Ce:0~0.500%, B:0~0.500%, Y:0~0.500%, P:0~0.500% and Sr:0~0.500%] Sb, Pb, Cu, Sn, Ti, Cr, Nb, Zr, Mn, Mo, Ag, Li, La, Ce, B, Y, P and Sr may not be contained in the plating layer, but may be present in the plating layer in an amount of 0.0001% or more or 0.001% or more. These elements do not adversely affect the performance of the plated steel sheet as long as they are within a predetermined content range. However, excessive content of each element may reduce corrosion resistance. Therefore, the content of Sb, Pb, La, Ce, B, Y, P and Sr is preferably 0.500% or less, and may be, for example, 0.300% or less, 0.100% or less, or 0.050% or less. Similarly, the content of Cu, Sn, Ti, Cr, Nb, Zr, Mn, Mo, Ag and Li is preferably 1.000% or less, and may be, for example, 0.800% or less, 0.500% or less, or 0.100% or less.
[0030] The remainder of the plating layer other than the above elements is composed of Zn and impurities. The impurities in the plating layer are components that are mixed in due to various factors in the manufacturing process, including raw materials, when the plating layer is manufactured.
[0031] The chemical composition of the plating layer can be determined by dissolving the plating layer in an acid solution containing an inhibitor that suppresses corrosion of the base steel sheet, and measuring the resulting solution using ICP (inductively coupled plasma) optical emission spectroscopy.
[0032] The plating layer may be any plating layer having the above chemical composition, but is not particularly limited thereto. For example, a hot-dip galvanized (GI) layer is preferable. For example, when alloying heat treatment is performed, the Fe content in the plating layer increases, and it may not be possible to obtain the desired chemical composition and the ratio of "Al concentration at the center of the plating layer" to "Al concentration at the plating layer position where the Fe concentration is 50% of that of the base steel sheet" in the final plating layer. The thickness of the plating layer may be, for example, 3 to 50 μm. The coating weight of the plating layer is not particularly limited, but is, for example, 10 to 170 g / m per side. 2 The coating weight of the plating layer is determined by dissolving the plating layer in an acid solution to which an inhibitor that suppresses corrosion of the base steel sheet has been added, and measuring the change in weight before and after pickling.
[0033] [Area ratio of η phase in plating layer of separation part: 10~100%] In an embodiment of the present invention, in the plating layer of the separation part in the region 500 μm from the end of the pressure weld, the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase is 10 to 100%. Since the region 500 μm from the end of the pressure weld corresponds to the region in the heat-affected zone, in general, alloying of Zn is likely to proceed in the plating layer in this region due to heat input during spot welding. In relation to this, the ratio of the Γ phase is high in the plating layer, and the ratio of the η phase mainly composed of Zn (Zn concentration 97 atomic % or more) is relatively low. However, according to an embodiment of the present invention, compared with the case of conventional spot welding of Zn-based plated steel sheet, a plating layer with a relatively high ratio of the η phase is formed in the separation part immediately outside the pressure weld, i.e., in the region 500 μm from the end of the pressure weld, specifically, a plating layer with a ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase of 10% or more is formed as described above. The fact that the ratio of the η phase is relatively high suggests that the alloying of Zn has not progressed sufficiently even with the heat input of spot welding, that is, it can be said that the direct contact between the molten Zn and the base steel sheet is suppressed or reduced. In relation to this, since the penetration of the molten Zn into the inside of the steel sheet during spot welding is suppressed or reduced, it is possible to improve the LME resistance of the obtained welded joint. Therefore, from the viewpoint of improving the LME resistance of the welded joint and further the corrosion resistance of the welded joint, the higher the ratio of the η phase in the plating layer in the separation part just outside the pressure welded part, the better. For example, the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase is preferably 15% or more, more preferably 25% or more, most preferably 40% or more, and may be, for example, 50% or more, 60% or more, or 70% or more. The ratio of the η phase can be increased by increasing the Al content of the entire plating layer and applying a manufacturing method of the plated steel sheet, which will be described in detail later. For example, in order to set the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase to 25% or more or 40% or more, the Al content of the entire coating layer is preferably 0.30% or more, while the upper limit can be appropriately set within a range of 100% or less.For example, the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase may be 95% or less, 90% or less, 85% or less, or 80% or less. Also, the structure of the plating layer in the separation part immediately outside the pressure-welded part is mainly composed of the η phase and the Γ phase. Although not particularly limited, the total area ratio of the η phase and the Γ phase may be 70% or more, or 80% or more. Similarly, the total area ratio of the η phase and the Γ phase may be 100% or less, 95% or less, or 90% or less.
[0034] [Method for measuring the area ratio of η phase in the plating layer of the separation part] The ratio of the η phase in the separation part in the region 500 μm from the end of the pressure weld is determined as follows. First, a cross-sectional sample of the spot weld is prepared, and then a backscattered electron image (BSE image) including the end of the pressure weld is obtained by a scanning electron microscope with an electron probe microanalyzer (SEM-EPMA). From the BSE image, the end of the pressure weld of the spot weld and the region 500 μm from the end of the pressure weld toward the separation part (the boundary part between the pressure weld and the separation part) are identified. Next, elemental analysis is performed on the identified boundary part to identify the area ratio of the η phase and the area ratio of the Γ phase at the boundary part. Specifically, the η phase is a phase with a Zn concentration of 97 atomic % or more, an Fe concentration of 3 atomic % or less, and other impurities of 3 atomic % or less, and the Γ phase is a phase with a Zn concentration of 87 atomic % or more, an Fe concentration of 8 to 13 atomic %, and other impurities of 3 atomic % or less. The field of view of the SEM image is 100 μm × 100 μm, and the same elemental analysis is performed on five different points in the boundary area to determine the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase in each field of view. Finally, these are averaged to determine the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase.
