Cold-rolled steel sheet with excellent heat resistance and formability and its manufacturing method
Patent Information
- Application Number
- JP2022538241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-14
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-12-14
AI Technical Summary
【0021】 本発明の一実施形態による耐熱性および成形性に優れた冷延鋼板は、高価の合金成分を 多量添加しないため、経済性を有しながらも、耐熱性と成形性に優れている。
Smart Images

Figure 0007588147000004 
Figure 0007588147000001 
Figure 0007588147000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cold-rolled steel sheet having excellent heat resistance and formability, and a method for producing the same. Steel plate for use in environments where it may be exposed to high temperatures and that maintains its original strength even at high temperatures. Steel plate with excellent heat resistance and formability that can be processed into various types of structures and its manufacturing method Regarding. [Background technology]
[0002] Cold-rolled steel sheets are used as structural materials for many purposes, including construction materials, after undergoing various surface treatments. When used as a structural material, if its strength is high, it can withstand a high load for the same cross-sectional area. This has the advantage of reducing the amount of material used. Since the load is determined by the yield strength, it is important to have a high yield strength.
[0003] Methods for increasing the strength of steel sheets include solid solution strengthening, precipitation strengthening, work hardening, and hard phase control. A variety of methods are used. Among them, solid solution strengthening requires the addition of large amounts of alloying elements, Methods for controlling the hard phase include adding a large amount of alloying elements to enhance hardening ability, or quenching after annealing. The disadvantage is that it requires a process, which reduces the economics of manufacturing. In order to form the alloy, it is necessary to add expensive alloying elements, and if excessive precipitates are formed, The drawback is that the ductility is significantly reduced.
[0004] Unlike the above method, in the case of work hardening, no alloying elements are added, and the material is hardened by simple cold rolling. expensive Dislocation Since the strength can be improved by the process, it can be utilized in an economical way. After work hardening, DislocationIts high density significantly reduces moldability, and it is difficult to heat treat it at temperatures above the recrystallization temperature. During processing, the strength is reduced again due to recrystallization, which results in poor heat resistance. When the material is insufficient, it loses strength when exposed to the temperatures used for hot-dip plating of Zn, Al, etc. Therefore, it is difficult to use it as a structural material that requires heat resistance, such as for high-temperature piping. The strength should not decrease significantly when exposed to a relatively high temperature Al plating bath for a certain period of time.
[0005] As a method to overcome these problems, the formation of fine precipitates By increasing the recrystallization temperature and performing recovery annealing at a temperature lower than the recrystallization temperature, There is a method to obtain a drawing rate of 100% by utilizing Ti and Nb, which have a high effect of improving the recrystallization temperature. High strength steel is manufactured by finely precipitating N, NbC, and TiC and then carrying out recovery annealing. However, this technology requires the addition of a large amount of P to ensure high strength. However, P reduces the room temperature toughness, making processing difficult and reducing the uniformity of the structure of the final product. In addition, the amount of Ti and Nb added varies depending on the ratio of Ti and Nb. However, the precipitation behavior of the precipitates is determined by the contents of C and N as well as Ti and Nb. Therefore, it is necessary to control both the C and N contents. Summary of the Invention [Problem to be solved by the invention]
[0006] To provide a cold-rolled steel sheet having excellent heat resistance and formability, and a manufacturing method thereof. Steel plate for use in environments where it may be exposed to heat, and which maintains its original strength even at high temperatures Steel plate with excellent heat resistance and formability that can be processed into various types of structures and manufacturing method thereof Provide the law. [Means for solving the problem]
[0007] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention comprises, in weight percent, C:0 .002~0.01%, Mn: 0.1~1.0%, P: less than 0.01% (excluding 0%). , N: 0.01% or less (excluding 0%), Nb: 0.01 to 0.05%, and Ti: 0 0.01-0.08%, the balance being Fe and unavoidable impurities, and the area fraction of recrystallized grains is 5 area % or less, Dislocation Density is 1x10 15 / m 2 The microstructure is as follows:
[0008] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention contains Si: 0.5% or less. below (except 0%), Al: 0.08% or less (except 0%), and S: 0.01% or less It may further contain one or more of the following (excluding 0%):
[0009] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention has a structure defined by the following formula 1. The precipitation index may be 10 or more. [Formula 1] Precipitation index=[Min([Ti], [N])+4xMin([Nb], [C])+2xM in([Ti]-[N], [C]-[Nb])]x10 4 In this case, in formula 1, [Ti], [N], [Nb], and [C] are expressed as the weight percent of each component. Min(A, B) means the smaller value of A and B, and Min( If A, B) is a negative value, it means 0.
