Optical Modulation Devices
By controlling substrate alignment and the K value of the light modulation layer, the device maintains optical characteristics and adhesive force, addressing encapsulation-induced issues in light modulation devices.
Patent Information
- Application Number
- JP2023500446
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-28
- Filing Date
- 2021-07-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-07-27
AI Technical Summary
Existing light modulation devices face issues with maintaining designed optical characteristics and adhesive force between substrates after encapsulation processes, such as an autoclave process, which can cause optical defects and misalignment of the light modulation layer.
The device is designed with specific angular and numerical ranges for substrate alignment, and the K value of the light modulation layer is controlled within 0.15 to 0.4 to stabilize optical properties and adhesive force, using materials like silicone adhesives and optically anisotropic films to maintain alignment and adhesion.
The solution ensures stable maintenance of optical characteristics and adhesive strength between substrates, even after pressure application, preventing optical defects and misalignment.
Smart Images

Figure 0007589423000006 
Figure 0007589423000007 
Figure 0007589423000008
Abstract
Description
[Technical field]
[0001] This application claims priority based on Korean Patent Application No. 10-2020-0093729 filed on July 28, 2020, the contents of which are incorporated herein by reference.
[0002] This application relates to light modulation devices. [Background technology]
[0003] 2. Description of the Related Art Light modulation devices having a light modulation layer containing a liquid crystal compound or the like disposed between two substrates are used for various purposes.
[0004] In order for the light modulation device to exhibit performance suitable for the intended use, it is important to control the alignment state of the liquid crystal compound between the substrates according to the purpose. When the light modulation layer is a liquid crystal layer, the device to which the liquid crystal compound is applied usually forms an alignment film on both surfaces of the two opposing substrates in order to adjust the alignment (particularly the initial alignment) of the liquid crystal compound.
[0005] There is known a technique for constructing an optical device by encapsulating an optical modulation device with an encapsulating agent or the like, and pressure is applied to the optical device during the encapsulation process (for example, Patent Document 1).
[0006] In the encapsulation process, pressure is applied to the optical modulation device in most cases, and the applied pressure may cause the optical characteristics of the optical modulation device to differ from the designed characteristics, or may cause the opposing substrates to shift in position, resulting in optical defects. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent Publication No. 2018-0119517 Summary of the Invention [Problem to be solved by the invention]
[0008] The present application provides an optical modulation device, an optical device, or a manufacturing method thereof. The present application aims to provide an optical modulation device, an optical device, or a manufacturing method thereof, which can stably maintain the designed optical characteristics even after an encapsulation process in which pressure is applied, such as an autoclave process. The present application also aims to provide an optical modulation device, an optical device including the same, or a manufacturing method thereof, which can stably maintain the alignment state of the optical modulation layer while effectively ensuring the adhesive force between the upper and lower substrates. [Means for solving the problem]
[0009] In this specification, the terms vertical, parallel, orthogonal, or horizontal and the numerical values of the angles used to define the angles refer to substantially vertical, parallel, orthogonal, or horizontal and the numerical values as long as the intended effect is not impaired. The ranges of the vertical, parallel, orthogonal, or horizontal values include errors such as manufacturing errors or variations. For example, each of the above may include an error within about ±10 degrees, an error within about ±9 degrees, an error within about ±8 degrees, an error within about ±7 degrees, an error within about ±6 degrees, an error within about ±5 degrees, an error within about ±4 degrees, an error within about ±3 degrees, an error within about ±2 degrees, an error within about ±1 degree, an error within about ±0.8 degrees, an error within about ±0.6 degrees, or an error within about ±0.4 degrees.
[0010] In the present specification, when the measurement temperature affects the physical property, the physical property is measured at room temperature unless otherwise specified. The term "room temperature" refers to a temperature in a state where the temperature is not particularly increased or decreased, and may mean any one temperature within a range of about 10°C to 30°C, for example, a temperature of about 15°C or more, 18°C or more, 20°C or more, or about 23°C or more, and about 27°C or less. In addition, unless otherwise specified, the unit of temperature referred to in the present specification is °C.
[0011] The phase difference, refractive index and refractive index anisotropy referred to in this specification mean the phase difference, refractive index and refractive index anisotropy for light with a wavelength of about 550 nm, unless otherwise specified.
[0012] Unless otherwise specified, an angle between any two directions referred to in this specification may be an acute angle between the acute and obtuse angles between the two directions, or a smaller angle between angles measured clockwise and counterclockwise. Thus, unless otherwise specified, angles referred to in this specification are positive numbers. However, in some cases, in order to indicate a measurement direction between angles measured clockwise or counterclockwise, one of the angles measured clockwise and the angle measured counterclockwise may be expressed as a positive number and the other angle may be expressed as a negative number.
[0013] This application relates to light modulating devices. The term "light modulating device" may refer to a device capable of switching between at least two or more different light states, which may refer to states that differ at least in transmittance, reflectance, color and / or haze.
[0014] Examples of states that a light modulating device may embody include, but are not limited to, transmissive, blocking, high reflectance, low reflectance, and / or color mode states exhibiting a particular color.
[0015] As an example, the light modulating device may be a device capable of switching between at least the transmissive and blocking mode states.
[0016] The transmittance of the light modulation device in the transmission mode may be at least 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80%. As another example, the transmittance in the transmission mode may be about 100% or less, 95% or less, 90% or less, or 85% or less. However, since the higher the transmittance in the transmission mode, the more advantageous it is, the upper limit is not particularly limited.
[0017] The transmittance of the light modulation device in the blocking mode state may be 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, or 5% or less. As another example, the transmittance in the blocking mode may be about 0% or more, 5% or more, 10% or more, 15% or more, 20% or more, or 25% or more. However, since a lower transmittance is more advantageous in the blocking mode, the lower limit of the transmittance in the blocking mode state is not particularly limited.
[0018] The transmittance may be, for example, a rectilinear light transmittance. The rectilinear light transmittance is a percentage of the light transmitted in the same direction as the incident direction to the light incident on the device. For example, if the device is in the form of a film or sheet, the transmittance may be defined as a percentage of the light transmitted through the device in the direction aligned with the normal direction of the film or sheet surface out of the light incident in the direction aligned with the normal direction.
[0019] The transmittance may be a transmittance for any one wavelength in the visible light range, for example, within a range of about 400 to 700 nm or about 380 to 780 nm, a transmittance for the entire visible light range, a maximum or minimum transmittance among the transmittances for the entire visible light range, or an average value of the transmittances in the visible light range.
[0020] The light modulation device of the present application can be designed to be able to switch between any one of the above-mentioned transmission mode and blocking mode states and one other state, for example, and may also embody a third or more states in addition to the above-mentioned states, if necessary.
[0021] The switching of the light modulating device can be controlled by the application of an external signal, for example, the application of a voltage signal. For example, in the absence of an external signal such as a voltage, the light modulating device can maintain one of the states described above, and can be switched to another state when a voltage is applied. By changing the strength, frequency and / or form of the applied voltage, the mode state can also be changed or the third other mode state can be realized.
[0022] The light modulation device of the present application may include, as a basic unit, a light modulation film layer having two substrates arranged opposite to each other and a light modulation layer located between the substrates. FIG. 1 is a diagram showing an example of the light modulation film layer. As shown in the figure, the light modulation film layer includes a first substrate 100 and a second substrate 200 arranged opposite to each other. The first and second substrates may have a first surface and a second surface. The first surface may refer to one main surface of the substrate, and the second surface may refer to the main surface opposite to the first surface.
[0023] As shown in the figure, a functional layer may be formed on one surface (e.g., the first surface) of the first substrate 100, and a liquid crystal alignment film 2001 may be formed on one surface (e.g., the first surface) of the other second substrate 200. The functional layer may be a liquid crystal alignment film, or, as another example, an adhesive layer or a pressure-sensitive adhesive layer, which will be described later. A light modulation layer 600 is located between the first substrate 100 and the second substrate 200 arranged opposite to each other. When the light modulation layer is a liquid crystal layer, a liquid crystal alignment film is usually formed on both surfaces of the first and second substrates 100 and 200. However, by forming an adhesive layer or a pressure-sensitive adhesive layer instead of a liquid crystal alignment film on the first substrate 100 and forming a liquid crystal alignment film only on the second substrate 200, an alignment state of liquid crystal compounds that is very useful for a specific application (e.g., smart window or eye wear) may be obtained. In such a case, the first substrate may not be formed with a liquid crystal alignment film. In addition, although not shown, one of the first and second substrates of the light modulation film layer has a spacer that maintains the cell gap between the first and second substrates. When the functional layer on the first substrate 100 is an adhesive layer or glue layer 1001, the adhesive layer or glue layer 1001 is attached to the spacer, thereby greatly improving the adhesion between the first and second substrates.