[0035] [Ratio of "Al concentration at the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet": 0.10 to 1.50] In an embodiment of the present invention, when the plating layer in the separation part outside the heat-affected zone is measured by glow discharge optical emission spectrometry (GDS), the ratio of "Al concentration at the plating layer center" / "Al concentration at the plating layer position where the Fe concentration is 50% of the base steel sheet" is preferably 0.10 to 1.50. By controlling the ratio of "Al concentration at the plating layer center" to "Al concentration at the plating layer position where the Fe concentration is 50% of the base steel sheet" measured by GDS within such a range, the effect of adding Al to the plating layer can be fully exhibited, and it can be ensured that the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase is controlled within a range of 10 to 100% in the plating layer of the separation part in the region 500 μm from the end of the pressure weld part during spot welding. In the weld joint according to the embodiment of the present invention, the purpose of suppressing or reducing the occurrence of LME cracking during spot welding can be achieved by controlling the chemical composition of the plating layer and the ratio of the η phase in the plating layer in the separation part immediately outside the pressure weld part within the range described above. Therefore, the above requirements of the GDS are not essential technical features for achieving the object of the present invention, but are merely one of the preferred means for reliably controlling the ratio of the η phase in the coating layer of the separation portion within a desired range. Although not particularly limited, the ratio of "Al concentration at the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" may be, for example, 0.15 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more. Similarly, the ratio of "Al concentration at the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" may be 1.40 or less, 1.30 or less, 1.20 or less, 1.10 or less, or 1.00 or less.
[0036] [Method for measuring the ratio of "Al concentration at the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet"] The ratio of "Al concentration at the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" is determined as follows. First, a coated steel sheet sample is obtained by cutting into a size of 50 mm x 50 mm from the separation part outside the heat-affected zone of the welded joint, and then the coated steel sheet sample is measured by glow discharge optical emission spectrometry (GDS) to obtain the Al concentration distribution from the surface of the coating layer to a depth direction of 100 μm. Next, the Al concentration at the depth position where the Fe strength is 50% of the Fe strength of the base steel sheet (Fe strength at a depth of 100 μm from the surface of the coating layer of the sample) in the GDS measurement is determined as the "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet," and the distance from this depth position to the surface is defined as the thickness of the coating layer. The Al concentration measured by GDS at a position halfway through the thickness of the coating layer is determined as the "Al concentration at the center of the coating layer," and finally the ratio of "Al concentration at the center of the coating layer" / "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" is determined.
[0037] [Base material steel plate] In an embodiment of the present invention, the base steel sheet for forming the above-mentioned plating layer is not particularly limited and may be any appropriate material, particularly a cold-rolled steel sheet. For example, the base steel sheet may be a material having a chemical composition such that the tensile strength of the plated steel sheet is 780 MPa or more. In general, it is known that LME cracking occurs more significantly when a steel sheet having a relatively high strength is spot-welded, and the higher the strength of the steel sheet, the higher the susceptibility to LME cracking tends to be. Therefore, when a plated steel sheet having a high tensile strength of 780 MPa or more is used in a welded joint, the effect of suppressing LME cracking becomes particularly remarkable.
[0038] [Preferable chemical composition of base steel plate] As described above, the present invention aims to provide a welded joint capable of suppressing or reducing the occurrence of LME cracking during spot welding, and achieves the objective by making at least one of a plurality of overlapping steel sheets a plated steel sheet having a plated layer at least on a surface corresponding to the overlapping surface, controlling the plated layer to have a predetermined chemical composition in a separation part outside the heat-affected zone, and controlling the ratio of the area ratio of the η phase of the plated layer to the total area ratio of the η phase and the Γ phase in the separation part in a region 500 μm from the end of the pressure-welded part within a range of 10 to 100%. Therefore, it is clear that the chemical composition of the base steel sheet having the above-mentioned plated layer is not an essential technical feature for achieving the objective of the present invention. Hereinafter, a preferred chemical composition of the base steel sheet for plated steel sheets useful for use in welded joints according to embodiments of the present invention will be described in detail. However, these descriptions are intended to merely exemplify preferred chemical compositions of the base steel sheet for plated steel sheets having a tensile strength of 780 MPa or more at which the occurrence of LME is prominent when spot welded, i.e., plated steel sheets having a particularly prominent effect of suppressing LME cracking, and are not intended to limit the present invention to those using base steel sheets having such specific chemical compositions.
[0039] In an embodiment of the present invention, for example, the base steel plate has, in mass%, C: 0.01-0.50%, Si: 0.01 to 3.50%, Mn: 0.10-5.00%, P: 0.100% or less, S: 0.0300% or less, N: 0.0100% or less, O: 0 to 0.020%, Al: 0-1.000%, B: 0~0.010%, Nb: 0 to 0.150%, Ti: 0 to 0.20%, Mo: 0-3.00%, Cr: 0-2.00%, V: 0~1.00%, Ni: 0-2.00%, W: 0 to 1.00%, Ta: 0 to 0.10%, Co: 0-3.00%, Sn: 0-1.00%, Sb: 0-0.50%, Cu: 0-2.00%, As: 0~0.050%, Mg: 0~0.100%, Ca: 0 to 0.100%, Zr: 0 to 0.100%, Hf: 0~0.100%, REM: 0~0.10, and Remainder: Fe and impurities It is preferable that the composition of the element is as follows: Each element will be described in more detail below.
