Welding method for the manufacture of an assembly of at least two metal substrates

A spot welding method with pulsation and controlled current breaks down native oxide layers on hardened steel parts with zinc and silicon coatings, enabling effective welding and strong welds.

JP7588181B2Active Publication Date: 2024-11-21ARCELORMITTAL SA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023092953
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-13
Filing Date
2023-06-06
Publication Date
2024-11-21
Estimated Expiration
2039-09-09

AI Technical Summary

Technical Problem

Existing methods are inadequate for welding hardened parts with recently developed coatings based on aluminum or zinc due to the thickness and hardness of their native oxide layers, which complicates the welding process.

Method used

A spot welding method using an inverter direct current with a specific spot welding cycle that includes pulsation and welding currents, along with controlled welding force, to break down the native oxide and alloyed coatings on hardened steel parts, facilitating effective welding.

Benefits of technology

The method enables welding ranges of over 1 kA with reduced coating spalling, ensuring strong and reliable welds on metal substrates coated with specific zinc, silicon, and optionally magnesium-based coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588181000004
    Figure 0007588181000004
  • Figure 0007588181000005
    Figure 0007588181000005
  • Figure 0007588181000006
    Figure 0007588181000006
Patent Text Reader

Abstract

To provide an easily implemented welding method for manufacturing a hardening component covered with a specific coat with recently developed aluminum or zinc.SOLUTION: This welding method includes application of a spot welding cycle including a welding step of carrying out one pulsation energization having pulsation current (Cp) applied through two metal base materials joined by using a welding electrode connected to a spot welding power source and having welding current (Cw) to the two metal base materials immediately after. A welding force in the spot welding cycle is 50-350 daN, the current Cp is different from the current Cw, and pulsation duration is shorter than welding duration.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an assembly of at least two metal substrates and to this assembly.The invention is particularly well suited for the manufacture of automobiles. [Background technology]

[0002] In view of the weight reduction of vehicles, it is known to use high-strength steel sheets to achieve a lighter body and to improve crash safety. Hardened parts are also used in particular to reduce the weight of the vehicle. In fact, the tensile strength of these steels is a minimum of 1200 MPa and can go up to 2500 MPa. The hardened parts can be coated with an aluminum-based or zinc-based coating that has good corrosion resistance and thermal properties.

[0003] Typically, the manufacturing process for coated and hardened parts includes the following steps: A) providing a steel sheet pre-coated with a metallic coating, which is a conventional coating based on aluminum or zinc; B) Cutting of coated steel sheets to obtain blanks, C) heat treatment of the blank at high temperature to obtain a fully austenitic microstructure in the steel; D) Transfer of the blank to the press tool; E) Thermoforming of the blank to obtain the part; F) Cooling the part obtained in step E) to obtain a microstructure in the steel which is martensite or martensite-bainite or which is made up of at least 75% equiaxed ferrite, 5-20% martensite and an amount of bainite not exceeding 10%.

[0004] This is generally followed by welding two coated and hardened parts or one coated and hardened part to another metal substrate. Welding coated and hardened parts based on aluminum or zinc is very difficult to achieve due to the hard and thick coatings.

[0005] Patent application EP3020499 states: - a pulsation treatment in which an assembly of two or more overlapping steel plates, including at least one high-tensile steel plate, is fixed using a pair of welding electrodes connected to a spot welding power source using an inverter direct current method, and the welding electrodes are pressed against the steel plates while repeatedly energizing and deenergizing the plates; - A continuous current application process in which, after pulsation treatment, the steel plate is pressed with a welding electrode while current is applied continuously for a period longer than the maximum current application time of the pulsation treatment. A method of resistance spot welding is disclosed, comprising:

[0006] However, this method is only for hot stamped steel sheets coated with conventional zinc-based coatings or aluminum-based coatings. In fact, in the examples, the method was tested on 1500 MPa hot stamped steel sheets coated with aluminum, 1500 MPa-class hot stamped steel sheets coated with alloyed electrogalvanized coatings, and 1500 MPa-class hot stamped steel sheets coated with ZnO-skinned Al. Specific aluminum- or zinc-based coatings containing other elements are not included in this patent application.

[0007] Patent application EP3085485 discloses a resistance spot welding method for welding a plurality of steel plates including overlapping high tensile steel plates, in which the conduction system is a pulsation conduction system using an inverter DC welding power supply, and in each of the plurality of current pulses forming the pulsation conduction, the conduction time, the interval between the current pulses defined as the conduction idle time, and the welding current applied by the current pulse are variably controlled.

