Phosphor plate and light emitting device

By setting the maximum surface roughness heights of the phosphor plate to 5.00 μm or less, the light emission and manufacturing stability are improved, leading to a brighter and more efficient light-emitting device.

JP7587680B2Active Publication Date: 2024-11-20DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023508808
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-22
Filing Date
2022-02-21
Publication Date
2024-11-20
Estimated Expiration
2042-02-21

AI Technical Summary

Technical Problem

Existing phosphor plates exhibit suboptimal light emission characteristics due to rough excitation light entrance and exit surfaces.

Method used

The phosphor plate is designed with maximum surface roughness heights (Ry1 and Ry2) of 5.00 μm or less on both sides, optimizing the smoothness to enhance light emission properties.

Benefits of technology

The optimized surface roughness improves the light-emitting characteristics and manufacturing stability of the phosphor plate, resulting in a light-emitting device with enhanced brightness and reduced excitation light leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587680000002
    Figure 0007587680000002
  • Figure 0007587680000003
    Figure 0007587680000003
  • Figure 0007587680000004
    Figure 0007587680000004
Patent Text Reader

Abstract

This phosphor plate comprises a plate-like composite including: a base material; and phosphors dispersed in the base material, the phosphor plate being configured such that, when the maximum height on the front surface of the phosphor plate is Ry1 and the maximum height on the rear surface thereof is Ry2, Ry1 and Ry2 are each 5.00 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a phosphor plate and a light emitting device. [Background technology]

[0002] Various developments have been made so far regarding phosphor plates. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a wavelength conversion member in which an inorganic phosphor is dispersed in a glass matrix (claim 1 of Patent Document 1). According to the same document, the shape of the wavelength conversion member is not limited, and it may be a plate-like shape (paragraph 0054). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-199640 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of studies by the present inventors, it has been found that the plate-shaped wavelength conversion member described in Patent Document 1 has room for improvement in terms of light emission characteristics. [Means for solving the problem]

[0005] The inventors further studied and found that the light emission characteristics can be improved by increasing the smoothness of the entrance and exit surfaces of the excitation light in the phosphor plate. Based on this knowledge, the inventors further studied and found that the smoothness is expressed by the maximum height Ry, which means the distance between the highest peak top and the deepest peak bottom in a roughness curve that represents a surface roughness profile, and that the light emission characteristics of the phosphor plate can be improved by setting the maximum height Ry on the entrance and exit surfaces to a predetermined value or less, thereby completing the present invention.

[0006] According to the present invention, A phosphor plate having a plate-shaped composite including a base material and a phosphor dispersed in the base material, The maximum height of the phosphor plate on the surface is Ry 1 The maximum height on the back surface is Ry 2 Then, Ry 1 and Ry 2 and wherein each of the thicknesses of the phosphor plate is 5.00 μm or less.

[0007] Further, according to the present invention, A light-emitting element; and the phosphor plate provided on one surface of the light-emitting element. Effect of the Invention

[0008] According to the present invention, there are provided a phosphor plate having excellent light-emitting properties, and a light-emitting device using the phosphor plate. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic diagram showing an example of the configuration of a phosphor plate according to the present embodiment. [Diagram 2] FIG. 1A is a cross-sectional view showing a schematic configuration of a flip-chip type light-emitting device, and FIG. 1B is a cross-sectional view showing a schematic configuration of a wire-bonding type light-emitting element. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus for measuring the luminescence properties of a phosphor plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.

[0011] The phosphor plate of this embodiment will be outlined.

[0012] The phosphor plate of this embodiment will be outlined below. The phosphor plate of this embodiment includes a plate-shaped composite body including a base material and phosphors dispersed in the base material. The maximum height of this phosphor plate on the surface is Ry 1 The maximum height on the back surface is Ry 2 Then, Ry 1 and Ry 2 Each of these is configured to be 5.00 μm or less.