[0040] [C: 0.01~0.50%] C is an element that inexpensively increases tensile strength and is an important element for controlling the strength of steel. In order to fully obtain such an effect, the C content is preferably 0.01% or more. The C content may be 0.05% or more, 0.08% or more, 0.09% or more, 0.10% or more, 0.11% or more, 0.12% or more, or 0.15% or more. On the other hand, excessive C content may cause a decrease in elongation. For this reason, the C content is preferably 0.50% or less. The C content may be 0.40% or less, 0.35% or less, or 0.30% or less.
[0041] [Si: 0.01-3.50%] Si acts as a deoxidizer and is an element that suppresses the precipitation of carbides during the cooling process during cold-rolled sheet annealing. In order to fully obtain such an effect, the Si content is preferably 0.01% or more. The Si content may be 0.10% or more, 0.12% or more, 0.15% or more, 0.30% or more, or 0.80% or more. On the other hand, excessive Si content may increase the steel strength and decrease the elongation. For this reason, the Si content is preferably 3.50% or less. The Si content may be 2.50% or less, 2.00% or less, or 1.50% or less.
[0042] [Mn: 0.10~5.00%] Mn is an element that affects the ferrite transformation of steel and is effective in increasing strength. In order to fully obtain such effects, the Mn content is preferably 0.10% or more. The Mn content may be 0.50% or more, 1.00% or more, or 1.50% or more. On the other hand, excessive Mn content may increase the steel strength but decrease the elongation. For this reason, the Mn content is preferably 5.00% or less. The Mn content may be 4.00% or less, 3.00% or less, or 2.50% or less.
[0043] [P:0.100% or less] P is an element that segregates at grain boundaries and promotes embrittlement of steel. Since the lower the P content, the better, it is ideally 0%. However, excessive reduction in the P content may lead to a significant increase in costs. For this reason, the P content may be 0.0001% or more, or may be 0.001% or more, or 0.005% or more. On the other hand, excessive inclusion of P may lead to embrittlement of steel due to grain boundary segregation as described above. Therefore, the P content is preferably 0.100% or less. The P content may be 0.050% or less, 0.030% or less, or 0.010% or less.
[0044] [S:0.0300% or less] S is an element that generates nonmetallic inclusions such as MnS in steel, which leads to a decrease in ductility of steel parts. The lower the S content, the better, so ideally it is 0%. However, excessive reduction in the S content may lead to a significant increase in costs. For this reason, the S content may be 0.0001% or more, or may be 0.0002% or more, 0.0010% or more, or 0.0050% or more. On the other hand, excessive S content may lead to the occurrence of cracks originating from nonmetallic inclusions during cold forming. Therefore, the S content is preferably 0.0300% or less. The S content may be 0.0200% or less, 0.0150% or less, or 0.0100% or less.
[0045] [N:0.0100% or less] N is an element that forms coarse nitrides in a steel sheet and reduces the workability of the steel sheet. Since the lower the N content, the better, it is ideally 0%. However, excessive reduction in the N content may lead to a significant increase in manufacturing costs. For this reason, the N content may be 0.0001% or more, or may be 0.0005% or more, or 0.0010% or more. On the other hand, excessive inclusion of N may form coarse nitrides as described above, reducing the workability of the steel sheet. Therefore, the N content is preferably 0.0100% or less. The N content may be 0.0080% or less, or 0.0050% or less.
[0046] The basic chemical composition of the base steel sheet is as described above. Furthermore, the base steel sheet may contain, as necessary, O: 0-0.020%, Al: 0-1.000%, B: 0-0.010%, Nb: 0-0.150%, Ti: 0-0.20%, Mo: 0-3.00%, Cr: 0-2.00%, V: 0-1.00%, Ni: 0-2.00%, W: 0-1.00%, Ta: 0-0.10%, and / or Fe: 0-0.20%. %, Co: 0-3.00%, Sn: 0-1.00%, Sb: 0-0.50%, Cu: 0-2.00%, As: 0-0.050%, Mg: 0-0.100%, Ca: 0-0.100%, Zr: 0-0.100%, Hf: 0-0.100%, and REM: 0-0.100%. The content of each element may be 0.0001% or more, 0.0005% or more, or 0.001% or more.
[0047] The remainder of the base steel plate other than the above elements is composed of Fe and impurities. The impurities in the base steel plate are components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, when the base steel plate is industrially manufactured.
[0048] The chemical composition of the base steel sheet may be measured by a general analytical method. For example, the chemical composition of the base steel sheet may be measured by first removing the plating layer by mechanical grinding, and then using inductively coupled plasma-atomic emission spectrometry (ICP-AES). C and S may be measured using the combustion-infrared absorption method, N may be measured using the inert gas fusion-thermal conductivity method, and O may be measured using the inert gas fusion-non-dispersive infrared absorption method.
[0049] [Thickness of base steel plate] The thickness of the base steel plate is not particularly limited, and may be, for example, 0.2 mm or more, 0.3 mm or more, 0.6 mm or more, 1.0 mm or more, or 2.0 mm or more. Similarly, the thickness of the base steel plate may be, for example, 6.0 mm or less, 5.0 mm or less, or 4.0 mm or less.