[0010] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention has a yield strength of 450 MPa or more.
[0011] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention has an elongation ratio of 4% or more. It could be.
[0012] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention has an aluminum surface. A zinc or galvanized layer may be formed.
[0013] According to an embodiment of the present invention, a method for producing a cold-rolled steel sheet having excellent heat resistance and formability is provided, comprising the steps of: C: 0.002-0.01%, Mn: 0.1-1.0%, P: less than 0.01% (0% ), N: 0.01% or less (excluding 0%), Nb: 0.01 to 0.05%, and The slabs containing 0.01-0.08% Ti and the balance Fe and unavoidable impurities were processed. a step of heating the slab; a step of hot rolling the slab to produce a hot rolled steel sheet; and rolling the cold-rolled steel sheet at 500°C to produce a cold-rolled steel sheet. S Anneal at a temperature of stages;
[0014] R S is the recrystallization start temperature, which is the temperature at which the area fraction of recrystallized grains is 5 area %.
[0015] In the step of heating the slab, the slab may be heated to 1200° C. or higher.
[0016] In the step of producing the hot-rolled steel sheet, a finish rolling temperature may be Ar3 or higher.
[0017] The Ar3 temperature can be calculated by the following formula: Ar3 temperature=910-(310x[C])-(80x[Mn])-(20x[Cu]) -(15x[Cr])-(55x[Ni])-(80x[Mo])-(0.35x(25 .4-8)) In this case, [C], [Mn], [Cu], [Cr], [Ni], and [Mo] are the weights of each element. Quantity %.
[0018] After the step of producing the hot-rolled steel sheet, the hot-rolled steel sheet is coiled at 550 to 750° C. It may further include:
[0019] The step of producing the cold-rolled steel sheet includes cold rolling the steel sheet at a rolling reduction of 50 to 95%. It can be something like that.
[0020] After the step of manufacturing the cold-rolled steel sheet, the surface of the cold-rolled steel sheet is plated with aluminum or zinc. The method may further include the step of: Effect of the Invention
[0021] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention does not contain expensive alloy components. Since it is not added in large quantities, it is economical and has excellent heat resistance and moldability.
[0022] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention is subjected to heat exposure after processing. This steel sheet is used in environments where it may be damaged, and can maintain its original strength even at high temperatures. It has heat resistance and moldability that allows it to be processed into various types of structures. [Brief description of the drawings]
[0023] [Figure 1] 1 is a photograph showing the results of observation of the microstructure of a cross section of a cold-rolled steel sheet having excellent heat resistance and formability according to developed steel 1 of the present invention, taken under an optical microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Terms such as first, second and third refer to various portions, components, regions, layers and / or sections. These terms are used to describe, but are not limited to, , distinguishing one part, component, region, layer or section from another part, component, region, layer or section Therefore, the first portion, component, region, layer or The section may be a second part, component, region, layer or section without departing from the scope of the present invention. It may be referred to as a “process.”
[0025] The terminology used herein is merely to refer to particular embodiments and is not intended to limit the scope of the present invention. The singular forms used herein are not intended to limit the scope of the invention unless the language clearly contradicts it. Unless a paired meaning is indicated, the plural form is also included. embodied in a particular property, domain, integer, step, operation, element and / or component, and other properties, domains, does not exclude the presence or addition of ranges, integers, steps, operations, elements and / or components. .
[0026] Unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight. do.
[0027] In one embodiment of the present invention, the additional element is added to the remaining This means that it contains iron (Fe), which is a part of the iron.
[0028] All terms, including technical and scientific terms, used herein are intended to be used without limitation, unless otherwise defined. The terms used herein have the meanings commonly understood by those of ordinary skill in the art to which the present invention pertains. Terms defined in commonly used dictionaries have the same meaning as those in the relevant technical literature and the present disclosure. Unless otherwise defined, the terms and conditions of this Agreement shall have a meaning consistent with the terms and conditions set forth herein. It is not always interpreted in a formal sense.
[0029] The following describes the embodiments of the present invention, and is not intended to be limiting of the present invention. The present invention will be described in detail so as to be readily understood by those skilled in the art. The present invention can be implemented in various forms and is not limited to the embodiments described herein.
