Solder supply method
The method of monitoring solder levels and adjusting Bi content in solder baths using low-Bi alloys addresses Bi content fluctuations, ensuring consistent solderability and reducing environmental and cost burdens in Bi-containing soldering processes.
Patent Information
- Application Number
- JP2024105827
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2044-06-30
AI Technical Summary
Existing methods for soldering using Bi-containing solder alloys in immersion or flow methods face challenges in maintaining the Bi content at a predetermined level due to consumption of Sn and generation of dross, leading to increased Bi content, which affects solderability and results in poor soldering and environmental and cost issues.
A method involving a liquid level sensor to monitor the molten solder level, with additional supply of a low-Bi solder alloy to maintain the Bi content at the initial level, using alloys with adjusted Bi content and optional elements like In, Zn, Mn, Cr, Co, Fe, Si, Al, Ti, Ag, Cu, Ni, Sb, and rare earth elements, and periodic removal of dross to adjust the Bi content to the initial composition.
Maintains the Bi content in the solder bath, preventing solderability issues, reducing environmental impact, and minimizing costs by ensuring consistent soldering quality and process efficiency.
Smart Images

Figure 0007587198000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for supplying solder to a solder bath. [Background technology]
[0002] Electronic devices such as televisions, video recorders, radios, computers, copiers, and communication devices use printed circuit boards with electronic components mounted on them. These electronic components must be firmly fixed to the printed circuit board and must have good electrical conductivity with the printed circuit board. For this reason, solder alloys are used to connect the electronic components to the printed circuit board.
[0003] In recent years, electronic components have become smaller, and the thermal load during soldering has become greater, so soldering at low temperatures is desired. Lowering the soldering temperature reduces the load on electronic components and boards during soldering, and also reduces the environmental load. To solder at low temperatures, a solder alloy with a low melting point can be used.
[0004] As disclosed in JIS Z 3282 (2017), examples of low-melting-point solder alloys include Sn-58% Bi by mass and Sn-52% In by mass. The melting temperatures of these alloys are 139°C and 119°C, respectively, and both are representative alloy compositions of low-melting-point solders. In particular, Sn-58% Bi by mass is widely used as a low-cost solder alloy.
[0005] There are two methods for using solder alloys: the immersion method and the flow method. The immersion method involves melting solder in a solder bath and then contacting a printed circuit board with the molten solder to adhere the solder to the soldered portion. The flow method involves soldering a printed circuit board by jetting the molten solder from a jet nozzle installed in a solder bath that contains the molten solder.
[0006] As described above, each method uses a technique of contacting the printed circuit board with molten solder in a solder bath. However, when soldering a printed circuit board with Cu electrodes or Cu wiring using the dipping method or flow method, the Cu content in the molten solder increases because many printed circuit boards are brought into contact with the molten solder in the solder bath, which can cause problems such as an increase in the melting point and poor soldering.
[0007] Therefore, for example, Patent Document 1 proposes a method of additionally supplying a solder alloy with a low Cu content to a solder bath. In the invention described in this document, a solder alloy with a low Cu content is additionally supplied to the solder bath, so that the Cu content of the molten solder in the solder bath can be returned to a predetermined Cu content. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 3312618 Summary of the Invention [Problem to be solved by the invention]
[0009] However, the invention described in Patent Document 1 is a technology for adjusting the Cu content of molten solder. For example, as described above, a solder alloy mainly composed of Bi, which is known as a low melting point solder alloy, has a lower melting point and a lower Sn content than a solder alloy containing Cu. For this reason, when a solder alloy mainly composed of Bi is used in a dip method or a flow method, the amount of Cu dissolved into the molten solder is less than that of the Cu-containing solder alloy described in Patent Document 1. This is considered to be because the increase in the Cu content is more gradual in the solder alloy mainly composed of Bi than in the solder alloy described in Patent Document 1. Therefore, in consideration of the maintenance period, etc., when a solder alloy mainly composed of Bi is used in a dip method or a flow method, it is not realistic to apply the technology described in Patent Document 1.
