Encapsulating green sheet

A sealing green sheet with tailored glass and zirconia composition addresses load resistance and heat cycle issues in SOFCs, providing durable and airtight sealing.

JP7587456B2Active Publication Date: 2024-11-20NORITAKE MACHINE TECHNO CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021057235
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-11-20
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

The sealing green sheet in solid oxide fuel cells (SOFCs) faces challenges with insufficient load resistance and heat cycle performance due to stress from applied loads and temperature changes, leading to potential cracking and impaired sealing performance.

Method used

A sealing green sheet composed of glass powder, zirconia powder, and organic matter, with specific oxide molar ratios and thermal expansion coefficients, is developed to enhance load resistance and heat cycle performance by adjusting the softening point and thermal expansion mismatch between components.

Benefits of technology

The sealing green sheet maintains high sealing performance under load and withstands heat cycles, ensuring durability and airtightness in SOFCs by balancing strength and flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587456000003
    Figure 0007587456000003
  • Figure 0007587456000001
    Figure 0007587456000001
  • Figure 0007587456000002
    Figure 0007587456000002
Patent Text Reader

Abstract

To provide a green sheet for encapsulation capable of achieving an encapsulation part excellent in load bearing and heat cycle properties.SOLUTION: There is provided a green sheet for encapsulation including glass powder, zirconia powder, and an organic matter, in which a percentage content of the zirconia powder to 100 pts.mass of the glass powder is 5 pts.mass or greater and 25 pts.mass or less. The glass powder has the following composition in molar ratio expressed in terms of oxide: 8-30 mol% of SiO2; 0.5-10 mol% of Al2O3; 5-30 mol% of B2O3; 5-10 mol% of ZnO; and 50-75 mol% of RO, in which R is at least one element selected from a group consisting of Mg, Ca, Ba, Sr, and the glass powder does not substantially include alkali metal elements.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an encapsulating green sheet. [Background technology]

[0002] A single cell of a solid oxide fuel cell (SOFC) has a structure in which a porous fuel electrode (anode) and a porous air electrode (cathode) face each other through a dense solid electrolyte containing an oxide ion conductor. Gas pipes for supplying gas are connected to both electrodes of the SOFC, and a fuel gas (e.g., hydrogen gas) is supplied to the fuel electrode and an oxygen-containing gas (e.g., air) is supplied to the air electrode through the gas pipes. In such a SOFC, if gases are mixed at each electrode, problems such as a decrease in power generation performance may occur. For this reason, it is preferable to seal the space between the gas pipe and the single cell with high airtightness, and for example, a glass composition containing glass as a main component (e.g., a sealing green sheet) is used for such sealing (see, for example, Patent Documents 1 to 5).

[0003] In practical use, SOFCs are used as stacks in which a number of unit cells are layered together. In such stacks, interconnectors are used to connect the unit cells together, and the interconnectors electrically connect the unit cells and also serve as separators to separate gases. The sealing green sheet is placed between the unit cell and the interconnector to form a sealing portion therebetween. This bonds the unit cell and the interconnector, enabling the gas to be sealed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6546137 [Patent Document 2] JP 2020-167093 A [Patent Document 3] Patent No. 5128203 [Patent Document 4] Patent No. 5280963 [Patent Document 5] Special Publication No. 2008-529256 Summary of the Invention [Problem to be solved by the invention]

[0005] In the stack, since the sealing green sheet is installed between the single cell and the interconnector, the sealing portion formed by the sealing green sheet is always under load. Therefore, if the strength of the sealing portion is insufficient, the sealing portion is crushed and flows due to the load, and the joining function and gas sealing function of the sealing portion may be impaired. Therefore, it is desirable that the sealing portion has a shape retention (load resistance) to such an extent that it does not flow and spread from the installed position even when a load is applied. In addition, since the SOFC is operated at high temperatures (e.g., 800°C or higher), the sealing portion may be exposed to a wide range of temperature changes from room temperature to high temperatures. At this time, stress is generated in the sealing portion due to the temperature change, so that cracks occur in the sealing portion and the sealing property may be impaired. Therefore, it is desirable that the sealing portion has the ability to maintain the sealing property (also called "heat cycle property") even when exposed to a heat cycle in which the temperature is raised to a high temperature and then lowered to room temperature.

[0006] The present invention has been made in view of the above circumstances, and a main object of the present invention is to provide a sealing green sheet that realizes a sealing portion having excellent load resistance and heat cycle properties. In addition, according to the present teachings, a glass powder used in the sealing green sheet is provided. [Means for solving the problem]

[0007] In order to impart load resistance and heat cycle resistance to the sealing portion formed by the sealing green sheet, the present inventors have focused on the softening point of the glass powder contained in the sealing green sheet and conducted research. When the softening point of the glass powder is high, the strength of the sealing portion is maintained high even at high temperatures, and the load resistance is excellent, but on the other hand, the stress caused by the heat cycle is not sufficiently alleviated, and cracks are likely to occur. On the other hand, when the softening point of the glass powder is low, the fluidity of the sealing portion increases at high temperatures, so that the stress caused by the heat cycle can be alleviated, but in an environment where a load is applied, the sealing portion is crushed by the load, and the sealing property may be impaired. As a result of intensive research, the present inventors have found that the load resistance and heat cycle resistance of the sealing portion can be achieved by setting the softening point of the glass powder contained in the sealing green sheet to an appropriate range and adding zirconia powder as a filler at a predetermined ratio, and have completed the present invention.