[0024] The substrate is not particularly limited and may be made of any known substrate material, for example, a glass substrate, an inorganic substrate such as a crystalline or non-crystalline silicon substrate or a quartz substrate, or a plastic substrate. Examples of plastic substrates that can be used include, but are not limited to, TAC (triacetyl cellulose) substrates; COP (cyclo olefin copolymer) substrates such as norbornene derivative substrates; PMMA (poly(methyl methacrylate) substrates; PC (polycarbonate) substrates; PE (polyethylene) substrates; PP (polypropylene) substrates; PVA (polyvinyl alcohol) substrates; DAC (diacetyl cellulose) substrates; PAC (Polyacrylate) substrates; PES (poly ether sulfone) substrates; PEEK (polyetheretherketon) substrates; PPS (polyphenylsulfone), PEI (polyetherimide) substrates; PEN (polyethylenemaphthate) substrates; PET (polyethyleneterephtalate) substrates and other polyester substrates; PI (polyimide) substrates; PSF (polysulfone) substrates; PAR (polyarylate) substrates, and amorphous fluororesins. The thickness of such substrates is not particularly limited and can be selected within a suitable range.
[0025] In one example, an optically anisotropic film may be used as the substrate. Such an optically anisotropic film usually has anisotropic mechanical properties, and by utilizing such anisotropy, a light modulation device having superior durability can be provided.
[0026] As an example, the anisotropic film may have an in-plane retardation of about 500 nm or more. The in-plane retardation is a value for light with a wavelength of 550 nm, and is a physical quantity defined by the following mathematical formula 2. Other examples of the in-plane retardation of the retardation film include 600 nm or more, 700 nm or more, 800 nm or more, 900 nm or more, 1000 nm or more, 1100 nm or more, 1200 nm or more, 1300 nm or more, 1400 nm or more, 1500 nm or more, 2000 nm or more, 2500 nm or more, 3000 nm or more, 3500 nm or more, 4000 nm or more, 4500 nm or more, 5000 nm or more, 5500 nm or more, 6000 nm or more, 6500 nm or more, 7000 nm or more, 7500 nm or more, 8000 nm or more, 8500 nm or more, 9000 nm or more, or 9500 nm or more. or may be about 100,000nm or less, 90,000nm or less, 80,000nm or less, 70,000nm or less, 60,000nm or less, 50,000nm or less, 40,000nm or less, 30,000nm or less, 20,000nm or less, 15,000nm or less, 14,000nm or less, 13,000nm or less, 12,000nm or less, 10,000nm or less, 9500nm or less, 9000nm or less, 8500nm or less, 8000nm or less, 7500nm or less, 7000nm or less, 6500nm or less, 6000nm or less, 5500nm or less, 5000nm or less, or 4500nm or less.
[0027] In the present application, the specific type of the film that can be applied to the substrate is not particularly limited as long as it shows the in-plane retardation in the range mentioned above. For example, anisotropic polymer films that have been given optical anisotropy by stretching can be applied. Examples of polymer films include polyolefin films such as polyethylene films or polypropylene films, cycloolefin polymer (COP) films such as polynorbornene films, cellulose ester polymer films such as polyvinyl chloride films, polyacrylonitrile films, polysulfone films, polyacrylate films, PVA (poly(vinyl alcohol)) films, or TAC (Triacetyl cellulose) films, polyester films, polycarbonate films, and copolymer films of two or more monomers among the monomers that form the polymers.
[0028] In one example, the film may be a polyester film such as a PET (poly(ethylene terephthalate)) film. That is, films exhibiting an in-plane retardation in the above-mentioned range are well known in the art, and in the case of polymer films, such films exhibit not only large optical anisotropy but also asymmetric mechanical properties due to stretching during the manufacturing process. A representative example of such retardation films known in the art is a stretched polyester film such as a stretched PET (poly(ethylene terephthalate)) film.
[0029] Therefore, in one example, the film may be a polyester film such as a PET film, but the types of films that can be used as the substrate in this application are not limited thereto.
[0030] The in-plane retardation is a physical quantity defined by the following formula 2.
[0031] [Formula 2] Rin = d × (nx-ny)
[0032] In Equation 2, Rin is the in-plane retardation, nx is the refractive index of the film in the slow axis direction, ny is the refractive index of the film in the fast axis direction, and d is the thickness of the film. The meanings of the slow axis and fast axis are well known in the art.
[0033] Alternatively, when the anisotropic film is applied simultaneously to a first and a second substrate, the substrates may be arranged such that their slow axes are parallel or perpendicular to each other.
[0034] The light modulating layer between the substrates is a functional layer that can change the transmittance, reflectance, haze and / or color of light, either alone or in cooperation with other components, depending on the presence or absence of application of an external signal. Such a light modulating layer is referred to as an active light modulating layer in this specification.
[0035] In this specification, an external signal may refer to an external factor that can affect the behavior of a light-modulating material (e.g., a liquid crystal compound) contained in a light-modulating layer (e.g., a liquid crystal layer), for example, an electrical signal such as a voltage. Therefore, a state without an external signal may refer to a state in which no external electrical signal is applied.
[0036] In the present application, the type of the light modulation layer is not particularly limited as long as it has the above-described functions, and any known light modulation layer can be used. The light modulation layer can be, for example, a liquid crystal layer, an electrochromic material layer, a photochromic material layer, an electrophoretic material layer, or a dispersed particle alignment layer.
[0037] In one example, the liquid crystal layer can be applied as the light modulation layer. The liquid crystal layer is a layer containing a liquid crystal compound. In the present specification, the term "liquid crystal layer" includes all layers containing a liquid crystal compound, and for example, as described below, a so-called guest-host layer containing a liquid crystal compound (liquid crystal host) and a dichroic dye, or a layer containing other additives such as a chiral dopant together with a liquid crystal compound, are also types of liquid crystal layers defined in the present specification. The liquid crystal layer may be a light modulation film layer, and therefore the liquid crystal compound can exist in the liquid crystal layer so that the alignment direction changes depending on the presence or absence of application of an external signal. As the liquid crystal compound, any type of liquid crystal compound can be used as long as the alignment direction can be changed by application of an external signal. For example, the liquid crystal compound can be a smectic liquid crystal compound, a nematic liquid crystal compound, or a cholesteric liquid crystal compound. In addition, the liquid crystal compound can be, for example, a compound without a polymerizable group or a crosslinkable group so that the alignment direction can be changed by application of an external signal.
[0038] The liquid crystal layer may include a liquid crystal compound having a positive or negative dielectric anisotropy. The absolute value of the dielectric anisotropy of the liquid crystal may be appropriately selected in consideration of the object of the present application. The term "dielectric anisotropy βε" may mean the difference ε / / -ε⊥ between the horizontal dielectric constant ε / / and the vertical dielectric constant ε⊥ of the liquid crystal. In this specification, the term "horizontal dielectric constant ε / / " may mean a dielectric constant value measured along the direction of an electric field in a state where a voltage is applied so that the direction of the electric field caused by the director of the liquid crystal molecules and the applied voltage is substantially horizontal, and the vertical dielectric constant ε⊥ may mean a dielectric constant value measured along the direction of the electric field in a state where a voltage is applied so that the direction of the electric field caused by the director of the liquid crystal molecules and the applied voltage is substantially vertical.
[0039] Driving modes of the liquid crystal layer include, for example, Dynamic Scattering (DS) mode, Electrically Controllable Birefringence (ECB) mode, In-Plane Switching (IPS) mode, Fringe-Field Switching (FFS) mode, Optically Compensated Bend (OCB) mode, Vertical Alignment (VA) mode, Multi-domain Vertical Alignment (MVA) mode, Patterned Vertical Alignment (PVA) mode, Hybrid Aligned Nematic (HAN) mode, Twisted Nematic (TN) mode, Super Twisted Nematic (STN) mode, or Reversed Twisted Nematic (R-TN) mode.
