Red multi-layer coating and vehicle

The red multi-layer coating film addresses the trade-off between brightness and saturation by combining specific layers with tailored spectral reflectance, resulting in high brightness and chroma for enhanced vehicle design.

JP7587945B2Active Publication Date: 2024-11-21NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020152428
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-10
Publication Date
2024-11-21
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

Existing red single-layer paint films face a trade-off between brightness and saturation, making it difficult to achieve both high brightness and high saturation simultaneously.

Method used

A red multi-layer coating film comprising a white coating film with an L* value of 80 or higher, a first base coating with a hue of 1YR to 10Y, a second base coating with a hue of 1R to 10R, and a clear coating film, with specific spectral reflectance characteristics to balance brightness and saturation.

Benefits of technology

The multi-layer coating film achieves high brightness and high chroma, expanding the range of color expression and enhancing vehicle design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587945000005
    Figure 0007587945000005
  • Figure 0007587945000006
    Figure 0007587945000006
  • Figure 0007587945000007
    Figure 0007587945000007
Patent Text Reader

Abstract

To provide a red-based multilayer coating film having high brightness and high saturation.SOLUTION: A red-based multilayer coating film successively comprises: a white-based coating film with an L* value of 80 or more; a first base coating film having a color tone of 1YR-10Y in a Munsell color system; a second base coating film having a color tone of 1R-10R in a Munsell color system; and a clear coating film. The red-based multilayer coating film has a value at a wavelength of 580 nm of 5% or less in a curve obtained by a value SS acquired by multiplying a spectral reflectance by a spectrum luminous efficiency of the photopic vision of the red-based multilayer coating film, and has a maximum value of 15% or more at a wavelength of 590 nm-650 nm of the curve (here, the spectral reflectance is a spectral reflectance of light received at an acceptance angle of 45° to light exposed from an incident angle of 45° to a normal line of the red-based multilayer coating film at the clear coating film side of the red-based multilayer coating film).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a red-based multi-layer coating film and a vehicle. [Background technology]

[0002] A number of coating films with different functions are successively formed on the surface of an object to be coated, such as an automobile body, to protect the object while at the same time imparting excellent design properties.

[0003] For example, a common method for forming such multiple coating films on an automobile body is to form an undercoat coating film such as an electrodeposition coating film on the substrate, and then form an intermediate coating film and a topcoat coating film in sequence on top of that (see, for example, Patent Document 1). Of these coating films, it is the topcoat coating film that has a particularly large influence on the design of the coating film, and the topcoat coating film is composed of a base coating film and a clear coating film.

[0004] Furthermore, the base coating film can be roughly divided into so-called metallic coating film and solid coating film. Generally, the metallic coating film is a coating film containing a scaly pigment (e.g., aluminum flake) having a glittering feel, and the solid coating film is a coating film not containing a scaly pigment. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2020-099888 Summary of the Invention [Problem to be solved by the invention]

[0006] In addition to metallic paint films, one method of improving the design of automobiles is to use colors with high value (brightness of color) and high saturation (vividness of color).

[0007] Red cars are produced in large numbers, and there are many red car paint colors available, so red is one of the major colors.

[0008] However, in a single-layer red coating, there is generally a trade-off between lightness and saturation, so that increasing the amount of white pigment to increase the lightness of the coating will decrease the saturation of the coating, and increasing the amount of red pigment to increase the saturation of the coating will decrease the lightness.

[0009] The present inventors considered that if a solid coating film could achieve both high brightness and high saturation, the range of color expression would be greatly expanded, and the design of automobiles would be further improved.

[0010] Therefore, an object of the present invention is to provide a reddish coating film having high brightness and high chroma.

[0011] Another object of the present invention is to provide a vehicle having a reddish paint film having high brightness and high chroma. [Means for solving the problem]

[0012] The red-based multi-layer coating film according to the present invention is In order, L * White coating with a value of 80 or more, a first base coat having a hue of 1YR to 10Y in the Munsell Color System; A second base coat having a hue of 1R to 10R in the Munsell Color System; A red-based multi-layer coating film having a clear coating film, A reddish multilayer coating film, in which a value at a wavelength of 580 nm is 5% or less in a curve obtained from a value SS obtained by multiplying the spectral reflectance of the reddish multilayer coating film by the photopic spectral luminous efficiency, and which has a maximum value of 15% or more in the wavelength range of 590 nm to 650 nm on the curve (wherein the spectral reflectance is the spectral reflectance of light received at a receiving angle of 45° with respect to light irradiated at an incident angle of 45° with respect to the normal to the reddish multilayer coating film on the clear coating film side of the reddish multilayer coating film). As a result, the reddish multilayer coating film has high brightness and high saturation.

[0013] In one embodiment of the red multilayer coating film according to the present invention, the curve has a maximum value within a range of 1.5 to 5% at wavelengths of 500 nm to 570 nm.

[0014] The vehicle according to the present invention has a red-based multi-layer paint film, and the clear paint film side is positioned on the outer side. This gives the vehicle high lightness and high saturation. Effect of the Invention

[0015] According to the present invention, it is possible to provide a reddish paint film having high lightness and high chroma. According to the present invention, it is possible to provide a vehicle having a reddish paint film having high lightness and high chroma. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a red multilayer coating film of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the configuration of the red multilayer coating film of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a method for measuring the spectral reflectance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, embodiments of the present invention will be described. These descriptions are intended to be illustrative of the present invention and are not intended to limit the present invention in any way.

[0018] In the present invention, two or more embodiments can be combined in any manner.

