Fuel debris disposal method

A multi-stage fluoridation process separates and converts fuel debris into a vitrified material with a balanced composition, addressing the challenge of high actinide oxide content in fuel debris and facilitating safe disposal.

JP7588611B2Active Publication Date: 2024-11-22HITACHI GE NUCLEAR ENERGY LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022011582
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-01-28
Publication Date
2024-11-22
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

Fuel debris from nuclear reactors contains a high proportion of actinide oxides relative to fission product oxides, making it difficult to convert into a vitrified material suitable for geological disposal.

Method used

A multi-stage fluoridation process is employed to separate and volatilize nuclear fuel materials, convert the remaining fluoride residue into oxides, and mix these with a glass base material to form a vitrified material with a balanced composition ratio.

Benefits of technology

The process facilitates the conversion of fuel debris into a vitrified material suitable for disposal, reducing the generation of secondary waste and ensuring stability over long periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588611000014
    Figure 0007588611000014
  • Figure 0007588611000015
    Figure 0007588611000015
  • Figure 0007588611000001
    Figure 0007588611000001
Patent Text Reader

Abstract

To provide a treatment method of fuel debris for fluoridating fuel debris and to fluorinate the nuclear fuel material, in which the remaining fluoride residue is converted to oxide and then vitrified with the proven composition ratio for easily vitrify to finally dispose of the fuel debris as vitrification.SOLUTION: To solve the above problem, a disclosed treatment method of fuel debris is a treatment method of fuel debris for vitrifying fuel debris. After fluoridating the fuel debris in the halogenation process to volatilize the nuclear fuel material, the remaining fluoride residue is converted into an oxide. After that, the obtained oxide is mixed with the glass base material to form a vitrified body.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for treating fuel debris in a nuclear power plant. [Background technology]

[0002] The fuel debris from the Fukushima Daiichi Nuclear Power Plant (1F) will be stored for a while after it is removed from the reactors. Because the fuel debris contains radioactive materials such as nuclear fuel material and fission products, it needs to be processed into a stable form and then ultimately disposed of safely.

[0003] Radioactive waste generated from nuclear power generation and reprocessing is stably solidified and then buried in various disposal sites according to its properties. High-level radioactive waste generated from reprocessing contains radioactive materials with long half-lives, so it is considered to be stably vitrified, then disposed of in a geological repository after applying multiple barriers.

[0004] Fuel debris is produced by melting spent fuel and contains radioactive materials with long half-lives. Therefore, in order to ultimately dispose of the fuel debris, it must be processed into waste forms that will remain stable for the long term, and then disposed of in a manner that will ensure safety for the same period.

[0005] For these reasons, a method of converting fuel debris into stable vitrified bodies and disposing of them in a geological repository, like the high-level radioactive waste generated during reprocessing, is one of the most promising methods for processing and disposing of fuel debris.

[0006] An example of a typical composition (unit: wt%) of high-level radioactive waste (vitrified waste) is described in Non-Patent Document 1 and is shown in Table 1.

[0007] [Table 1]

[0008] In vitrified waste, radionuclides are trapped in the glass matrix to make them less likely to be released. As shown in Table 1, the base material of glass is mainly SiO2 or B2O3, and the radionuclides trapped are oxides of fission products (FPs) and oxides of actinides (ACs). According to Table 1, the ratio of the amount of AC oxides to FP oxides is approximately 1:14 for composition A and approximately 1:4 for composition B. In other words, vitrified waste is characterized by having less AC oxides than FP oxides, and it can be said that the ratio of AC oxides to FP oxides in typical vitrified waste is in the range of 1:4 to 1:14.

[0009] Meanwhile, in Non-Patent Document 2, Washiya et al. estimate the amount of fuel debris at the Fukushima Daiichi Nuclear Power Plant (1F). Based on the estimate by Washiya et al., the amount of fuel debris was set assuming that the amount of concrete generated is approximately equal to the amount of nuclear fuel material, as shown in Table 2.

[0010] [Table 2]

[0011] On the other hand, Patent Document 1 describes a fluorination process as a method for recovering nuclear fuel material from fuel debris.