[0008] However, this method is only for hot stamped steel sheets which contain intermetallic compounds and solid solutions of iron on their surface due to alloying reactions between conventional zinc-based (pure Zn, Zn-Fe, Zn-Ni, Zn-Al, Zn-Mg, Zn-Mg-Al, etc.) or conventional aluminum-based (Al-Si, etc.) coatings and the base steel. These surfaces are formed with oxide layers mainly composed of zinc or aluminum. Furthermore, the surface of a coating mainly composed of intermetallic compounds of iron and aluminum may be formed with a thin film mainly composed of zinc oxide. In the examples, the method was tested on hot stamped steel sheets coated with an alloy of an aluminum coating containing 9% by weight of Si and Fe and very small amounts of ZnO, and on hot stamped steel sheets coated with an alloyed electrogalvanized coating. Usually, the natural oxide layers of these coatings have a thickness between 10 and 100 nm. The deposition of a thin layer of ZnO on the aluminum-based coated hardened parts before austenitization results in alloying of the ZnO and aluminum-based coatings. A very thin layer of ZnO is deposited on the aluminum-based coating so that the native oxide, consisting mainly of aluminum, remains very thin after austenitization, i.e., 10-100 nm, resulting in easy welding. Specific aluminum or zinc-based coatings containing other elements are not covered by this patent application.

[0009] Patent application GB2468011 discloses a method for applying an electric current for resistance welding of an assembly of plates, at least one of which is made of a high tensile material, the method comprising: - a first step of continuously applying a first amperage for a first predetermined period of time that softens the surface of the high tensile material at the joining location; - a second step of switching the current from the first amperage to a second amperage after the first predetermined duration to grow a nugget at the joint location; and - a third step of continuously applying a second amperage for a second predetermined duration. Includes.

[0010] This method is dedicated to high tensile or hot stamped materials. The hot stamped material can be coated with a plating layer. However, the nature of the plating layer is not specified. In addition, in a first step, a low amperage is applied to soften the surface at the joining location, and in a second step, a high amperage is applied to induce nugget growth at the joining location of the high tensile material. Nevertheless, the low amperage in the first step is not sufficient for welding of certain coated hot stamped parts, where the coating contains elements other than zinc or aluminum.

[0011] Recently, new coatings have been developed for hot-formed steel sheets. Patent application WO2017017521 discloses phosphate-treatable hardened parts coated with alloyed coatings containing 0.4-20.0% by weight zinc, 1.0-3.5% by weight silicon, optionally 1.0-4.0% by weight magnesium, with a Zn / Si ratio between 3.2 and 8.0. Patent application WO2017 / 017514 discloses hardened parts coated with alloyed coatings containing 2.0-24.0% by weight zinc, 1.1-7.0% by weight silicon, optionally 1.1-8.0% magnesium, the remainder being aluminum, with an Al / Zn ratio above 2.9 to improve liquid metal embrittlement (LME) resistance. Patent application WO2017 / 017513 discloses sacrificial steel sheets coated with a coating containing 2.0 and 24% by weight zinc, 7.1-12.0% silicon, optionally 1.1-8.0% by weight magnesium, the remainder being aluminum, with an Al / Zn ratio above 2.9, and the coated sacrificially hardened parts obtained after a method of press hardening. These particular coatings have a native oxide layer with a thickness of micrometers. Due to the thickness and hardness of the native oxide layer, these coatings are very difficult to weld.

[0012] Nevertheless, no method has been developed for welding hardened components that have these particular coatings. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] European Patent Application Publication No. 3020499 [Patent Document 2] European Patent Application Publication No. 3085485 [Patent Document 3] GB Patent Application Publication No. 2468011 [Patent Document 4] International Publication No. 2017 / 017521 [Patent Document 5] International Publication No. 2017 / 017514 [Patent Document 6] International Publication No. 2017 / 017513 Summary of the Invention [Problem to be solved by the invention]

[0014] The object of the present invention is therefore to provide an easy to implement welding method for the production of hardened parts coated with recently developed specific coatings based on aluminum or zinc. In particular for production lines, the object of the present invention is to obtain a welding range of 1 kA or more for such specific coated hardened parts. [Means for solving the problem]

[0015] This object is achieved by providing a welding method for the production of an assembly as claimed in claim 1. The welding method can also have the features of claims 2-10.