[0030] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention is useful as various structural materials. The cold-rolled steel sheet used in this application has formability for making shapes and is suitable for the shape of the structure. The strength required to maintain the shape of the container must be sufficient. The strength must not decrease when surface treatment such as plating or coating is performed or when used at high temperatures. stomach.
[0031] If excessive alloying elements are added to obtain the above physical properties, the cost of the material increases, reducing its economic viability. Therefore, it is possible to obtain heat resistance and structural integrity without adding large amounts of expensive alloy elements. A method is needed that can simultaneously ensure morphology.
[0032] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention comprises, in weight percent, C:0 .002~0.01%, Mn: 0.1~1.0%, P: less than 0.01% (excluding 0%). , N: 0.01% or less (excluding 0%), Nb: 0.01 to 0.05%, and Ti: 0 Contains 0.01 to 0.08%, with the balance being Fe and unavoidable impurities.
[0033] Each component will be described in detail below.
[0034] Carbon (C): 0.002~0.01% by weight If the C content is low, it is difficult to use it as a structural material due to its low strength. In order to obtain the above, an additional refining process is required, which reduces productivity. C bonds with Nb and Ti. The strength can be greatly improved by combining and precipitating NbC and The above-mentioned C content is sufficient to obtain the effect of precipitating TiC. If it is too much, it may be difficult to prevent aging caused by solute carbon. Therefore, C should be set to 0.002 More specifically, it may contain 0.002 to 0.0095% by weight. It is possible to do so.
[0035] Manganese (Mn): 0.1 to 1.0% by weight Mn combines with the dissolved S in steel and precipitates as MnS, which reduces red shortness caused by dissolved S. It is an element that prevents hot shortness. Mn can be contained in an amount of 0.1% by weight or more. However, if too much Mn is added, the material may deteriorate. If too little Mn is added, the alloy may harden and lose its softness. The disadvantage is that S does not precipitate sufficiently as MnS, and brittleness increases significantly during hot rolling. More specifically, Mn can be contained in an amount of 0.15 to 1.0% by weight. It may contain 0.35% by weight, and more specifically, 0.18 to 0.22% by weight.
[0036] Phosphorus (P): Less than 0.01% by weight (excluding 0%) Adding P to a certain amount or less is an element that can increase the strength of steel without significantly decreasing its softness. However, if a large amount of P is added, it segregates in the grain system, causing the steel to become excessively hard and reducing the elongation rate. Therefore, it can be limited to less than 0.01% by weight. Also, if a large amount of P is added, P reduces the room temperature toughness, making processing difficult and reducing the uniformity of the structure of the final product. This has the disadvantage of reducing the formability and uniformity of the steel sheet. More specifically, 0. It may be 0.008% by weight or less, and more specifically, it may be 0.006% by weight or less.
[0037] Nitrogen (N): 0.01% by weight or less (excluding 0%) N is an inevitable element contained in steel, and in the present invention, it combines with Ti to promote precipitation hardening. However, because there is too much N, it is not precipitated but exists in solid solution, which can cause softening. Not only does it reduce the strength and ageing resistance, but it also reduces the formability. Taking into account the total content that may be precipitated, the total content may be 0.01% by weight or less. , may be 0.009% by weight or less.
[0038] Titanium (Ti): 0.01 to 0.08% by weight Ti can be effectively used to increase strength by combining with C and N and precipitating. In addition, such precipitates are finely dispersed in the steel and are easily dissipated during annealing after cold rolling. Dislocation oh The recrystallization temperature can be increased by impeding the grain movement. Since an increase in temperature has a direct effect on improving heat resistance, the increase in recrystallization temperature in the present invention It is very important that Ti is added at a concentration of 0.01 wt% or more to obtain a visible effect. When added in an excessively small amount, the amount of precipitates formed is small, and the strength and heat resistance are improved. When added in excess, Ti does not combine with C and N and exists in a solid solution state. Ti in the solid solution state has the effect of improving strength and raising the recrystallization temperature. Therefore, the upper limit may be 0.08% by weight. In particular, the content may be 0.01 to 0.07% by weight.
