Low free 2-mercaptoethanol esters and uses thereof
Low free 2-mercaptoethanol esters address thermal instability and odor problems in PVC stabilizers by significantly reducing residual 2-mercaptoethanol content, enhancing thermal performance and expanding PVC application possibilities.
Patent Information
- Application Number
- JP2021510947
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-24
- Filing Date
- 2019-08-28
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2039-08-28
AI Technical Summary
Existing tin-based stabilizers for halogen-containing polymers like PVC suffer from thermal instability and malodor issues due to residual 2-mercaptoethanol, which are not effectively addressed by current methods, limiting their commercial application in processes like window frames and calendering.
The development of low free 2-mercaptoethanol esters (LFMEE) is achieved through methods such as washing, vacuum stripping, molecular sieving, and membrane separation to reduce residual 2-mercaptoethanol content below 1.0%, enhancing thermal performance and reducing odor.
LFMEE-based stabilizers exhibit improved thermal stability and reduced odor, offering cost advantages over traditional stabilizers and enabling broader applications in PVC production without storage stability issues.
Smart Images

Figure 0007588067000001 
Figure 0007588067000002 
Figure 0007588067000003
Abstract
Description
[Technical field]
[0001] Inventors: ROSS, Kevin, John (a U.S. citizen living in Rockwood, Ontario, CA), NORRIS, Gene, Kelly (a U.S. citizen living in West Chester, OH, US), and DUNLAP, Jeremy (a U.S. citizen living in Walton, KY, US)
[0002] Assignee: PMC Organometallix, Inc., a Delaware company located at 1288 Route 73, Suite 401, Mount Laurel, NJ 08054.
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 62 / 723,943, filed August 28, 2018, and U.S. Provisional Patent Application No. 62 / 878,040, filed July 24, 2019, both of which are incorporated herein by reference. Priority to U.S. Provisional Patent Application No. 62 / 723,943, filed August 28, 2018, and U.S. Provisional Patent Application No. 62 / 878,040, filed July 24, 2019, is hereby claimed.
[0004] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT N / A
[0005] REFERENCE TO "MICROFICHE APPENDIX" N / A
[0006] 1.Technical Field The present invention relates to low free 2-mercaptoethanol esters and their uses. More specifically, the present invention relates to the use of low free 2-mercaptoethanol esters to improve the heat stability of halogen-containing polymers, such as polyvinyl chloride, i.e. PVC. [Background technology]
[0007] 2.Background technology PVC is a thermally unstable polymer at conventional processing temperatures, and many stabilizer systems have been developed in an attempt to address its inherent thermal instability. These technologies include organic, mixed metal, and tin-based stabilizers. Tin-based stabilizers are broadly classified into two main technologies: thioglycolic acid (TGA) or reverse ester (RE). TGA or 2-ethylhexyl methacrylate (EHMA)-based stabilizers have been used successfully since the 1950s, and reverse ester, or RE, stabilizers were introduced in the 1970s. The majority of tin-based PVC heat stabilizers contain both mono- and di-alkyl moieties. This class of stabilizers has also been modified to contain sulfur bridges, which can improve both performance and cost compared to their non-crosslinked counterparts (see U.S. Pat. No. 3,565,931).
[0008] U.S. Patent No. 4,062,881 to Kugele teaches that when free mercaptan is added to tin mercaptan, synergistic stabilizer performance results. A more recent development from U.S. Patent No. 6,846,861 to Herzig et al. teaches that organotin mercaptoalkyl heptonaotes provide improved odor over traditional mercaptoesters such as 2-mercaptoethyl tallate and 2-mercaptoethyl oleate. However, this approach has been slowed by regulatory and commercial reasons, and this approach has not been commercially successful. The use of 2-mercaptoethanol esters (hereinafter referred to as 2ME esters) is generally accepted in PVC applications where odor concerns are not generally found, such as PVC pipe, PVC siding substrates, and PVC fence substrates. In other applications, such as window frames and calendaring, odors generated during downstream processing through blending, extrusion, calendaring, cutting, welding, etc. have been found to be unacceptable. A typical 2ME-based ester intended for the production of a tin-based stabilizer may contain up to 3% by weight of residual or free 2ME. Residual 2ME in the 2ME-based ester may be the result of excess 2ME used to increase the yield of the desired 2ME ester. Similarly, the tin stabilizer produced therefrom may also contain up to 2% by weight of residual 2-ME. Furthermore, additional 2ME can be added to the reverse ester stabilizer at a later time to improve some aspects of the performance of the final 2ME-based ester stabilizer.
