Microencapsulated polyaddition catalysts
Microencapsulated polyaddition catalysts with acrylic copolymer shells and intermolecular anhydrides address the viscosity issues in chemically curing resins, enabling controlled release for optimal curing times in construction and manufacturing processes.
Patent Information
- Application Number
- JP2023023736
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-03-09
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2038-03-08
AI Technical Summary
Conventional chemically curing resins exhibit a continuous increase in viscosity, leading to an uncomfortably short open time and undesirably extended drying time, making it difficult to achieve optimal curing time optimization for construction and manufacturing applications.
Microencapsulated polyaddition catalysts with a capsule core containing a polyaddition catalyst and an acrylic copolymer shell, where the acrylic copolymer includes intermolecular anhydrides of ethylenically unsaturated carboxylic acids, are used to control the release of the catalyst upon contact with isocyanate-curing substances, such as polyols or water, thereby optimizing curing times.
The microencapsulated catalysts provide a well-defined release mechanism, allowing for extended pot life and rapid curing times, ensuring effective resin application and hardening without premature curing.
Smart Images

Figure 0007587613000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a microencapsulated polyaddition catalyst, its preparation method and its use.
[0002] In the construction and manufacturing industry, chemically curable resins that exist as one- or two-component systems are often used to fasten components or coat surfaces. When using these resins, it is desirable to optimize the curing time, which consists of two points: the so-called open time (also called gel time or pot life) is the period during which the reactive system can be processed unaffected, and the drying time indicates the point of curing at which it becomes tacky. On the one hand, it is desirable to have a pot life as long as possible, for example to allow rational working by applying the resin over a wide area and, if necessary, subsequent joining of the components within the time required for operation. On the other hand, it is desirable to have a curing time as short as possible, so that the joint hardens quickly, does not shift the components, avoids subsequent soiling, and / or allows for early use, for example accessibility of floor coatings.
[0003] Resin curing is typically achieved using a catalyst to catalyze a polymerization reaction, such as a polyaddition reaction between reactive resin components. In most conventional resin systems, a continuous increase in viscosity is observed, and the open time is often reached after an inconveniently short time for the user, yet the drying time is undesirably extended.
[0004] Attempts have already been made to encapsulate polyaddition catalysts, so that their release is delayed and rapid curing occurs only when the catalyst is released. Depending on the nature of the capsules in terms of wall size, type, thickness, etc., the time until release, i.e. the opening time, can be defined and optimized.
[0005] Adv. Mater. 2016, DOI: 10.1002 / adma.201600830 describes the production of thermally latent catalytic nanocapsules. The capsule core consists of isooctane and dimethyltin neodecanoate, and the capsule shell consists of poly(methyl methacrylate-co-butyl methacrylate-co-methacrylic acid) crosslinked via butanediol dimethacrylate. The capsules are produced by miniemulsion technology. The only stimulus described for catalyst release is the thermal opening of the capsules, which prevents their use at ambient temperature, for example in floor coatings or sealing membranes.
[0006] It is an object of the present invention to provide a microencapsulated polyaddition catalyst which is released upon chemical stimulation, for example upon contact with an isocyanate-curing substance such as a polyol or water.
[0007] This problem is solved by a microencapsulated polyaddition catalyst, which comprises a capsule core containing a polyaddition catalyst and an acrylic copolymer as a capsule shell, where the acrylic copolymer contains copolymerized units of intermolecular anhydrides of ethylenically unsaturated carboxylic acids. The polyaddition catalyst is selected from acyclic tertiary amines, alicyclic tertiary amines, N-alkylimidazoles, phosphines and organometallic salts.
[0008] The copolymerized units of intermolecular anhydrides of ethylenically unsaturated carboxylic acids act as temporary crosslinkers, and the crosslinking action is terminated by solvolysis of the anhydride bonds in the application environment, thereby destabilizing the capsule shell and releasing the capsule contents, including the polyaddition catalyst.
[0009] The average particle size D(0.5) of the microcapsules used according to the invention (volume-weighted average determined by light scattering) is advantageously 1 to 50 μm, preferably 1 to 20 μm, in particular 2 to 10 μm. Here, D(0.5) is defined as the particle size at which the cumulative particle volume reaches 50%. Capsules with this diameter have sufficient mechanical stability to be able to be handled without damage and to be incorporated into the composition to be cured. The size is selected so that unintentional breakage of individual capsules can be tolerated, because unintentional breakage of individual capsules releases only small amounts of polyaddition catalyst, which does not lead to premature curing of the composition. On the other hand, a sufficient amount of catalyst for complete curing is introduced by a capsule volume that can be easily handled.
[0010] In certain embodiments, the microencapsulated polyaddition catalyst is present as a dry powder, granules or agglomerates.
[0011] The weight ratio of the capsule core to the capsule shell is generally 50:50 to 95:5, preferably 60:40 to 94:6, and particularly preferably 70:30 to 93:7.
[0012] As polyaddition catalysts it is possible to use the urethanization catalysts customarily used in polyurethane chemistry: these are compounds which promote the reaction of reactive hydrogen atoms of the isocyanate-reactive component with the organic polyisocyanates.
[0013] Possible polyaddition catalysts are acyclic tertiary amines, alicyclic tertiary amines, N-alkylimidazoles, phosphines and organometallic salts.
[0014] Alicyclic tertiary amines are compounds that have at least one tertiary amine functional group that is not part of a cyclic structure. Examples include triethylamine, tributylamine, N,N-dimethylcyclohexylamine (DMCHA), N-methyldicyclohexylamine, N,N-dimethylbenzylamine (BDMA), N,N-dimethylaminopropylamine, bis-(dimethylaminopropyl)amine, N,N-dimethylaminopropyl-N'-methylethanolamine, dimethylaminoethoxyethanol, bis-(dimethylaminopropyl)amino-2-propanol, N,N-dimethylaminopropyl-dipropanolamine, N,N,N'-trimethyl-N'-hydroxyethyl-bisaminoethyl-ether, N,N-dimethylaminopropylurea, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutylenediamine, and the like. amine, N,N,N',N'-tetramethyl-1,6-hexylenediamine, N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA), N,N,N',N'',N''-pentamethyldipropylenetriamine (PMDPTA), N,N,N-tris-(3-dimethylaminopropyl)-amine, bis-(2-dimethylaminoethyl)-ether (BDMAEE), bis-(dimethylaminopropyl)-urea, 2,4,6-tris(dimethylaminomethyl)phenol, and its salts with 2-ethylhexanoic acid and their isomers; and tris-(dialkylaminoalkyl)-s-hexahydrotriazines such as 1,3,5-tris(3-[dimethylamino]propyl)-hexahydro-triazine.
