Diaphragm for alkaline water electrolysis

The diaphragm for alkaline water electrolysis, featuring a porous membrane with organic polymer resin and inorganic particles, addresses the issue of component shedding and gas mixing, ensuring stable high-purity hydrogen production by maintaining strength and gas barrier properties.

JP7587969B2Active Publication Date: 2024-11-21NIPPON SHOKUBAI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020193567
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-20
Publication Date
2024-11-21
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

Conventional diaphragms for alkaline water electrolysis suffer from deterioration and component shedding, leading to gas mixing, electrolyte contamination, and increased replacement frequency, which compromises the stability and purity of hydrogen production.

Method used

A diaphragm for alkaline water electrolysis comprising a porous membrane with specific void structures, containing organic polymer resin and inorganic particles, designed to maintain strength and gas barrier properties, with controlled mass reduction rates and improved ion permeability.

Benefits of technology

The diaphragm ensures stable production of high-purity hydrogen over a long period by reducing component shedding, maintaining gas barrier properties, and enhancing electrolyte integrity, thus improving the efficiency and durability of the electrolysis process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587969000001
    Figure 0007587969000001
Patent Text Reader

Abstract

To provide an alkaline water electrolysis diaphragm, in which the diaphragm strength is excellent, the gas barrier property is well maintained, and a high-purity hydrogen gas is able to be stably produced for a long period of time.SOLUTION: An alkaline water electrolysis diaphragm includes a porous membrane. The porous membrane includes an organic polymer resin and an inorganic particle. The porous membrane has voids, in which the void rate is 20% or greater in the diaphragm surface layer from the diaphragm surface to 30 μm in depth. The alkaline water electrolysis diaphragm is subjected to ultrasonic treatment in water at 30°C, at the frequency 38 kHz and at the output power 100 W for three minutes. As a result, the dropout of diaphragm components causes a decrease of mass, and the rate of decrease is 2% or smaller relative to the diaphragm before the ultrasonic treatment.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a diaphragm for alkaline water electrolysis. More specifically, the present invention relates to a diaphragm for alkaline water electrolysis that has excellent strength, maintains good gas barrier property, and is capable of stably producing high-purity hydrogen gas for a long period of time. [Background technology]

[0002] Water electrolysis (also called "electrolysis") is known as one of the industrial methods for producing hydrogen gas, and is generally carried out by applying an electric current to water to which an electrolyte such as sodium hydroxide or potassium hydroxide has been added to increase the electrical conductivity. For such water electrolysis, an electrolytic cell is used which has an anode chamber and a cathode chamber, each of which is separated by a diaphragm.

[0003] Water electrolysis is carried out by the transfer of electrons (or ions). Therefore, the diaphragm is required to have high ion permeability in order to efficiently carry out the electrolysis reaction. In addition, the diaphragm is required to have gas barrier properties capable of blocking oxygen gas generated in the anode chamber and hydrogen gas generated in the cathode chamber. Furthermore, water electrolysis is carried out using alkaline water with a high concentration of about 30%, at 80 to 100°C, and in some cases under a pressure of 1 MPa, so heat resistance, pressure resistance, alkali resistance, and mechanical strength are also required.

[0004] Various diaphragms for use in water electrolysis have been known to date. For example, Patent Document 1 discloses a diaphragm for alkaline water electrolysis that has a porous polymer membrane containing a polymer resin and inorganic particles, in which the porosity of the porous polymer membrane, the average pore size on the surface, and the ratio of the mode particle size of the inorganic particles to the average pore size are controlled within specific ranges. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2016 / 148302 Summary of the Invention [Problem to be solved by the invention]

[0006] However, conventional diaphragms have a problem in that some of the diaphragm components fall off during use, causing them to deteriorate. When the diaphragm deteriorates, the separator function decreases, oxygen gas and hydrogen gas may mix, or the electrolyte may be contaminated by the fallen material, requiring the separator to be replaced more frequently or the electrolyte to be replaced more frequently. As a result, hydrogen gas cannot be produced stably, and costs are high.

[0007] The present invention has been made in consideration of the above-described current situation, and an object of the present invention is to provide a diaphragm for alkaline water electrolysis that has excellent strength, maintains good gas barrier property, and is capable of stably producing high-purity hydrogen gas for a long period of time. [Means for solving the problem]

[0008] The present inventors have conducted various studies on a diaphragm for alkaline water electrolysis and found that when the diaphragm comprises a porous membrane containing specific components and having a specific void structure, and further has a mass reduction rate due to ultrasonic treatment within a specific range, the strength of the diaphragm is improved, the amount of material falling off from the diaphragm is reduced to suppress contamination of the electrolytic solution, and the gas barrier property is favorably maintained, thereby enabling high-purity hydrogen gas to be produced stably for a long period of time, which has led to the completion of the present invention.

[0009] That is, the present invention relates to a diaphragm for alkaline water electrolysis comprising a porous membrane, the porous membrane comprising an organic polymer resin and inorganic particles, the porous membrane having voids, the void fraction in a diaphragm surface layer up to a depth of 30 µm from the diaphragm surface being 20% ​​or more, and the diaphragm for alkaline water electrolysis exhibits a rate of mass loss due to drop-off of diaphragm components after ultrasonic treatment in water at 30°C at a frequency of 38 kHz and an output of 100 W for 3 minutes being 2% or less relative to the diaphragm before the ultrasonic treatment.

[0010] In the diaphragm for alkaline water electrolysis, the voids preferably have a width of 4 µm or more and a length of 10 µm or more.

[0011] The inorganic particles are preferably in the form of a plate.

[0012] The porous film preferably contains 40 to 80 parts by mass of an organic polymer resin relative to 100 parts by mass of the inorganic particles.

[0013] It is preferable that the diaphragm for alkaline water electrolysis further includes a porous support.

[0014] The diaphragm for alkaline water electrolysis preferably has a layer composed of the porous membrane, and an impregnation layer in which the porous membrane is impregnated into the porous support.

[0015] The fallen matter resulting from the falling off of the membrane components preferably has an average particle size of 2 μm or less.

[0016] The diaphragm for alkaline water electrolysis preferably has an air permeability retention rate of 80% or more after ultrasonic treatment in water at 30° C. at a frequency of 38 kHz and an output of 100 W for 3 minutes. Effect of the Invention

[0017] The diaphragm for alkaline water electrolysis of the present invention has excellent diaphragm strength, is less susceptible to falling off from the diaphragm, is less susceptible to contamination of the electrolytic solution, and maintains good gas barrier properties, enabling stable production of high-purity hydrogen gas for a long period of time. The use of the diaphragm for alkaline water electrolysis of the present invention enables extremely efficient water electrolysis and provides a highly efficient water electrolysis apparatus. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram of an example of a part of a cross section of a diaphragm for alkaline water electrolysis of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention.

[0020] 1. Diaphragms for alkaline water electrolysis The diaphragm for alkaline water electrolysis of the present invention is a diaphragm for alkaline water electrolysis comprising a porous membrane, the porous membrane comprising an organic polymer resin and inorganic particles, and characterized in that the porous membrane has voids, and a void fraction in a diaphragm surface layer to a depth of 30 µm from the diaphragm surface is 20% or more, and the diaphragm for alkaline water electrolysis exhibits a rate of mass loss due to drop-off of diaphragm components after ultrasonic treatment in water at 30°C at a frequency of 38 kHz and an output of 100 W for 3 minutes of 2% or less relative to the diaphragm before the ultrasonic treatment.

