Cyclic self-limiting etching process.

A self-limiting etching process with an oxidizing agent and etchant combination addresses the challenge of high aspect ratio channels in 3D NAND architectures, achieving uniform polysilicon thickness and improved transistor performance.

JP7587734B2Active Publication Date: 2024-11-21TOKYO ELECTRON LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022559551
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-14
Filing Date
2021-01-04
Publication Date
2024-11-21
Estimated Expiration
2041-01-04

AI Technical Summary

Technical Problem

The integration of 3D NAND architectures poses challenges in defining polysilicon transistor channels due to high aspect ratios, leading to non-uniformity and performance variability in transistors.

Method used

A self-limiting etching process using an oxidizing agent forms an oxide layer on the polysilicon surface, followed by removal with a specific etchant, allowing precise control of polysilicon thickness with atomic precision, independent of etchant concentration.

Benefits of technology

This process ensures uniformity and precision in polysilicon channel thickness, reducing transistor-to-transistor variation and enhancing the performance of 3D NAND devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587734000001
    Figure 0007587734000001
  • Figure 0007587734000002
    Figure 0007587734000002
  • Figure 0007587734000003
    Figure 0007587734000003
Patent Text Reader

Abstract

A method for processing a substrate includes forming a channel through the substrate, depositing a layer of polycrystalline silicon on sidewalls of the channel, and oxidizing the uncovered surface of the polycrystalline silicon with an oxidizing agent. The oxidizing agent forms an oxidized layer, the oxidized layer having a uniform thickness on the uncovered surface of the polycrystalline silicon. The method includes removing the oxidized layer from the channel with a removing agent and repeating the steps of oxidizing the uncovered surface and removing the oxidized layer until a predetermined amount of the layer of polycrystalline silicon is removed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 63 / 002,771, filed March 31, 2020, and U.S. Nonprovisional Patent Application No. 17 / 121,546, filed December 14, 2020, which are incorporated herein by reference.

[0002] The present invention relates generally to methods for etching silicon, and in particular embodiments to methods for pseudo atomic layer etching of silicon-based materials. [Background technology]

[0003] Planar NAND reached its physical scaling limit in 193nm immersion systems around 2013. To improve performance and keep up with bit demands, the industry is moving towards 3D designs incorporating high aspect ratio structures with more than 128 layers. The integration of such 3D architectures has introduced many novel challenges.

[0004] The move from planar integration to vertical integration places some stringent demands on the etching in the 3D NAND manufacturing process. Conventional 3D NAND devices contain multiple layers of non-volatile transistors stacked and connected through a vertical channel. As design density increases, the resulting aspect ratio increases due to the additional non-volatile transistors added to the word line stack. This increase in aspect ratio presents a fundamental challenge with respect to defining the polysilicon transistor channel within this vertical channel. Summary of the Invention [Means for solving the problem]

[0005] A method of treating a substrate includes forming a channel through the substrate, depositing a layer of polysilicon on sidewalls of the channel, oxidizing an uncovered surface of the polysilicon with an oxidizing agent, where the oxidizing agent forms an oxidized layer having a uniform thickness on the uncovered surface of the polysilicon, removing the oxidized layer from the channel with a removing agent, and repeating the steps of oxidizing the uncovered surface and removing the oxidized layer until a predetermined amount of the layer of polysilicon is removed.

[0006] A method of treating a substrate includes forming a layer of silicon-based material on a semiconductor substrate having a first thickness, growing a layer of oxidized silicon-based material on the layer of silicon-based material by wetting the layer of silicon-based material with an oxidizing solution, etching the layer of oxidized silicon-based material by wetting the layer of oxidized silicon-based material with an oxide etching solution, and repeating the growing and etching steps until the layer of silicon-based material has a second thickness that is less than the predetermined thickness.

[0007] A method of forming a 3D NAND device includes forming a channel in a 3D NAND dielectric stack; depositing a layer of polysilicon having a first thickness on sidewalls of the channel; and performing a cyclic etching process, each cycle including forming an oxide layer on the layer of polysilicon by wetting an exposed surface of the layer of polysilicon with a first solution including an oxidizer; and removing the oxidized layer from the layer of polysilicon with a second solution including an oxide etchant, the cyclic etching process being stopped after the layer of polysilicon has a second thickness on sidewalls of the channel, the second thickness being less than the first thickness by a predetermined thickness.

[0008] A method of treating a substrate includes depositing a layer of silicon-based material on the substrate; oxidizing an uncovered surface of the silicon-based material with an oxidizing agent, where the oxidizing agent forms an oxidized layer having a uniform thickness on the uncovered surface of the silicon-based material; removing the oxidized layer from the silicon-based material with a removing agent; and repeating the steps of oxidizing the uncovered surface and removing the oxidized layer until a predetermined amount of the layer of silicon-based material is removed.

