β-type sialon phosphor and light-emitting device

By controlling the aluminum element ratio at specific depths within the β-sialon phosphor through a two-stage firing process, the brightness and emission efficiency of light-emitting devices are enhanced, addressing the need for improved phosphor performance in LED applications.

JP7588589B2Active Publication Date: 2024-11-22DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021540767
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-20
Filing Date
2020-08-14
Publication Date
2024-11-22
Estimated Expiration
2040-08-14

AI Technical Summary

Technical Problem

Existing β-sialon phosphors and light-emitting devices require further improvements in brightness and heat resistance.

Method used

A β-sialon phosphor with a specific aluminum element ratio at different depths from the surface, optimized through a two-stage firing process and subsequent treatments, is developed to enhance brightness.

Benefits of technology

The optimized β-sialon phosphor exhibits improved brightness and emission efficiency, suitable for use in light-emitting devices such as LEDs and liquid crystal display panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588589000004
    Figure 0007588589000004
  • Figure 0007588589000001
    Figure 0007588589000001
  • Figure 0007588589000002
    Figure 0007588589000002
Patent Text Reader

Abstract

A β-form Sialon fluorescent substance containing europium as a solute and satisfying P8 / P80≤0.9, where P8 [at%] is the content of aluminum element at a depth of 8 nm from a surface of the fluorescent substance and P80 [at%] is the content of aluminum element at a depth of 80 nm from the surface of the fluorescent substance, the contents being obtained by X-ray photoelectron spectroscopy; and a light-emitting device including the β-form Sialon fluorescent substance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a β-sialon phosphor and a light-emitting device.

Background Art

[0002] A light-emitting device combining a light-emitting element that emits primary light and a phosphor that absorbs the primary light and emits secondary light is known. In recent years, with the increase in the output of light-emitting devices, the requirements for the heat resistance and durability of phosphors have been increasing. For this reason, β-sialon phosphors with a stable crystal structure have attracted attention.

[0003] A phosphor in which Eu 2+ is solid-solved in the crystal structure of β-sialon is a phosphor that is excited by ultraviolet to blue light and exhibits green light emission with a wavelength of 520 nm or more and 550 nm or less. β-sialon in which Eu 2+ is solid-solved is also called Eu solid-solved β-sialon. This phosphor is used as a green light-emitting component of a light-emitting device such as a white light-emitting diode (white LED (Light Emitting Diode)). Eu solid-solved β-sialon has a very sharp emission spectrum among the phosphors in which Eu 2+ is solid-solved. Therefore, Eu solid-solved β-sialon is a phosphor suitable for the green light-emitting component of a backlight light source of a liquid crystal display panel that requires narrow-band light emission composed of the three primary colors of blue, green, and red light in particular.

[0004] As a technology related to β-sialon phosphors, for example, those described in Patent Document 1 can be mentioned. Patent Document 1 describes a β-sialon represented by the general formula: Si 6-Z Al Z O Z N 8-Z (0 < Z ≤ 0.42), which is a β-sialon in which Eu is solid-solved, and the 50% area average diameter of the primary particles of the β-sialon is 5 μm or more.

Prior Art Documents

Patent Documents

[0005] [Patent Document 1] International Publication No. 2012 / 011444 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, there has been a demand for further improvement in brightness of β-sialon phosphors and light emitting devices. The present invention has been made in view of the above circumstances and provides a β-sialon phosphor and a light emitting device with improved luminance. [Means for solving the problem]

[0007] The present inventors have carried out various studies to improve the brightness, and as a result of the studies, have completed the invention provided below.

[0008] According to the present invention, A β-type sialon phosphor containing europium as a solid solution, The ratio of aluminum elements at a depth of 8 nm from the surface of the phosphor obtained by X-ray photoelectron spectroscopy measurement is defined as P(Al). 8 [at%], and the ratio of aluminum elements at a depth of 80 nm from the surface of the phosphor is P(Al) 80 [at%], P(Al) 8 / P(Al) 80 β-type sialon phosphor having a refractive index of ≦0.9 is provided.

[0009] Further, according to the present invention, A light emitting device including a light emitting source and a wavelength conversion member, The wavelength conversion member includes a phosphor, A light emitting device, wherein the phosphor contains the above-mentioned β-type sialon phosphor. is provided. Effect of the Invention

[0010] According to the present invention, a β-sialon phosphor with improved luminance and a light-emitting device are provided.

Brief Description of the Drawings

[0011] [Figure 1] It is a cross-sectional view schematically showing an example of the structure of the device.

Modes for Carrying Out the Invention

[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In all the drawings, the same components are denoted by the same reference numerals, and the description will be omitted as appropriate. All the drawings are for illustrative purposes only. The shapes and dimensional ratios of the respective members in the drawings do not necessarily correspond to actual articles.

[0013] In this specification, the term "substantially" means including a range considering manufacturing tolerances, assembly variations, etc. without specific explicit description.