[0016] Another object is achieved by providing an assembly as claimed in claim 11. Moreover, this assembly can have any of the features as claimed in claims 12-20.

[0017] Finally, another object is achieved by providing a use of an assembly as claimed in claim 21.

[0018] Other features and advantages of the present invention will become apparent from the following detailed description of the invention.

[0019] In order to illustrate the invention, various embodiments and testing non-limiting examples will now be described with particular reference to the following figures. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 shows an embodiment according to the present invention. [Diagram 2] FIG. 2 shows an example of a spot welding cycle according to the present invention. [Diagram 3] FIG. 3 shows an example of a spot welding cycle according to the present invention. [Figure 4] FIG. 4 shows an example of a spot welding cycle according to the present invention. [Diagram 5] FIG. 5 shows an example of a spot welding cycle according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Other features and advantages of the present invention will become apparent from the following detailed description of the invention.

[0022] The term "hardened steel parts" refers to hot-formed or hot-stamped steel sheets having a tensile strength of up to 2500 MPa, more preferably up to 2000 MPa, for example with a tensile strength of at least 500 MPa, advantageously at least 1200 MPa, preferably at least 1500 MPa.

[0023] The present invention comprises the following steps: A. Providing at least two metal substrates, the first of which is a hardened steel component coated with an alloyed coating comprising: An alloyed coating containing zinc, silicon, optionally magnesium, with the remainder being aluminium, directly covered by a native oxide layer of: A native oxide layer containing ZnO and optionally MgO, B. A spot welding cycle for the at least two metal substrates of step A) using a spot welding machine including a welding electrode and a spot welding power source that applies an inverter direct current, the spot welding cycle comprising the following sub-steps: i. One pulsation having a pulsation current (Cp) applied through the at least two metal substrates joined together using a welding electrode connected to a spot welding power source, followed immediately by ii. a welding step having a welding current (Cw) applied to the at least two metal substrates; Applying spot welding cycles including wherein the welding force during the spot welding cycle is between 50 and 350 daN, the current Cp is different from the current Cw, and the pulsation duration is shorter than the welding duration.

[0024] Without wishing to be bound by any theory, it appears that the welding method according to the invention, carried out on two metal substrates, including at least one hardened steel part coated with a specific coating containing zinc, silicon, optionally magnesium, the remainder being aluminum, allows a welding range of more than 1 kA and a reduction in the scattering of the coating at the assembly surface. Indeed, ZnO and optionally MgO appear to be naturally present on the surface of the hardened steel part due to oxidation of the hardened steel by air. It is believed that the pulsation destroys at least a part of the ZnO and optionally MgO oxide layer and / or layer of the alloyed coating present on the coated hardened steel part, opening a path for the welding current. Furthermore, it appears that the method according to the invention, including one pulsation, is easy to carry out on an industrial scale. Finally, it appears that the welding is improved when the welding force is between 50 and 350 daN, since the current is more localized at the electrode center, leading to a better elimination of the alloyed coating and / or oxide layer. However, if the welding force is outside the range of the present invention, i.e., exceeds 350 daN, the current will spread over a larger surface area of ​​the coated hardened part, and there is a risk that a nugget will not form at the interface between at least two metal substrates.

[0025] As shown in FIG. 1, a spot welding machine (not shown) is used, equipped with a welding electrode 1, 1' and a spot welding source 2. In this example, the electrode makes it possible to join two hardened steel parts 3, 3' coated with a coating 4, 4', 4" according to the invention. During welding, a nugget 5 is formed between the two hardened steel parts through diffusion. The nugget is an alloy of the residual coating and the steel parts. It is assumed that as a result of the spot welding cycle according to the invention, at least a part of the coating is removed in the nugget. It is also assumed that at the top of the spot adhesive joint 6, 6', at least a part of the native oxide layer and / or the alloyed coating is absent. Indeed, at least one pulsation destroys the native oxide layer and removes the spot adhesive joint 6, 6'. It appears that the welding between the two coated hardened steel parts is initiated by melting and removing the coating on top of the pot weld joint and within the nugget. This allows current to flow through the two hardened steel parts, which allows for an improved weld. Finally, cooling between the at least one pulsation and the welding step does not appear to be necessary. In fact, cooling between these steps would likely stop the formation of the nugget between the two hardened steel parts, as the steel parts would begin to solidify. Conversely, without cooling, the steel parts would remain liquid and would likely join easily.