[0009] For a more complete understanding of the present invention, and the advantages thereof, reference is now made to the following descriptions taken in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0010] [Figure 1A] 1 is a cross-sectional projection view of a 3D-NAND memory array formed in accordance with an embodiment of the present invention. [Figure 1B] 1 is a cross-sectional view of a stack of memory transistors in a 3D-NAND memory array formed in accordance with an embodiment of the present invention. [Figure 2A] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2B] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2C] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2D] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2E] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2F]1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2G] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2H] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2I] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Figure 2J] 1A-1D are cross-sectional views of major processing steps in forming polysilicon transistor channels within channel openings in a 3D NAND memory array. [Diagram 3] FIG. 2 is a flow diagram illustrating the processing steps in FIGS. 2A to 2J. [Figure 4] 1 is a cross-sectional view of a fully depleted silicon-on-insulator (FDSOI) transistor formed in accordance with an embodiment of the present invention. [Figure 5A] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5B] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5C] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5D] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5E] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5F] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5G] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 5H] 1A-1D are cross-sectional views of major processing steps in forming a channel in a fully depleted silicon-on-insulator (FDSOI) transistor. [Figure 6] FIG. 5 is a flow diagram illustrating the processing steps in FIGS. 5A to 5H. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Various embodiments provide a self-limiting etching method with atomic layer precision. The etching techniques described herein are applicable to many different semiconductor device fabrication schemes and are useful for any integration scheme involving silicon-based etching. For example, the etching techniques herein can be used to etch layers or structures of single crystal silicon, polycrystalline silicon, and any other silicon-containing layer that can be oxidized. Although the etching techniques herein can be applied to many different etching schemes, for convenience of describing the embodiments herein, the discussion will focus primarily on the application to two sample cases: etching polysilicon in 3D memory architectures, and etching single crystal silicon in planar fully depleted silicon-on-insulator (FDSOI) integrated circuits. However, the embodiments herein can be applied to other types of 3D stacked memory and logic devices, as well as the formation of other high aspect ratio features such as through vias and deep trench structures.

[0012] 3D architectures have unique challenges presented by the topology of the 3D structures. Controlling the thickness and uniformity of the polysilicon transistor channel within this high aspect ratio vertical channel is critical to maintain transistor performance and reduce transistor-to-transistor variation. Various embodiments described in this disclosure enable chipmakers to tightly control polysilicon etching with atomic level precision.

[0013] A challenge with FDSOI architecture is the need to form a very thin single crystal silicon channel with a very uniform thickness. In fully depleted silicon-on-insulator (FDSOI) transistors, a thin layer of single crystal silicon forms the FDSOI transistor channel. Controlling the thickness and uniformity of the FDSOI transistor channel is important to maintain FDSOI transistor performance and reduce transistor-to-transistor variation. Various embodiments described in this disclosure enable chip manufacturers to tightly control the single crystal silicon etching of the FDSOI transistor channel with atomic level precision.

[0014] Although the embodiments are described in the particular context of 3D NAND and even FDSOI applications, the various embodiments may be applied to any silicon-based etch in semiconductor manufacturing. Accordingly, the various embodiments disclose etching with atomic precision and control of silicon-based materials in semiconductor manufacturing processes. The various embodiments provide an etch method that is self-limiting and not dependent on etchant concentration (rather than transport limited), thereby providing atomic control.

[0015] Increased density in 3D NAND device designs is achieved by increasing the number of layers in the 3D NAND stack. Each set of layers forms an individual non-volatile memory transistor. Over the last few years, the number of layers in the word line stack has increased from 32 to 64 layers, with future architectures potentially including 128 layers or more. These layers are typically composed of alternating layers of polysilicon and oxide, or alternating layers of dielectric materials, such as silicon dioxide and silicon nitride.

[0016] A first embodiment of the pseudo atomic layer silicon based material etching process is described using the cross-sectional view of the 3D NAND structure shown in Figure 1, which is fabricated using Figures 2A-2J according to the flow diagram of Figure 3. Then, a second embodiment of the pseudo atomic layer silicon based material etching process is described using the cross-sectional view of the FDSOI structure shown in Figure 4, which is fabricated using Figures 5A-5H according to the flow diagram of Figure 6.

[0017] Figure 1A is a cross-sectional projection of a 3D-NAND memory array formed in accordance with an embodiment of the present invention. Figure 1B shows a cross-sectional view of an example of a 3D NAND word line stack with alternating metal gates (word lines 106) and silicon dioxide 104 formed in accordance with an embodiment of the present invention.

[0018] FIG. 1A shows a semiconductor substrate 102 on which a common drain bit line 114 is formed. The cross-sectional view shows alternating layers of dielectric material, e.g., silicon dioxide 104, which electrically insulate a layer of word lines 106, e.g., made of tungsten. The word lines 106, e.g., made of tungsten, are alternating metal gates of stacked memory transistors in a 3D NAND array. A common source bit line 122, e.g., made of polysilicon, crosses the top surface of the 3D NAND memory array perpendicular to the word lines 106 (metal gates). The drain bit line 114 and the source bit line 122 are connected to a thin transistor channel 126 (shown in FIG. 1B), e.g., made of polysilicon, on the sidewall of the channel 130. All memory transistors in the layer of word lines 106 share a common source bit line 122 and a common drain bit line 114.

[0019] A cross-sectional view of a stack of SONOS nonvolatile transistors in a 3D NAND memory array, shown in FIG. 1B and subsequently in FIGS. 2A-2J, is illustrated by the dotted box 100 in FIG. 1A.