[0014] <β-sialon phosphor> The β-sialon phosphor of this embodiment is a β-sialon phosphor in which europium is dissolved. Let the ratio of aluminum element at a depth of 8 nm from the surface of this phosphor obtained by X-ray photoelectron spectroscopy measurement be P(Al) 8 [at%], and the ratio of aluminum element at a depth of 80 nm from the surface of this phosphor be P 80 [at%]. When P(Al) 8 / P(Al) 80 ≤0.9.

[0015] The β-sialon phosphor of this embodiment is represented by, for example, the general formula Si 6-z Al z O z N 8-z :Eu 2+ (0 < Z ≤ 4.2), and Eu 2+Hereinafter, the β-sialon having europium dissolved therein will be simply referred to as β-sialon. General formula Si 6-z Al z O z N 8-z :EU 2+ In the above, the Z value and the europium content are not particularly limited. The Z value is, for example, more than 0 and not more than 4.2, and from the viewpoint of further improving the emission intensity of the β-sialon phosphor, is preferably 0.005 to 1.0. The europium content is preferably 0.1% by mass to 2.0% by mass. β-SiAlON phosphors are usually made up of multiple particles that are tightly integrated together during heat treatment in the firing process. Each of the multiple particles is called a primary particle, and multiple particles that are tightly integrated together are called secondary particles.

[0016] In the β-type SiAlON phosphor of this embodiment, P(Al) 8 / P(Al) 80 ≦0.9, the luminance is improved. The reason for this is not necessarily clear. However, the inventors presume that the luminance may be reduced if an Al-containing compound is present on the surface of the phosphor particles, and that the luminance is improved by having a small amount of Al-containing compound on the surface of the phosphor particles as in this embodiment.

[0017] In order to obtain the β-SiAlON phosphor of this embodiment, it is preferable to select an appropriate manufacturing method in addition to the selection of appropriate raw materials. For example, P(Al) can be obtained by performing two-stage firing, i.e., a first firing step and a second firing step, removing coarse particles by appropriate sieving after the second firing, and / or performing an acid treatment as a post-firing treatment. 8 / P(Al) 80 It is possible to obtain a β-SiAlON phosphor having a refractive index of ≦0.9.

[0018] The β-sialon phosphor of this embodiment will be described in more detail below.

[0019] (P(Al) 8 , P(Al) 80 , P(Al) 8 / (Al)P 80 (preferable range) P(Al) 8 is preferably 0.8 [at%] or less, more preferably 0.75 [at%] or less, and further preferably 0.7 [at%] or less. 8 may be 0, but from the viewpoint of practical design / manufacturing, it is usually 0.1 [at %] or more, preferably 0.3 [at %] or more. P(Al) 80 is preferably 0.9 at % or more and 5 at % or less, more preferably 0.9 at % or more and 3 at % or less, and further preferably 0.9 at % or more and 2 at % or less. P(Al) 8 / P(Al) 80 is preferably 0.2 or more and 0.9 or less, more preferably 0.3 or more and 0.8 or less, and further preferably 0.4 or more and 0.8 or less. By adjusting these values ​​appropriately, the brightness can be further increased.

[0020] (Ratio of aluminum element at the outermost surface P(Al) 0 ) The ratio of aluminum elements at the outermost surface of the phosphor obtained by X-ray photoelectron spectroscopy was defined as P(Al). 0 [at%], P(Al) 0 is preferably 0.1 at % or less. The amount of aluminum element on the outermost surface of the phosphor is extremely small, which can further increase the brightness.

[0021] (Amount of elements other than aluminum) The β-sialon phosphor of this embodiment is a "sialon", and therefore typically contains Si, O, and N in addition to Al. The β-sialon phosphor of this embodiment also contains Eu. The general formula of the β-sialon phosphor of this embodiment is as described above. For the sake of certainty, the preferred ratios of each element other than Al at a depth of 8 nm or 80 nm from the surface of the phosphor, or at the outermost surface of the phosphor, are listed below. It is believed that brightness can be further improved by keeping these ratios within appropriate ranges. These ratios can also be determined by X-ray photoelectron spectroscopy.

[0022] - Ratio of each element at a depth of 8 nm from the surface of the phosphor Si: preferably 35 at% or more and 45 at% or less, more preferably 38 at% or more and 43 at% or less, and further preferably 40 at% or more and 43 at% or less. Eu: preferably 0.05 at % or more and 0.5 at % or less, more preferably 0.1 at % or more and 0.4 at % or less N: preferably 42.5 at% or more and 52.5 at% or less, more preferably 45 at% or more and 50 at% or less O: preferably 5 at % or more and 15 at % or less, more preferably 7.5 at % or more and 12.5 at % or less, and even more preferably 8 at % or more and 10.5 at % or less

[0023] - Ratio of each element at a depth of 80 nm from the surface of the phosphor Si: preferably 40 at % or more and 50 at % or less, more preferably 43 at % or more and 49 at % or less, and further preferably 45 at % or more and 49 at % or less. Eu: preferably 0.05 at % or more and 0.5 at % or less, more preferably 0.1 at % or more and 0.4 at % or less N: preferably 42 at% or more and 50 at% or less, more preferably 42.5 at% or more and 47 at% or less O: preferably 5 at % or more and 15 at % or less, more preferably 5 at % or more and 12.5 at % or less, and even more preferably 5 at % or more and 10 at % or less