[0009] The following U.S. patents are incorporated herein by reference: Kugele, U.S. Pat. No. 4,062,881, and Herzig et al., U.S. Pat. No. 6,846,861. Summary of the Invention
[0010] The present invention is a stabilizer composition for halogen-containing polymers. It has recently been discovered that the odor of 2ME esters, and the resulting tin-based stabilizers, can be dramatically improved by significantly reducing the residual 2-mercaptoethanol from the esters. This effect can be achieved in several ways, including but not limited to washing with water, stripping under heat and vacuum, using additional water to aid in removal under heat and vacuum, molecular sieves, or membrane separation techniques.
[0011] It should also be noted that it is generally recognized that the performance of tin-based stabilizers for halogen-containing polymers is directly related to the tin content of the tin stabilizer. However, the stabilizers derived from 2ME esters provide surprising performance considering that their thermal performance is in line with the higher tin content of the stabilizer and therefore exhibits higher thermal performance efficacy than would be expected based solely on the tin content.
[0012] When used as enhancers of tin-based stabilizers, 2ME-based esters offer cost advantages over other approaches such as epoxidized soybean oil, commonly referred to as ESO. ESO has been used for many years in both flexible and rigid PVC applications as a co-stabilizer to improve the performance of both Ca / Zn and tin-based stabilized systems. ESO has typically been used for its low odor, along with its low cost compared to tin-based stabilizers. Color development as outlined in Table 1 indicates that low free 2-mercaptoethanol esters (LFMEEs) offer similar performance to ESO, but the use of LFMEEs also avoids the storage stability issues typically seen with ESO-based tin stabilizers. TIFF0007588067000001.tif79138
[0013] Test Conditions: PVC compounds were blended according to standard addition order and temperature. Color stability of each compound was evaluated using a Brabender experiment operating at 190 degrees Celsius / 60 rpm with samples taken at 2 minute intervals. The color of each chip was measured compared to a standard white tile and the "L value" reported in Table 2 below. TIFF0007588067000002.tif95138
[0014] The above samples were prepared with ADVASTAB® brand TM-181FS, however similar results are expected with general compounds of similar composition.
[0015] The present invention also offers the advantage of utilizing renewable source fatty acids for the production of 2-mercaptoethyl esters. In contrast, TGA or EHMA based stabilizers are based entirely on petroleum derived intermediates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] All experiments to remove residual 2-mercaptoethanol utilized standard 2-mercaptoethyl ester prepared at PMC Organometallix's commercial facility. The process involves reacting 2-mercaptoethanol with C16-C18 fatty acids using an acid catalyst. As representative methods for the preparation, the following three methods of LFMEE generation are considered in detail:
[0017] Synthesis of standard 2-mercaptoethyl ester: In the following experiment, 2-mercaptoethyl esters were prepared by reacting one equivalent of fatty acid with 1.18 moles of 2-mercaptoethanol in the presence of an acid catalyst and slowly heating to 80-85 degrees Celsius under vacuum. The water of esterification is removed to drive the reaction. The reaction mixture is then washed with water to remove the acid catalyst, the wash water is separated, and the organic layer is then dried under vacuum and heat. Any other acceptable method for preparing standard 2-ME esters may also be used.
[0018] Experiment A: 300 grams of standard 2-mercaptoethyl ester was washed ten times with 100 gram aliquots of water. The washes were performed in a 500 ml separatory funnel and allowed to settle for 30 minutes. The water (bottom phase) was drained and the next aliquot of water was added. After the final wash was completed, the organic phase was dried by applying a vacuum and heating to 110°C.
[0019] Experiment B: 100 grams of standard 2-mercaptoethyl ester was treated with 4 x 2.5 grams of water. The standard 2-mercaptoethyl ester was heated to 70°C and then a 2.5 gram aliquot of water was added. The water was removed by applying a vacuum and heating to 70°C. Once the temperature was achieved, the next 2.5 gram aliquot of water was added. This was repeated with all four water aliquots.
[0020] Run C: 450 grams of standard 2-mercaptoethyl ester was treated with 112 grams of water, then the water was removed under vacuum and heated to 85°C.