[0026] Preferably, in step Bi), the pulsation current (Cp) is between 0.1 and 30 kA, preferably between 0.1 and 20 kA, more preferably between 8.0 and 20 kA and advantageously between 8.0 and 15 kA.

[0027] Advantageously, in step Bi), the pulsation duration is between 5 and 60 ms, preferably between 4 and 30 ms.

[0028] Preferably, in step B.ii), the welding current (Cw) is between 0.1 and 30 kA, preferably between 0.1 and 20 kA, more preferably between 0.1 and 10 and advantageously between 1 and 7.5 kA.

[0029] Advantageously, in step B.ii), the welding duration is between 150 and 500 ms, more preferably between 250 and 400 ms.

[0030] In a preferred embodiment, the current Cp is less than the current Cw.

[0031] In another preferred embodiment, the current Cp exceeds the current Cw. Indeed, without wishing to be bound by any theory, the inventors have found that when Cp exceeds Cw, the weld coverage is further improved.

[0032] Preferably, the welding force during the spot welding cycle is between 100 daN and 250 daN, more preferably between 150 and 250 daN.

[0033] Preferably, the welding frequency is between 500 and 5000 Hz, more preferably between 500 and 3000 Hz, for example between 800 and 1200 Hz.

[0034] Preferably, the welding step B.ii) comprises a plurality of pulses, with at least one pulsation Bi being directly followed by the first pulse of the welding step. In this case, no cooling takes place between the pulsation and the first pulse. The first pulse is followed by one or more pulses, with a pause between each subsequent pulse. Preferably, the pause is between 20 and 80 ms, preferably between 30 and 60 ms.

[0035] The spot welding cycle according to the invention can have different shapes. Figure 2 shows one preferred embodiment in which the spot welding cycle 21 has a rectangular shape with a rectangular pulsation peak 22 and a rectangular welding peak 23. Figure 3 shows another preferred embodiment in which the spot welding cycle 31 has a parabolic shape with a parabolic pulsation peak 32 and a parabolic welding peak 33. Figure 4 shows another preferred embodiment in which the spot welding cycle 41 has a triangular shape with a triangular pulsation peak 42 and a triangular welding peak 43. According to other embodiments, the spot welding cycle has a parabolic and rectangular shape with a parabolic pulsation peak and a rectangular welding peak, or a triangular and rectangular shape with a triangular pulsation peak and a rectangular welding peak.

[0036] FIG. 5 shows one preferred embodiment in which a spot welding cycle includes one pulsation Bi directly followed by the first pulse of the welding step. In this example, the spot welding cycle 51 has a rectangular shape including a rectangular pulsation peak 52 and three rectangular welding peaks 53, 53', 53".

[0037] The present invention also relates to an assembly of at least two metal substrates spot-welded together by at least one spot weld joint, obtainable by the method of the present invention, - a first metal substrate which is a hardened steel part coated with an alloyed coating comprising: An alloyed coating containing zinc, silicon, optionally magnesium, the remainder being aluminium, directly covered by a native oxide layer of A native oxide layer containing ZnO and optionally MgO, - a spot welded joint including a nugget, the top of which is free of at least a portion of a native oxide layer and / or alloyed coating. The present invention relates to an assembly including:

[0038] Without wishing to be bound by any theory, it is believed that when the assembly includes the above-mentioned specific coating on the hardened parts welded using the welding method according to the invention, the welding range is greater than 1 kA. Indeed, although the thickness of the native oxide layer is greater than the prior art coatings, it is believed that the welding method according to the invention destroys the native oxide layer and removes at least a portion of the native oxide layer and / or coating, allowing good weldability of the assembly.

[0039] The alloyed coating on the hardened steel component contains between 0.1 and 40.0% by weight of zinc, more preferably between 0.1 and 20.0% by weight of zinc, advantageously between 5.0 and 14% by weight of zinc, for example between 7.0 and 12.0% by weight.

[0040] Preferably, the alloyed coating on the hardened steel part comprises 0.1 to 20.0% by weight of silicon, more preferably 0.1 to 12.0% by weight of silicon, advantageously 0.1 to 6.0% by weight of silicon, for example 2.0 to 6.0% by weight of silicon.

[0041] Preferably, the alloyed coating on the hardened steel component contains 0.1-20.0% by weight magnesium, 0.1-10.0%, preferably 0.1-4.0% by weight magnesium.