[0015] Acyclic tertiary amines are compounds that have at least one tertiary amine functional group that is part of a non-aromatic ring structure. Examples include 1,4-dimethylpiperazine (DMP), 1-methyl-4-(2-dimethylaminoethyl)piperazine, 1-aza-bicyclo-[3.3.0]-octane, 1,4-diaza-bicyclo-[2.2.2]-octane (DABCO), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]-non-7-ene (DBN), N-methylmorpholine, N-ethylmorpholine, N-cyclohexylmorpholine, and 2,2'-dimorpholinodiethyl ether (DMDEE).
[0016] Suitable N-alkylimidazoles include N-methylimidazole, 1,2-dimethylimidazole, N-(2-hydroxypropyl)-imidazole, N-(2-hydroxyethyl)-imidazole and N-(2-aminopropyl)-imidazole.
[0017] The phosphines considered as polyaddition catalysts are advantageously tertiary phosphines, such as triphenylphosphine or methyldiphenylphosphine.
[0018] The organometallic salts which come into consideration as polyaddition catalysts are advantageously those of the general formula L m M n+ nA - [In the formula, the ligand L is an organic group or an organic compound selected from alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl and acyl, where the ligand L has 1 to 20 C atoms, and the m ligands L may be identical or different, m is 0, 1, 2, 3, 4, 5 or 6; M is a metal, n is 1, 2, 3, or 4, and Anion A -is a carboxylate ion, an alkoxylate ion, or an enolate ion.
[0019] The metal M is advantageously selected from lithium, potassium, caesium, magnesium, calcium, strontium, barium, boron, aluminum, indium, tin, lead, bismuth, cerium, cobalt, iron, copper, lanthanum, manganese, mercury, scandium, titanium, zinc and zirconium; in particular lithium, potassium, caesium, tin, bismuth, titanium, zinc and zirconium.
[0020] The ligand L is advantageously alkyl having 1 to 20 C atoms. Particularly preferably, L is alkyl having 1 to 10 C atoms, in particular having 1 to 4 C atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl or tert-butyl.
[0021] The carboxylate ion is advantageously of formula R 1 -COO - wherein R 1 is selected from H, alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl and acyl, and the group R 1 has up to 20 C atoms, advantageously from 6 to 20 C atoms. Particularly preferred carboxylate ions are selected from the anions of natural and synthetic fatty acids, such as neodecanoic acid, isooctanoic acid and lauric acid, and the anions of resin acids and naphthenic acids.
[0022] The enolate ion is advantageously of formula R 2 CH=CR 3 -O - wherein R 2 and R 3is selected from H, alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl, and acyl, and each of the groups R 2 and R 3 Each of the has up to 20 C atoms. Particular examples are ethylacetonate, heptylacetonate or phenylacetonate. The enolate ions are advantageously derived from 1,3-diketones having 5 to 8 C atoms. Possible examples include acetylacetonate, the enolate of 2,4-hexanedione, the enolate of 3,5-heptanedione and the enolate of 3,5-octanedione.
[0023] The alkoxylate ion is advantageously of formula R 4 -O - wherein R 4 is selected from alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl and acyl, where the group R 4 has up to 20 C atoms.
[0024] In certain embodiments, the organometallic compound is Alkali metal carboxylates, such as lithium ethylhexanoate, lithium neodecanoate, potassium acetate, potassium ethylhexanoate, cesium ethylhexanoate; alkaline earth metal carboxylates, such as calcium ethylhexanoate, calcium naphthenate, calcium octanoate (available as Octa-Soligen® Calcium from OMG Borchers), magnesium stearate, strontium ethylhexanoate, barium ethylhexanoate, barium naphthenate, barium neodecanoate; Aluminum compounds, such as aluminum acetylacetonate, aluminum diacetate (e.g., K-KAT® 5218 from King Industries); Zinc compounds, such as zinc(II) diacetate, zinc(II) ethylhexanoate and zinc(II) octanoate, zinc neodecanoate, zinc acetylacetonate; Tin compounds, such as tin(II) carboxylates, for example tin(II) acetate, tin(II) octanoate, tin(II) ethylhexanoate, tin(II) neodecanoate, tin(II) isononanoate, tin(II) laurate, and Dialkyltin(IV) salts of organic carboxylic acids, such as dimethyltin diacetate, dibutyltin diacetate, dibutyltin dibutyrate, dibutyltin bis(2-ethylhexanoate), dibutyltin dilaurate, dibutyltin maleate, dioctyltin dilaurate and dioctyltin diacetate, in particular dibutyltin dilaurate; Titanium compounds, such as tetra(2-ethylhexyl) titanate; Zirconium compounds, such as zirconium ethylhexanoate, zirconium neodecanoate, zirconium acetylacetonate (e.g., K-KAT® 4205 from King Industries); Zirconium dionates (e.g., King Industries' K-KAT® XC-9213; XC-A 209, and XC-6212); zirconium-2,2,6,6-tetramethyl-3,5-heptanedionate; Bismuth compounds, such as bismuth carboxylates, in particular bismuth octanoate, bismuth ethylhexanoate, bismuth neodecanoate or bismuth pivalate (e.g. K-KAT® 348, XC-B221; XC-C227, XC-8203 from King Industries, TIB KAT 716, 716LA, 716XLA, 718, 720, 789 from TIB Chemicals, and the products of Shepherd Lausanne); Manganese salts, such as manganese neodecanoate, manganese naphthenate; Cobalt salts, such as cobalt neodecanoate, cobalt ethylhexanoate, cobalt naphthenate; Iron salts, such as iron ethylhexanoate; Mercury compounds, e.g. phenylmercuric carboxylates is selected from.
[0025] Preferred organometallic compounds are dibutyltin dilaurate, dioctyltin dilaurate, zinc(II) diacetate, zinc(II) dioctoate, zirconium acetylacetonate and zirconium-2,2,6,6-tetramethyl-3,5-heptanedionate, bismuth neodecanoate, bismuth dioctoate and bismuth ethylhexanoate.
[0026] The capsule core advantageously comprises, in addition to the polyaddition catalyst, a hydrophobic core material, which allows the production of well-defined capsules of uniform size distribution and reduces the distribution of the polyaddition catalyst released into the application medium as soon as the capsule shell opens.