[0008] The sealing green sheet disclosed herein contains glass powder, zirconia powder, and an organic substance, and the content of the zirconia powder is 5 parts by mass or more and 25 parts by mass or less with respect to 100 parts by mass of the glass powder. The glass powder has the following composition in terms of oxide molar ratio: SiO2 8~30mol%, Al2O3 0.5-10mol%, B2O3 5-30mol%, ZnO 5 to 10 mol%, RO 50-75mol% (wherein R is at least one element selected from the group consisting of Mg, Ca, Ba, and Sr) and is characterized in that it contains substantially no alkali metal elements.

[0009] In the above glass powder composition, RO accounts for a large proportion of 50 mol% to 75 mol%, so that the softening point of the glass powder can be appropriately adjusted and stress caused by heat cycles can be alleviated. In addition, by setting the content of zirconia powder as a filler in the above range for the glass powder of this composition, load resistance can be imparted while maintaining heat cycle properties. This allows the realization of a sealing green sheet with excellent load resistance and heat cycle properties.

[0010] In a preferred embodiment of the sealing green sheet disclosed herein, the softening point of the glass powder is 600° C. or more and 750° C. or less, which allows the glass powder to exhibit excellent heat cycle properties even when exposed to a heat cycle from room temperature to a high temperature (e.g., about 850° C.).

[0011] In a preferred embodiment of the encapsulating green sheet disclosed herein, the difference between the thermal expansion coefficient of the glass powder from 30° C. to 500° C. and the thermal expansion coefficient of the zirconia powder from 30° C. to 500° C. is 0.9×10 -6 K -1 As a result, the difference in the volume change rate caused by temperature change between the glass powder and the zirconia powder is small, so that the stress caused by the heat cycle can be further alleviated.

[0012] In a preferred embodiment of the encapsulating green sheet disclosed herein, a disk-shaped test piece having a diameter of 16 mm and a thickness of 1.5 mm is prepared from the encapsulating green sheet, and when the test piece is fired for 2 hours at a temperature of 750° C. in an air atmosphere while applying a load of 7.5 kPa from the thickness direction of the test piece, the compression ratio of the test piece in the thickness direction is 0.9% to 10.5%. This allows the test piece to exhibit high sealing performance even when the sealing part is placed at a position where a load is applied.

[0013] In a preferred embodiment of the sealing green sheet disclosed herein, the glass powder contains BaO in an amount of 19 mol % or more in terms of the molar ratio of the oxide. In a preferred embodiment, the thermal expansion coefficient of the glass powder from 30° C. to 500° C. is 9.7×10 -6 K -1 More than 11.4 x 10 -6 K -1 If the thermal expansion coefficient of the glass powder is within the above range, the thermal expansion coefficient can be matched with that of the sealed member having a relatively high thermal expansion coefficient, such as a metal member, and therefore the sealing property can be further improved. In addition, if the molar ratio of BaO is within the above range, the thermal expansion coefficient of the glass powder can be suitably adjusted.

[0014] In a preferred embodiment of the encapsulating green sheet disclosed herein, the organic material contains an acrylic binder, which enhances the quality stability of the encapsulating green sheet during storage, and allows the encapsulating green sheet to stably maintain its shape even after long-term storage.

[0015] In one embodiment of the encapsulating green sheet disclosed herein, the green sheet further contains an aqueous solvent. According to the technology disclosed herein, even if an aqueous solvent is used, an encapsulating green sheet having excellent load resistance and heat cycle properties is realized. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is an exploded perspective view showing a schematic diagram of a SOFC system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, preferred embodiments of the technology disclosed herein will be described. Note that matters other than those specifically mentioned in this specification (e.g., the configuration of the sealing green sheet, etc.) that are necessary for implementation (e.g., the general manufacturing process of SOFC and the configuration of the SOFC system, etc.) can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The content of the technology disclosed here can be implemented based on the content disclosed in this specification and the technical common sense in the field. Note that in this specification, "A to B (where A and B are any value)" means "A or more and B or less," and includes a range above A and below B.

[0018] In this specification, the term "green sheet" can include a sheet in a completely unfired state (raw sheet), as well as a sheet dried at a temperature of 100°C or less (dried sheet) and a sheet pre-fired at a temperature of 150°C or less (pre-fired sheet). In this specification, the term "thermal expansion coefficient" refers to the average linear expansion coefficient measured using a thermomechanical analyzer. For example, in accordance with JIS R 3102 (1995), the term refers to the average linear expansion coefficient when a sample is heated at a constant rate of 10°C / min. In the following description, unless otherwise specified, the term "thermal expansion coefficient" refers to the average linear expansion coefficient when the temperature is raised from 30°C to 500°C.

[0019] <Sealing green sheet> The sealing green sheet disclosed herein is intended to form a sealing portion between two or more sealed members by placing it between the members and firing it. This sealing green sheet contains glass powder, zirconia powder, and an organic substance as essential components. Other properties are not particularly limited and can be determined arbitrarily in light of various standards. For example, various components can be blended and the composition can be changed. In this specification, the term "powder" includes cullet, powder, frit, and the like.

[0020] The glass powder is a component that functions as an inorganic binder and acts to enhance the adhesion and bonding between the members to be sealed. In addition, the glass powder disclosed herein has appropriate fluidity at high temperatures (e.g., 750°C to 900°C), and can impart appropriate strength and fluidity to the sealing portion formed by the sealing green sheet. This allows the load-bearing capacity of the sealing portion to be maintained even at high temperatures, while mitigating the stress generated in the sealing portion due to the heat cycle from room temperature to high temperatures.