[0024] As an additional finding of the present inventors, the ratio of silicon atoms at a depth of 8 nm from the surface of the phosphor is P(Si)8 [at%], the ratio of silicon atoms at a depth of 80 nm from the surface of the phosphor is P(Si) 80 [at%], P(Si) 8 / P(Si) 80 It is preferable to design the phosphor so that the luminance is ≦0.95, which can further increase the luminance. The inventors speculate that the Al-containing compound present on the surface of the phosphor particles, which may cause a decrease in luminance, is specifically a compound containing Al and Si. Therefore, it is believed that the luminance is further improved by having not only a relatively small amount of Al but also a relatively small amount of Si on the surface of the phosphor particles. P(Si) 8 / P(Si) 80 The value is preferably 0.5 to 0.95, and more preferably 0.7 to 0.95.

[0025] (Additional information on X-ray photoelectron spectroscopy measurements) A further note on X-ray photoelectron spectroscopy measurements. P(Al) 8 , P(Al) 80 and P(Al) 0 For the measurement, the β-SiAlON phosphor is usually etched away by 8 nm or 80 nm using ion etching or the like, and then irradiated with X-rays. Ion etching can usually be performed using Ar ions. The ion etching rate and the etching depth calculated by multiplying the rate by time are usually 2 A conversion value may be adopted. As the X-ray source, Al-Kα rays can be used. For specific conditions of the X-ray photoelectron spectroscopy measurement and ion etching, please refer to the Examples described later.

[0026] (About particle size) The β-sialon phosphor particles of this embodiment have an appropriate particle size, so that the brightness can be further increased. Specifically, the 50% diameter D of the β-type SiAlON phosphor particles of this embodiment based on the volumetric cumulative fractionV50 (volume-based median diameter) is preferably 5 μm or more, more preferably 10 μm or more. V50 The upper limit is preferably 50 μm, more preferably 30 μm. D V50 can be determined by a laser diffraction scattering method in accordance with JIS R 1629:1997. V50 When measuring the particle size, it is preferable to carry out a pretreatment such as a dispersion treatment using an ultrasonic homogenizer so as to minimize particle aggregation. For specific conditions of the pretreatment and details of the measuring device, please refer to the Examples given later.

[0027] The β-sialon phosphor particles of this embodiment are excited by a wide wavelength range from ultraviolet light to visible light, and emit green light with a main wavelength in the range of 520 nm to 550 nm with high efficiency, making them excellent as green-emitting phosphors. In addition, the β-SiAlON phosphor particles of this embodiment can be suitably used as a material for a phosphor layer in a light-emitting element. The light-emitting element can be applied to a light-emitting device such as a backlight source for a display or a lighting device. The light-emitting element is not particularly limited, but includes an LED and a phosphor layer laminated on the light-emitting surface side of the LED. As the LED, an ultraviolet LED or a blue LED that emits light with a wavelength of 300 nm or more and 500 nm or less, particularly a blue LED that emits light with a wavelength of 440 nm or more and 480 nm or less, can be used. In particular, the β-SiAlON phosphor particles obtained by the manufacturing method described below are excited by a wide range of wavelengths from ultraviolet to blue light and exhibit high-luminance green light emission, and therefore can be suitably used as a phosphor for a white LED that uses blue or ultraviolet light as a light source.

[0028] (Method of manufacturing β-type Sialon phosphor) As briefly described above, the β-sialon phosphor of this embodiment is produced by selecting appropriate raw materials and an appropriate manufacturing method. Specifically, the β-sialon phosphor of this embodiment can be obtained by adopting manufacturing process innovations such as adding a europium compound, which is one of the raw materials for β-sialon phosphors, in two or more batches and performing a firing process, adding a sufficiently large amount of europium compound in the second firing process, performing an annealing process, and performing an acid treatment after firing. However, for the β-sialon phosphor of this embodiment, various specific manufacturing conditions can be adopted, provided that the above-mentioned manufacturing techniques are adopted.

[0029] The method for producing the β-sialon phosphor will now be described in more detail. The method for producing a β-SiAlON phosphor of the present embodiment preferably includes two firing steps. That is, the method for producing a β-SiAlON phosphor of the present embodiment preferably includes the following steps: (i) a first firing step of firing a first raw powder containing a first europium compound to obtain a first fired powder containing β-sialon particles; (ii) a second firing step of firing the obtained first fired powder and a second raw material powder containing a second europium compound to obtain the β-sialon phosphor of the present embodiment; Includes. Here, in the second firing step, it is preferable to add the second europium compound in an amount larger than the conventional standard. Specifically, in the second firing step, it is preferable to add the second europium compound so that the amount of Eu is in excess of the amount of Eu that can be dissolved in the β-sialon.

[0030] Although the details are unclear, it is believed that by adding a second europium compound in the second firing step so that the amount of Eu is in excess of the amount that can be dissolved in β-sialon, the element distribution in the surface layer and the inside of the phosphor particles becomes different, and thus P(Al) 8 / P(Al) 80 It is considered that it becomes easier to obtain a β-SiAlON phosphor having a refractive index of ≦0.9.