[0021] The % 2-mercaptoethanol removed was determined by measuring the % reduction in mercaptosulfur compared to the standard 2-mercaptoethyl ester at the start. TIFF0007588067000003.tif54159
[0022] Experiments A, B, and C provided high levels of free 2-ME removal. The resulting lower free 2-ME esters were used in subsequent studies to determine their effectiveness when incorporated as co-stabilizers and / or as bound species within tin-based stabilizers, but without the traditional malodors resulting from the use of higher free 2-ME esters. Other acceptable methods of removing 2-ME from 2-ME esters may be used to generate the novel LFMEEs of the present invention.
[0023] Stabilizer preparation description ADVASTAB® TM-181FS was prepared using the following process. 1.03 equivalents (eq) of 2-ethylhexyl thioglycolate (2-ethylhexyl thioglycolate) were reacted with an aqueous mixture of monomethyltin trichloride (25% by weight) and dimethyltin dichloride (75% by weight), representing 1.0 equivalent of chloride, using aqueous sodium hydroxide solution to convert the chloride to the mercaptide. The mixture is allowed to settle for 60 minutes to separate the organic and aqueous phases. The bottom organic layer is removed and dried under vacuum and heat. This layer is then filtered to obtain a clear liquid. TIFF0007588067000004.tif171158TIFF0007588067000005.tif66143*ADVASTAB® TM-181FS was provided by PMC Organometallix, Inc. It is the industry standard for many PVC applications. Other suitable stabilizers may be used.
[0024] A preferred stabilizer composition is similar to the general composition of ADVASTAB® TM-181FS, shown below: TIFF0007588067000006.tif25149
[0025] PVC blends using the stabilizer compositions in Table 5 were subjected to two roll mill performance tests and the corresponding color data (L values) are summarized in Table 6. As shown in Table 6, tin stabilizer blends containing up to 25 wt. % LFMEE provided similar performance to the control stabilizer. It should further be noted that the performance of Samples 5 and 6, for example, is achieved at significantly lower tin contents.
[0026] Procedure for the synthesis of stabilizers A and B: During preparation of PVC blends for evaluation, it was observed that the odor of the blends of ADVASTAB® TM-181FS and LFMEE had an odor similar to that of unmodified ADVASTAB® TM-181FS. The odor of ADVASTAB® TM-181FS containing standard 2-mercaptoethyl monoester, i.e., ester containing >2 wt.% free 2-ME, was significantly stronger and more unpleasant. It is expected that similar results would be achieved with conventional stabilizers of similar composition.
[0027] The utility of LFMEE in the synthesis of stabilizers was also investigated. The performance of the LFMEE-based high monooctyltin stabilizer was compared to its 2-EHMA analogue, the commercially available Thermolite 895. In the context of this study, high monooctyltin refers to a tin-based stabilizer with a mono content of greater than 75% with a corresponding di content of less than 25%, and the following examples are based on materials with a mono content of greater than 90%. The LFMEE-based high monooctyltin was prepared in a conventional manner from high monooctyl chloride as detailed in the experimental section. The tin content was directed to the high monooctyltin LFMEE stabilizer containing a tin content that allows comparison of stabilizers within a narrower range of tin weight percentages, which allows different stabilizers to be compared at equal tin content and therefore similar loading levels. This approach reduces or eliminates any effect on performance from different loading levels of the thermal stabilizer. Thus, through the use of high monooctyltin chloride, LFMEE, and sodium sulfide, a sulfurized version of the original high monooctyltin LFMEE was produced by methodology well known to those skilled in the art of stabilizer manufacturing (see Examples for details). This material will be described as high sulfurized monooctyl LFMEE and referred to as Stabilizer A. Initially, these stabilizers were compared on an equal tin basis and evaluated in a two-roll mill stability test. These results are summarized in Table 8.
[0028] Stabilizer preparation description THERMOLITE® 895 and Stabilizer A were prepared using the following process: 1.02 equivalents of mercaptosulfur-containing ester (2-ethylhexylthioglycolate for THERMOLITE® 895 and a combination of LFMEE and disodium sulfide for Stabilizer A) were reacted with a mixture of monooctyltin trichloride (95% by weight) and dioctyltin dichloride (5% by weight), representing 1.0 equivalent of chloride, using aqueous sodium hydroxide solution to convert the chloride to mercaptide. The mixture was allowed to settle for 60 minutes to separate the organic and aqueous phases. The bottom aqueous layer was removed and the remaining organic phase was dried under vacuum and heat. It was then filtered to obtain a clear liquid. The generic equivalent of THERMOLITE® 895 may be used. It is expected that similar results would occur with the generic equivalent of THERMOLITE® 895.