[0021] In order to provide the sealing portion with suitable fluidity at high temperatures (e.g., 750°C to 900°C), the softening point of the glass powder is preferably 750°C or lower, more preferably 740°C or lower, and may be, for example, 730°C or lower. If the softening point of the glass powder is too low, the fluidity becomes too high at high temperatures (e.g., 750°C to 900°C), and the load-bearing capacity is significantly impaired. Therefore, the softening point of the glass powder is, for example, preferably 600°C or higher, more preferably 620°C or higher, and may be, for example, 640°C or higher. In this specification, the term "softening point" refers to the temperature at which glass begins to soften and deform under its own weight, and is the temperature at which glass begins to soften and deform under its own weight. 7.6 This is the temperature at which the viscosity is dPa·s. This softening point can be measured in accordance with JIS R 3103-1 (2001).

[0022] The coefficient of thermal expansion (CTE) of the glass powder is not particularly limited. In one example, the coefficient of thermal expansion of the glass powder is approximately the same as the coefficient of thermal expansion of the member to be sealed (for example, the difference between the two is 2×10 -6 K -1 This reduces the difference in volume change between the sealing portion and the sealed member, improving the adhesion and bonding of the sealing portion. The thermal expansion coefficient of the glass powder is, for example, 9×10 -6 K -1 Above, 9.7×10 -6 K -1 may be greater than or equal to 10.3×10 -6 K -1The thermal expansion coefficient of the glass powder may be, for example, 12×10 -6 K -1 Less than or equal to 11.4×10 -6 K -1 may be less than or equal to 10.8 x 10 -6 K -1 It may be the following:

[0023] The glass powder disclosed herein contains at least SiO2, Al2O3, B2O3, ZnO, and RO (R is at least one element selected from the group consisting of Mg, Ca, Ba, and Sr) as its constituent components. The glass powder is thus composed of a multi-component system, which improves chemical resistance. In addition, the glass powder is characterized by being substantially free of alkali metal elements (Li, Na, Ka, Rb, Cs, and Fr).

[0024] The silicon component (typically SiO2) is a component that constitutes the skeleton of glass, has high thermal stability, and adjusts the softening point of glass. When the entire glass powder is taken as 100 mol% in terms of oxide molar ratio, SiO2 is preferably 8 mol% or more, and may be 12 mol% or more, or may be 15 mol% or more. Moreover, SiO2 is preferably 30 mol% or less (for example, 29.4 mol% or less), and may be 25 mol% or less, or may be 20 mol% or less. This allows the softening point of the glass powder to be suitably adjusted.

[0025] The aluminum component (typically Al2O3) is a component that controls the fluidity of the glass powder when it melts (when the temperature of the glass powder is equal to or higher than the softening point) and is also involved in adhesion stability. When the entire glass powder is taken as 100 mol% in terms of oxide molar ratio, Al2O3 is preferably 0.5 mol% or more, may be 1 mol% or more, or may be 2 mol% or more. Moreover, Al2O3 is preferably, for example, 10 mol% or less, may be, for example, 5 mol% or less, or may be, for example, 2.5 mol% or less. According to such a range, the fluidity of the glass powder when it melts can be suitably controlled, and the load resistance and heat cycle property of the sealing part can be improved.

[0026] The boron component (typically B2O3) is a component that contributes to adjusting the softening point of the glass powder. When the entire glass powder is taken as 100 mol% in terms of oxide molar ratio, B2O3 is preferably 5 mol% or more (e.g., 7 mol% or more), may be 10 mol% or more, or may be 15 mol% or more. Moreover, B2O3 is preferably, for example, 30 mol% or less (e.g., 29.7 mol% or less), may be 25 mol% or less, for example, 20 mol% or less. According to such a range, the softening point of the glass powder is suitably adjusted, and the load resistance and heat cycle property of the sealing part can be improved.

[0027] The zinc component (typically ZnO) is a component that adjusts the fluidity of the glass powder when melted and improves the airtightness and stability of the sealing portion. When the entire glass powder is taken as 100 mol% in terms of molar ratio of oxide, ZnO is preferably 5 mol% or more, and may be 6 mol% or more. Moreover, ZnO is preferably 10 mol% or less, more preferably 8 mol% or less, and may be, for example, 7 mol% or less. Within this range, the high temperature viscosity of the glass powder can be suitably adjusted, and the load resistance and heat cycle properties of the sealing portion can be suitably realized.

[0028] The Group 2 element component (typically RO: at least one selected from the group consisting of MgO, CaO, BaO, and SrO) is a component that improves the thermal stability of the glass powder and adjusts the softening point and thermal expansion coefficient of the glass powder. When the entire glass powder is taken as 100 mol% in terms of a molar ratio of oxide, the glass powder contains RO at 50 mol% or more, for example, 52 mol% or more, or 55 mol% or more. This allows the softening point and thermal expansion coefficient of the glass powder to be suitably adjusted. Although not particularly limited, RO is, for example, 75 mol% or less, may be 65 mol% or less, or may be 60 mol% or less. RO may be composed of any one of MgO, CaO, BaO, and SrO, but is preferably composed of two kinds, and more preferably three or more kinds. In one preferred example, RO is composed of MgO, CaO, and BaO. By RO being composed of multiple components, the thermal expansion coefficient and softening point of the glass powder can be more suitably adjusted and the chemical resistance can be improved.