[0020] Each SONOS transistor includes a metal gate (wordline 106), e.g., comprising tungsten, insulated from a transistor channel 126, e.g., comprising polysilicon, by a gate dielectric layer 108. Although sometimes referred to as a SONOS transistor, each SONOS transistor is a metal / oxide / nitride / oxide / silicon (MONOS) stack. During programming, electrons can be trapped in the silicon nitride layer within the gate dielectric layer 108. The trapped electrons increase the turn-on voltage of the SONOS nonvolatile transistor. SONOS transistors with electrons trapped in the silicon nitride layer store a logic state of "1," whereas SONOS transistors with no trapped electrons store a logic state of "0." These logic states are retained for over 10 years, even when the 3D NAND memory is not connected to a power source.

[0021] In a wordline stack, multiple SONOS transistors are stacked on top of each other. The metal gate (wordline 106) of a SONOS transistor is insulated by a layer of silicon dioxide 104 from the other non-volatile SONOS transistors stacked above and below. The stack of SONOS transistors share a common source terminal 112 and also a common drain terminal 116. Lightly doped, e.g., 10 14 cm -3 ~10 17 cm -3 A thin layer of polysilicon layer 110 doped with n-type dopants forms the channel 126 for stacked SONOS transistors in a 3D NAND memory array. The thin layer of lightly doped polysilicon layer 110 may be doped in situ with n-type dopants to form n-channel transistors. One end of the thin layer of lightly doped polysilicon layer 110 is shorted to a common source bitline 122 while the opposite end of the thin layer of lightly doped polysilicon layer 110 is shorted to a common drain bitline 114.

[0022] In operation, a voltage can be applied to the common drain bit line 114 (drain terminal 116) while the common source bit line 122 (source terminal 112) is held at ground. A voltage at the gate terminal 118 can be connected to one of the metal gates (word lines 106) by turning on one of the gate select transistors 120. If the SONOS transistor is programmed to a zero (no electrons trapped), the polysilicon channel will turn on and additional current will flow through the transistor's channel 126. However, if the SONOS transistor is programmed to a one (electrons trapped), the channel 126 will remain OFF and no additional current will flow. The variation from one SONOS transistor to the next in a 3D NAND memory array depends on the uniformity of the thickness of the lightly doped polysilicon transistor channel 126 from one SONOS transistor to the next.

[0023] As described in various embodiments herein, a uniform lightly doped polysilicon transistor channel 126 is formed using a cyclic self-limiting deposition and etch process as further described using Figures 2A-2J and 3.

[0024] Reference is now made to Figure 2A, which illustrates a cross-sectional view of a 3D NAND substrate 300. Alternating dielectric layers of silicon dioxide 104 and silicon nitride 124 are layered over a semiconductor substrate 102. At this stage of processing, the semiconductor substrate 102 includes a number of device regions, including active transistor regions associated with array programming and logic transistors, as well as drain bitlines 114 formed as diffusion regions within the semiconductor substrate 102 to form the common bitlines of the 3D NAND memory.

[0025] In Figure 2A, six alternating layers are shown, but a 3D NAND memory can have more than 100 alternating layers. A channel pattern 128 having openings is formed on the 3D NAND substrate (step 140, Figure 3), through which channels are etched to expose the surface of the dielectric stack.

[0026] Next, as shown in FIG. 2B (step 142, FIG. 3), channels 130 are formed through the stacked dielectric layers of silicon dioxide 104 and silicon nitride 124 after using a lithography process to form a channel pattern 128. The channel pattern 128 may include a hard mask layer that is resistant to etching from a subsequent plasma etching process. For example, the channel pattern 128 may include a metal nitride, such as a titanium nitride layer, in one embodiment.

[0027] The channel 130 stops on the diffusion region of the bitline 114 in the underlying semiconductor substrate 102 or on an etch stop layer. The channel 130 can be formed using a plasma etching process in a plasma tool. In various embodiments, the plasma etching process forms trenches with substantially vertical sidewalls. The plasma etching process, in embodiments, can include a cyclic process designed to alternately etch alternating layers of silicon dioxide 104 and silicon nitride 124. Alternatively, the plasma etching process can include a plasma etch tuned to have the same selectivity to etching silicon dioxide and silicon nitride and to stop on the underlying semiconductor substrate 102.

[0028] In various embodiments, the channel 130 may have an aspect ratio of 50:1 to 100:1. In further embodiments, the channel 130 may have an aspect ratio of more than 100:1, such as up to 500:1. Any remaining channel pattern 128 is removed after the channel etch.

[0029] In Figure 2C, after depositing the SONOS gate dielectric layer 108, a layer of lightly doped polysilicon layer 110 is deposited (step 144, Figure 3). The SONOS gate dielectric layer 108 is deposited to have a uniform thickness on the vertical sidewalls of the channel 130. In various embodiments, the SONOS gate dielectric layer 108 may be formed using an atomic layer deposition process. Alternatively, the SONOS gate dielectric layer 108 is formed using other deposition processes including chemical vapor deposition, plasma deposition, and the like.