[0029] These stabilizers were evaluated for their effect on PVC processing, specifically, their effect on color development as a function of heat and time. These stabilizers were formulated into the PVC formulations shown in Table 7. TIFF0007588067000007.tif78142
[0030] Generic equivalent trade name components may be used, and it is expected that similar results will occur with generic equivalent trade name components. TIFF0007588067000008.tif74156
[0031] As shown by the L values in Table 8, it can be clearly seen that Stabilizer A provides better initial color, better color development, and term stability versus the conventional EHMA-based stabilizer, control T895.
[0032] To better understand whether the improved performance of the LFMEE-based stabilizer can be extended to lower mono stabilizers, an LFMEE-based stabilizer was prepared from 25% mono / 75% di starting material and compared to the commercial T890F with a similar mono / di ratio. Both T895 and T890F are used in a variety of rigid PVC applications, but find particular use in film and sheet applications. The performance of these materials at equal tin content was compared on a two-roll mill to evaluate color development, time stability, and relative odor and roll tack, and the results are summarized in Tables 10 and 11.
[0033] These stabilizers were evaluated for their effect on PVC processing, specifically, their effect on color development as a function of heat and time. These stabilizers were formulated into the PVC formulations shown in Table 9. TIFF0007588067000009.tif85116
[0034] Generic equivalent trade name components may be used, and it is expected that similar results will occur with generic equivalent trade name components. TIFF0007588067000010.tif78117
[0035] Generic equivalent trade name components may be used, and it is expected that similar results will occur with generic equivalent trade name components.
[0036] As can be seen from Table 10, the performance of Stabilizer B exceeds that of Thermolite® 890F in terms of color development, indicating that the improved performance of LFMEE-based stabilizers can be found across a wide range of mono / di. TIFF0007588067000011.tif35156
[0037] Generic equivalent trade name components may be used, and it is expected that similar results will occur with generic equivalent trade name components.
[0038] At similar loading levels, Stabilizer A provided improved color and duration stability compared to T890F and T895. In addition, it provided improved roll tack and odor during processing. These performance features are critical for films produced by calendaring, a process that requires the peeling of a hot plastic melt from a heat treated roll to produce a sheet or film. The odor improvement may also provide benefits in a production environment, since a large surface area of high temperature is created during the calendaring process.
[0039] Further studies were directed to exploring the relative efficiency of Stabilizer A versus its EHMA-based counterpart T895. Samples were prepared for study using a two-roll mill in stability testing using the PVC formulations listed, used to generate the data in Table 8 above. The results are summarized in Table 12. TIFF0007588067000012.tif96131
[0040] Generic equivalent trade name components may be used, and it is expected that similar results will occur with generic equivalent trade name components.
[0041] Table 12 shows that Stabilizer A at lower loading levels has similar time period stability and provides good color development at its T895. All else being equal, it can be concluded that Stabilizer A will provide a more cost-effective stabilizer solution with improved processability than its EHMA-based analogue.
[0042] The malodor of 2-mercaptoethanol can also be addressed by reacting 2-mercaptoethanol as a ligand with a halogen alkyl tin intermediate. This conversion of 2-mercaptoethanol to a tin-bound mercaptoethanol ligand would reduce volatility and improve odor characteristics. However, this potential route is difficult in that precise control of stoichiometry is required and, if not controlled, can result in undesirable by-products.
[0043] A further alternative to reacting residual 2-mercaptoethanol as well as any other active mercaptan groups is to use the addition of alkyltin oxides which can scavenge the mercaptans through reaction with the mercaptans to form alkyltin mercaptides. Examples of alkyltin oxides include, but are not limited to, dioctyltin oxide, dibutyltin oxide, butylstannoic acid, and octylstannoic acid.
[0044] In the present invention, a low free 2-mercaptoethanol ester (LFMEE) is obtained through the removal of 2-mercaptoethylethanol from standard 2-mercaptoethanol ester, the resulting LFMEE having less than 1.0 wt% residual 2-mercaptoethanol.