[0040] The liquid crystal layer of the present application may be designed (formed) to realize at least a twisted alignment among the above modes. The twisted alignment refers to a state in which the liquid crystal compound in the liquid crystal layer is aligned in a twisted form based on a virtual helical axis, and such a twisted alignment may be realized in a state in which the liquid crystal compound in the liquid crystal layer is aligned horizontally, vertically, tilted, or splayed. The twisted alignment may also be realized in an initial state of the liquid crystal layer or in a state in which an external signal is applied. The initial state may refer to a state in which no external signal capable of controlling the alignment of the liquid crystal compound is applied to the liquid crystal layer.
[0041] For example, the liquid crystal layer may be a light modulation layer that is initially vertically aligned and that realizes the twisted alignment when an external signal (e.g., an electrical signal such as a voltage) is applied.
[0042] The light modulating layer which is a liquid crystal layer essentially contains the liquid crystal compound and may contain further components as required.
[0043] For example, the liquid crystal layer, which is a light modulating layer, may contain a so-called chiral dopant together with the liquid crystal compound, which can induce a helical structure orientation, i.e., the twisted orientation, in the liquid crystal compound.
[0044] The chiral dopant can be any one that can induce the desired twisting without damaging the liquid crystal property, for example, the nematic regularity. The chiral dopant for inducing the rotation of the liquid crystal molecules must at least have chirality in its molecular structure. Examples of the chiral dopant include compounds having one or more asymmetric carbons, compounds having an asymmetric point on a heteroatom such as chiral amine or chiral sulfoxide, or compounds having an axially asymmetric, optically active site such as cumulene or binaphthol. The chiral dopant can be, for example, a low molecular weight compound having a molecular weight of 1,500 or less. Examples of the chiral dopant include commercially available chiral nematic liquid crystals, such as the commercially available chiral dopant liquid crystal S811 manufactured by Merck or LC756 manufactured by BASF.
[0045] The ratio of the chiral dopant is not particularly limited, but the chiral dopant can be added so that the ratio t / p of the thickness t (cell gap) of the light modulation layer and the pitch p of the helical structure of the liquid crystal compound (the pitch of the twisted orientation) generated by the addition of the chiral dopant satisfies the K value described later.
[0046] The pitch p of the so-called twisted-alignment light modulation layer (liquid crystal layer) to which the chiral dopant is applied can be measured by a measurement method using a wedge cell, and can be measured by the method described in Simple method for accurate measurements of the cholesteric pitch using a stripe-wedge Grandjean-Cano cell by D. Podolskyy et al. (Liquid Crystals, Vol. 35, No. 7, July 8, 2008, 789-791). The content (wt%) of the chiral dopant is calculated by the formula 100 / (HTP (Helixcal Twisting power) x pitch (nm), and can be selected at an appropriate ratio taking into account the desired pitch p.
[0047] As an example, the light modulation layer can be designed (formed) so that the K value in the following formula 1 is within the range of 0.15 to 0.4.
[0048] [Formula 1] K = △n × p / t
[0049] In Equation 1, Δn is the refractive index anisotropy of the liquid crystal layer, p is the pitch in the twisted orientation, and t is the thickness of the liquid crystal layer.
[0050] In the above formula 1, the thickness t of the liquid crystal layer is a thickness known in the art as a cell gap. In the formula 1, the refractive index anisotropy has no unit, and the pitch p and the thickness t of the liquid crystal layer have the same unit, so there is no unit for the K value.
[0051] The refractive index anisotropy related to Formula 1 can be measured by the method described in the Examples.
[0052] By setting the K value in Equation 1 to be within the range of 0.15 to 0.4, it is possible to provide an optical modulation device that can stably maintain the designed optical characteristics even after an encapsulation process in which pressure is applied, such as an autoclave process.
[0053] The method of designing the light modulation layer so that the K value falls within the above range is not particularly limited, and for example, a method of adjusting the ratio of chiral dopants so that a pitch p that can exhibit a desired K value appears taking into account the refractive index anisotropy Δn and thickness t (cell gap) of the liquid crystal layer.
[0054] As another example, the K value may be 0.16 or more, 0.17 or more, 0.18 or more, 0.19 or more, 0.2 or more, or more than 0.2, or may be 0.39 or less, 0.38 or less, 0.37 or less, 0.36 or less, 0.35 or less, 0.34 or less, 0.33 or less, 0.32 or less, 0.31 or less, 0.3 or less, or less than 0.3.
[0055] The ranges of the refractive index anisotropy Δn of the liquid crystal layer, the pitch p, and the thickness t of the liquid crystal layer in Equation 1 can be selected within the ranges that can exhibit the K value.
[0056] For example, the refractive index anisotropy Δn of the liquid crystal layer may be in the range of 0.01 to 0.5. As another example, the refractive index anisotropy may be 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, or 0.085 or more, or about 0.45 or less, 0.4 or less, 0.35 or less, 0.3 or less, 0.25 or less, 0.2 or less, 0.15 or less, or 0.1 or less.
[0057] The pitch p of the twist orientation may be in the range of 1 to 100 μm. As another example, the pitch may be 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, or 9.5 μm or more, or may be about 95 μm or less, 90 μm or less, 85 μm or less, 80 μm or less, 75 μm or less, 70 μm or less, 65 μm or less, 60 μm or less, 55 μm or less, 50 μm or less, 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, or 25 μm or less.
[0058] The thickness t(cell gap) of the liquid crystal layer may be in the range of 0.5 μm to 50 μm. As another example, the thickness t(cell gap) may be 1 μm or more, 1.5 μm or more, 2 μm or more, 2.5 μm or more, 3 μm or more, or 3.5 μm or more, or may be about 48 μm or less, 46 μm or less, 44 μm or less, 42 μm or less, 30 μm or less, 38 μm or less, 36 μm or less, 34 μm or less, 32 μm or less, 30 μm or less, 28 μm or less, 26 μm or less, 24 μm or less, 22 μm or less, 20 μm or less, 18 μm or less, 16 μm or less, 14 μm or less, 12 μm or less, or 10 μm or less.
[0059] In addition, a ratio t / p of the pitch p of the twist alignment to the thickness t (cell gap) of the light modulation layer (liquid crystal layer) may be less than 1. As another example, the ratio t / p may be 0.95 or less, 0.9 or less, 0.85 or less, 0.8 or less, 0.75 or less, 0.7 or less, 0.65 or less, 0.6 or less, 0.55 or less, 0.5 or less, 0.45 or less, 0.4 or less, or 0.35 or less, or may be about 0.1 or more, 0.15 or more, 0.2 or more, 0.25 or more, 0.3 or more, 0.35 or more, or 0.4 or more.
[0060] Through the above design, an optical modulation device can be provided that can more efficiently achieve the objectives of the present application.
[0061] The light modulation layer (liquid crystal layer) may contain other necessary components (for example, a dichroic dye, etc.).
[0062] The type of liquid crystal alignment film that may be formed on the first surface of the first and / or second substrate is not particularly limited. As the alignment film, a known vertical or horizontal alignment film or other alignment film can be applied in consideration of the desired initial alignment. As for the type of alignment film, a contact type alignment film such as a rubbing alignment film or a non-contact type alignment film such as a photo-alignment film can be applied. In one example, a vertical alignment film can be used as the alignment film. For example, a combination of a vertical alignment film and a pressure-sensitive adhesive layer or adhesive layer described later can induce an alignment state of liquid crystal compounds suitable for various applications.
[0063] When forming an adhesive layer or a pressure-sensitive adhesive layer on the first surface of the first substrate in the light modulation film layer, the type of the adhesive layer or the pressure-sensitive adhesive layer is not particularly limited. For example, various types of adhesives or adhesives known in the art as OCA (Optically Clear Adhesive) or OCR (Optically Clear Resin) can be combined with a liquid crystal alignment film to induce a suitable alignment of liquid crystal compounds. As the adhesive or adhesive, for example, an acrylic, silicone, epoxy, or urethane adhesive or adhesive can be used.