[0050] [Mechanical properties of plated steel sheets] The plated steel sheet useful for use in the welded joint according to the embodiment of the present invention may have any suitable tensile strength, and is not particularly limited, but preferably has a tensile strength of 780 MPa or more. As described above, LME cracking occurs significantly when a steel sheet having a relatively high strength is spot welded. Therefore, when the plated steel sheet has a high tensile strength of 780 MPa or more, the effect of suppressing LME cracking is particularly significant compared to the case of a conventional plated steel sheet having the same tensile strength. For example, in the embodiment of the present invention, the tensile strength of the plated steel sheet may be 980 MPa or more, 1080 MPa or more, or 1180 MPa or more. The upper limit is not particularly limited, but the tensile strength of the plated steel sheet may be, for example, 2300 MPa or less, 2000 MPa or less, 1800 MPa or less, or 1500 MPa or less. The tensile strength is measured by taking a JIS No. 5 test piece from a direction in which the longitudinal direction of the test piece is parallel to the rolling perpendicular direction of the plated steel sheet, and performing a tensile test in accordance with JIS Z 2241:2011.
[0051] <Method of manufacturing plated steel sheets> Next, a preferred method for producing a plated steel sheet useful for use in a welded joint according to an embodiment of the present invention, more specifically, a plated steel sheet having a plated layer in which the ratio of "Al concentration at the center of the plated layer" to "Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet" is 0.10 to 1.50 when measured by glow discharge optical emission spectrometry (GDS), will be described. The following description is intended to exemplify a characteristic method for producing the plated steel sheet, and is not intended to limit the plated steel sheet to one produced by the production method described below.
[0052] The plated steel sheet can be manufactured by, for example, carrying out a casting process in which molten steel with an adjusted chemical composition is cast to form a steel slab, a hot rolling process in which the steel slab is hot rolled to obtain a hot rolled steel sheet, a coiling process in which the hot rolled steel sheet is coiled, a cold rolling process in which the coiled hot rolled steel sheet is cold rolled to obtain a cold rolled steel sheet, a pretreatment process, an annealing process in which the pretreated cold rolled steel sheet is annealed, and a plating process in which a plating layer is formed on the obtained base steel sheet. Alternatively, the cold rolling process may be carried out directly after the hot rolling process without coiling, after which the steel sheet is pickled. Each process will be described in detail below.
[0053] [Casting process] The conditions for the casting process are not particularly limited. For example, after melting in a blast furnace or an electric furnace, various secondary smelting processes may be carried out, and then casting may be carried out by a method such as ordinary continuous casting or casting by an ingot method.
[0054] [Hot rolling process] A hot-rolled steel sheet can be obtained by hot rolling the cast steel slab. The hot rolling step is performed by reheating the cast steel slab directly or after cooling once, and then hot rolling it. When reheating is performed, the heating temperature of the steel slab may be, for example, 1100 to 1250°C. In the hot rolling step, rough rolling and finish rolling are usually performed. The temperature and reduction of each rolling step can be appropriately determined according to the desired metal structure and plate thickness. For example, the end temperature of the finish rolling may be 900 to 1050°C, and the reduction of the finish rolling may be 10 to 50%.
[0055] [Winding process] The hot-rolled steel sheet can be coiled at a predetermined temperature. The coiling temperature can be appropriately determined depending on the desired metal structure, etc., and may be, for example, 500 to 800°C. The hot-rolled steel sheet may be recoiled before or after coiling and subjected to a predetermined heat treatment. Alternatively, the coiling step may be omitted, and the hot-rolled steel sheet may be pickled after the hot-rolling step and then subjected to the cold-rolling step described below.
[0056] [Cold rolling process] After the hot-rolled steel sheet is subjected to pickling or the like, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The rolling reduction in the cold rolling can be appropriately determined according to the desired metal structure and sheet thickness, and may be, for example, 20 to 80%. After the cold rolling process, the steel sheet may be cooled to room temperature, for example, by air cooling.
[0057] [Pretreatment process] Next, it is effective to carry out a predetermined pretreatment process before annealing the cold-rolled steel sheet. Such a pretreatment process may include a degreasing process and an optional grinding process. The degreasing process may include passing an electric current through the cold-rolled steel sheet in a solution having a pH of 8.0 or more (electrolysis process). The current density during the current passing is 1.0 to 8.0 A / dm 2 The current application time may be 5 to 10 seconds. On the other hand, the optional grinding process is preferably performed using a heavy grinding brush. By introducing strain into the surface of the cold-rolled steel sheet by grinding with a heavy grinding brush, the nucleation of the Fe-Al barrier layer is promoted during the plating process after the annealing process, and the Fe-Al barrier layer can be densified. In connection with this, the growth rate of the Fe-Al barrier layer is slowed down, so that the thickness can be reduced. As a result, the amount of Al consumed in the formation of the Fe-Al barrier layer can be reduced. Therefore, the amount of Al in the plating layer other than the Fe-Al barrier layer can be increased, so that the ratio of "Al concentration at the center of the plating layer" to "Al concentration at the plating layer position where the Fe concentration is 50% of that of the base steel sheet" can be increased in the finally obtained plated steel sheet. The grinding process is not particularly limited, but for example, a grinding amount of 10 to 200 g / m is used using a heavy grinding brush. 2 The grinding amount by the heavy grinding brush can be adjusted by any suitable method known to those skilled in the art, and is not particularly limited, but can be adjusted, for example, by appropriately selecting the number of heavy grinding brushes, the rotation speed, the brush pressing amount, and the coating liquid used.