[0027] The proportion of polyaddition catalyst is advantageously 10-100% by weight, for example 20-90% by weight, in particular 30-70% by weight, based on the total weight of polyaddition catalyst and hydrophobic core material.
[0028] Examples of hydrophobic core materials are aliphatic hydrocarbons, aromatic hydrocarbons, halogenated hydrocarbons, saturated or unsaturated C6-C 30 Fatty acids, fatty alcohols, oxo alcohols, fatty alcohol ethers, C6-C 30 Examples of hydrophobic core materials include fatty amines, fatty acid esters, triglycerides, esters of aliphatic or aromatic polycarboxylic acids, natural and synthetic waxes, and trialkyl phosphates. The hydrophobic core material can also be used as a mixture of two or more materials.
[0029] Suitable substances include, by way of example only: - aliphatic hydrocarbons, for example branched or preferably linear, saturated or unsaturated C 10 ~C 40Hydrocarbons, such as n-tetradecane, n-pentadecane, n-hexadecane, n-heptadecane, n-octadecane, n-nonadecane, n-eicosane, n-heneicosane, n-docosane, n-tricosane, n-tetracosane, n-pentacosane, n-hexacosane, n-heptacosane, n-octacosane, and cyclic hydrocarbons, such as cyclohexane, cyclooctane, cyclodecane; - Aromatic hydrocarbons, such as benzene, naphthalene, biphenyl, o- or m-terphenyls, C1-C 40 Alkyl-substituted aromatic hydrocarbons, such as dodecylbenzene, tetradecylbenzene, hexadecylbenzene, hexylnaphthalene or decylnaphthalene; - halogenated hydrocarbons, such as chloroparaffins, bromooctadecane, bromopentadecane, bromononadecane, bromoeicosane, bromodocosane; - Saturated or unsaturated C6-C 30 fatty acids, such as lauric acid, stearic acid, oleic acid or behenic acid; - mixtures of fatty alcohols, such as lauryl alcohol, stearyl alcohol, oleyl alcohol, myristyl alcohol, cetyl alcohol, coconut oil fatty alcohols, etc., as well as the so-called oxo alcohols which are obtainable by hydroformylation and further reaction of α-olefins; - C6~C 30 fatty amines, such as decylamine, dodecylamine, tetradecylamine or hexadecylamine; - Fatty acid esters, e.g. C1-C fatty acids 10 Alkyl esters, such as propyl palmitate, methyl stearate or methyl palmitate and preferably their eutectic mixtures or methyl cinnamate; - Linear and branched C3-C 21 Triglycerides of carboxylic acids, such as olive oil, soybean oil, corn oil, cottonseed oil, sunflower oil, peanut oil, palm oil, coconut oil and wheat germ oil; - esters of aliphatic or aromatic polycarboxylic acids, in particular the esters of adipic acid, sebacic acid, succinic acid, citric acid, acetylcitric acid, cyclohexane-1,2-dicarboxylic acid or phthalic acid, such as di-2-ethylhexyl adipate, di-n-hexyl adipate, di-n-octyl adipate, diisooctyl adipate, di-n-decyl adipate, diisodecyl adipate, ethylhexyl sebacate, diisodecyl sebacate, di-n-butyl phthalate, di-n-octyl phthalate, di-n-hexyl phthalate, di-n-decyl phthalate, dicyclohexyl phthalate, diisodecyl phthalate, butylcyclohexyl phthalate, diisooctyl phthalate, isooctylisodecyl phthalate; - natural and synthetic waxes, such as Montan acid waxes, Montan ester waxes, Carnauba waxes, polyethylene waxes, oxidized waxes, polyvinyl ether waxes, ethylene vinyl acetate waxes or Fischer-Tropsch hard waxes; - Trialkyl phosphates, for example trimethyl phosphate.
[0030] Of these, the esters of aliphatic or aromatic polycarboxylic acids, particularly the adipates, 1,2-cyclohexanedicarboxylates, phthalates, triglycerides and trialkylphosphates, are generally preferred due to their ready availability and compatibility with the composition to be cured. A particularly preferred hydrophobic core material is 1,2-cyclohexanedicarboxylate diisononyl ester.
[0031] The acrylic copolymers constituting the capsule shell are intermolecular anhydrides of ethylenically unsaturated carboxylic acids, particularly ethylenically unsaturated C3-C 12The copolymer contains copolymerized units of intermolecular anhydrides of carboxylic acids, particularly preferably intermolecular anhydrides of ethylenically unsaturated C3-C8 carboxylic acids. By intermolecular acid anhydrides is meant those which produce two acid molecules upon cleavage of the anhydride bond. The intermolecular anhydrides may include symmetric or asymmetric anhydrides of ethylenically unsaturated carboxylic acids. Examples of suitable ethylenically unsaturated carboxylic acids are acrylic acid, methacrylic acid, ethylacrylic acid, allylacetic acid, crotonic acid, vinylacetic acid, vinylbenzoic acid, etc. Symmetric or asymmetric anhydrides of monoesters of ethylenically unsaturated dicarboxylic acids with each other or with ethylenically unsaturated monocarboxylic acids are also considered. Acrylic anhydride, methacrylic anhydride and 4-vinylbenzoic anhydride are preferred, of which methacrylic anhydride is most preferred.
[0032] In addition to the intermolecular anhydride units of an ethylenically unsaturated carboxylic acid, the acrylic copolymers generally contain copolymerized units of one or more ethylenically unsaturated monomers other than the anhydrides.
[0033] Generally, the acrylic copolymer is (a) Ethylenically unsaturated C3-C 12 5 to 50% by weight, advantageously 10 to 30% by weight, of at least one intermolecular anhydride of a carboxylic acid, (b) C1 to C of acrylic acid 24 Alkyl esters, C1-C methacrylic acid 24 30 to 90% by weight, advantageously 35 to 80% by weight, of at least one monomer selected from alkyl esters and vinyl aromatics, (c) 5 to 20% by weight, preferably 10 to 15% by weight, of at least one monomer having at least two ethylenic unsaturations, and (d) 0 to 30% by weight, preferably 0 to 20% by weight, of one or more other monomers, each based on the total weight of the monomers. It is composed of units.
[0034] Preferred monomers (a) are those mentioned above, especially acrylic anhydride, methacrylic anhydride and 4-vinylbenzoic anhydride, of which methacrylic anhydride is most preferred.