[0064] Suitable adhesives or bonding agents include silicone adhesives or bonding agents. The unique surface properties of silicone adhesives or bonding agents can induce an alignment state of liquid crystal compounds suitable for the purpose in combination with a liquid crystal alignment film (particularly, a vertical alignment film).
[0065] The silicone-based adhesive or adhesive may be a cured product of a curable silicone adhesive or adhesive composition (hereinafter, simply referred to as a curable silicone composition). The type of the curable silicone composition is not particularly limited, and may be, for example, a heat-curable silicone composition or an ultraviolet-curable silicone composition.
[0066] In one example, the curable silicone composition may contain, as an addition-curable silicone composition, (1) an organopolysiloxane containing two or more alkenyl groups in the molecule and (2) an organopolysiloxane containing two or more silicon-bonded hydrogen atoms in the molecule. Such silicone compounds can form a cured product by addition reaction in the presence of a catalyst such as a platinum catalyst.
[0067] The (1) organopolysiloxane is a main component constituting a silicone cured product and contains at least two alkenyl groups in one molecule. Specific examples of the alkenyl group include vinyl, allyl, butenyl, pentenyl, hexenyl, and heptenyl groups, among which vinyl groups are usually used, but are not limited thereto. In the (1) organopolysiloxane, the bonding position of the alkenyl group is not particularly limited. For example, the alkenyl group may be bonded to the end of the molecular chain and / or to the side chain of the molecular chain. In the (1) organopolysiloxane, examples of the substituents that may be contained in addition to the alkenyl mentioned above include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl and phenethyl; and halogen-substituted alkyl groups such as chloromethyl, 3-chloropropyl, and 3,3,3-trifluoropropyl. Of these, methyl and phenyl groups are usually used, but the examples are not limited to these.
[0068] The molecular structure of the (1) organopolysiloxane is not particularly limited, and may have any shape, such as linear, branched, cyclic, network, or linear with some branching, etc. Of the molecular structures described above, those having linear molecular structures are usually used, but are not limited thereto.
[0069] More specific examples of the organopolysiloxane (1) include dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with trimethylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, R 1 2SiO 2 / 2 The siloxane unit represented by R 1 2R 2 SiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 2R 2 SiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 R 2 SiO 2 / 2 The siloxane unit represented by R 1 SiO 3 / 2 Siloxane units represented by R 2 SiO 3 / 2 and mixtures of two or more of the foregoing. 1is a hydrocarbon group other than an alkenyl group, specifically, an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group; an aralkyl group such as a benzyl group or a phenethyl group; or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group. 2 is an alkenyl group, specifically, a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, or the like.
[0070] In the addition curable silicone composition, the (2) organopolysiloxane can crosslink the (1) organopolysiloxane. In the (2) organopolysiloxane, the bond position of the hydrogen atom is not particularly limited, and may be bonded to, for example, the end of the molecular chain and / or the side chain. In the (2) organopolysiloxane, the type of the substituent that may be contained other than the silicon-bonded hydrogen atom is not particularly limited, and examples thereof include alkyl groups, aryl groups, aralkyl groups, and halogen-substituted alkyl groups, as mentioned in the (1) organopolysiloxane, and among these, methyl groups or phenyl groups are usually used, but are not limited thereto.
[0071] The molecular structure of the (2) organopolysiloxane is not particularly limited, and may have any shape, such as linear, branched, cyclic, network, or partially branched linear, etc. Among the molecular structures described above, a linear molecular structure is usually used, but is not limited thereto.
[0072] More specific examples of the organopolysiloxane (2) include methylhydrogenpolysiloxanes capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogen copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, dimethylsiloxane-methylphenylsiloxane copolymers capped with dimethylhydrogensiloxane groups at both molecular chain terminals, methylphenylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, R 1 3SiO 1 / 2 The siloxane unit represented by R 1 2HSiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 2HSiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 HSiO 2 / 2 The siloxane unit represented by R 1 SiO 3 / 2 Siloxane units represented by HSiO 3 / 2 and mixtures of two or more of the foregoing. 1 is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group; an aralkyl group such as a benzyl group or a phenethyl group; or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group.
[0073] The content of the (2) organopolysiloxane is not particularly limited as long as it is contained in an amount sufficient to allow suitable curing. For example, the (2) organopolysiloxane may be contained in an amount such that the number of silicon-bonded hydrogen atoms is 0.5 to 10 per alkenyl group contained in the (1) organopolysiloxane. Within this range, curing can be sufficiently promoted and heat resistance can be ensured.
[0074] The addition curable silicone composition may further contain platinum or a platinum compound as a catalyst for curing. The specific type of platinum or platinum compound is not particularly limited. The ratio of the catalyst may be adjusted to a level that allows suitable curing.
[0075] The addition-curable silicone composition may further contain necessary and suitable additives in appropriate proportions from the standpoint of improving storage stability, handling, and workability.
[0076] As another example, the silicone composition may be a condensation-curable silicone composition, for example, comprising: (a) an alkoxy-containing siloxane polymer; and (b) a hydroxyl-containing siloxane polymer.
[0077] The (a) siloxane polymer may be, for example, a compound represented by the following Chemical Formula 1:
[0078] [Chemical formula 1] R 1 a R 2 b SiO c (OR 3 ) d
[0079] In formula 1, R 1 and R 2 each independently represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group; R 3 represents an alkyl group, R 1 , R 2 and R 3When there are multiple of each, they may be the same or different, a and b each independently represent a number greater than or equal to 0 and less than 1, a+b represents a number greater than 0 and less than 2, c represents a number greater than 0 and less than 2, d represents a number greater than 0 and less than 4, and a+b+c×2+d is 4.
[0080] In the definition of Chemical Formula 1, the monovalent hydrocarbon group may be, for example, an alkyl group having 1 to 8 carbon atoms, a phenyl group, a benzyl group, or a tolyl group, and in this case, the alkyl group having 1 to 8 carbon atoms may be a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, or an octyl group. In addition, in the definition of Chemical Formula 1, the monovalent hydrocarbon group may be substituted with a known substituent such as a halogen, an amino group, a mercapto group, an isocyanate group, a glycidyl group, a glycidoxy group, or a ureido group.
[0081] In the definition of Chemical Formula 1, R 3 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, and a butyl group. Among the alkyl groups, a methyl group or an ethyl group is usually applied, but is not limited thereto.
[0082] Among the polymers of Chemical Formula 1, branched or tertiary crosslinked siloxane polymers can be used. In addition, the (a) siloxane polymer may have residual hydroxyl groups within a range that does not impair the purpose, specifically, within a range that does not inhibit the dealcoholization reaction.
[0083] Said (a) siloxane polymer can be produced, for example, by hydrolysis and condensation of polyfunctional alkoxysilane or polyfunctional chlorosilane. An average technician in this field can easily select a suitable polyfunctional alkoxysilane or chlorosilane according to the desired (a) siloxane polymer, and can easily control the conditions of hydrolysis and condensation reaction using it. Meanwhile, when producing said (a) siloxane polymer, a suitable monofunctional alkoxysilane can also be used in combination depending on the purpose.
[0084] As the (a) siloxane polymer, for example, commercially available organosiloxane polymers such as X40-9220 or X40-9225 from Shin-Etsu Silicones, and XR31-B1410, XR31-B0270 or XR31-B2733 from GE Toray Silicones can be used.
[0085] As the (b) hydroxyl group-containing siloxane polymer contained in the condensation-curable silicone composition, for example, a compound represented by the following chemical formula 2 can be used.
[0086] [Chemical formula 2] [ka]
[0087] In Chemical Formula 2, R4 and R5 each independently represent a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group, and when there are multiple R4 and multiple R5, they may be the same or different, and n represents an integer of 5 to 2,000.
[0088] In the definition of Chemical Formula 2, specific examples of the monovalent hydrocarbon group include the same hydrocarbon groups as those in Chemical Formula 1 above.
[0089] Said (b) siloxane polymer can be produced, for example, by hydrolysis and condensation of dialkoxysilane and / or dichlorosilane. An average technician in this field can easily select a suitable dialkoxysilane or dichlorosilane according to the desired (b) siloxane polymer, and can easily control the conditions of hydrolysis and condensation reaction using it. As said (b) siloxane polymer, for example, commercially available bifunctional organosiloxane polymers such as XC96-723, YF-3800, YF-3804, etc., from GE Toray Silicone Co., Ltd. can be used.
