Method for evaluating primary particles in porous secondary particles

The method of binarization and watershed algorithm applied to electron microscopy images allows for precise evaluation of primary particle connections in porous secondary particles, addressing the trade-off between void volume and crushing strength, enhancing material design precision.

JP7589491B2Active Publication Date: 2024-11-26SUMITOMO METAL MINING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2020173415
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-27
Filing Date
2020-10-14
Publication Date
2024-11-26
Estimated Expiration
2040-10-14

AI Technical Summary

Technical Problem

Existing methods for evaluating the connection area between primary particles in porous secondary particles are inadequate for precise material design, as they rely on macro physical properties and do not provide microscopic analysis of the connection volume or area, leading to a trade-off between void volume and crushing strength.

Method used

A method involving binarization, watershed algorithm, and image analysis is used to evaluate the degree of connection between primary particles in porous secondary particles, utilizing focused ion beam processing and electron microscopy to obtain detailed three-dimensional images, followed by pixel size equalization, noise removal, and morphological processing to define and quantify the connection areas.

Benefits of technology

Enables precise evaluation of the connection degree of primary particles, correlating with the crushing strength of porous secondary particles, allowing for improved material design by balancing void volume and strength properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589491000001
    Figure 0007589491000001
  • Figure 0007589491000002
    Figure 0007589491000002
  • Figure 0007589491000003
    Figure 0007589491000003
Patent Text Reader

Abstract

To provide a technique of evaluating the degree of connection of primary particles in porous secondary particles from an observed image.SOLUTION: There is provided a method for evaluating primary particles in porous secondary particles formed by connecting primary particles, the method including: a binarization step of obtaining a binarization image formed by binarizing an observed image of porous secondary particles; a connection part defining step of defining a connection part between primary particles in the binarization image, using a watershed algorithm; and a connection degree evaluation step of evaluating the degree of connection of primary particles in porous secondary particles from the area or the volume of the connection part. There is also provided a technique related to the method.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating primary particles in porous secondary particles. [Background technology]

[0002] As shown in Non-Patent Document 1, a method is known in which the breaking strength and deformation strength of a microparticle are measured by applying a load to the microparticle. [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] JIS Z 8844:2019 (Method of measurement for breaking strength and deformation strength of microparticles) Summary of the Invention [Problem to be solved by the invention]

[0004] In particulate materials used in electronic devices, etc., material design may be implemented to make the particles porous in order to increase the reaction area, etc.

[0005] Porous particles are made by linking primary particles into a complex network to form secondary particles that contain numerous internal voids.

[0006] In this specification, primary particles are particles generated by the growth of a single crystal nucleus, and secondary particles are particles generated by the coalescence, growth, aggregation, solidification, etc. of primary particles. Also, porous secondary particles, as the name suggests, are secondary particles in which a large number of pores are formed (for example, a porosity of 1% or more).

[0007] The trade-off in material design of making particles porous is that the connection area between primary particles becomes smaller compared to solid particles (non-porous particles), resulting in a smaller crushing strength (i.e., the maximum load that can be withstood).

[0008] Since there is a trade-off between the void volume in the porous secondary particles and the crushing strength, it is necessary to design materials that balance both properties.

[0009] In order to increase the void volume within the secondary particles while maintaining the crushing strength as much as possible, it is necessary to make the connecting area between the primary particles porous to a certain extent, and various measures for improving this have been attempted.

[0010] The effects of such improvement measures have conventionally only been evaluated using evaluation methods based on macroscopic physical property information such as crushing strength as shown in Non-Patent Document 1. On the other hand, in order to carry out more precise material design, there has been an increasing need for microscopic analysis methods that analyze the size of the connection area or connection volume between primary particles.

[0011] An object of the present invention is to provide a method for evaluating the degree of connectivity of primary particles within a porous secondary particle from an observed image. [Means for solving the problem]

[0012] The first aspect of the present invention is A method for evaluating primary particles in porous secondary particles formed by connecting a plurality of primary particles, comprising the steps of: a binarization step of binarizing the observation image of the porous secondary particles to obtain a binarized image; defining connections between primary particles in the binarized image using a watershed algorithm; a step of evaluating the degree of connectivity of the primary particles in the porous secondary particles based on the area or volume of the connection portions; The present invention relates to a method for evaluating primary particles in porous secondary particles.

