Method for manufacturing a semiconductor device

The method enhances semiconductor device performance by forming a metal oxide film under controlled atmospheric conditions, addressing issues of electrical stability, power consumption, and manufacturing efficiency, resulting in high-purity devices with low impurity concentrations and defect levels.

JP7588668B2Active Publication Date: 2024-11-22SEMICON ENERGY LAB CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023016945
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-11-30
Filing Date
2023-02-07
Publication Date
2024-11-22
Estimated Expiration
2037-08-01

AI Technical Summary

Technical Problem

Existing semiconductor devices face challenges in achieving good electrical characteristics, stable performance, low power consumption, high reliability, and high productivity, as well as high yield in manufacturing.

Method used

A method for manufacturing semiconductor devices involving the formation of a metal oxide film on an insulating film, performed under an atmosphere with a lower partial pressure of water vapor, at specific temperature and time ranges, using a sputtering method with controlled atomic ratios of In, M, and Zn, and ensuring minimal impurities such as hydrogen and moisture at the film interfaces.

Benefits of technology

The method results in semiconductor devices with improved electrical characteristics, stable performance, low power consumption, high reliability, and high manufacturing yield, with reduced impurity concentration and defect levels in the metal oxide film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588668000003
    Figure 0007588668000003
  • Figure 0007588668000004
    Figure 0007588668000004
  • Figure 0007588668000005
    Figure 0007588668000005
Patent Text Reader

Abstract

To provide a semiconductor device with good electrical characteristics. To provide a semiconductor device with stable electrical characteristics. A method for manufacturing a semiconductor device with high yield is provided. The method includes a first step of forming an insulating film on a substrate, and a second step of transporting the substrate in an atmospheric environment. a third step of heating the insulating film, and a fourth step of forming a metal oxide film. The third and fourth steps are carried out consistently in an atmosphere having a water vapor partial pressure lower than that of the atmosphere. This is carried out.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to a semiconductor device including an oxide semiconductor film. The embodiment also relates to a display device having the semiconductor device.

[0002] Note that one embodiment of the present invention is not limited to the above technical fields. The technical field of one embodiment of the present invention is a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, The present invention relates to a driving method thereof or a manufacturing method thereof.

[0003] In this specification and the like, a semiconductor device is a device that can function by utilizing semiconductor characteristics. Refers to devices in general. Semiconductor elements such as transistors, semiconductor circuits, computing devices, memory The device is one aspect of a semiconductor device. Optical devices, power generation devices (including thin-film solar cells, organic thin-film solar cells, etc.), and electronic devices The device may include a semiconductor device. [Background technology]

[0004] In recent years, metal oxides have been attracting attention as materials for the semiconductor layer of transistors. For example, a transistor using an amorphous oxide containing indium, gallium, and zinc is known. (See Patent Document 1.)

[0005] Metal oxides that can be used for the semiconductor layer can be formed by using a sputtering method or the like. Therefore, it can be used for the semiconductor layer of a transistor that constitutes a large display device. It is possible to use some of the production facilities for amorphous silicon transistors by improving them. This reduces capital investment. In addition, oxide-based transistors have a high field effect. Since the organic EL display device has a high mobility, it is possible to realize a highly functional display device in which a driving circuit is integrally formed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-165528 A Summary of the Invention [Problem to be solved by the invention]

[0007] An object of one embodiment of the present invention is to provide a semiconductor device with favorable electrical characteristics. Another object of the present invention is to provide a semiconductor device having stable electrical characteristics. Another object of the present invention is to provide a semiconductor device having low resistance and high reliability. Another object of the present invention is to provide a method for manufacturing a semiconductor device with high productivity. Another object of the present invention is to provide a method for manufacturing a semiconductor device with high yield. This is one of the challenges.

[0008] The description of these problems does not preclude the existence of other problems. It is not necessary to solve all of these problems. Problems other than those mentioned above are not necessarily solved. It is possible to extract such information from descriptions in the fine print, etc. [Means for solving the problem]

[0009] One embodiment of the present invention is a method for manufacturing a semiconductor device, comprising: a first step of forming an insulating film over a substrate; a second step of transporting the substrate in an air atmosphere; and a third step of heating the insulating film. and a fourth step of forming a metal oxide film on the insulating film. The process is characterized in that it is consistently carried out in an atmosphere in which the partial pressure of water vapor is less than atmospheric.

[0010] In the above, the third step is carried out at a temperature range of 100° C. or more and 500° C. or less, Moreover, the treatment time is preferably within the range of 1 minute to 120 minutes.

[0011] In the above, the third step is carried out under a pressure of 1×10 -7 Pa or more 1×10 -3 Pa It is preferable to carry out the process below.

[0012] In the above, the metal oxide film is preferably formed by a sputtering method. It is.

[0013] In the above, the metal oxide film is formed at a temperature between room temperature and 200° C. is preferred.

[0014] In the above, the metal oxide film is formed at a temperature between room temperature and 130° C. is preferred.

[0015] In the above, the metal oxide film is preferably formed at a temperature at which heating is not intentionally performed. I wish.

[0016] In the above, the metal oxide film is an In-M-Zn oxide (M is Ga, Al, Y, In this case, it is preferable to deposit the film using a target containing In, M, and Sn. The atomic ratio of Zn is preferably In:M:Zn=4:2:4.1 or close to it. Or, the atomic ratio of In, M, and Zn is In:M:Zn=5:1:7 or Preferably, it is in the vicinity. Effect of the Invention

[0017] According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. A semiconductor device having stable characteristics can be provided. Alternatively, a semiconductor device with low power consumption can be provided. Alternatively, a semiconductor device with high reliability can be provided. Alternatively, a semiconductor device with high productivity can be manufactured. Alternatively, a method for manufacturing a semiconductor device with high yield can be provided.

[0018] Note that one embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the descriptions in the specification, etc. [Brief description of the drawings]

[0019] [Figure 1] 1 is a flowchart illustrating a method for manufacturing a semiconductor device. [Diagram 2] FIG. [Diagram 3] FIG. [Figure 4] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device. [Diagram 5] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device. [Figure 6] 1 is a cross-sectional view illustrating a semiconductor device. [Figure 7] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device. [Figure 8] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device. [Figure 9] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device. [Figure 10] FIG. 2 is a diagram for explaining the range of the atomic ratio of the metal oxide according to the present invention. [Figure 11] FIG. 2 is a diagram illustrating the measurement results of an XRD spectrum. [Figure 12] TEM image of a sample and a diagram explaining an electron beam diffraction pattern. [Figure 13] FIG. 1 is a diagram illustrating EDX mapping of a sample. [Figure 14]FIG. 1 is a top view illustrating one embodiment of a display device. [Figure 15] FIG. 1 is a cross-sectional view showing one embodiment of a display device. [Figure 16] FIG. 1 is a cross-sectional view showing one embodiment of a display device. [Figure 17] FIG. 1 is a cross-sectional view showing one embodiment of a display device. [Figure 18] FIG. 1 is a cross-sectional view showing one embodiment of a display device. [Figure 19] FIG. 1 is a cross-sectional view showing one embodiment of a display device. [Figure 20] 1A and 1B are a block diagram and a circuit diagram illustrating a display device. [Figure 21] FIG. 2 is a diagram illustrating a display module. [Figure 22] 1A to 1C are diagrams illustrating electronic devices. [Diagram 23] 1A to 1C are diagrams illustrating electronic devices. [Figure 24] TDS analysis results. [Diagram 25] TDS analysis results. [Figure 26] Transistor Id-Vg characteristics. [Figure 27] Transistor Id-Vg characteristics. [Figure 28] Transistor Id-Vg characteristics. [Figure 29] Transistor Id-Vg characteristics. [Diagram 30] Transistor Id-Vg characteristics. [Diagram 31] Transistor Id-Vg characteristics. [Diagram 32] Transistor Id-Vg characteristics. [Diagram 33] Transistor Id-Vg characteristics. [Diagram 34] FIG. 4 is a diagram for explaining measurement positions of film density. [Diagram 35] Measurement results of film density of metal oxide film. [Diagram 36] FIG. 4 is a diagram for explaining the measurement positions of the energy gap. [Figure 37] Measurement results of the energy gap of a metal oxide film. [Figure 38] FIG. [Figure 39] FIG. 2 is a circuit diagram of a pixel of a display device. [Diagram 40] A model diagram of the configuration used in the simulation and a timing chart. [Diagram 41] Simulation results of field-effect mobility and write time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the embodiments will be described with reference to the drawings. The present invention may be embodied in various different forms without departing from its spirit and scope. It will be readily understood by those skilled in the art that various modifications and changes may be made to the embodiments and details of the present invention. However, the present invention should not be construed as being limited to the description of the following embodiments.

[0021] Also, in the drawings, the size, layer thickness, or area are exaggerated for clarity. Therefore, the scale is not necessarily limited to that shown in the drawings. The drawings are merely schematic illustrations and are not limited to the shapes or values ​​shown in the drawings.

[0022] In addition, the ordinal numbers "first," "second," and "third" used in this specification refer to the components of the It should be noted that this is added to avoid confusion and is not intended to limit the numbers.

[0023] In addition, in this specification, the words "above" and "below" indicating the position of the components are used. The positional relationship is used for convenience in describing the drawings. The relationship changes depending on the direction in which each component is depicted. The above words and phrases are not limited to those used above, but can be rephrased appropriately depending on the situation.

[0024] In this specification, a transistor includes a gate, a drain, and a source. The drain terminal is a diode that has at least three terminals. Between the drain region or drain electrode and the source (source terminal, source region or source electrode) A channel region is provided between the source and drain, and a current flows between the source and drain through the channel region. In this specification and the like, the channel region is a region through which a current mainly flows. This refers to the area in which the fluid flows.

[0025] In addition, the functions of the source and drain may differ depending on whether transistors of different polarities are used or the circuit In operation, when the direction of the current changes, the positions may be reversed. In the specification, the terms source and drain may be used interchangeably. do.

[0026] In addition, in this specification, "electrically connected" means "something that has some kind of electrical effect." This includes cases where the device is connected via a "device having some electrical function." "of" is not subject to any particular restrictions as long as it enables the transmission and reception of electrical signals between connected objects. For example, "something that has an electrical effect" includes electrodes, wiring, and transistors. These devices have various functions such as switching elements, resistor elements, inductors, capacitors, etc. This includes elements such as:

[0027] In addition, in this specification, "parallel" means that two straight lines are at an angle of -10° or more and 10° or less. Therefore, it includes the case where the angle is between -5° and 5°. "Perpendicular" means that two straight lines are arranged at an angle of 80° or more and 100° or less. Therefore, this also includes cases where the angle is between 85° and 95°.

[0028] In addition, in this specification and the like, the terms "film" and "layer" are interchangeable. For example, the term "conductive layer" can be changed to the term "conductive film." Alternatively, for example, the term "insulating film" may be changed to "insulating layer." It may be possible to change the term to:

[0029] In this specification and the like, unless otherwise specified, the off-state current refers to the current that occurs when a transistor is off. This refers to the drain current when the device is in a non-conducting state (also called a cut-off state). Unless otherwise specified, for n-channel transistors, V is the voltage between the gate and source gs is the threshold voltage V th In a p-channel transistor, the gate and The voltage Vgs between the th For example, n-channel The off-state current of a transistor is the voltage between the gate and source, Vgs, that is, the threshold voltage, V t h This may refer to the drain current when the input voltage is lower than

[0030] The off-state current of a transistor may depend on Vgs. The off-state current is I or less if there exists a Vgs value at which the off-state current of the transistor is I or less. The off-state current of a transistor is the current that flows through it in the off-state at a given Vgs. , an off-state at Vgs within a given range or a sufficiently reduced off-current is obtained. In some cases, it may refer to the off-state current at Vgs.

[0031] As an example, the threshold voltage V th When Vgs is 0.5V, the drain The current is 1×10 -9 A, and the drain current at Vgs of 0.1 V is 1×10 -1 3 A, and the drain current at Vgs -0.5 V is 1×10 -19 A and Vg The drain current at s = -0.8 V is 1 × 10 -22 A n-channel transistor The drain current of the transistor is as follows when Vgs is -0.5V: , or 1×10 when Vgs is in the range of -0.5V to -0.8V -19 A or below Therefore, the off-state current of the transistor is 1×10 -19 There are cases where it is said to be A or lower. The drain current of the transistor is 1×10 -22 A or less Vgs exists. Therefore, the off-state current of the transistor is 1×10 -22 It may be said that it is below A.

[0032] In this specification, the off-state current of a transistor having a channel width W is expressed as It is sometimes expressed as the current value that flows per watt. Also, for a given channel width (for example, 1 μm), In the latter case, the unit of the off-state current is current / length. It may be expressed in units with an element (e.g., A / μm).

[0033] The off-state current of a transistor may depend on temperature. Unless otherwise specified, the operating temperature is room temperature, 60°C, 85°C, 95°C, or 125°C. Or, the reliability of a semiconductor device including the transistor may be guaranteed. The temperature at which the transistor is certified, or the temperature at which a semiconductor device or the like that contains the transistor is used (e.g. For example, the off-state current at any one of temperatures from 5° C. to 35° C. The off-state current of the transistor is I or less at room temperature, 60°C, 85°C, 95°C, 125°C, The temperature at which the reliability of a semiconductor device including the transistor is guaranteed, or The temperature at which the semiconductor device containing the transistor is used (for example, any one of 5°C to 35°C) (temperature), there exists a value of Vgs at which the off-state current of the transistor is equal to or less than I. There are cases where it is pointed out.

[0034] The off-state current of a transistor may depend on the voltage Vds between the drain and source In this specification, unless otherwise specified, the off-state current is measured when Vds is 0.1 V, 0.8 V, 1V, 1.2V, 1.8V, 2.5V, 3V, 3.3V, 10V, 12V, 16V, and In some cases, it indicates the off-state current at 20 V. In other cases, it indicates the off-state current at 20 V. Vds that guarantees the reliability of semiconductor devices, or semiconductor devices including the transistor The term may refer to the off-state current at Vds used in the transistor off-state. The current is equal to or less than I when Vds is 0.1V, 0.8V, 1V, 1.2V, 1.8V, 2.5V, 3V, 3.3V, 10V, 12V, 16V, 20V, transistors included Vds that guarantees the reliability of the semiconductor device in which the transistor is used, or Vds used in semiconductor devices, etc., where the off-state current of the transistor is I or less This may refer to the existence of a gs value.

[0035] In the above description of the off-state current, the drain may be read as the source. The current may also refer to the current through the source when the transistor is in the off state.

[0036] In this specification and the like, the term "leak current" may be used to mean the same thing as the "off current." In this specification, the off-state current refers to, for example, the current flowing when a transistor is in an off state. , may refer to the current flowing between the source and drain.

[0037] In this specification, the threshold voltage of a transistor is the threshold voltage of a transistor. This refers to the gate voltage (Vg) when a gate is formed. Specifically, it refers to the threshold voltage of a transistor. Voltage is plotted on the horizontal axis as gate voltage (Vg) and on the vertical axis as the square root of drain current (Id). The line obtained by extrapolating the tangent line with the maximum slope in the simulated curve (Vg-√Id characteristics) is , the gate voltage (Vg Alternatively, the threshold voltage of a transistor can be expressed as the channel length L and the The channel width is W, and the value of Id[A]×L[μm] / W[μm] is 1×10 -9 [A] Sometimes it refers to the gate voltage (Vg) applied to the device.

[0038] In addition, even when the term "semiconductor" is used in this specification, for example, If the electrical conductivity is low enough, the material may have the properties of an insulator. The boundary between "insulators" and "insulators" is unclear, and it may not be possible to strictly distinguish them. In the above, the terms "semiconductor" and "insulator" may be interchangeable.

[0039] In addition, even when the term "semiconductor" is used in this specification, for example, When it is extremely high, it may have the characteristics of a "conductor". Also, the boundary between "semiconductor" and " "conductor" is ambiguous, and there may be cases where they cannot be strictly distinguished. Therefore, the "semiconductor" described in this specification and the "conductor" may be interchangeable with each other .

[0040] In addition, regarding this specification, etc., In:Ga:Zn = 4:2:3 or in the vicinity thereof means that when In is 4 with respect to the total number of atoms, Ga is 1 or more and 3 or less (1 ≤ Ga ≤ 3), and Zn is 2 or more and 4 or less (2 ≤ Zn ≤ 4). Also, In:Ga:Zn = 5:1:6 or in the vicinity thereof means that when In is 5 with respect to the total number of atoms, Ga is greater than 0.1 and 2 or less ( 0.1 < Ga ≤ 2), and Zn is 5 or more and 7 or less (5 ≤ Zn ≤ 7). Also, In: Ga:Zn = 1:1:1 or in the vicinity thereof means that when In is 1 with respect to the total number of atoms, Ga is greater than 0.1 and 2 or less (0.1 < Ga ≤ 2), and Zn is greater than 0.1 and 2 or less (0.1 < Zn ≤ 2).

[0041] In this specification, etc., "metal oxide" is an oxide of a metal in a broad sense. Metal oxides are classified into oxide insulators, oxide conductors (including transparent oxide conductors ), oxide semiconductors (also referred to as Oxide Semiconductor or simply OS) and so on. For example, when a metal oxide is used for the active layer of a transistor, the metal oxide may be referred to as an oxide semiconductor. That is, when a metal oxide has at least one of an amplification effect, a rectification effect , and a switching effect, the metal oxide is called a metal oxide semiconductor (metal oxide semiconductor), abbreviated as OS for short . In addition, when describing OS FET, it is possible to use a metal oxide or an oxide semiconductor. In other words, it is a transistor having a conductor.

[0042] In the present specification and the like, metal oxides having nitrogen are also referred to as metal oxides. Metal oxides containing nitrogen are also called metal oxynitrides (MEs). It may also be called tal oxynitride.

[0043] In the present specification, CAAC (c-axis aligned crystal l), and CAC (Cloud-Aligned Composite) CAAC represents an example of a crystal structure, and CAC represents a function or a material configuration. Shows an example.

[0044] In the present specification and the like, CAC-OS or CAC-metal oxide means A part of the material has a conductive function and a part of the material has an insulating function, and the whole material has It functions as a semiconductor. When de is used in the active layer of a transistor, the conductive function is to transport electrons (or The function of insulating is to allow the flow of electrons (carriers) and not allow the flow of electrons (electrons). The conductive function and the insulating function work in a complementary manner, The switching function (the function to turn on / off) can be set to CAC-OS or CAC-metal. It can be added to CAC-OS or CAC-metal oxide. By separating the functions of each, it is possible to maximize the functions of both. can.

[0045] In the present specification and the like, CAC-OS or CAC-metal oxide is The conductive region has the above-mentioned conductive function and the insulating function. The conductive region has the insulating function described above. The regions may be separated at the nanoparticle level. The conductive regions may be unevenly distributed in the material. They may be observed connected in a dot-like pattern.

[0046] In addition, in the CAC-OS or CAC-metal oxide, a conductive region and The insulating regions are each 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm. They may be dispersed in the material at sizes of less than one millimeter.

[0047] In addition, CAC-OS or CAC-metal oxide has different band gaps For example, CAC-OS or CAC-metal ox The ide consists of a wide gap component due to the insulating region and a conductive region. In this configuration, when the carrier flows, In addition, carriers mainly flow in the narrow gap component. The component with a gap acts complementary to the component with a wide gap to produce a narrow gap. Carriers also flow to the wide gap component in conjunction with the component with a large gap. CAC-OS or CAC-metal oxide is used for the channel region of a transistor. When the transistor is in the on-state, the current drive capability is high, i.e., the on-current is large, and Therefore, a high field effect mobility can be obtained.

[0048] That is, CAC-OS or CAC-metal oxide is a matrix composite. matrix composite, or metal matrix composite It can also be called a composite matrix.

[0049] An example of the crystal structure of a metal oxide will be described. In the following, In-Ga-Zn oxide Sputtering was performed using a Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]). A metal oxide film formed by the ring method will be described as an example. Metal oxide formed by sputtering at a plate temperature of 100°C to 130°C is called sIGZO, and the above target is used, with the substrate temperature at room temperature (RT), Metal oxides formed by sputtering are called tIGZO. For example, sIGZ O is either nc (nano crystal) or CAAC or both. In addition, tIGZO has a crystal structure of nc. RT) includes temperatures at which the substrate is not intentionally heated.

[0050] (Embodiment 1) In this embodiment, a manufacturing method of a semiconductor device according to one embodiment of the present invention will be described.

[0051] One aspect of the present invention includes a first step of forming an insulating film on a substrate, and a second step of transferring the substrate in an air atmosphere. a second step of transferring the insulating film, a third step of heating the insulating film, and a fourth step of forming a metal oxide film. and a step of: The present invention relates to a method for manufacturing a semiconductor device, the method being characterized in that the steps of:

[0052] When a metal oxide film that functions as an active layer of a transistor is formed by laminating it on an insulating film, In this case, impurities at the interface between the insulating film and the metal oxide film become a problem.

[0053] Impurities adhere to or are mixed into the interface between the insulating film and the metal oxide film, resulting in a semiconductor device Therefore, hydrogen is not allowed to exist at the interface between the insulating film and the metal oxide film. The fewer impurities such as moisture, the more preferable.

[0054] Therefore, in one aspect of the present invention, a first step of forming an insulating film on a substrate and a second step of forming an insulating film on a substrate are provided. A second step of transporting the substrate is performed, followed by a third step of heating the insulating film and a third step of and a fourth step of forming an oxide film in an atmosphere having a water vapor partial pressure lower than that of the atmosphere; and For example, the third and fourth steps are performed in the same manner. These steps can be carried out consecutively without exposure to the atmosphere between them.

[0055] The second step can be carried out, for example, in an air atmosphere. In this case, insulation is required during transportation of the substrate. Hydrogen and moisture contained in the atmosphere may be adsorbed on the surface of the coating. In one embodiment, the insulating film is heated in the apparatus in a third step, and the insulating film is adsorbed on the insulating film surface. Furthermore, after the heat treatment, the partial pressure of water vapor becomes higher than that of the atmosphere. Since it is possible to deposit metal oxide films consistently in a small atmosphere, the insulating film and the metal This prevents impurities from adhering to or being mixed into the metal oxide film interfaces, and keeps these interfaces clean. In addition, hydrogen, moisture, etc. that may be contained in the insulating film can be removed. In addition, it is possible to prevent hydrogen, moisture, and the like from being mixed into the metal oxide film.

[0056] In addition, an atmosphere in which the partial pressure of water vapor is lower than that of the atmosphere means an atmosphere at least at a reduced pressure lower than that of the atmosphere. Specifically, the pressure is low or medium vacuum (several hundred Pa to 0.1 Pa). , or high or ultra-high vacuum (0.1 Pa to 1×10 -7 Pa).

[0057] In particular, the pressure is 1×10 -7 Pa or more 1×10 -3 It is preferable to carry out the heat treatment at a temperature of 0.1 Pa or less. I wish.

[0058] In addition, by adopting the above-mentioned embodiment, the metal oxide film has a low impurity concentration and a low defect level density. In this way, a thin oxide semiconductor film can be obtained.