[0090] The addition curing or condensation curing silicone composition described above is an example of a material for forming a silicone pressure sensitive adhesive or adhesive that can be used in the present application. In other words, basically, all silicone pressure sensitive adhesives or adhesives known in the art as OCA or OCR can be used in the present application.
[0091] The type of the adhesive or the curable composition forming the adhesive is not particularly limited and may be appropriately selected depending on the intended use. For example, a solid, semi-solid or liquid adhesive or the curable composition may be used. The solid or semi-solid adhesive or the curable composition may be cured before the objects to be bonded are bonded. The liquid adhesive or the curable composition may be called an optically clear resin (OCR) and may be cured after the objects to be bonded are bonded. According to one example, the adhesive or the curable composition may be a polydimethyl siloxane-based adhesive or the curable composition, a polymethylvinyl siloxane-based adhesive or the curable composition, an alkoxy silicone-based adhesive or the curable composition, or the like, but is not limited thereto.
[0092] The thickness of the pressure sensitive adhesive layer or adhesive layer is not particularly limited and can be selected within an appropriate range for ensuring the desired adhesive strength or cohesive strength. The thickness can be within the range of about 1 μm to 50 μm. As another example, the thickness can be 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, or 10 μm or more, or about 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less.
[0093] When the above-mentioned pressure-sensitive adhesive layer or adhesive layer is formed on the first surface of the first substrate, a liquid crystal alignment film does not need to be formed on the first substrate.
[0094] In the liquid crystal layer, which is a light modulating layer, the initial alignment of the liquid crystal compound formed by the liquid crystal alignment film and / or the adhesive layer or the adhesive layer and the liquid crystal alignment film may be vertical alignment, horizontal alignment, tilt alignment or splay alignment. In addition, in the vertical alignment, horizontal alignment, tilt alignment or splay alignment state, the liquid crystal compound may be twisted to exist in the twist alignment or cholesteric alignment state, or it may not be. The initial alignment refers to the alignment in a state where no external signal is applied to the light modulating layer containing the liquid crystal compound.
[0095] The meanings of the horizontal alignment, tilt alignment, vertical alignment, and splay alignment are as known in the art. The liquid crystal compound of the light modulation layer maintains the horizontal alignment, tilt alignment, vertical alignment, or splay alignment state in the initial state, and can be changed to a different alignment state by an external signal.
[0096] In one example, the initial alignment of the liquid crystal compound in the light modulation layer may be vertical or a similar alignment state to the vertical alignment, and the twisted alignment may be realized when an external signal is applied. This alignment state is obtained by applying a vertical alignment film as the liquid crystal alignment film. This alignment is useful in a device that realizes a so-called R-TN (Reversed Twisted Nematic) alignment.
[0097] The in-plane retardation (based on a wavelength of 550 nm) of the light modulation layer in the vertical alignment or an alignment state similar to the vertical alignment may be, for example, about 30 nm or less, 25 nm or less, 20 nm or less, 15 nm or less, 10 nm or less, or 5 nm or less, or 0 nm or more, or more than 0 nm.
[0098] The in-plane retardation is calculated by the above-mentioned formula 2, where nx, ny, and d are the refractive index in the slow axis direction, the refractive index in the fast axis direction, and the thickness of the light modulation layer, respectively.
[0099] The light modulating film layer may further include a spacer for maintaining the distance between the first and second substrates. The spacer may be a commonly used spacer, such as a ball spacer, a column spacer, or a partition-type spacer, or a combination of two or more of the above. As a preferred example, the partition-type spacer may be used, and in particular, a partition-type spacer in which the partitions form at least one closed figure may be used. The closed figure formed by the partition-type spacer may be a hexagon (e.g., a regular hexagon, etc.) or a quadrangle (e.g., a square or a rectangle). The partition-type spacer in which the closed figure is a hexagon, particularly a regular hexagon, is also called a honeycomb-type spacer. As is well known, such a honeycomb-type or quadrangle-type partition spacer refers to a case in which the figure formed by the partition-type spacer is a honeycomb-type or quadrangle when the shape of the partition-type spacer formed on the substrate is observed from the normal direction of the substrate. The honeycomb type is generally composed of a combination of regular hexagons, and in the case of a quadrangle, it may be a square, a rectangle, or a combination of a square and a rectangle, etc. Considering the adhesive force between the first and second substrates, a partition type spacer may be used as the spacer, but is not limited thereto.
[0100] The pitch of the spacer can be appropriately selected in consideration of the desired adhesive force and the efficiency of maintaining the cell gap. For example, when a partition-type spacer is applied, the pitch of the partition-type spacer can be in the range of 50 μm to 2,000 μm. A method for determining the pitch of a partition-type spacer is publicly known. For example, if the partition-type spacer is a honeycomb type, the pitch is determined from the distance between the opposing sides of the hexagon forming the honeycomb, and if the spacer is a rectangle, the pitch is determined from the length of the side of the rectangle. If the distance between the opposing sides of the hexagon forming the honeycomb or the length of the side of the rectangle are not constant, the average value thereof can be defined as the pitch.
[0101] When the partition-type spacer forms a closed shape, the area of the closed shape (i.e., the area of a hexagon or a rectangle, for example) is, for example, about 1 to 200 mm 2 In the case where a plurality of closed figures are formed by the partition-type spacer and the areas of the closed figures are different from one another, the area is an arithmetic average value.
[0102] The line width of the partition-type spacer, for example, the width of each side of the hexagon or rectangle forming the honeycomb, may be, for example, in the range of about 5 μm to 50 μm. As another example, the line width may be about 10 μm or more or 15 μm or more, or about 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, or 20 μm or less.
[0103] Within the above range, the cell gap is appropriately maintained and the adhesive strength between the substrates is also excellent. For example, when the pressure sensitive adhesive layer or adhesive layer is formed on the first substrate, the combination with the partition wall type spacer can provide excellent adhesive strength between the substrates.
[0104] An electrode layer may be formed on each substrate of the light modulating film layer as a component for applying an external signal to the light modulating layer. For example, an electrode layer may be present between the first surface and the functional layer (liquid crystal alignment film, adhesive or adhesive layer (between 100 and 1001 in FIG. 1)) of the first substrate and / or between the first surface and the liquid crystal alignment film (between 200 and 2001 in FIG. 1) of the second substrate (between the spacer and the alignment film if a spacer is present). In the case of the second substrate, it is common to first form an electrode layer on the first surface, and then form a spacer and an alignment film on top of it in sequence. Therefore, if a spacer is present, the electrode layer may be located between the first surface of the second substrate and the spacer and the alignment film.
[0105] The electrode layer may be a known transparent electrode layer, for example, a so-called conductive polymer layer, a conductive metal layer, a conductive nanowire layer, or a metal oxide layer such as ITO (Indium Tin Oxide). In addition, various materials and methods for forming a transparent electrode layer are known, and may be used without any limitation.
[0106] The light modulation device basically includes the light modulation film layer, and may further include other components as necessary. That is, depending on the driving mode, the light modulation film layer alone can realize the above-mentioned transmission, blocking, high reflection, and / or low reflection modes and switch between them, but it may also include additional components to facilitate the realization or switching of such modes.
[0107] For example, the device may further include a polarizing layer (passive polarizing layer) disposed on one or both sides of the light modulating film layer. In one example, the device further includes a polarizing layer disposed on the second surface of the first or second substrate. FIG. 2 is an example of the structure, in which the polarizing layer 400 is disposed on only one side of the light modulating film layer in the structure of FIG. 1, and FIG. 3 is an example of the structure in which the polarizing layer 400 is disposed on both sides of the light modulating film layer in the structure of FIG. 1. In addition, when the partition-type spacer is applied as the spacer and has a quadrilateral (square or rectangular) shape, it is preferable that the sides of the quadrilateral and the absorption axis of the polarizing layer are disposed substantially perpendicular or horizontal to each other. In one example, the small angle between the slow axis of the first or second substrate and the absorption axis of the polarizing layer may be in the range of 80 degrees to 100 degrees.