[0013] The phosphor plate can function as a wavelength converter that converts irradiated blue light into orange light and emits it. When used as a wavelength converter, the rear surface of the phosphor plate becomes the light input surface and the front surface becomes the light output surface.

[0014] According to the inventors' findings, the luminescence characteristics can be stably evaluated by using the maximum height Ry on the front and back surfaces of the phosphor plate as an index, and further investigation has revealed that the luminescence characteristics can be improved by setting the maximum height Ry on the front and back surfaces to be equal to or less than the above-mentioned upper limit value.

[0015] Maximum height Ry on the surface of the phosphor plate 1 The upper limit of the thickness is 5.00 μm or less, preferably 3.00 μm or less, and more preferably 2.00 μm or less, which can improve the light emitting characteristics of the phosphor plate. The above Ry 1 The lower limit of is not particularly limited, but may be the detection limit or may be 0.10 μm or more, preferably 0.30 μm or more, and more preferably 0.50 μm or more. This can improve the production stability of the phosphor plate.

[0016] Maximum height Ry on the back surface of the phosphor plate 2 The upper limit of the thickness is 5.00 μm or less, preferably 3.00 μm or less, more preferably 2.00 μm or less, and further preferably 1.00 μm or less, which can improve the light emitting properties of the phosphor plate. The above Ry 2 The lower limit of is not particularly limited, but may be the detection limit or may be 0.10 μm or more, preferably 0.30 μm or more, and more preferably 0.50 μm or more. This can improve the production stability of the phosphor plate.

[0017] One embodiment of the phosphor plate is the above-mentioned Ry 1 and Ry 2 At least one of these is 3.00 μm or less, preferably Ry 1 and Ry 2 At least one of these is 3.00μm or less and Ry 1 >Ry 2 , more preferably Ry 1 and Ry 2 In this case, the distance between the excitation light emitting element and the light receiving element may be set to 2.80 μm or less. This makes it possible to suppress the leakage of excitation light. Another embodiment of the phosphor plate may be configured to satisfy the following condition A1 and / or condition A2, which can further suppress excitation light leakage. Condition A1: Above Ry 1 and Ry 2 The absolute value of the difference is 1.10 μm or less. Condition A2: Above Ry 1 and Ry 2 At least one of the above is 0.90μm or less. Another aspect of the phosphor plate may be configured to satisfy the following condition B1 or B2, which can further improve the light-emitting characteristics of the phosphor plate. Condition B1: Above Ry 1 and Ry 2 The absolute value of the difference is 1.60 μm or less. Condition B2: Above Ry 1 and Ry 2 The absolute value of the difference is more than 1.60 μm and less than 1.90 μm, and Ry 1 >Ry 2 To be.

[0018] In this embodiment, for example, by appropriately selecting the type and amount of each component contained in the phosphor plate, the manufacturing method of the phosphor plate, etc., the above-mentioned Ry 1 and Ry 2 Among these, for example, grinding and / or polishing the front and back surfaces of the phosphor plate with a grindstone or abrasive grains of a predetermined grain size can be used to control the Ry 1 and Ry 2 are cited as factors for setting the desired numerical range.

[0019] When the phosphor plate is irradiated with blue light having a wavelength of 455 nm, the peak wavelength of the wavelength-converted light emitted from the phosphor plate is preferably 585 nm or more and 605 nm or less. In addition, by combining the phosphor plate with a light-emitting element that emits blue light, a light-emitting device that emits orange light with high luminance can be obtained.

[0020] The configuration of the phosphor plate of this embodiment will be described in detail.

[0021] (base material) In the composite constituting the phosphor plate, the phosphor and the base material composed of an inorganic substance are mixed together. Specifically, the phosphor may have a structure in which the phosphor is dispersed in a sintered product of a compound constituting the inorganic base material. The phosphor may be uniformly dispersed in the inorganic base material in a particulate state.

[0022] The base material may be a main component in the composite. In this case, the content of the base material in the composite may be, for example, 50 vol% or more, preferably 60 vol% or more, in terms of volume.