[0035] Suitable monomers (b) are C1-C acrylic and / or methacrylic acid 24 It is an alkyl ester. Suitable monomers (b) are isopropyl acrylate, isobutyl acrylate, sec-butyl acrylate and tert-butyl acrylate and the corresponding methacrylates, and particularly preferably methyl acrylate, ethyl acrylate, n-propyl acrylate and n-butyl acrylate and the corresponding methacrylates. Generally, methacrylates are preferred. Further suitable monomers (b) are vinyl aromatics such as styrene or α-methylstyrene.
[0036] In certain embodiments, the monomer (b) has a glass transition temperature T g and at least one monomer having a glass transition temperature T g The glass transition temperature T g A preferred monomer having a glass transition temperature T of 50° C. or less is methyl methacrylate. g Preferred monomers having the formula: are n-butyl acrylate or n-butyl methacrylate.
[0037] Monomers (c) have at least two ethylenic unsaturations. They cause crosslinking of the capsule shell during polymerization, giving it mechanical stability. Suitable monomers (c) are ethylenically unsaturated monomers with two, three, four or more non-conjugated ethylenic unsaturations. It is preferred to use monomers with vinyl, allyl, acrylic and / or methacrylic groups. Preferred monomers are those which are insoluble or sparingly soluble in water, but have good to limited solubility in lipophilic substances. Sparingly soluble means a solubility of less than 60 g / l at 20°C.
[0038] Suitable monomers with two ethylenic unsaturations are divinylbenzene and divinylcyclohexane; diesters of diols with acrylic or methacrylic acid, as well as the diallyl ethers and divinyl ethers of these diols. Examples include ethanediol diacrylate, ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, methallyl methacrylamide, allyl acrylate and allyl methacrylate. Particularly preferred are propanediol diacrylate, butanediol diacrylate, pentanediol diacrylate and hexanediol diacrylate and the corresponding methacrylates.
[0039] Preferred monomers with 3, 4 or more non-conjugated ethylenic unsaturations are the esters of polyhydric alcohols with acrylic acid and / or methacrylic acid, as well as the allyl and vinyl ethers of these polyhydric alcohols, trivinylbenzene and trivinylcyclohexane. Here, mention may be made, in particular, of trimethylol and pentaerythritol as polyhydric alcohols. Particularly preferred are trimethylolpropane triacrylate and trimethylolpropane trimethacrylate, pentaerythritol triallyl ether, pentaerythritol tetraallyl ether, pentaerythritol triacrylate and pentaerythritol tetraacrylate, and technical mixtures thereof. Pentaerythritol tetraacrylate is therefore generally present in technical mixtures in a mixture with pentaerythritol triacrylate and small amounts of oligomerization products.
[0040] Particularly preferred monomers (c) are 1,4-butanediol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate and triethylene glycol dimethacrylate.
[0041] Optional monomers (d) that come into consideration are other monomers different from the monomers (a) to (c), such as vinyl acetate, vinyl propionate, vinylpyridine, acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinylphosphonic acid, maleic anhydride, 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate, acrylamido-2-methylpropanesulfonic acid, methacrylonitrile, acrylonitrile, methacrylamide, N-vinylpyrrolidone, N-methylol acrylamide, N-methylol methacrylamide, dimethylaminoethyl methacrylate and diethylaminoethyl methacrylate.
[0042] The acrylic copolymers are available in various ways, but are advantageously obtained by free radical suspension polymerization in an oil-in-water emulsion or in a water-in-oil emulsion, the choice of which will be made by the skilled artisan according to the hydrophilic or lipophilic nature of the catalyst to be encapsulated.
[0043] One method of free radical suspension polymerization in a water-in-oil emulsion is described, for example, in International Publication No. WO 2013 / 092158 and International Publication No. WO 2014 / 198531, the contents of which are incorporated by reference in their entireties.
[0044] The microcapsules are advantageously obtained by polymerization of the monomer mixture constituting the capsule shell in the oil phase of a stable oil-in-water emulsion, the oil phase being composed of a hydrophobic material containing a polyaddition catalyst. This preparation method is known per se and is described, for example, in DE 4321205 or WO 2014 / 127951.
[0045] The core of the microcapsules is formed of a hydrophobic material that can be emulsified in water. The hydrophobic material simultaneously functions as a solvent or dispersant for the monomer mixture used in the production of the capsule shell by polymerization. The polymerization is then carried out in the oil phase of a stable oil-in-water emulsion. This emulsion is obtained, for example, by first dissolving the monomer and the polymerization initiator and optionally a chain transfer agent in the hydrophobic material and emulsifying the solution thus obtained in an aqueous medium containing an emulsifier and / or a protective colloid. However, it is also possible to first emulsify the hydrophobic phase or its components in the aqueous phase and then add the monomer or the polymerization initiator and optionally further auxiliaries to be used in combination, such as a protective colloid or a chain transfer agent, to the emulsion. In another variant of this method, it is also possible to emulsify the hydrophobic material and the monomer in water and subsequently add only the polymerization initiator. Since the hydrophobic material is microencapsulated as completely as possible in the emulsion, advantageously only hydrophobic materials are used that have limited solubility in water. The solubility should advantageously not exceed 5% by weight at 25°C. To completely encapsulate the hydrophobic material in the oil phase of the oil-in-water emulsion, it is useful to select the monomer according to its solubility in the hydrophobic material. The monomer is substantially soluble in oil, but when polymerized in the individual oil droplets, it produces oligomers and polymers that are insoluble in neither the oil nor the water phase of the oil-in-water emulsion and migrate to the interface between the oil droplets and the water phase. There, in the course of further polymerization, they form the wall material, which finally encases the hydrophobic material as the core of the microcapsule.
[0046] To form a stable oil-in-water emulsion, protective colloids and / or Pickering stabilizers are generally used in combination. Both protective colloids and Pickering stabilizers may be ionic or neutral. Protective colloids and Pickering stabilizers can be used individually or in mixtures of multiple representatives with the same or different charges.
[0047] The protective colloid is preferably a water-soluble polymer which reduces the surface tension of water from a maximum of 73 mN / m to 45-70 mN / m and thus ensures the formation of a closed capsule wall.
[0048] Anionic protective colloids are sodium alginate, polymethacrylic acid and their copolymers, copolymers of sulfoethyl acrylate and sulfoethyl methacrylate, copolymers of sulfopropyl acrylate and sulfopropyl methacrylate, copolymers of N-(sulfoethyl)-maleimide, copolymers of 2-acrylamido-2-alkylsulfonic acid, copolymers of styrenesulfonic acid and vinylsulfonic acid. Preferred anionic protective colloids are naphthalenesulfonic acid and naphthalenesulfonic acid-formaldehyde condensates, and especially polyacrylic acid and phenolsulfonic acid-formaldehyde condensates.