[0108] The term "polarizing layer" may refer to an element that converts natural light or non-polarized light into polarized light. In one example, the polarizing layer may be a linear polarizing layer. A linear polarizing layer refers to a case where selectively transmitted light is linearly polarized light that vibrates in one direction, and selectively absorbed or reflected light is linearly polarized light that vibrates in a direction perpendicular to the vibration direction of the linearly polarized light. That is, the linear polarizing layer may have a transmission axis and an absorption axis or a reflection axis that are perpendicular to each other in the plane direction.
[0109] The polarizing layer may be an absorptive polarizing layer or a reflective polarizing layer, and may be, for example, a polarizing layer obtained by dyeing a polymer stretched film such as a PVA (poly(vinyl alcohol)) stretched film with iodine, or a guest-host polarizing layer in which a liquid crystal polymerized in an oriented state serves as a host and a dichroic dye aligned by the orientation of the liquid crystal serves as a guest, but is not limited thereto.
[0110] The reflective polarizing layer may be, for example, a reflective polarizing layer known as a dual brightness enhancement film (DBEF) or a reflective polarizing layer formed by coating a liquid crystal compound such as lyotropic liquid crystal (LLC), but is not limited thereto.
[0111] The light modulation film layer may have a structure in which the polarizing layers are disposed on both sides thereof as shown in Fig. 3. In such a case, the angle formed by the transmission axes of the polarizing layers disposed on both sides may be within a range of 85 degrees to 95 degrees or may be approximately perpendicular.
[0112] As an example, the optical device can be constructed without a polarizing layer, for example, after incorporating a dichroic dye as an additional component into the liquid crystal layer, the optical device can be constructed without applying a polarizing layer.
[0113] The optical modulation device may further include other necessary components in addition to the above components.
[0114] For example, the light modulation device may further include an optically anisotropic film that satisfies the refractive index relationship of the following formula 3. Such a film can optically compensate the substrate and the light modulation layer to further improve the performance of the device.
[0115] [Formula 3] nz <ny
[0116] In the formula 3, ny is the refractive index at a wavelength of 550 nm in the fast axis direction of the optically anisotropic film, and nz is the refractive index at a wavelength of 550 nm in the thickness direction of the optically anisotropic film.
[0117] An optically anisotropic film that satisfies the relationship of Equation 3 is a film that exhibits the properties of a so-called negative C plate.
[0118] The thickness direction retardation of such an optically anisotropic film may be, for example, within the range of -700 nm to -10 nm. The optically anisotropic film may be present in one layer or two or more layers in an optical device, and the thickness direction retardation is the thickness direction retardation of the film when one optically anisotropic film is present, and is the total thickness direction retardation of the mode films when two or more layers are present.
[0119] The thickness direction retardation is a physical quantity defined by the following formula 4.
[0120] [Formula 4] Rth = d × (nz-ny)
[0121] In Equation 4, Rth is the thickness direction retardation, nz is the refractive index of the film in the thickness direction, ny is the refractive index of the film in the fast axis direction, and d is the thickness of the film. The meanings of the thickness direction and the fast axis are well known in the art.
[0122] The optically anisotropic film may be a known retardation film that satisfies the above mathematical formula 3. In the art, various types of films are known, such as stretched polymer films and liquid crystal films.
[0123] The optically anisotropic film may be present on the first and / or second substrate, and may be formed on the first surface of the first and / or second substrate. In this case, the optically anisotropic film may be present between the first and / or second substrate and the light modulation layer, and when a liquid crystal alignment film or the pressure sensitive adhesive layer or adhesive layer (such as a liquid crystal alignment film) is formed on the first surface, the optically anisotropic film may be formed between the first and / or second substrate and the liquid crystal alignment film, etc., and when an electrode layer is formed on the first surface, the optically anisotropic film may be formed between the first and / or second substrate and the electrode layer.
[0124] The light modulation device may include other components as necessary in addition to the above components. For example, in addition to the adhesive layer or glue layer formed on the first surface of the first substrate, any other components necessary for driving or using the light modulation device may be added, such as an adhesive layer or glue layer for attaching other components, a hard coating film, an anti-reflection film, and / or a NIR (Near-Infrared) cut layer.
[0125] The method for manufacturing the optical modulation device is not particularly limited, and the device can be manufactured by a known method other than the application of the above-mentioned elements as each component.
[0126] The present application also relates to an optical device, which may have a structure in which the light modulating device is encapsulated with an encapsulant.
[0127] Such an optical device may include first and second outer substrates disposed opposite to each other, and the light modulating device encapsulated with an encapsulant between the first and second outer substrates. The first and second outer substrates are separate substrates that are distinct from the substrates included in the light modulating film layer, and therefore are referred to as outer substrates. Thus, the optical device may include at least four substrates, including the first and second substrates included in the light modulating film layer and the first and second outer substrates.
[0128] The expressions "first" and "second" in the names of the substrates are merely for convenience in distinguishing the substrates, and do not define the order or hierarchical relationship of the substrate or the outer substrate. The light modulation device may be encapsulated between the two outer substrates. Such encapsulation may be performed using an encapsulant, which may be an adhesive film.
[0129] The outer substrate may be, for example, an inorganic substrate made of glass or a plastic substrate. Examples of the plastic substrate include, but are not limited to, triacetyl cellulose (TAC) film, cycloolefin copolymer (COP) film such as norbornene derivatives, poly(methyl methacrylate) film, and acrylic film such as poly(methyl methacrylate) (PMMA), polycarbonate (PC) film, polyethylene (PE) film, polypropylene (PP) film, polyvinyl alcohol (PVA) film, diacetyl cellulose (DAC) film, polyacrylate (PAC) film, polyether sulfone (PES) film, polyetheretherketon (PEEK) film, polyphenylsulfone (PPS) film, polyetherimide (PEI) film, polyethylenemaphthate (PEN) film, polyethyleneterephtalate (PET) film, polyimide (PI) film, polysulfone (PSF) film, polyarylate (PAR) film, and fluororesin film. The outer substrate may have a coating layer of gold, silver, silicon dioxide, silicon monoxide, or other silicon compound, or an anti-reflection layer, if necessary.
[0130] The thickness of the outer substrate is not particularly limited and may be, for example, about 0.3 mm or more. As another example, the thickness may be about 0.5 mm or more, about 1 mm or more, about 1.5 mm or more, or about 2 mm or more, or may be about 10 mm or less, 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, or 3 mm or less.
[0131] The outer substrate may be a flat substrate or a substrate having a curved shape. For example, the two outer substrates may both be flat substrates or may both be curved substrates, or one of the substrates may be a flat substrate and the other may be a curved substrate.
[0132] When both of the above surfaces have a curved shape, the respective curvatures or radii of curvature may be the same or different.
[0133] The optical device may further include an encapsulant, e.g., an adhesive film, encapsulating the light modulating device within the outer substrate. Such an adhesive film may be present, for example, at least between the outer substrate and the light modulating device. For example, when the light modulating device includes both the light modulating film layer and the polarizing layer, the encapsulant (adhesive film) may be present at at least one of the positions between the outer substrate and the light modulating film layer, between the light modulating film layer and the polarizing layer, and between the polarizing layer and the outer substrate. Also, the encapsulant may be present on the sides (preferably all sides) of the light modulating device, for example, on the sides (preferably all sides) of the light modulating film layer and the polarizing layer.
[0134] An adhesive film as an encapsulant may encapsulate the light modulating device by adhering the outer substrate and at least one component of the light modulating device to each other.
[0135] For example, the structure can be realized through an autoclave process in which an outer substrate, an optical modulation device, and an encapsulant (adhesive film) are laminated and then pressurized according to a desired structure. Even after such a pressurization process, the present application can efficiently maintain the performance of the optical modulation device as designed.
[0136] The encapsulating agent (adhesive film) is not particularly limited, and known materials can be used. For example, a suitable film can be selected from known thermoplastic polyurethane adhesive films (TPU: Thermoplastic Polyurethane), TPS (Thermoplastic Starch), polyamide adhesive films, polyester adhesive films, EVA (Ethylene Vinyl Acetate) adhesive films, polyolefin adhesive films such as polyethylene or polypropylene, or polyolefin elastomer films (POE films).
[0137] The thickness of the encapsulating agent (such as an adhesive film) is not particularly limited and may be, for example, within a range of about 200 μm to 600 μm. The thickness of the adhesive film may be the thickness of the adhesive film between the outer substrate and the optical modulation device, for example, the gap between the two.