[0023] The base material is Al 2 0 3 Sintered material, SiO 2 Sintered material and spinel compound M 2x Al 4-4x O 6-4x(However, M is at least one of Mg, Mn, and Zn, and 0.2 < x < 0.6), and it may be composed of a sintered body of a metal oxide containing at least one kind of sintered body. These may be used alone or in combination of two or more. Among these, the base material may be composed of a sintered body containing an alumina or a spinel-based compound from the viewpoints of thermal characteristics and transparency.)

[0024] Al 2 0 3 The sintered body of has little absorption of visible light, so the emission intensity of the phosphor plate can be increased. Also, Al 2 0 3 The sintered body of has high thermal conductivity, so the heat resistance of the phosphor plate can be improved. Furthermore, Al 2 0 3 The sintered body of is also excellent in mechanical strength, so the durability of the phosphor plate can be enhanced.)

[0025] SiO 2 The sintered body of may be composed of a glass matrix. As the glass matrix, silica glass or the like is used.)

[0026] The sintered body containing a spinel-based compound is usually obtained by mixing a powder of a metal oxide represented by the general formula MO (M is at least one of Mg, Mn, and Zn) and a powder of Al 2 O 3 and sintering them.) Spinel, stoichiometrically, has a composition represented by x = 0.5 (that is, the general formula MAl 2 O 4 ).) However, depending on the ratio of the amount of MO of the raw material to the amount of Al 2 O 3 , it becomes a spinel-based compound of a non-stoichiometric composition in which MO or Al 2 O 3 is excessively solid-solved.) The sintered body containing the spinel-based compound represented by the above general formula is relatively transparent. Therefore, excessive scattering of light in the phosphor plate is suppressed. Furthermore, from the viewpoint of transparency, it is preferable to use a spinel-based compound in which M in the above general formula is Mg.)

[0027] (Phosphor) The phosphor contained in the composite may contain one or more selected from the group consisting of, for example, sialon phosphors, CASN phosphors, and SCASN phosphors. Examples of the sialon phosphor include α-type sialon phosphors.

[0028] As the α-type sialon phosphor, those containing an α-type sialon phosphor containing Eu element represented by the following general formula (1) are used. (M) m(1-x) / p (Eu) mx / 2 (Si) 12-(m+n) (Al) m+n (O) n (N) 16-n ··General formula (1)

[0029] In the above general formula (1), M represents one or more elements selected from the group consisting of Li, Mg, Ca, Y, and lanthanide elements (excluding La and Ce), p represents the valence of the M element, 0 < x < 0.5, 1.5 ≤ m ≤ 4.0, and 0 ≤ n ≤ 2.0. n may be, for example, 2.0 or less, 1.0 or less, or 0.8 or less. Generally, the one with M being Ca is called a Ca-α-type sialon phosphor.

[0030] The solid solution composition of α-type sialon is obtained by substituting m Si-N bonds of the unit cell of α-type silicon nitride (Si 12 N 16 ) with Al-N bonds and n Si-N bonds with Al-O bonds, and in order to maintain electrical neutrality, m / p cations (M, Eu) penetrate and solidify in the crystal lattice and are represented by the above general formula. In particular, when Ca is used as M, α-type sialon is stabilized in a wide composition range, and by substituting a part of it with Eu as the emission center, a phosphor that is excited by light in a wide wavelength range from ultraviolet to blue and exhibits visible emission from yellow to orange can be obtained.

[0031] The solid solution composition of α-SiAlON cannot be strictly defined because of the presence of a second crystal phase different from α-SiAlON and an amorphous phase that inevitably exists. α-SiAlON can be found in other crystal phases such as β-SiAlON, aluminum nitride or its polytypoid, Ca 2 S 5 N 8 , CaAlSiN 3 etc. may be included.