[0021] The diaphragm for alkaline water electrolysis of the present invention has the above-mentioned configuration, and therefore has excellent diaphragm strength and maintains good gas barrier property. When the diaphragm strength and gas barrier property are excellent, there is little material falling off the diaphragm, contamination of the electrolyte is suppressed, and the diaphragm function is maintained, so that high-purity hydrogen gas can be produced stably for a long period of time. The reason why the diaphragm for alkaline water electrolysis of the present invention has excellent diaphragm strength and maintains good gas barrier property is thought to be because the diaphragm includes a porous film having voids with an appropriately controlled structure in a surface layer portion of the diaphragm by inorganic particles and an organic polymer resin.

[0022] The diaphragm for alkaline water electrolysis of the present invention includes a porous membrane. The presence of the porous membrane allows the membrane to be impregnated with a large amount of electrolyte and exhibits ion permeability.

[0023] <Porous membrane> The porous membrane contains an organic polymer resin and inorganic particles. (Organic polymer resin) Examples of the organic polymer resin include fluorine-based resins, olefin-based resins, and aromatic hydrocarbon-based resins. Examples of the fluorine-based resin include ethylene-tetrafluoroethylene copolymer, polyvinylidene fluoride, polyvinyl fluoride, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, polytetrafluoroethylene, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, polychlorotrifluoroethylene, tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer, and the like.

[0024] Examples of the olefin resin include polyethylene, polypropylene, polybutene, and polymethylpentene.

[0025] Examples of the aromatic hydrocarbon resin include polyethylene terephthalate, polybutylene terephthalate, polybutylene naphthalate, polystyrene, polysulfone, polyethersulfone, polyphenylene sulfide, polyphenylsulfone, polyarylate, polyetherimide, polyimide, and polyamideimide.

[0026] Among these, the organic polymer resin is preferably an aromatic hydrocarbon resin, which has excellent heat resistance, pressure resistance, and alkali resistance, and is more preferably at least one selected from the group consisting of polysulfone, polyethersulfone, and polyphenylsulfone. The organic polymer resins may be used alone or in combination of two or more kinds.

[0027] When the diaphragm for alkaline water electrolysis does not contain a porous support described below, the content of the organic polymer resin is preferably 28 to 45 mass% relative to 100 mass% of the diaphragm for alkaline water electrolysis. When the content of the organic polymer resin is within the above range, a void structure controlled by the organic polymer resin is easily formed in the diaphragm. The content of the organic polymer resin is more preferably 31 mass% or more, more preferably 42 mass% or less, and even more preferably 38 mass% or less, relative to 100 mass% of the diaphragm for alkaline water electrolysis.

[0028] Furthermore, when the diaphragm for alkaline water electrolysis contains a porous support described below, the content of the organic polymer resin is preferably 10 to 35 mass% relative to 100 mass% of the diaphragm for alkaline water electrolysis. When the content of the organic polymer resin is within the above range, a void structure controlled by the organic polymer resin is easily formed in the diaphragm. The content of the organic polymer resin is more preferably 12 mass% or more, even more preferably 15 mass% or more, even more preferably 17 mass% or more, and more preferably 30 mass% or less, even more preferably 25 mass% or less, even more preferably 23 mass% or less, and particularly preferably 21 mass% or less, relative to 100 mass% of the diaphragm for alkaline water electrolysis.

[0029] (Inorganic particles) Examples of the inorganic particles include metal hydroxides or oxides such as magnesium, zirconium, titanium, zinc, aluminum, and tantalum, sulfates such as calcium, barium, lead, and strontium, nitrides such as titanium, zirconium, and hafnium, and carbides such as titanium, zirconium, and hafnium. The inorganic particles may contain only one type, or two or more types. Among these, metal hydroxides or metal oxides are preferred from the viewpoint of improving ion permeability, magnesium hydroxide, zirconium hydroxide and titanium hydroxide are more preferred, and magnesium hydroxide is even more preferred.

[0030] The inorganic particles may be surface-untreated or surface-treated, for example, by known surface treatments using a silane coupling agent, stearic acid, oleic acid, phosphoric acid ester, or the like.

[0031] The shape of the inorganic particles is not particularly limited and may be any of irregular, granular, flaky, hexagonal or other plate-like shapes, fibrous, etc. Among these, the inorganic particles are preferably plate-like, and more preferably flaky, in that the structure becomes dense and the diaphragm strength can be improved.

[0032] The inorganic particles preferably have an average particle size of 0.05 to 2 μm, since this leads to a dense structure and improves the strength of the membrane.The average particle size of the inorganic particles is more preferably 0.08 μm or more, and even more preferably 0.1 μm or more, more preferably 1.5 μm or less, and even more preferably 1 μm or less. The above-mentioned average particle size is the volume average particle size (D50) obtained by measuring the particle size distribution by the laser diffraction method. Specifically, the average particle size is measured by using a laser diffraction / scattering type particle size distribution measuring device (for example, "Model LA-920" manufactured by Horiba, Ltd.), and the median diameter (D50) in the volume-based particle size distribution is taken as the average particle size. Note that the particles are mixed in ethanol and dispersed by ultrasonic irradiation to be the measurement sample.

[0033] The inorganic particles preferably have an aspect ratio of 2.0 to 8.0. When the aspect ratio is within the above range, a membrane having even more excellent ion permeability and excellent uniformity can be obtained. The aspect ratio is more preferably 2.5 to 7.0, and further preferably 3.0 to 6.0. The aspect ratio means the ratio [(a) / (b)] of the longest diameter (a) to the shortest diameter (b), and can be obtained by observing inorganic particles with a SEM, measuring the ratio [(a) / (b)] of the longest diameter (a) to the shortest diameter (b) of each particle for any 10 particles in the obtained image using analysis software, etc., and calculating the simple average value of these ratios as the aspect ratio of the particle. Usually, it is preferable to use the shortest diameter (b) as the shortest diameter among the diameters that pass through the midpoint of the longest diameter (a) and are perpendicular to the longest diameter. As the above-mentioned longest diameter (a), for example, when the particle has a plate-like shape such as a flaky or hexagonal plate-like shape, the longest diameter of the plate surface of the particle is used, and when the particle has a fibrous shape, the length of the fiber is used. As the shortest diameter (b), for example, when the particle shape is a plate shape such as a thin plate or a hexagonal plate, the thickness of the particle is used, and when the particle shape is a fiber shape, the thickness of the fiber is used. As the thickness of the particle and the thickness of the fiber, it is preferable to use the thickness and the thickness at the midpoint of the longest diameter a, respectively.

[0034] Among these, magnesium hydroxide is preferred as the inorganic particles since it has particularly excellent alkali resistance and durability and can provide a diaphragm for alkaline water electrolysis at relatively low cost. The magnesium hydroxide used in the present invention preferably has a crystallite diameter of 35 nm or more in the direction perpendicular to the (110) plane as measured by X-ray diffraction. When the crystallite diameter in the direction perpendicular to the (110) plane is within the above-mentioned range, the ion permeability and uniformity of the diaphragm are further improved. The crystallite size in the direction perpendicular to the (110) plane is preferably 40 nm or more, more preferably 50 nm or more, further preferably 60 nm or more, and particularly preferably 65 nm or more. The upper limit of the crystallite size in the direction perpendicular to the (110) plane is not particularly limited, but is usually, for example, 400 nm or less, preferably 350 nm or less, and more preferably 300 nm or less.