[0012] That is, Patent Document 1 describes a method in which, in order to shorten the time required for recovering molten nuclear fuel material, fluorine gas is supplied into a reactor pressure vessel surrounded by a reactor containment vessel, the fluorine gas reacts with uranium and plutonium contained in the fuel debris present in the reactor pressure vessel to generate volatile uranium fluoride and volatile plutonium fluoride, and the generated volatile uranium fluoride and volatile plutonium fluoride are guided from the reactor pressure vessel to a cold trap present outside the reactor containment vessel and solidified in the cold trap for recovery. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] JP 2016-48209 A [Non-patent literature]

[0014] [Non-Patent Document 1] JNC TN8400 99-085 (1999). [Non-Patent Document 2] T. Washiya et al., “Study of Treatment Scenarios for Fuel Debris Removed from FUKUSHIMA DAIICHI NPS”, Proceedings of ICONE-23, ICONE23-1953, May 17-21, 2015, Chiba, Japan (2015). Summary of the Invention [Problem to be solved by the invention]

[0015] The fuel debris is composed of nuclear fuel material derived from the fuel, cladding tube material, structural materials, and concrete, and its representative components are assumed to be UO2, Zr, Fe, and SiO2, respectively.

[0016] When considering vitrifying fuel debris as it is, it is necessary to classify each component of the fuel debris as either a glass matrix or a target for containment.

[0017] First, the uranium in the nuclear fuel material is an actinide element, so it corresponds to AC oxides trapped in a glass matrix. On the other hand, the SiO2 in concrete is a component of glass, so it corresponds to the glass matrix. The Zr in the cladding tube material and the Fe in the structural material are not contained in the glass matrix, or even if they are contained, the amount is very small, so it is considered appropriate to consider them as targets to be trapped in the glass matrix, and since Zr and Fe are not actinide elements, it is appropriate to classify them as FP oxides.

[0018] If we classify them in this way and evaluate the ratio of AC oxides to FP oxides to be vitrified based on the quantities in Table 2, the ratio is approximately 1:0.8, which shows that the proportion of AC oxides in fuel debris is very high. In other words, when vitrifying fuel debris, it will be significantly outside the range of the AC oxide to FP oxide ratio in existing vitrified bodies, so it is difficult to vitrify fuel debris as is.

[0019] The above-mentioned Patent Document 1 and Non-Patent Documents 1 and 2 do not disclose any measures to solve the above-mentioned problems.

[0020] The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a method for treating fuel debris by fluorinating the fuel debris, fluorinating and volatilizing the nuclear fuel material, separating it, and converting the remaining fluoride residue into an oxide and then vitrifying it, thereby ultimately turning the fuel debris into a vitrified body suitable for disposal, and also by providing a fuel debris treatment method which facilitates vitrification because the vitrification has a proven composition ratio. [Means for solving the problem]

[0021] The inventors considered the possibility of selectively recovering nuclear fuel material from the fuel debris, since it is a resource, and vitrifying the remaining material as waste.

[0022] That is, in order to achieve the above object, the fuel debris processing method of the present invention is a method for processing fuel debris by converting the fuel debris into a vitrified body, In the halogenation process After volatilizing the nuclear fuel material by fluorination, the remaining fluoride residue is converted into an oxide, and then the obtained oxide is mixed with a glass base material to produce a vitrified body. Hit it, The halogenation treatment step is carried out in multiple stages, The fuel debris is reacted with excess fluorine gas in a first halogenation treatment step, and silicon fluoride, excess fluorine gas B, oxygen gas B, and nuclear fuel material A are generated as volatile components by the halogenation in the first halogenation treatment step, and these are sent to a gas separation step A to separate only the nuclear fuel material A, On the other hand, the fluorinated residue A fluorinated in the first halogenation treatment step is sent to a second halogenation treatment step, in which it is reacted with fluorine gas, and the fluorinated residue A is halogenated in the second halogenation treatment step to generate nuclear fuel material B, excess fluorine gas A and oxygen gas A as volatile components, which are sent to a gas separation step B to separate only the nuclear fuel material B, Furthermore, the fluorinated residue B fluorinated in the second halogenation process is sent to an oxidation process, in which the chemical form is converted to an oxide by reacting with water vapor, and the resulting solid is sent to a vitrification process as waste, in which the waste and the glass base material are melted, and then cooled and solidified to obtain a vitrified body. It is characterized by:

[0023] When UO2, a nuclear fuel material, reacts with fluorine gas, it volatilizes as hexafluoride (sublimation point: 56.5°C), as shown in equation (1).