[0049] Neutral protective colloids are, for example, cellulose derivatives such as hydroxyethylcellulose, methylhydroxyethylcellulose, methylcellulose and carboxymethylcellulose, polyvinylpyrrolidone, copolymers of vinylpyrrolidone, gelatin, gum arabic, xanthan, casein, polyethylene glycol, polyvinyl alcohol and partially hydrolyzed polyvinyl acetate and methylhydroxypropylcellulose. Preferred neutral protective colloids are polyvinyl alcohol and partially hydrolyzed polyvinyl acetate and methylhydroxy-(C1-C4)-alkylcellulose.
[0050] Methylhydroxy-(C1-C4)-alkylcellulose means methylhydroxy-(C1-C4)-alkylcellulose with a very wide range of degrees of alkoxylation as well as methylation. Preferred methylhydroxy-(C1-C4)-alkylcellulose has an average degree of substitution DS of 1.1 to 2.5 and a molar degree of substitution MS of 0.03 to 0.9.
[0051] Examples of suitable methylhydroxy-(C1-C4)-alkylcelluloses are methylhydroxy-ethylcellulose or methylhydroxypropylcellulose. Methylhydroxypropylcellulose is particularly preferred. These types of methylhydroxy-(C1-C4)-alkylcelluloses are available, for example, under the trade name Culminal® from Hercules / Aqualon.
[0052] Pickering stabilizer is inorganic solid particle. Such Pickering system may be composed of solid particle only or may further comprise auxiliary agent that enhances the dispersibility of particle in water or the wettability of particle by lipophilic phase. Its mode of action and its application are described in EP-A-1 029 018 and EP-A-1 321 182, the contents of which are expressly incorporated by reference.
[0053] The inorganic solid particles may be metal salts such as salts, oxides and hydroxides of calcium, magnesium, iron, zinc, nickel, titanium, aluminum, silicon, barium and manganese. They include magnesium hydroxide, magnesium carbonate, magnesium oxide, calcium oxalate, calcium carbonate, barium carbonate, barium sulfate, titanium dioxide, aluminum oxide, aluminum hydroxide and zinc sulfide. Silicates, bentonite, hydroxyapatite and hydrotalcite are also included. SiO2-based silica, magnesium pyrophosphate and tricalcium phosphate are particularly preferred.
[0054] Suitable SiO2-based Pickering stabilizers are highly disperse silicas. They can be dispersed as fine solid particles in water. However, it is also possible to use so-called colloidal dispersions of silica in water. Such colloidal dispersions are alkaline aqueous mixtures of silica. In the alkaline pH range, the particles swell and become stable in water. When using these dispersions as Pickering stabilizers, it is advantageous to adjust the pH value of the oil-in-water emulsion to pH 2-7 with an acid. A preferred colloidal dispersion of silica is 70-90 m at a pH of 9.3. 2 / g range of specific surface area.
[0055] Preferred SiO2-based Pickering stabilizers are highly disperse silicas with an average particle size in the range of 40 to 150 nm at pH values in the range of 8 to 11. By way of example, mention may be made of Levasil® 50 / 50 (HC Starck), Koestrosol® 3550 (CWK Bad Koestritz) and Bindzil® 50 / 80 (Akzo Nobel Chemicals).
[0056] The polymerization is generally carried out in the presence of a radical-forming polymerization initiator. For this purpose, all conventional peroxo and azo compounds can be used, for example in amounts usually used of, for example, 0.1 to 5% by weight, based on the weight of the monomer to be polymerized. Preferred polymerization initiators are those that are soluble in the oil phase or in the monomer. Such examples are t-butyl peroxyneodecanoate, t-butyl peroxypivalate, t-amyl peroxypivalate, dilauroyl peroxide, t-amyl peroxy-2-ethylhexanoate, etc.
[0057] The polymerization of oil-in-water emulsions is usually carried out at 20-100°C, advantageously at 40-90°C. The polymerization is usually carried out under standard pressure, but may also be carried out under reduced or elevated pressure, for example in the range of 0.5-20 bar. A useful procedure is to emulsify a mixture of water, protective colloid and hydrophobic material, polymerization initiator and monomers to the desired droplet size of the hydrophobic material using a high-speed disperser, and to heat the stable emulsion with stirring up to the decomposition temperature of the polymerization initiator. Here, the polymerization rate can be controlled in known manner by selecting the temperature and the amount of polymerization initiator. After reaching the polymerization temperature, it is useful to continue the polymerization for a further time, for example 2-6 hours, in order to complete the conversion of the monomers.
[0058] In a particularly preferred operation, the temperature of the polymerization reaction mixture is increased continuously or periodically during the polymerization. This is carried out by a temperature increase program. For this purpose, the overall polymerization time can be divided into two or more periods. The first polymerization period is characterized by a slow decomposition of the polymerization initiator. In the second and possibly further polymerization periods, the temperature of the reaction mixture is increased in order to accelerate the decomposition of the polymerization initiator. The temperature may be increased linearly or non-linearly in one step, or in two or more steps, or continuously. The temperature difference between the beginning and the end of the polymerization can be up to 50°C. Typically, this difference is between 3 and 40°C, advantageously between 3 and 30°C. After the end of the polymerization, the microcapsule dispersion is cooled to room temperature.
[0059] If the microcapsule dispersion is to be stored for a relatively long period of time, the suspension can be stabilized and creaming prevented by the addition of a thickener such as Rheovis® AS 1125, Rheovis® AT 120, Rheovis® AS 1130 (available from BASF SE, Germany) or xanthan.
[0060] The microcapsule dispersion obtained by the above procedure can be spray-dried in the usual way. To reduce redispersion of the spray-dried microcapsules, an additional amount of emulsifier and / or protective colloid may optionally be added to the dispersion before spray-drying. Spray-drying of the microcapsule dispersion can be carried out in the usual way. Typically, this procedure is carried out such that the inlet temperature of the drying gas, which is generally nitrogen or air, is in the range of 100-200°C, advantageously 120-160°C, and the outlet temperature of the drying gas is in the range of 30-90°C, advantageously 60-80°C. Atomization of the aqueous microcapsule dispersion with the drying gas stream can be carried out, for example, by means of a single-fluid or multi-fluid nozzle or via a rotating disk. Typically, the microcapsule dispersion is fed in the range of 2-200 bar. Advantageously, a single-fluid nozzle equipped with a vortex generator is used. The choice of the vortex generator can further influence the droplet size and the spray angle. For example, a single-fluid nozzle from Delavan can be used, which has a typical structure consisting of a vortex chamber, which influences the spray angle, and a perforated plate, which influences the throughput.