[0035] The magnesium hydroxide preferably has a crystallite size of 15 nm or more in the direction perpendicular to the (001) plane as measured by X-ray diffraction. The crystallite size in the direction perpendicular to the (001) plane is more preferably 18 nm or more, further preferably 21 nm or more, and particularly preferably 24 nm or more. The upper limit of the crystallite diameter in the direction perpendicular to the (001) plane is not particularly limited, but is usually, for example, 300 nm or less, preferably 250 nm or less, and more preferably 200 nm or less.

[0036] The crystallite size can be determined by measuring the X-ray diffraction pattern of magnesium hydroxide particles using powder X-ray diffraction method, and calculating the crystallite size (crystallite size perpendicular to the lattice plane) using Scherrer's formula from the spread (half-width) of the diffraction line assigned to the target lattice plane.

[0037] As a method for obtaining magnesium hydroxide having the above-mentioned specific crystallite size range, for example, the following method can be mentioned. Magnesium hydroxide is prepared by hydration reaction using an aqueous solution of magnesium salt (magnesium chloride, magnesium nitrate, etc.) or an aqueous dispersion of magnesium oxide obtained by a conventional method as a raw material and adding an alkaline substance (lithium hydroxide, sodium hydroxide, calcium hydroxide, ammonia water, etc.). At this time, by adding an organic acid such as formic acid, acetic acid, propionic acid, etc., a polybasic acid such as nitric acid, sulfuric acid, or a mixture thereof, the solubility of the generated magnesium hydroxide can be adjusted, and by appropriately adjusting the temperature (e.g., 150°C to 270°C) and time (e.g., 30 minutes to 10 hours) of the hydrothermal reaction, particles with different crystallite sizes can be prepared. The more the amount of acid added, the more the crystal growth advances and the larger the crystallite size. Also, the higher the temperature of the hydrothermal reaction and the longer the time, the more the crystal growth advances and the larger the crystallite size.

[0038] In the present invention, general commercial products can be used as inorganic particles. For example, commercially available magnesium hydroxide products that can be used in the present invention include 200-06H manufactured by Kyowa Chemical Industry Co., Ltd., UP650-1 manufactured by Ube Materials Co., Ltd., MAGSTAR #20 manufactured by Tateho Chemical Industry Co., Ltd., and #200 manufactured by Konoshima Chemical Co., Ltd.

[0039] When the diaphragm for alkaline water electrolysis does not contain a porous support described below, the content of the inorganic particles is preferably 55 to 72 mass% relative to 100 mass% of the diaphragm for alkaline water electrolysis. The content of the inorganic particles in this range can make the structure dense and improve the strength of the diaphragm. The content of the inorganic particles is more preferably 69 mass% or less, more preferably 58 mass% or more, and even more preferably 62 mass% or more, relative to 100 mass% of the diaphragm for alkaline water electrolysis.

[0040] Furthermore, when the diaphragm for alkaline water electrolysis contains a porous support described below, the content of the inorganic particles is preferably 20 to 50 mass% relative to 100 mass% of the diaphragm for alkaline water electrolysis. The content of the inorganic particles in this range can make the structure dense and improve the strength of the diaphragm. The content of the inorganic particles is more preferably 24 mass% or more, even more preferably 30 mass% or more, even more preferably 32 mass% or more, particularly preferably 34 mass% or more, and is more preferably 42 mass% or less, even more preferably 39 mass% or less, and even more preferably 37 mass% or less, relative to 100 mass% of the diaphragm for alkaline water electrolysis.

[0041] The porous membrane preferably contains 40 to 80 parts by mass, more preferably 45 to 70 parts by mass, and even more preferably 45 to 60 parts by mass of the organic polymer resin relative to 100 parts by mass of the inorganic particles. When the content ratio of the inorganic particles to the organic polymer resin is within the above-mentioned range, the strength of the diaphragm can be improved, and a diaphragm having a mass reduction rate within a predetermined range can be easily obtained. Furthermore, the diaphragm for alkaline water electrolysis preferably contains 40 to 80 parts by mass, more preferably 45 to 70 parts by mass, and even more preferably 45 to 60 parts by mass of the organic polymer resin relative to 100 parts by mass of the inorganic particles.

[0042] The porous membrane has voids (air spaces), and the void fraction in the diaphragm surface layer up to a depth of 30 µm from the diaphragm surface is 20% or more. The diaphragm for alkaline water electrolysis of the present invention has a porous membrane having such a specific structure, and therefore the diaphragm has excellent strength and can maintain good gas barrier property.

[0043] The void fraction can be measured by the following method. First, a cross section of the diaphragm for alkaline water electrolysis of the present invention, cut perpendicularly to the surface of the diaphragm, is observed with a field emission scanning electron microscope (FE-SEM) to obtain a cross-sectional image. In the obtained cross-sectional image, a region extending from the diaphragm surface to 30 µm in the thickness direction (y direction) and 400 µm in the width direction (x direction) is defined as the measurement region. Then, in the measurement area, image analysis software (e.g., Scion Image, manufactured by Scion) is used to extract the void areas as bright areas, and the ratio (percentage) of the total area of ​​the bright areas (i.e., the total area of ​​each void area) (a) to the area (Z) of the measurement area is calculated, thereby obtaining the void ratio.

[0044] The following will be described in more detail with reference to the drawings. FIG. 1 shows an example of a schematic diagram of a part of the cross section of the diaphragm for alkaline water electrolysis of the present invention. The cross section of the diaphragm in FIG. 1 has a porous membrane 2 on a substrate 1 (e.g., a porous support described later), and an impregnation layer 4 in which the porous membrane 2 has impregnated the substrate 1 therebetween. Voids 3 are present in the porous membrane 2. y represents the surface layer of the diaphragm to a depth of 30 μm from the diaphragm surface. In FIG. 1, the region (x×y) is the measurement region, which is represented by diagonal lines. In FIG. 1, the void portion in the measurement region is extracted as a bright portion. When the area of ​​the measurement region is (Z) and the area of ​​the bright portion is (a), the void fraction (%) is calculated by (a) / (Z)×100.

[0045] The measurement magnification using FE-SEM was 300. For the diaphragm for alkaline water electrolysis, five arbitrary measurement regions were set and measured in the same manner to obtain values, and the average value was defined as the void fraction of the diaphragm.

[0046] The void ratio is preferably 22% or more, more preferably 25% or more, and even more preferably 28% or more, in order to provide a membrane with superior strength and to maintain good gas barrier properties. If the void ratio is too high, through holes are likely to occur in the porous membrane, and the gas barrier properties are likely to deteriorate, so the void ratio is preferably 35% or less, more preferably 32% or less, and even more preferably 30% or less.

[0047] The shape of the void is not particularly limited and may be any shape, but is preferably cylindrical.

[0048] The voids preferably have a width of at least 4 μm and a length of at least 10 μm. When the size of the voids is within the above range, the gas barrier properties can be maintained better. The width of the void is preferably 4 μm or more, more preferably 5 μm or more, and more preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less. The length of the void is preferably 10 μm or more, more preferably 12 μm or more, and more preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less.