[0039] Niobium (Nb): 0.01 to 0.05% by weight Nb is a precipitation-strengthening element like Ti, and has relatively high strength and recrystallization properties compared to Ti. The effect of increasing temperature is very large. When added in combination with Ti, the temperature rise rate is very high when the steel is cooled from a high temperature. As a result, TiN, NbC, and TiC are precipitated in that order. The effect of increasing the recrystallization temperature is more pronounced. In the present invention, when the composition system is given, TiN, The content of NbC and TiC was calculated and the relative effect of each precipitate was considered. The precipitation index was developed as an example. The precipitation index will be described later. It was confirmed that the suitability of the component system for obtaining the effect of increasing the temperature and strength could be primarily verified. When Nb is added too little, the formation of precipitates is small, and strength is improved and recrystallization is not possible. The disadvantage is that the effect of increasing the temperature is slight. On the other hand, if Nb is added in excess, the hot rolling Since it excessively increases the load on the alloy, its content can be limited to 0.05% by weight. More specifically, 0.01 to 0.045% by weight, and even more specifically, 0.015 to 0.025 It may be in weight percent.
[0040] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention contains Si: 0.5% or less. below (except 0%), Al: 0.08% or less (except 0%), and S: 0.01% or less It may further contain one or more of the following (excluding 0%):
[0041] Silicon (Si): 0.5% by weight or less (excluding 0%) Silicon is an element that can be used as a decarburizing agent and contributes to improving strength through solid solution strengthening. However, if it is too much, silicon oxide is generated on the surface during annealing, which may cause problems during plating. It may cause defects and deteriorate plating properties. More specifically, it is 0.3% by weight or less. More specifically, the amount may be 0.01 to 0.1% by weight.
[0042] Aluminum (Al): 0.08% by weight or less (excluding 0%) Al is an element with a very strong deoxidizing effect, and reacts with N in the steel to precipitate AlN. This prevents the deterioration of formability caused by solute N. However, when added in large amounts, In this case, the softness may be rapidly decreased. More specifically, the content is 0.01 to 0.05% by weight. obtain.
[0043] Sulfur (S): 0.01% by weight or less (excluding 0%) S is an element that induces red shortness when in solid solution, but it is difficult to completely remove it during the steelmaking process. Therefore, the precipitation of MnS must be induced through the addition of Mn. The precipitation of is undesirable because it hardens the steel. When considering productivity and physical properties, specifically, 0 It may be between 0.002 and 0.009% by weight.
[0044] In addition to the above-mentioned alloy composition, the balance contains Fe and unavoidable impurities. The addition of other compositions is not excluded in the embodiment. The unavoidable impurities are the same as those in ordinary steel manufacturing. During the manufacturing process, it may be unintentionally mixed in from raw materials or the surrounding environment, and it must be excluded. The above-mentioned unavoidable impurities are well understood by ordinary steel manufacturing engineers. For example, Cr: 0.02% by weight or less, Ni: 0.02% by weight or less, Cu: 0.02% by weight and Mo: 0.01 wt % or less.
[0045] The cold-rolled steel sheet having excellent heat resistance and formability according to an embodiment of the present invention has an area distribution of recrystallized grains. The rate is 5% by area or less, Dislocation Density is 1x10 15 / m 2 The microstructure is as follows:
[0046] The area fraction of recrystallized grains means the area fraction of recrystallized grains relative to the total area of the cross section of a cold-rolled steel sheet. The total area of the cross section and the area of the recrystallized grains were determined by optical microstructural observation of the cross section of the steel sheet and E BSD (Electron backscatter diffraction) observation It can be measured from.
[0047] Here, recrystallized grains are grains that have been recrystallized. In the present invention, the term refers to the crystal grains formed by recrystallization through annealing of cold-rolled steel sheets. This refers to crystal grains that have been crushed.
[0048] The portion excluding the crystal grains recrystallized by annealing can be defined as non-recrystallized grains. The distinction between crystal grains and non-recrystallized grains can be made based on their shape and orientation. The grains are elongated in the rolling direction, and the orientation is unclear within the grains. The crystal grains are relatively spherical and have a clear crystal grain orientation.
[0049] on the other hand, Dislocation Density is the amount of material penetrating a unit area. Dislocation It means a number. Dislocation The density was measured by XRD. It can be measured by Dislocation Changes in peak position and width depending on density It can be quantitatively measured.
[0050] The annealing temperature of the cold-rolled steel sheet (described later) (500°C to R S ;where R S is the recrystallization onset temperature, When cold-rolled steel sheets are annealed, this refers to the temperature at which the area fraction of recrystallized grains is 5% by area. In this case, the area fraction of recrystallized grains is 5 area % or less, Dislocation Density is 1x10 15 / m 2 Below If recrystallization proceeds excessively and the area fraction of recrystallized grains is high, the strength of the steel plate will be low. Even if the area fraction of recrystallized grains is 5% or less, Dislocation Excessive density If this is the case, the strength of the steel sheet is high, but the elongation rate is low, which reduces formability.