[0031] The method for producing a β-sialon phosphor may further include one or more third firing steps in which the second fired powder is further fired to obtain a third fired powder, and in this step, a europium compound may be further added.

[0032] Here, in this embodiment, the "first firing step" refers to the first firing step in which a raw material powder containing a first europium compound is heat-treated, the "second firing step" refers to the second firing step in which a second europium compound is added and heat-treated, and the "third firing step" refers to a firing step carried out after the second firing step. In addition, in this embodiment, the "first europium compound" means the europium compound added in the first firing step, and the "second europium compound" means the europium compound added in the second firing step. In the present embodiment, the term "first raw material powder" refers to the raw material powder used in the first firing step, and the term "second raw material powder" refers to the raw material powder used in the second firing step. It is preferable that the respective raw material powders are mixed. In addition, in this embodiment, "first calcined powder" means the product obtained in the first calcination process, "second calcined powder" means the product obtained in the second calcination process, and "third calcined powder" means the product obtained in the third calcination process.

[0033] In the present embodiment, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. When multiple substances corresponding to europium are present in the composition, the content of europium in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified.

[0034] The first raw material powder preferably contains silicon nitride and aluminum nitride in addition to the first europium compound. The silicon nitride and aluminum compounds are materials for forming the skeleton of the β-sialon, and the europium compound is a material for forming the luminescence center. The first raw material powder may further contain β-sialon. The β-sialon is a material that serves as an aggregate or a core. The form of each of the above components contained in the first raw powder is not particularly limited, but each is preferably in powder form.

[0035] The europium compound that can be used is not particularly limited. For example, there can be mentioned oxides containing europium, hydroxides containing europium, nitrides containing europium, oxynitrides containing europium, halides containing europium, etc. These can be used alone or in combination of two or more. Among these, it is preferable to use europium oxide, europium nitride, and europium fluoride alone, and it is more preferable to use europium oxide alone.

[0036] The europium compound is preferably added separately before each of the multiple firing steps, specifically, before each of the first and second firing steps.

[0037] In each firing step, europium is divided into those that dissolve in the β-sialon, those that volatilize, and those that remain as hetero-phase components. The hetero-phase components containing europium can be removed by acid treatment or the like. However, if too much is produced, insoluble components may be produced by acid treatment, which may reduce brightness. On the other hand, if the hetero-phase does not absorb excess light, such a hetero-phase may remain, and europium may be contained in this hetero-phase. When a europium compound is added before firing in multiple firing steps, a β-sialon phosphor raw material other than the europium compound may be added together with the europium compound.

[0038] In the method for producing a β-sialon phosphor, when the total of the first fired powder and the second europium compound is taken as 100% by mass, from the viewpoint of more effectively removing Eu that does not contribute to improving the brightness of the β-sialon phosphor and further improving the brightness of the obtained β-sialon phosphor, the ratio of the second europium compound is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and even more preferably 3.0% by mass or more. Also, from the viewpoint of reducing the amount of insoluble heterogeneous phase components generated by the acid treatment and further improving the brightness of the obtained β-sialon phosphor, the ratio of the second europium compound is preferably 18.0% by mass or less, more preferably 17.0% by mass or less, and even more preferably 15.0% by mass or less. In the manufacturing method of the β-sialon phosphor of this embodiment, when the ratio of the second europium compound is within the above range, Eu that does not contribute to improving the brightness of the β-sialon phosphor can be more effectively removed, and the generation of heterophase components that are insoluble in acid treatment can be suppressed. Therefore, the manufacturing process for removing the heterophase components can be simplified, and as a result, the manufacturing time of the β-sialon phosphor can be shortened.

[0039] The total amount of europium contained in the first raw powder and the second raw powder is not particularly limited, but is preferably at least three times, and more preferably at least four times, the amount of europium dissolved in the final β-sialon phosphor. Moreover, the total amount of europium contained in the first raw material powder and the second raw material powder is preferably 18 times or less the amount of europium dissolved in the finally obtained β-sialon phosphor, which can reduce the amount of insoluble heterogeneous phase components generated by the acid treatment and further improve the brightness of the obtained β-sialon phosphor.

[0040] The amount of europium contained in the first raw material powder is not particularly limited, but it is preferable that this amount is greater than the amount of europium dissolved in the final β-sialon phosphor. Moreover, the amount of europium contained in the first raw powder is preferably three times or less than the amount of europium dissolved in the finally obtained β-sialon phosphor, which can reduce the amount of insoluble hetero-phase components generated by the acid treatment and further improve the brightness of the obtained β-sialon phosphor.

[0041] In each firing step, the raw material powder containing the europium compound can be obtained by, for example, a dry mixing method, or a wet mixing method in an inert solvent that does not substantially react with each component of the raw material and then removing the solvent, etc. The mixing device is not particularly limited, but for example, a V-type mixer, a rocking mixer, a ball mill, a vibration mill, etc. can be used.