[0049] The void width refers to the minor axis length when the void shape is approximated to an ellipse, and the void length refers to the major axis length when the void shape is approximated to an ellipse. The minor axis length and major axis length when the void shape is approximated to an ellipse can be determined by obtaining a cross-sectional observation image of the diaphragm by the above-mentioned FE-SEM observation and using the above-mentioned image analysis software, as in the above-mentioned method for measuring the void fraction, and specifically, can be determined by the method described in the examples below.

[0050] The thickness of the porous membrane is preferably 30 to 100 μm, more preferably 30 to 80 μm, and further preferably 30 to 60 μm.

[0051] <Porous support> The diaphragm for alkaline water electrolysis preferably further comprises a porous support. The inclusion of a porous support can improve the strength of the diaphragm. The porous support is porous and ion permeable, and can serve as a base material (support) of a diaphragm for alkaline water electrolysis. By further including the porous support, the strength of the porous membrane can be improved, the strength of the diaphragm for alkaline water electrolysis can be improved, and damage to the ion permeable membrane during electrolysis, etc. can be suppressed. The porous support is preferably a sheet-like member.

[0052] When the diaphragm for alkaline water electrolysis includes a porous support, the diaphragm for alkaline water electrolysis may be configured such that a layer made of a porous membrane is formed on one or both surfaces of the porous support, or the layer made of the porous membrane may be integrated with part or all of the porous support. The layer made of the porous membrane being integrated with part or all of the porous support means that a layer made of the porous membrane is impregnated into part or all of the porous support.

[0053] In particular, the diaphragm for alkaline water electrolysis preferably has a layer made of the porous membrane and an impregnation layer in which the porous membrane has impregnated into the porous support, in that this further increases the strength of the diaphragm for alkaline water electrolysis. One preferred embodiment of the diaphragm for alkaline water electrolysis having an impregnation layer is an embodiment in which the diaphragm for alkaline water electrolysis has an impregnation layer 4 in which a part of a porous membrane 2 has been impregnated into a substrate 1, which is a porous support, as shown in Fig. 1.

[0054] Examples of the material of the porous support include resins such as polyethylene, polypropylene, polysulfone, polyethersulfone, polyphenylsulfone, polyphenylene sulfide, polyketone, polyimide, polyetherimide, and fluorine-based resins. These may be used alone or in combination of two or more. Among them, in terms of excellent heat resistance and alkali resistance, it is preferable to contain at least one resin selected from the group consisting of polypropylene, polyethylene, and polyphenylene sulfide, and it is more preferable to contain at least one resin selected from the group consisting of polypropylene and polyphenylene sulfide.

[0055] Examples of the form of the porous support include nonwoven fabric, woven fabric, mesh, porous membrane, or a mixture of nonwoven fabric and woven fabric. Preferably, the support is in the form of a nonwoven fabric, woven fabric, or mesh, more preferably, in the form of a nonwoven fabric or mesh, and even more preferably, in the form of a nonwoven fabric.

[0056] The porous support is preferably a nonwoven fabric, a woven fabric, or a mesh containing at least one resin selected from the group consisting of polypropylene, polyethylene, and polyphenylene sulfide.Furthermore, the porous support is preferably a nonwoven fabric or a mesh containing polyphenylene sulfide.

[0057] When the porous support is in the form of a sheet, the thickness of the porous support is not particularly limited as long as the diaphragm for alkaline water electrolysis can exhibit the effects of the present invention; however, the thickness is, for example, preferably 30 to 300 μm, more preferably 50 to 250 μm, and even more preferably 100 to 200 μm.

[0058] The diaphragm for alkaline water electrolysis of the present invention has a mass loss due to falling off of diaphragm components of 2% or less after ultrasonic treatment in water at 30°C for 3 minutes at a frequency of 38 kHz and an output of 100 W. When the membrane is subjected to ultrasonic treatment, some of the membrane components may fall off. If the membrane has low strength, the membrane components are more likely to fall off due to ultrasonic treatment, and the amount of the membrane components that fall off increases. The diaphragm for alkaline water electrolysis of the present invention has high diaphragm strength, and the rate of mass loss due to falling-off of the diaphragm components is 2% or less, preferably 1.5% or less, more preferably 1.2% or less, and even more preferably 1% or less.

[0059] The mass loss rate due to the dropping off of the membrane components can be calculated by the following formula. Mass reduction rate (%) =100-(membrane mass after ultrasonic treatment) / (membrane mass before ultrasonic treatment)×100

[0060] The ultrasonic treatment of the diaphragm is carried out for 3 minutes in water at 30° C. at a frequency of 38 kHz and an output of 100 W. The diaphragm is placed so that the entire diaphragm is immersed in water.

[0061] The fallen matter resulting from the detachment of the diaphragm components preferably has an average particle size of 2 µm or less. The fallen matter refers to part of the diaphragm components that have fallen off due to ultrasonic treatment. The diaphragm for alkaline water electrolysis of the present invention has high diaphragm strength, and therefore the size of the fallen matter after ultrasonic treatment is small. The average particle size of the fallen off material is more preferably 1.5 μm or less, and even more preferably 1 μm or less. The lower limit of the average particle size is not particularly limited, but is usually 0.001 μm or more, and preferably 0.01 μm or more. The above-mentioned average particle size can be obtained by measuring the median diameter (d50) in the number-based particle size distribution in water using a particle size distribution measuring device based on dynamic light scattering (e.g., Otsuka Electronics Co., Ltd., product name FPAR-1000), and the obtained median diameter is defined as the average particle size.

[0062] The fallen material resulting from the falling off of the membrane components preferably contains an organic polymer resin in an amount of 0.1% by mass or more relative to 100% by mass of the fallen material. When the amount of organic polymer resin in the fallen matter is within the above-mentioned range, the diaphragm for alkaline water electrolysis of the present invention has excellent strength. Falling off of the organic polymer resin is likely to affect the strength of the diaphragm for alkaline water electrolysis. Even if the fallen matter contains 0.1 mass% or more of organic polymer resin, a diaphragm having the above-mentioned mass loss rate of 2% or less has few coating film defects, can maintain gas barrier property, and has excellent strength. In other words, the higher the content of organic polymer resin in the fallen matter, the greater the effect of suppressing the mass loss rate of the diaphragm to 2% or less. It is more preferable that the fallen material contains an organic polymer resin in an amount of 1% by mass or more relative to 100% by mass of the fallen material. The fallen material preferably contains an organic polymer resin in an amount of 30% by mass or less, based on 100% by mass of the fallen material. When the amount of organic polymer resin in the fallen material is 30% by mass or less, a large proportion of the organic polymer resin remains in the diaphragm, allowing the inorganic particles to be sufficiently retained in the diaphragm, and increasing the strength of the diaphragm. The above-mentioned fallen material more preferably contains 20% by mass or less of organic polymer resin, further preferably 10% by mass or less, and particularly preferably 6% by mass or less, based on 100% by mass of the fallen material. The organic polymer resin contained in the fallen matter may be the same as the organic polymer resin described above.

[0063] The diaphragm for alkaline water electrolysis preferably has an air permeability of 80 to 500 sec / 100 cc. When the air permeability is in the above range, the gas barrier property is good and mixing of oxygen gas and hydrogen gas can be effectively prevented. The air permeability is preferably 100 to 300 sec / 100 cc, and more preferably 100 to 250 sec / 100 cc.