[0051] The area fraction of the recrystallized grains may more specifically be 4.7 area % or less.
[0052] Dislocation The density is specifically 9x10 14 / m 2 More specifically, 5~10x10 14 / m 2 , and more specifically 5~9x10 14 / m 2 It could be.
[0053] The present invention provides a cold-rolled steel sheet having excellent heat resistance and formability, which is defined by the following formula 1: The precipitation index may be 10 or more. Specifically, the precipitation index may be 10 to 20.
[0054] [Formula 1] Precipitation index=[Min([Ti], [N])+4xMin([Nb], [C])+2xM in([Ti]-[N], [C]-[Nb])]x10 4 In formula 1, [Ti], [N], [Nb], and [C] are calculated by dividing the weight percent of each component by its atomic weight. Min(A,B) means the smaller value of A and B. If is a negative value, it means 0.
[0055] Specifically, [Ti] is (Ti content) / 47.867, [N] is (N content) / 1 4.007, [Nb] is (Nb content) / 92.906, [C] is (C content) / 1 It means 2.011.
[0056] In the present invention, Nb and Ti are added as alloying components. As the steel is cooled, TiN, NbC, and TiC are precipitated in that order. The effect of increasing the temperature and recrystallization temperature is more pronounced. Calculation of the contents of TiN, NbC, and TiC and the shape of precipitates considering the relative effect of each precipitate. We developed a precipitation index that is proportional to the degree of formation of precipitates. The precipitation index can be used to determine the composition for increasing the recrystallization temperature and strength. The suitability of the system can be verified in a primary manner.
[0057] The cold-rolled steel sheet having excellent heat resistance and formability according to one embodiment of the present invention has a yield strength of 450 MPa or more, and the elongation rate may be 4% or more. The material may be a plated steel sheet having a zinc-plated layer or a galvanized layer.
[0058] According to an embodiment of the present invention, a method for producing a cold-rolled steel sheet having excellent heat resistance and formability is provided. a step of hot rolling the slab to produce a hot rolled steel sheet; and manufacturing a cold-rolled steel sheet by subjecting the cold-rolled steel sheet to a 500°C-R S annealing at a temperature of; include.
[0059] Each step will be explained in detail below.
[0060] First, the slab is heated. The alloy composition of the slab has been explained in the cold-rolled steel sheet section above, so a duplicate explanation will be omitted. The alloy composition does not change substantially during the manufacturing process of cold-rolled steel sheets with excellent heat resistance and formability. Therefore, the alloy composition of the cold rolled steel sheet and the alloy composition of the slab are substantially the same.
[0061] The heating temperature of the slab can reach 1200°C or more. Partial redissolution may be required, which may require temperatures of 1200°C or higher. Typically the slab heating temperature can be up to 1250°C or higher.
[0062] The slab is then hot rolled to produce a hot rolled steel sheet. At this time, the finish rolling temperature can be Ar3 or higher.
[0063] The Ar3 temperature can be calculated by the following formula: Ar3 temperature=910-(310x[C])-(80x[Mn])-(20x[Cu]) -(15x[Cr])-(55x[Ni])-(80x[Mo])-(0.35x(25 .4-8)) In this case, [C], [Mn], [Cu], [Cr], [Ni], and [Mo] are the weights of each element. Quantity %.
[0064] This is because the rolling is carried out in the austenite single phase region.
[0065] After the step of producing the hot-rolled steel sheet, the method further includes a step of coiling the hot-rolled steel sheet at 550 to 750 ° C. By coiling at 550℃ or higher, the N remaining in the solid solution can be removed. Since AlN can be additionally precipitated, excellent aging resistance can be ensured. When coiling at temperatures below 550°C, the workability is improved due to the presence of dissolved N that does not precipitate in AlN. If coiling is performed at 750℃ or higher, the crystal grains become coarse and the cold rolling properties deteriorate. This could be a factor in the decline.
[0066] After the step of producing the hot-rolled steel sheet, the hot-rolled steel sheet is cold-rolled to produce a cold-rolled steel sheet. The rolling reduction may be 50 to 95%. The rolling reduction determines the final thickness of the cold-rolled steel sheet. If the reduction rate is less than 50%, it is difficult to secure the final target thickness, and if it is less than 95%, If it exceeds this limit, the rolling load is large and cold rolling may become difficult.