[0019] In the present invention, L * Value, a * Value, b * Value and C * The values ​​are the CIE 1976 lightness index and CIELAB 1976 a defined in JIS Z 8781-4:2013, respectively. * Coordinates, CIELAB 1976 b * Coordinates are CIELAB 1976 ab chroma. * The higher the value, the higher the whiteness and brightness of the object being measured. * The smaller the value, the higher the blackness of the object being measured. * The more negative the value, the more green the object being measured is, and the more positive the value, the more magenta the object being measured is. * The larger the negative value, the greater the blueness of the object being measured, and the larger the positive value, the greater the yellowness of the object being measured. * The value is an index of saturation, with a larger value indicating that the color of the object being measured is more vivid, and a smaller value indicating that the object being measured is more achromatic.

[0020] In the present invention, the L of the red-based multi-layer coating film and the white-based coating film * Value, a * Value, b * Value and C * The value is measured by the method described in the Examples.

[0021] In the present invention, the spectral reflectance of the red multilayer coating film is measured by the method described in the Examples.

[0022] In the present invention, the thickness of each coating film or layer is referred to as "film thickness."

[0023] In this specification, unless otherwise specified, numerical ranges are intended to include the upper and lower limits of the range. For example, 590 to 650 nm means not less than 590 nm and not more than 650 nm.

[0024] In the present invention, the paint and the paint composition can be used interchangeably.

[0025] The accompanying drawings are schematic diagrams given priority in order to facilitate understanding of the present invention, and therefore the coatings and layers in the drawings are not drawn to exact scale.

[0026] In the present invention, terms such as first, second, etc. are used herein to describe various layers, but these layers are not limited by these terms, and these terms are used only to distinguish one layer from another.

[0027] (Red multi-layer coating) The red-based multi-layer coating film according to the present invention is In order, L * White coating with a value of 80 or more, a first base coat having a hue of 1YR to 10Y in the Munsell Color System; A second base coat having a hue of 1R to 10R in the Munsell Color System; A red-based multi-layer coating film having a clear coating film, A reddish multilayer coating film, in which, on a curve obtained from a value SS obtained by multiplying the spectral reflectance of the reddish multilayer coating film by the photopic spectral luminous efficiency, a value at a wavelength of 580 nm is 5% or less, and which has a maximum value of 15% or more in the wavelength range of 590 nm to 650 nm on the curve (wherein the spectral reflectance is the spectral reflectance of light received at a receiving angle of 45° with respect to light irradiated at an incident angle of 45° with respect to the normal to the reddish multilayer coating film on the clear coating film side of the reddish multilayer coating film).

[0028] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of the red-colored multi-layer coating film of the present invention. The red-colored multi-layer coating film 1 of the example of FIG. 1 is, in order, * The apparatus has a white coating film 10 having a value of 80 or more, a first base coating film 20 having a hue of 1YR to 10Y in the Munsell color system, a second base coating film 30 having a hue of 1R to 10R in the Munsell color system, and a clear coating film 40.

[0029] The essential components of the reddish multilayer coating film of the present invention, that is, the white coating film, the first base coating film, the second base coating film, and the clear coating film, are exemplified below. Hereinafter, the white coating film and the clear coating film of the reddish multilayer coating film of the present invention may be simply referred to as the "white coating film" and the "clear coating film", respectively.

[0030] ·White paint film The white-based coating film of the red-based multi-layer coating film of the present invention is L * It is a white coating film having a value of 80 or more, and is an intermediate coating film. The white coating film of the red multilayer coating film of the present invention has the function of imparting brightness to the red multilayer coating film.

[0031] The "white" in white-based coating refers to N8.0 to N10.0 on the Japan Paint Color Sample.

[0032] White coating L * The value is 80 or more, L * If the value is less than 80, it is not possible to achieve both high brightness and high chroma of the reddish multi-layer coating film. * The value is, for example, 80 to 95. In one embodiment, the L * The value is 80 or more, 81 or more, 82 or more, 83 or more, 84 or more, 85 or more, 86 or more, 87 or more, 89 or more, 90 or more, 91 or more, 92 or more, 93 or more, or 94 or more. * The values ​​are 95 or less, 94 or less, 93 or less, 92 or less, 91 or less, 90 or less, 89 or less, 88 or less, 87 or less, 86 or less, 85 or less, 84 or less, 83 or less, 82 or less, or 81 or less.

[0033] The white coating film contains a white pigment and a coating film-forming resin.

[0034] The white pigment is not particularly limited, and known white pigments such as titanium oxide, barium sulfate, zinc oxide, etc. The white pigments may be used alone or in combination of two or more.

[0035] The amount of white pigment in a white coating is L * The content may be appropriately adjusted so that the value is 80 or more, for example, 1 to 60 parts by mass per 100 parts by mass of the solid content of the coating film-forming resin for a white coating film.

[0036] The white coating film may contain a known luster pigment such as a scaly aluminum flake pigment, a mica pigment, a graphite pigment, or a glass flake pigment, as long as the effect of the present invention is not impaired. When the white coating film contains a luster pigment, the content is, for example, 5 parts by mass or less, 4 parts by mass or less, 3 parts by mass or less, 2 parts by mass or less, 1 part by mass or less, 0.5 parts by mass or less, or 0.1 parts by mass or less, relative to 100 parts by mass of the solid content of the coating film-forming resin of the white coating film. In one embodiment, the white coating film does not contain a luster pigment.

[0037] The film-forming resin of the white coating film is not particularly limited, and a known film-forming resin of an intermediate coating film can be used. Examples of the film-forming resin of the white coating film include acrylic resin, polyester resin, polyurethane resin, epoxy resin, fluororesin, silicone resin, and polyether resin. The film-forming resin may be used alone or in combination of two or more.

[0038] The white coating film only needs to contain a white pigment and a coating film-forming resin, and may also contain other components such as pigments other than the white pigment, a curing agent, a dispersing agent, an antifoaming agent, and a leveling agent.