[0064] The diaphragm for alkaline water electrolysis preferably has an air permeability retention rate of 80% or more before and after ultrasonic treatment in water at 30° C. at a frequency of 38 kHz and an output of 100 W for 3 minutes. When the air permeability retention rate is within the above range, the gas barrier properties can be maintained for a long period of time, and therefore high-purity hydrogen gas can be stably produced. The air permeability retention rate is preferably 85% or more, and more preferably 90% or more, in order to maintain the gas barrier properties for a long period of time. The air permeability retention rate can be calculated by the following formula. Air permeability retention rate (%) = (air permeability of membrane after ultrasonic treatment) / (air permeability of membrane before ultrasonic treatment) x 100 The air permeability can be determined using an Oken air permeability tester (eg, model number EGBO, manufactured by Asahi Seiko Co., Ltd.), and specifically, can be determined by the method described in the examples below.

[0065] The thickness of the diaphragm for alkaline water electrolysis is preferably 150 to 400 μm. If the thickness is less than 150 μm, the diaphragm is likely to wrinkle and may be difficult to handle when assembling the alkaline water electrolysis apparatus. If the thickness is more than 400 μm, the diaphragm has reduced flexibility and is likely to break and crack. The thickness of the diaphragm for alkaline water electrolysis is more preferably 150 to 350 μm, and further preferably 150 to 300 μm. There are no particular limitations on the method for measuring the thickness of the diaphragm for alkaline water electrolysis and it can be measured using a commercially available measuring device, but it is preferably measured using a Digimatic Micrometer (manufactured by Mitutoyo Corporation). It is preferable to measure the thickness at any 10 points and take the average value as the thickness of the diaphragm.

[0066] 2. Manufacturing method of diaphragm for alkaline water electrolysis The method for producing the diaphragm for alkaline water electrolysis of the present invention will be described. The method for producing the diaphragm for alkaline water electrolysis of the present invention is not particularly limited and any known method can be applied. However, the non-solvent induced phase separation method is preferred in that it can efficiently produce a diaphragm having the above-described structure. Specifically, a production method including the following steps (1) to (4) is preferred: (1) A step of preparing a dispersion solution containing an organic polymer resin, inorganic particles, and a solvent. (2) forming a coating film using the dispersion solution; (3) contacting the coating with a non-solvent for the organic polymer resin to solidify the coating and form a porous structure; (4) A step of drying the coating film with the porous structure to obtain a porous film.

[0067] In step (3) of the production method, the solidified coating film preferably contains the non-solvent and a solvent for the second component, and the content of the solvent for the second component is 30 parts by mass or less per 100 parts by mass of the non-solvent. By containing such a solvent, a diaphragm for alkaline water electrolysis can be obtained, which has a porous membrane having the above-mentioned void ratio. Each step in the method for producing a diaphragm for alkaline water electrolysis of the present invention will be described below.

[0068] Process (1) The method for producing a diaphragm for alkaline water electrolysis of the present invention includes a step (1) of preparing a dispersion solution containing an organic polymer resin, inorganic particles, and a solvent. The dispersion solution is a solution for forming the above-mentioned porous membrane.

[0069] The preparation of the dispersion solution is not particularly limited, and can be carried out by mixing an organic polymer resin, inorganic particles, and a solvent. When mixing an organic polymer resin, inorganic particles, and a solvent, the three components may be mixed simultaneously, or a dispersion solution (slurry) in which inorganic particles are dispersed in a solvent may be prepared in advance, and then the dispersion solution and the organic polymer resin may be mixed, or a dispersion solution (slurry) or solution in which inorganic particles and an organic polymer resin are dispersed or dissolved in a solvent may be prepared in advance, and then these dispersion solutions and solutions may be mixed. Among them, a method in which a dispersion solution is prepared by dispersing or dissolving inorganic particles and an organic polymer resin in a solvent, respectively, in order to uniformly mix the organic polymer resin and the inorganic particles and to easily produce a membrane with a smooth surface, is preferred. The organic polymer resin and the inorganic particles are the same as those described above.

[0070] The solvent to be mixed with the organic polymer resin or inorganic particles is preferably one having a property capable of dissolving the organic polymer resin, and examples thereof include organic solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethylsulfoxide. These solvents may be used alone or in combination of two or more. Among them, N-methyl-2-pyrrolidone is preferred because it is excellent in the property of easily dissolving the organic polymer resin and dispersing the inorganic particles. The solvent may contain other solvents in addition to the organic solvents described above.

[0071] The above-mentioned mixing and dispersion method is not particularly limited, and examples thereof include known mixing and dispersion means such as a method using a mixer, a ball mill, a jet mill, a disperser, a sand mill, a roll mill, a pot mill, a paint shaker, etc. In addition, a dispersant, etc. may be appropriately added.

[0072] The concentration of the inorganic particles in the dispersion liquid in which the inorganic particles are dispersed is preferably 30 to 60% by mass, more preferably 40 to 60% by mass, and even more preferably 50 to 60% by mass, in terms of ease of mixing.

[0073] The concentration of the organic polymer resin in the solution in which the organic polymer resin is dissolved is preferably 10 to 50% by mass, more preferably 20 to 40% by mass, and even more preferably 25 to 35% by mass, in terms of ease of mixing.

[0074] The solution containing the organic polymer resin and the dispersion containing the inorganic particles are preferably mixed so that the organic polymer resin is 40 to 80 parts by mass per 100 parts by mass of the inorganic particles. This ratio improves the strength of the diaphragm, and makes it easier to obtain a diaphragm having a mass reduction rate within a specified range. The solution containing the organic polymer resin and the dispersion containing the inorganic particles are preferably mixed so that the organic polymer resin is present in an amount of 40 to 70 parts by mass, and more preferably 40 to 60 parts by mass, per 100 parts by mass of the inorganic particles.

[0075] Process (2) The method for producing a diaphragm for alkaline water electrolysis of the present invention subsequently includes a step (2) of forming a coating film using the dispersion solution obtained in the step (1). A preferred method for forming the coating film is, for example, a method of applying the dispersion onto a substrate, etc. The step (2) preferably includes a step of applying the dispersion onto a porous support.

[0076] The coating method is not particularly limited, and examples thereof include known coating means such as die coating, spin coating, gravure coating, curtain coating, spraying, and methods using an applicator or coater.

[0077] The substrate is not particularly limited as long as it can be coated with the dispersion solution to form a coating film, and examples thereof include films or sheets made of resins such as polytetraethylene terephthalate, polyethylene naphthalate, polypropylene, polyethylene, polyvinyl chloride, polyvinyl acetal, polymethyl methacrylate, polycarbonate, etc., glass plates, etc. Among these, polytetraethylene terephthalate films or sheets are preferred.

[0078] When the diaphragm for alkaline water electrolysis includes a porous support, the dispersion solution may be applied to the porous support. As a coating method, a method of directly coating the dispersion solution on the porous support, similar to the case of using the porous support as a substrate, and a method of immersing the porous support in the dispersion solution may be mentioned. In addition, a method of coating the dispersion solution on the substrate described above, bringing the porous support into contact with the coating, and impregnating the porous support with the dispersion solution may be mentioned. By impregnating the porous support with the dispersion solution, a composite in which the porous membrane and the porous support are integrated can be produced. The porous support is the same as that described above.

[0079] The amount of the dispersion solution to be applied is not particularly limited, and may be appropriately set so that the resulting membrane has a thickness that allows the above-mentioned effects to be exhibited.