[0067] After the cold-rolled steel sheet is manufactured, the cold-rolled steel sheet is heated at 500℃ to S The annealing is performed at a temperature of . Annealing can mean recovery annealing. S is the recrystallization start temperature, and the surface integral of the recrystallized grains The temperature at which the rate of R is 5% by area is defined as the temperature at which the rate of R is 5% by area. S is the annealing temperature of cold-rolled steel sheet. This can be confirmed by measuring the recrystallized grain fraction according to the recrystallization annealing temperature. The heat resistance accumulated during cold rolling is reduced by recovery annealing at a temperature of Dislocation A significant amount of is removed. This improves the elongation rate. If annealing is performed at an excessively low temperature, Ta Dislocation The softness may decrease due to insufficient removal of the S If annealing at the above temperature, In the case of , the elongation rate is greatly improved by recrystallization, but the strength may drop rapidly. Typically, the annealing temperature may be 600 to 800°C.
[0068] Also, 500℃~RS The annealing time at this temperature may be 10 to 300 seconds. More specifically, The annealing time can be 20 to 60 seconds. If the annealing time is too short, Dislocation The disadvantage is that it is difficult to remove However, if the annealing time is too long, the recrystallization rate increases, resulting in softening.
[0069] Meanwhile, the annealing process can be a batch annealing or a continuous annealing process.
[0070] After the annealing, the shape can be corrected by performing correction rolling of 2% or less. It is possible to achieve the desired physical properties without correction rolling. EXAMPLES
[0071] The present invention will be described in more detail with reference to the following examples. However, these examples are merely illustrative and are not intended to be limiting. The above is merely for illustrative purposes and is not intended to limit the scope of the present invention.
[0072] Steel having the composition shown in Table 1 below was manufactured, and the components are shown as actual values. Steel slabs having the composition shown in Table 1 are reheated at 1250°C and hot rolled at 900°C or higher. The wire was then coiled at 650°C and cold rolled at a reduction ratio of 70%.
[0073] [Table 1]
[0074] For the cold-rolled steel sheets manufactured, R S (Recrystallization start temperature) was measured. The recrystallization start temperature is determined as the temperature at which the area fraction of recrystallized grains is 5% by area. The annealing temperature was set taking these factors into consideration, and annealing was carried out to produce annealed steel sheets. It can be seen that there is a difference in the recrystallization onset temperature.
[0075] [Table 2]
[0076] The precipitation index, recrystallization area fraction, Dislocation density, yield strength, The elongation rate, aging property and heat resistance were calculated and measured, and are shown in Table 3 below.
[0077] The precipitation index was calculated according to the following formula 1.
[0078] [Formula 1] Precipitation index=[Min([Ti], [N])+4xMin([Nb], [C])+2xM in([Ti]-[N], [C]-[Nb])]x10 4
[0079] In formula 1, [Ti], [N], [Nb], and [C] are calculated by dividing the weight percent of each component by its atomic weight. Min(A,B) means the smaller value of A and B. When it was a negative value, it was calculated as 0.
[0080] Specifically, [Ti] is (Ti content) / 47.867, [N] is (N content) / 1 4.007, [Nb] is (Nb content) / 92.906, [C] is (C content) / 1 Calculated at 2.011.
[0081] After annealing, the area fraction of recrystallized grains was measured from the optical microstructure observation of the cross section of the steel sheet. FIG. 1 is a photograph showing the observation result of the optical microstructure of an embodiment of the present invention. The recrystallized area was calculated.
[0082] DislocationThe density is measured through XRD (X-ray Diffraction). The change was measured from the change in the width of the peak.
[0083] The yield strength and elongation were measured through a room temperature tensile test, and the plate specimens were tensile tested in the rolling direction. The results were tested and measured.
[0084] To confirm the soundness against aging, the specimen was kept at 100℃ for 1 hour and the yield strength was 30MPa. If the value increases below this level, it is displayed as good, and if the value increases too much, it is displayed as bad.
[0085] Heat resistance is considered good if it has a yield strength of 500 MPa or more after being maintained at 650°C for 10 minutes. If it was less than this it was marked as poor.