[0024] [ka]

[0025] In addition, when SiO2, a concrete component, reacts with fluorine gas, it volatilizes as tetrafluoride (sublimation point: -95.7°C), as shown in equation (2).

[0026] [ka]

[0027] As shown in equations (3) and (4), Zr and Fe react with fluorine gas to produce fluorides, but because of their low volatility, they remain as solids.

[0028] [ka]

[0029] [ka]

[0030] The fluorinated and volatilized uranium can be recovered and effectively used as nuclear fuel material, so the residue after fluorination (hereafter referred to as fluoride residue) will ultimately become waste. Because fluoride cannot be vitrified as it is, it is converted to oxide before vitrification. The weight of each substance when the fluoride residue is converted to oxide is shown in Table 2.

[0031] In principle, all of U and Si react with fluorine gas and volatilize as gas, but the weight of the fluorination residue was evaluated conservatively assuming that the volatilization rate during fluorination was 90%.

[0032] When fluoride residues are solidified into glass, as in the case of fuel debris mentioned above, the nuclear fuel material corresponds to AC oxide, while the cladding tube material and structural materials correspond to FP oxide, being other solidification targets.

[0033] In this case, the amount of AC oxide is 30t and the amount of FP oxide is 318t, and the ratio of AC oxide to FP oxide is approximately 1:11. This ratio is within the range of 1:4 to 1:14, which is the ratio of AC oxide to FP oxide in typical vitrified waste, and it can be said that vitrification is easy.

[0034] In other words, by first fluorinating the fuel debris, converting the fluoride residue into an oxide, and then vitrifying it, the fuel debris can be turned into a vitrified body suitable for geological disposal, and the vitrification process becomes easier because the composition ratio is proven to be effective. Effect of the Invention

[0035] According to the present invention, fuel debris is fluorinated to volatilize and separate the nuclear fuel material, and the remaining fluoride residue is converted to an oxide and then vitrified. This ultimately makes it possible to turn the fuel debris into a vitrified body suitable for disposal, and also has the effect of making vitrification easier because the composition ratio during vitrification has a proven track record. [Brief description of the drawings]

[0036] [Figure 1] 1 is a flowchart showing a first embodiment of a method for treating fuel debris according to the present invention. [Diagram 2] 1 is a flowchart showing a second embodiment of the fuel debris processing method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] Hereinafter, the fuel debris processing method of the present invention will be described based on the illustrated embodiment. EXAMPLES

[0038] A first embodiment of the fuel debris processing method of the present invention will be described with reference to FIG.

[0039] Fig. 1 is a flow chart showing a fuel debris processing method according to a first embodiment. As shown in Fig. 1, the fuel debris processing method according to this embodiment includes a first halogenation treatment step 1, a second halogenation treatment step 2, a gas separation step A6 in the first halogenation treatment step 1, a gas separation step B3 in the second halogenation treatment step 2, an oxidation treatment step 4, and a vitrification step 5.

[0040] The fuel debris processing method of this embodiment will be described in detail below.

[0041] The fuel debris 10 is reacted with fluorine gas in the first halogenation treatment process 1. The gas used in the first halogenation treatment process 1 is excess fluorine gas A11, which is a gas obtained by separating nuclear fuel material B18 from the off-gas of the second halogenation treatment process 2. The excess fluorine gas A11 is accompanied by oxygen gas A12, which is a reaction product, as an impurity.

[0042] The halogenation in the first halogenation process 1 generates silicon fluoride 13, excess fluorine gas B14, oxygen gas B15, and nuclear fuel material A24 as volatile components. These gases are sent to the gas separation process A6, and only the nuclear fuel material A24 is separated.

[0043] The equipment used in the gas separation step A6 is specifically a cold trap that condenses and recovers UF6. The temperature of the cold trap is a temperature at which only UF6 condenses, without condensing fluorine gas or oxygen gas, and is preferably, for example, about 0°C. The condensed and recovered UF6 is recycled as nuclear fuel material. The remaining gas from which the nuclear fuel material has been separated is treated and disposed of as secondary waste, but silicon fluoride may be converted into oxide to make SiO2 and then used as a glass base material in the vitrification step 5.