[0059] As the metal oxide film, a metal oxide film having a low impurity concentration and a low defect level density is used. By using this, a transistor having excellent electrical characteristics can be manufactured. In this case, the low impurity concentration and low defect level density (including few oxygen vacancies) are considered to be the This is called high-purity intrinsic or substantially high-purity intrinsic. The impurities in the metal oxide film are as follows: Representative examples include water and hydrogen. The reduction or removal of water and hydrogen is sometimes referred to as dehydration or dehydrogenation. The addition of oxygen to a metal oxide film is sometimes referred to as oxygenation. A state in which there is excess oxygen compared to the stoichiometric composition is sometimes referred to as a hyperoxygenated state.

[0060] High-purity intrinsic or substantially high-purity intrinsic metal oxide films have fewer carrier generation sources Therefore, the carrier density can be reduced. The transistors formed have electrical characteristics in which the threshold voltage is negative (normally on and Also, high purity intrinsic or substantially high purity intrinsic metals are rarely used. Since the oxide film has a low defect state density, the trap state density may also be low. High-purity intrinsic or substantially high-purity intrinsic metal oxide films have significantly lower off-state currents, Channel width is 1×10 6 Even if the device has a channel length L of 10 μm, the source electrode and When the voltage between the drain electrodes (drain voltage) is in the range of 1V to 10V, the off-state current is Below the measurement limit of the semiconductor parameter analyzer, i.e. 1×10 -13 Characteristics below A can be obtained.

[0061] <1-1. Manufacturing method of semiconductor device> Next, a manufacturing method of a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. FIG. 1 is a flowchart illustrating a method for manufacturing a semiconductor device of one embodiment of the present invention.

[0062] [First step: Deposition of insulating film] The first step is to form an insulating film on a substrate (FIG. 1, step S101).

[0063] For insulating films, sputtering, CVD, evaporation, pulsed laser deposition (PLD) The insulating film can be formed by appropriately using a deposition method, a printing method, a coating method, or the like. For example, a single layer or a stacked layer of an oxide insulating film or a nitride insulating film can be formed. In order to improve the interface characteristics with the metal oxide film, the insulating film is preferably made of at least a metal oxide. The region in contact with the film is preferably formed of an oxide insulating film. By using an oxide insulating film that releases oxygen, the heat treatment after the formation of the metal oxide film can be performed without any problems. This makes it possible for oxygen contained in the insulating film to move to the metal oxide film.

[0064] The insulating film may be, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, or silicon nitride. ZnO, aluminum oxide, hafnium oxide, gallium oxide, Ga-Zn oxide, etc. It may be used in the form of a single layer or a multilayer.

[0065] [Second step: Transfer of substrate] The second step is to transport the substrate on which the insulating film has been formed to an apparatus for forming a metal oxide film. (FIG. 1, step S102).

[0066] The substrate can be transported in an atmosphere having a water vapor partial pressure less than that of the atmosphere. By transporting the substrate in the air, the device This allows for greater freedom in installation method (layout).

[0067] The substrate transport process also includes a waiting state for the next process. In the waiting state, the substrate is placed in an air atmosphere. Alternatively, the substrate can be stored in an atmosphere where the partial pressure of water vapor is less than that of air. By storing the substrates in air, the equipment can be simplified. When using such a substrate, it is preferable to store the substrate under an air atmosphere.

[0068] In the second step, moisture, hydrogen, and the like may be adsorbed onto the surface of the insulating film.

[0069] [Third step: Heat treatment] The third step is to heat the insulating film (FIG. 1, step S103).

[0070] During the transportation of the substrate, moisture and hydrogen may be adsorbed on the surface of the insulating film. When a metal oxide film is formed on an insulating film, water, hydrogen, etc. may be present at the interface between the metal oxide film and the insulating film. Therefore, in the third step, before the deposition of the metal oxide film, the water vapor content is reduced. The heat treatment is performed in an atmosphere with a pressure lower than that of the atmosphere to remove the water and hydrogen adsorbed on the insulating film surface. Remove.

[0071] The temperature to which the insulating film is heated is set to a temperature at which water or hydrogen can be desorbed from the insulating film surface. On the other hand, if the heating temperature is too high, the oxygen contained in the insulating film is released, This may result in a decrease in the amount of oxygen that can be supplied to the metal oxide film.

[0072] The temperature to which the insulating film is heated is 100° C. or higher and 500° C. or lower, preferably 100° C. or higher. The temperature is preferably 450° C. or lower, more preferably 200° C. or higher and 400° C. or lower. The treatment time of the step is from 1 minute to 120 minutes, preferably from 2 minutes to 60 minutes. More preferably, the heating time is from 3 minutes to 10 minutes. Since it affects the throughput of the deposition equipment, it is important for the operator to select the optimal time appropriately. In addition, when heating at a high temperature, the desorption of oxygen from the insulating film is suppressed. The treatment time is preferably 10 minutes or less.

[0073] The insulating film is preferably heated in an atmosphere in which the water vapor pressure is lower than that of the atmosphere. This makes it possible to efficiently remove water and hydrogen adsorbed on the surface of the insulating film. For example, it is preferable to heat the material under a pressure lower than atmospheric pressure (reduced pressure atmosphere). The higher the value, the more efficiently the water and hydrogen adsorbed on the surface of the insulating film can be desorbed. For example, when inserting a substrate into a chamber where heat treatment is performed (i.e., immediately before inserting the substrate), pressure, or the pressure immediately after inserting the board) is 1×10 -7 Pa or more 1×10 -3 Pa or less, preferably 1×10 -6 Pa or more 1×10 -4 Pa or less. During the heat treatment, evacuation may or may not be performed.

[0074] [Fourth step: forming a metal oxide film] The fourth step is to form a metal oxide film on the insulating film (FIG. 1, step S10 4).

[0075] The metal oxide film contains In, M (wherein M is Ga, Al, Y, or Sn), and Zn. It is preferable that the metal oxide film has a region in which the atomic ratio of In is greater than the atomic ratio of M. As an example, it is preferable to set the ratio of the number of In, M, and Zn atoms in the metal oxide film to I n:M:Zn=4:2:3 or nearby, or In:M:Zn=5:1:7 or It is preferable to set it in the vicinity of that.

[0076] In addition, the gas used in forming the metal oxide film is an inert gas (typically argon). ), and oxygen gas may be used.

[0077] For example, when forming a metal oxide film, either argon gas or oxygen gas is used. In addition, the ratio of the oxygen gas flow rate to the total gas flow rate when forming a metal oxide film (oxygen The ratio of the flow rate of the oxygen to the oxygen concentration (also called the oxygen flow rate ratio) is 0% or more and 30% or less, preferably 5% or more and 15% or less. By setting the oxygen flow rate ratio as described above, the crystallinity of the metal oxide film can be reduced. In addition, by setting the above-mentioned oxygen flow rate ratio, the material composition of the metal oxide film is changed to the CAC-OS It can be said that:

[0078] Alternatively, the oxygen flow rate ratio when forming a metal oxide film is greater than 30% and less than 100%. Preferably, the ratio is 50% or more and 100% or less, and more preferably, 70% or more and 100% or less. By setting the oxygen flow rate ratio as described above, the crystallinity of the metal oxide film can be increased. Cut.

[0079] The substrate temperature during the formation of the metal oxide film is from room temperature (25°C) to 200°C. The substrate temperature is preferably from room temperature to 130° C. By setting the substrate temperature in the above range, When a laminated glass substrate is used, bending or distortion of the substrate can be suppressed.

[0080] The metal oxide film may have a laminated structure. In this case, the first metal oxide film and the second metal oxide film are By making the metal oxide films of each layer approximately the same composition, the same sputtering target can be used to form the layers. This allows the manufacturing cost to be reduced. When using a ferroelectric film, the first metal oxide film and the second metal oxide film are consistently formed in a vacuum in the same film forming apparatus. Since a first metal oxide film and a second metal oxide film can be formed, This can prevent impurities from being introduced into the interface.

[0081] The third and fourth steps are carried out in an atmosphere in which the partial pressure of water vapor is lower than that of the atmosphere. The process is carried out consistently in the order of the first step, the second step, the third step, and the fourth step. It can be done.

[0082] <1-2. Example of film formation equipment configuration> Here, the configuration of a film formation apparatus that can be used in the manufacturing method of a semiconductor device of one embodiment of the present invention will be described. An example will be described with reference to FIGS.

[0083] By using the deposition apparatus shown in FIG. 2 and FIG. 3, the interface between the insulating film and the metal oxide film and the metal It is possible to reduce impurities (especially hydrogen and water) that may enter the oxide film.

[0084] FIG. 2 is a schematic top view of a single-wafer multi-chamber film forming apparatus 4000. As shown in FIG. The film forming apparatus 4000 includes a cassette port 4101 for accommodating a substrate and a and an atmosphere-side substrate supply chamber 4001 having an alignment port 4102 for performing alignment. The substrate is loaded from the supply chamber 4001 to the atmospheric substrate transfer chamber 4002, A load lock chamber 4 for switching the pressure in the chamber from atmospheric pressure to reduced pressure or from reduced pressure to atmospheric pressure. 003a, the substrate is removed, and the pressure in the chamber is reduced from reduced pressure to atmospheric pressure, or reduced from atmospheric pressure to atmospheric pressure. and an unload lock chamber 4003b for switching to a vacuum. 04, a substrate heating chamber 4005 for heating the substrate, and a film forming chamber in which a target is placed and a film is formed. The chamber 4006a, the chamber 4006b, and the chamber 4006c.

[0085] As shown in FIG. 2, the cassette port 4101 has a plurality of ports (three ports in FIG. 2). It is okay to do so.

[0086] The atmospheric substrate transfer chamber 4002 includes a load lock chamber 4003a and an unload lock The load lock chamber 4003a and the unload lock chamber 4003b are connected to each other. The transfer chamber 4004 is connected to a substrate heating chamber 4005 and a film forming chamber 400. Connect to 6a, 4006b, and 4006c.

[0087] A gate valve 4104 is provided at the connection between the chambers, and the atmosphere side substrate supply chamber 4 Except for the atmospheric side substrate transfer chamber 4001 and the atmospheric side substrate transfer chamber 4002, each chamber can be independently maintained in a vacuum state. The atmospheric substrate transfer chamber 4002 and the transfer chamber 4004 are connected to a transfer robot 4103. and capable of transporting a glass substrate.

[0088] In addition, it is preferable that the substrate heating chamber 4005 also serves as a plasma processing chamber. Since the substrate can be transported between processes without being exposed to the atmosphere, It is possible to suppress the adsorption of pure substances. In addition, the order of film formation and heat treatment can be freely constructed. In addition, the transfer chamber, the film formation chamber, the load lock chamber, the unload lock chamber, and the substrate processing chamber can be The number of heat chambers is not limited to the above number, but can be set to an optimal number according to the installation space and process conditions. can be provided.

[0089] Next, the dashed lines A1-A2, B1-B2, and B2-B of the film forming apparatus 4000 shown in FIG. The cross sections corresponding to the cross section of 3 are shown in Figures 3(A), (B), and (C), respectively.

[0090] FIG. 3A is a cross-sectional view of the substrate heating chamber 4005 and the transfer chamber 4004. The substrate heating chamber 4005 shown includes multiple heating stages 4105 capable of housing substrates. Yes.

[0091] In FIG. 3(A), the heating stage 4105 is shown to have a seven-stage configuration. However, the present invention is not limited to this, and may be configured with 1 to 7 stages or 8 or more stages. By increasing the number of stages in the 4105, multiple substrates can be heated at the same time, improving productivity. In addition, the substrate heating chamber 4005 is connected to a vacuum pump 4200 via a valve. The vacuum pump 4200 may be, for example, a dry pump or a mechanical pump. A booster pump or the like can be used.

[0092] In addition, examples of heating mechanisms that can be used in the substrate heating chamber 4005 include resistance heating. Alternatively, the heating mechanism may be a mechanism that uses a medium such as a heated gas to heat the device. The heating mechanism may be a device that heats the device by thermal conduction or thermal radiation. For example, GRTA (G as Rapid Thermal Anneal), LRTA(Lamp Rapid Thermal Anneal) and other RTA (Rapid Thermal Anneal) eal) can be used. LRTA can be used with halogen lamps, metal halide lamps, Xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure mercury lamp The object to be treated is heated by radiating light (electromagnetic waves) emitted from lamps such as the following: Heat treatment is performed using high-temperature gas, preferably an inert gas.

[0093] The substrate heating chamber 4005 is connected to a refiner 43 via a mass flow controller 4300. The mass flow controller 4300 and the refiner 4301 are connected to the gas Although the number of the types is equal to the number of types, only one is shown for simplicity. The gas used has a dew point of -80°C or less, preferably -100°C or less. For example, oxygen gas, nitrogen gas, and rare gas (such as argon gas) are used.

[0094] The transfer chamber 4004 has a transfer robot 4103. The transfer robot 4103 has a plurality of The substrate transport apparatus has a number of movable parts and an arm that holds the substrate, and is capable of transporting the substrate to each chamber. The transfer chamber 4004 is connected to a vacuum pump 4200 and a cryopump 420 via valves. With this configuration, the transfer chamber 4004 is connected to a low pressure Use the Vacuum Pump 4200 to create a vacuum or medium vacuum (several hundred Pa to about 0.1 Pa). The vacuum is evacuated, and the valve can be switched to change the vacuum from medium to high or ultra-high (0.1 Pa to 1×1 0 -7 The pressure is evacuated to a temperature of about 100 Pa using the cryopump 4201.

[0095] In addition, for example, two or more cryopumps 4201 are connected in parallel to the transfer chamber 4004. With this configuration, even if one cryopump is in regeneration, Even if the amount of the cryopump is increased, the remaining cryopump can still be used to pump the remaining cryopumps. Cryopump refers to the process of releasing molecules (or atoms) stored in the cryopump. If the Lyopump accumulates too many molecules (or atoms), its pumping capacity will decrease. Regeneration occurs periodically.

[0096] FIG. 3B shows the film forming chamber 4006b, the transfer chamber 4004, and the load lock chamber 4003a. The details of the film formation chamber (sputtering chamber) will be described with reference to FIG. do.

[0097] The film-forming chamber 4006b shown in FIG. 3(B) includes a target 4106, an adhesion prevention plate 4107, and a substrate. The substrate stage 4108 has a substrate 41 The substrate stage 4108 holds the substrate 4109, although not shown. A substrate holding mechanism for holding the substrate 4109 and a back heater for heating the substrate 4109 from the back side may be provided. .

[0098] During film formation, the substrate stage 4108 is held approximately perpendicular to the floor. When the product is handed over, it is held in a roughly horizontal position relative to the floor. The portion indicated by the dashed line is the position where the substrate stage 4108 is held when the substrate is transferred. By adopting such a configuration, dust or particles that may be mixed in during film formation are prevented from adhering to the substrate 4109. However, the probability of the substrate touching the stage can be reduced more than if the substrate stage were held horizontally. If 4108 is held vertically (90°) to the floor, the substrate 4109 may fall. Therefore, the angle of the substrate stage 4108 with respect to the floor surface should be set to 80° or more and less than 90°. It is preferable that

[0099] In addition, the adhesion prevention plate 4107 prevents particles sputtered from the target 4106 from being generated. The deposition of the deposition shield 4107 can be suppressed in the region. It is desirable to process the particles so that they do not peel off. For example, a brush that increases the surface roughness The surface of the adhesion prevention plate 4107 may be subjected to a blast treatment or may have projections and recesses.

[0100] The deposition chamber 4006b is connected to a mass flow controller 4302 via a gas heating mechanism 4302. 300, and the gas heating mechanism 4302 is precisely controlled via the mass flow controller 4300. The gas is introduced into the deposition chamber 4006b by a gas heating mechanism 4302. The gas can be heated to 40°C or higher and 400°C or lower. The number of mass flow controllers 4300 and refiners 4301 is the same as the number of gas types. The gas introduced into the deposition chamber 4006b has a dew point of -80 Gases having a temperature of 0.4 ° C or less, preferably 0.4 ° C or less, can be used, for example, oxygen gas, Nitrogen gas and rare gas (such as argon gas) are used.

[0101] The film-forming chamber 4006b is connected to a turbo molecular pump 4202 and a vacuum pump 4203 via a valve. It is connected to P4200.

[0102] Further, the film formation chamber 4006b is provided with a cryotrap 4110.

[0103] The Cryotrap 4110 is designed to adsorb molecules (or atoms) with relatively high melting points, such as water. The turbo molecular pump 4202 is a mechanism that can pump large molecules (or atoms). It is highly productive because it stably exhausts hydrogen and other gases and requires little maintenance. Therefore, in order to improve the pumping capacity for water, etc., a cryotrap is The cryotrap 4110 is connected to the deposition chamber 4006b. The temperature of the refrigerator is 100K or less, preferably 80K or less. If the 4110 has multiple refrigerators, changing the temperature for each refrigerator will allow for more efficient exhaust. For example, the temperature of the first stage refrigerator is set to 100K or less, and The temperature of the first stage refrigerator should be set to 20K or less.

[0104] The method of exhausting the film forming chamber 4006b is not limited to this, and may be the same as that of the transfer chamber 4004. The exhaust method may be the same as that of a cryopump and a vacuum pump. Of course, the exhaust method for the transfer chamber 4004 is the same as that for the film forming chamber 4006b (a turbo molecular pump, etc.). (Exhaust method with a vacuum pump) may also be used.

[0105] In addition, the back pressure ( It is preferable that the total pressure, and the partial pressure of each gas molecule (atom) are as follows. The back pressure of the membrane chamber 4006b and the partial pressure of each gas molecule (atom) are used to determine the amount of impurities in the membrane. Caution is required as there is a possibility that

[0106] The back pressure (total pressure) of each of the above mentioned chambers is 1×10 -4 Pa or less, preferably 3×10 -5 Pa Less than 1×10, more preferably -5 The mass-to-charge ratio (m / The partial pressure of a gas molecule (atom) with z=18 is 3 × 10 -5 Pa or less, preferably 1×1 0 -5 Pa or less, more preferably 3×10 -6 In addition, the above-mentioned The partial pressure of a gas molecule (atom) with m / z of 28 is 3 x 10 -5 Pa or less, preferably 1× 10 -5 Pa or less, more preferably 3×10 -6 In addition, the above-mentioned room temperature is 100°C or less. The partial pressure of a gas molecule (atom) with m / z of 44 is 3×10 -5 Pa or less, preferably 1 ×10 -5 Pa or less, more preferably 3×10 -6 Pa or less.

[0107] The total and partial pressures in the vacuum chamber can be measured using a mass spectrometer. For example, the quadrupole mass spectrometer (also called Q-mass) manufactured by ULVAC, Inc. lee CGM-051 can be used.

[0108] Next, the transfer chamber 4004 and the load lock chamber 4003a shown in FIG. ) will be described in detail with respect to the atmospheric substrate transfer chamber 4002 and the atmospheric substrate supply chamber 4001. FIG. 3C shows the atmospheric substrate transfer chamber 4002 and the atmospheric substrate supply chamber 400 FIG. 1 is a cross-sectional view of FIG.

[0109] The transfer chamber 4004 shown in FIG. 3B is the same as the transfer chamber 4004 shown in FIG. can be taken into consideration.

[0110] The load lock chamber 4003a includes a substrate transfer stage 4111. The pressure in the chamber 4003a is increased from a reduced pressure state to atmospheric pressure, and the pressure in the load lock chamber 4003a is When the pressure becomes atmospheric pressure, the transfer robot 41 installed in the atmospheric side substrate transfer chamber 4002 The substrate transfer stage 4111 receives the substrate from the load lock chamber 40. After the vacuum is drawn in the transfer chamber 4003a to create a reduced pressure state, the transfer robot installed in the transfer chamber 4004 The stage 4103 receives the substrate from the substrate transfer stage 4111 .

[0111] The load lock chamber 4003a is connected to a vacuum pump 4200 and a cryogenic coolant supply 4201 via a valve. The vacuum pump 4200 and the cryopump 4201 are connected to the The exhaust system can be connected by referring to the connection method of the transfer chamber 4004. The unload lock chamber 4003b shown in FIG. It can have a configuration similar to that of the chamber 4003a.

[0112] The atmospheric substrate transfer chamber 4002 includes a transfer robot 4103. The substrate is transferred between the cassette port 4101 and the load lock chamber 4003a. In addition, above the atmospheric substrate transfer chamber 4002 and the atmospheric substrate supply chamber 4001, HEPA filter (High Efficiency Particulate A A mechanism to prevent the intrusion of dust or particles such as infrared filters is provided. Good too.

[0113] The atmospheric substrate supply chamber 4001 has a plurality of cassette ports 4101. The container 4101 can store multiple substrates.

[0114] By forming a metal oxide film using the above-mentioned film forming apparatus, the amount of impurities in the metal oxide film can be reduced. Furthermore, the above-mentioned film forming apparatus can be used to form a film in contact with a metal oxide film. By forming a film, it is possible to suppress the intrusion of impurities into the metal oxide film from the film in contact with the metal oxide film. Cut.

[0115] For example, a semiconductor device according to one embodiment of the present invention can be manufactured using the deposition apparatus shown in FIGS. If so, this can be done in the following order:

[0116] First, a substrate on which an insulating film has been formed is carried into the film forming apparatus, and the insulating film is heated in the substrate heating chamber 4005. Then, a metal oxide film is formed in the film formation chamber 4006a.

[0117] Alternatively, a substrate on which an insulating film has been formed is first carried into the film forming apparatus, and heated in the substrate heating chamber 4005. The insulating film is heated. Then, a first metal oxide film is formed in the film forming chamber 4006a. Then, a second metal oxide film is formed in the film formation chamber 4006b. The first metal oxide film and the second metal oxide film are formed by changing the flow rate of oxygen gas during film formation. This makes it possible to change the crystallinity or material composition of the metal oxide film.

[0118] In the above, the first metal oxide film and the second metal oxide film are formed in different film formation chambers. Although the above-mentioned film formation method is exemplified, the present invention is not limited to this. For example, the following method can be used by using the same film formation chamber: A first metal oxide film and a second metal oxide film may be formed. When a thermal mechanism is installed, it is used for heat treatment of insulating films and deposition of metal oxide films, The heat treatment of the insulating film, the formation of the first metal oxide film, and the formation of the second metal oxide film are performed simultaneously. The deposition may be performed in the same deposition chamber.

[0119] <1-3. Effects of heat treatment> In the following, we will analyze the samples prepared using the above method using thermal desorption spectroscopy (TDS). Thermal Desorption Spectroscopy (TDS) analysis We will explain about this.

[0120] [Sample preparation] First, four insulating layers were formed on a glass substrate. (PECVD:Plasma Enhanced Chemical Vapor De The insulating film was formed in a vacuum using the 50 mm thick SiO2 thin film deposition method. nm thick silicon nitride film, 300 nm thick silicon nitride film, 50 nm thick silicon nitride film A silicon oxynitride film having a thickness of 50 nm and a silicon nitride film having a thickness of 50 nm were used.

[0121] Next, the substrate was transported in the air and loaded into a film forming apparatus.

[0122] Next, the pressure is increased to about 1×10 -5 The substrate is inserted into a heat treatment chamber at 10 Pa and heat treatment is performed. I did.