[0029] MgO is a component that contributes to adjusting the viscosity when the glass powder is melted. The glass powder does not need to contain MgO, but preferably contains MgO. When MgO is contained and RO is composed of two or more oxides, when the whole glass powder is taken as 100 mol% in terms of molar ratio of oxide, MgO is preferably 5 mol% or more (for example, 5.6 mol% or more), and may be 10 mol% or more. In addition, although not particularly limited, MgO is, for example, 25 mol% or less, and may be, for example, 15 mol% or less, and may be 12 mol% or less. Within such range, the viscosity when the glass powder is melted can be suitably adjusted, and the load resistance and heat cycle property of the sealing part can be improved.

[0030] CaO is a component that can improve the hardness of glass and improve the wear resistance and load resistance. The glass powder does not need to contain CaO, but it is preferable that it contains CaO. When CaO is contained and RO is composed of two or more oxides, when the whole glass powder is taken as 100 mol% in terms of molar ratio of oxide, CaO is preferably 5 mol% or more, may be 10 mol% or more, or may be 20 mol% or more. In addition, although not particularly limited, CaO is preferably 35 mol% or less (for example, 30.1 mol% or less), and may be, for example, 25 mol% or less. Within such a range, the load resistance and wear resistance of the sealing part can be suitably improved.

[0031] BaO is a component that can improve high heat resistance and high temperature durability. The glass powder does not need to contain BaO, but it is preferable that it contains BaO. When BaO is contained and RO is composed of two or more oxides, BaO is preferably 19 mol% or more (for example, 19.6 mol or more) and may be 25 mol% or more when the whole glass powder is taken as 100 mol% in terms of molar ratio of oxide. In addition, although not particularly limited, BaO is preferably 45 mol% or less, more preferably 40 mol% or less, and may be, for example, 35 mol% or less. Within such ranges, the thermal expansion coefficient and softening point of the glass powder can be suitably adjusted.

[0032] Oxides of alkali metal elements (e.g., Li2O, Na2O, K2O, etc.) are components that lower the glass transition point and increase the fluidity during glass melting. If such components are contained in the glass powder, the fluidity becomes too high in a high-temperature environment, and the load-bearing capacity is impaired. Therefore, it is preferable that the glass powder does not substantially contain alkali metal elements. Here, "substantially does not contain" means that unavoidable mixing is allowed. In other words, when the entire glass powder is taken as 100 mol% in terms of molar ratio of oxides, the alkali metal elements are less than 0.5 mol% in terms of molar ratio of oxides, more preferably 0.3 mol% or less, even more preferably 0.1 mol% or less, and particularly preferably 0 mol% (i.e., not contained).

[0033] The glass powder may contain any additive components other than the above-mentioned components, as long as the effects of the technology disclosed herein are not impaired. Examples of the additive components include Cu, Fe, Ni, Zr, La, Sn, and Ti.

[0034] The average particle size of the glass powder is not particularly limited, but is typically nanometer to micron size. When the average particle size is 0.1 μm or more, for example 0.5 μm or more, the handling and workability during molding of the encapsulation green sheet can be improved. When the average particle size is about 40 μm or less, for example 30 μm or less, the encapsulation temperature can be set low, and thermal shrinkage (distortion due to thermal stress) during firing can be better suppressed. In this specification, the "average particle size" refers to the particle size (particle diameter) corresponding to the cumulative 50% from the fine particle side in the volume-based particle size distribution measured by the laser diffraction / light scattering method.

[0035] Zirconia (ZrO2) powder is a highly heat-resistant filler and is a component that improves the shape retention (load resistance) of the sealing part. By including zirconia powder, the sealing green sheet is less likely to be compressed in the load direction even in a load-bearing environment, and therefore can exhibit good load resistance.

[0036] The thermal expansion coefficient of the zirconia powder is not particularly limited, but is preferably about the same as that of the glass powder. For example, the difference between the thermal expansion coefficient of the zirconia powder and the thermal expansion coefficient of the glass powder is 0.9×10 -6 K -1 It is preferable that the value is equal to or less than 0.8×10 -6 K -1 or less), e.g. 0.6×10 -6 K -1 may be less than or equal to 0.3 x 10 -6 K -1 Within this range, the difference in volume change caused by temperature change between the zirconia powder and the glass powder is small, so that the stress caused by the heat cycle can be further alleviated.

[0037] The zirconia powder is not particularly limited as long as it contains zirconia. For example, commercially available zirconium dioxide, zircon sand, zircon flower, desiliconized zirconia, fused zirconia, etc. can be appropriately selected and used. In addition, stabilized zirconia stabilized with at least one of yttria, calcia, magnesia, scandia, and ceria, that is, yttria stabilized zirconia (YSZ), calcia stabilized zirconia (CSZ), magnesia stabilized zirconia (MSZ), scandia stabilized zirconia (ScSZ), ceria stabilized zirconia (CeSZ), etc. can be used. The stabilized zirconia may be partially stabilized partially stabilized zirconia.

[0038] Among these, it is preferable to use stabilized zirconia as the zirconia powder. Stabilized zirconia has high stability at high temperatures and can have a thermal expansion coefficient similar to that of the glass powder disclosed herein, so that cracks are unlikely to occur in the sealing portion. In one suitable example, YSZ is used as the stabilized zirconia powder. The thermal expansion coefficient of YSZ is, for example, 10×10 -6 K -1 ~11×10 -6 K -1 Therefore, the difference in thermal expansion coefficient between the glass powder and the glass powder disclosed herein is small. As a result, the difference in volume change due to temperature is small, and the occurrence of cracks can be suitably prevented.

[0039] The average particle size of the zirconia powder is not particularly limited, but is typically equal to or smaller than the average particle size of the glass powder. This allows a homogeneous sealing portion to be suitably realized. As an example, the average particle size is preferably about 30 μm or less, typically 20 μm or less, for example, about 2 μm to 15 μm.