[0058] [Annealing process] The cold-rolled steel sheet that has been subjected to the pretreatment process is annealed. The holding temperature in the annealing process is preferably 700 to 900°C. If the holding temperature in the annealing process exceeds 900°C, an outer oxide layer may be formed on the surface of the steel sheet, and the galvanizing property may be deteriorated. The heating rate to the holding temperature is not particularly limited, but may be 1 to 10°C / sec. The holding time at the holding temperature is preferably 10 to 300 seconds, more preferably 80 to 120 seconds. If the holding time exceeds 300 seconds, the outer oxide may grow excessively, and the galvanizing property may be deteriorated. The dew point of the atmosphere in the annealing process is preferably -20 to 10°C, more preferably -10 to 5°C. If the dew point is too low, an outer oxide layer may be formed on the surface of the steel sheet, and the galvanizing property may be deteriorated. On the other hand, if the dew point is too high, Fe oxide may be formed as an outer oxide on the surface of the steel sheet, and the galvanizing property may be deteriorated. The atmosphere in the annealing step may be a reducing atmosphere, more specifically a reducing atmosphere containing nitrogen and hydrogen, for example a reducing atmosphere containing 1 to 10% hydrogen (for example, 4% hydrogen and the balance nitrogen).
[0059] [Plating process] Next, in the plating process, a plating layer having the above-described chemical composition and structure is formed on at least one, preferably both, surfaces of the cold-rolled steel sheet (base steel sheet). More specifically, the plating process is performed, for example, by hot-dip plating using a plating bath whose components are adjusted so that the chemical composition of the plating layer falls within the above-described range. In the plating process, it is extremely important to first control the time from immersing the steel sheet in the plating bath to the start of cooling to 6 seconds or less, and then control the average cooling rate from the bath temperature (for example, 420 to 480°C) to 370°C to 20°C / second or more. By satisfying these requirements, the Fe-Al barrier layer can be made thin, the amount of Al consumed in forming the Fe-Al barrier layer can be reduced, and the amount of Al present in the plating layer other than the Fe-Al barrier layer can be sufficiently secured. As a result, in the finally obtained plated steel sheet, the ratio of "Al concentration at the center of the plating layer" / "Al concentration at the plating layer position where the Fe concentration is 50% of that of the base steel sheet" can be made 0.10 or more. On the other hand, if any one of these requirements is not satisfied, i.e., if the time from the start of immersion of the steel sheet in the coating bath to the start of cooling exceeds 6 seconds and / or the average cooling rate from the bath temperature to 370°C is less than 20°C / s, a large amount of Al is consumed in forming the Fe-Al barrier layer, and the amount of Al in the coating layer other than the Fe-Al barrier layer decreases. As a result, the desired ratio of "Al concentration in the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" cannot be obtained in the finally obtained coated steel sheet.
[0060] From the viewpoint of further improving the LME resistance of the welded joint, it is preferable that the time from the start of immersion of the steel sheet in the coating bath to the start of cooling is shorter and the average cooling rate from the bath temperature to 370°C is faster. For example, the LME resistance of the welded joint can be further improved by setting the Al content of the entire coating layer to 0.30% or more, setting the time from the start of immersion of the steel sheet in the coating bath to the start of cooling to 4 seconds or less, and setting the average cooling rate from the bath temperature to 370°C to 40°C / second or more. When performing grinding treatment using a heavy grinding brush as the pretreatment process described above, similarly higher LME resistance can be achieved by combining the condition of an Al content of the entire coating layer of 0.30% or more, even if the time from the start of immersion of the steel sheet in the coating bath to the start of cooling is 6 seconds or less and the average cooling rate from the bath temperature to 370°C is 20°C / second or more. Alternatively, the LME resistance of the welded joint can be improved more significantly by setting the Al content of the entire coating layer to 0.30% or more, performing grinding treatment with a heavy grinding brush as the pretreatment process described above, and setting the time from the start of immersion of the steel sheet in the coating bath to the start of cooling to 4 seconds or less and the average cooling rate from the bath temperature to 370°C to 40°C / second or more. The lower limit of the time from the start of immersion of the steel sheet in the coating bath to the start of cooling is not particularly limited, but for example, the time from the start of immersion of the steel sheet in the coating bath to the start of cooling may be 2 seconds or more. Similarly, the upper limit of the average cooling rate from the bath temperature to 370°C is not particularly limited, but for example, the average cooling rate from the bath temperature to 370°C may be 80°C / second or less. Other conditions of the coating process may be appropriately set in consideration of the thickness and adhesion amount of the coating layer, etc. For example, after immersing a cold-rolled steel sheet in a coating bath, it is pulled out and immediately sprayed with N2 gas or air by a gas wiping method, and then cooled, so that the coating weight of the coating layer can be kept within a predetermined range, for example, 10 to 170 g / m per side. 2 can be adjusted within the range.
[0061] In the plated steel sheet produced by this manufacturing method, the ratio of "Al concentration at the center of the plated layer" to "Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet" is controlled within the range of 0.10 to 1.50. Therefore, when used in spot welding, the structure of the initial plated layer changes in the separation area 500 μm from the end of the pressure weld, and a plated layer is formed in which the ratio of the area ratio of the η phase to the total area ratio of the η phase and Γ phase is 10 to 100%. In relation to this, it is possible to significantly suppress or reduce the penetration of molten Zn into the steel sheet during spot welding.
[0062] [Other steel plates] Among the multiple steel sheets used in the welded joint according to the embodiment of the present invention, any appropriate steel sheet or plated steel sheet can be used as a steel sheet other than the plated steel sheet described above. Such a steel sheet may have a tensile strength of 780 MPa or more, as in the preferred embodiment of the plated steel sheet, or may have a tensile strength of less than 780 MPa. Therefore, for the steel sheet other than the plated steel sheet described above, an appropriate steel sheet or plated steel sheet may be appropriately selected depending on the application and desired properties of the welded joint, such as the desired joint strength.