[0123] Next, the substrate was carried into a film-forming chamber, and a metal oxide film was formed by sputtering. The metal oxide film was formed by ionizing the metal oxide with indium, gallium, and zinc without heating the substrate (approximately 25°C). A metal oxide target having the following atomic ratio (In:Ga:Zn=4:2:4.1) was used. A film was formed to a thickness of about 100 nm using this.

[0124] Moreover, here, a number of samples were prepared with different heat treatment conditions.

[0125] [TDS rating] The results of the TDS measurement are shown in FIG. 24(A). This is the result of measuring the amount of gas released at / z=18, which corresponds to the amount of water molecules. ), the horizontal axis is temperature and the vertical axis is detection intensity.

[0126] In FIG. 24(A), there is a sample that has not been subjected to heat treatment (denoted as "no bake"), and a sample that has been subjected to heat treatment at 250° C. The figures show samples that were heat-treated at 350°C or 450°C for one hour.

[0127] In each sample, the first peak was observed at a temperature of about 100°C. It is presumed that this peak is due to the desorption phenomenon of water molecules that were adsorbed on the surface of the oxide film.

[0128] Moreover, a second peak is observed in the temperature range from 350°C to 450°C. This is presumably due to the influence of water and hydrogen present at the interface between the insulating film and the metal oxide film. When hydrogen diffuses into the metal oxide film, it combines with oxygen in the metal oxide film to form water molecules. The metal oxide film may be oxidized and released from the surface of the metal oxide film. The first peak is due to both water and hydrogen contained in the insulating film or at the interface between the insulating film and the metal oxide film. It is presumed that this peak is due to

[0129] FIG. 24(B) shows the results of quantifying the amount of water molecules desorbed per unit area. Here, the quantification was performed within the range excluding the peak around 100°C seen in Figure 24(A). It is.

[0130] As shown in Figures 24(A) and (B), the higher the heat treatment temperature, the lower the peak intensity. In other words, the heat treatment causes the It can be seen that the amount of water and hydrogen in the fuel is reduced.

[0131] FIG. 25(A) shows the results of the treatment at a temperature of 350° C. for 300 seconds, 600 seconds, and 1800 seconds. The results are shown for conditions of 3600 seconds and 3600 seconds.

[0132] FIG. 25(B) shows the results of the treatment at a temperature of 450° C. for 300 seconds, 600 seconds, and 1 The results are shown for conditions of 800 seconds and 3600 seconds.

[0133] As shown in Fig. 25(A) and (B), regardless of the treatment temperature, the treatment time was 300 seconds or longer. Under these conditions, the amount of water molecules desorbed is about the same. It can be confirmed that the water and hydrogen adsorbed on the surface of the coating film have been sufficiently reduced. Therefore, it is expected that sufficient effects can be expected even if the treatment time is shorter than 300 seconds. Furthermore, it is expected that sufficient effects can be expected even if the treatment temperature is lower than 350°C.

[0134] The above is an explanation of the effect of the heat treatment.

[0135] This embodiment may be combined, at least in part, with other embodiments described in this specification. It can be implemented in combination.

[0136] (Embodiment 2) In this embodiment, a semiconductor device and a manufacturing method of the semiconductor device according to one embodiment of the present invention will be described. The following description will be given with reference to FIG. 4 to FIG.

[0137] <2-1. Configuration example 1 of semiconductor device> FIG. 4A is a top view of a transistor 100 which is a semiconductor device of one embodiment of the present invention. 4B corresponds to a cross-sectional view taken along the dashed line X1-X2 in FIG. 4A. FIG. 4(C) is a cross-sectional view taken along the dashed line Y1-Y2 in FIG. 4(A). In FIG. 4A, in order to avoid complication, the transistor 100 Some of the components (such as the insulating film that functions as the gate insulating film) are omitted in the figure. The dashed line X1-X2 direction is the channel length direction, and the dashed line Y1-Y2 direction is the channel width direction. In the top view of the transistor, 4(A), some of the components may be omitted.

[0138] The transistor 100 shown in FIGS. 4A, 4B, and 4C is a so-called top-gate transistor. It's Jista.

[0139] The transistor 100 includes an insulating film 104 on a substrate 102 and a metal oxide film on the insulating film 104. a film 108, an insulating film 110 on the metal oxide film 108, and a conductive film 112 on the insulating film 110. , an insulating film 116 on the insulating film 104, a metal oxide film 108, and a conductive film 112. .

[0140] For example, the metal oxide film 108 may be made of In and M (wherein M is Al, Ga, Y, or Sn). ) and Zn.

[0141] In addition, the metal oxide film 108 is not overlapped with the conductive film 112 and is in contact with the insulating film 116. The region includes a region 108n. The region 108n is a region in which a part of the metal oxide film 108 is The region 108n is an n-type region. Note that the region 108n is connected to the insulating film 116 containing nitrogen or hydrogen. Therefore, when nitrogen or hydrogen in the insulating film 116 is added to the region 108n, , the carrier density increases and the material becomes n-type.

[0142] In addition, the metal oxide film 108 has a region in which the atomic ratio of In is greater than the atomic ratio of M. As an example, the ratio of the number of atoms of In, M, and Zn in the metal oxide film 108 is preferably I It is preferable that n:M:Zn=approximately 4:2:3.

[0143] The composition of the metal oxide film 108 is not limited to the above. The atomic ratio of In, M, and Zn in No. 8 may be approximately In:M:Zn=5:1:6. Here, "near" means that when In is 5, M is 0.5 or more and 1.5 or less, and Zn is 5 or less. Includes the top 7 and below.

[0144] The metal oxide film 108 has a region in which the atomic ratio of In is greater than the atomic ratio of M, The field effect mobility of the transistor 100 can be increased. The field effect mobility of 100 is 10 cm 2 / V s More preferably, a transistor The field effect mobility of 100 is 30 cm 2 / V s It is possible to exceed this limit.

[0145] For example, the above-mentioned high field effect mobility transistor is used as a gate driver for generating a gate signal. By using this in a driver, it is possible to provide a display device with a narrow frame width (also called a narrow frame). In addition, the above-mentioned transistor having high field effect mobility is provided as a The source driver that supplies the signal (especially the output of the shift register that the source driver has) By using it in a 10-pin demultiplexer (connected to the output terminal), the number of wires connected to the display device can be reduced. Therefore, a display device with fewer display elements can be provided.

[0146] On the other hand, the metal oxide film 108 has a region in which the atomic ratio of In is greater than the atomic ratio of M. However, if the crystallinity of the metal oxide film 108 is high, the field effect mobility may be reduced. .

[0147] The crystallinity of the metal oxide film 108 can be measured by, for example, X-ray diffraction (XRD). Diffraction or transmission electron microscopy (TEM) Analyze the data using a transmission electron microscope (TEM) It can be analyzed with.

[0148] Next, oxygen vacancies that can be formed in the metal oxide film 108 will be described.

[0149] The oxygen vacancies formed in the metal oxide film 108 are problematic because they affect the transistor characteristics. For example, when oxygen vacancies are formed in the metal oxide film 108, hydrogen is introduced into the oxygen vacancies. The carrier supply source is generated in the metal oxide film 108. and the fluctuation of the electrical characteristics of the transistor 100 having the metal oxide film 108, typically at a threshold level. Therefore, in the metal oxide film 108, there is little oxygen vacancy. The less the better.

[0150] Therefore, in one embodiment of the present invention, the insulating film in the vicinity of the metal oxide film 108, specifically, The insulating film 110 formed above the metal oxide film 108 and the insulating film 10 formed below the metal oxide film 108 Either or both of the insulating film 104 and the insulating film 105 contain excess oxygen. Transferring oxygen or excess oxygen from either or both of the films 110 to the metal oxide film 108 By this, it becomes possible to reduce oxygen vacancies in the metal oxide film.

[0151] Impurities such as hydrogen or moisture that are mixed into the metal oxide film 108 affect the transistor characteristics. Therefore, in the metal oxide film 108, hydrogen or water The fewer impurities such as fluorine, the more preferable.

[0152] The metal oxide film 108 is made of a metal oxide having a low impurity concentration and a low defect level density. By using a thin film, a transistor having excellent electrical characteristics can be fabricated. Here, a low impurity concentration and a low defect level density (few oxygen vacancies) are considered to be high purity. High purity genuine or substantially high purity genuine gold Metal oxide films have fewer carrier generation sources, so the carrier density can be reduced. Therefore, the transistor in which the channel region is formed in the metal oxide film has a threshold voltage of 100 V. The electrical characteristics are rarely abnormal (also called normally-on). Metal oxide films that are pure or substantially intrinsic in nature have a low density of defect states, which reduces the number of traps. The level density may also be low. In addition, high purity intrinsic or substantially high purity intrinsic metals The oxide film has a remarkably small off-state current and a channel width of 1×10 6 The channel length is 10 μm. Even with a micrometer element, the voltage between the source and drain electrodes (drain voltage) can be as low as 1V. In the range of 10 V, the off-state current is below the measurement limit of the semiconductor parameter analyzer, that is, Wachi 1×10 -13 It is possible to obtain a characteristic of A or less.

[0153] As shown in FIGS. 4A, 4B, and 4C, the transistor 100 has a through the insulating film 118 and the openings 141a and 141b provided in the insulating films 116 and 118. and conductive films 120a and 120b electrically connected to the regions 108n, respectively. It's fine.

[0154] In this specification and the like, the insulating film 104 is referred to as a first insulating film, and the insulating film 110 is referred to as a second insulating film. The insulating film 116 is referred to as a third insulating film, and the insulating film 118 is referred to as a fourth insulating film. In addition, the conductive film 112 may function as a gate electrode. a functions as a source electrode, and the conductive film 120b functions as a drain electrode. Yes.

[0155] The insulating film 110 also functions as a gate insulating film. The insulating film 110 has an excess oxygen region. Therefore, excess oxygen can be supplied to the metal oxide film 108. Since the oxygen deficiency can be compensated for by excess oxygen, a highly reliable semiconductor device can be provided. It is possible.

[0156] In order to supply excess oxygen into the metal oxide film 108, Excess oxygen may be supplied to the insulating film 104 formed below. In this case, the insulating film 104 The excess oxygen contained in the region 108n may also be supplied to the region 108n. If the metal oxide film 108 is supplied to the region 108n, the resistance in the region 108n becomes high, which is undesirable. By configuring the insulating film 110 formed above the conductive film 110 to have excess oxygen, This makes it possible to selectively supply excess oxygen only to the region overlapping with 2.

[0157] <2-2. Components of Semiconductor Device> Next, components included in the semiconductor device of this embodiment will be described in detail.

[0158] [substrate] There is no particular restriction on the material of the substrate 102, but it should be strong enough to withstand the subsequent heat treatment. For example, glass substrates, ceramic substrates, quartz substrates, and sa A fire substrate or the like may be used as the substrate 102. Also, a material such as silicon or silicon carbide may be used. Single crystal semiconductor substrates, polycrystalline semiconductor substrates, compound semiconductors such as silicon germanium, etc. It is also possible to use a substrate, an SOI substrate, or the like, on which a semiconductor element is provided. The substrate 102 may be a glass substrate. If you have 6th generation (1500mm x 1850mm), 7th generation (1870mm x 220 0mm), 8th generation (2200mm x 2400mm), 9th generation (2400mm x 280 By using large-area substrates such as 10th generation (2950mm x 3400mm), Larger display devices can be manufactured.

[0159] In addition, a flexible substrate is used as the substrate 102, and the transistor 10 is directly formed on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 102 and the transistor 100. The release layer is preferably removed from the substrate 102 after a semiconductor device is partially or entirely completed thereon. The transistor 100 can be separated and used for transfer to another substrate. It can also be transferred to substrates with poor thermal properties or flexible substrates.

[0160] [First insulating film] The insulating film 104 can be formed by sputtering, CVD, vapor deposition, pulsed laser deposition ( The insulating film 104 can be formed by appropriately using a photolaser laser deposition (PLD) method, a printing method, a coating method, or the like. For example, a single layer or a stacked layer of an oxide insulating film or a nitride insulating film can be formed. In order to improve the interface characteristics with the metal oxide film 108, the insulating film 104 is At least the region in contact with the metal oxide film 108 is preferably formed of an oxide insulating film. In addition, by using an oxide insulating film that releases oxygen by heating as the insulating film 104, The heat treatment can move oxygen contained in the insulating film 104 to the metal oxide film 108. It is possible.

[0161] The thickness of the insulating film 104 is 50 nm or more, or 100 nm or more and 3000 nm or less, or The thickness of the insulating film 104 can be set to 200 nm or more and 1000 nm or less. This can increase the amount of oxygen released from the insulating film 104 and also increase the amount of oxygen released from the insulating film 104 and the metal oxide. The interface state at the interface with the metal oxide film 108 and the oxygen vacancies in the metal oxide film 108 are It is possible to reduce the

[0162] The insulating film 104 may be, for example, silicon oxide, silicon oxynitride, silicon nitride oxide, or nitrogen. Silicon oxide, aluminum oxide, hafnium oxide, gallium oxide or Ga-Zn oxide The insulating film may be a single layer or a stacked layer. The layer structure of the silicon nitride film and the silicon oxynitride film is used as the layer 104. The insulating film 104 has a laminated structure, with a silicon nitride film on the lower layer and an oxynitride film on the upper layer. By using the silicon film, oxygen can be efficiently introduced into the metal oxide film 108. do.

[0163] [Conductive film] A conductive film 112 that functions as a gate electrode, a conductive film 120a that functions as a source electrode, The conductive film 120b functioning as the drain electrode may be made of chromium (Cr), copper (Cu), or aluminum. Aluminum (Al), gold (Au), silver (Ag), zinc (Zn), molybdenum (Mo), tantalum (Ta), Ta, Ti, W, Mn, Ni, A metal element selected from the group consisting of Ni, iron (Fe), and cobalt (Co), or the above-mentioned metal elements. The alloys are formed by using alloys containing the above-mentioned metal elements or alloys combining the above-mentioned metal elements. It is possible.

[0164] The conductive films 112, 120a, and 120b are made of an oxide containing indium and tin (I n-Sn oxide), oxide containing indium and tungsten (In-W oxide), Indium, tungsten and zinc oxide (In-W-Zn oxide), indium and titanium (In-Ti oxide), and oxide having indium, titanium, and tin oxides containing indium and zinc (In-Ti-Sn oxides), and oxides containing indium and zinc (In-Zn oxides). oxides having indium, tin and silicon (In-Sn-Si oxides); Conductive oxides such as oxides containing aluminum, gallium and zinc (In-Ga-Zn oxide) Alternatively, a metal oxide film can be applied.

[0165] Here, the oxide conductor will be described. In this specification, the oxide conductor is referred to as OC (Oxide Conductor). Examples of oxide conductors include: When oxygen vacancies are formed in a metal oxide and hydrogen is added to the oxygen vacancies, donor states are formed near the conduction band. As a result, the metal oxide becomes conductive and becomes a conductor. In general, metal oxides can store energy. The large gap between the oxides allows them to transmit visible light. Therefore, oxide conductors are metal oxides that have donor levels near the band. The effect of absorption due to position is small, and the transparent property to visible light is comparable to that of metal oxides.

[0166] In particular, when the conductive film 112 is made of the oxide conductor, excess oxygen is added to the insulating film 110. This is preferable because it can be added.

[0167] The conductive films 112, 120a, and 120b are made of a Cu-X alloy film (X is Mn, Ni, Cr, Fe, Co, Mo, Ta, or Ti) may be applied. This allows processing using a wet etching process, which reduces manufacturing costs. It becomes possible.

[0168] Furthermore, the conductive films 112, 120a, and 120b contain, among the above-mentioned metal elements, titanium. tungsten, tantalum, and molybdenum. In particular, the conductive films 112, 120a, and 120b are preferably made of tantalum nitride. The tantalum nitride film is preferably a conductive film and is resistant to copper or hydrogen. In addition, the tantalum nitride film has high barrier properties against hydrogen. Since the amount of the metal oxide film 108 is small, the conductive film in contact with the metal oxide film 108 or the conductive film in the vicinity of the metal oxide film 108 It can be suitably used as a conductive film.

[0169] Moreover, the conductive films 112, 120a, and 120b can be formed by electroless plating. Materials that can be formed by the electroless plating method include, for example, Cu, Ni, Al, One or more selected from Au, Sn, Co, Ag, and Pd may be used. In particular, the resistance of the conductive film can be reduced by using Cu or Ag. Therefore, it is preferable.

[0170] [Second insulating film] The insulating film 110 functioning as the gate insulating film of the transistor 100 is a plasma-treated PECVD (PlasmaEnhancedChemicalVapor) Silicon oxide film, silicon oxynitride film, etc. are formed by deposition, sputtering, etc. Silicon film, silicon oxynitride film, silicon nitride film, aluminum oxide film, hafnium oxide film film, yttrium oxide film, zirconium oxide film, gallium oxide film, tantalum oxide film, oxide Contains one or more of magnesium oxide, lanthanum oxide, cerium oxide, and neodymium oxide films Note that the insulating film 110 may have a stacked structure of two layers or three or more layers. A laminated structure may also be used.

[0171] In addition, the metal oxide film 108 that functions as the channel region of the transistor 100 is in contact with the The insulating film 110 is preferably an oxide insulating film, and has a stoichiometric composition in excess of oxygen. In other words, it is more preferable that the insulating film 11 has a region containing The insulating film 110 is an insulating film capable of releasing oxygen. To provide the insulating film 110, for example, the insulating film 110 is formed in an oxygen atmosphere, or the insulating film 110 is formed by insulating the insulating film 110 after the film formation. The film 110 may be heat treated in an oxygen atmosphere.

[0172] Furthermore, when hafnium oxide is used as the insulating film 110, the following effects are obtained. Hafnium has a higher dielectric constant than silicon oxide and silicon oxynitride. Compared to the case where silicon oxide is used, the thickness of the insulating film 110 can be made larger, so that the tunnel This reduces the leakage current caused by the current. Furthermore, hafnium oxide, which has a crystalline structure, can be used to realize an amorphous structure. It has a higher relative dielectric constant than hafnium oxide, which has a low off-current. To form a transistor, it is preferable to use hafnium oxide having a crystalline structure. Examples of the crystal structure include monoclinic and cubic. The types are not limited to these.

[0173] In addition, it is preferable that the insulating film 110 has few defects. (ESR: Electron Spin Resonance) signals are small. For example, the above-mentioned signal is E' observed at a g value of 2.001. The E' center is caused by the dangling bond of silicon. The insulating film 110 has a spin density due to the E' center of 3×10 17 spins / cm 3 Less than or equal to 5×10 16 spins / cm 3 A silicon oxide film having the following structure: Alternatively, a silicon oxynitride film may be used.

[0174] [Metal oxide film] The metal oxide film 108 can be made of the metal oxides listed above.

[0175] <Atomic ratio> The following describes the gold alloy of the present invention with reference to Figs. 10(A), 10(B) and 10(C). The preferred range of the atomic ratio of indium, element M, and zinc in the metal oxide is explained. In addition, in Fig. 10(A), Fig. 10(B), and Fig. 10(C), the atomic ratio of oxygen In addition, the indium, element M, and zinc atoms of the metal oxide are not described. The respective terms in the numerical ratio are [In], [M], and [Zn].

[0176] In Figures 10(A), 10(B), and 10(C), the dashed lines indicate the ratio of [In]:[M ]:[Zn]=(1+α):(1-α):1 atomic ratio (-1≦α≦1), The line where the atomic ratio of [In]:[M]:[Zn]=(1+α):(1-α):2, The line where the atomic ratio of In]:[M]:[Zn]=(1+α):(1-α):3, [I n]:[M]:[Zn]=(1+α):(1-α):4, and The line showing the atomic ratio of [In]:[M]:[Zn]=(1+α):(1-α):5 is shown. vinegar.

[0177] The dashed line indicates the atomic ratio of [In]:[M]:[Zn]=5:1:β (β≧0). The line where the atomic ratio of [In]:[M]:[Zn]=2:1:β is The line where the atomic ratio is 1:1:β, [In]:[M]:[Zn ]=1:2:β atomic ratio line, [In]:[M]:[Zn]=1:3:β atomic ratio line The line showing the atomic ratio of [In]:[M]:[Zn]=1:4:β Represents a line.

[0178] In addition, the [In]:[M]: Metal oxides with an atomic ratio of [Zn]=0:2:1 and its neighboring values ​​form spinel-type crystals. Easy to structure.

[0179] In addition, multiple phases may coexist in a metal oxide (two-phase coexistence, three-phase coexistence, etc.). For example, For example, when the atomic ratio is close to [In]:[M]:[Zn]=0:2:1, the spinel In addition, the two phases of the hexagonal crystal structure and the layered crystal structure tend to coexist. When [M]:[Zn] is close to 1:0:0, the bixbyite-type crystal structure and layered structure When multiple phases coexist in a metal oxide, different crystal structures are formed. Between the crystal structures, grain boundaries may be formed.

[0180] Region A shown in FIG. 10(A) is a region of indium, element M, and zinc contained in a metal oxide. An example of a preferable range of the atomic ratio is shown.

[0181] By increasing the indium content of metal oxide, the carrier mobility of the metal oxide ( Therefore, metal oxides with a high indium content The carrier mobility is higher than that of metal oxides with a lower indium content.

[0182] On the other hand, when the content of indium and zinc in the metal oxide is low, the carrier mobility Therefore, the atomic ratio [In]:[M]:[Zn]=0:1:0 and its vicinity When it is near the value (for example, region C shown in FIG. 10C), the insulating property is high.

[0183] Therefore, the metal oxide of one embodiment of the present invention has high carrier mobility, and is in the region of FIG. It is preferable that the atomic ratio is A.

[0184] In particular, in the region B shown in FIG. 10B, the carrier mobility is high and the reliability is high, even among the regions A. As a result, an excellent metal oxide with high thermal conductivity can be obtained.

[0185] In addition, the region B is [In]:[M]:[Zn]=4:2:3 to 4.1 and its vicinity. Nearest values ​​are included. Nearest values ​​include, for example, [In]:[M]:[Zn]=5:3:4. In addition, region B is [In]:[M]:[Zn]=5:1:6 and its neighboring values, and [In]:[M]:[Zn]=5:1:7, and neighboring values.

[0186] The properties of metal oxides are not uniquely determined by the atomic ratio. Even if the ratio is the same, the properties of the metal oxide may differ depending on the formation conditions. When depositing a film of a silicide using a sputtering device, the atomic ratio of the target may deviate from the atomic ratio of the target. In addition, depending on the substrate temperature during film formation, the film may be formed with a higher concentration of [Zn] than the target. The [Zn] of the film may be small. Therefore, the region shown is a region where the metal oxide has a specific characteristic. The boundary between region A and region C is not strict. stomach.

[0187] In addition, when the metal oxide film 108 is an In-M-Zn oxide, the sputtering target It is preferable to use a target containing polycrystalline In-M-Zn oxide as the target. The atomic ratio of the metal oxide film 108 to be formed is The atomic ratio of the metal elements in the metal oxide film can vary by ±40%. The composition of the sputtering target used in 08 is In:Ga:Zn=4:2:4.1[ In the case of the atomic ratio of In:Ga:Zn, the composition of the metal oxide film 108 formed is In:Ga:Zn=4:2: In addition, the sputtering used for the metal oxide film 108 may be close to 3 [atomic ratio]. When the composition of the target is In:Ga:Zn=5:1:7 [atomic ratio], the film is formed. The composition of the metal oxide film 108 is approximately In:Ga:Zn=5:1:6 [atomic ratio]. There are cases.