[0042] The firing temperature in each firing step is not particularly limited, but is preferably in the range of 1800° C. or higher and 2100° C. or lower. When the firing temperature is 1800° C. or higher, the grain growth of the β-sialon phosphor proceeds more effectively, and the light absorptance, internal quantum efficiency, and external quantum efficiency can be further improved. If the firing temperature is 2100° C. or less, the decomposition of the β-sialon phosphor can be further suppressed, and the light absorptance, internal quantum efficiency, and external quantum efficiency can be further improved. Other conditions such as the temperature rise time, temperature rise rate, heating retention time, and pressure in each firing step are not particularly limited and may be appropriately adjusted depending on the raw materials used, etc. Typically, the heating retention time is 3 hours or more and 30 hours or less, and the pressure is 0.6 MPa or more and 10 MPa or less.

[0043] In each firing step, the mixture can be fired, for example, by filling the mixture into a container made of a material that does not react with the mixture during firing (e.g., boron nitride) and heating it in a nitrogen atmosphere. By using such a method, crystal growth reactions and solid-solution reactions can be promoted to obtain a β-SiAlON phosphor.

[0044] The first fired powder and the second fired powder are granular or agglomerated sintered bodies, which can be made into a β-sialon phosphor of a predetermined size by crushing, grinding, classifying, or other processes alone or in combination. A specific processing method is, for example, a method of pulverizing the sintered body to a predetermined particle size using a general pulverizer such as a ball mill, a vibration mill, or a jet mill. However, excessive pulverization may not only generate fine particles that easily scatter light, but may also cause crystal defects on the particle surface. In other words, it should be noted that excessive pulverization may cause a decrease in the luminous efficiency of β-sialon. Incidentally, this processing may be performed after the acid treatment or alkali treatment described later.

[0045] The method for producing a β-sialon phosphor may further include, after the second firing step, an annealing step of heating the second fired powder at a temperature lower than the firing temperature of the second firing step to obtain an annealed product. The annealing step is preferably carried out in a non-oxidizing atmosphere other than pure nitrogen, such as an inert gas, such as a rare gas or nitrogen gas, a reducing gas, such as hydrogen gas, carbon monoxide gas, hydrocarbon gas, or ammonia gas, or a mixture of these gases, or in a vacuum, etc. It is particularly preferably carried out in a hydrogen gas atmosphere or an argon atmosphere. The annealing step may be carried out either at atmospheric pressure or under elevated pressure. The heat treatment temperature in the annealing step is not particularly limited, but is preferably 1200° C. or higher and 1700° C. or lower, and more preferably 1300° C. or higher and 1600° C. or lower. By carrying out the annealing process, the luminous efficiency of the β-SiAlON phosphor can be further improved, and the transparency can also be improved since the rearrangement of the elements removes distortions and defects. Incidentally, a heterogeneous phase may be generated during the annealing process, but this can be removed by an acid treatment or the like, which will be described later.

[0046] Before the annealing step, a compound of an element constituting the β-SiAlON phosphor may be added and mixed in. The compound to be added is not particularly limited, but examples thereof include oxides, nitrides, oxynitrides, fluorides, chlorides, etc. of each element. In particular, the luminance of the β-sialon phosphor can be further improved by adding silica, aluminum oxide, europium oxide, europium fluoride, etc. to each heat-treated product. However, it is preferable that the undissolved residue of the added raw material can be removed by acid treatment or alkali treatment after the annealing step.

[0047] In the manufacturing method of the β-SiAlON phosphor, it is preferable to sieve the second fired powder or the annealed product of the second fired powder through a sieve with suitable openings to remove coarse particles. This is because, according to the knowledge of the present inventors, the coarse particles may contain a relatively large amount of Al-containing compounds that may reduce the luminance. The opening of the sieve is preferably about 75 μm / ♯200 or finer.

[0048] In the method for producing a β-sialon phosphor, a step of treating the second fired powder or the annealed product of the second fired powder with an acid, an alkali and / or a fluorine may be further carried out. The acid treatment or alkali treatment is, for example, a treatment in which an acidic or alkaline liquid is brought into contact with the second fired powder or the annealed product of the second fired powder, and the fluorine treatment is, for example, a step in which a fluorine-containing gas is brought into contact with the second fired powder or the annealed product of the second fired powder. It is believed that carrying out such a process makes it possible to dissolve and remove heterogeneous phase components (luminescence inhibitors) generated during the firing process, annealing process, etc. Therefore, it is possible to further improve the light absorption rate, internal quantum efficiency, and external quantum efficiency of the β-SiAlON phosphor.

[0049] The acidic liquid may be, for example, an aqueous solution containing one or more acids selected from hydrofluoric acid, sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid. The alkaline liquid may be, for example, an aqueous solution containing one or more alkalis selected from potassium hydroxide, ammonia water, and sodium hydroxide, but an acidic aqueous solution is more preferable, and a mixed aqueous solution of hydrofluoric acid and nitric acid is particularly preferable.