[0061] The deposition of the particulate microcapsule composition is usually carried out using a cyclone or filter separator. The sprayed aqueous microcapsule dispersion and the drying gas stream are advantageously guided in parallel. The drying gas stream is preferably blown into the tower from above in parallel with the microcapsule dispersion.
[0062] As spray towers, for example, dryers from the companies Anhydro, Miro or Nubilosa can be used, with a tower height of 12 to 30 meters and a width of 3 to 8 meters. The throughput of drying gas in such spray towers is typically in the range of 20 to 30 t / h. The throughput of the microcapsule dispersion in that case is generally 1 to 1.5 t / h.
[0063] According to a variant of this process, it is possible to insert a fluidized bed downstream of the dryer to remove any residual moisture. Methods in which spray drying is followed by fluidized bed drying are advantageous because they result in a microcapsule composition with a smaller fine fraction.
[0064] The polyaddition catalysts microencapsulated according to the invention are suitable for curing addition resins, for example polyurethane, polyurea or epoxy systems.
[0065] The polyaddition catalysts microencapsulated according to the invention are suitable for use in the construction industry, preferably in floor coatings, sealants, adhesives and sealing films.
[0066] The microencapsulated polyaddition catalysts of the present invention are particularly suitable for catalyzing the reaction of polyol compounds with polyisocyanate compounds.
[0067] The most important polyisocyanate compounds are the isomeric mixtures and prepolymers of diphenylmethane diisocyanate (MDI). In addition, oligomers and / or adducts of hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI) and prepolymers of toluene diisocyanate (TDI) and isophorone diisocyanate (IPDI) are also utilized.
[0068] As reaction partners, polyhydroxy compounds are available, but also aromatic and sterically hindered aliphatic amines and latent hardeners. The latter are converted to reactive products by exposure to moisture. Furthermore, in classical one-component systems (1K-PUR), the reaction of polyurethane prepolymers with moisture is utilized to form the polymer.
[0069] The polyaddition catalysts microencapsulated according to the invention are also suitable for use with polyol dispersions. In this case, it is possible to cover a wide range of layer thicknesses. At higher layer thicknesses, cement and / or hydrated lime (so-called 3K systems) are generally used in combination to capture the carbon dioxide produced when exposed to water. This type of coating is distinguished by its very high chemical resistance.
[0070] The polyaddition catalyst microencapsulated according to the invention can be mixed with the polyisocyanate compound. Alternatively, the polyaddition catalyst microencapsulated according to the invention can be mixed with the components of the resin system at the time of application. In a preferred embodiment, the polyaddition catalyst microencapsulated according to the invention is mixed with an aggregate or filler system. The aggregate or filler system is generally present in powder form and is mixed with the liquid components of the resin system at the time of application.
[0071] The polyaddition catalyst microencapsulated according to the present invention allows for a sufficiently long pot life and a short curing time to be set.
[0072] The present invention will now be described in more detail with reference to the following examples.
[0073] The particle size distribution of the microcapsules was measured using a Malvern Mastersizer 2000, a sample dispersion unit Hydro 2000S, according to standard methods described in the literature. The values given are the mean values, i.e. D(0.5).
[0074] For freeze-drying, the samples were frozen on dry ice in a metal tray 25 mm deep. Drying was performed in a Christ Alpha 2-4 freeze dryer equipped with a temperature controller LDC-1M at 1.013 mbar. The sample temperature was regulated at -20 °C. The ice condenser temperature was below -60 °C. The drying process was finished when the temperature of both the sample and the mounting surface was below 0 °C. The drying duration depends on the amount and physical properties of the material to be dried. After drying, the apparatus is ventilated with ambient air and the samples are removed by scraping them from the molds using a spatula.
[0075] Example 1 aqueous phase Distilled water 463.15g 150 g of a 10% by weight aqueous solution of polyvinyl alcohol (Mowiol 18 / 88 from Kuraray Europe GmbH, viscosity of a 4% by weight solution at 20° C.: 18 mPas measured according to DIN 53015, and degree of hydrolysis 88%) 2g of 2.5% by weight aqueous solution of sodium nitrite 0.12 g of 25% by weight aqueous solution of sodium hydroxide Feed 1 Dibutyltin dilaurate 200g Diisononyl cyclohexane-1,2-dicarboxylate 200g Feed 2 1,4-Butanediol diacrylate 10g Methyl methacrylate 50g Methacrylic anhydride 40g Feed 3 2.05g tert-butyl peroxyneodecanoate Feed 4 10 g of a 10% by weight aqueous solution of tert-butyl hydroperoxide Feed 5 26 g of 3.85% by weight aqueous solution of ascorbic acid
[0076] The aqueous phase is placed in a receiving vessel at 25° C. Feeds 1 and 2 are added and the mixture is stirred at 3500 rpm for 40 minutes. A stable emulsion is formed. After the addition of Feed 3, the following temperature program is carried out: heat to 75° C. in 180 minutes and hold this temperature for 60 minutes. Feed 4 is then added and, in the course of cooling to 20° C., Feed 5 is added over 60 minutes.
[0077] This gave a dispersion with a solids content of 45.2% by weight and an average particle size D(0.5) of 2.54 μm. The water was then removed by freeze-drying the dispersion, resulting in a colorless powder.
[0078] Example 2 Example 1 was repeated, but with the amounts of the following ingredients changed as follows: Methyl methacrylate 70g Methacrylic anhydride 20g
[0079] This gave a dispersion with a solids content of 44.8% by weight and an average particle size D(0.5) of 2.25 μm. The water was then removed by freeze-drying the dispersion, resulting in a colorless powder.
[0080] Example 3 aqueous phase Distilled water 570.7g Approximately 80m 2 150 g of a 50% by weight aqueous solution of silica sol having a specific surface area of 1 / g 7 g of a 5% by weight aqueous solution of methylhydroxypropylcellulose having an average molecular weight of 26000 g / mol 2g of 2.5% by weight aqueous solution of sodium nitrite 3.85g of 20% by weight aqueous solution of nitric acid Feed 1 Dibutyltin dilaurate 200g Diisononyl cyclohexane-1,2-dicarboxylate 200g Feed 2 1,4-Butanediol diacrylate 10g Methyl methacrylate 50g Methacrylic anhydride 40g Feed 3 1.35 g of a 75% by weight solution of tert-butyl perpivalate in an aliphatic hydrocarbon Feed 4 50 g of 2% by weight aqueous solution of sodium peroxodisulfate Feed 5 14.4 g of 10% by weight aqueous solution of sodium hydroxide
[0081] The aqueous phase is placed in a receiving vessel at 25° C. Feeds 1 and 2 are added and the mixture is stirred at 3500 rpm for 40 minutes. A stable emulsion is formed. After the addition of Feed 3, the following temperature program is carried out: heat to 65° C. in 60 minutes, heat to 90° C. in 60 minutes and hold this temperature for 150 minutes. During the first 90 minutes of this period, Feed 4 is added. After cooling to 20° C., Feed 5 is added.