[0013] The second aspect of the present invention is the invention according to the first aspect, The observation image is a three-dimensional observation image obtained by acquiring two-dimensional observation images in the depth direction, which are obtained by cross-sectional processing of a porous secondary particle using a focused ion beam processing and observation device (FIB) and image observation using a scanning electron microscope (SEM), or a three-dimensional observation image obtained by a tomography method using a transmission electron microscope (TEM) on a porous secondary particle.

[0014] A third aspect of the present invention is the invention according to the first or second aspect, a number evaluation step of evaluating the number of primary particles after separating the primary particles at the connection portion in the binarized image, In the connectivity evaluation step, a value is obtained by dividing the area or volume of the connected portion obtained in the connected portion definition step by the number of primary particles obtained in the number evaluation step.

[0015] A fourth aspect of the present invention is the invention according to the third aspect, In the number evaluation step, an image of primary particles separated at the connection portion is obtained, The area or volume of the connection portion is obtained by subtracting the area or volume of the post-separation primary particle image from the area or volume of the primary particle before separation in the binarized image before the connection portion defining step.

[0016] A fifth aspect of the present invention is the invention according to any one of the first to fourth aspects, The method further includes, prior to the binarization step, a pixel size equalization step of making equivalent pixel sizes in the X-axis and Y-axis or the X-axis, Y-axis and Z-axis of the observation image of the porous secondary particles, taking into account the incident angle of the electron beam of the electron microscope used to obtain the observation image with respect to the porous secondary particles.

[0017] A sixth aspect of the present invention is the invention according to any one of the first to fifth aspects, a tertiary particle observation image pixel size equalization step of equalizing pixel sizes in the X-axis and Y-axis or the X-axis, Y-axis, and Z-axis directions for an observation image of a tertiary particle formed by connecting a plurality of porous secondary particles, taking into account the incident angle of an electron beam of an electron microscope used to obtain the observation image of the tertiary particle with respect to the tertiary particle; a tertiary particle observation image binarization step of obtaining a binarized image by binarizing the observation image of the tertiary particles after the size equalization step; a binary image smoothing step of performing morphology processing on the binary tertiary particle image; a connection portion defining step of defining connections between secondary particles in the tertiary particle binary image after the binary image smoothing step using a watershed algorithm; and The porous secondary particles separated at the connection portions in the binarized tertiary particle image are used as the subject of evaluation of the degree of connection of primary particles.

[0018] A seventh aspect of the present invention is the invention according to any one of the first to sixth aspects, The method further includes a crushing strength evaluation step in which, when the degree of connectivity obtained in the connectivity evaluation step is large, the crushing strength of the porous secondary particles is evaluated to be large, and, when the degree of connectivity obtained in the connectivity evaluation step is small, the crushing strength of the porous secondary particles is evaluated to be small. Effect of the Invention

[0019] According to the present invention, the degree of connectivity of primary particles within a porous secondary particle can be evaluated from an observed image. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic diagram showing an example of the binarization process. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a junction definition process using the watershed algorithm. [Diagram 3] FIG. 3 is a schematic diagram showing an example of the number evaluation step. [Figure 4]FIG. 4 is a schematic diagram showing an example of a method for acquiring the area or volume of a connected portion in the connection degree evaluation step. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] This embodiment relates to a method for evaluating primary particles in porous secondary particles formed by connecting a plurality of primary particles. Hereinafter, this embodiment will be described with reference to the drawings. "~" indicates a predetermined value or more and a predetermined value or less.

[0022] [Observation image acquisition] First, an observation image to be used for analysis is obtained. In this embodiment, as the observation image to be obtained first, an observation image of a tertiary particle formed by connecting a plurality of porous secondary particles is exemplified by an electron microscope. Since a tertiary particle is formed by connecting a plurality of porous secondary particles, the tertiary particle should be described as a porous tertiary particle in principle, but for convenience of explanation, it will be simply described as a tertiary particle. The tertiary particle, the porous secondary particle, and the primary particle are all conductive particles or particles to which conductivity has been imparted. The tertiary particle will also be simply referred to as a "sample." Since the sample refers to a tertiary particle, the sample also includes a porous secondary particle and a primary particle.