[0188] The metal oxide film 108 has an energy gap of 2 eV or more, preferably 2.5 e In this way, by using metal oxides with a wide energy gap, The off-current of the transistor 100 can be reduced.

[0189] In addition, the metal oxide film 108 preferably has a non-single crystal structure. Examples of such structures include CAAC-OS, polycrystalline structures, microcrystalline structures, and amorphous structures, which will be described later. Among crystal structures, the amorphous structure has the highest density of defect states.

[0190] [Third insulating film] The insulating film 116 contains nitrogen or hydrogen. For example, the insulating film 116 is a nitride insulating film. Examples of the nitride insulating film include silicon nitride, silicon oxynitride, and oxynitride. The insulating film 116 can be formed using silicon hydride or the like. The hydrogen concentration in the insulating film 116 is 1× 10 22 atoms / cm 3 The insulating film 116 is preferably made of a metal oxide. Therefore, in the region 108n that contacts the insulating film 116, The impurity (nitrogen or hydrogen) concentration is increased, which increases the carrier density in the region 108n. can.

[0191] [Fourth insulating film] The insulating film 118 can be an oxide insulating film. For the insulating film 118, a stacked film of an oxide insulating film and a nitride insulating film can be used. For example, silicon oxide, silicon oxynitride, silicon nitride oxide, aluminum oxide, Hafnium oxide, gallium oxide, Ga-Zn oxide, or the like may be used.

[0192] The insulating film 118 functions as a barrier film against hydrogen, water, and the like from the outside. It is preferable that

[0193] The thickness of the insulating film 118 is 30 nm or more and 500 nm or less, or 100 nm or more and 400 nm or less. m or less.

[0194] <2-3. Transistor configuration example 2> Next, regarding a transistor having a structure different from that shown in FIG. 4(A), (B), and (C), Explain using (B) and (C).

[0195] 5A is a top view of a transistor 150, and FIG. 5B is a dot-dash diagram of FIG. 5A. 5(C) is a cross-sectional view taken along the dashed line Y1-Y2 in FIG. 5(A). FIG.

[0196] The transistor 150 shown in FIGS. 5A, 5B, and 5C includes a conductive film 106 over a substrate 102 and a , an insulating film 104 on the conductive film 106, a metal oxide film 108 on the insulating film 104, An insulating film 110 on the metal film 108, a conductive film 112 on the insulating film 110, an insulating film 104, a metal The insulating film 116 is formed over the oxide film 108 and the conductive film 112 .

[0197] The metal oxide film 108 is the same as that of the transistor 100 shown in FIGS. The transistor 150 shown in FIGS. In addition to the configuration of the transistor 100 , a conductive film 106 and an opening 143 are provided.

[0198] The opening 143 is provided in the insulating films 104 and 110. The conductive film 106 is also provided with the opening The conductive film 106 is electrically connected to the conductive film 112 through the conductive film 143. The same potential is applied to the conductive film 106 and the conductive film 112. A potential different from that of the conductive film 112 may be applied to the conductive film 111. The film 106 may be used as a light-shielding film. For example, the conductive film 106 may be formed of a light-shielding material. This can suppress light from below being irradiated onto the channel formation region.

[0199] In the case of forming the transistor 150, the conductive film 106 is a first gate electrode ( The conductive film 112 functions as a second gate electrode (also called a TOM gate electrode). The insulating film 104 functions as a first gate electrode. The insulating film 110 functions as a second gate insulating film. .

[0200] The conductive film 106 is made of the same material as the conductive films 112, 120a, and 120b described above. In particular, the conductive film 106 can be formed of a material containing copper. For example, the conductive film 106 may be a titanium nitride film or a titanium nitride film. A laminate structure in which a copper film is provided over a tantalum film or a tungsten film is formed. 0b is a laminated structure in which a copper film is provided on a titanium nitride film, a tantalum nitride film, or a tungsten film. In this case, the transistor 150 is preferably a pixel transistor of the display device. By using the conductive film 106 and the conductive film 12 in either one or both of the driving transistors, 0a, and the parasitic capacitance occurring between the conductive film 106 and the conductive film 120b. Therefore, the conductive film 106, the conductive film 120a, and the conductive film 1 20b as the first gate electrode, source electrode, and drain electrode of the transistor 150; It is not only used for power supply wiring, signal supply wiring, or connection wiring for display devices. It can also be used for wiring, etc.

[0201] In this way, the transistor 150 shown in FIGS. 5(A), 5(B), and 5(C) has the same structure as the transistor described above. Unlike the transistor 100, conductive films functioning as gate electrodes are provided above and below the metal oxide film 108. As shown in the transistor 150, the semiconductor device of one embodiment of the present invention has a structure in which A plurality of gate electrodes may be provided.

[0202] As shown in FIG. 5(B) and (C), the metal oxide film 108 is used as a first gate electrode. and a conductive film 112 that functions as a second gate electrode. They are positioned opposite each other and are sandwiched between two conductive films that function as gate electrodes.

[0203] The length of the conductive film 112 in the channel width direction is equal to the length of the metal oxide film 108 in the channel width direction. The length of the metal oxide film 108 in the channel width direction is longer than the length of the insulating film 110. The conductive film 112 and the conductive film 106 are covered with the insulating film 10. 4 and the opening 143 provided in the insulating film 110, the metal oxide film One of the side surfaces of the 108 in the channel width direction faces the conductive film 112 with the insulating film 110 sandwiched therebetween. is doing.

[0204] In other words, the conductive film 106 and the conductive film 112 are formed on the insulating films 104 and 110. A region connected at the opening 143 and positioned outside the side end of the metal oxide film 108 It has a range.

[0205] With such a structure, the metal oxide film 108 included in the transistor 150 A conductive film 106 functions as a first gate electrode and a conductive film 107 functions as a second gate electrode. The electric field of the conductive film 112 can electrically surround the transistor 150. A channel region is formed by the electric field of the first gate electrode and the second gate electrode. The device structure of the transistor that electrically surrounds the metal oxide film 108 is called the Surround This can be called a dchannel (S-channel) structure.

[0206] Since the transistor 150 has an S-channel structure, the conductive film 106 or the conductive The electric field is effectively applied to the metal oxide film 108 to induce a channel by the conductive film 112. This improves the current driving capability of the transistor 150 and provides high on-current characteristics. In addition, since the on-current can be increased, The transistor 150 can be miniaturized. Since the conductive film 108 is surrounded by the conductive film 106 and the conductive film 112, The mechanical strength of the transistor 150 can be increased.

[0207] In the channel width direction of the transistor 150, the opening 1 An opening different from the opening 143 may be formed on the side where the opening 43 is not formed.

[0208] As shown in the transistor 150, a transistor is provided with a semiconductor film sandwiched therebetween. In the case where a pair of gate electrodes are connected to each other, a signal A is applied to one gate electrode and a signal B is applied to the other gate electrode. A fixed potential Vb may be applied to the electrodes. A signal A may be applied to one gate electrode and a signal B may be applied to the other gate electrode. A signal B may be applied to the gate electrode of the other gate electrode. However, the other gate electrode may be supplied with a fixed potential Vb.

[0209] The signal A is, for example, a signal for controlling the conductive state or the non-conductive state. It is a digital signal that can take two types of potential: potential V1 or potential V2 (V1>V2). For example, the potential V1 may be a high power supply potential and the potential V2 may be a low power supply potential. Signal A may be an analog signal.

[0210] The fixed potential Vb is, for example, the threshold voltage V th Electric potential to control A The fixed potential Vb may be the potential V1 or the potential V2. This is preferable because it is not necessary to provide a separate potential generating circuit for generating the fixed potential Vb. The fixed potential Vb may be a potential different from the potential V1 or the potential V2. and the threshold voltage V th In some cases, A can be increased. As a result, the gate-source voltage By reducing the drain current when Vgs is 0V, the leakage current of the circuit containing the transistor is reduced. For example, the fixed potential Vb may be set lower than the low power supply potential. By increasing the fixed potential Vb, the threshold voltage V th There are cases where A can be lowered. As a result, the drain current is improved when the gate-source voltage Vgs is at a high power supply potential, and the transistor In some cases, the operating speed of a circuit having a transistor can be improved. For example, by lowering the fixed potential Vb, It may be higher than the power supply potential.

[0211] The signal B is, for example, a signal for controlling the conductive state or the non-conductive state. It is a digital signal that can take two types of potential: potential V1, potential V2, or potential V3 (V3>V4). For example, the potential V3 may be a high power supply potential and the potential V4 may be a low power supply potential. Signal B may be an analog signal.

[0212] If signal A and signal B are both digital signals, signal B will have the same digital value as signal A. In this case, the on-current of the transistor is improved, and the transistor In this case, the operation speed of the circuit having the potential V1 and The potential V2 may be different from the potentials V3 and V4 in the signal B. For example, The gate insulating film corresponding to the gate to which signal B is input is the gate insulating film corresponding to the gate to which signal A is input. If the gate insulating film is thicker than the gate insulating film, the potential amplitude of signal B (V3-V4) is It may be larger than (V1-V2). This will allow the transistor to be in a conducting state or The effect of signal A on the non-conducting state is set to the same degree as the effect of signal B on the non-conducting state. It may be possible to do so.

[0213] If signal A and signal B are both digital signals, signal B has a different digital value than signal A. In this case, the transistors are controlled by signals A and B separately. For example, a transistor can be In the case of the channel type, when signal A is at potential V1 and signal B is at potential V3, When only the signal A is in a conductive state, or when the signal B is at a potential V4, If only one transistor is non-conducting, a single transistor can function as a NAND circuit or a NOR circuit. In addition, the signal B is a threshold voltage V thA signal to control For example, the signal B may be a period during which a circuit having a transistor is in operation. The signal B may be a signal having a different potential during a period when the circuit is not operating. In this case, signal B may be a signal with a different potential depending on the operation mode of the circuit. In some cases, the potential may not switch as frequently as

[0214] When signal A and signal B are both analog signals, signal B is an analog signal with the same potential as signal A. analog signal obtained by multiplying the potential of signal A by a constant, or adding a constant to the potential of signal A Alternatively, it may be an analog signal obtained by subtracting the signal. In this case, the on-current of the transistor is The signal B may be increased in response to the signal P, thereby increasing the operating speed of a circuit having a transistor. A may be a different analog signal. In this case, the transistor control is signal A and signal B can be performed separately, which may result in higher functionality.

[0215] Signal A may be a digital signal and signal B may be an analog signal. Or, signal A may be It is also possible that signal A is an analog signal and signal B is a digital signal.

[0216] When a fixed potential is applied to both gate electrodes of a transistor, the transistor is For example, a transistor can function as an n-channel transistor. In the case of a transistor type, the fixed potential Va or the fixed potential Vb can be increased (or decreased). In some cases, the effective resistance of the resistor can be lowered (higher). By making both Vb high (low), a transistor with only one gate In some cases, a lower (higher) effective resistance may be obtained.

[0217] The other configurations of the transistor 150 are the same as those of the transistor 100 described above. This has the same effect.

[0218] In addition, an insulating film may be further formed on the transistor 150. The transistor 150 shown in FIG. 1C has an insulating film on the conductive films 120a and 120b and the insulating film 118. It has a veneer 122.

[0219] The insulating film 122 has a function of planarizing unevenness due to transistors and the like. The film 122 may be made of any insulating material, and may be made of an inorganic or organic material. The inorganic material may be a silicon oxide film, a silicon oxynitride film, a silicon nitride oxide film, a nitride Examples of the organic material include a silicon film, an aluminum oxide film, and an aluminum nitride film. Examples of the material include photosensitive resin materials such as acrylic resin and polyimide resin. .

[0220] <2-4. Transistor configuration example 3> Next, regarding a structure different from that of the transistor 150 shown in FIGS. 5A, 5B, and 5C, This will be explained using:

[0221] 6A and 6B are cross-sectional views of the transistor 160. Since the top view of the transistor 150 is similar to that of the transistor 150 in FIG. The details are omitted.

[0222] The transistor 160 shown in FIGS. 6A and 6B has a stacked structure of a conductive film 112, a conductive film 11 The shape of the insulating film 110 and the shape of the second insulating film 110 are different from those of the transistor 150.

[0223] The conductive film 112 of the transistor 160 is a conductive film 112_1 on the insulating film 110 and a conductive film For example, the conductive film 112_1 may be an oxide film. By using a conductive film, excess oxygen can be added to the insulating film 110. The conductive film may be formed by sputtering in an atmosphere containing oxygen gas. The oxide conductive film may be, for example, an oxide having indium and tin, or a tin oxide. oxides containing tungsten and indium, and oxides containing tungsten, indium, and zinc oxides containing titanium and indium, oxides containing titanium, indium and tin , an oxide having indium and zinc, an oxide having silicon, indium and tin, Examples of the oxide include oxides containing indium, gallium, and zinc.

[0224] As shown in FIG. 6B, in the opening 143, the conductive film 112_2 and the conductive film When the opening 143 is formed, the conductive film that becomes the conductive film 112_1 is After the formation, an opening 143 is formed, so that the shape shown in FIG. 6(B) can be obtained. When an oxide conductive film is used as the conductive film 112_1, the conductive film 112_2 and the conductive film 106 By using a structure in which the conductive film 112 and the conductive film 106 are connected to each other, the connection resistance between the conductive film 112 and the conductive film 106 can be reduced. It is possible.

[0225] The conductive film 112 and the insulating film 110 of the transistor 160 have a tapered shape. More specifically, the lower end of the conductive film 112 is formed outside the upper end of the conductive film 112. In addition, the lower end of the insulating film 110 is formed outside of the upper end of the insulating film 110. In addition, the lower end of the conductive film 112 is formed at approximately the same position as the upper end of the insulating film 110 .

[0226] The conductive film 112 and the insulating film 110 of the transistor 160 are tapered. In comparison with the case where the conductive film 112 and the insulating film 110 of the transistor 160 are rectangular, the insulating film 116 This is preferable because it can improve the covering property.

[0227] The other configurations of the transistor 160 are similar to those of the transistor 150 described above. This has the same effect.

[0228] <2-5. Manufacturing method of semiconductor device> Next, an example of a method for manufacturing the transistor 150 shown in FIGS. 7 to 9. Note that FIGS. 7 to 9 show a method for manufacturing the transistor 150. 1A and 1B are cross-sectional views illustrating the channel length direction and the channel width direction.

[0229] First, the conductive film 106 is formed on the substrate 102. Next, the substrate 102 and the conductive film 106 are An insulating film 104 is formed on the insulating film 104, and a metal oxide film is formed on the insulating film 104. The metal oxide film is processed into islands to form the metal oxide film 108 (see FIG. 7A).

[0230] Here, the insulating film 104 and the metal oxide film 108 are formed by the method exemplified in the first embodiment. That is, the first step of forming the insulating film 104 on the substrate 102 and the conductive film 106 can be applied. the second step of transporting the substrate 102 to the device, and the third step of heating the insulating film 104. and a fourth step of forming a metal oxide film 108. The process is performed in an atmosphere where the partial pressure of water vapor is lower than that of the atmosphere, and is performed consistently. 104 and a metal oxide film 108 can be formed.

[0231] The conductive film 106 can be formed by selecting the above-mentioned material. In this example, a tungsten film having a thickness of 50 nm was deposited as the conductive film 106 using a sputtering apparatus. A laminate film is formed of a silicon film and a copper film having a thickness of 400 nm.

[0232] The conductive film to be the conductive film 106 can be processed by wet etching and drapery. In this embodiment, either one or both of the wet etching methods may be used. After etching the copper film by etching method, the tungsten film is removed by dry etching method. The conductive film is processed by etching to form the conductive film 106 .

[0233] The insulating film 104 can be formed by sputtering, CVD, vapor deposition, pulsed laser deposition ( The film can be formed by appropriately using a PLD method, a printing method, a coating method, or the like. In this case, a silicon nitride film having a thickness of 400 nm was deposited as the insulating film 104 using a PECVD apparatus. Then, a silicon oxynitride film having a thickness of 50 nm is formed.

[0234] After the insulating film 104 is formed, oxygen may be added to the insulating film 104. The oxygen added to 4 can be oxygen radicals, oxygen atoms, oxygen atomic ions, or oxygen molecular ions. The doping method includes ion doping, ion implantation, plasma treatment, etc. In addition, a film that suppresses oxygen desorption is formed on the insulating film, and then the insulating film is formed through the film. The film 104 may be doped with oxygen.

[0235] The above-mentioned oxygen desorption-suppressing film may be made of indium, zinc, gallium, tin, aluminum, or the like. Aluminum, Chromium, Tantalum, Titanium, Molybdenum, Nickel, Iron, Cobalt, or Tungsten The insulating film can be formed using a conductive film or a semiconductor film having one or more tennines.

[0236] In addition, when oxygen is added in plasma treatment, the oxygen is excited by microwaves to produce high-density oxygen. By generating atomic plasma, the amount of oxygen added to the insulating film 104 can be increased. .

[0237] When forming the metal oxide film 108, in addition to oxygen gas, an inert gas (for example, Gas such as sodium gas, argon gas, and xenon gas may be mixed. The ratio of oxygen gas to the total deposition gas when forming the film 108 (hereinafter, also referred to as the oxygen flow rate ratio) The ratio c) is from 0% to 100%, preferably from 5% to 20%.

[0238] The conditions for forming the metal oxide film 108 are preferably a substrate temperature of room temperature or higher and 180° C. or lower. Preferably, the substrate temperature is set to a temperature between room temperature and 140° C. It is preferable to set the substrate temperature to, for example, room temperature or higher and lower than 140° C., since this increases productivity.

[0239] The thickness of the metal oxide film 108 is 3 nm or more and 200 nm or less, preferably 3 The thickness may be from 3 nm to 100 nm, and more preferably from 3 nm to 60 nm.

[0240] As the substrate 102, a large glass substrate (for example, 6th to 10th generation) is used. In this case, the substrate temperature during the formation of the metal oxide film 108 is set to 200° C. or more and 300° C. or less. In this case, the substrate 102 may be deformed (distorted or warped). In the case of using a plate, the substrate temperature during the formation of the metal oxide film 108 is set to 20° C. or higher than room temperature. By setting the temperature to less than 0° C., deformation of the glass substrate can be suppressed.

[0241] In addition, the sputtering gas must be highly purified. The oxygen gas and argon gas used in the present invention have a dew point of -40°C or less, preferably -80°C or less, and Preferably, the gas is purified to a temperature of -100°C or lower, more preferably -120°C or lower. By using this, it is possible to prevent moisture and the like from being taken into the metal oxide film as much as possible.

[0242] In addition, when forming a metal oxide film by sputtering, The chamber is cryopreserved to remove as much water and other impurities as possible from the metal oxide. A high vacuum (5×10 -7 Pa to 1×10 -4 It is preferable to evacuate the gas to a pressure of about 10 Pa. The gas molecules equivalent to H2O (gas molecules equivalent to m / z = 18) in the chamber Voltage division is 1×10 -4 Pa or less, preferably 5×10 -5 It is preferable to set the pressure to 0.1 Pa or less.

[0243] In this embodiment, the conditions for forming the metal oxide film 108 are as follows.

[0244] The metal oxide film 108 is formed by sputtering using an In-Ga-Zn metal oxide target. The substrate temperature and the oxygen flow rate ratio during the formation of the metal oxide film 108 are The pressure in the chamber is set to 0.6 Pa, and the sputtering temperature is set to 100° C. Supplying 2500W of AC power to a metal oxide target placed in a ring apparatus Then, an oxide film is formed.

[0245] In order to process the formed metal oxide film into the metal oxide film 108, wet etching is performed. Either or both of a polishing method and a dry etching method may be used.

[0246] After the metal oxide film 108 is formed, a heat treatment is performed to dehydrate the metal oxide film 108. The temperature of the heat treatment is typically 150° C. or higher, and the distortion of the substrate may be reduced. The temperature is below the melting point, or 250°C or higher and 450°C or lower, or 300°C or higher and 450°C or lower.

[0247] Heat treatment is carried out using rare gases such as helium, neon, argon, xenon, krypton, or This can be done in an inert atmosphere containing nitrogen, or after heating in an inert atmosphere, in an oxygen atmosphere. The heating may be performed in an atmosphere containing hydrogen, water, etc. in the inert atmosphere and oxygen atmosphere. The treatment time may be from 3 minutes to 24 hours.

[0248] The heat treatment can be performed using an electric furnace, an RTA device, or the like. Therefore, heat treatment can be performed at a temperature above the distortion point of the substrate for a short period of time. The processing time can be reduced.

[0249] The metal oxide film is formed while being heated, or the metal oxide film is formed and then subjected to a heat treatment. By performing this, the hydrogen concentration in the metal oxide film obtained by SIMS was increased to 5×10 19 a toms / cm 3 or less, or 1×10 19 atoms / cm 3 Below, 5 x 10 18 at oms / cm 3 or less, or 1×10 18 atoms / cm 3or less, or 5×10 17 atoms / cm 3 or less, or 1×10 16 atoms / cm 3 It can be do.

[0250] Next, an insulating film 110_0 is formed on the insulating film 104 and the metal oxide film 108. (FIG. 7 (See (B)).

[0251] The insulating film 110_0 is a silicon oxide film or a silicon oxynitride film, which is formed by plasma treatment. Formed using a chemical vapor deposition (PECVD) system or simply a plasma CVD system. In this case, the source gas may be a deposition gas containing silicon and an oxidizing gas. It is preferable to use a gas containing silicon. Representative examples of deposition gases containing silicon include silane, diphenyl ether, and dimethyl ether. Examples of oxidizing gases include oxygen, ozone, monooxygen, and silane. Examples include dinitrogen fluoride and nitrogen dioxide.

[0252] In addition, for the insulating film 110_0, the flow rate of the oxidizing gas is set to 20 times the flow rate of the deposition gas. The pressure in the treatment chamber should be 100P or more but less than 100 times, or 40 times or more but less than 80 times. By using a PECVD device with a pressure of less than a or 50 Pa or less, the amount of defects is reduced. A silicon nitride film can be formed.

[0253] In addition, the insulating film 110_0 is placed in a vacuum-evacuated processing chamber of a PECVD apparatus. The substrate is maintained at a temperature of 280° C. or higher and 400° C. or lower, and a source gas is introduced into the processing chamber. The pressure in the chamber is set to 20 Pa or more and 250 Pa or less, and more preferably 100 Pa or more and 250 Pa or less. Under the conditions of supplying high frequency power to an electrode provided in the processing chamber, the insulating film 110 is 0, a dense silicon oxide film or silicon oxynitride film can be formed. .

[0254] The insulating film 110_0 may be formed by using a PECVD method using microwaves. Microwaves refer to the frequency range from 300MHz to 300GHz. The temperature is low and the electron energy is small. Also, the amount of power used to accelerate the electrons is small. The proportion of the oxygen that can be absorbed is small, and the oxygen can be used to dissociate and ionize a larger number of molecules. It is possible to excite a high density plasma. and forming an insulating film 110_0 with few defects while minimizing plasma damage to the deposit. can be done.