[0044] The temperature for the halogenation treatment in the first halogenation treatment step 1 may be set to 350° C. or lower at which UF6 is not produced by fluorination. The reaction in this case is shown in the following formula (5).

[0045] [ka]

[0046] In this reaction, solid UO2F2 is produced, and therefore no volatile nuclear fuel material such as nuclear fuel material A24 is produced, making it unnecessary to recover nuclear fuel material A24 from the gas. In this case, the gas separation step A6 can be omitted.

[0047] On the other hand, from the viewpoint of improving the reaction rate while suppressing adhesion of fluorinated volatile gases of impurity components to the reaction vessel, the temperature of the halogenation treatment is preferably 100° C. or higher.

[0048] The fluorination residue A16 is sent to the second halogenation process 2. In the second halogenation process 2, fluorine gas 17 is used. In this process, since it is desired to fluorinate and volatilize the nuclear fuel material B18, the temperature for the halogenation process is desirably 350°C or higher at which UF6 is produced by fluorination.

[0049] Volatile components generated by halogenation in the second halogenation process 2 are nuclear fuel material B18, excess fluorine gas A11, and oxygen gas A12. These gases are sent to the gas separation process B3, where only the nuclear fuel material B18 is separated.

[0050] The equipment used in the gas separation step B3 is specifically a cold trap that condenses and recovers UF6. The temperature of the cold trap is a temperature at which only UF6 condenses, and not fluorine gas or oxygen gas, and is preferably, for example, about 0°C. The condensed and recovered UF6 is recycled as a nuclear fuel material.

[0051] When the temperature in the first halogenation treatment step 1 is set to 350° C. or lower, the reaction in the second halogenation treatment step 2 is as shown in formula (6) below.

[0052] [ka]

[0053] The fluoride residue B19 is sent to the oxidation treatment process 4, where it is reacted with steam 20 to convert its chemical form into an oxide. The resulting solid is sent to the vitrification process 5 as waste 21. Here, the waste 21 and glass base material 22 are melted at high temperature, and then cooled and solidified to obtain a vitrified body 23.

[0054] The amount of fluorine gas used in this embodiment will be described.

[0055] Table 3 shows the amounts of substances contained in the fuel debris and the amount of fluorine required to completely fluorinate them, based on the fluorination reaction formula.

[0056] [Table 3]

[0057] Assuming that the total amount of fuel debris is 826.6 t, the total amount of material can be roughly calculated as 9.4 Mmol (9.4 × 10 6 mol). Furthermore, when the amount of fluorine required for fluorination is evaluated based on the fluorination reaction formula, the amount of F2 required to fluorinate the entire amount of fuel debris is 18.9 Mmol. In Example 1, 18.9 Mmol of fluorine gas is supplied in the first halogenation treatment step 1. Since fluorine is a strong reactant, in principle it is completely consumed in the fluorination reaction.

[0058] In this example, it is conservatively assumed that 90% is consumed in the fluorination reaction, leaving 10% as unreacted fluorine gas (excess fluorine gas B14) as secondary waste (1.9 Mmol).

[0059] The fluorine mass balance was evaluated at this time and the results are shown in Table 4.

[0060] [Table 4]

[0061] Next, the fluorination residue A16 is reacted with 18.9 Mmol of fluorine gas in the second halogenation process 2. The fluorination residue A16 is reacted with the excess fluorine gas A11 in the first halogenation process 1 and is 90% fluorinated. Therefore, the amount of fluorine required to fluorinate the fluorination residue A16 is 1.9 Mmol, and in the second halogenation process 2, 10 times the amount of fluorine required for fluorination is supplied. Since a considerable excess of fluorine is supplied for fluorination, the fluorination residue A16 is completely fluorinated. The excess fluorine gas A11 is reused in the first halogenation process 1, so no secondary waste is generated. The excess fluorine gas A11 is used in the first halogenation process 1 by adding fluorine gas to make up for the shortage.

[0062] The fluorine mass balance in the second halogenation treatment step 2 was evaluated, and the results are shown in Table 5.

[0063] [Table 5]

[0064] For comparison, the amount of secondary waste generated when complete fluorination is achieved in a single halogenation treatment, rather than in two stages as in Example 1, is evaluated. Table 6 shows the results.