[0010] In addition, when using SnBi solder alloys in the dipping method or flow method, there is a concern that the change in the Bi content may affect the desired characteristics when soldering a large number of printed circuit boards. This is because, for example, as is clear from the equilibrium diagram, in the SnBi eutectic solder alloy, the melting point increases when the Bi content changes, and there is a concern that the solderability may be impaired.
[0011] Therefore, an object of the present invention is to provide a solder supplying method that maintains the Bi content in the solder alloy in a solder bath at a predetermined amount even after a large number of boards have been soldered with the Bi-containing solder alloy. [Means for solving the problem]
[0012] The present inventors have studied the cause of the change in the Bi content in the molten solder when soldering a printed circuit board by the dipping method or the flow method, and have found that this is because the molten solder in the solder bath comes into contact with a large number of printed circuit boards during soldering. Accordingly, the present inventors have found that when a SnBi solder alloy is used in the dipping method or the flow method, the Sn in the solder alloy in the solder bath is consumed because soldering is performed continuously, and the Bi content increases relatively.
[0013] In the dipping and flow soldering methods, the time that the molten solder is in contact with the board during soldering is short, and the mass of Sn consumed to join one printed circuit board is very small. However, even if the mass of Sn consumed to join one printed circuit board is small, the number of printed circuit boards soldered in mass production is large. Therefore, the mass of Sn consumed from the molten solder in the solder bath ultimately becomes large. As a result, the mass of Sn contained in the molten solder is much reduced from the initial input composition. Thus, when an SnBi solder alloy is used in the dipping and flow soldering methods, the Bi content becomes relatively high.
[0014] In addition, in the immersion method and the flow method, the molten solder in the solder bath adheres to the board, so when soldering a large number of boards, the mass of the solder alloy in the solder bath decreases. Furthermore, in molten soldering, dross is generated by the reaction of the solder alloy with oxygen, so the mass of the solder in the solder bath decreases when the dross is removed. In the immersion method and the flow method, the board is soldered by contacting it with the molten solder, and if the liquid level of the molten solder is not within a specified range, normal soldering cannot be performed. In other words, if the solder alloy in the solder bath adheres to the board and decreases when soldering a large number of boards, and the liquid level of the molten solder drops, the molten solder cannot contact the board flowing at a certain position, and poor soldering occurs.
[0015] For this reason, a level sensor is installed in the solder bath to constantly monitor the level of the molten solder, and when the mass of the molten solder decreases and the level of the molten solder drops, the level sensor sounds an alarm. When this alarm is sounded, an operator or an automatic supply device supplies solder bars or solder wires to the solder bath to maintain a specified level.
[0016] In general, when the liquid level of the molten solder drops, the Bi-containing solder alloy supplied to the solder bath has the same Bi content as the Bi content of the initial composition. For example, if the Bi content is 58 mass%, the solder alloy supplied has a Bi content of 58 mass%. In addition, in the past, in order to suppress deviation in the composition after additional supply, the Bi-containing solder alloy of the initial composition was introduced into the solder bath after all the solder alloy in the solder bath was drawn out of the solder bath. Alternatively, about half the mass of the Bi-containing solder alloy in the solder bath was replaced with the Bi-containing solder alloy of the initial composition.
[0017] In this way, when a solder alloy of the same composition as that initially charged is additionally supplied to a molten solder bath with a reduced Sn content, the above-mentioned findings indicate that the Bi content in the molten solder in the solder bath increases from a predetermined amount as the number of boards to be soldered increases. Also, as the amount of used solder alloy recovered from the solder bath increases, problems such as an increase in environmental load, an increase in soldering process time, and an increase in soldering costs have arisen.
[0018] As described above, in the dipping method and the flow method, a large number of substrates are brought into contact with the molten solder in a solder bath, and as a result, Sn is consumed and the Bi content increases relatively. Therefore, the inventors of the present invention have focused on the fact that if the relatively increased Bi content can be returned to the initial Bi content at the time of input, the above-mentioned concerns caused by the increase in Bi content can be resolved, and have completed the present invention. The completed present invention is as follows.
[0019] (1) A solder supplying method, characterized in that an additional supply solder, which is a low-Bi solder alloy having a lower Bi content than the Sn and / or Bi-containing solder alloy, is supplied to a solder bath into which a Bi-containing solder alloy has been introduced, to adjust the Bi content in the solder bath to the Bi content of the Bi-containing solder alloy when it was initially placed in the solder bath.