[0255] In addition, the insulating film 110_0 can be formed by a CVD method using an organic silane gas. As an organic silane gas, ethyl silicate (TEOS: chemical formula Si(OC2H5)4 ), tetramethylsilane (TMS: chemical formula Si(CH3)4), tetramethylcyclotetramethylsilane (TMS: chemical formula Si(CH3)4), Lasiloxane (TMCTS), Octamethylcyclotetrasiloxane (OMCTS), Hexamethyldisilazane (HMDS), triethoxysilane (SiH(OC2H5)3), Silicon-containing compounds such as trisdimethylaminosilane (SiH(N(CH3)2)3) By using the CVD method using organic silane gas, it is possible to obtain a high coating property. An insulating film 110_0 can be formed.

[0256] In this embodiment, a PECVD apparatus is used to deposit a 100 nm thick insulating film 110_0. A silicon oxynitride film is formed.

[0257] Next, a mask is formed by lithography at a desired position on the insulating film 110_0, The insulating film 110_0 and part of the insulating film 104 are etched to reach the conductive film 106. An opening 143 is formed through the insulating film 144 (see FIG. 7(C)).

[0258] The opening 143 can be formed by wet etching or dry etching. In this embodiment, a dry etching method is used. 2. The opening 143 is formed using the fluorine-containing ...

[0259] Next, the conductive film 11 is formed on the conductive film 106 and the insulating film 110_0 so as to cover the opening 143. In addition, when a metal oxide film is used as the conductive film 112_0, for example, In some cases, oxygen may be added to the insulating film 110_0 during the formation of the conductive film 112_0 (FIG. 7(D) )reference).

[0260] In FIG. 7D, oxygen added to the insulating film 110_0 is represented by arrows. In addition, the conductive film 112_0 is formed so as to cover the opening 143. The film 106 and the conductive film 112_0 are electrically connected to each other.

[0261] When a metal oxide film is used as the conductive film 112_0, the conductive film 112_0 is formed by In this case, it is preferable to use a sputtering method and form the layer in an atmosphere containing oxygen gas. The conductive film 112_0 is formed in an atmosphere containing oxygen gas, so that the insulating film 110 In addition, oxygen can be suitably added to the conductive film 112_0. The deposition method is not limited to the sputtering method, and other methods, such as the ALD method, may be used.

[0262] In this embodiment, the conductive film 112_0 is formed by a sputtering method. The thickness of the IGZO film is 100 nm. 4.1 (atomic ratio). Also, before the formation of the conductive film 112_0 or the conductive film 112 After the insulating film 110_0 is formed, oxygen addition treatment may be performed in the insulating film 110_0. The method for this can be the same as the oxygen addition treatment that can be performed after the formation of the insulating film 104. Good.

[0263] Next, a mask 140 is formed at a desired position on the conductive film 112_0 by a lithography process. (See FIG. 8(A)).

[0264] Next, etching is performed from above the mask 140 to remove the conductive film 112_0 and the insulating film 110 After the conductive film 112_0 and the insulating film 110_0 are processed, the mask 14 By processing the conductive film 112_0 and the insulating film 110_0, an island-shaped conductive A film 112 and an island-shaped insulating film 110 are formed (see FIG. 8(B)).

[0265] In this embodiment, the conductive film 112_0 and the insulating film 112_1 are formed by dry etching. Process 110_0.

[0266] Note that when the conductive film 112 and the insulating film 110 are processed, the conductive film 112 is not overlapped with the insulating film 110. The thickness of the metal oxide film 108 may become thin. During the processing of 110, the thickness of the insulating film 104 in the region where the metal oxide film 108 does not overlap is thin. In addition, when processing the conductive film 112_0 and the insulating film 110_0, etching may occur. A solvent or etching gas (e.g., chlorine) is added to the metal oxide film 108. Alternatively, the conductive film 112_0 or the insulating film 110_0 may have a metal oxide film 108 It may be added inside.

[0267] Next, the insulating film 116 is formed on the insulating film 104, the metal oxide film 108, and the conductive film 112. Note that by forming the insulating film 116, the metal oxide film 108 in contact with the insulating film 116 is A part of this becomes the region 108n (see FIG. 8C).

[0268] The insulating film 116 can be formed by selecting the above-mentioned material. In this example, a silicon oxynitride film having a thickness of 100 nm is deposited as the insulating film 116 using a PECVD apparatus. In forming the silicon oxynitride film, a plasma treatment is performed. The two steps of the plasma treatment, the deposition treatment and the deposition treatment, are carried out at a temperature of 220° C. Argon gas with a flow rate of 100 sccm and nitrogen gas with a flow rate of 1000 sccm were introduced into the chamber before the The pressure in the chamber was set to 40 Pa, and the RF power source (27.12 MHz) was turned on. The power of 1000W is supplied to the silane gas at a flow rate of 50sccm for the film formation process. The mixture was mixed with nitrogen gas at a flow rate of 5000 sccm and ammonia gas at a flow rate of 100 sccm. The pressure in the chamber was set to 100 Pa, and the RF power source (27.12 M It supplies 1000W of power to a frequency of 1000 Hz.

[0269] By using a silicon nitride oxide film as the insulating film 116, the region in contact with the insulating film 116 Nitrogen or hydrogen in the silicon nitride oxide film can be supplied to 108n. By setting the temperature during the formation of the film 116 to the above temperature, the excess oxygen contained in the insulating film 110 is It is possible to suppress the release of the hydrogen to the outside.

[0270] Next, the insulating film 118 is formed on the insulating film 116 (see FIG. 9A).

[0271] The insulating film 118 can be formed by selecting the above-mentioned material. In this example, a PECVD apparatus is used to deposit a silicon oxynitride film having a thickness of 300 nm as the insulating film 118. Form a cone film.

[0272] Next, a mask is formed by lithography at a desired position on the insulating film 118, and then the insulating film 118 and a part of the insulating film 116 are etched to form an opening 111 reaching the region 108n. 41a and 141b are formed (see FIG. 9(B)).

[0273] The method for etching the insulating film 118 and the insulating film 116 is a wet etching method. Either one or both of the dry etching method and the dry etching method may be used. For this purpose, the insulating film 118 and the insulating film 116 are processed by dry etching.

[0274] Next, a conductive layer is formed on the region 108n and the insulating film 118 so as to cover the openings 141a and 141b. The conductive film is then processed into a desired shape to form the conductive films 120a and 120b. (See FIG. 9(C)).

[0275] The conductive films 120a and 120b can be formed by selecting the above-mentioned materials. In the embodiment, a sputtering device is used to deposit the conductive films 120a and 120b. A laminate film of a 50 nm thick tungsten film and a 400 nm thick copper film is formed.

[0276] The conductive films 120a and 120b are processed by wet etching. Either one or both of a rubbing method and a dry etching method may be used. The copper film is etched by wet etching, and then the tin film is removed by dry etching. The conductive film is processed by etching the stainless steel film to form conductive films 120a and 120b. do.

[0277] Next, the insulating film 122 is formed to cover the conductive films 120a and 120b and the insulating film 118. do.

[0278] Through the above steps, a transistor 150 shown in FIGS. 5(A), 5(B), and 5(C) is manufactured. can be done.

[0279] The films (insulating film, metal oxide film, conductive film, etc.) constituting the transistor 150 include In addition to the above-mentioned forming method, sputtering method, chemical vapor deposition (CVD) method, vacuum deposition method, pas The thin-film transistor can be formed by using pulsed laser deposition (PLD) or ALD. It can be formed by a cloth method or a printing method. The film forming method includes a sputtering method, a plasma A typical example is a chemical vapor deposition (PECVD) method, but a thermal CVD method may also be used. Examples of thermal CVD methods As an example, metal-organic chemical vapor deposition (MOCVD) is mentioned.

[0280] In the thermal CVD method, the pressure in the chamber is set to atmospheric pressure or reduced pressure, and the source gas and the oxidizing agent are simultaneously The reaction is carried out in the chamber near or on the substrate, where it is deposited on the substrate to form a film. As described above, the thermal CVD method is a film formation method that does not generate plasma. This has the advantage that defects are not generated due to damage.

[0281] Thermal CVD methods such as MOCVD can be used to form the above-mentioned conductive films, insulating films, metal oxide films, and other films. can be formed.

[0282] For example, when forming a hafnium oxide film using a film forming apparatus that uses ALD, the solvent and a liquid containing a hafnium precursor (hafnium alkoxide or tetrakis(dimethylamine) (TDMAH, Hf[N(CH3)2]4) and tetrakis(ethylmethyl The raw material gas is made of vaporized hafnium amide, such as hafnium amide, and oxidizer, oxynitride, etc. Two types of gases are used: O2, O3, and NH3.

[0283] In addition, when forming an aluminum oxide film using a film forming apparatus that uses ALD, a solvent and a liquid containing an aluminum precursor (trimethylaluminum (TMA, Al(CH3)3 Two types of gases are used: the raw material gas made by vaporizing ethanol, etc., and H2O as an oxidizing agent. The materials used are tris(dimethylamido)aluminum, triisobutylaluminum, and aluminium. Aluminum tris(2,2,6,6-tetramethyl-3,5-heptanedionate), etc. There is.

[0284] In addition, when forming a silicon oxide film using a deposition system that uses ALD, The silane is adsorbed on the surface to be coated and the radicals of oxidizing gases (O2, nitrous oxide) are provided. is fed to react with the adsorbate.

[0285] In addition, when forming a tungsten film using a deposition system that uses ALD, WF6 gas is used. The initial tungsten film is formed by sequentially introducing WF6 gas and H The tungsten film is formed using the B2H6 gas instead of the SiH4 gas. may also be used.

[0286] In addition, metal oxide films, such as In-Ga-Zn-O films, can be formed using ALD deposition equipment. In the case of forming a film, the In-O layer is formed using In(CH3)3 gas and O3 gas, and then Then, a GaO layer was formed using Ga(CH3)3 gas and O3 gas, and then a Zn( The ZnO layer is formed using CH3)2 gas and O3 gas. The order of these layers is as follows: In addition, the following examples are not limited to the above. In-Ga-O layers, In-Zn-O layers, and G A mixed compound layer such as a-Zn-O layer may be formed. Note that, instead of O3 gas, Ar gas, etc. HO gas obtained by bubbling water with an inert gas may be used, but O gas containing no H It is preferable to use three gases.

[0287] The above is a description of the method for manufacturing a semiconductor device.

[0288] This embodiment may be combined, at least in part, with other embodiments described in this specification. It can be implemented in combination.

[0289] (Embodiment 3) In this embodiment, the CAC (Cloud-A) of the oxide semiconductor film of one embodiment of the present invention is This paper explains the structure of the Integrated Composite Operating System (ILOS).

[0290] <3-1. CAC Structure> CAC is a film in which an element constituting an oxide semiconductor film is formed with a thickness of 0.5 nm or more and 10 nm or less. In general, the material is unevenly distributed in the size range of 1 nm to 2 nm, or in the vicinity thereof. In the following description, it is assumed that one or more metal elements in an oxide semiconductor film are 0.5 nm or more and 10 nm or less, preferably 1 nm or more and 2 nm or less, or a size close to that. The mixed state is also called a mosaic or patch pattern.

[0291] For example, CAC-IG in In-Ga-Zn oxide (hereinafter also referred to as IGZO) ZO is indium oxide (InO X1 (X1 is a real number greater than 0.) or indium zinc oxide (hereinafter, In X2 Zinc Y2 O Z2 (X2, Y2, and Z2 are A real number greater than 0.)) and gallium oxide (GaO X3 (X3 is greater than 0 ) or gallium zinc oxide (Ga X4 Zinc Y4 O Z4 (X4, Y4 , and Z4 is a real number greater than . )) and so on, the material separates and becomes mosaic-like. , mosaic InO X1 , or In X2 Zinc Y2 O Z2 is distributed in the oxide semiconductor film It is a structure similar to that of a cloud.

[0292] In other words, CAC-IGZO is X2 Zinc Y2 O Z2 , or InO X1 is the main component A certain area and GaO X3 A composite structure in which the main component is unevenly distributed and mixed. The oxide semiconductor film is In X2 Zinc Y2 O Z2 , or InO X1 The main component is The area where GaO X3 The area where the main component is the area where the periphery is unclear (blurred) Therefore, the boundaries between them may not be clearly observable.

[0293] IGZO is a common name and refers to a compound made of In, Ga, Zn, and O. A typical example is InGaO3(ZnO). m1 (m1 is a natural number), or In (1+x0) Ga (1-x0) O3(ZnO) m0 (-1≦x0≦1, m0 is an arbitrary number) Examples of the crystalline compound include those represented by the following formula:

[0294] The crystalline compound has a single crystal structure, a polycrystalline structure, or a CAAC structure. The CAAC structure is a structure in which multiple IGZO nanocrystals have a c-axis orientation and are aligned in the ab plane. is a non-oriented connected crystal structure.

[0295] On the other hand, CAC refers to the material composition. CAC includes In, Ga, Zn, and O. In terms of the material composition, some areas are observed to be nanoparticles with Ga as the main component, while others are observed to be I The regions observed are randomly divided into mosaic-like regions, with the nanoparticles consisting mainly of n. Therefore, in CAC, the crystal structure is a secondary element. The regions mainly composed of Ga and the regions mainly composed of In were evaluated by EDX mapping. The region mainly composed of Ga and the region mainly composed of In can be divided into two groups. These may be called nanoparticles. The nanoparticles are those with a particle diameter of 0.5 nm or more and 10 nm or less. The nanoparticles are typically between 1 nm and 2 nm in size. In some cases, the boundaries may not be clearly visible due to the blurred nature of the image.

[0296] Note that CAC does not include a laminated structure of two or more films with different compositions. For example, a structure consisting of two layers, one containing In as the main component and the other containing Ga as the main component, is not included. .

[0297] In addition, GaO X3 The region where In is the main component and X2 Zinc Y2 O Z2 , or InO X1 In some cases, it may be difficult to observe a clear boundary between the area where the main component is the The density of the main component element gradually decreases from the center to the periphery. In the EDX mapping of Since the area has a gradient in the amount of light present, the periphery of the area is observed in an unclear (blurred) state. Specifically, GaO X3 In the region where Ga is the main component, Ga atoms are distributed from the center to the periphery. Instead, the number of Zn atoms increases, and the number of Ga atoms increases. X Zinc Y O Z is the main component Therefore, in EDX mapping, the GaO X3 Mainly The periphery of the component regions is observed to be unclear (blurred).

[0298] <3-2.Analysis of CAC-IGZO> Next, the oxide semiconductor film formed on the substrate was measured using various measurement methods. The results will be explained.

[0299] [Sample composition and preparation method] Nine samples according to one embodiment of the present invention will be described below. Each sample has the following characteristics: The oxide semiconductor film is formed under different conditions of the substrate temperature and the oxygen gas flow rate ratio. Note that the sample has a structure including a substrate and an oxide semiconductor film over the substrate.

[0300] The preparation method of each sample will be described.

[0301] First, a glass substrate is used as the substrate. Then, the glass is A 100 nm thick In-Ga-Zn oxide film is formed on the silicon substrate as an oxide semiconductor film. The film conditions were a pressure of 0.6 Pa in the chamber and a metal oxide target. In:Ga:Zn=4:2:4.1 [atomic ratio] is used. A metal oxide target placed in the apparatus is supplied with 2500 W of AC power.

[0302] As a condition for forming an oxide film, the substrate temperature is set to a temperature at which the substrate is not intentionally heated (hereinafter The temperature was set to 130°C, 170°C, or 180°C. The oxygen gas flow rate ratio to the gas (also called oxygen gas flow rate ratio) can be set to 10%, 30%, or 1 00%, and nine samples are prepared.

[0303] [X-ray diffraction analysis] In this section, X-ray diffraction (XRD) was performed on nine samples. The results of the measurement are described below. The XRD device used was a Bruker product. D8 ADVANCE was used. The conditions were θ / In 2θ scan, the scanning range is 15 deg. to 50 deg., and the step width is 0.02d. For example, the scanning speed was 3.0 deg. / min.

[0304] Figure 11 shows the results of measuring the XRD spectrum using the out-of-plane method. In addition, in Fig. 11, the upper row shows the measurement results for a sample where the substrate temperature during film formation was 170°C. The middle row shows the measurement results for a sample with a substrate temperature of 130°C during film formation, and the lower row shows the film formation The left column shows the results of measurements taken with the substrate temperature at RT. The center column shows the results of measurements taken with the gas flow rate ratio at 10%. The right column shows the results for the sample with a 30% oxygen gas flow rate, and the right column shows the results for the sample with a 100% oxygen gas flow rate. The measurement results are shown below.

[0305] The XRD spectrum shown in FIG. 11 shows that the increase in the substrate temperature during film formation or the increase in the amount of acid during film formation By increasing the ratio of the atomic gas flow rate, the peak intensity around 2θ=31° increases. The peak at 2θ=31° indicates that the c-axis is aligned in the direction approximately perpendicular to the surface on which the film is formed or the upper surface. The c-axis aligned crystal of IGZO compound (CAAC) It is known that this is due to the fact that it is an insulated gate oxide (IGZO).

[0306] In addition, the XRD spectrum shown in FIG. 11 shows that the substrate temperature during film formation was low or the oxygen gas The smaller the flow rate ratio, the less clear the peak. Alternatively, the sample with a small oxygen gas flow rate ratio had ab-plane and c-axis orientations in the measurement area. It can be seen that no direction is visible.

[0307] [Electron microscopy analysis] In this section, the samples were prepared at a substrate temperature of RT during film formation and an oxygen gas flow rate of 10%. ,HAADF(High-Angle Annular Dark Field)-S TEM(Scanning Transmission Electron Micro The results of the observation and analysis using the HAADF-scope are described below (hereafter, HAADF- Images obtained by STEM are also called TEM images.

[0308] Planar images (also called planar TEM images) and cross-sections obtained by HAADF-STEM The results of image analysis of the cross-sectional TEM image are explained below. The M image was observed using a spherical aberration correction function. Using an atomic resolution analytical electron microscope JEM-ARM200F manufactured by JEOL Ltd., The electron beam was irradiated at a voltage of 200 kV with a beam diameter of approximately 0.1 nmφ.

[0309] FIG. 12(A) shows a film formed at a substrate temperature of RT and an oxygen gas flow rate of 10%. The planar TEM image of the sample is shown in Fig. 12(B). The cross-sectional TEM image of a sample prepared with a gas flow rate of 10%.

[0310] [Analysis of electron diffraction patterns] In this section, the samples were prepared at a substrate temperature of RT during film formation and an oxygen gas flow rate of 10%. By irradiating the sample with an electron beam with a probe diameter of 1 nm (also called a nano-beam electron beam), The results of acquiring sagittal diffraction patterns will now be described.

[0311] As shown in FIG. 12(A), the substrate temperature during film formation was RT, and the oxygen gas flow rate was 10%. In the planar TEM image of the sample, black spots a1, a2, a3, a4, and The electron diffraction pattern shown at point a5 is observed. The line is projected and moved at a constant speed from the 0 second position to the 35 second position. The results for point a1 are shown in Fig. 12(C), the results for black point a2 are shown in Fig. 12(D), and the results for black point a3 are shown in Fig. 12(E). (E), the results for black spot a4 are shown in FIG. 12(F), and the results for black spot a5 are shown in FIG. 12(G).

[0312] From Fig. 12(C), Fig. 12(D), Fig. 12(E), Fig. 12(F), and Fig. 12(G) In the image, a circular (ring-shaped) area of ​​high brightness can be observed. Multiple spots can be observed.

[0313] In addition, as shown in FIG. 12(B), the substrate temperature RT during film formation and the oxygen gas flow rate ratio of 10% In the cross-sectional TEM image of the sample prepared in the above, black spots b1, b2, b3, b4, and Observe the electron diffraction patterns indicated by black spots b1 and b5. The results for point b2 are shown in Fig. 12(I), the results for black point b3 are shown in Fig. 12(J), and the results for black point b4 are shown in Fig. 12(K). The results for (K) and black spot b5 are shown in Figure 12(L).

[0314] From Fig. 12(H), Fig. 12(I), Fig. 12(J), Fig. 12(K), and Fig. 12(L) A ring-shaped area of ​​high brightness can be observed. In addition, multiple spots can be observed in the ring-shaped area. It can be measured.

[0315] For example, for a CAAC-OS having an InGaZnO4 crystal, When an electron beam with a probe diameter of 300 nm is incident on the row, the (00 9) The diffraction pattern includes spots due to the CAAC-OS It has been found that the film has a c-axis orientation, and the c-axis is oriented in a direction substantially perpendicular to the surface on which the film is formed or the upper surface. On the other hand, an electron beam with a probe diameter of 300 nm is incident perpendicularly to the surface of the same sample. In other words, the CAAC-OS has a ring-shaped diffraction pattern along the a-axis and It is clear that the b-axis has no orientation.

[0316] In addition, a nanocrystalline oxide semiconductor film e semiconductor. Hereafter referred to as nc-OS.) When electron diffraction is performed using an electron beam with a diameter (e.g., 50 nm or more), a halo pattern is observed. In addition, a small-diameter electron beam (e.g. When nanobeam electron diffraction is performed using a material with a diameter of less than 50 nm, bright spots are observed. In addition, when nanobeam electron diffraction was performed on nc-OS, a circular structure (ring) was observed. In some cases, a bright area with multiple bright spots (like a ring) is observed. It may be observed.

[0317] Electron beam diffraction of a sample prepared at substrate temperature RT during film formation and oxygen gas flow rate of 10% The pattern has a ring-shaped area of ​​high brightness and multiple bright points in the ring area. The sample was fabricated at a substrate temperature of RT and an oxygen gas flow rate of 10% during film formation. The folding pattern is nc-OS, and there is no orientation in the planar direction or cross-sectional direction. stomach.

[0318] From the above, the oxide semiconductor film formed at a low substrate temperature or a low oxygen gas flow rate is clearly different from an oxide semiconductor film having an amorphous structure and an oxide semiconductor film having a single crystal structure. It can be assumed that the material has the following properties.

[0319] [Elemental analysis] In this article, we will discuss energy dispersive X-ray spectroscopy (EDX). EDX mapping was obtained and evaluated using vective X-ray spectroscopy. By evaluating the film formation, the substrate temperature was set at RT and the oxygen gas flow rate was set at 10%. The results of elemental analysis of the samples are described below. The energy dispersive X-ray analyzer JED-2300T manufactured by JEOL Ltd. is used as the analyzer. A Si drift detector is used to detect the X-rays emitted from the sample.

[0320] In EDX measurement, each point in the analysis area of ​​the sample is irradiated with an electron beam, The energy and frequency of the characteristic X-rays of the sample are measured, and the EDX spectrum corresponding to each point is obtained. In this example, the peaks in the EDX spectrum at each point are determined as electron transitions to the L shell of the In atom, Electron transition to the K shell of Ga atom, electron transition to the K shell of Zn atom, and electron transition to the K shell of O atom The ratio of each atom at each point is calculated. By performing EDX analysis on the area, it is possible to obtain EDX mapping that shows the distribution of the ratio of each atom. can be done.