[0065] [Table 6]

[0066] In order to completely fluorinate, it was assumed that 10 times the amount of fluorine required for fluorination (189 Mmol) would be supplied, in which case the amount of fluorine that would become secondary waste would be 170.1 Mmol.

[0067] From the above results, it is found that by carrying out the halogenation treatment in two stages as in Example 1, the amount of fluorine that becomes secondary waste can be significantly reduced from approximately 170.1 Mmol to 1.9 Mmol.

[0068] According to this embodiment, the fuel debris is fluorinated to volatilize and separate the nuclear fuel material, and the remaining fluoride residue is converted to oxide and then vitrified, which ultimately makes the fuel debris into a vitrified body suitable for disposal, and also makes it easier to vitrify because the composition ratio (ratio of AC oxide to FP oxide) has a proven track record when vitrifying. In addition, by carrying out the fluorination treatment in multiple stages, the amount of secondary waste generated can be reduced. EXAMPLES

[0069] A second embodiment of the fuel debris processing method of the present invention will be described with reference to FIG.

[0070] 2 is a flow chart showing a fuel debris treatment method according to a second embodiment of the present invention, in which hydrogen fluoride is used as a halogenating agent.

[0071] As shown in FIG. 2 , the fuel debris processing method of this embodiment includes a first halogenation treatment process 30, a second halogenation treatment process 31, a gas separation process A 32 in the first halogenation treatment process 30, a gas separation process B 33 in the second halogenation treatment process 31, a third halogenation treatment process 34, a gas separation process C 35 in the third halogenation treatment process 34, an oxidation treatment process 36, and a vitrification process 37.

[0072] The fuel debris processing method of this embodiment will be described in detail below.

[0073] In this embodiment, first, the fuel debris 40 is fluorinated in a first halogenation treatment process 30. The gas used in the fluorination process is excess hydrogen fluoride gas A41, which is a gas obtained by separating silicon fluoride A48 from the off-gas in the second halogenation treatment process 31. The excess hydrogen fluoride gas A41 is accompanied by water vapor A42, which is a reaction product, as an impurity.

[0074] The reaction formula for fluorinating UO2 with hydrogen fluoride is shown in the following formula (7).

[0075] [ka]

[0076] The temperature for halogenation treatment is preferably 600°C or less, taking into consideration corrosion of the equipment materials.

[0077] Unlike Example 1, when fluorination is performed with excess hydrogen fluoride gas A41, uranium becomes non-volatile uranium tetrafluoride even if the reaction temperature is set to 350°C or higher. Therefore, it is not necessary to set the reaction temperature below 350°C in order to suppress the fluorination and volatilization of uranium, and the treatment temperature can be set to a higher temperature in order to increase the reaction rate.

[0078] Moreover, similarly to Example 1, from the viewpoint of improving the reaction rate while suppressing adhesion of fluorinated volatile gases of impurity components to the reaction vessel, the temperature of the halogenation treatment is desirably 100° C. or higher.

[0079] The halogenation in the first halogenation treatment step 30 generates silicon fluoride B43, excess hydrogen fluoride gas B44, and water vapor B45 as volatile components. These gases are sent to the gas separation step A32.

[0080] The gas separation step A32 is a cold trap that condenses and recovers the excess hydrogen fluoride gas B44 and water vapor B45. The temperature of the cold trap is a temperature at which only the excess hydrogen fluoride gas B44 and water vapor B45 condense without condensing silicon fluoride B43, and is preferably, for example, about 0°C. The condensed and recovered excess hydrogen fluoride gas B44 is recycled as a halogenating agent.

[0081] In addition, since fluorine gas was used in Example 1, silicon fluoride (sublimation point: -95.7°C) coexists with fluorine gas (boiling point: -188°C), and since the volatilization temperature is low, there was a problem that it was difficult to separate using a cold trap.

[0082] In Example 2, the halogenation is performed with hydrogen fluoride, and hydrogen fluoride (point: 19.5°C) and silicon fluoride can be easily separated using a cold trap. Therefore, there is an effect that hydrogen fluoride can be recycled without being converted into secondary waste. Silicon fluoride, which becomes waste, may be converted into oxide to make SiO2, and then used as a glass base material in the vitrification process 37.