[0020] (2) The solder supplying method according to (1) above, wherein the Bi-containing solder alloy and the additionally supplied solder each contain at least one of In, Zn, Mn, Cr, Co, Fe, Si, Al, Ti, Ag, Cu, Ni, Sb, and rare earth elements.
[0021] (3) The solder supplying method according to (1) or (2) above, wherein the Bi-containing solder alloy is a Sn-Bi solder alloy or a Sn-Bi-Ag solder alloy.
[0022] (4-5) A solder supplying method according to any one of (1) to (3) above, in which the Bi-containing solder alloy initially introduced into the solder bath is introduced at predetermined time intervals or at predetermined timings during the time period from when the Bi-containing solder alloy is initially introduced into the solder bath until immediately before additional solder is supplied.
[0023] (6-9) The solder supplying method according to any one of (1) to (5) above, in which additional solder is supplied based on the Bi content constituting the solder alloy in the solder bath immediately before the additional solder is supplied.
[0024] (10 to 13) The solder supplying method according to any one of (6) to (9) above, wherein a Bi-containing solder alloy having a mass approximately equal to the amount of additionally supplied solder is removed from the Bi-containing solder alloy in the solder bath, and then the additionally supplied solder is supplied into the solder bath. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention will be described in more detail below. In this specification, "%" relating to the solder alloy composition is "mass %" unless otherwise specified.
[0026] 1. Solder supply method The solder supplying method according to the present invention is a method for supplying solder to a solder bath containing a Bi-containing solder alloy. The present invention is applicable to soldering using a soldering apparatus equipped with a solder bath.
[0027] The capacity of the solder bath used in the solder supplying method according to the present invention may be large enough to pour in the amount of molten solder required to solder the printed circuit board, and may be, for example, from several grams to several hundred kilograms.
[0028] The initial composition of the solder alloy that is first charged into the solder bath is not particularly limited as long as it is a Bi-containing solder alloy, and examples thereof include a Sn-Bi solder alloy, a Sn-Bi-Ag solder alloy, etc. In the present invention, the "Bi-containing solder alloy" refers to the initial composition that is first charged into the solder bath, unless otherwise specified.
[0029] The Bi content in the Bi-containing solder alloy may be, for example, 10 to 60%, or may be 30 to 60%. Specific examples of the Bi content in the Bi-containing solder alloy include 58%, 57%, 40%, 35%, and 30%.
[0030] The Bi-containing solder alloy used in the present invention may contain at least one of In, Zn, Mn, Cr, Co, Fe, Si, Al, Ti, Ag, Cu, Ni, Sb, and rare earth elements as optional elements. The content of each element is preferably 5% or less in total for at least one of In, Sb, and Zn, and 1% or less in total for at least one of Mn, Cr, Co, Fe, Si, Al, Ti, and rare earth elements. In the present invention, rare earth elements refer to 17 elements including Sc and Y, which belong to Group 3 in the periodic table, and 15 elements of the lanthanum group with atomic numbers 57 to 71.
[0031] Examples of alloy compositions of Bi-containing solder alloys include Sn-57Bi-1Ag (melting temperature: 138-145°C), Sn-58Bi-0.5Sb-0.015Ni (melting temperature: 140-145°C), Sn-57Bi-0.4Ag (melting temperature: 138-141°C), Sn-40Bi-0.5Cu-0.03Ni (melting temperature: 139-174°C), and Sn-35Bi-0.5Cu-0.03Ni (melting temperature: 140-182°C). The melting points in parentheses indicate the temperature range from the solidus temperature to the liquidus temperature.
[0032] The solder alloy may contain unavoidable impurities as long as the properties of the solder alloy in the initial composition are not impaired. The melting temperature of the Bi-containing solder alloy is required to be 190° C. or lower.
[0033] The additional solder supplied to the solder bath is a low Bi solder alloy that has a lower Bi content than the Sn and / or Bi-containing solder alloy. The Bi-containing solder alloy in the solder bath consumes Sn during soldering of the board, so the Bi content increases relatively. For this reason, the Bi content of the additional solder supplied to adjust the Bi content of the solder alloy in the solder bath to the Bi content of the initially added composition must be lower than that of the Bi-containing solder alloy having the initially added composition.