[0321] FIG. 13 shows the results of the deposition of the sample at the substrate temperature RT and oxygen gas flow rate of 10%. FIG. 13(A) shows EDX mapping of Ga atoms. (The ratio of Ga atoms to the total atoms is in the range of 1.18 to 18.64 [atomic%].) (B) shows the EDX mapping of In atoms (the ratio of In atoms to the total atoms). The ratio of the number of children is in the range of 9.28 to 33.74 [atomic%]. (C) EDX mapping of Zn atoms (ratio of Zn atoms to total atoms is 6.69 to 8.74). 24.99 [atomic%] range.) Also, Fig. 13(A) and Fig. 13( 13B) and FIG. 13C show the substrate temperature RT and the oxygen gas flow rate ratio 10% during film formation. The cross section of the sample prepared in step 1 shows the same area. The more elements in the range are measured, the brighter the light becomes, and the fewer elements in the range are measured, the darker the light becomes. The ratio of elements is shown by light and dark in the EDX mapping shown in Fig. 13. The magnification of the EDX mapping shown in Fig. 13 was 72. 0 million times.

[0322] In the EDX mapping shown in Figures 13(A), 13(B), and 13(C), the images The relative light and dark distribution can be seen in the figure. The substrate temperature RT and oxygen gas flow rate ratio during film formation are In the sample made at %, it can be seen that each atom exists with a certain distribution. In Fig. 13(A), Fig. 13(B), and Fig. 13(C), the areas surrounded by solid lines and the areas surrounded by dashed lines are Pay attention to the range.

[0323] In FIG. 13(A), the area enclosed by the solid line includes many relatively dark areas, and the area enclosed by the dashed line includes many relatively dark areas. In FIG. 13B, the area surrounded by the solid line contains many relatively bright areas. The area surrounded by the dashed line contains many relatively bright areas, while the area surrounded by the dashed line contains many relatively dark areas.

[0324] In other words, the area surrounded by the solid line is the area with a relatively large amount of In atoms, and the area surrounded by the dashed line is the area with a relatively large amount of In atoms. This is a region with relatively few atoms. In FIG. 13C, the area surrounded by the solid line The right side is a relatively bright area, and the left side is a relatively dark area. The range is In X2 Zinc Y2 O Z2 , or InO X1 This is an area where the main components are:

[0325] The area surrounded by the solid line is the area with relatively few Ga atoms, and the area surrounded by the dashed line is the area with relatively few Ga atoms. In Fig. 13(C), the upper left area in the area enclosed by the dashed line is The upper right area is a relatively bright area, and the lower right area is a relatively dark area. The area enclosed by the dashed line is GaO X3 , or Ga X4 Zinc Y4 O Z4 Areas where the main components are It is.

[0326] In addition, from Fig. 13(A), Fig. 13(B), and Fig. 13(C), the distribution of In atoms is G It is relatively more uniformly distributed than a atoms, and InO X1 The region where is the main component is In X 2Zn Y2 O Z2 It appears that the two are connected to each other through the regions where In this way, X2 Zinc Y2 O Z2 , or InO X1 The area where is the main component is It spreads and forms like a cloud.

[0327] Thus, there are regions where GaO is the main component and regions where In is the main component. X2 Zinc Y2 O Z2 , or InO X In-Ga-Zn oxide with a structure in which the regions in which 1 is the main component are unevenly distributed and mixed This can be called CAC-IGZO.

[0328] In addition, from Figs. 13(A), 13(B), and 13(C), GaO X3 is the main component In a certain area, and In X2 Zinc Y2 O Z2 , or InO X1The size of the region in which is the principal component is observed to be 0.5 nm to 10 nm or 0.3 nm to 3 nm. Preferably, in the EDX mapping, the diameter of the region in which each metal element is the main component is 1n The thickness should be between m and 2 nm.

[0329] From the above, CAC-IGZO is different from IGZO compounds in which metal elements are uniformly distributed. CAC-IGZO has a Ga structure and has different properties from IGZO compounds. O X3 The main components are In X2 Zinc Y2 O Z2 , or InO X1 is the main component Therefore, when CAC-IGZO is used in a semiconductor device, X3 The properties due to In X2 Zinc Y2 O Z2 , or InO X1 Properties resulting from The complementary action of these two results in a high on-state current (I on ), and high field-effect mobility It is possible to achieve a degree (μ).

[0330] When CAC-IGZO is used in semiconductor devices, it has a high on-state current (I on ), and The conduction mechanism that realizes the extremely high field effect mobility (μ) is one of the percolation theories. It can be estimated by a random resistor network model where

[0331] In addition, semiconductor elements using CAC-IGZO have high reliability. ZO is ideal for a variety of semiconductor devices, including displays.

[0332] This embodiment may be combined, at least in part, with other embodiments described in this specification. It can be implemented in combination.

[0333] (Embodiment 4) In this embodiment, one of the display devices including the semiconductor device exemplified in the above embodiment is An example will be described below with reference to FIGS.

[0334] <4-1. Display device configuration examples> 14 is a top view showing an example of a display device. The display device 700 shown in FIG. A pixel portion 702 is provided on the first substrate 701, and a source driver is provided on the first substrate 701. A pixel portion 702, a source driver circuit portion 704, a gate driver circuit portion 706, A sealant 712 is disposed so as to surround the path portion 704 and the gate driver circuit portion 706. and a second substrate 705 disposed so as to face the first substrate 701. The first substrate 701 and the second substrate 705 are sealed with a sealant 712. That is, the pixel section 702, the source driver circuit section 704, and the gate driver circuit section 706 are The first substrate 701, the sealant 712, and the second substrate 705 seal the entire structure. Although not shown in FIG. 14, a display element is provided between the first substrate 701 and the second substrate 705. can be done.

[0335] The display device 700 is surrounded by a sealant 712 on the first substrate 701. A pixel section 702, a source driver circuit section 704, and a gate driver circuit section 705 are arranged in a region different from the region. The flexible printed circuit (FPC) terminals 708 (FPC: Flex) are electrically connected to the respective flexible printed circuit (FPC) terminals 706. Also, an FPC terminal portion 708 is provided. An FPC 716 is connected to the pixel section 702 and the source driver circuit. Various signals are supplied to the path section 704 and the gate driver circuit section 706. 702, a source driver circuit section 704, a gate driver circuit section 706, and an FPC terminal section Signal lines 710 are connected to the terminals 708. Various signals are supplied by the FPC 716. The signals are transmitted through a signal line 710 to a pixel section 702, a source driver circuit section 704, a gate driver A driver circuit portion 706 and an FPC terminal portion 708 are provided.

[0336] The display device 700 may include a plurality of gate driver circuits 706. The device 700 includes a source driver circuit section 704 and a gate driver circuit section 706. Although an example in which the pixel portion 702 is formed on the same first substrate 701 is shown, the present invention is not limited to this configuration. For example, only the gate driver circuit section 706 may be formed on the first substrate 701. Alternatively, only the source driver circuit section 704 may be formed on the first substrate 701. In this case, the substrate on which the source driver circuit or the gate driver circuit is formed (for example, A driving circuit board formed of a monocrystalline semiconductor film or a polycrystalline semiconductor film is formed on a first substrate 701. The method of connecting the separately formed drive circuit board is not particularly limited. Instead, we use COG (Chip On Glass) method, wire bonding method, etc. can be used.

[0337] The display device 700 also includes a pixel portion 702, a source driver circuit portion 704, and a gate The driver circuit section 706 includes a plurality of transistors.

[0338] The display device 700 can also include various elements, such as: For example, electroluminescence (EL) elements (EL elements including organic and inorganic materials, organic EL elements, inorganic EL elements, LEDs, etc.), light-emitting transistor elements (light-emitting elements that emit light according to electric current) transistors, electron emission elements, liquid crystal elements, electronic ink elements, electrophoretic elements, Rowetting element, plasma display panel (PDP), MEMS (microelectromechanical systems) Electro-mechanical systems) displays (e.g., grating light bars) GLV, Digital Micromirror Device (DMD), Digital Microsha Dispersive Modulation (DMS) element, Interferometric Modulation (IMOD) element ), piezoelectric ceramic displays, etc.

[0339] An example of a display device using an EL element is an EL display. An example of a display device using emission elements is a field emission display (FE D) or SED type flat panel display (SED: Surface-conductio n Electron-emitter Display) and others. An example of such a display device is a liquid crystal display (transmissive liquid crystal display, semi-transmissive liquid crystal display, etc.). Display, reflective LCD display, direct-view LCD display, projection LCD display Examples of display devices using electronic ink elements or electrophoretic elements include: Electronic paper. Semi-transmissive LCDs and reflective LCDs are also used. In this case, a part or the whole of the pixel electrode should function as a reflective electrode. For example, a part or the whole of the pixel electrode may be made of aluminum, silver, etc. In this case, a memory circuit such as an SRAM may be provided under the reflective electrode. This can further reduce power consumption.

[0340] The display method of the display device 700 may be a progressive method or an interlace method. In addition, the color elements controlled by pixels when displaying in color are R It is not limited to the three colors GB (R stands for red, G stands for green, B stands for blue). For example, It may be composed of four pixels: a pixel, a pixel, and a pixel of white (W). As in the column, two colors of RGB form one color element, and different two colors are generated depending on the color element. You can also select colors to configure the color. Or, you can select one or more colors such as yellow, cyan, and magenta for RGB. The size of the display area may be different for each dot of the color element. However, the disclosed invention is not limited to color display devices, and may be used in monochrome display devices. The present invention can also be applied to display devices.

[0341] Also, white light is emitted from the backlight (organic EL element, inorganic EL element, LED, fluorescent lamp, etc.) In order to display full color using (W), a colored layer (also called a color filter) is The colored layer may be, for example, red (R), green (G), blue (B), or red (C). ), yellow (Y), etc. can be used in appropriate combination. In this case, the color reproducibility can be improved compared to when no color layer is used. By disposing a region having a color layer and a region not having a color layer, The white light in the region may be directly used for display. This reduces the decrease in brightness caused by the colored layer during bright display, reducing power consumption by 20%. However, it may be possible to reduce the light emission by about 30% when using self-luminous elements such as organic EL elements and inorganic EL elements. When using a full-color display, R, G, B, Y, and W are each emitting different colors. By using a self-luminous element, it is possible to obtain a more uniform light emission than when a colored layer is used. In some cases, power consumption can be further reduced.

[0342] In addition, as a colorization method, a part of the light emitted from the above-mentioned white light is passed through a color filter. In addition to the color filter method, which converts the light into red, green, and blue by filtering the light, A method that uses two colors of light (three-color method), or a method that uses part of the light emitted from the blue light to emit red or A method for converting to green (color conversion method, quantum dot method) may be applied.

[0343] In this embodiment, a liquid crystal element and an EL element are used as display elements. 15 to 17. Note that FIGS. 15 and 16 are diagrams showing the dot-and-dash pattern shown in FIG. FIG. 1 is a cross-sectional view taken along line QR, showing a configuration in which a liquid crystal element is used as a display element. 17 is a cross-sectional view taken along the dashed line QR in FIG. 14, in which an EL element is used as a display element. This is the configuration used.

[0344] First, the common parts shown in FIGS. 15 to 17 will be described, and then the different parts will be described. This will be explained below.

[0345] <4-2. Explanation of common parts of display device> A display device 700 shown in FIGS. 15 to 17 includes a wiring portion 711 and a pixel portion 702. The display panel 700 includes a source driver circuit section 704 and an FPC terminal section 708. The line portion 711 includes a signal line 710. The pixel portion 702 includes a transistor 750 and The source driver circuit portion 704 includes a transistor 752. Yes.

[0346] Transistor 750 and transistor 752 are similar to transistor 150 shown above. The structures of the transistors 750 and 752 are the same as those described above. Any other transistors than those shown in the embodiment modes may be used.

[0347] The transistor used in this embodiment is made of a highly purified oxide film in which the formation of oxygen vacancies is suppressed. The transistor has a semiconductor film. The off-state current of the transistor can be reduced. It is possible to extend the retention time of electrical signals such as signals, and the write interval can be extended when the power is on. This allows the frequency of refresh operations to be reduced, resulting in reduced power consumption. It has the effect of suppressing power.

[0348] In addition, the transistor used in this embodiment has a relatively high field-effect mobility. For example, a transistor capable of such high speed operation can be used for a liquid crystal display. By using this in a display device, the switching transistor in the pixel section and the driver circuit section In other words, the driver transistor can be formed on the same substrate as the driver circuit. Therefore, it is not necessary to use a semiconductor device formed from a silicon wafer or the like. The number of parts can be reduced. By using a register, a high quality image can be provided.

[0349] The capacitor 790 includes a conductive film that functions as a first gate electrode of the transistor 750. The lower electrode formed through a process of processing the same conductive film and the Through a process of processing the same conductive film as the conductive film that functions as the source electrode and the drain electrode, and an upper electrode formed on the lower electrode. A step of forming an insulating film identical to the insulating film functioning as the first gate insulating film of 750. and an insulating film that functions as a protective insulating film over the transistor 750. In other words, the insulating film is formed through the same process as that for forming the capacitive element. The element 790 has a laminated structure in which an insulating film that functions as a dielectric film is sandwiched between a pair of electrodes. be.

[0350] 15 to 17, a transistor 750, a transistor 752, and a capacitor A planarization insulating film 770 is provided on the capacitor 790 .

[0351] 15 to 17, a transistor 750 and a A transistor having the same structure as the transistor 752 included in the source driver circuit portion 704 is used. The configuration used is illustrated above, but is not limited to this. For example, A transistor different from that in the driver circuit section 704 may be used. A top-gate transistor is used for the source driver circuit section 702, and a bottom-gate transistor is used for the source driver circuit section 704. A structure using a bottom-gate transistor in the pixel portion 702. The source driver circuit section 704 is configured to use a top-gate type transistor. The source driver circuit section 704 may be referred to as a gate driver circuit section. It may be read differently.

[0352] The signal line 710 is connected to the source and drain electrodes of the transistors 750 and 752. The signal line 710 is formed through the same process as the conductive film that functions as the signal line 710. When materials containing this material are used, signal delays caused by wiring resistance are minimal, making it possible to display images on a large screen. It becomes Noh.

[0353] The FPC terminal portion 708 includes a connection electrode 760, an anisotropic conductive film 780, and an FPC 71. 6. The connection electrode 760 is connected to the source and drain electrodes of the transistors 750 and 752. The connection electrode 760 is formed through the same process as the conductive film that functions as the drain electrode. , and is electrically connected to a terminal of the FPC 716 via an anisotropic conductive film 780 .

[0354] The first substrate 701 and the second substrate 705 may be, for example, a glass substrate. In addition, the first substrate 701 and the second substrate 705 may be flexible substrates. The flexible substrate may be, for example, a plastic substrate. do.

[0355] In addition, a structure 778 is provided between the first substrate 701 and the second substrate 705. The structure 778 is a columnar spacer obtained by selectively etching an insulating film. A device for controlling the distance (cell gap) between the first substrate 701 and the second substrate 705 is provided. It should be noted that the structures 778 may be spherical spacers.

[0356] In addition, on the second substrate 705 side, a light-shielding film 738 functioning as a black matrix and A colored film 736 that functions as a color filter, a light-shielding film 738 that is in contact with the colored film 736, and An insulating film 734 is provided.

[0357] <4-3. Configuration examples of display devices using liquid crystal elements> The display device 700 shown in FIG. 15 includes a liquid crystal element 775. The liquid crystal element 775 includes a conductive film The conductive film 774 is a second substrate 705. The display device 700 shown in FIG. The alignment state of the liquid crystal layer 776 changes depending on the voltage applied to the conductive film 772 and the conductive film 774. By controlling the light transmission or non-transmission, an image can be displayed.

[0358] The conductive film 772 serves as a source electrode or a drain electrode of the transistor 750. The conductive film 772 is formed over the planarization insulating film 770. The pixel electrode functions as one electrode of the display element.

[0359] The conductive film 772 may be a conductive film that transmits visible light or a conductive film that reflects visible light. A conductive film having a reflectivity can be used. For example, a material containing one of the elements indium (In), zinc (Zn), and tin (Sn) As a conductive film that is reflective in visible light, for example, aluminum Alternatively, a material containing silver may be used.

[0360] In the case where a conductive film having a reflectivity to visible light is used as the conductive film 772, the display device 700 has the following characteristics: The liquid crystal display device is a reflective type. In this case, the display device 700 becomes a transmissive liquid crystal display device.

[0361] In addition, by changing the structure on the conductive film 772, the driving method of the liquid crystal element can be changed. An example of this case is shown in FIG. 16. The display device 700 shown in FIG. This is an example of a configuration using a horizontal electric field method (e.g., FFS mode) as a driving method. In the structure shown in FIG. 1, an insulating film 773 is provided over a conductive film 772, and a conductive film In this case, the conductive film 774 is used as a common electrode. The insulating film 773 functions as a conductive film between the conductive film 772 and the conductive film 774. The alignment state of the liquid crystal layer 776 can be controlled by the field.

[0362] Although not shown in FIGS. 15 and 16, the conductive film 772 or the conductive film 774 An alignment film is provided on either one or both of the surfaces of the liquid crystal layer 776. Although not shown in FIG. 15 and FIG. 16, a polarizing member, a phase difference member, a reflecting member, etc. Optical members (optical substrates) such as a polarizing substrate and a positioning member may be provided as appropriate. Circularly polarized light produced by a retardation substrate may be used. Either may be used.

[0363] When liquid crystal elements are used as display elements, thermotropic liquid crystal, low molecular weight liquid crystal, high molecular weight liquid crystal, For example, a liquid crystal, a polymer-dispersed liquid crystal, a ferroelectric liquid crystal, an antiferroelectric liquid crystal, etc. can be used. Depending on the conditions, the liquid crystal material can have a cholesteric phase, a smectic phase, a cubic phase, or a chiral phase. It shows nematic phase, isotropic phase, etc.

[0364] In addition, when the in-plane switching method is adopted, liquid crystal that exhibits a blue phase without using an alignment film may be used. The blue phase is one of the liquid crystal phases. When the temperature of a cholesteric liquid crystal is increased, the cholesteric The blue phase appears just before the transition from the black phase to the isotropic phase. In order to improve the temperature range, a liquid crystal composition containing a chiral agent of several weight percent or more is used. The liquid crystal composition containing the liquid crystal exhibiting the blue phase and the chiral agent is used in the liquid crystal layer. Since the liquid crystal display has a short rotational angle and is optically isotropic, no alignment treatment is required. Since the rubbing process is unnecessary, electrostatic damage caused by the rubbing process is prevented. This can prevent the occurrence of defects or damage to the liquid crystal display device during the manufacturing process. Furthermore, liquid crystal materials exhibiting a blue phase have little viewing angle dependency.

[0365] In addition, when liquid crystal elements are used as display elements, TN (Twisted Nematic) ) mode, IPS (In-Plane-Switching) mode, FFS (Frin ge Field Switching) mode, ASM (Axially Symme tric aligned Micro-cell) mode, OCB(Optical Compensated Birefringence mode, FLC (Ferrero lectric Liquid Crystal) mode, AFLC (AntiFerr Electro-Oelectric Liquid Crystal mode can be used. .

[0366] In addition, normally black type liquid crystal display devices, for example, those using a vertical alignment (VA) mode The vertical alignment mode may be a transmission type liquid crystal display device. For example, MVA (Multi-Domain Vertical Alignment) ) mode, PVA (Patterned Vertical Alignment) mode mode, ASV mode, etc. can be used.

[0367] <4-4. Display devices using light-emitting elements> The display device 700 shown in FIG. 17 includes a light-emitting element 782. The light-emitting element 782 is a conductive film The display device 700 shown in FIG. The EL layer 786 of the light element 782 emits light, thereby displaying an image. The EL layer 786 includes an organic compound or an inorganic compound such as quantum dots.

[0368] Examples of materials that can be used for the organic compound include fluorescent materials and phosphorescent materials. In addition, materials that can be used for quantum dots include colloidal quantum dots. materials, alloy type quantum dot materials, core-shell type quantum dot materials, core type quantum dot materials, In addition, the elements of the 12th and 16th families, the 13th and 15th families, or the 14th and 16th families Materials containing the element group may also be used. Cadmium (Cd), selenium (Se), Zinc (Zn), Sulfur (S), Phosphorus (P), Indium (In), Tellurium (Te), Lead (P b) Quantum with elements such as gallium (Ga), arsenic (As), aluminum (Al), etc. Dot material may also be used.

[0369] In the display device 700 shown in FIG. 17, an insulating film 770 is formed on a planarizing insulating film 770 and a conductive film 772. The insulating film 730 covers part of the conductive film 772. The EL layer 788 has a top emission structure. In this embodiment, the top emission structure is For example, a bottom that emits light to the conductive film 772 side is shown. A dual emission structure in which light is emitted to both the conductive film 772 and the conductive film 788 is also used. It can also be applied to mission structures.

[0370] A colored film 736 is provided at a position overlapping the light emitting element 782, and a colored film 736 is provided at a position overlapping the insulating film 730. A light-shielding film 738 is provided at the position where the light-shielding film 738 is to be formed, the wiring portion 711, and the source driver circuit portion 704. The colored film 736 and the light-shielding film 738 are covered with an insulating film 734. In addition, the space between the light emitting element 782 and the insulating film 734 is filled with a sealing film 732. In the display device 700 shown in FIG. 1, a configuration in which a colored film 736 is provided is illustrated. For example, when the EL layer 786 is formed by coloring, The film 736 may not be provided.

[0371] <4-5. Example of a configuration in which an input / output device is provided on a display device> In addition, the display device 700 shown in FIG. 16 and FIG. 17 may be provided with an input / output device. An example of the force device is a touch panel.

[0372] 18 and 17 show a configuration in which a touch panel 791 is provided on the display device 700 shown in FIG. FIG. 19 shows a configuration in which a touch panel 791 is provided on a display device 700.

[0373] FIG. 18 is a cross-sectional view of a configuration in which a touch panel 791 is provided on the display device 700 shown in FIG. FIG. 19 is a cross-sectional view of a configuration in which a touch panel 791 is provided on the display device 700 shown in FIG. be.

[0374] First, the touch panel 791 shown in FIG. 18 and FIG. 19 will be described below.

[0375] The touch panel 791 shown in FIG. 18 and FIG. The touch panel 791 is a so-called in-cell type touch panel. 736 may be formed on the substrate 705 side before the colored film 736 is formed.

[0376] The touch panel 791 includes a light-shielding film 738, an insulating film 792, an electrode 793, and an electrode 794, an insulating film 795, an electrode 796, and an insulating film 797. When a detection object such as a stylus approaches, a change in capacitance between electrode 793 and electrode 794 occurs. It is possible to detect the change.

[0377] 18 and 19, an electrode 793 and The electrode 796 is formed by passing through an opening in the insulating film 795. The electrode 794 is electrically connected to the two electrodes 793 that sandwich the electrode 794 via the electrodes 793. 19, a configuration in which the region where the electrode 796 is provided is provided in the pixel portion 702 is illustrated. However, the present invention is not limited to this. For example, the light emitting diode 704 may be formed in the source driver circuit section 704.