[0050] The treatment method using an acidic or alkaline liquid is not particularly limited, but can be carried out by dispersing the second fired powder or the annealed second fired powder in an aqueous solution containing an acid or an alkali and stirring for several minutes to several hours (for example, 10 minutes to 6 hours). After this treatment, it is preferable to separate substances other than the β-SiAlON phosphor by filtration and wash the substances attached to the β-SiAlON phosphor with water.

[0051] <Light emitting device> The light emitting device of this embodiment is a light emitting device including a light source and a wavelength conversion member. The wavelength conversion member includes a phosphor. The phosphor includes the β-SiAlON phosphor of this embodiment (the β-SiAlON phosphor described above).

[0052] FIG. 1 is a cross-sectional view showing a schematic example of the structure of a light emitting device 10. As shown in FIG. 1 is formed of an LED chip as a light emitting source 12, a first lead frame 13 on which the light emitting source 12 is mounted, a second lead frame 14, a wavelength conversion member 15 that covers the light emitting source 12, a bonding wire 16 that electrically connects the light emitting source 12 and the second lead frame 14, and a synthetic resin cap 19 that covers these. The wavelength conversion member 15 has a phosphor 18 and a sealing resin 17 in which the phosphor 18 is dispersed.

[0053] A recess 13b is formed in the upper portion 13a of the first lead frame 13 for mounting a light emitting diode chip as the light emitting source 12. The recess 13b has a generally funnel shape with a hole diameter gradually increasing from the bottom surface toward the top, and the inner surface of the recess 13b serves as a reflective surface. An electrode on the lower surface of the light emitting source 12 is die-bonded to the bottom surface of this reflective surface. The other electrode formed on the upper surface of the light emitting source 12 is connected to the surface of the second lead frame 14 via a bonding wire 16.

[0054] Various LED chips can be used as the light emitting source 12. Particularly preferred is an LED chip that emits light with a wavelength of 300 nm or more and 500 nm or less, which is from near ultraviolet to blue light.

[0055] The phosphor 18 used in the wavelength conversion member 15 of the light emitting device 10 includes the β-sialon phosphor of this embodiment. From the viewpoint of controlling the light wavelength of the light emitting device 10, the phosphor 18 may include, in addition to the β-sialon phosphor of this embodiment, an α-sialon phosphor, a KSF phosphor, CaAlSiN 3 The phosphor may further include a phosphor such as a single substance or a mixture of YAG. Examples of elements dissolved in these phosphors include europium (Eu), cerium (Ce), strontium (Sr), calcium (Ca), manganese (Mn), etc. These phosphors may be used alone or in combination of two or more. Among these, the phosphor to be used in combination with the β-SiAlON phosphor of the present embodiment is preferably a KSF phosphor in which manganese is dissolved. By using the β-SiAlON phosphor of the present embodiment, which shows green, in combination with the KSF phosphor which shows red, it can be suitably used as a backlight LED suitable for a high color rendering TV or the like. By combining the light emitting source 12 and the wavelength conversion member 15, it is possible to emit light having a high emission intensity. Just to be clear, the KSF phosphor containing manganese in solid solution has the general formula: A 2 M (1-n) F6 :Mn 4+ n In this general formula, the element A is one or more alkali metal elements containing K, the element M is Si alone, Ge alone, or a combination of Si and one or more elements selected from the group consisting of Ge, Sn, Ti, Zr, and Hf, and 0 <n≦0.1である。

[0056] In the case of the light emitting device 10 using the β-SiAlON phosphor of this embodiment, by irradiating near-ultraviolet light or visible light containing a wavelength of 300 nm or more and 500 nm or less as an excitation source as the light emission source 12, it has green light emission characteristics with a peak in a wavelength range of 520 nm or more and 550 nm or less. Therefore, by using a near-ultraviolet LED chip or a blue LED chip and the β-SiAlON phosphor of this embodiment as the light emission source 12, and further combining it with a single substance or a mixture of a red light emitting phosphor, a blue light emitting phosphor, a yellow light emitting phosphor, or an orange light emitting phosphor having a wavelength of 600 nm or more and 700 nm or less, it is possible to produce white light.

[0057] The light emitting device 10 has good brightness since it contains a β-sialon phosphor with improved emission intensity.

[0058] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0059] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples.

[0060] Example 1 Using a V-type mixer (Tsutsui Rikagaku Kikai S-3), 95.80 mass% of α-type silicon nitride powder (SN-E10 grade, oxygen content 1.0 mass%) manufactured by Ube Industries, 2.74 mass% of aluminum nitride powder (F grade, oxygen content 0.8 mass%) manufactured by Tokuyama, 0.56 mass% of aluminum oxide powder (TM-DAR grade) manufactured by Taimei Chemical, and 0.90 mass% of europium oxide powder (RU grade) manufactured by Shin-Etsu Chemical were mixed, and then the resulting mixture was passed through a sieve with a mesh size of 250 μm to remove aggregates, thereby obtaining a first raw material mixed powder. The compounding ratio here (referred to as the first compounding composition (mass%)) is the general formula of β-type sialon: Si 6-Z Al Z O Z N 8-Z In this case, except for europium oxide, it was designed so that Z=0.22 was obtained by calculating from the Si / Al ratio.