[0030] In various embodiments, the SONOS gate dielectric 108 has a thickness between about 2 nm and about 10 nm. The SONOS gate dielectric layer 108 in one embodiment comprises an oxide / nitride / oxide (ONO) stack. In another embodiment, the gate dielectric layer 108 comprises a high-k dielectric / nitride / oxide stack.

[0031] In various embodiments, the polysilicon layer 110 is typically deposited using a deposition process, such as a chemical vapor deposition (CVD) process, capable of covering the surface of the 3D-NAND substrate 101 with a uniform thickness of polysilicon and covering the SONOS gate dielectric layer 108 (step 144, FIG. 4). 14 cm -3 ~10 18 cm -3 and may be doped n-type with phosphorus.

[0032] As discussed above with respect to FIG. 1B, polysilicon layer 110 must be very thin. Thinning avoids degradation and loss of control of the thin film transistor and improves the subthreshold characteristics of the transistor. In various embodiments, polysilicon layer 110 can be deposited slightly thicker than required and then thinned as required for the SONOS transistor using a pseudo atomic layer silicon etching process according to embodiments. In various embodiments, polysilicon layer 110 after thinning is about 5 nm to about 50 nm, such as 10 nm to 20 nm in one embodiment.

[0033] Typically, the polysilicon layer 110 must be thinned by a wet etching process. However, the high aspect ratio of the channel 130, e.g., 50:1 to 500:1, poses significant challenges to current etching solutions such as tetramethylammonium hydroxide (TMAH), because etching with TMAH becomes transport limited, resulting in an etching rate hindered by the concentration at the bottom of the channel. Limited evacuation of reaction by-products and replenishment of the etchant can result in non-uniform thinning of the polysilicon layer 110, compromising device performance. For example, the thickness of the polysilicon layer 110 may be greater at the bottom of the channel 130 and less at the top of the channel 130.

[0034] Embodiments herein overcome these limitations using a self-limiting cyclic process. Referring to FIG. 2D, the 3D-NAND substrate 101 is wetted by immersing it in a bath of oxidizing solution 132, which then penetrates into the channels 130 due to surface tension effects (step 146, FIG. 3). Alternatively, the surface of the polysilicon layer 110 is wetted with the oxidizing solution 132 using a wet spray etching tool. In one embodiment, the oxidizing solution 132 can be an aqueous solution of hydrogen peroxide with a concentration ranging from 1 to 30% by weight. In another embodiment, the oxidizing solution 132 may include ozone.

[0035] When the oxidizing solution 132 contacts the surface of the polysilicon layer 110, the oxidizing solution 132 rapidly oxidizes the surface to form an oxide layer 134 (step 146, FIG. 3). The thickness of the oxide layer 134 that forms is self-limiting and independent of the etchant concentration (rather than transport-limited), resulting in atomic-level control. Specifically, the oxide layer 134 forms a diffusion barrier to the diffusion of the oxidizing solution 132 and to the diffusion of silicon atoms from the polysilicon layer 110. This diffusion barrier prevents further oxidation after all exposed surfaces of the polysilicon layer 110 are covered with the oxide layer 134. Once the surface of the polysilicon layer 110 is covered with the oxide layer 134, further oxidizing solution 132, e.g., hydrogen peroxide, is blocked from the surface of the polysilicon layer 110, and further oxidation of the surface of the polysilicon layer 110 is substantially halted.

[0036] To facilitate the complete filling of the high aspect ratio channels 130 with the oxidizing solution 132, the 3D-NAND substrate 101 can be first cleaned using carbon dioxide. For example, high pressure carbon dioxide gas can be directed towards the surface of the 3D-NAND substrate 101. The expansion of the carbon dioxide gas causes it to cool and solidify as solid carbon dioxide, which is deposited on the surfaces of the 3D-NAND substrate 101 and the channels 130. When the solid carbon dioxide is warmed, it sublimes and increases in volume by as much as 800 times. During this process, the carbon dioxide becomes loose and dislodges particles.

[0037] 2F, the oxidizing solution 132 is removed (step 148, FIG. 3). The 3D-NAND substrate 101 can be rinsed with a solvent to aid in the removal of the oxidizing solution 132. In various embodiments, the 3D-NAND substrate 101 is rinsed by immersion in a bath or by rinsing with a solvent in a wet spray etch tool. In one embodiment, the solvent is deionized water.

[0038] Next, as shown in FIG. 2G, the 3D-NAND substrate 101 is exposed to an oxide remover 136 (step 150, FIG. 3). In the figure, the oxide remover 136 wets the oxide layer 134. The oxide remover 136 may be hydrogen fluoride diluted in water to a concentration in the range of 0.1-10% by weight. Once the oxide layer 134 is removed, the underlying polysilicon layer 110 is exposed and the etching stops. Advantageously, the oxide remover is selected so as not to etch the polysilicon layer 110.

[0039] FIG. 2H shows the 3D-NAND substrate 101 after the oxide layer 134 has been removed using an oxide remover 136 (step 150, FIG. 3).