[0039] White coating L *Examples of methods for achieving a value of 80 or more include blending 1 to 60 parts by mass of the above white pigment per 100 parts by mass of the solid content of the coating film-forming resin of the white coating film, and using a high refractive index pigment.

[0040] The thickness of the white coating film is not particularly limited and may be appropriately adjusted, for example, 5 to 50 μm, preferably 10 to 30 μm. In one embodiment, the thickness of the white coating film is 10 μm or more, 15 μm or more, 20 μm or more, or 25 μm or more. In another embodiment, the thickness of the white coating film is 30 μm or less, 25 μm or less, 20 μm or less, or 15 μm or less.

[0041] The white coating film may be used alone or in combination with L * Two or more types with different values, thicknesses, etc. may be used in combination. For example, in a part with a red multi-layer coating, the L * The value is 80, and in another part of the red multi-layer coating, the L value of the white coating is * The value may be 85.

[0042] First base coat The first base coating film of the red multi-layer coating film of the present invention is a coating film having a hue of 1YR to 10Y in the Munsell color system, and is the first topcoat coating film. The first base coating film of the red multi-layer coating film of the present invention has the function of imparting brightness and chroma to the red multi-layer coating film.

[0043] The first base coating has one or more hues selected from the group consisting of 1YR to 10Y in the Munsell Color System (100 hues), that is, 1YR, 2YR, 3YR, 4YR, 5YR, 6YR, 7YR, 8YR, 9YR, 10YR, 1Y, 2Y, 3Y, 4Y, 5Y, 6Y, 7Y, 8Y, 9Y and 10Y. If the hue of the first base coating is redder (5R) than 1YR or greener (5GY) than 10Y, the lightness and chroma of the red-based multi-layer coating cannot be highly balanced. In a preferred embodiment, the hue of the first base coating is one or more hues selected from the group consisting of 6YR, 4Y, 5Y, 6Y, 7Y, 8Y, 9Y and 10Y, from the viewpoint of increasing visual sensitivity. In another preferred embodiment, the hue of the first base coating is one or more selected from the group consisting of 4Y, 5Y, 6Y, 7Y, 8Y, 9Y, and 10Y. In yet another preferred embodiment, the hue of the first base coating is one or more selected from the group consisting of 5Y, 6Y, 7Y, 8Y, 9Y, and 10Y. In yet another preferred embodiment, the hue of the first base coating is one or more selected from the group consisting of 5Y and 10Y.

[0044] The first base coat includes a pigment and a film-forming resin.

[0045] The pigment of the first base coating film is not particularly limited as long as it can adjust the hue of the first base coating film to a hue range of 1YR to 10Y. For example, a known pigment such as Hoster Palm Yellow can be used as the pigment of the first base coating film. The pigment of the first base coating film may be used alone or in combination of two or more kinds.

[0046] The amount of pigment in the first base coating film may be appropriately adjusted so that the hue of the first base coating film is in the range of 1YR to 10Y, for example, 1 to 30 parts by mass per 100 parts by mass of the solid content of the coating film-forming resin of the first base coating film.

[0047] The first base coating film may contain the above-mentioned luster pigment as long as it does not impair the effects of the present invention. When the first base coating film contains the luster pigment, the content is, for example, 5 parts by mass or less, 4 parts by mass or less, 3 parts by mass or less, 2 parts by mass or less, 1 part by mass or less, 0.5 parts by mass or less, or 0.1 parts by mass or less, relative to 100 parts by mass of the solid content of the coating film-forming resin of the first base coating film. In one embodiment, the first base coating film does not contain the luster pigment.

[0048] The film-forming resin of the first base coating film is not particularly limited, and can be any known film-forming resin for topcoat coating films. For example, the film-forming resin of the first base coating film can be the film-forming resin listed in the white coating film above. The film-forming resin can be used alone or in combination of two or more.

[0049] The first base coating film contains a pigment and a coating film-forming resin, and its hue is required to be within the hue range of 1YR to 10Y. It may also contain other components such as pigments other than the pigments mentioned above, a curing agent, a dispersant, an antifoaming agent, and a leveling agent.

[0050] The thickness of the first base coating film is not particularly limited and may be appropriately adjusted, for example, 2 to 30 μm, preferably 5 to 15 μm. By making the thickness thicker than 5 μm, the brightness and chroma of the red-based multilayer coating film are likely to be highly increased. In addition, by making the thickness thinner than 15 μm, the brightness of the red-based multilayer coating film can be maintained higher while increasing the chroma by making use of the brightness of the white coating film as the base. In one embodiment, the thickness of the first base coating film is 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, 10 μm or more, 11 μm or more, 12 μm or more, 13 μm or more, or 14 μm or more. In another embodiment, the first base coating has a thickness of 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, or 6 μm or less.

[0051] The first base coating film may be used alone or in combination of two or more different types having different hues, film thicknesses, etc. For example, in one portion of the red-based multilayer coating film, the hue of the first base coating film may be 5Y, and in another portion of the red-based multilayer coating film, the hue of the first base coating film may be 10Y.

[0052] Second base coat The second base coating film of the reddish multi-layer coating film of the present invention is a coating film having a hue of 1R to 10R in the Munsell Color System, and is a second topcoat coating film. The second base coating film of the reddish multi-layer coating film of the present invention has the function of imparting chroma to the reddish multi-layer coating film.

[0053] The second base coating has one or more hues selected from the group consisting of 1R to 10R hues in the Munsell color system (100 hues), that is, 1R, 2R, 3R, 4R, 5R, 6R, 7R, 8R, 9R and 10R. If the hue of the second base coating is more purple than 1R or more orange than 10R, the lightness and chroma of the red-based multi-layer coating cannot be highly balanced. In a preferred embodiment, the hue of the second base coating is one or more hues selected from the group consisting of 3R, 4R, 5R, 6R and 7R, from the viewpoint of improving both lightness and chroma.