[0042] Optionally, the coating comprises additional elements selected from Sr, Sb, Pb, Ti, Ca, Mn, Sn, La, Ce, Cr, Zr or Bi, the weight content of each additional element being less than 0.3% by weight, and optionally residual elements resulting from the feeding of the ingot or the passage of the steel substrate through the molten bath, including iron, for example in an amount of up to 5% by weight.

[0043] In a preferred embodiment, the second metal substrate is a steel substrate or an aluminum substrate. Preferably, the second steel substrate is a hardened steel component according to the invention.

[0044] In another preferred embodiment, the assembly includes a third metal substrate plate, which is a steel substrate or an aluminum substrate, in which case there are two or more spot weld joints.

[0045] Finally, the invention relates to the use of an assembly according to the invention for the manufacture of a motor vehicle.

[0046] The invention is illustrated in the following test examples which are given for information only and are not limiting. EXAMPLES

[0047] [Example 1: Uniform welding test] Usibor® 1500 steel sheet, Examples 1-18, were hot-dip galvanized with a coating containing 3 wt.% silicon, 2 wt.% magnesium, 12 wt.% zinc, balance aluminum. Usibor® 1500 steel sheet, Example 19, was hot-dip galvanized with a coating containing 3 wt.% silicon, 2 wt.% magnesium, 10 wt.% zinc, balance aluminum. The steel sheets were then press hardened at austenitizing temperatures between 880-950°C for 3-7 minutes.

[0048] For each test example, two identical press-hardened parts were then welded together.

[0049] The welding range was determined according to standard SEP1220-2. The welding test started at 3 kA and was increased by 0.2 kA for every two spot welds. The splash limit was recognized if two consecutive splashes occurred at the same current level. When the splash limit was reached, the welding current was reduced in steps of 0.1 kA until three consecutive weld specimens at the same current level were obtained without rejection. This current level is defined as the upper weld limit Imax of the current range.

[0050] After that, a lower limit Imin was found. The search for Imin was performed using the 4√t (t is the plate thickness) criterion. This criterion defines the minimum allowable diameter value that guarantees the weld quality and strength. For confirmation, five consecutive weld samples were obtained with a weld diameter larger than the minimum weld diameter.

[0051] In examples 1-12 and 17-19, the welding cycle included one pulsation, possibly with pulsation current Cp, and one welding step with welding current Cw defined by Imin and Imax according to standard SEP 1220-2. In examples 13-16, the welding cycle included one pulsation with pulsation current Cp, and three or four welding steps with welding current Cw defined by Imin and Imax according to standard SEP 1220-2, with a temporary stop between each welding step.

[0052] The frequency was 1000 Hz. The obtained Imin, Imax and welding current ranges are shown in Table 1 below.

[0053] [Table 1]

[0054] Examples 5, 6, 11, 12 and 16 were not weldable, i.e. the Imin and Imax criteria defined in standard SEP 1220-2 were not achieved. The examples according to the invention have a weld range of 1 kA or more.

[0055] [Example 2: Non-uniform welding test] Usibor® 1500 steel sheets were hot-dip galvanized with a coating containing 3% by weight silicon, 2% by weight magnesium, 12% by weight zinc, the remainder being aluminum. The steel sheets were then press-hardened for 5 minutes at an austenitizing temperature of 900°C. They were welded with zinc-coated DP600 steel grade (C: 0.14% by weight, Mn: 2.1% by weight, Si: 0.4% by weight). The welding range was determined as in Example 1. The frequency was 1000 Hz. The obtained Imin, Imax and welding current range are given in Table 2 below.

[0056] [Table 2]

[0057] Test Example 22 was not weldable. Test examples according to the invention have a weld range of 1 kA or greater.

[0058] [Example 3: Electrode life test] The electrode life is defined as the final number of welds on the test strip before reaching more than 2 out of 8 welds below the defined minimum weld diameter. The minimum weld diameter was 4.7 mm.

[0059] Two coated hardened steel parts prepared as test example 7 were welded together using a welding method according to the present invention including one pulsation and welding step. The pulsation current was 10 kA for 10 ms. The welding current was Imax as determined in test example 7 of Example 1. The two coated hardened parts were spot welded with the electrodes and the weld diameter was measured for each spot weld. The results are shown in Table 3 below.

[0060] [Table 3]

[0061] In test example 7 according to the invention, the weld diameter was always greater than the minimum weld diameter.