[0032] One method for producing an α-sialon phosphor is to heat and react a mixed powder consisting of a compound of silicon nitride, aluminum nitride, and an interstitial solid solution element in a high-temperature nitrogen atmosphere. In the heating process, some of the components form a liquid phase, and substances move into this liquid phase to produce an α-sialon solid solution. After synthesis, the α-sialon phosphor is formed by sintering multiple equiaxed primary particles to form clumped secondary particles. In this embodiment, a primary particle refers to the smallest particle that has the same crystal orientation within the particle and can exist alone.

[0033] Examples of CASN phosphors include CaAlSiN 3 A phosphor in which Eu element is added to a host crystal of alkaline earth silicon nitride represented by the formula:

[0034] The SCASN phosphor is, for example, (Sr,Ca)AlSiN 3 The phosphor used is an alkaline earth silicon nitride host crystal represented by the formula:

[0035] The lower limit of the average particle diameter of the phosphor is, for example, preferably 1 μm or more, more preferably 2 μm or more. This can increase the luminescence intensity. The upper limit of the average particle diameter of the phosphor is preferably 30 μm or less, more preferably 20 μm or less. The average particle diameter of the phosphor is the dimension of the secondary particles. By setting the average particle diameter to 5 μm or more, the transparency of the composite can be further increased. On the other hand, by setting the average particle diameter of the phosphor to 30 μm or less, the occurrence of chipping can be suppressed when cutting the phosphor plate with a dicer or the like.

[0036] Here, the average particle size of the phosphor refers to the particle size D50 at which 50% of the particles pass through (accumulated passing fraction) from the small particle size side in the volumetric particle size distribution obtained by measurement using a laser diffraction scattering particle size distribution measurement method (LS13-320, manufactured by Beckman Coulter, Inc.).

[0037] The lower limit of the phosphor content is, for example, 5 vol% or more, preferably 10 vol% or more, more preferably 15 vol% or more in 100 vol% of the composite. This can increase the luminescence intensity of the thin phosphor plate. Also, the light conversion efficiency of the phosphor plate can be improved. On the other hand, the upper limit of the phosphor content is, for example, 60 vol% or less, preferably 50 vol% or less, and more preferably 40 vol% or less, based on 100 vol% of the composite, which can suppress a decrease in thermal conductivity of the phosphor plate.

[0038] In the phosphor plate, the upper limit of the light transmittance for blue light of 450 nm is, for example, 10% or less, preferably 5% or less, and more preferably 1% or less. This makes it possible to suppress the transmission of blue light through the phosphor plate, thereby increasing the luminance. By appropriately adjusting the phosphor content and the thickness of the phosphor plate, the light transmittance for blue light of 450 nm can be reduced. The lower limit of the light transmittance for 450 nm blue light is not particularly limited, but may be, for example, 0.01% or more, which can further increase the emission intensity.

[0039] The manufacturing process of the phosphor plate of this embodiment will be described in detail.

[0040] The method for producing the phosphor plate of this embodiment may include a step (1) of obtaining a mixture containing a metal oxide and a phosphor, and a step (2) of firing the obtained mixture.

[0041] Alternatively, the method for producing the phosphor plate may involve melting a metal oxide and mixing phosphor particles into the resulting melt.

[0042] In step (1), the phosphor or metal oxide powder used as the raw material is preferably as pure as possible, and the content of impurities of elements other than the constituent elements is preferably 0.1% or less, and more preferably 0.01% or less.

[0043] The raw material powders can be mixed by various methods, including dry and wet methods. However, a method that minimizes the pulverization of phosphor particles used as a raw material and minimizes the inclusion of impurities from the mixing device is preferred.

[0044] Al is used as a metal oxide for phosphor materials. 2 0 3 Powder, SiO 2 The powder may contain at least one of a powder of SiO 2 and a powder of a spinel raw material. These may be used alone or in combination of two or more. The metal oxide may be in the form of a fine powder, and the average particle size may be, for example, 1 μm or less.

[0045] Alumina powder (Al 2 0 3 ) may also be used.