[0378] The electrodes 793 and 794 are provided in a region overlapping with the light-shielding film 738. As shown in FIG. 1, the electrode 793 is preferably provided so as not to overlap with the light-emitting element 782. In addition, as shown in FIG. 19, the electrode 793 is provided so as not to overlap with the liquid crystal element 775. In other words, the electrode 793 overlaps with the light-emitting element 782 and the liquid crystal element 775. In other words, the electrode 793 has a mesh shape. By this configuration, the electrode 793 does not block the light emitted by the light emitting element 782. Alternatively, the electrode 793 may be configured so as not to block light passing through the liquid crystal element 775. Therefore, the reduction in brightness due to the placement of the touch panel 791 is extremely small. Since the number of pixels is small, a display device with high visibility and reduced power consumption can be realized. The pole 794 may be of a similar configuration.

[0379] In addition, since the electrodes 793 and 794 do not overlap with the light-emitting element 782, The electrode 794 may be made of a metal material having a low transmittance of visible light. Since the electrodes 793 and 794 do not overlap with the liquid crystal element 775, In addition, a metal material having a low transmittance of visible light can be used.

[0380] Therefore, compared with electrodes using oxide materials with high visible light transmittance, the electrodes 793 and The resistance of the electrode 794 can be reduced, improving the sensor sensitivity of the touch panel. It is possible.

[0381] For example, the electrodes 793, 794, and 796 may be made of conductive nanowires. The nanowires have an average diameter of 1 nm to 100 nm, preferably 5 nm to 50 nm. The size of the nanoparticles may be 5 nm or less, and more preferably 5 nm or more and 25 nm or less. The wires are metal nanowires such as Ag nanowires, Cu nanowires, or Al nanowires. For example, electrodes 664, 665, 6666, or a wire or a carbon nanotube may be used. When Ag nanowires are used for either 65 or 667 or for all of them, the The light transmittance is to be 89% or more, and the sheet resistance is to be 40Ω / □ or more and 100Ω / □ or less. can.

[0382] 18 and 19 show an example of the configuration of an in-cell type touch panel. However, the present invention is not limited to this. For example, a so-called on-cell type transistor formed on the display device 700 may be used. A so-called out-cell type touch panel that is attached to the display device 700. It is also possible to use the following.

[0383] In this manner, the display device according to one embodiment of the present invention can be used in combination with various types of touch panels. It can be used.

[0384] Note that the structure described in this embodiment mode may be used in appropriate combination with structures described in other embodiments. It is possible.

[0385] (Embodiment 5) In this embodiment, a display device including a semiconductor device of one embodiment of the present invention will be described with reference to FIG. This will be used to explain.

[0386] <Circuit configuration of display device> The display device shown in FIG. 20A includes a region having pixels (hereinafter, referred to as a pixel portion 502). A circuit section (hereinafter, a driving section) is disposed outside the pixel section 502 and has a circuit for driving the pixel. A circuit portion 504) and a circuit having a function of protecting the element (hereinafter referred to as a protection circuit 506) and a terminal portion 507. Note that the protection circuit 506 does not necessarily have to be provided.

[0387] A part or the whole of the driver circuit portion 504 is formed on the same substrate as the pixel portion 502. This makes it possible to reduce the number of parts and terminals. When a part or the whole of the pixel portion 502 is not formed on the same substrate, the driving circuit A part or the whole of the path portion 504 is COG or TAB (Tape Automated Band). It can be implemented by using the onding.

[0388] The pixel section 502 is arranged in X rows (X is a natural number of 2 or more) and Y columns (Y is a natural number of 2 or more). The display device has a circuit for driving a plurality of display elements (hereinafter, referred to as pixel circuit 501), The path section 504 is a circuit (hereinafter, a gate driver) that outputs a signal (scanning signal) for selecting a pixel. 504a) to provide a signal (data signal) for driving the display element of the pixel. The pixel circuit 504 includes a driver circuit such as a circuit (hereinafter, referred to as a source driver 504b).

[0389] The gate driver 504a includes a shift register and the like. A signal for driving the shift register is input via a terminal unit 507, and a signal is output. For example, a start pulse signal, a clock signal, etc. are input to the gate driver 504a. The gate driver 504a outputs a pulse signal. The gate has a function of controlling the potential of the scanning lines GL_1 to GL_X. A plurality of drivers 504a are provided, and the scanning lines GL_1 to Alternatively, the gate driver 504a may control the GL_X by dividing it. However, the gate driver 50 has a function of supplying 4a may also provide another signal.

[0390] The source driver 504b includes a shift register and the like. Through the terminal section 507, a signal for driving the shift register as well as a source of a data signal are input. The source driver 504b outputs a pixel circuit based on the image signal. The source driver 504b has a function of generating a data signal to be written to the source driver 501. A data signal is generated according to a pulse signal obtained by inputting a start pulse, a clock signal, etc. The source driver 504b has a function of controlling the output of a data signal. The data lines DL_1 to DL_Y are connected to the data line 101 through the data line 102. Alternatively, the source driver 504b may have a function of supplying an initialization signal. However, the present invention is not limited to this, and the source driver 504b may also supply other signals. It is possible.

[0391] The source driver 504b is configured using, for example, a plurality of analog switches. The source driver 504b sequentially turns on a number of analog switches, The image signal can be time-division-multiplexed and output as a data signal. Also, a shift register, etc. This may be used to configure the source driver 504b.

[0392] Each of the plurality of pixel circuits 501 is connected to one of the plurality of scanning lines GL to which a scanning signal is applied. A pulse signal is inputted through the data line DL, and a data signal is given through one of the data lines DL. A data signal is input to each of the pixel circuits 501. 504a controls writing and holding of data of the data signal. For example, The second pixel circuit 501 is connected to a gate driver GL_m (where m is a natural number equal to or smaller than X) via a scanning line GL_m. A pulse signal is input from 504a, and the data line DL_n ( A data signal is input from the source driver 504b via a source driver 504c (n is a natural number equal to or smaller than Y).

[0393] The protection circuit 506 shown in FIG. 20A includes, for example, a gate driver 504a and a pixel circuit 5 01. Alternatively, the protection circuit 506 is connected to the scanning line GL, which is the wiring between the source driver The data line DL is connected between the driver 504b and the pixel circuit 501. The protection circuit 506 can be connected to a wiring between the gate driver 504a and the terminal unit 507. Alternatively, the protection circuit 506 may be a wiring between the source driver 504b and the terminal unit 507. The terminal unit 507 can be connected to a power supply and a power supply line from an external circuit to the display device. This refers to the part provided with terminals for inputting control signals and image signals.

[0394] When a potential outside a certain range is applied to the wiring to which the protection circuit 506 is connected, the protection circuit This is a circuit that brings one wire into electrical continuity with another wire.

[0395] As shown in FIG. 20A, a protection circuit 50 is provided in each of a pixel section 502 and a driver circuit section 504. 6, ESD (Electro Static Discharge: This can improve the resistance of the display device to overcurrent caused by electrostatic discharge (ESD) and the like. However, the configuration of the protection circuit 506 is not limited to this. For example, A configuration in which a protection circuit 506 is connected, or a protection circuit 506 is connected to the source driver 504b Alternatively, a protection circuit 506 may be connected to the terminal portion 507. It can also be written as:

[0396] In FIG. 20A, the gate driver 504a and the source driver 504b Therefore, although an example in which the driver circuit portion 504 is formed is shown, the present invention is not limited to this configuration. For example, only the gate driver 504a is formed, and a source driver circuit is formed separately. A substrate (for example, a drive circuit substrate formed of a single crystal semiconductor film or a polycrystalline semiconductor film) is The configuration may be such that the

[0397] In addition, the pixel circuits 501 shown in FIG. 20(A) may be, for example, a configuration shown in FIG. 20(B). It can be said that:

[0398] The pixel circuit 501 shown in FIG. 20B includes a liquid crystal element 570, a transistor 550, and a capacitor. The transistor 550 may be any of the transistors described in the previous embodiment. can be applied.

[0399] The potential of one of the pair of electrodes of the liquid crystal element 570 is appropriately set according to the specifications of the pixel circuit 501. The alignment state of the liquid crystal element 570 is set by the written data. A common potential is applied to one of a pair of electrodes of the liquid crystal element 570 in each of the pixel circuits 501. A common potential may be applied to the pair of liquid crystal elements 570 of the pixel circuits 501 in each row. A different potential may be applied to one of the electrodes.

[0400] For example, the display device including the liquid crystal element 570 can be driven in a TN mode, an STN mode, or the like. Mode, VA mode, ASM (Axially Symmetric Aligned M icro-cell mode, OCB (Optically Compensated Birefringence mode, FLC (Ferroelectric Liquid id Crystal) mode, AFLC (AntiFerroelectric Li quid Crystal) mode, MVA mode, PVA (Patterned Ve Vertical Alignment mode, IPS mode, FFS mode, or TBA (Transverse Bend Alignment) mode, etc. may also be used. In addition to the above-mentioned driving method, the display device can be driven by an ECB (Electric Carrier Bipolar Transistor) or the like. Ally Controlled Birefringence mode, PDLC(P Oligomeric Dispersed Liquid Crystal (PNLC) mode (Polymer Network Liquid Crystal) mode, guest hole However, there are various types of liquid crystal elements and their driving methods, and they are not limited to these. A variety of different types of sensors can be used.

[0401] In the pixel circuit 501 in the mth row and the nth column, One of the electrodes is electrically connected to the data line DL_n, and the other is a pair of electrodes of the liquid crystal element 570. The gate electrode of the transistor 550 is electrically connected to the other of the scan lines G L_m. The transistor 550 can be turned on or off. Thus, the write control circuit 100 has a function of controlling the writing of data of the data signal.

[0402] One of a pair of electrodes of the capacitor 560 is connected to a wiring to which a potential is supplied (hereinafter, a potential supply line VL ) and the other is electrically connected to the other of the pair of electrodes of the liquid crystal element 570. The value of the potential of the potential supply line VL is set appropriately according to the specifications of the pixel circuit 501. The capacitor 560 functions as a storage capacitor for storing written data.

[0403] For example, in a display device having the pixel circuit 501 shown in FIG. The pixel circuits 501 in each row are sequentially selected by a gate driver 504a shown in FIG. 550 is turned on to write data of the data signal.

[0404] In the pixel circuit 501 in which data has been written, the transistor 550 is turned off. By repeating this process row by row, an image can be displayed.

[0405] In addition, the pixel circuits 501 shown in FIG. 20(A) may have a configuration shown in FIG. 20(C), for example. It can be said that:

[0406] The pixel circuit 501 shown in FIG. 20C includes transistors 552 and 554 and a capacitance element. The transistor 552 and the transistor 554 The transistor described in the above embodiment can be used for either or both of the above. .

[0407] One of the source electrode and the drain electrode of the transistor 552 is electrically connected to the data line DL_n. , and the gate electrode is electrically connected to the scanning line GL_m.

[0408] Transistor 552 is turned on or off to transfer the data of the data signal. It has the function of controlling the writing of data.

[0409] One of a pair of electrodes of the capacitor 562 is electrically connected to the potential supply line VL_a, and the other is electrically connected to the other of the source electrode and the drain electrode of the transistor 552.

[0410] The capacitor 562 functions as a storage capacitor for storing written data.

[0411] One of the source electrode and the drain electrode of the transistor 554 is connected to the potential supply line VL_a. In addition, the gate electrode of the transistor 554 is electrically connected to the It is electrically connected to the other of the source electrode and the drain electrode.

[0412] One of the anode and the cathode of the light-emitting element 572 is electrically connected to the potential supply line VL_b. The other one is electrically connected to the other of the source electrode and drain electrode of the transistor 554. will be done.

[0413] The light-emitting element 572 may be, for example, an organic electroluminescence element (also called an organic EL element). However, the light-emitting element 572 is not limited to this. Alternatively, an inorganic EL element made of an inorganic material may be used.

[0414] A high power supply potential VDD is applied to one of the potential supply lines VL_a and VL_b. and the other is supplied with a low power supply potential VSS.

[0415] In a display device having the pixel circuit 501 shown in FIG. 20C, for example, The pixel circuits 501 in each row are sequentially selected by the gate driver 504a, and the transistors 552 are turned on. The data signal is written by turning it on.

[0416] In the pixel circuit 501 to which the data has been written, the transistor 552 is turned off. Furthermore, the transistor 554 is in a holding state in response to the potential of the written data signal. The amount of current flowing between the source electrode and the drain electrode is controlled, and the light emitting element 572 The light is emitted with a brightness that corresponds to the flow rate. By performing this process row by row, an image can be displayed.

[0417] This embodiment may be combined, at least in part, with other embodiments described in this specification. It can be implemented in combination.

[0418] (Embodiment 6) In this embodiment, a display module and an electronic device each including a semiconductor device according to one embodiment of the present invention will be described. This will be described with reference to FIGS. 21 to 23.

[0419] <6-1. Display module> The display module 7000 shown in FIG. 21 includes an upper cover 7001 and a lower cover 7002. Between them, touch panel 7004 connected to FPC 7003 and A display panel 7006, a backlight 7007, a frame 7009, and a printed circuit board 701 0, has battery 7011.

[0420] The semiconductor device of one embodiment of the present invention can be used for the display panel 7006, for example.

[0421] The upper cover 7001 and the lower cover 7002 are connected to the touch panel 7004 and the display panel The shape and dimensions can be changed as appropriate to match the size of 7006.

[0422] The touch panel 7004 is a resistive or capacitive touch panel. The display panel 7006 may be overlapped with the opposing substrate (sealing substrate). It is also possible to provide the display panel 7 with a touch panel function. It is also possible to provide an optical sensor in each pixel of the display panel 006 to make it into an optical touch panel.

[0423] The backlight 7007 has a light source 7008. In FIG. In the above embodiment, the light source 7008 is disposed on the light source 7007. However, the present invention is not limited to this. For example, a light source 7008 is arranged at the end of a backlight 7007, and a light diffusion plate is further used. In addition, when a self-luminous light-emitting element such as an organic EL element is used, or when a reflective In the case of a liquid crystal panel, the backlight 7007 may not be provided.

[0424] The frame 7009 protects the display panel 7006 and also supports the movement of the printed circuit board 7010. It also functions as an electromagnetic shield to block electromagnetic waves generated by the operation of the frame. The frame 7009 may also function as a heat sink.

[0425] The printed circuit board 7010 includes a power supply circuit, a signal circuit for outputting a video signal, and a clock signal. The power supply circuit is provided with a signal processing circuit. Alternatively, the power source may be a battery 7011 provided separately. , this can be omitted when using a commercial power source.

[0426] In addition, the display module 7000 includes components such as a polarizing plate, a retardation plate, and a prism sheet. It may be added.

[0427] <6-2.Electronic equipment 1> Next, examples of electronic devices are shown in FIGS.

[0428] FIG. 22A shows the appearance of the camera 8000 with the viewfinder 8100 attached. This is a diagram.

[0429] The camera 8000 includes a housing 8001, a display unit 8002, an operation button 8003, and a shutter. The camera 8000 has a button 8004 and the like. The camera 8000 also has a detachable lens 8006. It is attached.

[0430] In this example, a camera 8000 is used, and a lens 8006 is detached from a housing 8001 and replaced. However, the lens 8006 and the housing may be integrated together.

[0431] The camera 8000 can capture an image by pressing the shutter button 8004. The display unit 8002 also functions as a touch panel. It is also possible to capture an image by doing so.

[0432] The housing 8001 of the camera 8000 has a mount having electrodes, and a finder 810 In addition to 0, strobe devices etc. can also be connected.

[0433] The finder 8100 includes a housing 8101, a display unit 8102, a button 8103, and the like. .

[0434] The housing 8101 has a mount that engages with the mount of the camera 8000, The mount can be attached to the camera 8000. The mount also includes an electrode The image received from the camera 8000 through the electrode is displayed on the display unit 8102. It is possible to do so.

[0435] The button 8103 functions as a power button. The 8102 display can be switched on and off.

[0436] The display unit 8002 of the camera 8000 and the display unit 8102 of the viewfinder 8100 are The display device according to one embodiment of the present invention can be applied.

[0437] In FIG. 22(A), the camera 8000 and the finder 8100 are treated as separate electronic devices. These are configured to be removable, but the camera 8000 has a housing 8001 equipped with a display device. The camera may have a built-in viewfinder that can be used to capture images.

[0438] FIG. 22B is a diagram showing the external appearance of the head mounted display 8200.

[0439] The head mounted display 8200 includes a mounting part 8201, a lens 8202, and a main body 82 8203, a display unit 8204, a cable 8205, etc. It has a built-in 8206 battery.

[0440] A cable 8205 supplies power from a battery 8206 to the main body 8203. 03 is equipped with a wireless receiver and the like, and image information such as image data received is displayed on a display unit 8204. In addition, the camera installed in the main body 8203 can record the movement of the user's eyeballs and eyelids. The system captures the user's gaze and calculates the coordinates of the user's gaze based on that information. It can be used as an input means.

[0441] Furthermore, the mounting unit 8201 may be provided with a plurality of electrodes at positions that come into contact with the user. The main body 8203 detects the current flowing through the electrodes in response to the movement of the user's eyeball, The device may have a function of recognizing the user's viewpoint. Also, the device may have a function of detecting the current flowing through the electrode. By doing so, the mounting unit 820 may have a function of monitoring the pulse of the user. The sensor 1 may have various sensors such as a temperature sensor, a pressure sensor, and an acceleration sensor. The device may have a function of displaying the user's biological information on the display unit 8204. The system detects the movement of the device and changes the image displayed on the display unit 8204 according to the movement. Good too.

[0442] The display device of one embodiment of the present invention can be applied to the display portion 8204.

[0443] 22(C), (D), and (E) are diagrams showing the appearance of the head mounted display 8300. The head mounted display 8300 includes a housing 8301, a display unit 8302, and a backlight. The optical element has a band-shaped fixture 8304 and a pair of lenses 8305.

[0444] A user can view the display on the display unit 8302 through the lens 8305 . It is preferable to arrange the display portion 8302 in a curved manner. By placing the device in the position shown in FIG. Although the configuration in which one display unit 8302 is provided has been illustrated, the present invention is not limited to this. For example, Two display units 8302 may be provided. In this case, one display unit is provided for each eye of the user. If the display unit is arranged in such a way that a 3D display using parallax is possible, do.

[0445] Note that the display device of one embodiment of the present invention can be applied to the display portion 8302. A display device including the semiconductor device of one embodiment of the present invention has extremely high definition. Even if the image is magnified using the lens 8305, the pixels are not visible to the user, and the image is more This makes it possible to display images with a higher sense of reality.

[0446] <6-3.Electronic equipment 2> Next, an example of an electronic device different from the electronic devices shown in FIG. 22(A) to FIG. 22(E) will be described. 3(A) to 23(G).

[0447] The electronic device shown in FIG. 23A to FIG. 23G includes a housing 9000, a display portion 9001, a switch A speaker 9003, an operation key 9005 (including a power switch or an operation switch), a connection terminal Child 9006, sensor 9007 (force, displacement, position, velocity, acceleration, angular velocity, rotation speed, distance, Light, liquid, magnetism, temperature, chemicals, sound, time, hardness, electric field, current, voltage, power, radiation, (including functions for measuring flow rate, humidity, gradient, vibration, odor, or infrared rays), 9008, etc.

[0448] The electronic devices shown in FIGS. 23A to 23G have various functions. Function to display various information (still images, videos, text images, etc.) on the display unit, touch panel function , calendar, date or time display functions, various software (programs) A function for controlling processing by wireless communication, a function for controlling various computers by using wireless communication, Functions for connecting to a network and transmitting or receiving various data using wireless communication functions A function to read out a program or data recorded on a recording medium and display it on the display unit. The electronic devices shown in FIGS. The functions that can be possessed by the can be not limited to these, and can have various functions. Although not shown in FIG. 23(A) to FIG. 23(G), the electronic device may have a plurality of display units. The electronic device may be provided with a camera or the like to capture still images. , the function to shoot videos, and save the captured images to a recording medium (external or built-in to the camera) The camera may have a function of capturing an image on a display unit, a function of displaying a captured image on a display unit, etc.

[0449] The electronic devices shown in FIGS. 23A to 23G will be described in detail below.

[0450] FIG. 23A is a perspective view showing a television device 9100. 100 is a display unit 9001 with a large screen, for example, 50 inches or more or 100 inches or more It is possible to incorporate.

[0451] FIG. 23B is a perspective view showing a portable information terminal 9101. For example, the device has one or more functions selected from a telephone, a notebook, an information viewing device, etc. Specifically, the mobile information terminal 9101 can be used as a smartphone. A speaker 9003, a connection terminal 9006, a sensor 9007, etc. may be provided. The information terminal 9101 can display text and image information on multiple sides. The four operation buttons 9050 (also called operation icons or simply icons) are provided on the display unit 9001. In addition, information 9051 indicated by a dashed rectangle can be displayed on one surface of the display unit 900. 1. An example of the information 9051 is an e-mail or Displays to notify you of incoming calls and SNS (social networking services), Subject of email or SNS, sender name of email or SNS, date and time, time, The remaining battery level, antenna reception strength, etc. Or, the information 9051 is displayed. In place of the information 9051, operation buttons 9050 or the like may be displayed.

[0452] FIG. 23C is a perspective view showing a portable information terminal 9102. , and has a function of displaying information on three or more faces of the display unit 9001. An example is shown in which information 9053 and information 9054 are displayed on different sides. The user of the portable information terminal 9102 holds the portable information terminal 9102 in the breast pocket of the clothes. In this state, the display (information 9053 in this case) can be confirmed. The telephone number or name of the caller is displayed on the mobile information terminal 9102 so that it can be observed from above. The user can read the display without taking the mobile information terminal 9102 out of his pocket. You can check the number and decide whether to answer the call or not.

[0453] 23(D) is a perspective view showing a wristwatch-type portable information terminal 9200. The 9200 is used for mobile phone calls, e-mail, document browsing and writing, music playback, and Internet communications. It is possible to execute various applications such as computer games. The display unit 9001 has a curved display surface, and displays information along the curved display surface. In addition, the portable information terminal 9200 can perform short-distance wireless communication according to a communication standard. For example, by communicating with a wireless headset, The mobile information terminal 9200 also has a connection terminal 9006. It has a connector and can directly exchange data with other information terminals. Charging can also be performed via the connection terminal 9006. Power may also be supplied wirelessly without going through 6.

[0454] 23(E), (F), and (G) are perspective views showing a foldable portable information terminal 9201. FIG. 23E is a perspective view of the portable information terminal 9201 in an unfolded state. (F) shows the mobile information terminal 9201 being changed from one of the unfolded and folded states to the other. FIG. 23(G) is a perspective view of the portable information terminal 9201 in a folded state. The portable information terminal 9201 is highly portable when folded and is unfolded. When the display is turned on, the seamless, wide display area provides excellent visibility of the display. The display unit 9001 of the display device 9001 is made up of three housings 9000 connected by hinges 9055. The two housings 9000 are supported by the hinge 9055. The portable information terminal 9201 can be reversibly transformed from an unfolded state to a folded state. For example, the portable information terminal 9201 can be bent with a radius of curvature of 1 mm or more and 150 mm or less. It can be done.

[0455] The electronic device described in this embodiment has a display unit for displaying some information. However, the semiconductor device of one embodiment of the present invention is an electronic device that does not have a display portion. This can also be applied to vessels.

[0456] This embodiment may be combined, at least in part, with other embodiments described in this specification. It can be implemented in combination. EXAMPLES

[0457] In this example, a transistor was manufactured by a manufacturing method of a semiconductor device according to one embodiment of the present invention. The results of evaluating the electrical characteristics are then explained.