[0054] The second base coat includes a pigment and a film-forming resin.

[0055] The pigment of the second base coating film is not particularly limited as long as it can adjust the hue of the second base coating film to a hue range of 1R to 10R. For example, a known pigment such as Irgazin DPP Red can be used as the pigment of the second base coating film. The pigment of the second base coating film may be used alone or in combination of two or more kinds.

[0056] The amount of pigment in the second base coating film may be appropriately adjusted so that the hue of the second base coating film is in the range of 1R to 10R, for example, 1 to 30 parts by mass per 100 parts by mass of the solid content of the coating film-forming resin of the second base coating film.

[0057] The second base coating film may contain the above-mentioned luster pigment as long as it does not impair the effects of the present invention. When the second base coating film contains the luster pigment, the content is, for example, 5 parts by mass or less, 4 parts by mass or less, 3 parts by mass or less, 2 parts by mass or less, 1 part by mass or less, 0.5 parts by mass or less, or 0.1 parts by mass or less, relative to 100 parts by mass of the solid content of the coating film-forming resin of the second base coating film. In one embodiment, the second base coating film does not contain the luster pigment.

[0058] The film-forming resin of the second base coating film is not particularly limited, and can be any known film-forming resin of a topcoat coating film. For example, the film-forming resin of the second base coating film can be the film-forming resin listed in the above white coating film. The film-forming resin can be used alone or in combination of two or more.

[0059] The second base coating film contains a pigment and a coating film-forming resin, and its hue is required to be within the hue range of 1R to 10R, and may contain other components such as pigments other than the pigments mentioned above, curing agents, dispersants, defoamers, and leveling agents.

[0060] The thickness of the second base coating film is not particularly limited and may be appropriately adjusted, for example, 2 to 30 μm, preferably 5 to 15 μm. By setting the thickness to 5 to 15 μm, the brightness and chroma of the red-based multilayer coating film can be more highly balanced. In one embodiment, the thickness of the second base coating film is 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, 10 μm or more, 11 μm or more, 12 μm or more, 13 μm or more, or 14 μm or more. In another embodiment, the thickness of the second base coating film is 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, or 6 μm or less.

[0061] The second base coating film may be used alone or in combination of two or more different types having different hues, film thicknesses, etc. For example, in one portion of the red-based multilayer coating film, the hue of the second base coating film may be 3R, and in another portion of the red-based multilayer coating film, the hue of the second base coating film may be 7R.

[0062] Clear coating The clear coating film of the red-based multilayer coating film of the present invention has the function of imparting weather resistance to the red-based multilayer coating film. The clear coating film is not particularly limited, and can be, for example, a known clear coating film described in JP-A-2016-188332.

[0063] The clear coating film includes a coating film-forming resin. The coating film-forming resin of the clear coating film is not particularly limited, and a known coating film-forming resin of a clear coating film can be used. For example, the coating film-forming resin of the clear coating film includes the coating film-forming resins listed in the above white coating film. The coating film-forming resin may be used alone or in combination of two or more.

[0064] The clear coating film may contain other components such as an ultraviolet absorbing agent, a pigment, a hardening agent, a dispersing agent, an antifoaming agent, and a leveling agent in addition to the coating film-forming resin.

[0065] The clear coating film may contain the above-mentioned luster pigment as long as it does not impair the effects of the present invention. When the clear coating film contains the luster pigment, the content is, for example, 3 parts by mass or less, 2 parts by mass or less, 1 part by mass or less, 0.5 parts by mass or less, or 0.1 parts by mass or less, relative to 100 parts by mass of the solid content of the coating film-forming resin of the clear coating film. In one embodiment, the clear coating film does not contain the luster pigment.

[0066] The thickness of the clear coating film is not particularly limited and may be appropriately adjusted, for example, 10 to 80 μm. In one embodiment, the thickness of the clear coating film is 10 μm or more, 20 μm or more, 30 μm or more, 35 μm or more, 40 μm or more, 50 μm or more, 60 μm or more, or 70 μm or more. In another embodiment, the thickness of the clear coating film is 80 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, or 20 μm or less.

[0067] Other layers The reddish multilayer coating film of the present invention may have, in order, a whiteish coating film, a first base coating film, a second base coating film, and a clear coating film, and may also have other layers in any position in addition to these.

[0068] Fig. 2 is a schematic cross-sectional view showing another example of the configuration of the reddish multilayer coating film of the present invention. The reddish multilayer coating film 1 of the example of Fig. 2 has, in order, a white coating film 10, a metal vapor deposition layer 50, a first base coating film 20, a second base coating film 30, and a clear coating film 40.

[0069] In one embodiment, the reddish multilayer coating film of the present invention has, in order, a whiteish coating film 10, a first base coating film 20, a second base coating film 30, and a clear coating film 40. In another embodiment, the reddish multilayer coating film of the present invention is composed of four layers, in order, a whiteish coating film 10, a first base coating film 20, a second base coating film 30, and a clear coating film 40.

[0070] In one embodiment, the red-based multi-layer coating film of Hontsuaki does not contain a luster pigment.

[0071] The thickness of the reddish multi-layer coating film is not particularly limited and may be appropriately adjusted, for example, 40 to 100. In one embodiment, the thickness of the reddish multi-layer coating film is 40 μm or more, 50 μm or more, 60 μm or more, 70 μm or more, 80 μm or more, 85 μm or more, or 90 μm or more. In another embodiment, the thickness of the reddish multi-layer coating film is 100 μm or less, 90 μm or less, 85 μm or less, 80 μm or less, 70 μm or less, 60 μm or less, or 50 μm or less.