[0046] The upper limit of the BET specific surface area of ​​the alumina powder is, for example, 10.0 m 2 / g or less, preferably 9.0m 2 / g or less, more preferably 8.0m 2 / g or less, more preferably 6.0m 2 / g or less. This makes it possible to suppress blackening of the phosphor plate. On the other hand, the lower limit of the BET specific surface area of ​​the alumina powder is, for example, 0.1 m 2 / g or more, preferably 0.5m 2 / g or more, more preferably 1.0m 2 / g or more, more preferably 2.0m 2 / g or more. This enhances the sinterability of the alumina powder and enables the formation of a dense composite.

[0047] In step (2), the mixture of alumina powder and phosphor powder may be sintered at, for example, 1300° C. to 1650° C. The heating temperature in the sintering step is more preferably 1500° C. to 1600° C. In order to densify the composite, a higher sintering temperature is preferred, but if the sintering temperature is too high, the phosphor and alumina react with each other, reducing the luminescence intensity of the phosphor plate, and therefore the above range is preferred. Furthermore, when the firing temperature is in the high temperature range of about 1600° C. to 1650° C., the retention time for this temperature is, for example, 20 minutes or less, and preferably 15 minutes or less, which can increase the luminescence intensity of the phosphor plate.

[0048] As the raw metal oxide, glass powder (SiO 2 Powders containing The glass powder is SiO 2 Powder (silica powder) or a general glass raw material can be used. These may be used alone or in combination of two or more.

[0049] As the raw metal oxide, a spinel raw material powder may be used. Here, the “spinel raw material powder” refers to, for example, (i) a powder of the above-mentioned general formula M 2x Al 4-4x O 6-4x and / or (ii) a powder containing a metal oxide powder represented by the general formula MO (wherein M is at least one of Mg, Mn, and Zn) and Al. 2 O 3 It is a mixture of powder.

[0050] In step (2), the spinel raw material powder may be sintered, for example, at a temperature of 1300° C. to 1650° C. The heating temperature in the sintering step is more preferably 1500° C. to 1600° C. In order to densify the composite, a higher sintering temperature is preferred, but if the sintering temperature is too high, the luminescence intensity of the phosphor plate decreases, so the above range is preferred. Furthermore, when the firing temperature is in the high temperature range of about 1600° C. to 1650° C., the retention time for this temperature is, for example, 20 minutes or less, and preferably 15 minutes or less, which can increase the luminescence intensity of the phosphor plate.

[0051] In the above manufacturing method, the firing method may be either pressureless sintering or pressure sintering. In order to suppress deterioration of the phosphor properties and to obtain a dense composite, pressure sintering is preferred, which is easier to densify than pressureless sintering.

[0052] Examples of pressure sintering methods include hot press sintering, spark plasma sintering (SPS), hot isostatic pressure sintering (HIP), etc. In the case of hot press sintering or SPS sintering, the pressure is 10 MPa or more, preferably 30 MPa or more, and 100 MPa or less, preferably 80 MPa or less. The firing atmosphere is preferably a non-oxidizing inert gas atmosphere such as nitrogen or argon, or a vacuum atmosphere, in order to prevent oxidation of the phosphor.

[0053] In this manner, the phosphor plate of this embodiment is obtained. The front and back surfaces of the obtained phosphor plate are subjected to appropriate surface treatment. Examples of surface treatment include grinding using a diamond grindstone or the like, lapping, polishing, and the like.

[0054] The light emitting device of this embodiment will be described.

[0055] The light emitting device of this embodiment includes a light emitting element and the above phosphor plate provided on one surface of the light emitting element. An example of a specific light emitting device includes, for example, a group III nitride semiconductor light emitting element (light emitting element 20) and the above phosphor plate 10 provided on one surface of the group III nitride semiconductor light emitting element. The group III nitride semiconductor light emitting element includes an n-layer, a light emitting layer, and a p-layer, each of which is made of a group III nitride semiconductor such as AlGaN, GaN, or InAlGaN-based material. A blue LED that emits blue light can be used as the group III nitride semiconductor light emitting element. The phosphor plate 10 may be disposed directly on one surface of the light emitting element 20, but may also be disposed via a light transparent member or a spacer.