[0080] Process (3) The method for producing a diaphragm for alkaline water electrolysis of the present invention includes a step (3) of contacting the coating film formed in the step (2) with a non-solvent for the organic polymer resin to solidify the coating film and form a porous structure. By contacting the coating with a non-solvent for the organic polymer resin, the non-solvent diffuses into the coating, and the organic polymer resin that is not soluble in the non-solvent solidifies. Meanwhile, the solvent in the coating that is soluble in the non-solvent dissolves from the coating. This phase separation causes the organic polymer resin to solidify, forming a porous structure.

[0081] Examples of a method for contacting the coating film with the non-solvent include a method in which the coating film is immersed in the non-solvent (coagulation bath). When the coating film is formed by applying or impregnating a porous support with the dispersion solution for forming a porous membrane, the porous support containing the dispersion solution may be immersed in the non-solvent.

[0082] The non-solvent for the organic polymer resin may be a solvent that does not substantially dissolve the organic polymer resin, where the solubility of the organic polymer resin in 100 g of the solvent at 25° C. is 100 mg or less. Examples of the non-solvent include water such as pure water, distilled water, and ion-exchanged water; lower alcohols such as methanol, ethanol, and propyl alcohol; and mixed solvents thereof, among which water is preferred from the viewpoint of economy and wastewater treatment, and ion-exchanged water is more preferred. In addition, the non-solvent in which the coating film is immersed may contain a small amount of the same solvent as the solvent contained in the coating film, in addition to the above-mentioned components.

[0083] In the step (3), the solidified coating film contains the non-solvent and a second component solvent, and the content of the second component solvent is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less, and is preferably 1 part by mass or more, and more preferably 5 parts by mass or more, relative to 100 parts by mass of the non-solvent. That is, the solvent used in the coagulation bath preferably contains the non-solvent and the solvent for the second component and satisfies the above-mentioned amount ratio. If such a solvent is used, the solvent is contained in the coagulated coating film, and a diaphragm for alkaline water electrolysis having the above-mentioned void fraction can be obtained by the drying step described below. The second component may be a solvent similar to the organic solvent described in step (1) above.

[0084] The temperature condition in the above step (3) is preferably 5 to 30°C, more preferably 10 to 30°C, and even more preferably 15 to 30°C, in order to enable the coating to be solidified uniformly.

[0085] Process (4) The method for producing a diaphragm for alkaline water electrolysis of the present invention further includes a step (4) of drying the coating film that has been made to have a porous structure in the step (3) to obtain a porous membrane. The coating film that has been solidified and made to have a porous structure in the step (3) is dried to remove the non-solvent, thereby obtaining a porous membrane. The drying temperature is preferably from 60 to 100°C, and more preferably from 60 to 80°C. The drying time is preferably from 2 to 60 minutes, more preferably from 2 to 30 minutes, and even more preferably from 5 to 30 minutes.

[0086] The diaphragm for alkaline water electrolysis of the present invention can be easily and efficiently produced by the above-mentioned steps (1) to (4). The method for producing the diaphragm for alkaline water electrolysis may include other known steps, such as a pressing step for making the density of the diaphragm uniform, in addition to the above-mentioned steps (1) to (4).

[0087] 3.Applications The diaphragm for alkaline water electrolysis of the present invention has excellent diaphragm strength and maintains good gas barrier property. Therefore, high-purity hydrogen gas can be produced stably for a long period of time. The diaphragm for alkaline water electrolysis of the present invention also has excellent ion permeability and alkali resistance. The diaphragm for alkaline water electrolysis of the present invention can be suitably used as a diaphragm for water electrolysis using an alkaline aqueous solution as the electrolyte. An electrolysis apparatus and an electrolysis method using the diaphragm for alkaline water electrolysis of the present invention are described below.

[0088] (electrolyzer) The diaphragm for alkaline water electrolysis of the present invention is used as a component of an alkaline water electrolysis apparatus. The alkaline water electrolysis apparatus may, for example, include an anode, a cathode, and the diaphragm for alkaline water electrolysis disposed between the anode and the cathode. More specifically, the alkaline water electrolysis apparatus has an electrolytic cell including an anode chamber in which the anode is present, and a cathode chamber in which the cathode is present, separated by the diaphragm for alkaline water electrolysis.

[0089] The diaphragm for alkaline water electrolysis is preferably installed so as to be in contact with the anode or the cathode, and more preferably so as to be in contact with the anode and the cathode. A smaller distance between the electrodes reduces the electrical resistance and enables the electrolysis efficiency of the electrolysis device to be increased. The diaphragm for alkaline water electrolysis of the present invention can also be suitably used in an electrolysis device of a so-called "zero gap structure" in which the diaphragm is installed so as to be in contact with each electrode so as to minimize the distance between the electrodes.

[0090] The anode and cathode are not particularly limited as long as they are known electrodes, and examples thereof include electrodes containing a known conductive substrate such as copper, lead, nickel, chromium, titanium, gold, platinum, iron, metal compounds thereof, metal oxides, and alloys containing two or more of these metals.

[0091] The electrode may be one in which a catalyst layer is formed on the conductive substrate. The catalyst layer is not particularly limited, and examples thereof include known catalyst layers including metal compounds, metal oxides, and alloys containing nickel, cobalt, palladium, iridium, platinum, or the like.

[0092] The shape of the electrode is not particularly limited and examples of known shapes include a sheet shape, a rod shape, and a rectangular column shape. A sheet shape is preferable since it has a large contact area with the diaphragm for alkaline water electrolysis and can further improve the electrolysis efficiency of the electrolysis device.

[0093] The electrolysis device may further include other commonly used components, such as a gas-liquid separation tank for separating the generated gas from the electrolytic solution, a condenser for stably performing electrolysis, and a mist separator.

[0094] (Electrolysis method) The method for electrolyzing water using an alkaline water electrolysis apparatus comprising the diaphragm for alkaline water electrolysis of the present invention is not particularly limited and can be performed by a known method. For example, water can be electrolyzed by filling an alkaline water electrolysis apparatus comprising the above-mentioned diaphragm for alkaline water electrolysis of the present invention with an electrolytic solution and applying a current in the electrolytic solution.

[0095] The electrolyte is preferably an alkaline aqueous solution in which an electrolyte such as potassium hydroxide or sodium hydroxide is dissolved. The concentration of the electrolyte in the electrolyte is not particularly limited, but is preferably 20 to 40 mass % in order to further increase the electrolysis efficiency.

[0096] The temperature for electrolysis is preferably 50 to 120° C., more preferably 80 to 90° C., in that the ionic conductivity of the electrolyte is further improved and the electrolysis efficiency can be further increased. The current application conditions can be known and are usually 0.2 A / cm. 2 More than 0.3A / cm 2That is all. The higher the applied current density, the more hydrogen gas and oxygen gas can be obtained in a short period of time, and hydrogen can be produced more efficiently. The electrolysis voltage is preferably adjusted to about 2 V, for example within a range not exceeding 1.5 to 2.5 V, so that the current density is high.

[0097] As described above, the diaphragm for alkaline water electrolysis of the present invention has excellent diaphragm strength and maintains good gas barrier property. In addition, it is excellent in ion permeability, gas barrier property and alkali resistance. Use of the diaphragm for alkaline water electrolysis of the present invention enables stable electrolysis over a long period of time and production of hydrogen gas. EXAMPLES

[0098] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0099] In the examples, each evaluation was carried out by the following methods. <How to measure film thickness> The thickness of the diaphragm for alkaline water electrolysis was measured using a Digimatic Micrometer (manufactured by Mitutoyo Corporation). Measurements were taken at 10 random points, and the average value was regarded as the membrane thickness.