[0063] <Method of manufacturing welded joints> The welded joint according to the embodiment of the present invention can be manufactured by applying any appropriate spot welding method known to those skilled in the art to a plurality of steel sheets in which all the steel sheets are plated steel sheets and the plated steel sheets are stacked together, or to a plurality of steel sheets in which the plated steel sheet is used as one or more steel sheets and the plated steel sheet is stacked together with another steel sheet or another plated steel sheet. For example, the welded joint according to the embodiment of the present invention can be manufactured by forming a nugget and a pressure welded portion around the nugget by applying pressure to the plurality of steel sheets stacked together as described above using a pair of opposing electrodes while passing current between the electrodes under normal conditions. The spot welding conditions may be any appropriate conditions known to those skilled in the art. For example, the welding electrode may be a dome radius type welding electrode with a tip diameter of 6 to 8 mm, the pressure may be 1.5 to 6.0 kN, the current flow time may be 0.1 to 1.0 s (5 to 50 cycles, power supply frequency 50 Hz), the current may be 4 to 15 kA, and the strike angle (the angle between the axial direction of the electrode and the direction perpendicular to the surface of the steel sheet) may be 0 to 10°.
[0064] The welded joint manufactured as described above can fully utilize the effect of adding Al to the coating layer, and can control the ratio of the η phase in the coating layer in the separation part immediately outside the pressure welded part within a desired range, and in connection with this, can suppress or reduce the penetration of molten Zn into the steel sheet during spot welding. Therefore, such a welded joint can achieve better LME resistance than when a conventional coated steel sheet having a coating layer with a similar chemical composition, more specifically, a Zn-based coating layer with a similar Al content, and can contribute to industrial development through improved collision safety and longer life, particularly in the automotive field.
[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. EXAMPLES
[0066] In the following examples, plated steel sheets were produced under various conditions, and the LME resistance of welded joints produced by spot welding the produced plated steel sheets was examined.
[0067] [Manufacturing of plated steel sheets] First, a molten steel having a chemical composition consisting of, in mass%, C: 0.15%, Si: 1.00%, Mn: 2.60%, P: 0.010%, S: 0.0020%, N: 0.0100%, Al: 0.020, and the balance: Fe and impurities was cast by a continuous casting method to form a steel billet, which was once cooled, reheated to 1200 ° C, hot rolled, and then coiled at 600 ° C. The hot rolling was performed by performing rough rolling and finish rolling, the finishing temperature of the finish rolling was 950 ° C, and the rolling reduction of the finish rolling was 30%. Next, the obtained hot-rolled steel sheet was pickled, and then cold-rolled at a rolling reduction of 50% to obtain a cold-rolled steel sheet having a sheet thickness of 1.6 mm. Next, the obtained cold-rolled steel sheet was subjected to a 5.0 A / dm 2 Then, if necessary, a 2.0% NaOH aqueous solution is applied to the cold-rolled steel sheet, and the sheet is polished with a heavy-duty abrasive brush (D-100 manufactured by Hotani Co., Ltd.) at a current density of 10 to 200 g / m. 2 The surface of the cold-rolled steel sheet was ground with a grinding amount of 1.0 mm, a brush reduction amount of 2.0 mm, and a rotation speed of 600 rpm to introduce strain into the surface of the cold-rolled steel sheet. Table 1 shows whether each cold-rolled steel sheet was ground with a heavy grinding brush.
[0068] Next, each cold-rolled steel sheet was cut into a size of 100 mm x 200 mm, and then annealed under conditions of a dew point of 0°C, a holding temperature of 870°C, and a holding time of 100 seconds (annealing atmosphere: hydrogen 4% and nitrogen balance). For all steel sheet samples, the heating rate during annealing was 5°C / sec. Next, the cut steel sheet samples were plated using a hot-dip galvanizing bath having a predetermined bath composition under the conditions of the bath temperature, the time from immersion in the plating bath to the start of cooling, and the average cooling rate from the bath temperature to 370°C shown in Table 1, thereby obtaining plated steel sheet samples in which a plating layer was formed on both surfaces of the steel sheet samples. The plating coverage was 50 g / m per side after immersion in the plating bath, and the steel sheet samples were pulled out and wiped with N2 gas before the start of cooling.2 In Comparative Example 28, after the hot dip galvanizing treatment, an alloying heat treatment was carried out at 520° C. for 10 seconds.
[0069] [Tensile strength of plated steel sheet] The tensile strength was measured by taking JIS No. 5 test pieces with the longitudinal direction parallel to the rolling direction of the plated steel sheet samples and conducting tensile tests in accordance with JIS Z 2241: 2011. As a result, the tensile strength of all plated steel sheet samples was 780 MPa or more.
[0070] [Measurement of Al concentration distribution in plating layer] First, the plated steel sheet sample was cut into a size of 50 mm x 50 mm, and then the cut plated steel sheet sample was subjected to GDS measurement to obtain the Al concentration distribution from the surface of the plated layer to a depth direction of 100 μm. Next, the Al concentration at the depth position where the Fe strength in the GDS measurement was 50% of the Fe strength of the base steel sheet (Fe strength at a depth of 100 μm from the surface of the plated layer of the sample) was determined as the "Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet," and the distance from this depth position to the surface was defined as the thickness of the plated layer. The Al concentration by GDS at a position half the thickness of the plated layer was determined as the "Al concentration at the center of the plated layer," and finally the ratio of "Al concentration at the center of the plated layer" / "Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet" was determined. As a result, in all of the plated steel sheet samples of the examples (invention examples), the ratio of "Al concentration at the center of the plated layer" to "Al concentration at the plated layer position where the Fe concentration is 50% of that of the base steel sheet" was controlled within the range of 0.10 to 1.50.