[0138] In addition to the above-mentioned components, the optical device may further include other necessary components, and examples of such components include, but are not limited to, a buffer layer, a retardation layer, an optical compensation layer, an anti-reflection layer, and / or a hard coating layer.
[0139] The optical device may include encapsulating the light modulation device between the first and second outer substrates disposed opposite to each other through a pressurizing process using the encapsulant.
[0140] In this case, the specific type of the pressurizing process is not particularly limited. For example, the pressurizing process may be an autoclave process.
[0141] Therefore, the method for manufacturing the optical device may include encapsulating the light modulation device between first and second outer substrates disposed opposite to each other through an autoclave process using an adhesive film.
[0142] The autoclave process can be carried out by disposing an adhesive film and a light modulation device between outer substrates according to a desired encapsulation structure, and applying heat and pressure.
[0143] For example, an optical device can be formed by arranging an outer substrate, an adhesive film, a light modulation device, an adhesive film, and an outer substrate in the above order, and then arranging an adhesive film on the side of the light modulation device as well, and then heating and pressurizing the laminate in an autoclave process.
[0144] The conditions of the autoclave process are not particularly limited, and for example, the process can be carried out under suitable temperature and pressure depending on the type of encapsulating agent (adhesive film) applied. The temperature of the typical autoclave process is about 40°C or more, 50°C or more, 60°C or more, 70°C or more, 80°C or more, 90°C or more, or 100°C or more, and the pressure is 2 atm or more, but is not limited thereto. The upper limit of the process temperature may be about 200°C or less, 190°C or less, 180°C or less, or 170°C or less, and the upper limit of the process pressure may be about 10 atm or less, 9 atm or less, 8 atm or less, 7 atm or less, or 6 atm or less.
[0145] Such optical devices can be used for a variety of purposes, including, for example, eyewear such as sunglasses and eyewear for AR (Argumented Reality) or VR (Virtual Reality), the exterior walls of buildings, and sunroofs for vehicles. Effect of the Invention
[0146] The present application can provide a light modulation device, an optical device, or a manufacturing method thereof, capable of stably maintaining designed optical characteristics even after an encapsulation process in which pressure is applied, such as an autoclave process, etc. The present application can also provide a light modulation device, an optical device including the same, or a manufacturing method thereof, capable of stably maintaining the alignment state of a light modulation layer while effectively ensuring adhesion between upper and lower substrates. [Brief description of the drawings]
[0147] [Figure 1] 1 is a schematic diagram of an exemplary light modulating device of the present application. [Diagram 2] 1 is a schematic diagram of an exemplary light modulating device of the present application. [Diagram 3] 1 is a schematic diagram of an exemplary light modulating device of the present application. [Figure 4] 11A to 11C are diagrams for explaining a process of determining the refractive index anisotropy of a light modulation layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0148] The present application will be described in detail with reference to the following examples, but the scope of the present application is not limited to the following examples.
[0149] 1. Evaluation of phase difference The in-plane retardation value (Rin) of the film was measured for light with a wavelength of 550 nm using Agilent UV / VIS spectroscope 8453. Two polarizers were installed in the UV / VIS spectroscope so that the transmission axes were perpendicular to each other, and the polymer film was installed between the two polarizers so that the slow axis was at 45 degrees to the transmission axes of the two polarizers, and then the transmittance was measured according to wavelength. The phase retardation order of each peak in the transmittance graph according to wavelength was calculated. Specifically, in the transmittance graph according to wavelength, the waveform satisfies the following formula A, and the condition for the maximum peak Tmax in a sine waveform satisfies the following formula B. When λmax is found in formula A, T in formula A and T in formula B are the same, so the formula is expanded. The formula is expanded for n+1, n+2 and n+3, n and n+1 formulas are rearranged, R is eliminated, and n is rearranged with λn and λn+1 formulas, leading to the following formula C. Since n and λ can be known based on the fact that T in formula A and T in formula B are the same, R is found for each λn, λn+1, λn+2 and λn+3. A linear trend line of R value by wavelength is found for the four points, and the R value for the formula 550 nm is calculated. The function of the linear trend line is Y=ax+b, where a and b are constants. The Y value when 550 nm is substituted for x in the above function is the Rin value for light with a wavelength of 550 nm.
[0150] [Formula A] T=sin 2 [(2πR / λ)]
[0151] [Formula B] T=sin 2 [((2n+1)π / 2)]
[0152] [Formula C] n=(λn-3λn+1) / (2λn+1+1-2λn)
[0153] In the above, R means an in-plane retardation Rin, λ means a wavelength, and n means an order of the peak of a sine wave.
[0154] 2. Evaluation of the thickness of the light modulation layer (liquid crystal layer) The thickness of the light modulation layer, i.e., the cell gap, is equal to the height of the spacer, so the height of the spacer was measured and used as the cell gap. The height of the spacer was measured using a measuring device (Optical Profiler, Nano View-E1000, manufactured by Nano System Co., Ltd.).
[0155] 3. Evaluation of refractive index anisotropy of the light modulation layer (liquid crystal layer) The refractive index anisotropy △n is evaluated using an Abbe refractometer in the following manner. A vertical alignment film is coated on the surfaces of the measuring prism and illumination prism of the Abbe refractometer, and the liquid crystal compound to be measured is applied to the measuring prism and then covered with the illumination prism. The liquid crystal compound is vertically aligned by the vertical alignment force of the two interfaces. The liquid crystal compound applied in this process is only the liquid crystal compound applied to the transmittance variable layer that is not mixed with other substances such as dichroic dyes. Then, as shown in FIG. 4, a linear polarizer is applied to the eyepiece side, and light is irradiated and observed, and θe and θo can be obtained as shown in FIG. 4. The extraordinary refractive index (ne=npsinθe) and the ordinary refractive index (no=npsinθo) can be obtained through the refractive index np of the measuring prism and the angles θe and θo, and the difference (ne-no) can be defined as the refractive index anisotropy. The reference wavelength in the measurement is about 550 nm.
[0156] 4. Evaluation of the pitch of the light modulation layer (liquid crystal layer) The pitch p in the twisted orientation was measured by a measurement method using a wedge cell, specifically, by the method described in "Simple method for accurate measurements of the cholesteric pitch using a stripe-wedge Grandjean-Cano cell" by D. Podolskyy et al. (Liquid Crystals, Vol. 35, No. 7, July 8 / 2008, 789-791).
[0157] Example 1. Fabrication of optical modulation devices A PET (poly(ethylene terephthalate)) film (Toyobo, SRF product) with a thickness of about 80 μm was used as the first substrate of the optical modulation device. The in-plane retardation (550 nm) of the PET film was about 9,000 nm. An optically anisotropic film (negative C film satisfying the formula 3), an ITO (indium tin oxide) layer, and a silicone adhesive layer were formed in this order on the surface of the PET film (a laminated structure of first substrate / optically anisotropic film / ITO layer / adhesive layer). The optically anisotropic film was formed by coating a polyamide coating liquid (a coating liquid obtained by diluting polyamide obtained by polymerizing terephthalic acid, isophthalic acid, and 2,2'-bis(trifluoromethyl)-4,4'-biphenyldiamine in a dimethylacetamide solution at a concentration of 5.3% by weight) on a substrate and then drying it, and the retardation in the thickness direction was about -220. The ITO layer was formed by a known deposition method, and the adhesive was formed by bar coating a silicone adhesive composition (Shinetsu, KR3700) and drying at about 150° C. for 5 minutes to a thickness of about 10 μm.
[0158] As the second substrate, a PET (poly(ethylene terephthalate)) film (SKC, highly stretched PET product) with a thickness of about 145 μm and an ITO (Indium Tin Oxide) layer deposited on the first surface was used. The in-plane retardation (550 nm) of the PET film was about 10,000 nm. On the ITO layer of the PET film, a honeycomb-type partition-type spacer was formed, in which the pitch of the regular hexagons (closed figures) constituting the honeycomb was about 350 μm and the line width was about 10 μm. The height of the spacer was formed so as to satisfy the thickness (cell gap) of the liquid crystal layer (light modulation layer) listed in Table 1 below. A vertical alignment film (5661LB3, Nissan) was formed on the spacer to a thickness of about 300 nm. The vertical alignment film was formed by rubbing in one direction. The rubbing direction was perpendicular to the slow axis direction of the second substrate.