[0040] Zirconia powder can improve the load resistance of the sealing part, but if the content of zirconia powder is too high, the sealing part cannot have appropriate fluidity at high temperatures. This causes insufficient relaxation of stress caused by heat cycles, and cracks are likely to occur in the sealing part. Therefore, the content of zirconia powder relative to 100 parts by mass of glass powder is appropriate to be 25 parts by mass or less, and preferably 20 parts by mass or less. In addition, if the content of zirconia powder is low, the load resistance of the sealing part may be insufficient. Therefore, the content of zirconia powder is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more.

[0041] The organic material is not particularly limited, and one or more of various components known to be added to general sealing materials can be appropriately selected and used. Examples of organic materials include organic binders, dispersants, thickeners, surfactants, plasticizers, defoamers, antioxidants, preservatives, antistatic agents, pH adjusters, colorants, and organic solvents. Among them, from the viewpoint of improving the handling and workability when applying the sealing green sheet to the member to be sealed, it is preferable to contain an organic binder. Also, from the viewpoint of improving the work efficiency (typically shortening the drying time), it is preferable to not contain an organic solvent.

[0042] The organic binder is a component that enhances the shape integrity of the sealing green sheet. Examples of the organic binder include acrylic resins, epoxy resins, phenolic resins, amine resins, alkyd resins, and cellulose polymers. Among them, it is preferable to include an acrylic resin. By including an acrylic resin, the adhesiveness of the sealing green sheet to the member to be sealed can be increased, and the handling and workability during the formation of the sealing portion can be improved. In addition, the quality stability during storage can be improved, and the shape of the sealing green sheet can be stably maintained, for example, even after long-term storage. Examples of the acrylic resin include a polymer containing an alkyl (meth)acrylate as a main monomer (a component that accounts for 50% by mass or more of the total monomers) and a copolymer containing such a main monomer and a sub-monomer that is copolymerizable with the main monomer. In this specification, "(meth)acrylate" is a term that means acrylate and methacrylate.

[0043] Since organic matter is a component that can burn out during firing, if the content in the sealing green sheet is too high, the denseness of the sealing portion may be impaired, and the sealing property may be impaired. Therefore, the content of the organic matter relative to 100 parts by mass of glass powder is, for example, appropriate to be 35 parts by mass or less, may be 25 parts by mass or less, and is preferably 20 parts by mass or less. In addition, although not particularly limited, from the viewpoint of workability, the content of the organic matter may be, for example, 10 parts by mass or more, and may be 15 parts by mass or more.

[0044] The encapsulating green sheet may be composed of the above three components (glass powder, zirconia powder, and organic material), or may contain other optional components in addition to the above three components. Examples of the other optional components include inorganic materials such as various fillers and sintering aids other than zirconia powder.

[0045] The sealing green sheet may contain an aqueous solvent as a solvent. In the technology disclosed herein, even when an aqueous solvent is used, a sealing portion having excellent load resistance and heat cycle properties can be realized. As described above, the sealing green sheet may contain an organic solvent as an organic substance, but the organic solvent requires safety management in compliance with the Fire Service Act and the like, and the operating cost may be high. On the other hand, the aqueous solvent can be preferably used because it can reduce costs, enable safe production, and reduce environmental load. As the aqueous solvent, water such as ion-exchanged water (deionized water), pure water, ultrapure water, and distilled water can be preferably used. In addition, the aqueous solvent may contain a non-aqueous solvent that can be mixed uniformly with water (for example, a solvent that dissolves in water such as a lower alcohol or a lower ketone) as necessary. In this case, it is preferable that 95% by volume or more of the aqueous solvent is water, and it is preferable that 99% by volume or more is water. The amount of the aqueous solvent added is not particularly limited because it can be appropriately adjusted in consideration of the moldability of the sealing green sheet.

[0046] The average thickness of the encapsulating green sheet is not particularly limited, but is generally 50 μm to 2000 μm, typically about 100 μm to 1500 μm. When the average thickness is a predetermined value or more, the mechanical strength can be improved. When the average thickness is a predetermined value or less, the volume change can be suppressed to a small value, and the durability can be improved.

[0047] <Method of manufacturing encapsulation green sheet> The encapsulating green sheet can be produced, for example, as follows: Note that the method for producing the encapsulating green sheet is not limited to this. First, glass powder, zirconia powder, organic substances (e.g., organic binders, dispersants, release agents, etc.), and other optional components are prepared, and these materials are mixed to prepare a composition. The composition can be prepared, for example, by putting the above materials into a mixer such as a ball mill and stirring them homogeneously.

[0048] Next, the obtained composition is granulated (molded) to a predetermined size to obtain so-called crumbly granulated particles. The granulation method is not particularly limited, and for example, spray granulation method (spray dry method), rolling granulation method, fluidized bed granulation method, stirring granulation method, compression granulation method, extrusion granulation method, crushing granulation method, etc. can be adopted. In one preferred example, the spray granulation method is adopted. Specifically, the above composition is prepared in a liquid state, sprayed in a dry atmosphere, and dried to be granulated (molded). In this method, the particles contained in the sprayed droplets are granulated into approximately one mass. Therefore, the size and mass of the granulated particles can be easily adjusted depending on the size of the droplets.

[0049] Next, the granulated particles obtained above are formed into a sheet shape. As a forming method, a roll forming method can be suitably adopted. In the doctor blade method, which is a common sheet forming method, an organic solvent is added to the composition as described above to prepare a slurry, which is then formed using a plate-shaped blade called a doctor blade, and the organic solvent is then dried. For this reason, the slurry needs to have a certain degree of viscosity, which inevitably increases the content of organic substances (typically organic solvents, organic binders, and thickeners). This can result in a longer time required for drying before firing, or environmental hygiene problems during drying.