[0056] The phosphor plate 10 arranged on the light emitting element 20 may be a disk-shaped phosphor plate 100 (phosphor wafer) shown in FIG. 1, but an individual piece of the phosphor plate 100 may also be used.

[0057] Fig. 1 is a schematic diagram showing an example of the configuration of a phosphor plate 100. The thickness of the phosphor plate 100 shown in Fig. 1 can be appropriately set depending on the application.

[0058] The lower limit of the thickness of the phosphor plate 100 shown in Fig. 1 is, for example, 0.050 mm or more, preferably 0.080 mm or more, and more preferably 0.100 mm or more. The upper limit of the thickness of the phosphor plate 100 is, for example, 1 mm or less, preferably 0.500 mm or less, and more preferably 0.300 mm or less. By keeping the thickness within such a range, it is possible to improve the light extraction efficiency and the luminous intensity.

[0059] The disk-shaped phosphor plate 100 is more durable and easier to transport than a rectangular one because chipping and cracking at the corners is suppressed.

[0060] An example of the above-mentioned semiconductor device is shown in Figures 2(a) and (b). Figure 2(a) is a cross-sectional view showing a schematic configuration of a flip-chip type light-emitting device 110, and Figure 2(b) is a cross-sectional view showing a schematic configuration of a wire-bonding type light-emitting device 120.

[0061] 2(a) includes a substrate 30, a light emitting element 20 electrically connected to the substrate 30 via solder 40 (die bond material), and a phosphor plate 10 provided on the light emitting surface of the light emitting element 20. The flip-chip type light emitting device 110 may have either a face-up type or a face-down type structure. Moreover, the light-emitting device 120 in FIG. 2(b) includes a substrate 30, a light-emitting element 20 electrically connected to the substrate 30 via a bonding wire 60 and an electrode 50, and a phosphor plate 10 provided on the light-emitting surface of the light-emitting element 20. In FIG. 2, the light emitting element 20 and the phosphor plate 10 are attached by a known method, and may be attached by, for example, a silicone adhesive or by heat fusion. Furthermore, the light emitting device 110 and the light emitting device 120 may be entirely sealed with a transparent sealing material.

[0062] Incidentally, the individualized phosphor plate 10 may be attached to the light emitting elements 20 mounted on the substrate 30. A plurality of light emitting elements 20 may be attached to a large-area phosphor plate 100, and then each light emitting element 20 with phosphor plate 10 may be diced into individual pieces. Alternatively, the large-area phosphor plate 100 may be attached to a semiconductor wafer having a plurality of light emitting elements 20 formed on its surface, and then the semiconductor wafer and phosphor plate 100 may be collectively diced into individual pieces.

[0063] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0064] <Preparation of phosphor plate> As the raw material for the phosphor plate, alumina powder (AA-03 (Sumitomo Chemical Co., Ltd., BET specific surface area: 5.2 m) 2 / g)) and a Ca-α type sialon phosphor (Alonbright YL-600B, manufactured by Denka Co., Ltd., D50 is 15 μm).

[0065] 7.857 g of alumina powder and 2.833 g of Ca-α type sialon phosphor powder were weighed and dry mixed in an agate mortar. The mixed raw materials were passed through a nylon mesh sieve with 75 μm openings to break up agglomerates, and a raw material mixed powder was obtained. The true density of the raw materials (alumina: 3.97 g / cm 3 , Ca-α type sialon phosphor: 3.34 g / cm 3 ) the compounding ratio calculated is alumina:Ca-α type sialon phosphor=70:30 vol%.

[0066] Approximately 11 g of the raw material powder mixture was filled into a carbon die with an inner diameter of 30 mm and a carbon lower punch set in place, and then an upper carbon punch was set to sandwich the raw material powder in place. A carbon sheet (GRAFOIL, manufactured by GraTech) with a thickness of 0.127 mm was set between the raw material powder mixture and the carbon jig to prevent adhesion.