[0072] - Curve obtained by multiplying spectral reflectance and photopic spectral luminous efficiency The reddish multilayer coating film of the present invention has a value of 5% or less at a wavelength of 580 nm in a curve obtained by multiplying the spectral reflectance (%) of the reddish multilayer coating film by the spectral luminous efficiency of photopic vision, and has a maximum value of 15% or more at wavelengths of 590 nm to 650 nm on the curve. This allows the reddish multilayer coating film to have high brightness and high saturation.

[0073] In the present invention, the spectral reflectance (%) is the spectral reflectance of light received at an angle of 45° (acceptance angle 45°) from the regular reflected light to the incident light direction, relative to light irradiated at an angle of 45° (incident angle 45°) to the normal line of the reddish multilayer coating film on the clear coating film side of the reddish multilayer coating film (see FIG. 3). The target wavelength range of the spectral reflectance is 400 nm to 700 nm, and the spectral reflectance is a value obtained by measuring at 10 nm intervals in the wavelength range of 400 nm to 700 nm.

[0074] Spectral luminous efficiency is a numerical value (maximum 1) that represents the intensity at which the human eye perceives brightness at each wavelength of light. Photopic spectral luminous efficiency is the CIE standard spectral luminous efficiency for photopic vision. The photopic spectral luminous efficiency values ​​at 5 nm intervals in the wavelength range of 360 nm to 830 nm are specified, for example, in Appendix 8 of the Measurement Unit Regulations, Ministry of International Trade and Industry Ordinance No. 80 of 1992. For example, the photopic spectral luminous efficiency for wavelengths of 450 nm to 650 nm is as shown in Table 1 below, with the maximum spectral luminous efficiency at a wavelength of 555 nm being 1. [Table 1]

[0075] In the present invention, it is believed that it is possible to evaluate the hue and texture more closely to visual evaluation by not only the spectral reflectance of a red-based multilayer coating film, but also by using the value SS obtained by multiplying that spectral reflectance by the spectral luminous efficiency in photopic vision.

[0076] Furthermore, in the present invention, the curve obtained from the value SS obtained by multiplying the spectral reflectance of the reddish multilayer coating film by the photopic spectral luminous efficiency (hereinafter, sometimes simply referred to as the "curve of the value SS") has a value of 5% or less at a wavelength of 580 nm, and has a maximum value of 15% or more at wavelengths of 590 nm to 650 nm. The reddish multilayer coating film has high brightness and high saturation by having such a curve. If the value of the curve of the value SS at a wavelength of 580 nm is greater than 5%, the color of the multilayer coating film becomes more yellowish and deviates from red. Also, if the maximum value is less than 15% at wavelengths of 590 nm to 650 nm of the curve of the value SS, the color of the reddish multilayer coating film becomes black and turbid, and high brightness and high saturation cannot be achieved at the same time.

[0077] The value of the curve of the value SS at a wavelength of 580 nm is 5% or less. The value of the curve of the value SS at a wavelength of 580 nm is, for example, 0.1 to 5.0%. In one embodiment, the value of the curve of the value SS at a wavelength of 580 nm is 5.0% or less, 4.7% or less, 4.6% or less, 4.5% or less, 4.2% or less, 4.0% or less, 3.8% or less, 3.7% or less, 3.5% or less, 3.0% or less, 2.5% or less, 2.0% or less, 1.5% or less, 1.0% or less, or 0.5% or less. In another embodiment, the value of the curve of the value SS at a wavelength of 580 nm is 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, 2.5% or more, 3.0% or more, 3.5% or more, 3.7% or more, 3.8% or more, 4.0% or more, 4.2% or more, 4.5% or more, 4.6% or more, or 4.7% or more. In yet another embodiment, the value of the curve of the value SS at a wavelength of 580 nm is 2.5 to 5.0%. In yet another embodiment, the value of the curve of the value SS at a wavelength of 580 nm is 3.0 to 4.7%.

[0078] In addition to forming the red-based multi-layer coating film into the above-mentioned four layers, for example, * Setting the value to 50 or more also contributes to setting the value SS to 5% or less at a wavelength of 580 nm.

[0079] The curve of the value SS has a maximum value of 15% or more at wavelengths of 590 nm to 650 nm. The maximum value of the curve of the value SS at wavelengths of 590 nm to 650 nm is, for example, 15.0 to 40.0%. In one embodiment, the maximum value of the curve of the value SS at wavelengths of 590 nm to 650 nm is 15.0% or more, 16.0% or more, 16.3% or more, 16.5% or more, 17.0% or more, 17.5% or more, 18.0% or more, 18.5% or more, 19.0% or more, 19.4% or more, 19.5% or more, 20.0% or more, 20.5% or more, 21.0% or more, 21.5% or more, 22.0% or more, 22.5% or more, 23.0% or more, 23.5% or more, 24.0% or more, 24.5% or more, 25.0% or more, 25.1% or more, 25.3% or more, 25.5% or more, 26.0% or more, 26.5% or more, 27.0% or more, 27.5% or more, 28.0% or more, 28.5% or more, 29.0% or more, 29.5% or more, 30.0% or more, 30.5% or more, 31.0% or more, 31.5% or more, 32.0% or more, 32.5% or more, 33.0% or more, 33.5% or more, 34.0% or more, 34.5% or more, 35.0% or more, 36.0% or more, 37.0% or more, 38.0% or more, or 39.0% or more. In another embodiment, the maximum value of the curve of the value SS at wavelengths of 590 nm to 650 nm is 40.0% or less, 39.0% or less, 38.0% or less, 37.0% or less, 36.0% or less, 35.0% or less, 34.5% or less, 34.0% or less, 33.5% or less, 33.0% or less, 32.5% or less, 32.0% or less, 31.5% or less, 31.0% or less, 30.5% or less, 30.0% or less, 29.5% or less, 29.0% or less, 28.5% or less, 28.0% or less, 27.5% or less, 27.0% or less, 26.5% or less, 26.0% or less, 25.5% or less, 25.3% or less, 25.1% or less, 25.0% or less, 24.5% or less, 24.0% or less, 23.5% or less, 23.0% or less, 22.5% or less, 22.0% or less, 21.5% or less, 21.0% or less, 20.5% or less, 20.0% or less, 19.5% or less, 19.4% or less, 19.0% or less, 18.5% or less, 18.0% or less, 17.5% or less, 17.0% or less, 16.5% or less, 16.3% or less, or 16.0% or less.