[0045] In certain embodiments, the resulting LFMEE may have less than 0.7% by weight residual 2-mercaptoethanol.
[0046] In certain embodiments, the resulting LFMEE has less than 0.5% by weight residual 2-mercaptoethanol.
[0047] The present invention provides a method for using the aforementioned LFMEE to improve the thermal performance of alkyltin thioglycolate stabilizers.
[0048] The present invention provides a method for using the aforementioned LFMEE to improve the thermal performance of alkyltin reverse ester stabilizers.
[0049] The present invention provides a method for using the aforementioned LFMEE to improve the thermal performance of alkyltin mercaptide stabilizers.
[0050] In certain embodiments, the mercaptide can be dodocylmercaptan or a carboxylate.
[0051] In certain embodiments, the mercaptide can be a maleate.
[0052] In certain embodiments of the invention, the stabilizer further comprises a sulfide bridge of an alkyl group ranging from C1 to C8.
[0053] In certain embodiments of the invention, the mono and di components of the alkyltin group are in ratios ranging from 100% di to 100% mono, and all combinations in between.
[0054] In certain embodiments of the present invention, the amount of LFMEE may range from 5% to 75% by weight.
[0055] In certain embodiments of the present invention, the amount of LFMEE may range from 10% to 40% by weight.
[0056] In certain embodiments of the present invention, the resulting stabilizer further comprises Ca / Zn-based enhancers, organic-based stabilizers, and / or other conventional performance enhancers such as BHT, polyols, metal salts, or other co-stabilizers.
[0057] The present invention relates to (a) an alkyltin reverse ester stabilizer; and (b) a composition comprising the LFMEE according to claims 1 to 3, The composition may include those in which the ratio of alkyltin reverse ester stabilizer:LFMEE ranges from 95%:5% to 25%:75% by weight.
[0058] In the present invention, the composition may include a ratio of alkyltin reverse ester stabilizer:LFMEE ranging from 85%:15% to 60%:40% by weight.
[0059] The invention may include a method using LFMEE obtained through removal of 2-mercaptoethylethanol from standard 2-mercaptoethanol esters with 2-EHMA, carboxylate, lauryl mercaptan, 2-mercaptothanol, thioglycolic acid, alkoxide, or sulfide as a ligand, where the resulting LFMEE has less than 1.0 wt% residual 2-mercaptoethanol.
[0060] The present invention may include methods in which the aforementioned LFMEE is used with other ligands in combination with 2-EHMA, carboxylates, lauryl mercaptan, 2-mercaptotanol, thioglycolic acid, alkoxides, or sulfides.
[0061] The present invention provides a method for preparing a PVC stabilizer, comprising the steps of: (a) reacting 1.02 equivalents of LFMEE obtained through removal of 2-mercaptoethylethanol from standard 2-mercaptoethanol ester, and disodium sulfide, with a mixture of monooctyltin trichloride (95% by weight) and dioctyltin dichloride (5% by weight), representing 1.0 equivalent of chloride, using aqueous sodium hydroxide solution, such that the resulting LFMEE has less than 1.0% by weight of residual 2-mercaptoethanol; (b) allowing the mixture to settle; and (c) removing the bottom aqueous layer; (d) drying the remaining organic phase; (e) filtering the dried organic phase.
[0062] The invention may include a method as described above, wherein the drying step (d) is carried out under vacuum.
[0063] The invention may include a method as described above, wherein the drying step (d) is carried out under heat.
[0064] The invention may include a method as described above, wherein the drying step (d) is carried out under vacuum and heat.
[0065] The invention may include the above method, wherein step (e) is carried out until a clear liquid is obtained.
[0066] List of initial letters 2ME 2-Mercaptoethanol EHMA 2-Ethylhexyl Methacrylate ESO Epoxidized Soybean Oil LFMEE Low Free 2-Mercaptoethanol Ester PHR Parts per 100 Resin PVC Polyvinyl chloride RE Reverse Ester RPM Revolutions per minute TGA Thioglycolic Acid
Claims
1. 1. A method of using low free 2-mercaptoethanol ester (LFMEE) to improve the thermal performance of an alkyltin thioglycolate stabilizer, comprising:
1. The method of claim 1, wherein the LFMEE is obtained through removal of 2-mercaptoethanol from standard 2-mercaptoethanol esters formed by reacting 2-mercaptoethanol with C16-C18 fatty acids, and the resulting LFMEE has less than 1.0 wt. % residual 2-mercaptoethanol.