[0100] <Measuring voids inside the membrane and calculating the void ratio> A cross-section perpendicular to the surface of the diaphragm for alkaline water electrolysis was observed using an FE-SEM (manufactured by JEOL Ltd., model number: JSM-7600F) to obtain a cross-sectional observation image at a magnification of 300x. For the obtained cross-sectional observation image, a range of 30 μm from the surface of the membrane in the depth direction and a range of approximately 400 μm in the direction perpendicular to the depth direction were set as measurement regions, and image analysis software (Scion Image) was used to extract voids as bright areas and other areas as dark areas, and calculate the width, length, and total area of ​​the voids. The void fraction (a / Z×100(%)) was then calculated from the ratio of the total area (a) to the measured area (Z). The same measurements were made in five random fields of view, and the average values ​​were taken as the void shape and void fraction. For each void observed in the above visual field (measurement area), the short axis length (void width) when the void shape was approximated to an ellipse and the long axis length (void length) when the void shape was approximated to an ellipse were obtained, and the average value based on the number of pieces was obtained and used as the void width and length in the above visual field. The same measurements were made in any five visual fields (measurement areas), and the simple average values ​​of the void width and length were used as the void width and void length in the diaphragm. When a part of a void was outside the measurement area, the outer periphery of the measurement area was regarded as the outer periphery of the void, and only the void part within the measurement area was regarded as the void, and the void shape, width, and length were determined.

[0101] <Ionic conductivity> (Measurement method) Two diaphragm samples were prepared for measurement. Using each membrane sample, a cell formed in the following cell configuration was placed in a thermostatic chamber at 25°C for 30 minutes, and then AC impedance measurement was performed under the following measurement conditions. Using the intercept component (Ra) obtained, the intercept component (Rb) when no measurement sample was placed, and the film thickness obtained by the above film thickness measurement method, the ionic conductivity was measured according to the following formula. The above measurements were carried out on two diaphragm samples, and the average value of the obtained measurements (at two points) was calculated and defined as the ionic conductivity of the diaphragm. [Ionic conductivity (mS / cm)]=[Thickness of film (cm)] / [(Ra-Rb)×1000×1.77]

[0102] (Measurement conditions) Cell configuration Working electrode: Ni plate Counter electrode: Ni plate Electrolyte: 30% by weight potassium hydroxide aqueous solution Sample pretreatment: Immerse in the above electrolyte overnight Effective measurement area: 1.77cm 2 AC impedance measurement conditions Applied voltage: 10mV vs. open circuit voltage Frequency range: 100kHz~100Hz

[0103] <Method of measuring air permeability> The air permeability of the diaphragm for alkaline water electrolysis was measured using an Oken air permeability tester (manufactured by Asahi Seiko Co., Ltd., model number: EGBO). Measurements were taken at three arbitrary points, and the average value was regarded as the air permeability.

[0104] <Evaluation method for ultrasonic testing> For the diaphragm for alkaline water electrolysis, the mass reduction rate, the air permeability retention rate, and the average particle size of the fallen matter were evaluated by the following ultrasonic test.

[0105] (Ultrasonic Testing) The alkaline water electrolysis membrane cut to a size of 5 x 5 cm and 6 cc of ion-exchanged water were placed in a plastic bag with a zipper (Unipack C-4, manufactured by Seisan Nippon Sha), sealed, and left to stand in a water tank for 1 hour using an ultrasonic cleaner (manufactured by SND Corporation, model number: US-103, high-frequency output: 100 w, transmission frequency: 38 kHz) with the water tank temperature adjusted to 30°C, and then irradiated with ultrasonic waves for 3 minutes.

[0106] (Mass loss rate after ultrasonic testing) The weight of each alkaline water electrolysis diaphragm cut to a size of 5 × 5 cm was measured before and after the ultrasonic test using a precision balance (manufactured by A&D Corporation, model number: GH-200), and the mass loss rate was calculated using the following formula. Mass reduction rate (%) =100-(mass after ultrasonic testing (g) / mass before ultrasonic testing (g) x 100)

[0107] (Air permeability retention rate before and after ultrasonic testing) The air permeability of each of the diaphragms for alkaline water electrolysis cut into a size of 5 × 5 cm was measured before and after the ultrasonic test using an Oken air permeability tester (manufactured by Asahi Seiko Co., Ltd., model number: EGBO), and the air permeability maintenance rate was calculated using the following formula. Air permeability maintenance rate (%) = Air permeability after ultrasonic testing / Air permeability before ultrasonic testing × 100

[0108] (Average particle size of fallen particles) The water in the zippered plastic bag in which the fallen particles were suspended after the ultrasonic test was measured for the fallen particles dispersed in the water using a particle size distribution analyzer using the dynamic light scattering method (product name: FPAR-1000, manufactured by Otsuka Electronics Co., Ltd.), and the median diameter (d50) in the particle size distribution based on number was taken as the average particle diameter (μm) of the fallen particles.

[0109] Example 1 (1. Preparation of Magnesium Hydroxide Dispersion) Magnesium hydroxide (average particle size 0.20 μm, plate-like, aspect ratio 6.21) and N-methyl-2-pyrrolidone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed in a mass ratio of 1:1, and a magnesium hydroxide dispersion was prepared by dispersing the mixture at room temperature for 6 hours in a pot mill containing zirconia media balls.

[0110] (2. Preparation of polysulfone resin solution) A polysulfone resin (manufactured by BASF, product number Ultrason S3010) was dissolved in N-methyl-2-pyrrolidone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) at a concentration of 30 mass %.

[0111] (3. Preparation of Coating Fluid) The magnesium hydroxide dispersion and polysulfone resin solution obtained above were weighed out so that the solid content was 42 mass% and the polysulfone resin (PSU) was 50 mass parts per 100 mass parts of magnesium hydroxide, and lithium chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was further added at 3 mass% per 100 mass% of magnesium hydroxide, and mixed at 1000 rpm at room temperature for about 10 minutes in a planetary centrifugal mixer (manufactured by Thinky Corporation, model number Awatori Rentaro ARE-500). The resulting mixture was filtered through a SUS 200 mesh to obtain a coating liquid.

[0112] (4. Formation of coating film) The coating liquid was applied onto a polyphenylene sulfide nonwoven fabric (manufactured by Toray Industries, Torcon Paper #100) so that the thickness of the diaphragm after drying would be 260 μm in total, and the nonwoven fabric was impregnated with the coating liquid. The nonwoven fabric impregnated with the coating liquid was then placed in a water bath at room temperature for 5 minutes to solidify the coating liquid and form a membrane. For the water bath, a liquid in which 100 parts by mass of water as a non-solvent and 5 parts by mass of a solvent for the second component (N-methyl-2-pyrrolidone, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed was used. After the water bath, the obtained membrane was dried in a dryer at 80° C. for 10 minutes to obtain a diaphragm for alkaline water electrolysis consisting of a composite of a nonwoven fabric and a membrane containing magnesium hydroxide and a polysulfone resin.