[0080] In addition to forming the red-based multi-layer coating film into the four layers described above, for example, the L of the first base coating film * Value and C * Setting the value to 65 or more also contributes to obtaining a value SS having a maximum value of 15% or more in the wavelength range of 590 nm to 650 nm.

[0081] The wavelength range in which the curve for the value SS has a maximum value of 15% or more is 590 nm to 650 nm, but from the viewpoint of obtaining a red color with higher brightness and higher saturation in a red-based multilayer coating film, in a preferred embodiment, the curve has a maximum value of 15% or more at a wavelength of 600 nm to 630 nm, and in another preferred embodiment, the curve has a maximum value of 15% or more at a wavelength of 610 nm.

[0082] The larger the value SS at a wavelength of 660 nm, the higher the brightness and saturation. The value SS at a wavelength of 660 nm of the curve of the value SS is, for example, 0.1 to 5.0%. In one embodiment, the value SS at a wavelength of 660 nm of the curve of the value SS is 5.0% or less, 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, 2.0% or less, 1.5% or less, 1.0% or less, or 0.5% or less. In another embodiment, the value SS at a wavelength of 660 nm of the curve of the value SS is 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, 2.5% or more, 3.0% or more, 3.5% or more, 4.0% or more, or 4.5% or more.

[0083] In the curve of the value SS, the value SS in the wavelength region shorter than 580 nm and the shape of the curve are not particularly limited, but for example, the curve of the value SS preferably has a maximum value of 5.0% or less in the wavelength region of 500 nm to 570 nm. This allows the lightness and chroma of the red multilayer coating film to be more highly balanced.

[0084] In one embodiment, the curve of the value SS has a maximum value of 1.0% or more, 1.5% or more, 1.6% or more, 1.9% or more, 2.0% or more, 2.1% or more, 2.2% or more, 2.3% or more, 2.4% or more, 2.5% or more, 3.0% or more, 3.5% or more, 4.0% or more, or 4.5% or more at wavelengths of 500 nm to 570 nm. In another embodiment, the curve of the value SS has a maximum value of 5.0% or less, 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, 2.4% or less, 2.3% or less, 2.2% or less, 2.1% or less, 2.0% or less, 1.6% or less, 1.5% or less, 1.0% or less, or 0.5% or less at wavelengths of 500 nm to 570 nm. In yet another embodiment, the curve for the value SS has a maximum value within the range of 1.5 to 5% at wavelengths between 500 nm and 570 nm.

[0085] As a means for adjusting the value of the SS curve at wavelengths of 500 nm to 570 nm to 1.5% or more, for example, the L * Value and C * The value of SS in the curve at wavelengths of 500 nm to 570 nm can be adjusted to 5% or less by, for example, adjusting the a * The value should be 50 or more.

[0086] In one embodiment, the curve of the value SS has a maximum value of 5.0% or less at wavelengths of 530 nm to 560 nm, in another embodiment, the curve of the value SS has a maximum value of 1.5 to 2.5% or less at wavelengths of 540 nm to 550 nm.

[0087] By reducing the value SS at wavelengths of 400 nm to 490 nm, the decrease in saturation of the red-based multilayer coating film can be suppressed. In one embodiment, the curve of the value SS is 1.0% or less, 0.7% or less, 0.5% or less, 0.3% or less, 0.2% or less, or 0.1% or less at wavelengths of 400 nm to 490 nm. In another embodiment, the curve of the value SS is 1.0% or less, 0.7% or less, 0.5% or less, 0.3% or less, 0.2% or less, or 0.1% or less at wavelengths of 400 nm to 450 nm.

[0088] In the curve of the value SS, the value SS and the shape of the curve in the wavelength region longer than 670 nm are not particularly limited. The larger the value SS in the wavelength region from 670 nm to 700 nm, the higher the brightness and saturation. The value SS in the curve of the value SS in the wavelength region from 670 nm to 700 nm is, for example, 0.1 to 5.0%. In one embodiment, the value SS in the curve of the value SS in the wavelength region from 670 nm to 700 nm is 5.0% or less, 4.5% or less, 4.0% or less, 3.5% or less, 3.0% or less, 2.5% or less, 2.0% or less, 1.5% or less, 1.0% or less, or 0.5% or less. In another embodiment, the value SS of the curve at a wavelength of 660 nm is 0.5% or more, 1.0% or more, 1.5% or more, 2.0% or more, 2.5% or more, 3.0% or more, 3.5% or more, 4.0% or more, or 4.5% or more. In yet another embodiment, the value of the curve at wavelengths of 670 nm to 700 nm of the value SS is 1.5 to 2.5%.