[0050] On the other hand, in the roll molding method, the raw material powder is compressed by a rotating roll and molded into a sheet. Therefore, the powdered or crumbly raw material can be directly fed into the roll molding machine. That is, it is not necessary to prepare the raw material into a slurry. In the roll molding method, for example, granulated particles are supplied between a pair of rolls rotating in opposite directions, and the granulated particles are compressed between the pair of rolls to be molded into a sheet. Therefore, the roll molding method can reduce the organic matter content and improve the work efficiency. In addition, the roll molding method can suitably manufacture the sealing green sheet even when an aqueous solvent is used instead of the organic solvent, which can lead to reduction in manufacturing costs and improvement of environmental hygiene. Furthermore, the sealing green sheet with excellent homogeneity can be stably molded.

[0051] <Applications of encapsulation green sheets> The sealing green sheet can be used to form a sealing portion by attaching it to a member to be sealed and then firing it. Therefore, compared to a method of applying a paste to a member to be sealed, the convenience of the worker can be improved. The sealing green sheet can be suitably used for electrical and physical sealing bonding between homogeneous or heterogeneous members, for example, sealing bonding between a plurality of metal members, sealing bonding between a plurality of ceramic members, and sealing bonding between a ceramic member and a metal member. In one example, the sealing green sheet is placed between a metal member and a ceramic member (sealing portion), and fired at a temperature range equal to or higher than the softening point of the glass powder contained in the sealing green sheet, generally 600°C or higher, for example, 700°C to 900°C. This allows a sealing portion to be formed between the metal member and the ceramic member. In addition, since the sealing green sheet disclosed herein has excellent load resistance, a sealing portion having high sealing properties can be formed even when fired under a high load (for example, about 7.5 kPa).

[0052] Specific examples of metal members include gas pipes for supplying gas to single cells of the SOFC, and interconnectors arranged between single cells of the SOFC to electrically connect the single cells. Materials for the metal members include stainless steel, aluminum, chromium, iron, nickel, copper, silver, manganese, and alloys thereof. The thermal expansion coefficient of these metal members is 10×10 -6 K -1 ~15×10 -6 K -1 It may be to some extent. Specific examples of ceramic members include anodes and cathodes of SOFCs, and interconnectors. Materials for the ceramic members include alumina, forsterite, titania, yttria, zirconia, stabilized zirconia, and the like. The ceramic members may be a single type of ceramic, or may be a composite material (e.g., mullite, steatite, alumina zirconia, and the like) in which two or more types of ceramics are combined. The thermal expansion coefficient of these ceramic members is 6×10 -6 K -1 ~8×10 -6 K -1 It may be to some extent.

[0053] According to the sealing green sheet disclosed herein, it is possible to seal between various members with high airtightness, and high airtightness can be stably maintained for a long time even under a load environment. For example, even when used in a high temperature range or when heat cycles are repeated in a normal temperature range to a high temperature range, high long-term durability and heat cycle resistance can be realized. Therefore, the sealing green sheet disclosed herein can be suitably used for the construction of, for example, parts that can be exposed to a high temperature range, high-temperature operating devices, specifically, various power generation systems such as SOFCs and power storage elements, manufacturing devices for manufacturing them, environmental devices such as waste incineration devices and exhaust gas removal devices, exhaust gas treatment devices for vehicles, engine combustion test devices, vacuum drying devices, semiconductor devices, and the like. For example, it can be suitably used for the construction of a single cell of SOFC or a stack of SOFCs in which a plurality of the above single cells are electrically connected. In other words, the technology disclosed herein provides a single cell or stack of SOFCs having a sealing portion composed of a sintered body of the sealing green sheet.

[0054] FIG. 1 is an exploded perspective view showing a schematic diagram of an SOFC system 30. The following description will be given with reference to FIG. 1. In the following drawings, members and parts having the same functions are denoted with the same reference numerals, and duplicated descriptions may be omitted or simplified. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not necessarily reflect the actual dimensional relationships. The SOFC system 30 can be manufactured in accordance with a conventionally known manufacturing method.

[0055] The SOFC system 30 includes a plurality of SOFC unit cells 10A, 10B and a plurality of interconnectors 20, 20A. The SOFC system 30 has a stack structure in which the unit cells 10A, 10B are stacked via the metal interconnector 20A. The unit cells 10A, 10B have a sandwich structure in which both sides of a layered solid electrolyte 14 are sandwiched between a layered fuel electrode (anode) 12 and a layered air electrode (cathode) 16. The solid electrolyte 14 is an oxide ion conductor such as yttria stabilized zirconia (YSZ) or gadolinia doped ceria (GDC). The fuel electrode 12 is, for example, nickel (Ni) or a cermet of nickel and YSZ. The air electrode 16 is, for example, a lanthanum cobaltate (LaCoO3)-based or lanthanum manganate (LaMnO3)-based perovskite oxide. In the unit cells 10A and 10B, the fuel electrode 12 is formed to be thicker than the solid electrolyte 14 and the air electrode 16. The unit cells 10A and 10B are so-called anode-supported cells (ASC), in which the fuel electrode 12 functions as a support.