[0067] The hot press jig filled with this raw material powder mixture was set in a multipurpose high-temperature furnace (Hi-Multi 5000, manufactured by Fuji Electric Industrial Co., Ltd.) with a carbon heater. The inside of the furnace was evacuated to 0.1 Pa or less, and while maintaining the reduced pressure, the upper and lower punches were pressed with a press pressure of 55 MPa. While maintaining the pressurized state, the temperature was raised to 1600°C at a rate of 5°C per minute. Immediately after reaching 1600°C, heating was stopped, and the material was slowly cooled to room temperature and depressurized (firing process). Then, a fired product with an outer diameter of 30 mm was collected. The sides of the recovered fired product were ground using a cylindrical grinder, and then ground using a surface grinder and polished using a polishing machine according to the conditions below to obtain a circular phosphor plate having the thickness (mm) and diameter of 25 mm shown in Table 1.

[0068] (Conditions of surface grinding and polishing in each example and comparative example) [Example 1] Front and back surfaces: Grinding with a diamond grinding wheel (#400) → Polishing with 9 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 3 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 1 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 3 minutes). [Example 3] Surface: Grinding with a diamond grinding wheel (#400) → Polishing with 9 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 3 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 1 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 3 minutes). Back side: Grinded with diamond grindstone (#400) [Example 5] Front and back surfaces: Grinded with diamond wheels (#400) [Example 7] Surface: Grind with diamond grinding wheel (#400) → Polish with 9μm diamond abrasive grains (polishing disk rotation speed 150rpm, polishing time: 6 minutes). Back side: Grinded with diamond grindstone (#400) [Example 9] Surface: Grind with diamond grinding wheel (#400) → Polish with 9μm diamond abrasive grains (polishing disk rotation speed 150rpm, polishing time: 6 minutes). Back side: Grinding with a diamond grinding wheel (#400) → Polishing with 9 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 3 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 1 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 3 minutes). [Comparative Example 1] Surface: Grinding with a diamond grinding wheel (#400) → Polishing with 9 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 3 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 6 minutes) → Polishing with 1 μm diamond abrasive grains (polishing plate rotation speed 150 rpm, polishing time: 3 minutes). Back side: Grinded with diamond wheel (#200) [Comparative Example 3] Surface: Grinded with diamond wheel (#400) Back side: Grinded with diamond wheel (#200)

[0069] [Example 2] The phosphor plate of Example 1 was used upside down. [Example 4] The phosphor plate of Example 3 was used upside down. [Example 6] The phosphor plate of Example 5 was used upside down. [Example 8] The phosphor plate of Example 7 was used upside down. [Example 10] The phosphor plate of Example 9 was used upside down. [Comparative Example 2] The phosphor plate of Comparative Example 1 was used upside down. [Comparative Example 4] The phosphor plate of Comparative Example 3 was used upside down.

[0070] Ry on the surface of the phosphor plate 1 and Ry on the back 2 was measured using a surface roughness measuring instrument (Mitutoyo, SJ-400) in accordance with JIS B 0031:1994.

[0071] [Table 1]

[0072] The obtained phosphor plate was evaluated for the following items.

[0073] [Evaluation of optical properties] For the phosphor plates obtained in each of the Examples and Comparative Examples, the luminescence intensity was measured according to the following procedure. The optical characteristics of the phosphor plate were measured using a chip-on-board (COB) type LED package 130. FIG. First, phosphor plate 100 and an aluminum substrate (substrate 30) on which recesses 70 were formed were prepared for each of the Examples and Comparative Examples. The diameter φ of the bottom surface of recesses 70 was set to 13.5 mm, and the diameter φ of the opening of recesses 70 was set to 16 mm. Next, inside the recess 70 of the substrate 30, a blue LED (light emitting element 20) was mounted as a blue light source. Thereafter, a circular phosphor plate 100 was placed on the blue LED so as to cover the opening of the recess 70 of the substrate 30, thereby producing the device (chip-on-board (COB) type LED package 130) shown in FIG.