[0061] 200 g of the resulting raw powder having the first composition was packed into a cylindrical boron nitride container with a lid, having an inner diameter of 10 cm and a height of 10 cm, and was subjected to a heat treatment (first firing step) at 1950°C for 10 hours in a nitrogen atmosphere pressurized at 0.8 MPa in an electric furnace with a carbon heater. The powder subjected to the heat treatment was pulverized with a supersonic jet pulverizer (Nippon Pneumatic Mfg. Co., Ltd., PJM-80SP), and the pulverized material was then passed through a nylon sieve with an opening of 45 μm to obtain a first fired powder. The first calcined powder was mixed with europium oxide powder (RU grade) manufactured by Shin-Etsu Chemical Co., Ltd. in a mixing ratio of 90:10 (referred to as the second blending composition (mass%)), and the first calcined powder and europium oxide powder were mixed using a V-type mixer (S-3 manufactured by Tsutsui Rikagaku Kikai Co., Ltd.) The mixture was then passed through a nylon sieve with a mesh size of 250 μm to remove aggregates, and a second raw material mixed powder was obtained.

[0062] 200 g of the raw material powder having the obtained second composition was filled into a cylindrical boron nitride container with a lid having an inner diameter of 10 cm and a height of 10 cm, and heat treatment (second firing step) was performed at 2020 °C for 12 hours in a pressurized nitrogen atmosphere of 0.8 MPa in an electric furnace with a carbon heater. The powder subjected to the above heat treatment was pulverized by a supersonic jet mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd., PJM-80SP), and then the obtained pulverized product was passed through a nylon sieve with an opening of 45 μm to obtain a second fired powder. The passing rate of the sieve was 92%.

[0063] 20 g of the obtained second fired powder was filled into a cylindrical boron nitride container with a lid having an inner diameter of 5 cm and a height of 3.5 cm, and annealing treatment was performed at 1500 °C for 8 hours in an argon atmosphere at atmospheric pressure in an electric furnace with a carbon heater. The powder subjected to the annealing treatment was subjected to an acid treatment of immersing it in a 1:1 mixed acid of 50% hydrofluoric acid and 70% nitric acid at 75 °C for 30 minutes. The powder after the acid treatment was allowed to settle as it was, and decantation for removing the supernatant and fine powder was repeated until the pH of the solution was 5 or more and the supernatant became transparent. Finally, the obtained precipitate was filtered and dried to obtain the phosphor powder of Example 1. As a result of powder X-ray diffraction measurement, the existing crystal phase was a single phase of β-sialon, and it was found that a β-sialon phosphor was obtained. The Eu content measured by ICP emission spectroscopic analysis was 0.72 mass%. The first composition and the second composition in Example 1 are shown in Table 1 below.

[0064] <Ratio of aluminum element etc. determined by X-ray photoelectron spectroscopy measurement> First, the β-sialon phosphor was etched by 8 nm or 80 nm in terms of SiO 2 using Ar ions by ion etching. The β-sialon phosphor etched by 8 nm or 80 nm was subjected to XPS analysis under the following equipment and conditions to obtain information on the element ratio at each depth. · Equipment: X-tool manufactured by ULVAC-PHI · Analysis conditions: Al-Kα line, 15 kV, 50 W · Analysis area: 200 μmφ

[0065] In addition, the β-SiAlON phosphor that was not ion-etched with Ar ions was also subjected to XPS analysis in the same manner, thereby obtaining information on the elemental composition of the outermost surface.

[0066] Table 2 shows the element ratio information.

[0067] <D V50 Measurements > The particle size distribution of the β-sialon phosphor particles of Example 1 was measured by a laser diffraction scattering method in accordance with JIS R1629: 1997 using a Microtrac MT3300EX II (Microtrac Bell Co., Ltd.) The measurement sample was pretreated as follows. 0.5 g of β-type sialon phosphor particles were added to 100 cc of ion-exchanged water, and a dispersion treatment was carried out for 3 minutes using an Ultrasonic Homogenizer US-150E (Nihon Seiki Seisakusho Co., Ltd., tip size φ20 mm, Amplitude 100%, oscillation frequency 19.5 KHz, amplitude approximately 31 μm). This was used as a measurement sample. The particle size distribution of the measurement sample was measured using the above-mentioned device. V50 D V50 are shown in Table 1 below.

[0068] <Evaluation of fluorescent properties> The fluorescent properties of the β-sialon phosphor were evaluated based on the peak intensity and peak wavelength measured by the following method. The equipment used was a spectrofluorophotometer (Hitachi High-Technologies Corporation, F-7000) calibrated with the Rhodamine B method and a standard light source. The obtained phosphor powder was filled into a dedicated solid sample holder, and then the fluorescence spectrum was measured using the spectrofluorophotometer when irradiated with excitation light split to a wavelength of 455 nm, and the peak intensity and peak wavelength were obtained from the obtained fluorescence spectrum. The results are shown in Table 3.