[0458] The configuration of the transistor is the same as that of the transistor 150 illustrated in the second embodiment. Ta.

[0459] [Sample preparation] In this embodiment, a number of samples were prepared by varying the conditions of the heat treatment before the deposition of the metal oxide film. Made.

[0460] First, a titanium film having a thickness of 10 nm and a copper film having a thickness of 100 nm were sputtered on a glass substrate. The conductive film was then processed by photolithography. Then, a conductive film to be a first gate electrode was formed.

[0461] Next, four insulating layers were laminated on the substrate and the conductive film. The insulating film was formed in a vacuum using a PECVD (Prod. No. 13311) system. From the silicon nitride film with a thickness of 50 nm, the silicon nitride film with a thickness of 300 nm, A silicon nitride film and a silicon oxynitride film having a thickness of 50 nm were used.

[0462] Next, the substrate was transported to a film-forming device. After the insulating film was formed, the substrate was transported to the device. The test was conducted under two conditions: waiting time of about 5 hours and about 2 weeks. The substrate was stored with the surface exposed to the air.

[0463] Next, the pressure was increased to about 1×10 -5 Heat treatment at Pa The substrate was inserted into the chamber and the insulating film was heated at 350°C. The three conditions were: 350°C, 5 minutes, 350°C, 60 minutes, and 450°C, 5 minutes. For comparison, a sample was also prepared in which the insulating film was not subjected to heat treatment.

[0464] Next, a metal oxide film is formed on the insulating film, and the metal oxide film is processed into an island shape. A semiconductor layer was formed.

[0465] The metal oxide film was formed by sputtering after the substrate was carried into the film-forming chamber. The oxide film was formed by ionizing indium, gallium, zinc, and Zn without heating the substrate (approximately 25°C). A metal oxide target with In:Ga:Zn=4:2:4.1 [atomic ratio] was used. A film was formed to a thickness of about 100 nm while flowing argon gas and oxygen gas. The oxygen flow rate ratio during film formation was set to 10%.

[0466] Next, an insulating film was formed over the insulating film and the oxide semiconductor layer. A 0 nm silicon oxynitride film was formed using a PECVD apparatus.

[0467] Next, a heat treatment was performed at 350° C. for 1 hour in a nitrogen gas atmosphere. After that, a plasma treatment was performed in an atmosphere containing oxygen gas.

[0468] Next, openings were formed in desired areas of the insulating film. The etching method was used.

[0469] Next, a conductive film is formed on the insulating film so as to cover the opening, and the conductive film is processed into an island shape. A conductive film that will become the gate electrode of 2 is formed. After the conductive film is formed, the lower side of the conductive film is The insulating film in contact with the insulating film was processed to form an insulating film.

[0470] The conductive film is a laminate of a 10 nm thick metal oxide film and a 90 nm thick metal oxide film. The metal oxide film was a metal oxide film having indium, gallium, and zinc. Sputtering using a metal target (In:Ga:Zn=4:2:4.1 [atomic ratio]) The film was formed by the bonding method.

[0471] Next, a plasma treatment was performed on the metal oxide film, the insulating film, and the conductive film. The treatment was carried out using a PECVD apparatus under a mixed gas atmosphere of argon gas and nitrogen gas. went.

[0472] Next, an insulating film was formed over the metal oxide film, the insulating film, and the conductive film. A silicon nitride film having a thickness of 100 nm and a silicon oxynitride film having a thickness of 300 nm were deposited by PECVD. The layers were formed using a device.

[0473] Next, a mask is formed on the formed insulating film, and an opening is formed in the insulating film using the mask. did.

[0474] Next, a conductive film is formed to fill the opening, and the conductive film is processed into an island shape. A conductive film having a thickness of 50 mm was formed to become the source electrode and the drain electrode. A titanium film with a thickness of 400 nm, an aluminum film with a thickness of 400 nm, and a titanium film with a thickness of 50 nm were Each was formed using a sputtering device.

[0475] Next, an insulating film was formed on the insulating film and the conductive film. An acrylic photosensitive resin was used.

[0476] In this manner, each sample was prepared.

[0477] [Electrical characteristics of transistors] Next, the Id-Vg characteristics of the transistors were measured for the samples fabricated as described above. The Id-Vg characteristics of the transistor were measured under the following conditions: The voltage applied to the gate electrode (hereinafter also referred to as gate voltage (Vg)) and the second gate electrode The voltage applied to the conductive film that functions as a switch is changed from 0 to +20 V (also called Vbg). The voltage applied to the conductive film acting as the source electrode was 0.25 V. (Hereinafter, also referred to as source voltage (Vs)) is set to 0V (comm), and the The voltage applied to the conductive film (hereinafter also referred to as drain voltage (Vd)) was set to 0.1 V and The voltage was set to 20 V. The number of measurements was 20 for each sample.

[0478] First, FIG. 26 shows the results when the waiting time for the heat treatment was about 5 hours. The left side shows a sample that has not been subjected to heat treatment (denoted as bake before deposition), and the right side shows a sample that has been subjected to heat treatment for 350 The Id-Vg characteristics of the samples were measured at 5°C for 5 minutes. The results are shown for transistors with channel lengths L of 2 μm, 3 μm, and 6 μm. The channel width W is 50 μm.

[0479] In addition, in the Id-Vg characteristic shown in FIG. 26, the first vertical axis represents Id(A) and the second vertical axis represents current. Field effect mobility (μFE(cm 2 / Vs) and the horizontal axis represents Vg (V). The field effect mobility is a value measured at Vd=20V.

[0480] In FIG. 26, the upper limit of Id during measurement is set to 1 mA. When Id exceeds this upper limit, the field effect mobility is calculated to decrease rapidly. As shown.

[0481] As shown in FIG. 26, the heat-treated sample shows a higher solubility than the non-heat-treated sample. It can be seen that the variation is reduced. In particular, under the condition of the shortest channel length L (L / W=2 / 50μm), the effect of reducing the variation is remarkable.

[0482] Figure 27 shows the results when the waiting time was about two weeks. This is the result under conditions in which more water and hydrogen are adsorbed onto the insulating film compared to FIG.

[0483] In Figure 27, from the left, there is a sample that was not heated, and a sample that was heated at 350°C for 5 minutes. The samples were heat-treated at 350°C for 1 hour, and at 450°C for 5 minutes. The prices are listed.

[0484] As shown in Figure 27, the electrical properties of the samples that were not heat-treated were not uniform. In particular, when the channel length L is the shortest (L / W=2 / 50μm), On the other hand, the difference was more pronounced in all heat-treated samples than in the non-heat-treated samples. It was confirmed that the variation in electrical characteristics was reduced compared to the conventional method.

[0485] In particular, when comparing under the condition where the channel length L is the shortest (L / W=2 / 50μm), the heat treatment The samples with the lowest temperature and shortest time conditions (350°C, 5 minutes) showed the lowest variability. This is because the lower the temperature of the heat treatment and the shorter the heat treatment, The amount of oxygen contained in the insulating film that can be supplied to the metal oxide film is prevented from decreasing. It is thought that...

[0486] From the above results, it can be seen that the electrical characteristics of a semiconductor device can be improved by using the manufacturing method of a semiconductor device according to one embodiment of the present invention. It has been confirmed that it is possible to fabricate highly reliable transistors with good properties and small variations. Done. EXAMPLES

[0487] The transistor 150 described in the above embodiment is used after the formation of the metal oxide film 108. We investigated the relationship between the heat treatment and the electrical characteristics of the transistor. The width W (also called "L / W") of the panel is set to 1.5 / 50μm, 2 / 50μm, or 3 / 50μm. , and 6 / 50 μm. Heat treatment after the formation of the metal oxide film 108 was performed without, 40 A total of 12 combinations of transistors were fabricated for the three levels of temperature: 0°C, 450°C, and 450°C. Measure the Vg-Id characteristics and field effect mobility (μFE) of 20 transistors for each combination When the electrical characteristics were measured, the potential of the back gate of the transistor 150 was the same as that of the gate. It was decided.

[0488] The measurement results for each transistor are shown in Figure 28 and Figure 29. For each measurement result, the horizontal axis indicates Vg. One vertical axis indicates the drain current (Id) in logarithm. The vertical axis of the graph shows μFE. Figure 28 shows the four L / W levels and the results for the samples without or with heat treatment. The measurement results of the combination of the 400°C treatment are shown in Fig. 29. The results are shown for a combination of 450°C and 450°C. Note that the Vg-Id characteristics are measured when Vd is set to 0. The figures show the cases where Vd is 1V and Vd is 20V. is set to 20V.

[0489] 28 and 29, by performing a heat treatment after forming the metal oxide film 108, It is clear that the variation in electrical characteristics is reduced especially in transistors with short channel length L. In addition, it was confirmed that the heat treatment improved the mobility, especially when Vg was small. came. EXAMPLES

[0490] The transistor 150 described in the above embodiment was used to form a metal oxide film. The relationship between the electrical characteristics of the transistor was investigated. a, 0.8 Pa, three levels of deposition power, 0.5 kW, 1.5 kW, 2.5 kW, 4.5 kW We created transistors with a total of 12 combinations for four levels of W, and The Vg-Id characteristics and field effect mobility (μFE) of 20 transistors were measured. During the measurement of the characteristics, the potential of the back gate of the transistor 150 was set to the same potential as that of the gate.

[0491] The measurement results for each transistor are shown in Figure 30 and Figure 31. For each measurement result, the horizontal axis indicates Vg. One vertical axis indicates the drain current (Id) in logarithm. The vertical axis of the graph shows μFE. FIG. 30 shows the results of the three levels of deposition pressure and the deposition power of 0.5 kW. The results are shown for a combination of 1.5kW and 0.8Pa. The measurement results for the transistor with a membrane power of 0.5 kW are missing data. The measurement results for three levels of film pressure and a film deposition power of 2.5 kW and 4.5 kW are shown. The Vg-Id characteristics are shown in Fig. 1 when Vd is 0.1 V and when Vd is 20 V. In addition, μFE is shown when Vd is set to 20 V.

[0492] From Figures 30 and 31, it was confirmed that μFE decreased significantly when the deposition power was 0.5 kW. In addition, when the deposition pressure was high and the deposition power was low, the variation in electrical properties was reduced, and It was confirmed that the variation in electrical characteristics increases when the film formation power is high and the temperature is low. EXAMPLES

[0493] The transistor 150 described in the above embodiment is used to form a second gate insulating film. The relationship between the conditions for forming the insulating film 110 and the electrical characteristics of the transistor was investigated. The channel length L / channel width W is set to three values: 2 / 50 μm, 3 / 50 μm, and 6 / 50 μm. The conditions for forming the insulating film 110 are set to three levels: a reference condition, a comparative condition A, and a comparative condition B. A total of nine combinations of transistors were created, with 20 transistors per combination. The Vg-Id characteristics and field effect mobility (μFE) of the transistor were measured. The potential of the back gate of the transistor was set to the same potential as that of the gate.

[0494] The above "reference conditions" are a substrate temperature of 350°C, a silane gas flow rate of 20sccm, and Nitrous oxide gas with a flow rate of 18,000 sccm was used as the source gas in the deposition chamber of the PECVD equipment. The pressure in the deposition chamber was controlled to 200 Pa, and the deposition power was 100 W. The deposition rate was 14.3 nm / min.

[0495] In addition, under "Comparative Condition A," the substrate temperature was set at 350° C. and the silane gas flow rate was set at 100 sccm. The PECVD equipment was operated using 18,000 sccm of nitrous oxide gas as the source gas. The pressure in the deposition chamber was controlled to 200 Pa, and the deposition power was set to 300 W. The deposition rate at this time was 73.8 nm / min.

[0496] In addition, under "Comparative Condition B," the substrate temperature was set at 350° C. and the silane gas flow rate was set at 100 sccm. The PECVD equipment was operated using 18,000 sccm of nitrous oxide gas as the source gas. The pressure in the deposition chamber was controlled to 200 Pa, and the deposition power was set to 500 W. The deposition rate at this time was 78.7 nm / min.

[0497] The measurement results for each transistor are shown in Figure 32 and Figure 33. For each measurement result, the horizontal axis indicates Vg. One vertical axis indicates the drain current (Id) in logarithm. The vertical axis of the graph shows μFE. Figure 32 shows the relationship between the three levels of L / W and the reference condition or the comparison condition. Figure 33 shows the measurement results for the combination of L / W and comparison condition B. The Vg-Id characteristics are shown when Vd is set to 0.1 V. The figures show the results when Vd is set to 20 V and when Vd is set to 20 V. This shows the case where

[0498] 32 and 33, in particular in transistors with a channel length L of 3 μm or more, It can be seen that the variation in electrical characteristics is reduced under comparative conditions A and B. All 20 samples showed normally-off characteristics in which Id increased rapidly after Vg exceeded 0 V. It can be seen that the insulating film 110 formed under the comparative conditions A and B exhibits excellent properties. The transistor has better electrical characteristics than the transistor in which the insulating film 110 is formed under the standard conditions. In addition, it was found that the comparative conditions A and B had a higher film formation rate than the standard condition. The speed is high, which can increase the productivity of transistors. EXAMPLES

[0499] In this example, a metal oxide film according to one embodiment of the present invention was formed, and the film density and The in-plane distribution of the energy gap was also evaluated.

[0500] <Sample preparation> The glass substrate used was a 600 mm × 720 mm square glass substrate. A metal oxide film was formed using the sputtering method to a thickness of about 100 nm. The film formation conditions were In:G The target was a:Zn=1:1:1 [atomic ratio], the substrate temperature was 170°C, and the deposition gas Argon and oxygen are used as the gases, and the flow rate of oxygen is set to 50% of the total flow rate of the deposition gas. The pressure was 0.6 Pa and the power was 2.5 kW.

[0501] <Evaluation of film density> The film density was determined by XRR measurement. Figure 34 shows the measurement points. In 34, the long axis direction in the substrate plane is taken as the X axis, and the short axis direction is taken as the Y axis.

[0502] Figure 35 shows the film density obtained by XRR. The horizontal axis shows the coordinate in the Y-axis direction, and the vertical axis shows the film density. The median film density is 6.319 g / cm 3 The difference between the maximum and minimum values ​​was 0 .1020g / cm 3 , with a standard deviation of 0.0362 g / cm 3 The variation is small and good. Good results were obtained.

[0503] <Energy gap evaluation> Next, the in-plane distribution of the energy gap was evaluated. The absorption coefficient α was calculated using the overabsorption measurement, and the tauc plot assuming an indirect transition type was used. The energy gap was calculated by the above method. Figure 36 shows the points where the measurements were performed.

[0504] The energy gaps obtained are shown in Figure 37. The median energy gap obtained The difference between the maximum and minimum values ​​was 0.050 eV, and the standard deviation was 0.0 The energy was 19 eV, and good results were obtained with little variation. EXAMPLES

[0505] In this example, a transistor according to one embodiment of the present invention is used to produce a large 8K-OLED display. In order to examine the feasibility of (i), we conducted a simulation and will now explain the results.

[0506] [Verification model] Figure 38 shows a schematic diagram of the display device under study. Table 1 shows the specifications of the display device under study. The screen size of the display device is 65 inches. The number of stages of the light register is 4320, and the single water The average selection period is 1.92 μs.

[0507] [Table 1]

[0508] FIG. 39 shows a circuit diagram of the pixel of the display device used in the verification. Each pixel is red. It has four sub-pixels corresponding to red (R), green (G), blue (B), and white (W). The subpixel includes a transistor M1, a transistor M2, a capacitance element Cs, and a light-emitting element OLED. The transistor M1, which functions as a selection transistor, has one gate at a low potential. The other gate is connected to the gate line GL1. The transistor connected to ED has a configuration in which a pair of gates are connected. s is provided between the gate of transistor M2 and the ANODE line.

[0509] Here, FIG. 40(A) shows a block diagram of the configuration used in the simulation. The actual measured values ​​of the transistors applied with CAC-OS are used for the transistors of the circuit and gate driver. The model parameters were extracted based on the source driver IC. In addition, the parasitic capacitance of the gate line and source line in the pixel area and the parasitic capacitance of the CLK line of the gate driver An RC load model was used for the components. The boundary element method was used to extract the parasitic capacitance and resistance. The pixel with the largest RC load in the pixel area requires the maximum time required for writing the video signal. The time it takes to

[0510] FIG. 40B shows a timing chart of a write operation to a pixel. The signal is written to the pixel after the selection FET of the previous row is turned off. That is, the time (c) required to write to a pixel is the time from when the CLK signal is input to the gate driver. From the above, the time required for the selection FET to turn off ((a) gate line fall time) and the The time from when a video signal is input until the potential inside the pixel actually reaches the potential of the video signal (( b) source line rise time) and b) source line rise time. Here, the gate line fall time is the target amplitude. The source line rise time is the period until it reaches 75% of the target potential. The time required to write to the pixel was calculated from the total period. If the time required for writing is shorter than one horizontal selection period (here, 1.92 μs), the operation It can be determined that this is possible.

[0511] In this study, we performed calculations for two different transistor configurations. 5 (hereafter referred to as the TGSA structure), and the other is a structure with a back gate. The transistor is a bottom-gate channel-etched structure (hereafter referred to as CE structure). .

[0512] [Calculation result] First, we will explain the relationship between the structure of a transistor and the parasitic capacitance. The capacitance was 326 pF in the CE structure, whereas it was 28 pF in the TGSA structure. The parasitic capacitance was reduced to 4 pF. This is because the TGSA structure has a capacitance between the source line and the gate line. This shows that it is possible to form a thick insulating film and reduce the parasitic capacitance.

[0513] Table 2 shows the results of the gate line fall time and the source line rise time.

[0514] [Table 2]

[0515] The sum of the gate line fall time and source line rise time is one horizontal selection period. If it is shorter than 92μs, it indicates that operation is possible. As shown in Table 2, the TGSA structure When a transistor with this structure is used, the time required to write to a pixel is longer than one horizontal selection period. The result was shorter than that of the conventional method, and it was confirmed that the operation was possible.

[0516] FIG. 41 shows the relationship between the field effect mobility of a transistor and the time required to write to a pixel. The vertical axis shows the time required to write to the pixel, and the horizontal axis shows the CAC-O The value of the field effect mobility when the field effect mobility of the transistor to which S is applied is set to 1 is It is clear that the lower the field effect mobility, the longer it takes to write to a pixel. By using transistors that use CAC-OS, In addition, the large 65-inch OLED display can be driven at a high frame rate of 120Hz. I was able to confirm that it can be moved. [Explanation of symbols]

[0517] 100 Transistors 102 Substrate 104 Insulating film 106 Conductive Film 108 Metal oxide film 108n area 110 Insulating film 110_0 Insulating film 112 Conductive film 112_0 Conductive film 112_1 Conductive film 112_2 Conductive film 116 Insulating film 118 Insulating film 120a Conductive film 120b Conductive film 122 Insulating film 140 Mask 141a opening 141b opening 143 Opening 150 Transistors 160 Transistors 300 Processing hours 501 Pixel circuit 502 Pixel section 504 Drive circuit section 504a Gate Driver 504b source driver 506 Protection circuit 507 Terminal section 550 Transistor 552 Transistor 554 Transistor 560 Capacitive element 562 Capacitive element 570 Liquid crystal element 572 Light emitting element 664 Electrode 665 Electrode 667 Electrode 700 Display device 701 Substrate 702 Pixel section 704 Source driver circuit section 705 Substrate 706 Gate driver circuit section 708 FPC terminal section 710 Signal Line 711 Wiring section 712 Sealing material 716 FPC 730 Insulating film 732 Sealing film 734 Insulating film 736 Colored film 738 Light-shielding film 750 Transistors 752 Transistor 760 Connection electrode 770 Planarizing Insulating Film 772 Conductive Film 773 Insulating Film 774 Conductive Film 775 Liquid crystal elements 776 Liquid crystal layer 778 Structure 780 Anisotropic Conductive Film 782 Light emitting element 786 EL layer 788 Conductive Film 790 Capacitive element 791 Touch Panel 792 Insulating film 793 Electrode 794 Electrode 795 Insulating Film 796 Electrode 797 Insulating Film 4000 Film deposition equipment 4001 Atmospheric side substrate supply chamber 4002 Atmospheric side substrate transfer chamber 4003a Load Lock Chamber 4003b Unloading lock room 4004 Transport Room 4005 Substrate heating chamber 4006a Deposition chamber 4006b Deposition chamber 4006c Deposition chamber 4101 Cassette port 4102 Alignment Port 4103 Transport robot 4104 Gate valve 4105 Heating stage 4106 Target 4107 Anti-adhesion plate 4108 Substrate stage 4109 Substrate 4110 Cryotrap 4111 Stage 4200 Vacuum Pump 4201 Cryopump 4202 Turbomolecular pump 4300 Mass Flow Controller 4301 Refiner 4302 Gas heating mechanism 7000 Display Module 7001 Top cover 7002 Lower cover 7003 FPC 7004 Touch Panel 7005 FPC 7006 Display Panel 7007 Backlight 7008 Light source 7009 Frame 7010 Printed Circuit Board 7011 Battery 8000 Camera 8001 Case 8002 Display section 8003 Operation button 8004 Shutter button 8006 Lens 8100 Finder 8101 Case 8102 Display section 8103 Button 8200 Head Mounted Display 8201 Mounting part 8202 Lens 8203 Main unit 8204 Display section 8205 Cable 8206 Battery 8300 Head Mounted Display 8301 Case 8302 Display section 8304 Fixtures 8305 Lens 9000 Chassis 9001 Display section 9003 Speaker 9005 Operation key 9006 Connection terminal 9007 Sensor 9008 Microphone 9050 Operation button 9051 Information 9052 Information 9053 Information 9054 Information 9055 Hinge 9100 Television equipment 9101 Portable information terminal 9102 Portable information terminal 9200 Mobile Information Terminal 9201 Portable information terminals

Claims

[Claim 1] forming a first conductive film on a substrate; The first conductive film is processed into an island shape; forming a first insulating film on the island-shaped first conductive film; forming a metal oxide film on the first insulating film; The metal oxide film is processed into islands, forming a second insulating film on the island-shaped metal oxide film; forming a second conductive film on the second insulating film by a sputtering method in an atmosphere containing oxygen; After forming the second conductive film, an opening is formed down to the first conductive film; a third conductive film is formed over the second conductive film after the opening is formed, The formation of the first insulating film and the metal oxide film includes: a first step of forming the first insulating film on the first conductive film; a second step of transporting the substrate in an air atmosphere; a third step of heating the first insulating film at a temperature of 200° C. to 400° C. for a treatment time of 3 minutes to 10 minutes; a fourth step of forming the metal oxide film on the first insulating film, The third step and the fourth step are consistently performed in an atmosphere having a water vapor partial pressure lower than that of the atmosphere; the second conductive film is an oxide conductive film, the third conductive film is connected to the island-shaped first conductive film in the opening.

Citation Information

Patent Citations

  • Image display

    JP2006165528A

  • Organic el display and manufacturing method thereof

    JP2008216529A

  • Semiconductor element, semiconductor element manufacturing method and semiconductor device using semiconductor element

    JP2013128105A

  • Method for manufacturing semiconductor device

    JP2015188079A