[0082] This resulted in a dispersion with a solids content of 44.6% by weight and an average particle size D(0.5) of 4.00 μm. The water was then removed by freeze-drying the dispersion, resulting in a colorless powder.
[0083] Example 4 Example 3 was repeated, but with the amounts of the following ingredients changed as follows: Methyl methacrylate 70g Methacrylic anhydride 20g Sodium hydroxide 0.73g
[0084] This resulted in a dispersion with a solids content of 44.7% by weight and an average particle size D(0.5) of 4.16 μm. The water was then removed by freeze-drying the dispersion, resulting in a colorless powder.
[0085] Example 5 aqueous phase Distilled water 570.7g Approximately 80m 2 150 g of a 50% by weight aqueous solution of silica sol having a specific surface area of 1 / g 7 g of a 5% by weight aqueous solution of methylhydroxypropylcellulose having an average molecular weight of 26000 g / mol 2g of 2.5% by weight aqueous solution of sodium nitrite 3.85g of 20% by weight aqueous solution of nitric acid Feed 1 Bismuth neodecanoate 200g Diisononyl cyclohexane-1,2-dicarboxylate 200g Feed 2 1,4-Butanediol diacrylate 10g Methyl methacrylate 70g Methacrylic anhydride 20g Feed 3 1.35 g of a 75% by weight solution of tert-butyl perpivalate in an aliphatic hydrocarbon Feed 4 50 g of 2% by weight aqueous solution of sodium peroxodisulfate Feed 5 0.73g of 10% by weight aqueous solution of sodium hydroxide
[0086] The method was the same as that described in experiment 4. This resulted in a dispersion with a solids content of 42.5% by weight and an average particle size D(0.5) of 3.64 μm. The water was subsequently removed by freeze-drying the dispersion. In this case, a colorless powder was obtained.
[0087] Examples 1-5 were tested according to the following procedure: Test system: A masterbatch was prepared from 91 g (0.5 mol NCO) of Desmodur N3600 (HDI trimer) and 124 g (0.55 mol OH) of Lupranol 1200 (polypropylene glycol with number average molecular weight of 450); 0.15 g of catalyst or an amount of microcapsules whose catalyst content corresponds to the free amount of catalyst were used for 15 g of masterbatch, corresponding to a catalyst loading of 1% (w / w).
[0088] measurement: 1) Weigh the appropriate amount of catalyst into a snap-lid glass container containing a stir bar. 2) A masterbatch is prepared by mixing Bayer Material Science component Desmodur N3600 with BASF component Lupranol 1200 at 400 rpm for 5 minutes under a slow nitrogen flow. 3) The mixture is packed into a glass sample container and stirred with a stir bar. 4) Potlife: When the stirrer remains stationary 5) Curing time: The final curing time was determined as soon as the cured resin could no longer be pushed in using a spatula after the surface of the resin no longer moved when the glass container was tilted. [Table 1] The present disclosure also includes the following: [1] A microencapsulated polyaddition catalyst comprising a capsule core containing a polyaddition catalyst and an acrylic copolymer as a capsule shell, the acrylic copolymer being an ethylenically unsaturated C 3 ~C 12 A microencapsulated polyaddition catalyst comprising copolymerized units of intermolecular anhydrides of carboxylic acids, and the polyaddition catalyst is selected from acyclic tertiary amines, alicyclic tertiary amines, N-alkylimidazoles, phosphines and organometallic salts. [2] The ethylenically unsaturated C 3 ~C 12 2. The microencapsulated polyaddition catalyst according to embodiment 1, wherein the intermolecular anhydride of a carboxylic acid is selected from acrylic anhydride, methacrylic anhydride, and 4-vinylbenzoic anhydride. [3] The acrylic copolymer is (a) Ethylenically unsaturated C 3 ~C 12 5 to 50% by weight of at least one intermolecular anhydride of a carboxylic acid, (b) C of acrylic acid 1 ~C 24 Alkyl esters, methacrylic acid C 1 ~C 24 30 to 90% by weight of at least one monomer selected from alkyl esters and vinyl aromatics; (c) 5 to 20% by weight of at least one monomer having at least two ethylenic unsaturations, and (d) 0 to 30% by weight of one or more other monomers, each based on the total weight of the monomers. 3. The microencapsulated polyaddition catalyst according to claim 1 or 2, which is composed of units [4] The acyclic tertiary amines include triethylamine, tributylamine, N,N-dimethylcyclohexylamine (DMCHA), N-methyldicyclohexylamine, N,N-dimethylbenzylamine (BDMA), N,N-dimethylaminopropylamine, bis-(dimethylaminopropyl)amine, N,N-dimethylaminopropyl-N'-methylethanolamine, dimethylaminoethoxyethanol, bis-(dimethylaminopropyl)amino-2-propanol, N,N-dimethylaminopropyl-dipropanolamine, N,N,N'-trimethyl-N'-hydroxyethyl-bisaminoethyl-ether, N,N-dimethylaminopropylurea, and N,N,N',N'-tetramethylethylenediamine; selected from N,N,N',N'-tetramethylbutylenediamine, N,N,N',N'-tetramethyl-1,6-hexylenediamine, N,N,N',N'',N''-pentamethyldiethylenetriamine (PMDETA), N,N,N',N'',N''-pentamethyldipropylenetriamine (PMDPTA), N,N,N-tris-(3-dimethylaminopropyl)-amine, bis-(2-dimethylaminoethyl)-ether (BDMAEE), bis-(dimethylaminopropyl)-urea, 2,4,6-tris(dimethylaminomethyl)phenol and its salts with 2-ethylhexanoic acid and their isomers, 1,3,5-tris(3-[dimethylamino]propyl)-hexahydro-triazine; the alicyclic tertiary amine is selected from 1,4-dimethylpiperazine (DMP), 1-methyl-4-(2-dimethylaminoethyl)piperazine, 1-aza-bicyclo-[3.3.0]-octane, 1,4-diaza-bicyclo-[2.2.2]-octane (DABCO), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]-non-7-ene (DBN), N-methylmorpholine, N-ethylmorpholine, N-cyclohexylmorpholine, and 2,2′-dimorpholinodiethyl ether (DMDEE); The N-alkylimidazole is selected from N-methylimidazole, 1,2-dimethylimidazole, N-(2-hydroxypropyl)-imidazole, N-(2-hydroxyethyl)-imidazole and N-(2-aminopropyl)-imidazole; A microencapsulated polyaddition catalyst according to any one of embodiments 1 to 3. [5] The organometallic salt has the general formula L m M n+ nA - [In the formula, the ligand L is an organic