[0159] Next, a liquid crystal composition was coated on the surface of the vertical alignment film of the second substrate, and the adhesive layer of the first substrate was laminated to face the surface coated with the liquid crystal composition to prepare a light modulating film layer. At this time, the slow axes of the first and second substrates were adjusted to be parallel to each other.
[0160] The liquid crystal composition used herein includes a liquid crystal compound (Merck, MAT-19-753) and a chiral dopant (Merck, S811). The content of the chiral dopant was adjusted so that the pitch (chiral pitch) p of the twisted orientation could satisfy Table 1 below.
[0161] Fabrication of optical devices The manufactured light modulating film layer was encapsulated with a PVA (poly(vinyl alcohol)) polarizing layer between two outer substrates using an adhesive film (encapsulating agent). During the encapsulation, the PVA polarizing layer was present on the second surface of each of the first and second substrates of the light modulating film layer, and the absorption axis of the PVA polarizing layer present on the second surface of the second substrate was perpendicular to the slow axis of the second substrate, and the absorption axis of the PVA polarizing layer present on the second surface of the first substrate was parallel to the slow axis of the first substrate. A thermoplastic polyurethane adhesive film (thickness: about 0.38 mm, manufacturer: Argotec, product name: ArgoFlex) was used as the adhesive film, and a glass substrate with a thickness of about 3 mm was used as the outer substrate. A laminate was produced by stacking the first outer substrate, the adhesive film, the PVA polarizing layer, the adhesive film, the light modulating film layer, the adhesive film, the PVA polarizing layer, the adhesive film and the second outer substrate in the above order, and also placing the adhesive film on all sides of the light modulating film layer.Then, an autoclave process was performed at a temperature of about 100°C and a pressure of about 2 atmospheres to produce an optical device.
[0162] Examples 2 to 9. An optical modulation device and an optical device were fabricated in the same manner as in Example 1, except that the thickness (cell gap, t) of the liquid crystal layer (light modulation layer) and the pitch of the twist orientation were adjusted as shown in Table 1 below when fabricating the optical modulation device (in Table 1 below, Δn is the refractive index anisotropy of the liquid crystal layer, t is the thickness of the liquid crystal layer, p is the pitch, and K is a value calculated by Δn×p / t).
[0163] [Table 1]
[0164] Comparative Examples 1-7. An optical modulation device and an optical device were fabricated in the same manner as in Example 1, except that the thickness t (cell gap) of the liquid crystal layer (light modulation layer) and the pitch of the twist orientation were adjusted as shown in Table 2 below when fabricating the optical modulation device (in Table 2 below, Δn is the refractive index anisotropy of the liquid crystal layer, t is the thickness of the liquid crystal layer, p is the pitch, and K is a value calculated by Δn×p / t).
[0165] [Table 2]
[0166] The transmittance was evaluated in a state where a voltage of about 60 V was applied to the light modulation device and the optical device of each of the examples and comparative examples, and the results are summarized and shown in Tables 3 and 4 below. That is, the transmittance for the light modulation device is the transmittance before the pressurizing step (autoclave) is performed, and the transmittance for the optical device is the transmittance after the pressurizing step (autoclave) is performed. The rate of change in transmittance before and after the pressurizing step is also summarized and shown in Tables 3 and 4 below. The transmittance was evaluated using a Hazemeter (NDH-5000SP).
[0167] [Table 3]
[0168] [Table 4]
[0169] As summarized in Tables 3 and 4, the optical modulation devices of the examples exhibited appropriate transmittance, and the transmittance was stably maintained even after the pressurization step (autoclave step).
[0170] On the other hand, in the comparative examples, the change in transmittance before and after the pressurization step was large, or the transmittance itself did not reach the target value. Also, in the comparative examples 5 to 7, the alignment of the liquid crystal compound itself was not performed well, so that it was impossible to measure the transmittance.
Claims
1. a first substrate and a second substrate each having a first surface and a second surface and disposed opposite to each other; a liquid crystal layer between the first substrate and the second substrate, the liquid crystal layer being formed to realize a twisted orientation; and a pressure sensitive adhesive layer formed on the first surface of the first substrate; and a first electrode layer disposed between the first surface of the first substrate and the pressure-sensitive adhesive layer or the adhesive layer; a second electrode layer formed on the first surface of the second substrate; a partition-type spacer formed on the second electrode layer; a liquid crystal alignment film formed on the partition-type spacer; Including, the first substrate and the second substrate are disposed such that the first surfaces face each other; An optical modulation device having a K value in the following formula 1 in the range of 0.19 to 0.4: [Formula 1] K = Δn × p / t In Equation 1, Δn is the refractive index anisotropy of the liquid crystal layer, p is the pitch in the twisted orientation, and t is the thickness of the liquid crystal layer.
2. An optical modulation device as described in claim 1, wherein the liquid crystal alignment film is a rubbed alignment film or a photo-aligned film, and a second electrode layer is arranged between the first surface of the second substrate and the liquid crystal alignment film.
3. 3. The light modulation device according to claim 1, wherein the pressure-sensitive adhesive layer is a silicone pressure-sensitive adhesive layer.
4. The optical modulation device according to claim 1 , wherein the liquid crystal alignment film is not formed on the first substrate.
5. The optical modulation device according to claim 1 , wherein the liquid crystal alignment film is a vertical alignment film.
6. 6. The light modulation device according to claim 1, wherein the refractive index anisotropy Δn of the liquid crystal layer is in the range of 0.01 to 0.
5.
7. 7. The optical modulation device according to claim 1, wherein the pitch p of the twisted orientation is in the range of 1 μm to 100 μm.
8. A light modulation device according to any one of the preceding claims, wherein the thickness t of the liquid crystal layer is in the range of 0.5 μm to 50 μm.
9. 9. The light modulation device according to claim 1, wherein the ratio t / p of the pitch p of the twisted orientation and the thickness t of the liquid crystal layer is less than 1.
10. 10. The light modulation device according to claim 1, wherein the liquid crystal layer is initially in a vertical alignment state and is formed so as to realize a twisted alignment when a voltage is applied.
11. 11. A light modulating device according to claim 1, wherein the liquid crystal layer comprises a liquid crystal compound and a chiral dopant.
12. The optical modulation device according to claim 1 , wherein the first substrate or the second substrate has an in-plane retardation of 500 nm or more for light having a wavelength of 550 nm.
13. 13. The light modulation device of claim 1, further comprising a polarizing layer disposed on a second surface of the first substrate or the second substrate.
14. The optical modulation device according to any one of claims 1 to 13, further comprising a polarizing layer disposed on the second surface of the first substrate or the second substrate, wherein the first substrate or the second substrate has an in-plane retardation of 500 nm or more for light having a wavelength of 550 nm, and a small angle between the slow axis of the first substrate or the second substrate and the absorption axis of the polarizing layer is in the range of 80 degrees to 100 degrees.
15. The light modulation device according to claim 1 , further comprising an optically anisotropic film between the first substrate or the second substrate and the liquid crystal layer, the optically anisotropic film satisfying the following formula 3: [Formula 3] nz < ny In Equation 3, ny is the refractive index of the optically anisotropic film at a wavelength of 550 nm in the fast axis direction, and nz is the refractive index of the optically anisotropic film at a wavelength of 550 nm in the thickness direction.
16. An optical device comprising: a first outer substrate and a second outer substrate arranged opposite each other; and a light modulation device according to any one of claims 1 to 15, encapsulated with an encapsulating agent between the first outer substrate and the second outer substrate.
17. A method for manufacturing an optical device, comprising the step of encapsulating an optical modulation device according to any one of claims 1 to 15 between a first outer substrate and a second outer substrate arranged opposite to each other through a pressure process using an encapsulating agent.
18. A window comprising a light modulating device according to any one of claims 1 to 15.
19. A sunroof comprising a light modulating device according to any one of claims 1 to 15.
Citation Information
Patent Citations
Dimming device and its manufacture
JP1989186911A
Liquid crystal display element and method for manufacturing the same
JP2008046662A
Liquid crystal display element and method of manufacturing the same
JP2009181063A
Vertically oriented liquid crystal display
JP2010039281A