[0056] Interconnector 20A, located in the center of the drawing, is sandwiched on both sides between unit cells 10A, 10B, with one opposing surface 22 facing air electrode 16 of unit cell 10A and the other opposing surface 26 facing fuel electrode 12 of unit cell 10B. A sintered body (not shown) of the sealing green sheet disclosed herein is disposed between opposing surfaces 22, 26 of interconnector 20A and the corresponding opposing surfaces of fuel electrode 12 or air electrode 16 of unit cells 10A, 10B, respectively, to form a sealing portion.

[0057] A plurality of grooves are formed on the opposing surface 22 of the interconnector 20A, forming an oxygen-containing gas flow path 24 through which a supplied oxygen-containing gas (typically air) flows. A plurality of grooves are also formed on the opposing surface 26, forming a fuel gas flow path 28 through which a supplied fuel gas (typically H2 gas) flows. In the interconnector 20A, the oxygen-containing gas flow path 24 and the fuel gas flow path 28 are perpendicular to each other.

[0058] When the SOFC system 30 is in operation, a fuel gas (here, hydrogen (H2) gas) is supplied to the fuel gas flow passage 28, and an oxygen (O2)-containing gas (here, air) is supplied to the oxygen-containing gas flow passage 24. In the SOFC system 30, oxygen is reduced to oxide ions at the air electrode 16. The oxide ions reach the fuel electrode 12 via the solid electrolyte 14, oxidize the fuel gas, and release electrons. This generates electrical energy.

[0059] Although the single cells 10A and 10B of the SOFC shown in FIG. 1 are planar, the present invention is not limited thereto and various other shapes are possible. For example, a conventionally known polygonal type, a cylindrical type, or a flat tubular type in which the peripheral side of a cylinder is vertically crushed can be adopted. In addition to the anode-supported type (ASC) disclosed herein, the flat SOFC can be, for example, an electrolyte-supported type (ESC) in which the solid electrolyte is thickened, or a cathode-supported type (CSC) in which the cathode is thickened. In addition, a metal-supported cell (MSC) in which a porous metal sheet is inserted under the anode (the side away from the solid electrolyte) can be adopted. The size of the SOFC is not particularly limited.

[0060] Test examples relating to the technology disclosed herein will be described below, but it is not intended that the technology disclosed herein be limited to those shown in these test examples.

[0061] <Test 1> In Test 1, 12 types of sealing green sheets were produced, Examples 1 to 12. Specifically, in each example, glass powder (average particle size: 25 μm) having the glass composition shown in Table 1 and zirconia powder (yttria-stabilized zirconia, average particle size: 2 μm, coefficient of thermal expansion (CTE) 10.5×10 -6 K -1 ) and organic matter (acrylic binder (ESZ-4366-02) manufactured by Japan Coating Resin Co., Ltd., glycerin as a plasticizer, and Cellosol 920 manufactured by Chukyo Yushi Co., Ltd. as a mold release agent) were prepared. In each example, 10 parts by mass of zirconia powder and 16 parts by mass of organic matter were mixed with respect to 100 parts by mass of glass powder to obtain a mixed powder. Next, water was added to the obtained mixed powder and kneaded in a pot mill for 24 hours to prepare an aqueous slurry. Thereafter, the obtained aqueous slurry was granulated by spray drying to obtain a granulated powder having an average particle size of about 30 μm. Then, the obtained granulated powder was pressure-molded into a sheet shape (thickness: 1.5 mm) by roll molding to obtain the sealing green sheets of Examples 1 to 12. The physical properties (coefficient of thermal expansion (CTE), transition point (Tg), softening point (Ts)) of the glass powder contained in the sealing green sheet of each example are as shown in Table 1. Table 1 also shows the difference (ΔCTE) between the thermal expansion coefficient of the glass powder and the thermal expansion coefficient of the zirconia powder.

[0062] [He gas leak evaluation test] A disk-shaped test piece with a diameter of 16 mm and a thickness of 1.5 mm was prepared from the obtained sealing green sheet. Next, a doughnut-shaped measuring jig (made of SUS403) with an opening in the center was prepared, and the test piece was placed so as to close the opening of the jig. Then, an alumina plate was placed on the test piece via NCA-1 foil, and a crucible with an adjusted weight was placed on the alumina plate so that a load of 7.5 kPa was applied in the thickness direction of the test piece. Then, in this state, a firing process was performed in an electric furnace in an air atmosphere at 750°C for 2 hours. This formed a sealing part that sealed the opening of the measuring jig.

[0063] Next, a gas leak evaluation device with a cylindrical measurement section with an open top was prepared, and a measurement jig with a sealing section was attached so as to cover the top of the cylindrical measurement section. He gas was then supplied into the inside of the measurement section to increase the pressure to 5 kPa, after which the internal pressure of the measurement section was maintained for 1 minute while being measured. The amount of He gas leakage (Pa m 3 ·sec -1 The evaluation of the amount of He gas leakage at this time is shown in "First joining" in Table 1. The amount of He gas leakage was calculated as 1×10 -5 Pa·m 3 ·sec -1 The following cases are evaluated as "〇" and 1×10 -5 Pa·m 3 ·sec -1 Cases where the number was greater than this were rated as "X".

[0064] [Thermal cycle test] Next, a thermal cycle test was performed on the measurement jig on which the sealing portion was formed, in which the amount of He gas leakage at the time of initial bonding was measured, and the sealing property after the thermal cycle (heat cycle) was evaluated. The thermal cycle test was performed while applying a load of 7.5 kPa in the thickness direction of the sealing portion in the same manner as when the sealing portion was formed. The measurement jig on which the sealing portion was formed was heated from room temperature to 850°C in an electric furnace under an air atmosphere and maintained for one hour. Then, the temperature was lowered from 850°C to room temperature. This heating and lowering from room temperature to 850°C was considered as one cycle, and a total of 10 cycles were performed. Then, the amount of He gas leakage was measured in the same manner as in the gas leakage test described above. The evaluation of the amount of He gas leakage at this time is shown in "After the thermal cycle test" in Table 1. The evaluation criteria are the same as those for "At the time of initial bonding."