group or an organic compound selected from alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl and acyl, where the ligand L has 1 to 20 C atoms, and the m ligands L may be identical or different, m is 0, 1, 2, 3, 4, 5 or 6; M is a metal, n is 1, 2, 3, or 4, and Anion A - is a carboxylate ion, an alkoxylate ion, or an enolate ion. [6] 6. The microencapsulated polyaddition catalyst according to embodiment 5, wherein the metal M is selected from lithium, potassium, cesium, magnesium, calcium, strontium, barium, boron, aluminum, indium, tin, lead, bismuth, cerium, cobalt, iron, copper, lanthanum, manganese, mercury, scandium, titanium, zinc and zirconium. [7] The anion A - is the formula R 1 -COO - where R 1 is selected from H, alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl and acyl, and the group R 1 7. The microencapsulated polyaddition catalyst according to embodiment 5 or 6, wherein [8] The anion A - is the formula R 2 CH=CR 3 -O - where R 2 and R 3 is selected from H, alkyl, alkenyl, alkynyl, aryl, arylalkyl, alkylaryl, heteroaryl, heteroarylalkyl, alkylheteroaryl, and acyl, and each of the groups R 2 and R 3 7. The microencapsulated polyaddition catalyst according to embodiment 5 or 6, wherein each of said has up to 20 C atoms. [9] 9. The microencapsulated polyaddition catalyst of any of the preceding aspects, wherein the capsule core comprises a hydrophobic core material.
[10] 10. The microencapsulated polyaddition catalyst according to embodiment 9, wherein the hydrophobic core material is selected from esters of aliphatic or aromatic polycarboxylic acids, triglycerides and trialkyl phosphates.
[11] 11. The microencapsulated polyaddition catalyst according to any one of aspects 1 to 10, wherein the microcapsules have a diameter D(0.5) of 1 to 50 μm.
[12] 12. The microencapsulated polyaddition catalyst according to any of the preceding aspects, wherein the microencapsulated polyaddition catalyst is present as a dry powder, granules or agglomerates.
[13] A method for producing the microencapsulated polyaddition catalyst according to any one of the first to second aspects by radical polymerization of a monomer mixture constituting the capsule shell in the oil phase of a stable oil-in-water emulsion, the oil phase comprising the polyaddition catalyst and the monomer mixture comprising ethylenically unsaturated C 3 ~C 12 The process comprises the step of preparing an intermolecular anhydride of a carboxylic acid.
[14] 14. The method of embodiment 13, wherein the oil-in-water emulsion is stabilized by a protective colloid and / or a Pickering stabilizer.
[15] 13. Use of the microencapsulated polyaddition catalyst according to any of embodiments 1 to 12 for catalyzing the reaction of a polyol compound with a polyisocyanate compound.
Claims
1. A microencapsulated polyaddition catalyst comprising a capsule core comprising a hydrophobic core material comprising a polyaddition catalyst, and an acrylic copolymer as a capsule shell, said polyaddition catalyst being selected from organometallic salts; the organometallic salt is selected from dibutyltin dilaurate and bismuth neodecanoate; the hydrophobic core material is diisononylcyclohexane-1,2-dicarboxylate; The acrylic copolymer is (a) 5 to 50% by weight of methacrylic anhydride, (b) 30 to 90% by weight of methyl methacrylate monomer; (c) 5 to 20% by weight of 1,4-butanediol diacrylate monomer; and (d) 0 to 30% by weight of one or more other monomers different from the units (a) to (c). in each case based on the total weight of the monomers, the sum of monomers (a) through (d) being 100%, (d) the one or more other monomers different from the units (a) to (c) are selected from vinyl acetate, vinyl propionate, vinylpyridine, acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinylphosphonic acid, maleic anhydride, 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate, acrylamido-2-methylpropanesulfonic acid, methacrylonitrile, acrylonitrile, methacrylamide, N-vinylpyrrolidone, N-methylol acrylamide, N-methylol methacrylamide, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate.
2. 2. The microencapsulated polyaddition catalyst of claim 1, wherein the hydrophobic core material forms the oil phase of an oil-in-water emulsion.
3. 3. The microencapsulated polyaddition catalyst according to claim 1, wherein the microcapsules have a diameter D(0.5) of 1 to 50 μm.
4. 4. The microencapsulated polyaddition catalyst according to claim 1, wherein the microencapsulated polyaddition catalyst is present as a dry powder, granules or agglomerates.
5. 5. A method for producing a microencapsulated polyaddition catalyst according to any one of claims 1 to 4 by radical polymerization of a monomer mixture constituting the capsule shell in the oil phase of a stable oil-in-water emulsion, the oil phase comprising the polyaddition catalyst and the monomer mixture comprising: (a) 5 to 50% by weight of methacrylic anhydride, (b) 30 to 90% by weight of methyl methacrylate monomer; (c) 5 to 20% by weight of 1,4-butanediol diacrylate monomer; and (d) 0 to 30% by weight of one or more other monomers different from the units (a) to (c). in each case based on the total weight of monomers, the sum of monomers (a) through (d) being 100%.
6. 6. The method of claim 5, wherein the oil-in-water emulsion is stabilized by a protective colloid and / or a Pickering stabilizer.
7. 5. Use of the microencapsulated polyaddition catalyst according to any one of claims 1 to 4 for catalyzing the reaction of a polyol compound with a polyisocyanate compound.
Citation Information
Patent Citations
Microcapsules containig bleaching aids
EP0839902A2
Microcapsules for epoxy resin curing agents
JP1993247179A
Microencapsulated type curing accelerator, epoxy resin composition comprising the same and cured product thereof
JP1994073163A
Microcapsule, preparation thereof and method for releasing substance under control
JP1995144126A
Encapsulated active substance
JP2002513045A