[0086] [Table 3]
[0087] The developed steels 1 to 10 in Table 3 have a precipitation index of 10 or more, and the cold-rolled steel sheets as shown in Table 2 500℃~R S When annealed at a temperature of 0.5°C, the area fraction of recrystallized grains is 5% or less. Although the grain area fraction is low and the yield strength is high at 500 MPa, Dislocation Density is 1.0 X10 15 / m 2 The elongation rate is less than 4% and the strength and workability as a structural material are ensured at the same time. In addition, it has good aging and heat resistance, and satisfies all the characteristics required for a high-strength heat-resistant material.
[0088] Comparative steel 1 has the same composition as developed steel 1, but the annealing temperature is very low at less than 500°C. As a result, no recrystallization occurred at all when the area fraction of recrystallized grains was 0%, Dislocation Density 14 .2X10 14 / m 2 The yield strength is very high at over 650MPa, but the elongation rate is 2 %, making it very difficult to process.
[0089] The comparative steels 2 and 3 have the same composition as the developed steel 1, but the annealing temperature is 680°C or higher. The surface area fraction of recrystallized grains was 10% or more. Dislocation Density is 3X10 14 / m 2 The elongation rate is higher than 10%, but the yield strength is 4 The strength is too low (less than 50 MPa) and is insufficient for use as a structural material.
[0090] Comparative steel 4 has a very low C content of 0.0011%. The carbon content that can be precipitated is low, so the precipitation index is very low at 6.4, and the recrystallization start temperature is 610 As a result, when annealing is performed below the recrystallization temperature, the yield strength and elongation immediately after manufacturing are The optimum level is ensured, but the yield strength is reduced due to recrystallization during heat treatment at 650°C. It dropped significantly and had poor heat resistance.
[0091] On the other hand, comparative steel 5 has a high C content, a high precipitation index, a high recrystallization start temperature, and low strength. Although it has good elongation, elongation rate, and heat resistance, the aging property is poor due to the solid solution C that remains without being precipitated. If the aging property is poor, the elongation rate gradually decreases due to aging, making processing difficult. .
[0092] Comparative steel 6 has a very high Mn content of over 1%. The addition of Mn increases strength through solid solution strengthening. The yield strength is high at 600MPa or more, but the elongation rate is low at less than 4%. Excessive addition of Mn should be avoided.
[0093] Comparative steel 7 has a low Mn content. Although other physical properties are satisfactory, hot rolling embrittlement occurs. There was a drawback to this.
[0094] Comparative steels 8 and 9 have a high P content of 0.015% or more. Therefore, it can be confirmed that the effect of increasing the yield strength is observed. Even a small amount of P added has a large effect on strength improvement. However, when added in excess, room temperature brittleness increases and elongation decreases. It was confirmed that when 0.015% or more was added, the elongation rate decreased to less than 4%. Therefore, from the viewpoint of workability, the P content is preferably less than 0.01%.
[0095] Comparative steel 10 contains a large amount of N, exceeding 0.01%. N combines with Ti at high temperatures and However, when there is an excess of N, Ti is relatively insufficient and N remains in a solid solution state. For this reason, comparative steel 9 has the disadvantage of aging. TiN also precipitates. As a precipitate, it contributes to increasing the recrystallization temperature and improving heat resistance, but compared to other precipitates, The effect of N is relatively small, and an increase in the amount of TiN precipitates leads to a decrease in the amount of TiC precipitates. The content preferably does not exceed 0.01%.
[0096] Comparative steel 11 has a very small Nb content of less than 0.01% and a precipitation index of less than 10. Nb precipitates as NbC, reducing the grain size and improving the recrystallization temperature. However, in the case of Comparative Steel 11, the amount of Nb is small and the effect is insignificant. As a result, the recrystallization start temperature is low at 620℃. This indicates that the heat resistance is poor.
[0097] On the other hand, Comparative Steel 12 has an excessively high Nb content and has a low elongation of 3.8%. In addition, excessive load on hot rolling during the process I was able to confirm that it was added.
[0098] Comparative steel 13 has a Ti content of less than 0.01%. As described above, Ti is However, if the amount of TiN and TiC precipitates is small, it may be difficult to improve recrystallization. The effect of this is reduced, and heat resistance is reduced. In addition, N cannot be sufficiently precipitated as TiN. It can be confirmed that N remains in solid solution and aging has occurred.