[0071] [Manufacturing of welded joints] Of the obtained plated steel sheet samples, a plated steel sheet sample having a size of 100 × 100 mm was subjected to spot welding. Two pieces were prepared by cutting to a size of 50 mm × 100 mm, and these two plated steel sheet samples were spot welded using a dome radius type welding electrode having a tip diameter of 8 mm at an impact angle of 5°, a pressure of 4.0 kN, a current flow time of 0.5 seconds, and a current flow current of 9 kA to produce welded joints.
[0072] [Chemical composition analysis of plating layer] The chemical composition of the plating layer was determined by immersing a 30mm x 30mm sample taken from the outer separation area of the heat-affected zone of the welded joint in a 10% HCl solution containing an inhibitor (Ibit, manufactured by Asahi Chemical Industry Co., Ltd.), peeling off the plating layer by pickling, and then measuring the plating components dissolved in the solution by ICP emission spectroscopy. The results are shown in Table 1.
[0073] [Measurement of the area ratio of η phase in the plating layer of the separation part] The ratio of the η phase in the separation part in the region 500 μm from the end of the pressure weld was determined as follows. First, a cross-sectional sample of the spot weld was prepared, and then a BSE image including the end of the pressure weld was obtained by SEM-EPMA. From the BSE image, the end of the pressure weld of the spot weld and the region 500 μm from the end of the pressure weld toward the separation part (the boundary part between the pressure weld part and the separation part) were identified. Next, elemental analysis was performed on the identified boundary part to identify the area ratio of the η phase and the area ratio of the Γ phase at the boundary part. Specifically, the η phase was a phase with a Zn concentration of 97 atomic % or more, an Fe concentration of 3 atomic % or less, and other impurities of 3 atomic % or less, and the Γ phase was a phase with a Zn concentration of 87 atomic % or more, an Fe concentration of 8 to 13 atomic %, and other impurities of 3 atomic % or less. The field of view of the SEM image was 100 μm × 100 μm, and the same elemental analysis was performed on five different points in the boundary, and the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase was obtained in each field of view. Finally, by averaging these, the ratio of the area ratio of the η phase to the total area ratio of the η phase and the Γ phase was determined. In this regard, in the welded joints of all the examples (invention examples), the total area ratio of the η phase and the Γ phase in the separation part in the region 500 μm from the end of the pressure weld was 80% or more.
[0074] [Evaluation of LME resistance] The cross-section of the welded joint produced was polished and then observed under an optical microscope. The length of the LME crack that had occurred in the cross-section of the separation area around the pressure weld was measured, and the LME resistance was evaluated as follows. AAA: No LME cracking, AA: LME crack length 0μm to 100μm, A: LME crack length: over 100μm to 500μm, B: LME crack length over 500μm
[0075] [Evaluation of corrosion resistance of welded joints] The produced welded joints were coated with chemical conversion paint and electrochemical coating, and subjected to a cyclic corrosion test in accordance with JASO (M609-91), to evaluate the corrosion resistance of the spot welds based on the corrosion state of the steel material. After the above corrosion test was completed, the corrosion resistance of the welds was evaluated according to the following criteria, based on the cycles at which red rust appeared, depending on the rust state of the spot welds. AAA: No red rust occurs after 240 to 360 cycles AA: No red rust occurs after 180 to 240 cycles A: No red rust occurs after 90 to 180 cycles B: Red rust occurs after 90 cycles
[0076] Welded joints with LME resistance ratings of AAA, AA, and A were evaluated as being capable of suppressing or reducing the occurrence of LME cracking during spot welding. The results are shown in Table 1 below.
[0077] [Table 1]
[0078] Referring to Table 1, in Comparative Example 26, since the Al content of the entire coating layer was low, the effect of suppressing LME cracking by adding Al could not be fully exhibited, and the LME resistance was reduced. In Comparative Example 27, since the Al content of the entire coating layer was high, it is considered that the melting point of the coating layer was reduced. As a result, Zn in the coating layer was easily melted during spot welding, and the LME resistance was reduced. In Comparative Example 28, the Fe content in the coating layer was increased by the alloying heat treatment, and the desired coating chemical composition was not obtained, and the ratio of "Al concentration at the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" was also less than 0.10. In relation to this, the area ratio of the η phase in the coating layer immediately outside the pressure welded part was 0%. In Comparative Example 28, the desired ratio of "Al concentration at the center of the coating layer" / "Al concentration at the coating layer position where the Fe concentration is 50% of the base steel sheet" was not obtained, so that the Al in the coating layer could not suppress or reduce direct contact between the molten Zn and the base steel sheet during spot welding, and it is considered that alloying of Zn in the coating layer was promoted. As a result, the LME resistance was deteriorated. In Comparative Example 29, since the time from immersion in the coating bath to the start of cooling was long, a lot of Al was consumed in the formation of the Fe-Al barrier layer, and it is considered that the amount of Al in the coating layer other than the Fe-Al barrier layer was reduced. As a result, the ratio of "Al concentration at the center of the coating layer" / "Al concentration at the coating layer position where the Fe concentration is 50% of the base steel sheet" was less than 0.10, and for the same reason as in Comparative Example 28, the ratio of the area ratio of the η phase in the coating layer immediately outside the pressure welded part was reduced, and the LME resistance was deteriorated. In Comparative Example 30, since the average cooling rate from the bath temperature of 370°C was slow, a lot of Al was consumed in forming the Fe-Al barrier layer, which is considered to have reduced the amount of Al in the coating layer other than the Fe-Al barrier layer. As a result, the ratio of "Al concentration in the center of the coating layer" to "Al concentration at the coating layer position where the Fe concentration is 50% of that of the base steel sheet" was less than 0.10, and for the same reason as in Comparative Examples 28 and 29, the area ratio of the η phase in the coating layer immediately outside the pressure welded part decreased, and the LME resistance decreased.In addition, in Comparative Examples 26 and 28 to 30, in which the area ratio of the η phase in the plating layer immediately outside the pressure welded portion was low, the proportion of the Zn-based η phase was low, and therefore the welded portion corrosion resistance also decreased.