[0040] 2I, the oxide remover 136 is removed (step 152, FIG. 3). The 3D-NAND substrate 101 can then be rinsed with a solvent to aid in the removal of the oxide remover 136. In various embodiments, the 3D-NAND substrate 101 is rinsed by immersion in a bath or by rinsing with a solvent in a wet spray etch tool. In one embodiment, the solvent is deionized water.

[0041] Steps 146-152 can be repeated as many times as necessary to remove a predetermined thickness of polysilicon layer 110 (step 154, FIG. 3). With every cycle, while the surface of polysilicon layer 110 is wetted by oxidizing solution 132, a surface layer of silicon atoms is converted to oxide layer 134 (e.g., silicon dioxide). This surface layer of silicon atoms is removed when oxide layer 134 is etched away by oxide remover 136. By repeating steps 146-152, silicon atoms are removed one layer at a time in a very controlled and uniform manner, while at the same time reducing the surface roughness of remaining polysilicon layer 110. By removing a predetermined thickness of polysilicon layer 110 in such a controlled and uniform manner, the performance of SONOS transistors in a 3D-NAND memory array can be precisely defined and the variation between SONOS transistors can be minimized. In various embodiments, the predetermined thickness of polysilicon layer 110 can be selected to achieve a target surface roughness or target thickness uniformity of polysilicon layer 110. In an exemplary embodiment, the predetermined thickness of the polysilicon layer 110 may be a portion of the initial thickness of the polysilicon layer 110, for example, 5% to 20% of the initial thickness of the polysilicon layer 110.

[0042] After the polysilicon layer 110 has been thinned to specification, additional processing can be performed to build the 3D NAND structure shown in FIGS. 1A and 1B, including replacing silicon nitride 124 with CVD-tungsten to form the SONOS transistor gates, forming the bitlines by forming a common source bitline 122 and an electrical connection to the source terminal 112, forming a common drain bitline 114 and an electrical connection to the drain terminal 116, forming an electrical connection to the gate terminal 118, and forming the gate select transistor 120.

[0043] FIG. 4 illustrates a cross-sectional view of a fully depleted silicon-on-insulator (FDSOI) transistor 200 formed in accordance with one embodiment of the present application.

[0044] A layer of buried oxide (BOX) 204 insulates the channel formed in the single crystal silicon 206 of the transistor from the underlying substrate 202. The single crystal silicon 206 in the FDSOI transistor 200 is a very thin layer of single crystal silicon, typically less than 150 nm. For FDSOI transistors with ultra-thin channels, the silicon may be 25 nm or less. A transistor gate 210 is insulated from the channel in the single crystal silicon 206 by a gate dielectric layer 208. Silicon regions adjacent to the transistor channel in the single crystal silicon 206 are heavily doped to form a transistor source 214 and a transistor drain 216. Shallow trench isolation 212 electrically insulates the FDSOI transistor 200 from adjacent transistors and other semiconductor devices in the substrate 202. The performance of the FDSOI transistor is very sensitive to the thickness of the channel formed in the single crystal silicon 206. The variability between FDSOI transistors is highly sensitive to thickness variations of the transistor channel in the single crystal silicon 206 from FDSOI transistor to FDSOI transistor.

[0045] The performance of a fully depleted silicon-on-insulator (FDSOI) transistor 200 is highly sensitive to the thickness of the thin channel formed in the single crystal silicon 206. The variability between FDSOI transistors 200 is sensitive to the transistor-to-transistor variation in the thickness of the transistor channel in the single crystal silicon 206. The thickness of the single crystal silicon 206 in FDSOI transistors 200 is typically less than 150 nm. In ultra-thin FDSOI transistors, the single crystal silicon 206 can be 25 nm or less.

[0046] As will be further explained, embodiments of the present invention can be applied to control the thickness uniformity of the thin single crystal silicon 206.

[0047] Thin film transistors (TFTs) with polysilicon channels can also be fabricated. For example, they are used in liquid crystal displays. These transistors with polysilicon channels are formed on insulating substrates and have characteristics similar to partially depleted silicon-on-insulator (PDSOI) transistors or fully depleted silicon-on-insulator (FDSOI) transistors, depending on the thickness of the polysilicon channel. Like PDSOI and FDSOI transistors with single crystal silicon transistor channels, the performance of TFTs with polysilicon channels is sensitive to the thickness and thickness uniformity of the polysilicon transistor channel. The techniques of the embodiments for controlling the thickness and thickness uniformity of the polysilicon transistor channel with atomic layers are equally applicable to polysilicon TFT transistors.

[0048] 5A shows a cross-sectional view of a fully depleted silicon-on-insulator (FDSOI) substrate 202. The electrically isolated single crystal silicon 206 that forms the transistor channel of the FDSOI transistor can then be thinned with high precision using the pseudo atomic layer silicon-based material etching process of the embodiment. In this way, the thickness of the transistor channel in the single crystal silicon 206 can be reduced to the final thinness required for FDSOI transistor performance.

[0049] An FDSOI transistor channel pattern 128 can be formed on the FDSOI substrate 202 to expose a channel region in the single crystal silicon 206 of one FDSOI transistor and not expose the transistor channel region of another FDSOI transistor. In this manner, the thickness of the single crystal silicon 206 can be etched to different thicknesses for different FDSOI transistors to create FDSOI transistors with different performance characteristics (step 230, FIG. 6).