[0099] The present invention is not limited to the above embodiment and may be manufactured in various different forms. A person having ordinary skill in the art to which the present invention pertains would be able to understand the technical concept of the present invention. It is understood that the invention may be embodied in other specific forms without changing the concept or essential characteristics. Therefore, the above-described embodiments are illustrative in all respects. It should be understood that this is not limiting.
Claims
1. In mass%, C: 0.002 to 0.01%, Mn: 0.1 to 1.0%, P: less than 0.01%. Less than (except 0%), N: 0.01% or less (except 0%), Nb: 0.01-0.05 %, Ti: 0.01-0.08%, Si: 0.5% or less (excluding 0%), Al: 0.0 8% or less (excluding 0%), and S: 0.01% or less (excluding 0%), the balance being F e and unavoidable impurities, The area fraction of recrystallized grains is 5% or less, and the number of dislocations per unit area is defined as the number of dislocations. Density is 1x10 15 / m 2 Cold-rolled steel with excellent heat resistance and formability, having a microstructure of steel plate.
2. The heat resistance and moldability according to claim 1, wherein the precipitation index defined by the following formula 1 is 10 or more. Superior cold rolled steel. [Formula 1] Precipitation index = [Min ([Ti], [N]) + 4xMin ([Nb], [C]) + 2xM in([Ti]-[N]、[C]-[Nb])]x10 4 (In formula 1, [Ti], [N], [Nb], and [C] represent the mass% content of each component in atomic weight. Min(A,B) means the smaller value of A and B, and Min(A,B ) is a negative value, it means 0.
3. The heat-resistant and moldable composite material according to claim 1 or 2, having a yield strength of 450 MPa or more. Cold rolled steel sheet.
4. The heat-resistant and moldable polyester film according to any one of claims 1 to 3, wherein the stretching ratio is 4% or more. Cold rolled steel sheet.
5. The cold rolled steel sheet has an aluminum or zinc plating layer formed on the surface thereof.
13. The cold-rolled steel sheet having excellent heat resistance and formability according to claim 12.
6. In mass%, C: 0.002 to 0.01%, Mn: 0.1 to 1.0%, P: less than 0.01%. Less than (except 0%), N: 0.01% or less (except 0%), Nb: 0.01-0.05 %, Ti: 0.01-0.08%, Si: 0.5% or less (excluding 0%), Al: 0.0 8% or less (excluding 0%), and S: 0.01% or less (excluding 0%), the balance being F heating the slab consisting of e and unavoidable impurities; hot rolling the slab to produce a hot rolled steel sheet; cold rolling the hot rolled steel sheet to produce a cold rolled steel sheet; and The cold-rolled steel sheet is heated to 500°C. S annealing at a temperature of The area fraction of recrystallized grains is 5% or less, and the number of dislocations per unit area is defined as the number of dislocations. Density is 1x10 15 / m 2 Cold-rolled steel sheet with excellent heat resistance and formability and a microstructure that satisfies the following criteria: Manufacturing method. (Here, R S is the recrystallization start temperature, which is the temperature at which the area fraction of recrystallized grains is 5% by area when annealed for 300 seconds.
7. Heating the slab, The cold-rolled slab having excellent heat resistance and formability according to claim 6, wherein the slab is heated to 1200°C or higher. Manufacturing method of steel plate.
8. In the step of producing the hot-rolled steel sheet, The finishing rolling temperature was Ar 3 The heat resistance and moldability excellent polymer composition according to claim 6 or 7, A method for manufacturing cold rolled steel sheet.
9. After the step of producing the hot rolled steel sheet, Any one of claims 6 to 8, further comprising a step of coiling the hot-rolled steel sheet at 550 to 750°C.
3. A method for producing a cold-rolled steel sheet having excellent heat resistance and formability according to claim 1.
10. The step of manufacturing the cold rolled steel sheet comprises: Any one of claims 6 to 9 is used to produce a cold-rolled steel sheet by cold rolling at a rolling reduction of 50 to 95%.
2. A method for producing a cold-rolled steel sheet having excellent heat resistance and formability according to claim 1.
11. After the step of producing the cold rolled steel sheet, The method according to claim 1, further comprising the step of plating the surface of the cold-rolled steel sheet with aluminum or zinc.
11. A method for producing a cold-rolled steel sheet having excellent heat resistance and formability according to any one of claims 6 to 10.
Citation Information
Patent Citations
Steel plate for container and manufacturing method thereof
JP2007520628A
Method for manufacturing steel sheet for can-making
JP2010150571A
Ultra-thin steel sheet and process for production thereof
WO2010134616A1