[0034] The Bi content of the low Bi solder alloy may be about 0 to 90% of the Bi content contained in the Bi-containing solder alloy, and may be changed depending on the time of supply. The solder alloy may not contain Bi. The additionally supplied solder may contain unavoidable impurities within a range that does not impair the properties of the Bi-containing solder alloy. The additionally supplied solder may contain the above-mentioned optional elements, like the Bi-containing solder alloy.
[0035] When using additional solder with a Bi content slightly lower than the initially added composition, it may be necessary to increase the amount of additional supply in order to restore the Bi content to the initially added composition. Therefore, the composition of the additional solder can be determined arbitrarily, taking into account the amount of additional supply and the Bi content of the additional solder. However, as mentioned above, the additional solder composition must have a Bi content at least lower than that of the initially added composition.
[0036] In the present invention, the Bi content increased in the solder bath can be adjusted to the Bi content of the Bi-containing solder alloy having the initial composition by using the additionally supplied solder. This is possible because the Bi content of the additionally supplied solder is less than the Bi content of the initial composition. A preferred embodiment will be described later.
[0037] As described above, in the case of soldering using the immersion method or the flow method, it is necessary to periodically remove dross. Also, the more substrates to be soldered, the more solder is consumed for soldering. Therefore, in the present invention, the Bi-containing solder alloy initially introduced into the solder bath may be introduced at predetermined time intervals or at predetermined timings during the time period from when the Bi-containing solder alloy is initially introduced into the solder bath until immediately before the additional solder is supplied.
[0038] The predetermined timing is, for example, the timing for removing dross. The predetermined time is, for example, when the number of boards soldered per unit time is constant over a long period of time, the amount of molten solder in the solder bath decreases according to the soldering time. Under such circumstances, additional solder can be supplied at predetermined time intervals.
[0039] The timing for additionally supplying solder may be, for example, when the liquid level of the Bi-containing solder alloy has dropped by about 1 to 20 mm from the initial liquid level when the Bi-containing solder alloy was poured into the solder bath, or may be 5 to 8 mm. Depending on the liquid level at the time of supply, a low Bi solder alloy with an adjusted Sn or Bi content as described above may be supplied.
[0040] In the present invention, another timing may be based on the content of Bi constituting the solder alloy in the solder bath immediately before the additional supply of solder. For example, additional supply may be performed when the increase rate of the Bi content in the solder bath immediately before the additional supply is 2% or more, or when it is 2.4% or more. This increase rate can be calculated by [{(Bi content immediately before additional supply)-(Bi content in the initial composition)} / (Bi content in the initial composition)]×100(%). The Bi content in the solder bath immediately before the additional supply may be determined, for example, by ICP mass spectrometry.
[0041] In the present invention, the amount of additionally supplied solder can be calculated as follows: (Bi content of the initial input composition)-(Bi content of the additionally supplied solder)=X, and (Bi content just before the additional supply)-(Bi content of the initial input composition)=Y. Using these, the amount can be calculated by (initial input amount) / {(X / Y)+1}. For example, if the initial input amount is 420 kg, the Bi content of the initial input composition is 58 mass%, the Bi content of the additionally supplied solder is 0% (e.g., Sn), and the Bi content just before the additional supply is 59.77 mass%, then X=58, Y=1.77, and therefore (amount of additionally supplied solder)=420 / {(58 / 1.77)+1}≈12.44 kg.
[0042] In the present invention, the additional supply amount of the additional supply solder thus obtained is added to the solder bath, but as described above, when a Bi-containing solder alloy having the same composition as the initially charged composition is periodically supplied, the amount of solder in the solder bath is always almost full. In such a case, before the additional supply solder is supplied, molten solder of approximately the same mass as the additional supply amount of the additional supply solder may be led out of the solder bath. When a Bi-containing solder alloy having the same composition as the initially charged composition is not periodically supplied, the additional supply may be supplied when the amount of solder in the solder bath is reduced by the additional supply amount. The reduction in the amount of solder in the solder bath can be obtained based on the change in the height of the liquid level of the molten solder in the solder bath.