[0050] In FIG. 5B, the surface of the single crystal silicon channel is wetted with an oxidizing solution 132 (step 232, FIG. 6).

[0051] In FIG. 5C, an oxide layer 220, e.g., silicon dioxide, is formed on the single crystal silicon 206 by exposing the single crystal silicon 206 to an oxidizing solution 132 (step 232, FIG. 6). The FDSOI substrate 202 can be wetted by immersion in a bath of the oxidizing solution 132. Alternatively, the surface of the single crystal silicon 206 can be wetted with the oxidizing solution 132 using a wet spray etching tool. The oxidizing solution 132 can be an aqueous solution of hydrogen peroxide having a concentration in the range of about 1-30% by weight. When the hydrogen peroxide contacts the surface of the single crystal silicon 206, it rapidly oxidizes the surface to form an oxide layer 220. The oxide layer 220 that is formed is self-limiting. Once the surface of the single crystal silicon 206 is covered with the oxide layer 220, further hydrogen peroxide is blocked from the surface and further oxidation of the surface of the single crystal silicon 206 is substantially stopped. Beneficially, the oxidation smoothes out any protrusions or trenches on the surface of the single crystal silicon 206, reducing the surface roughness of the single crystal silicon 206.

[0052] In Figure 5D, the oxidizing solution 132 is removed (step 234, Figure 6). The FDSOI substrate 202 can be rinsed with a solvent to aid in the removal of the oxidizing solution 132. The substrate can be rinsed by immersion in a bath or by rinsing with a solvent in a wet spray etch tool. The solvent is typically deionized water.

[0053] 5E shows the FDSOI substrate 202 with the oxide layer 220 exposed to the oxide remover 136 (step 236, FIG. 6). In the figure, the oxide remover 136 wets the oxide layer 220.

[0054] FIG. 5F shows the FDSOI substrate 202 after the surface oxide layer 220 has been etched from the surface by an oxide remover 136 (step 236, FIG. 6). The oxide remover 136 can be an aqueous solution of hydrogen fluoride having a concentration in the range of about 0.1-10% by weight. Once the oxide layer 220 is removed, the underlying single crystal silicon 206 is exposed and the etching stops. The oxide remover 136 does not etch the single crystal silicon 206.

[0055] In Figure 5G, the oxide remover 136 is removed (step 238, Figure 6). The FDSOI substrate 202 can be rinsed with a solvent to aid in the removal of the oxide remover 136. The substrate can be rinsed by immersion in a bath or by rinsing with the solvent in a wet spray etch tool. The solvent is typically deionized water.

[0056] Steps 232-238 can be repeated as many times as necessary to remove a predetermined thickness of SOI single crystal silicon 206 (step 240, FIG. 6). Whenever the surface of SOI single crystal silicon 206 is wetted by oxidizing solution 132, a surface layer of silicon atoms is converted to oxide layer 220. This surface layer of silicon atoms is then removed when oxide layer 220 is exposed to oxide remover 136. By repeating steps 232-238, the surface layer of silicon atoms is removed one layer at a time in a very controlled manner. This tightly controlled and uniform removal of a predetermined thickness of SOI single crystal silicon 206 allows for precise definition of FDSOI transistor performance and minimizes FDSOI transistor-to-transistor variation.

[0057] After the SOI single crystal silicon 206 has been thinned to meet specifications, additional processing can be performed including depositing a gate dielectric 208, depositing and etching a FDSOI transistor gate 210, and doping the source 214 and drain 216 to produce the FDSOI transistor 200 shown in FIG.

[0058] Exemplary embodiments of the present invention are summarized here. Other embodiments can be seen throughout the specification and claims set forth herein.

[0059] Example 1. A method of processing a substrate, the method comprising: forming a channel through the substrate; depositing a layer of polysilicon on sidewalls of the channel; oxidizing an uncovered surface of the polysilicon with an oxidizing agent, the oxidizing agent forming an oxidized layer having a uniform thickness on the uncovered surface of the polysilicon; removing the oxidized layer from the channel with a removing agent; and repeating the steps of oxidizing the uncovered surface and removing the oxidized layer until a predetermined amount of the layer of polysilicon has been removed.

[0060] Example 2. The method of example 1, wherein oxidizing the uncovered surface is carried out using a solution comprising an oxidizing agent.

[0061] Example 3. The method of example 1 or 2, wherein the removal agent comprises a solution comprising HF.

[0062] Example 4. The method of any one of Examples 1-3, wherein forming the channel includes forming the channel through a stack of alternating layers of dielectric material as part of a NAND memory manufacturing process.

[0063] Example 5. The method of any one of Examples 1-4, wherein the channel has an aspect ratio greater than 50:1.

[0064] Example 6. The method of any one of Examples 1 to 5, wherein the oxidizing agent comprises an aqueous hydrogen peroxide solution.