2. 1. A method of using low free 2-mercaptoethanol ester (LFMEE) to improve the thermal performance of an alkyltin reverse ester stabilizer, comprising:
1. The method of claim 1, wherein the LFMEE is obtained through removal of 2-mercaptoethanol from standard 2-mercaptoethanol esters formed by reacting 2-mercaptoethanol with C16-C18 fatty acids, and the resulting LFMEE has less than 1.0 wt. % residual 2-mercaptoethanol.
3. 1. A method of using low free 2-mercaptoethanol ester (LFMEE) to improve the thermal performance of an alkyltin mercaptide stabilizer, comprising:
1. The method of claim 1, wherein the LFMEE is obtained through removal of 2-mercaptoethanol from standard 2-mercaptoethanol esters formed by reacting 2-mercaptoethanol with C16-C18 fatty acids, and the resulting LFMEE has less than 1.0 wt. % residual 2-mercaptoethanol.
4. The method of claim 3 , wherein the mercaptide is dodecyl mercaptan or a carboxylate.
5. The method of claim 4 , wherein the mercaptide is a maleate.
6. The method of claim 3, wherein the stabilizer further comprises a sulfide bridge of an alkyl group ranging from C1 to C8.
7. 4. The method of claim 3, wherein the mono and di components of the alkyltin group are in ratios ranging from 100% di to 100% mono, and all combinations therebetween.
8. A method using low free 2-mercaptoethanol ester (LFMEE) as a ligand with 2-EHMA, carboxylate, lauryl mercaptan, 2-mercaptoethanol, thioglycolic acid, alkoxide, or sulfide, comprising the steps of:
1. The method of claim 1, wherein the LFMEE is obtained through removal of 2-mercaptoethanol from standard 2-mercaptoethanol esters formed by reacting 2-mercaptoethanol with C16-C18 fatty acids, and the resulting LFMEE has less than 1.0 wt. % residual 2-mercaptoethanol.
9. The method of claim 8, wherein the LFMEE is used with other ligands in combination with 2-EHMA, carboxylate, lauryl mercaptan, 2-mercaptoethanol, thioglycolic acid, alkoxide, or sulfide.
10. 1. A method for preparing a PVC stabilizer comprising the steps of: (a1) forming a standard 2-mercaptoethanol ester by reacting 2-mercaptoethanol with a C16-C18 fatty acid; (a2) obtaining low free 2-mercaptoethanol esters (LFMEE) through removal of 2-mercaptoethanol from the standard 2-mercaptoethanol esters, the resulting LFMEE having less than 1.0 wt.% residual 2-mercaptoethanol; (a3) reacting 1.02 equivalents of LFMEE and disodium sulfide obtained in step (a2) with a mixture of monooctyltin trichloride and dioctyltin dichloride, representing 1.0 equivalent of chloride, using aqueous sodium hydroxide solution; (b) allowing the mixture to settle to obtain a bottom aqueous layer and a remaining organic phase; (c) removing the bottom aqueous layer; (d) drying the remaining organic phase; (e) filtering the dried organic phase; A method comprising:
11. The method of claim 10, wherein the drying step (d) is performed under vacuum.
12. The method of claim 10, wherein the drying step (d) is carried out under heat.
13. The method of claim 10, wherein the drying step (d) is carried out under vacuum and heat.
14. 11. The method of claim 10, wherein the filtering step (e) is performed until a clear liquid is obtained.
15. The step (a3) 11. The method according to claim 10, which comprises the step of: (a3') reacting 1.02 equivalents of the LFMEE and disodium sulfide obtained in step (a2) with a mixture of monooctyltin trichloride (95% by weight) and dioctyltin dichloride (5% by weight), representing 1.0 equivalent of chloride, using aqueous sodium hydroxide solution.
Citation Information
Patent Citations
Aliphatic acid mercaptoethanol ester methyl tin heat stabilizer and preparation method thereof
CN102796282A
Surufuidoganjusuzuanteizai
JP1976044149A
Ioganjujukisuzukagobutsuoganjusuru harogenganjujugotaisoseibutsu
JP1976073045A
D*1*55methyltetrahydrochlorophylate and process for preparing same
JP1978124297A
Stabilizer of polymer made of phenol derivative and manufacture of said phenol derivative