[0065] [Table 1]

[0066] As shown in Table 1, in Examples 1 to 7, the amount of He gas leakage was small both before and after the heat cycle test. In this test, the test pieces were sintered while applying a load (7.5 kPa) to form the sealing portion, so those that were evaluated as "good" in the He gas leakage evaluation test at the time of initial bonding were found to have load resistance. In addition, in Examples 1 to 7, the evaluation of the He gas leakage test after the heat cycle test was "good," so it is found that excellent heat cycle properties are achieved by using a glass powder having a specified composition (SiO2, Al2O3, B2O3, ZnO, and RO) in a specified range in combination with a zirconia powder.

[0067] <Test 2> In Test 2, the amount of zirconia powder added to the glass powder was examined. The zirconia powder used in Test 1 was prepared so that it was 0, 3, 5, 10, 15, 20, 25, and 30 parts by mass relative to 100 parts by mass of the glass powder used in Example 1. Other than this, green sheets were prepared in the same manner as in Test 1, and sealing green sheets of Examples 1 and 13 to 19, which have different amounts of zirconia powder added, were obtained. Using the obtained sealing green sheets, a He gas leakage evaluation test and a thermal cycle test were performed in the same manner as in Test 1. The results are shown in Table 2. In each example, the thickness of the test piece (sealing portion) after firing under a load of 7.5 kPa was measured, and the compression ratio in the thickness direction ((thickness before firing-thickness after firing) / thickness before firing x 100) was calculated. The results are shown in Table 2.

[0068] [Table 2]

[0069] As shown in Table 2, in Example 1 and Examples 15 to 18, the amount of He gas leakage was small both before and after the heat cycle test. This shows that excellent load resistance and heat cycle properties are achieved by including 5 parts by mass or more and 25 parts by mass or less of zirconia powder per 100 parts by mass of glass powder. In Examples 13 and 14, the results of the He gas leakage evaluation test from the initial bonding are considered to be due to the fact that the strength of the green sheet is weak due to the small amount of zirconia powder added, and the thickness cannot be maintained due to the load during the firing process. On the other hand, in Example 19, the flexibility is insufficient due to the large amount of zirconia powder added, and cracks occur due to stress caused by temperature changes, so the result of the He gas leakage evaluation test is considered to be "X". This shows that the appropriate compression ratio in the thickness direction of the sealing green sheet is within the range of 0.9% to 10.5%.

[0070] Although specific examples of the technology disclosed herein have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]

[0071] 10A, 10B SOFC single cell 12 Fuel electrode (anode) 14 Solid electrolyte 16 Air electrode (cathode) 20, 20A Interconnector 30 SOFC system

Claims

1. A sealing green sheet containing glass powder, zirconia powder, and an organic substance, The content of the zirconia powder relative to 100 parts by mass of the glass powder is 5 parts by mass or more and 25 parts by mass or less, The softening point of the glass powder is 600° C. or more and 750° C. or less, the difference between the thermal expansion coefficient of the glass powder from 30° C. to 500° C. and the thermal expansion coefficient of the zirconia powder from 30° C. to 500° C. is 0.9×10 −6 K −1 or less; The glass powder has the following composition in terms of oxide molar ratio: SiO 2 8~30mol%、 Al 2 9 3 0.55100%、 B 2 O 3 5~30mol%、 ZnO 5-10 mol%, RO 50-75mol% (wherein R is at least one element selected from the group consisting of Mg, Ca, Ba, and Sr). and the green sheet for sealing does not contain an alkali metal element or, even if it inevitably contains an alkali metal element, the molar ratio calculated as the oxide is less than 0.5 mol %.

2. 2. The sealing green sheet according to claim 1, wherein a disk-shaped test piece having a diameter of 16 mm and a thickness of 1.5 mm is prepared from the sealing green sheet, and fired at a temperature of 750° C. in an air atmosphere for 2 hours while applying a load of 7.5 kPa from the thickness direction of the test piece, and the compression ratio of the test piece in the thickness direction is 0.9% or more and 10.5% or less.

3. 3. The sealing green sheet according to claim 1, wherein the glass powder contains BaO in an amount of 19 mol % or more in terms of a molar ratio calculated as oxide.

4. The thermal expansion coefficient of the glass powder from 30° C. to 500° C. is 9.7×10 -6 K -1 11.4 x 10 -6 K -1 The encapsulating green sheet according to any one of claims 1 to 3, wherein:

5. 5. The sealing green sheet according to claim 1, wherein the organic matter contains an acrylic binder.

6. The sealing green sheet according to any one of claims 1 to 5, wherein the zirconia powder comprises a stabilized zirconia powder stabilized with at least one selected from the group consisting of yttria, calcia, magnesia, scandia and ceria.

7. The encapsulating green sheet according to any one of claims 1 to 6, further comprising an aqueous solvent.

Citation Information

Patent Citations

  • Ryutaikudo no danseifukuroryonohonpu

    JP1976028203A

  • Cushion frame

    JP1977080963A

  • Glass ceramic composition for substrate

    JP2007254213A

  • Low-alkali sealing frits and seals and devices using such frits

    JP2008529256A

  • High-temperature glass solder and its use

    JP2011168480A