[0083] Next, in the first halogenation treatment step 30, the fluoride residue A46 that has been almost fluorinated is sent to the second halogenation treatment step 31, where it is reacted with hydrogen fluoride gas 47 to be completely fluorinated. The halogenation in the second halogenation treatment step 31 generates silicon fluoride A48, excess hydrogen fluoride gas A41, and water vapor A42 as volatile components. These gases are sent to the gas separation step B33, where silicon fluoride A48 is separated. The hydrogen fluoride recovered by condensation is recycled as a halogenating agent.

[0084] The fluorination residue B49 from the second halogenation treatment process 31 is sent to the third halogenation treatment process 34. Here, the uranium in the fluorination residue is fluorinated to uranium hexafluoride by reacting with fluorine gas 50, and is volatilized. The generated gas is sent to the gas separation process C35, where the nuclear fuel material C51 and excess fluorine gas 52 are separated by the cold trap described in the first embodiment. The separated fluorine gas (excess fluorine gas 52) is recycled as a halogenation agent. The fluorination residue C53 is sent to the oxidation treatment process 36.

[0085] As in the first embodiment, in the oxidation treatment process 36, the fluoride residue C53 is reacted with steam 54 to convert the chemical form into an oxide. The obtained solid is sent to the vitrification process 37 as waste 55. Here, the waste 55 and the glass base material 56 are melted at high temperature, and then cooled and solidified to finally obtain a vitrified body 57.

[0086] According to this embodiment, not only can the same effects as those of Example 1 be obtained, but also, by using hydrogen fluoride as the halogenating agent, it is possible to obtain an effect that the halogenating agent and silicon fluoride can be easily separated during the process, and an effect that the reaction temperature can be increased in the halogenation step using hydrogen fluoride, thereby accelerating the reaction.

[0087] The present invention is not limited to the above-described embodiments, and includes various modified examples. For example, the above-described embodiments have been described in detail to clearly explain the present invention, and the present invention is not necessarily limited to those including all of the configurations described. In addition, it is possible to replace a part of the configuration of one embodiment with the configuration of another embodiment, and it is also possible to add the configuration of another embodiment to the configuration of one embodiment. In addition, it is possible to add, delete, or replace a part of the configuration of each embodiment with another configuration. [Explanation of symbols]

[0088] 1, 30...First halogenation treatment process, 2, 31...Second halogenation treatment process, 3, 33...Gas separation process B in the second halogenation treatment process, 4, 36...Oxidation treatment process, 5, 37...Vitrification process, 6, 32...Gas separation process A in the first halogenation treatment process, 10, 40...Fuel debris, 11...Excess fluorine gas A, 12...Oxygen gas A, 13...Silicon fluoride, 14...Excess fluorine gas B, 15...Oxygen gas B, 16, 46...Fluorination residue A, 17, 50...Fluorine gas, 18...Nuclear fuel material B, 19, 49...Fluorination residue B, 20, 54...Water vapor, 21, 55...Waste, 22, 56...Glass base material, 23, 57...Vitrified body, 24...Nuclear fuel material A, 34...Third halogenation treatment process, 35...Gas separation process C in the third halogenation treatment process, 41...Excess hydrogen fluoride gas A, 42...Water vapor A, 43...Silicon fluoride B, 44...Excess hydrogen fluoride gas B, 45...Water vapor B, 47...Hydrogen fluoride gas, 48...Silicon fluoride A, 51...Nuclear fuel material C, 52...Excess fluorine gas, 53...Fluorination residue C.

Claims

1. A method for treating fuel debris by vitrifying the fuel debris, comprising the steps of: The fuel debris is fluorinated in a halogenation treatment step to volatilize the nuclear fuel material, and the remaining fluoride residue is converted into an oxide. The oxide is then mixed with a glass base material to produce a vitrified body, The halogenation treatment step is carried out in multiple stages, The fuel debris is reacted with excess fluorine gas in a first halogenation treatment step, and silicon fluoride, excess fluorine gas B, oxygen gas B, and nuclear fuel material A are generated as volatile components by the halogenation in the first halogenation treatment step, and these are sent to a gas separation step A to separate only the nuclear fuel material A, On the other hand, the fluorinated residue A fluorinated in the first halogenation treatment step is sent to a second halogenation treatment step, in which it is reacted with fluorine gas, and the fluorinated residue A is halogenated in the second halogenation treatment step to generate nuclear fuel material B, excess fluorine gas A and oxygen gas A as volatile components, which are sent to a gas separation step B to separate only the nuclear fuel material B, The method for treating fuel debris further comprises: sending the fluorination residue B fluorinated in the second halogenation treatment step to an oxidation treatment step, in which the fluorination residue B is reacted with water vapor to convert its chemical form into an oxide, and sending the resulting solid as waste to a vitrification step, in which the waste and a glass base material are melted and then cooled and solidified to obtain a vitrified body.