[0043] The difference between the Bi content in the solder bath after the additional solder alloy is added and the Bi content in the initial composition of the Bi-containing solder alloy is preferably small. For example, the ratio of the difference between the Bi content in the initial composition and the Bi content after the additional addition [{(Bi content after additional addition)-(Bi content in the initial composition)} / (Bi content in the initial composition)]×100(%) should be within ±1.0% of the Bi content in the initial composition, and preferably within ±0.57%. Within this range, the properties of the initially added Bi-containing solder alloy are maintained.
[0044] In this embodiment, the supply method focusing on Bi has been described, but it can also be applied to elements whose content increases relatively by soldering. In particular, the content of Ag can be adjusted to the initial input composition by the same method as for Bi.
[0045] According to this embodiment, when soldering is performed using a Bi-containing solder alloy by the immersion method or flow method, even if Sn is consumed from the molten solder in the solder bath and the Bi content increases, the additionally supplied solder is a low Bi solder alloy with less Sn or Bi content than the initial input composition, so the Bi content in the solder bath can be made approximately the same as the initial input composition. Therefore, if additional solder is supplied to the solder bath by the solder supply method of the present invention, the solderability can be prevented from decreasing, and the occurrence of soldering defects is greatly reduced. In addition, the amount of used solder alloy removed from the solder bath that is collected can be reduced, reducing the environmental load, shortening the soldering process time, and further preventing the increase in soldering costs. EXAMPLES
[0046] The present invention will be described with reference to the following examples, but the present invention is not limited to the following examples. Example 1: Using a flow soldering device (MTF-300) manufactured by Senju Metal Industry Co., Ltd., 420 kg of SnBi solder alloy (Bi content was 58 mass%, the remainder being Sn and unavoidable impurities) with the initial composition shown in Table 1 below was added to the solder bath. After that, until additional solder was added, Bi-containing solder alloy with the same composition as the initial composition (additional supply composition 1) was continuously introduced into the solder bath every time dross was removed. Soldering of Cu-clad substrates (Cu area: 200 mm x 350 mm) was continued using the flow method in this solder bath.
[0047] After the Bi content in the solder bath reached 59.77% by mass, Sn (the remainder being unavoidable impurities) was used as additional solder, and the amount of additional solder was calculated to be 12.44 kg. 12.44 kg of molten solder was removed from the solder bath, and 12.44 kg of additional solder Sn (the remainder being unavoidable impurities) (additional supply composition 2) was introduced. The Bi content in the solder bath was measured by ICP analysis using an Agilent Technologies ICP mass spectrometer (ICP-MS) (RF power: 1600 W).
[0048] The Bi content in the molten solder after additional solder having additional supply composition 2 was added to the SnBi solder alloy in the solder bath was measured using the ICP mass spectrometer described above. As a result, the Bi content was 58.25 mass%, which was close to the composition of the solder alloy initially added.
[0049] Examples 2 to 4, Examples 7 to 10 Additional solder was supplied in the same manner as in Example 1, except that the initial input composition, additional supply compositions 1 and 2, additional supply timing, and additional supply amount were as shown in Table 1. As shown in Table 1, in all cases, the composition was close to that of the solder alloy of the initial input composition.
[0050] Examples 5, 6, 11, and 12 A small flow device (Flow Simulator, manufactured by Malcom) was used to solder a Cu-clad board with a Cu area of 70 mm x 100 mm, and additional supply was performed under the conditions shown in Table 1 for the initial input amount, initial input composition, additional supply composition 1, 2, additional supply timing, and additional supply amount. As shown in Table 1, all of the results were close to the composition of the solder alloy with the initial input composition.
[0051] Example 13 In Example 13, a Bi-containing solder alloy (additional supply composition 1) having the same composition as the initial input composition was not introduced into the solder bath, and soldering of a Cu-clad substrate (Cu area: 200 mm x 350 mm) was performed in the same manner as in Example 1 until the liquid level of the molten solder in the solder bath dropped by 5 mm from the initial liquid level. After that, additional supply solder (additional supply composition 2) was supplied until the liquid level returned to the initial level.