Claims

1. 1. A welding method for manufacturing an assembly, comprising: A. Providing at least two metal substrates (3, 3') including a first metal substrate (3) and a second metal substrate (3') which are hardened steel components coated with an alloyed coating as follows: an aluminium-based alloyed coating (4) comprising 0.1-20.0% by weight zinc, 0.1-15.0% by weight silicon, 0.1-10.0% by weight magnesium, the remainder being aluminium, directly covered by a native oxide layer of: a native oxide layer comprising ZnO and optionally MgO; B. A spot welding cycle (21, 31, 41, 51) for the at least two metal substrates of step A) using a spot welding machine including welding electrodes (1, 1') and a spot welding power source (2) that applies inverter direct current, the spot welding cycle (21, 31, 41, 51) includes the following sub-steps: i. a single pulsation (22, 32, 42, 52) with a pulsation current (Cp) applied through the at least two metal substrates to be joined together using a welding electrode connected to a spot welding power source, where the pulsation current (Cp) is between 0.1 and 30 kA, followed immediately by ii. welding (23, 33, 43, 53) the at least two metal substrates with a welding current (Cw), where the welding current (Cw) is between 0.1 and 30 kA; Applying spot welding cycles including wherein the welding pressure during the spot welding cycle is between 200-350 daN, the pulsation current (Cp) is greater than the welding current (Cw), the pulsation duration is less than the welding duration, the pulsation duration is 5-60 ms, and the welding duration is 150-500 ms; method.

2. The welding method according to claim 1, wherein the welding frequency is 500 to 5000 Hz.

3. 3. The method of claim 2, wherein the welding step B.ii) comprises a plurality of pulses, one of said pulsations B.i being immediately followed by the first pulse of the welding step.

4. The shape of the spot welding cycle (21, 31, 41, 51) is as follows: A rectangular shape including a rectangular pulsation peak (22) and a rectangular welding peak (23) Parabolic, including a parabolic pulsation peak (32) and a parabolic welding peak (33) A triangular shape including a triangular pulsation peak (42) and a triangular weld peak (43) A parabolic and rectangular shape, including a parabolic pulsation peak and a rectangular weld peak; and - Triangular and rectangular shapes with triangular pulsation peaks and rectangular weld peaks The welding method according to any one of claims 1 to 3, wherein the welding temperature is selected from the following:

5. An assembly of at least two metal substrates (3, 3') spot welded together via at least one spot weld joint, obtained according to any one of claims 1 to 4, a first metal substrate (3) which is a hardened steel part coated with an alloyed coating: an aluminium-based alloyed coating (4) comprising 0.1-20.0% by weight zinc, 0.1-15.0% by weight silicon, 0.1-10.0% by weight magnesium, the remainder being aluminium, directly covered by a native oxide layer of: a native oxide layer comprising ZnO and optionally MgO; a second metal substrate (3'), - a spot welded joint including a nugget (5), the upper part (6) of which is free of at least a portion of a native oxide layer and / or alloyed coating. An assembly comprising:

6. 6. The assembly of claim 5, wherein the alloyed coating on the hardened steel component comprises 5.0 to 14 weight percent zinc.

7. 7. The assembly of claim 6, wherein the alloyed coating on the hardened steel component comprises 7.0 to 12.0 weight percent zinc.

8. An assembly according to any one of claims 5 to 7, wherein the alloyed coating on the hardened steel component comprises 0.1 to 6.0% by weight silicon.

9. 9. The assembly of claim 8, wherein the alloyed coating on the hardened steel component comprises 2.0 to 6.0 weight percent silicon.

10. An assembly according to any one of claims 5 to 9, wherein the alloyed coating on the hardened steel component comprises 0.1 to 4.0% by weight magnesium.

11. An assembly according to any one of claims 5 to 10, wherein the second metal substrate (3') is a steel substrate or an aluminium substrate.

12. An assembly according to claim 11, wherein the second metal substrate (3') is a hardened steel part according to any one of claims 5 to 10.

13. An assembly according to any one of claims 5 to 12, wherein the assembly comprises a third metal substrate which is a steel substrate or an aluminium substrate.

14. Use of an assembly according to any one of claims 5 to 13 or obtained according to the method according to any one of claims 1 to 4 for the manufacture of a motor vehicle.

Citation Information

Patent Citations

  • Resistive spot welding method

    EP3020499A1

  • Resistance spot welding method

    EP3085485A1

  • Method for applying current for resistive welding

    GB2468011A

  • Blood sampling tube for blood test

    JP1988015161A

  • Resistance spot welding method for aluminum material and steel material, and weld joint