[0065] Example 7. A method of processing a substrate, the method comprising: forming a layer of silicon-based material on a semiconductor substrate having a first thickness; growing a layer of oxidized silicon-based material on the layer of silicon-based material by wetting the layer of silicon-based material with an oxidizing solution; etching the layer of oxidized silicon-based material by wetting the layer of oxidized silicon-based material with an oxide etching solution; and repeating the growing and etching steps until the layer of silicon-based material has a second thickness that is less than a predetermined thickness.

[0066] Example 8. The method of example 7, wherein the silicon-based material is polysilicon or single crystal silicon.

[0067] Example 9. The method of example 7 or 8, further comprising forming a pattern on the silicon-based material prior to growing the layer of oxidized silicon-based material on the exposed areas of the silicon-based material.

[0068] Example 10. The method according to any one of Examples 7-9, further comprising: rinsing the oxidized silicon-based material with a first rinsing solution before etching the oxidized silicon-based material; and rinsing the silicon-based material with a second rinsing solution after etching and removing the oxidized silicon-based material.

[0069] Example 11. The method of any one of Examples 7 to 10, wherein the first rinse solution and the second rinse solution are deionized water.

[0070] Example 12. The method according to any one of Examples 7 to 11, wherein the oxidizing solution is an aqueous hydrogen peroxide solution having a concentration of about 1 to 30% by weight.

[0071] Example 13. The method of any one of Examples 7-12, wherein the oxide etching solution is an aqueous hydrogen fluoride solution having a concentration of about 0.1-10 wt.%.

[0072] Example 14. The method of any one of Examples 7-13, wherein the silicon-based material is wetted with an oxidizing solution by immersion in a first bath, and the layer of oxidized silicon-based material is wetted with an oxide etching solution by immersion in a second bath.

[0073] Example 15. The method of any one of Examples 7-14, wherein the silicon-based material is wetted with the oxidizing solution by immersion in a bath, and the layer of oxidized silicon-based material is wetted with an oxide etching solution in a wet spray etching tool.

[0074] Example 16. The method of one of examples 7-15, wherein the silicon-based material is wetted with an oxidizing solution in a wet spray etching tool, and the layer of oxidized silicon-based material is wetted with an oxide etching solution in a wet spray etching tool.

[0075] Example 17. A method of forming a 3D NAND device, the method comprising: forming a channel in a 3D NAND dielectric stack; depositing a layer of polysilicon having a first thickness on sidewalls of the channel; and performing a cyclical etching process, each cycle comprising forming an oxide layer on the layer of polysilicon by wetting an exposed surface of the layer of polysilicon with a first solution comprising an oxidizer; and removing the oxidized layer from the layer of polysilicon with a second solution comprising an oxide etchant, the cyclical etching process being stopped after the layer of polysilicon has a second thickness on sidewalls of the channel, the second thickness being a predetermined thickness less than the first thickness.

[0076] Example 18. The method of example 17, further comprising rinsing the oxidized silicon-based material with deionized water prior to etching the oxidized silicon-based material, and rinsing the silicon-based material with deionized water after etching and removing the oxidized silicon-based material.

[0077] Example 19. The method of example 17 or 18, wherein the first solution is an aqueous hydrogen peroxide solution having a concentration of about 1-30% by weight.

[0078] Example 20. The method according to any one of Examples 17 to 19, wherein the second solution is an aqueous hydrogen fluoride solution having a concentration of about 0.1 to 10% by weight.

[0079] Example 21. A method of treating a substrate, comprising: depositing a layer of silicon-based material on the substrate; oxidizing an uncovered surface of the silicon-based material with an oxidizing agent, the oxidizing agent forming an oxidized layer having a uniform thickness on the uncovered surface of the silicon-based material; removing the oxidized layer from the silicon-based material with a removing agent; and repeating the steps of oxidizing the uncovered surface and removing the oxidized layer until a predetermined amount of the layer of silicon-based material has been removed.

[0080] Example 22. The method of example 21, wherein oxidizing the uncovered surface is carried out using a solution comprising an oxidizing agent.

[0081] Example 23. The method of example 21 or 22, wherein the oxidizing agent comprises an aqueous hydrogen peroxide solution.

[0082] Example 24. The method of any one of Examples 21-23, wherein the removal agent comprises a solution containing HF.

[0083] Example 25. The method of any one of Examples 21-24, further comprising forming a transistor, wherein the silicon-based material is a channel of the transistor.

[0084] Example 26. The method of any one of Examples 21 to 25, wherein the transistor is a silicon-on-insulator transistor (SOI) having a single crystal silicon channel.

[0085] Example 27. The method according to any one of Examples 21 to 26, wherein the SOI transistor is a fully depleted SOI transistor or a partially depleted SOI transistor.

[0086] Example 28. The method of any one of Examples 21 to 27, wherein the transistor is a polysilicon thin film transistor (TFT).

[0087] Example 29. The method of any one of Examples 21 to 28, wherein the transistor is a NAND nonvolatile transistor having a polysilicon transistor channel.

[0088] Example 30. The method of one of examples 21-29, wherein a polysilicon transistor channel is formed on a sidewall of the channel in a 3D NAND memory array.