[0089] ·How to form red multi-layer coating The method for forming the red-based multi-layer coating film of the present invention is not particularly limited, as long as a predetermined white-based coating film, a first base coating film, a second base coating film and a clear coating film are formed on the surface of the substrate in order, and the above-mentioned predetermined value SS is obtained. For example, an electrodeposition coating film is formed on the substrate, then a coating composition for a white-based coating film is applied on the electrodeposition coating film to form a white-based coating film, and dried to form a white-based coating film, then a coating composition for a first base coating film is applied on the white-based coating film to form a first base coating film, and dried to form a first base coating film, then a coating composition for a second base coating film is applied on the first base coating film to form a second base coating film, and dried to form a second base coating film, then a coating composition for a clear coating film is applied on the second base coating film to form a clear coating film, and dried to form a clear coating film, thereby obtaining a red-based multi-layer coating film. Alternatively, one or more of the coating composition for the white coating film, the coating composition for the first base coating film, the coating composition for the second base coating film and the coating composition for the clear coating film may be applied to form an uncured coating film, and then the next coating composition may be applied onto the uncured coating film to form a further uncured coating film, and the two or more uncured coating films may be cured together.

[0090] The coating composition for each coating film can be prepared by mixing, in addition to the pigment and film-forming resin described above, optionally a solvent, an ultraviolet absorber, a curing agent, a dispersant, an antifoaming agent, a leveling agent, a curing catalyst, an antioxidant, and the like.

[0091] The coating composition of each coating film may be a water-based coating composition or a solvent-based coating composition.

[0092] Examples of the solvent include water, ester-based solvents, ether-based solvents, alcohol-based solvents, ketone-based solvents, aliphatic hydrocarbon-based solvents, and aromatic solvents.

[0093] When any of the coating films in the red multilayer coating film is heated to cure, the heating temperature is not particularly limited and may be appropriately adjusted. The heating temperature is, for example, 80 to 180° C. The heating time is, for example, 5 to 60 minutes. The coating film may be dried at room temperature without heating.

[0094] The substrate on which the reddish multilayer coating film of the present invention is formed is not particularly limited, and examples thereof include metals, plastics, foams, etc. Examples of metals include iron, copper, aluminum, tin, zinc, and alloys thereof.

[0095] (vehicle) The vehicle according to the present invention has the above-mentioned red-based multi-layer paint film, with the clear paint film side positioned on the outside, thereby giving the vehicle high lightness and high chroma.

[0096] The vehicle is not particularly limited and may be any known vehicle, including, for example, automobiles such as passenger cars, buses, trucks, and motorcycles, motorized bicycles, trains, and racing cars.

[0097] The vehicle may have a red-based multi-layer coating film on at least a part thereof, for example, the vehicle body, tires, wheels, or vehicle interior.

[0098] The red-based multi-layer paint film on the vehicle may be of one type alone or a combination of two or more types.

[0099] In the method for producing a vehicle of the present invention, a vehicle can be produced by carrying out the above-mentioned method for forming a reddish multi-layer coating film using a vehicle as a substrate.

[0100] (Goods) In another embodiment of the present disclosure, it is also possible to provide an article having the above-mentioned red-based multi-layer coating film, with the clear coating film side being positioned on the outside. This allows the article to have high brightness and high chroma.

[0101] The article or substrate is not particularly limited, and examples include vehicle tires; ships; aircraft such as airplanes and helicopters; walls, floors, ceilings, roofs, pillars, signs, electronic signs (digital signage), doors, gates, windows of buildings or structures such as detached houses, apartment complexes, office buildings, public facilities, commercial facilities, research facilities, military facilities, and tunnels; glass of vehicles and buildings; bridges; vending machines; road signs; traffic lights; street lights; electronic billboards such as LED, LCD, and light bulb types; work machines, construction machines; stone monuments; gravestones; packaging materials; mirrors; toys; and transparent bodies such as glass, acrylic, and polycarbonate cases, containers, resin plates, and films.

[0102] The red-based multi-layer coating film on the article may be of one type alone or a combination of two or more types.

[0103] As a method for producing an article, the article can be produced by carrying out the above-mentioned method for forming a reddish multilayer coating film on the article as a substrate. EXAMPLES

[0104] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.

[0105] Details of the materials used in the examples are as follows: Polyester-melamine paint: Nippon Paint Automotive Coatings' product name "OP-30P White" White pigment: CR-97 Acrylic resin emulsion: Prepared in the same manner as in Production Example 13 described in paragraph

[0100] of JP 2020-002244 A. Phosphate group-containing acrylic resin: Prepared in the same manner as in Production Example 4 described in paragraph

[0121] of JP 2018-135439 A Nonionic surfactant: Trade name "Noigen EA-207D" manufactured by Daiichi Kogyo Seiyaku Co., Ltd., amphiphilic compound, number average molecular weight 4200, solid content 55% Linoleic acid: Kishida Chemical Co., Ltd. Mixed alkylated melamine resin: Allnex, Cymel 327 (90% solids) Electrodeposition paint composition: Nippon Paint Automotive Coatings' product name "Power Top U-50" Paint composition for clear coating: Product name "Macflow-O-1810" manufactured by Nippon Paint Automotive Coatings Co., Ltd.

[0106] Details of the apparatus used in the examples are as follows. Spray gun: Anest Iwata product name "W-101-132G" Multi-angle spectrophotometer: X-Rite product name "MA68II"

[0107] Preparation of white coating composition 1 White pigment CR-97 was mixed into "OP-30P White" at 70% by mass. The mixture was diluted using a No. 4 Ford cup so that the outflow time measured at 20°C was 25 seconds, to prepare coating composition 1 for white coating films.

[0108] Preparation of white coating composition 2 Coating composition 2 for white coating films was prepared in the same manner as in preparation of coating composition 1 for white coating films, except that the amount of white pigment was changed to 69 mass %.