[0069] Just to mention for the sake of certainty, since the peak intensity varies depending on the measuring device and conditions, the unit is an arbitrary unit. Measurements were taken under the same conditions for each example and comparative example, and the β - type sialon phosphors of each example and comparative example were measured continuously for comparison. Table 3 shows the peak intensities of the phosphors when the peak intensity of the β - type sialon phosphor of Comparative Example 1 was set to 100%.

[0070] <CIE Chromaticity> The CIE (International Commission on Illumination) chromaticity of the fluorescence spectrum was determined by measuring the emission spectrum of the total luminous flux collected using an integrating sphere for fluorescence against 455 - nm excitation with an instantaneous multi - photometry system (manufactured by Otsuka Electronics Co., Ltd., MCPD - 7000).

[0071] (Example 2) β - type sialon phosphor powders were obtained in the same manner as in Example 1, except that the second composition was changed to the mixing ratio shown in Table 1. As a result of performing powder X - ray diffraction measurement on the obtained β - type sialon phosphors, the existing crystal phase was β - type sialon single phase in all cases. Also, the same evaluation as in Example 1 was performed. The obtained results are shown in Tables 2 and 3.

[0072] (Comparative Example 1) β - type sialon phosphor powder was obtained in the same manner as in Example 1, except that the process corresponding to the second firing process of Example 1 was not performed. As a result of performing powder X - ray diffraction measurement on the obtained β - type sialon phosphor, the existing crystal phase was β - type sialon single phase. Also, the same evaluation as in Example 1 was performed. The obtained results are shown in Tables 2 and 3.

[0073]

Table 1

[0074]

Table 2

[0075] In Examples 1 and 2, P(Al) 0 The value was less than 0.1 at% which is the detection limit of the instrument.

[0076] [Table 3]

[0077] As shown in Table 3, P(Al) 8 / P(Al) 80 The emission peak intensity of the β-SiAlON phosphors of Examples 1 and 2, which is ≦0.9, is P(Al) 8 / P(Al) 80 The emission peak intensity was 10% or more higher than that of the β-SiAlON phosphor of Comparative Example 1, in which P(Al) 8 / P(Al) 80 It was shown that the luminance can be improved by using a β-SiAlON phosphor with a refractive index of ≦0.9.

[0078] This application claims priority based on Japanese Patent Application No. 2019-150289, filed on August 20, 2019, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]

[0079] 10 Light emitting device 12 Light emitting source (LED chip) 13 First lead frame 13a Upper 13b Recess 14 Second Lead Frame 15 Wavelength conversion material 16 Bonding Wire 17 Sealing resin 18 Phosphor (β-type Sialon phosphor) 19 Cap

Claims

1. A β-type sialon phosphor containing europium as a solid solution, The ratio of aluminum element at a depth of 8 nm from the surface of the phosphor obtained by X-ray photoelectron spectroscopy is defined as P(Al). 8 [at %], the ratio of aluminum element at a depth of 80 nm from the surface of the phosphor is P(Al) 80 When expressed as [at %], P(Al) 8 / P(Al) 80 ≦0.9, A β-type sialon phosphor represented by the general formula Si6-zAlzOzN8-z:Eu2+ (0<Z≦4.2).

2. The β-sialon phosphor according to claim 1, Said P(Al) 8 A β-SiAlON phosphor having a content of 0.8 at % or less.

3. 3. The β-sialon phosphor according to claim 1, Said P(Al) 80 The β-sialon phosphor has a content of 0.9 at % or more and 5 at % or less.

4. The β-sialon phosphor according to any one of claims 1 to 3, The ratio of aluminum elements at the outermost surface of the phosphor obtained by X-ray photoelectron spectroscopy is defined as P(Al). 0 When expressed as [at %], P(Al) 0 The β-type sialon phosphor has a content of 0.1 at % or less.

5. The β-sialon phosphor according to any one of claims 1 to 4, 50% diameter D in cumulative volumetric fraction V50 A β-sialon phosphor having a particle size of 5 μm or more and 50 μm or less.

6. 6. The β-sialon phosphor according to claim 1, The ratio of silicon atoms at a depth of 8 nm from the surface of the phosphor obtained by X-ray photoelectron spectroscopy is defined as P(Si) 8 [at %], the ratio of silicon atoms at a depth of 80 nm from the surface of the phosphor is P(Si) 80 When expressed as [at %], P(Si) 8 / P(Si) 80 ≦0.

95.

7. A light emitting device including a light emitting source and a wavelength conversion member, The wavelength conversion member includes a phosphor, A light emitting device, comprising the phosphor according to claim 1 .

8. 8. The light emitting device according to claim 7, The light emitting device, wherein the light emitting source includes an LED chip that generates light with a wavelength of 300 nm to 500 nm.

9. 9. The light emitting device according to claim 7, The light emitting device, wherein the phosphor further includes a KSF phosphor in which manganese is dissolved.

Citation Information

Patent Citations

  • Method for producing β-sialon phosphor

    JP2017036430A

  • Method for producing β-sialon phosphor

    JP2017110206A

  • Β type sialon phosphor and method for producing the same and light emitting device using the same

    JP2018002870A

  • Manufacturing method of β type sialon phosphor

    JP2019199531A

  • JPP6572373B