[0079] In contrast, in the welded joints of all the examples, the specified plating chemical composition was used, and the area ratio of the η phase in the plating layer immediately outside the pressure weld was controlled within the range of 10 to 100%, thereby fully exerting the effect of adding Al to the plating layer and reliably suppressing or reducing LME cracking. Furthermore, the high ratio of the η phase, mainly composed of Zn, also improved the corrosion resistance of the weld. In particular, in Examples 3 to 5 in which the Al content of the entire coating layer was 0.30% or more and grinding with a heavy abrasive brush was performed as a pretreatment for the annealing process (however, the time from the start of immersion of the steel sheet in the coating bath to the start of cooling was 6 seconds and the average cooling rate from the bath temperature to 370°C was 20°C / sec) and in Example 16 (without grinding with a heavy abrasive brush) in which the Al content of the entire coating layer was 0.30% or more, the time from the start of immersion of the steel sheet in the coating bath to the start of cooling was 4 seconds and the average cooling rate from the bath temperature to 370°C was 40°C / sec, the area ratio of the η phase in the coating layer immediately outside the pressure welded portion was 25% or more, and as a result, the evaluations of LME resistance and weld corrosion resistance were also AA, and the LME resistance and weld corrosion resistance were further improved. In addition, in Examples 6 to 15, 17, and 19 to 25, in which the Al content of the entire coating layer was 0.30% or more, grinding was performed with a heavy abrasive brush as a pretreatment for the annealing process, and the time from the start of immersion of the steel sheet in the coating bath to the start of cooling was 4 seconds and the average cooling rate from the bath temperature to 370°C was 40°C / second, the area ratio of the η phase in the coating layer immediately outside the pressure welded portion was 40% or more, and as a result, the LME resistance and weld corrosion resistance were also evaluated as AAA, and the LME resistance and weld corrosion resistance were further improved. [Explanation of symbols]
[0080] 1 Welded joints 11 Steel plate 12. Nugget 13 Pressure Welding Part 14 Pressure weld end 15 Heat affected zone 16 Spot welds 17 Separation section 18 Plating layer
Claims
1. A plurality of overlapping steel plates; a nugget that joins the plurality of steel plates, and a spot weld having a pressure welded portion and a heat affected zone formed around the nugget; a separation portion located around the pressure-welded portion; A welded joint comprising: At least one of the plurality of steel sheets is a plated steel sheet comprising a base steel sheet and a plating layer formed on at least a surface of the base steel sheet that corresponds to an overlapping surface of the plurality of steel sheets, The plating layer in the separation portion outside the heat-affected zone has, in mass %, Al: 0.10 to 1.50%, and Fe:0.01~2.00% and further comprising Mg: 0-1.500%, Si: 0 to 1.000%, Ni: 0-1.000%, Ca: 0-4.000%, Sb: 0 to 0.500%, Pb: 0 to 0.500%, Cu: 0-1.000%, Sn: 0-1.000%, Ti: 0 to 1.000%, Cr: 0-1.000%, Nb: 0 to 1.000%, Zr: 0 to 1.000%, Mn: 0 to 1.000%, Mo: 0-1.000%, Ag: 0-1.000%, Li: 0 to 1.000%, La: 0 to 0.500%, Ce: 0-0.500%, B: 0 to 0.500%, Y: 0 to 0.500%, P: 0 to 0.500%, and Sr: 0~0.500% At least one of the above is contained in a total amount of 5.000% or less, The balance has a chemical composition consisting of Zn and impurities, A welded joint, characterized in that in the plating layer of the separation portion in a region 500 μm from an end of the pressure-welded portion, a ratio of an area ratio of the η phase to a total area ratio of the η phase and the Γ phase is 10 to 100%.
2. 2. The welded joint according to claim 1, characterized in that the chemical composition contains, in mass%, Al: 0.30 to 1.50%, and in the plating layer of the separation portion in a region 500 μm from an end of the pressure-welded portion, a ratio of an area ratio of the η phase to a total area ratio of the η phase and the Γ phase is 25 to 100%.
3. 2. The welded joint according to claim 1, characterized in that the chemical composition contains, in mass%, Al: 0.30 to 1.50%, and in the plating layer of the separation portion in a region 500 μm from an end of the pressure-welded portion, a ratio of an area ratio of the η phase to a total area ratio of the η phase and the Γ phase is 40 to 100%.
4. The welded joint according to any one of claims 1 to 3, characterized in that the plating layer is a hot-dip galvanized (GI) layer.
5. The welded joint according to any one of claims 1 to 3, characterized in that the plated steel sheet has a tensile strength of 780 MPa or more.
Citation Information
Patent Citations
Hot dip galvanized steel sheet excellent in plating adhesion
JP2000119832A
Method for producing hot dip galvannealed steel sheet having pure zinc layer
JP2005248236A
Hot-dip galvannealed steel sheet having excellent plating adhesion
JP2010043296A
Hot dip galvannealed steel sheet and method for producing the same
JP2010222674A
Spot welding method
JP2017047475A