2. A method for treating fuel debris according to claim 1, comprising:

4. A method for treating fuel debris, comprising the steps of: (a) providing an off-gas from the second halogenation treatment step and separating the nuclear fuel material from the off-gas;

3. A method for treating fuel debris according to claim 1 or 2, comprising: In the gas separation step A or the gas separation step B, UF 6 a cold trap for condensing and recovering said nuclear fuel material A or B, thereby separating only said nuclear fuel material A or B.

4. A method for treating fuel debris according to any one of claims 1 to 3, comprising: The temperature at which the halogenation is carried out in the first halogenation treatment step is set to 100° C. 6 The temperature of the halogenation treatment in the second halogenation treatment step is 350° C. or less at which UF is not generated, and 6 The method for treating fuel debris, wherein the temperature is 350°C or higher.

5. A method for treating fuel debris by vitrifying the fuel debris, comprising: The fuel debris is fluorinated in a halogenation treatment step to volatilize the nuclear fuel material, and the remaining fluoride residue is converted into an oxide. The oxide is then mixed with a glass base material to produce a vitrified body, The halogenation treatment step is carried out in multiple stages, The fuel debris is reacted with excess hydrogen fluoride gas A in a first halogenation treatment step, and silicon fluoride B, excess hydrogen fluoride gas B, and water vapor B are generated as volatile components by the halogenation in the first halogenation treatment step, and these are sent to a gas separation step A to separate only the silicon fluoride B, On the other hand, the fluoride residue A fluorinated in the first halogenation treatment step is sent to a second halogenation treatment step, in which it is reacted with hydrogen fluoride gas, and silicon fluoride A, excess hydrogen fluoride gas A, and water vapor A are generated as volatile components by the halogenation of the fluoride residue A in the second halogenation treatment step, and these are sent to a gas separation step B to separate only the silicon fluoride A, Furthermore, the fluorinated residue B fluorinated in the second halogenation treatment step is sent to a third halogenation treatment step, in which it is reacted with fluorine gas, and the fluorinated residue B is halogenated in the third halogenation treatment step to generate nuclear fuel material C and excess fluorine gas as volatile components, which are sent to a gas separation step C to separate only the nuclear fuel material C, The method for treating fuel debris further comprises: sending the fluorination residue C fluorinated in the third halogenation treatment step to an oxidation treatment step, in which the fluorination residue C is reacted with water vapor to convert its chemical form into an oxide, and sending the resulting solid as waste to a vitrification step, in which the waste and a glass base material are melted and then cooled and solidified to obtain a vitrified body.

6. A method for treating fuel debris according to claim 5, comprising the steps of:

4. A method for treating fuel debris, comprising the steps of: providing an off-gas from the second halogenation treatment step with a surplus fluorine gas; and separating the silicon fluoride A from the off-gas from the second halogenation treatment step.

7. A method for treating fuel debris according to claim 5 or 6, comprising the steps of: In the gas separation step A, only the silicon fluoride B is separated using a cold trap that condenses and recovers hydrogen fluoride and water vapor, and in the gas separation step C, 6 a cold trap for condensing and recovering the nuclear fuel material C, thereby separating only the nuclear fuel material C.

8. A method for treating fuel debris according to any one of claims 5 to 7, comprising the steps of:

2. The method for treating fuel debris, wherein the halogenation treatment temperature in the first halogenation treatment step is 600° C. or lower.

Citation Information

Patent Citations

  • Reprocessing method by fluoride volatilization method using solid-gas separation method

    JP2006046967A

  • Method of processing damaged or molten nuclear fuel

    JP2014029319A

  • Recovery method of nuclear fuel material

    JP2016048209A

  • Actinide separation method and actinide separation apparatus