[0089] Although the present invention has been described with reference to exemplary embodiments, this specification is not intended to be construed in a limiting sense. Various modifications and combinations of those exemplary embodiments, as well as other embodiments of the present invention, will become apparent to those skilled in the art upon reference to this specification. Therefore, the appended claims are intended to cover any such modifications or embodiments.

Claims

1. 1. A method for processing a substrate, comprising: forming a high aspect ratio (HAR) channel through a substrate, the HAR channel having an aspect ratio greater than 50:1; depositing a layer of polycrystalline silicon on sidewalls of the HAR channel; delivering an oxidizer solution into the HAR channel to oxidize an uncovered surface of the layer of polysilicon, the oxidizer solution forming an oxidized layer, the oxidized layer having a uniform thickness on the uncovered surface of the layer of polysilicon; delivering a remover solution into the HAR channel to remove the oxidized layer from the HAR channel; repeating the steps of oxidizing the uncovered surfaces and removing the oxidized layer until a predetermined amount of the layer of polycrystalline silicon is removed.

2. The method of claim 1 , wherein oxidizing the uncovered surface is performed with a solution that includes the oxidizer solution.

3. The method of claim 1 , wherein the remover solution comprises a solution containing HF.

4. 10. The method of claim 1, wherein forming the HAR channel comprises forming a channel through a stack of alternating layers of dielectric material as part of a NAND memory manufacturing process.

5. The method of claim 1 , wherein the oxidizer solution comprises an aqueous hydrogen peroxide solution.

6. The method of claim 1 , wherein the oxidizer solution comprises a solution containing ozone.

7. The method of claim 1 , wherein the polycrystalline silicon is doped with phosphorus.

8. The method of claim 1 , further comprising rinsing the oxidized layer with deionized water prior to removing the oxidized layer.

9. The method of claim 1 , further comprising, after removing the oxidized layer, rinsing the oxidized layer with deionized water.

10. 2. The method of claim 1, wherein after removing the predetermined amount of the layer of polysilicon, the layer of polysilicon on the sidewalls has a final thickness between 5 nm and 50 nm.

11. 1. A method of forming a 3D NAND device, the method comprising: Forming a high aspect ratio (HAR) channel in a 3D NAND dielectric stack; depositing a layer of polysilicon having a first thickness on sidewalls of the HAR channel; and performing a cyclical etching process, each cycle comprising: forming an oxide layer on the layer of polysilicon by wetting an exposed surface of the layer of polysilicon in the HAR channel with a first solution comprising an oxidizing agent; removing an oxidized layer in the HAR channel from the layer of polysilicon with a second solution comprising an oxide etchant, the cyclic etching process being stopped after the layer of polysilicon has a second thickness on the sidewalls of the HAR channel, the second thickness being a predetermined thickness less than the first thickness.

12. 12. The method of claim 11, further comprising: rinsing the oxidized silicon-based material with deionized water prior to etching the oxidized silicon-based material; and rinsing the silicon-based material with deionized water after etching away the oxidized silicon-based material.

13. The method of claim 11, wherein the first solution is an aqueous hydrogen peroxide solution having a concentration of 1 to 30% by weight.

14. The method of claim 11, wherein the second solution is an aqueous hydrogen fluoride solution having a concentration of 0.1 to 10% by weight.

15. 1. A method of forming a 3D NAND device, the method comprising: Forming a high aspect ratio (HAR) channel in a 3D NAND dielectric stack; depositing a layer of polysilicon having a first thickness on sidewalls of the HAR channel; and performing a cyclical etching process, each cycle comprising: forming an oxide layer on the layer of polysilicon by wetting an exposed surface of the layer of polysilicon in the HAR channel with a first solution comprising an oxidizing agent; rinsing the oxide layer with deionized water; removing the oxidized layer in the HAR channel from the layer of polysilicon using a second solution including an oxide etchant; and rinsing the polysilicon with deionized water, wherein the cyclic etching process is stopped after the layer of polysilicon has a second thickness on the sidewalls of the HAR channel, the second thickness being a predetermined thickness less than the first thickness.

16. The method of claim 15, wherein the first solution is an aqueous hydrogen peroxide solution having a concentration of 1 to 30% by weight.

17. The method of claim 15, wherein the second solution is an aqueous hydrogen fluoride solution having a concentration of 0.1 to 10% by weight.

18. 16. The method of claim 15, wherein the exposed surface of the polysilicon layer is wetted with the first solution by immersion in a first bath and the oxide layer is wetted with an oxide etch solution by immersion in a second bath.

19. 16. The method of claim 15, wherein the exposed surface of the polysilicon layer is wetted with the first solution by immersion in a bath and the oxide layer is wetted with an oxide etch solution in a wet spray etch tool.

20. 16. The method of claim 15, wherein the exposed surface of the polysilicon layer is wetted with the first solution in a wet spray etch tool and the oxide layer is wetted with the second solution in the wet spray etch tool.

Citation Information

Patent Citations

  • Etching method for thin silicon film

    JP1989107545A

  • Method of etching polycrystalline silicon

    JP1990081429A

  • Method for etching

    JP2003037099A

  • Substrate washing apparatus and substrate washing method

    JP2004121907A

  • Etching method of silicon material

    JP2004343013A