[0109] Preparation of Coating Compositions 1 to 6 for First Base Coating The components shown in Table 2 were mixed and uniformly dispersed. Dimethylaminoethanol was then added to the dispersion so that the pH was 8.1. The dispersion was then diluted with deionized water to prepare first base coating coating compositions 1 to 6 having the resin solid content concentrations shown in Table 2.

[0110] Preparation of Coating Compositions 1 to 3 for Second Base Coating The components shown in Table 2 were mixed and uniformly dispersed. Dimethylaminoethanol was then added to the dispersion so that the pH was 8.1. The dispersion was then diluted with deionized water to prepare coating compositions 1 to 3 for second base coating film having the resin solid content concentrations shown in Table 2.

[0111] The following coated plate was prepared as a substrate intended for a vehicle body: a zinc phosphate-treated dull steel plate 0.8 mm thick, 30 cm long and 40 cm wide was electrocoated with the electrodeposition paint composition so that the dry film thickness was 20 μm, and the plate was baked at 160° C. for 30 minutes to prepare a coated plate.

[0112] Example 1 The coating composition 1 for a white coating film was applied onto the coated plate using a spray gun, and the plate was baked at 140°C for 30 minutes to form a white coating film. Next, the coating composition 1 for a first base coating film was applied using a spray gun, and the plate was left to set (stand) for 4 minutes, and preheated at 80°C for 5 minutes. Next, the coating composition for a second base coating film was applied using a spray gun, and the plate was left to set for 4 minutes, and preheated at 80°C for 5 minutes. Next, the coated plate (hereinafter referred to as "coated plate") was allowed to cool to room temperature, and the coating composition for a clear coating film was applied using a spray gun, and the plate was left to set for 7 minutes. Next, the coated plate was baked at 140°C for 30 minutes to obtain a coated plate having a red multi-layer coating film.

[0113] Example 2 4、6~ 7 The same as Example 1, except that the first base coating composition 1 was changed to that shown in Table 3. A multi-layer coating film was formed in the same manner to obtain a coated plate having a red multi-layer coating film.

[0114] Comparative Example 1 A multilayer coating film was formed in the same manner as in Example 1, except that the thickness of the white coating film was changed to 20 μm, the paint composition for the first base coating film was not used (a first base coating film was not formed), and the paint composition 1 for the second base coating film was replaced with paint composition 2 for the second base coating film, and a coated plate having a multilayer coating film was obtained.

[0115] Comparative Example 2 Except for replacing the white-based coating film coating composition 1 with the white-based coating film coating composition 2 and replacing the second base coating film coating composition 2 with the second base coating film coating composition 3, a multilayer coating film was formed in the same manner as in Comparative Example 1, and a coated plate having a multilayer coating film was obtained.

[0116] Using a multi-angle spectrophotometer, the L of a white coating was measured as shown in Figure 3. * value and L of multi-layer coating * Value, a * Value, b * Value and C * The values ​​were measured under the following conditions: room temperature measurement: about 25° C., three measurements were taken, and the average value of the three measurements was calculated. The measurement results are also shown in Table 4.

[0117] Using a multi-angle spectrophotometer, the spectral reflectance of the multi-layer coating film was measured under the following conditions, as shown in Figure 3: Room temperature measurement: Approximately 25°C, 3 measurements were taken at 10 nm intervals in the measurement wavelength range of 400 to 700 nm, and the average value of the 3 measurements was calculated. The obtained spectral reflectance was multiplied by the photopic spectral luminous efficiency in Appendix 8 above to obtain the value SS. The results are also shown in Table 4.

[0118] [Table 2]

[0119] [Table 3]

[0120] [Table 4]

[0121] According to the present invention, it is possible to provide a reddish multi-layer coating film having high brightness and high chroma. According to the present invention, it is possible to provide a vehicle having a reddish coating film having high brightness and high chroma. [Industrial Applicability]

[0122] According to the present invention, a reddish multi-layer coating film having high brightness and high chroma can be provided. According to the present invention, a vehicle having a reddish coating film having high brightness and high chroma can be provided. [Explanation of symbols]

[0123] 1: Red multi-layer coating 10: White paint film 20: First base coat 30: Second base coat 40: Clear coating 50:Metal deposition layer

Claims

1. In order, L * A white coating film having a value of 88; a first base coat having a hue of 1YR to 10Y on the Munsell Color System; a second base coat having a hue of 1R to 10R on the Munsell Color System; A red-based multi-layer coating film having a clear coating film, A reddish multilayer coating film, in which a value SS obtained by multiplying the spectral reflectance of the reddish multilayer coating film by the photopic spectral luminous efficiency is 3.0 to 4.7% at a wavelength of 580 nm, and has a maximum value of 16.3 to 33.0% at wavelengths of 590 nm to 650 nm on the curve (wherein the spectral reflectance is the spectral reflectance of light received at a receiving angle of 45° with respect to light irradiated at an incident angle of 45° with respect to the normal to the reddish multilayer coating film on the clear coating film side of the reddish multilayer coating film).

2. The red-based multilayer coating film according to claim 1, which has a maximum value within a range of 1.5 to 5% at wavelengths of 500 nm to 570 nm of the curve.

3. A vehicle having the red-based multilayer paint film according to claim 1 or 2, wherein the clear paint film side is positioned on the outer side.

Citation Information

Patent Citations

  • Colored clear coat paint system

    JP1985132679A

  • Multilayer-coated base material and method for multilayer coating of base material

    JP1990120369A

  • Coating group having metallic undercoat showing dichrdmic color shift effect

    JP1991028276A

  • Coating composition for determining film thickness and method for producing multilayer coating film

    JP2002080787A

  • Method for forming coating film, and adhesive sheet

    JP2010240596A