[0074] The emission spectrum on the surface of phosphor plate 100 was measured using a total luminous flux measuring system (HalfMoon / φ1000 mm integrating sphere system, manufactured by Otsuka Electronics Co., Ltd.) when the blue LED of the manufactured LED package 130 was turned on.

[0075] In the obtained emission spectrum, the maximum emission intensity (W / nm) of orange light (Orange) having a wavelength of 585 nm to 605 nm was obtained. Table 1 shows the relative values ​​(%) of the maximum emission intensity of orange light of other Examples and Comparative Examples, normalized to Example 1 as 100%. In the emission spectrum, the maximum emission intensity of orange light with a wavelength of 585 nm to 605 nm is defined as T O The maximum emission intensity of blue light (Blue) with a wavelength of 445 nm to 465 nm is defined as T B When the amount of blue light transmitted from the blue LED (excitation light loss) is T B / T O × 100 and the results are shown in Table 1.

[0076] The phosphor plates of Examples 1 to 10 exhibited superior luminescence intensity compared to Comparative Examples 1 to 4. Moreover, Examples 1 to 6 and 9 to 10 showed results in which the transmission of blue light, which is excitation light, was suppressed compared to Examples 7 and 8, and Examples 1, 2, and 4 to 10 showed results in which the luminescence intensity was improved compared to Example 3. It was found that the phosphor plate of this embodiment had excellent light emitting properties.

[0077] This application claims priority based on Japanese Patent Application No. 2021-047097, filed on March 22, 2021, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]

[0078] 10 Phosphor Plate 20 Light emitting element 30 Substrate 40 Solder 50 electrodes 60 Bonding Wire 70 Recess 100 Phosphor Plate 102 Surface 104 Back side 100 Light emitting device 120 Light emitting device 130 LED packages

Claims

1. A phosphor plate having a plate-shaped composite including a base material and a phosphor dispersed in the base material, The maximum height of the phosphor plate on the surface is Ry 1 The maximum height on the back surface is Ry 2 Then, Ry 1 and Ry 2 any of the above has a thickness of 5.00 μm or less; The base material is composed of an inorganic material, The phosphor plate satisfies the following condition A1 and / or condition A2: Condition A1: The absolute value of the difference between Ry 1 and Ry 2 is 1.10 μm or less. Condition A2: At least one of Ry 1 and Ry 2 is 0.90 μm or less.

2. 2. The phosphor plate of claim 1, Ry 1 and Ry 2 At least one of the above is 3.00 μm or less.

3. 3. The phosphor plate according to claim 1, The phosphor plate, wherein the host material comprises an alumina or spinel-based compound.

4. A phosphor plate according to any one of claims 1 to 3, The phosphor plate, wherein the phosphor comprises one or more selected from the group consisting of a sialon phosphor, a CASN phosphor, and a SCASN phosphor.

5. A phosphor plate according to any one of claims 1 to 4, A phosphor plate, wherein the content of the phosphor is 5 vol% or more and 60 vol% or less in 100 vol% of the complex.

6. A phosphor plate according to any one of claims 1 to 5, A phosphor plate having a plate thickness of 0.050 mm or more and 1 mm or less.

7. A light-emitting element; A light emitting device comprising: the phosphor plate according to any one of claims 1 to 6 provided on one surface of the light emitting element.

Citation Information

Patent Citations

  • Multicolor luminescent device

    JP1998241860A

  • Wavelength conversion member and light-emitting device using the same

    JP2015199640A

  • Phosphor element and lighting device

    JP2019105846A

  • Semiconductor light-emitting device and manufacturing method therefor

    JP2019186300A

  • Wavelength conversion element, method for manufacturing wavelength conversion element, light source device and projector

    JP2020052413A