[0052] Comparative Example 1 In Example 1, additionally supplied compositions 1 and 2 were the same as the initially charged compositions, and soldering was performed on a Cu-clad substrate (Cu area: 200 mm x 350 mm) in the same manner as in Example 1, with additional solder supply under the conditions shown in Table 1. As shown in Table 1, the Bi content was significantly increased compared to the initially charged composition. All of the solder compositions in Table 1 contain unavoidable impurities.
[0053] [Table 1]
[0054] Thus, it was found that in all of the Examples, the Bi content in the solder bath after the solder of additionally supplied composition 2 was supplied was adjusted to a composition close to the initially charged composition. On the other hand, in Comparative Example 1, after 210 kg, which is half the mass of the solder bath, additionally supplied solder of the same composition as the initially charged composition was supplied, so it was not possible to adjust it to the initially charged composition.
Claims
1. A solder supplying method comprising the steps of: supplying a low-Bi solder alloy having a lower Bi content than the Bi-containing solder alloy, or additional solder which is Sn, to a solder bath into which a Bi-containing solder alloy has been introduced, thereby adjusting the Bi content in the solder bath to the Bi content of the Bi-containing solder alloy when it was initially placed in the solder bath.
2. 2. The solder supply method of claim 1, wherein the Bi-containing solder alloy and the additional supply solder each contain at least one of In, Zn, Mn, Cr, Co, Fe, Si, Al, Ti, Ag, Cu, Ni, Sb, and rare earth elements.
3. 3. The solder supplying method according to claim 1, wherein the Bi-containing solder alloy is a Sn--Bi solder alloy or a Sn--Bi--Ag solder alloy.
4. 3. The solder supply method according to claim 1, wherein the Bi-containing solder alloy initially introduced into the solder bath is introduced at predetermined time intervals or at predetermined timings during a time period from when the Bi-containing solder alloy is initially introduced into the solder bath until immediately before the additional supply solder is supplied.
5. 4. The solder supply method according to claim 3, wherein the Bi-containing solder alloy initially introduced into the solder bath is introduced at predetermined time intervals or at predetermined timings during the time period from when the Bi-containing solder alloy is initially introduced into the solder bath until immediately before the additional supply solder is supplied.
6. 3. The solder supplying method according to claim 1, wherein the additional solder is supplied based on a Bi content constituting the solder alloy in the solder bath immediately before the additional solder is supplied.
7. 4. The solder supplying method according to claim 3, wherein the additionally supplied solder is supplied based on a Bi content constituting the solder alloy in the solder bath immediately before the additionally supplied solder is supplied.
8. 5. The solder supplying method according to claim 4, wherein the additionally supplied solder is supplied based on a Bi content constituting the solder alloy in the solder bath immediately before the additionally supplied solder is supplied.
9. 6. The solder supplying method according to claim 5, wherein the additionally supplied solder is supplied based on a Bi content constituting the solder alloy in the solder bath immediately before the additionally supplied solder is supplied.
10. 7. The solder supply method according to claim 6, further comprising: withdrawing from the solder bath an amount of the Bi-containing solder alloy having a mass approximately equal to the amount of the additionally supplied solder; and then supplying the additionally supplied solder into the solder bath.
11. 8. The solder supply method according to claim 7, further comprising: withdrawing from the solder bath an amount of the Bi-containing solder alloy having a mass approximately equal to the amount of the additionally supplied solder; and then supplying the additionally supplied solder into the solder bath.
12. 9. The solder supply method according to claim 8, further comprising: withdrawing from the solder bath an amount of the Bi-containing solder alloy having a mass approximately equal to the amount of the additionally supplied solder; and then supplying the additionally supplied solder into the solder bath.
13. 10. The solder supply method according to claim 9, further comprising: withdrawing from the solder bath an amount of the Bi-containing solder alloy having a mass substantially equal to the amount of the additionally supplied solder; and then supplying the additionally supplied solder into the solder bath.
Citation Information
Patent Citations
Recycled solder, manufacture thereof, and soldering method
JP2000340947A
Method and device for removing impurity in flow soldering equipment
JP2003136234A
Soldering method