[0113] The obtained diaphragms for alkaline water electrolysis were evaluated by the methods described above. The membrane thickness was 260 μm. The void shape was 4 μm wide and 15 μm long, with a void ratio of 30%. The ionic conductivity was 155 mS / cm. The air permeability was 120 sec / 100 cc. The mass reduction rate after the ultrasonic test was 1.6%. The air permeability maintenance rate was 90%. The average particle size of the fallen matter was 0.8 μm. The amount of organic polymer resin in the fallen matter was 2% by mass relative to 100% by mass of the fallen matter.

[0114] Example 2 A diaphragm for alkaline water electrolysis was obtained in the same manner as in Example 1, except that in (3. Preparation of coating solution), the polysulfone resin (PSU) was weighed out to be 42 parts by mass per 100 parts by mass of magnesium hydroxide, and in (4. Formation of coating film), coating was performed so that the diaphragm had a total thickness of 270 µm after drying.

[0115] The obtained diaphragms for alkaline water electrolysis were evaluated by the methods described above. The membrane thickness was 270 μm. The void shape was 4.2 μm wide and 15 μm long, with a void ratio of 33%. The ionic conductivity was 172 mS / cm. The air permeability was 100 sec / 100 cc. The mass reduction rate after the ultrasonic test was 1.8%. The air permeability retention rate was 93%. The average particle size of the fallen matter was 1.4 μm. The amount of organic polymer resin in the fallen matter was 3.5% by mass relative to 100% by mass of the fallen matter.

[0116] Example 3 A diaphragm for alkaline water electrolysis was obtained in the same manner as in Example 1, except that in (3. Preparation of coating solution), the magnesium hydroxide dispersion and the polysulfone resin solution were weighed so that the solid content was 36 mass% and the polysulfone resin (PSU) was 70 parts by mass per 100 parts by mass of magnesium hydroxide, and that in (4. Formation of coating film), coating was performed so that the diaphragm had a total thickness of 275 µm after drying.

[0117] The obtained diaphragms for alkaline water electrolysis were evaluated by the methods described above. The membrane thickness was 275 μm. The void shape was 7.5 μm wide and 17 μm long, with a void ratio of 38%. The ionic conductivity was 105 mS / cm. The air permeability was 260 sec / 100 cc. The mass loss rate after the ultrasonic test was 0.8%. The air permeability retention rate was 97%. The average particle size of the fallen matter was 0.3 μm. The amount of organic polymer resin in the fallen matter was 0.5% by mass relative to 100% by mass of the fallen matter.

[0118] Comparative Example 1 (1. Preparation of Magnesium Hydroxide Dispersion) Magnesium hydroxide (average particle size 0.20 μm, plate-like, aspect ratio 6.21) and N-methyl-2-pyrrolidone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed in a mass ratio of 1:1, and a magnesium hydroxide dispersion was prepared by dispersing the mixture at room temperature for 6 hours in a pot mill containing zirconia media balls.

[0119] (2. Preparation of polysulfone resin solution) A polysulfone resin (manufactured by BASF, product number Ultrason S3010) was dissolved in N-methyl-2-pyrrolidone (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) at a concentration of 30 mass %.

[0120] (3. Preparation of Coating Fluid) The magnesium hydroxide dispersion and polysulfone resin solution obtained above were weighed out so that the solid content was 48% by mass and the polysulfone resin (PSU) was 25 parts by mass per 100 parts by mass of magnesium hydroxide, and mixed at room temperature and 1000 rpm for about 10 minutes in a planetary centrifugal mixer (Thinky Corporation, model number Awatori Rentaro ARE-500). The resulting mixture was filtered through a SUS 200 mesh to obtain a coating liquid.

[0121] (4. Formation of coating film) The coating liquid was applied onto a polyphenylene sulfide nonwoven fabric (manufactured by Toray Industries, Torcon Paper #100) so that the thickness of the diaphragm after drying would be 260 μm in total, and the nonwoven fabric was impregnated with the coating liquid. The nonwoven fabric impregnated with the coating liquid was then placed in a water bath at room temperature for 5 minutes to solidify the coating liquid and form a membrane. For the water bath, a liquid in which 100 parts by mass of water as a non-solvent and 35 parts by mass of a solvent for the second component (N-methyl-2-pyrrolidone, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed was used. After the water bath, the obtained membrane was dried in a dryer at 80° C. for 10 minutes to obtain a diaphragm for alkaline water electrolysis consisting of a composite of a nonwoven fabric and a membrane containing magnesium hydroxide and a polysulfone resin.

[0122] The obtained diaphragm for alkaline water electrolysis was evaluated by the method described above in the same manner as in Example 1. The membrane thickness was 260 μm. The void shape was 3.5 μm wide and 8 μm long, and the void ratio was 18%. The ionic conductivity was 130 mS / cm. The air permeability was 180 sec / 100 cc. The mass loss rate after the ultrasonic test was 5%. The air permeability retention rate was 55%. The average particle size of the fallen matter was 3.5 μm. The amount of organic polymer resin in the fallen matter was 8% by mass relative to 100% by mass of the fallen matter.

[0123] From the above, it was confirmed that the diaphragms for alkaline water electrolysis of Examples had smaller mass loss rates after ultrasonic testing and smaller average particle sizes of fallen matter than the diaphragms for alkaline water electrolysis of Comparative Examples, and therefore had excellent diaphragm strength and maintained good gas barrier properties. It is believed that such diaphragms for alkaline water electrolysis of Examples are capable of stably producing high-purity hydrogen gas for a long period of time. [Explanation of symbols]

[0124] 1 Base material 2. Porous membrane 3. Void 4 Impregnated layer

Claims

1. A diaphragm for alkaline water electrolysis comprising a porous membrane, The porous membrane contains an organic polymer resin and inorganic particles, and contains 40 to 80 parts by mass of the organic polymer resin per 100 parts by mass of the inorganic particles; the porous membrane has voids, and the void ratio in the membrane surface layer from the membrane surface to a depth of 30 μm is 20% or more; The voids have a width of 4 μm or more and a length of 10 μm or more; The diaphragm for alkaline water electrolysis has a mass reduction rate due to falling off of diaphragm components after ultrasonic treatment in water at 30° C. at a frequency of 38 kHz and an output of 100 W for 3 minutes of 2% or less relative to the diaphragm before the ultrasonic treatment. A diaphragm for alkaline water electrolysis characterized in that

2. The diaphragm for alkaline water electrolysis according to claim 1, wherein the inorganic particles have a plate-like shape.

3. The diaphragm for alkaline water electrolysis according to claim 1 or 2, further comprising a porous support.

4. The diaphragm for alkaline water electrolysis according to claim 3, comprising: a layer made of the porous membrane; and an impregnation layer in which the porous membrane is impregnated into the porous support.

5. The diaphragm for alkaline water electrolysis according to any one of claims 1 to 4, wherein the fallen off matter produced by the fall-off of the diaphragm components has an average particle size of 2 µm or less.

6. The diaphragm for alkaline water electrolysis according to any one of Claims 1 to 5, wherein the diaphragm for alkaline water electrolysis has an air permeability retention of 80% or more after ultrasonic treatment for 3 minutes in water at 30°C at a frequency of 38 kHz and an output of 100 W.

Citation Information

Patent Citations

  • Diaphragm for alkaline water electrolysis, alkaline water electrolysis apparatus, method for producing hydrogen, and method for producing diaphragm for alkaline water electrolysis

    WO2016148302A1

  • Diaphragm for electrolysis of alkaline water

    WO2020066911A1