[0023] The average particle diameter of the primary particles (calculated, for example, by a laser diffraction particle size distribution analyzer) may be, for example, several nm to several hundreds of nm, and the average particle diameter of the porous secondary particles may be, for example, several hundreds of nm to several hundreds of μm.

[0024] Observation is performed by selecting an evaluation device and observation conditions with appropriate spatial resolution, taking into consideration the size of the target sample and the expected contact area with the probe. For example, it is possible to observe images using a scanning electron microscope (hereinafter abbreviated as SEM) for samples of several tens of nm to several hundreds of μm, and a transmission electron microscope (hereinafter abbreviated as TEM) for particles of several nm to several hundreds of nm. Note that scanning transmission electron microscopes (STEM) belong to both types.

[0025] In addition to two-dimensional observation images, three-dimensional observation images can be used. Since the connections between particles (specifically, the connection network) are formed three-dimensionally, it is desirable to use three-dimensional observation images in order to understand the material properties in more detail.

[0026] In the case of SEM, a 3D observation image can be obtained by repeating cross-sectional processing at a fixed processing width and SEM observation using an SEM device equipped with a focused ion beam processing and observation device (FIB). A set of 2D observation images (i.e., images obtained for each depth direction) can be used to obtain a 3D constructed image using image analysis software.

[0027] It is also possible to obtain a three-dimensional image by using TEM tomography to reconstruct two-dimensional images taken at different tilt angles.

[0028] As the pre-processed sample, in the case of SEM, a sample whose cross section has been processed by FIB or cross-section polisher, polishing, etc. may be used. In the case of TEM, a sample prepared by the dispersion method, transfer method, FIB processing, etc. may be used.

[0029] The image acquisition conditions may be changed as appropriate depending on the size of the particle to be observed, etc. For example, in SEM observation, each measurement parameter may generally be changed based on the following considerations.

[0030] <Accelerating voltage> The higher the accelerating voltage, the more information from the deeper part of the sample from the top surface is mixed into the observed image. In other words, even though the observed image is a two-dimensional image, information in the depth direction (such as information on particles buried in the cross section) is also mixed into the observed image. For this reason, it is preferable to use conditions with as low an accelerating voltage as possible within the range that can guarantee the required spatial resolution.

[0031] <Current> In general, a lower current value (smaller aperture size) results in higher spatial resolution. On the other hand, the brightness decreases, the signal level decreases, noise increases, and image quality deteriorates. Therefore, it is preferable to select conditions that balance spatial resolution and image quality.

[0032] <Working distance> In SEM observation, shortening the working distance reduces lens aberration and increases resolution. In particular, shortening the working distance is preferable when observing under low accelerating voltage conditions, as it increases spatial resolution.

[0033] <Magnification and number of pixels in observed image> The higher the magnification, the higher the spatial resolution; however, the observable range and number of particles decrease. Therefore, a balanced condition should be selected, taking into consideration the number of particles required for observation and the spatial resolution.

[0034] The greater the number of pixels, the higher the image resolution will be, but on the other hand, there is a tradeoff, such as the longer the image acquisition time. Therefore, an appropriate value should be selected depending on the required image resolution.

[0035] The size of one pixel (hereafter referred to as pixel in the case of two dimensions and voxel in the case of three dimensions) is the smallest unit of processing in the image analysis that will be performed later. In image analysis, the magnification and number of pixels (and therefore the dimensions of one pixel in real space) are determined with the required resolution in mind.

[0036] <Beam dwell time per sweep> The longer the dwell time, the greater the signal amount, the less noise there is, and the better the image quality will be; however, this is a trade-off as it also lengthens the observation time, so appropriate conditions should be selected within the necessary range.

[0037] <Detector> Electrons generated by an electron beam incident on a sample can be broadly divided into secondary electrons (inelastically scattered electrons) and backscattered electrons (elastically scattered electrons). In SEM, the ratio of secondary electron and backscattered electron signals in the observation image is generally adjusted by adjusting various detectors and detection conditions to obtain the desired observation image. When performing image analysis, materials are often separated by contrast due to their composition. In addition, the contrast caused by the unevenness of the sample, which occurs during cross-sectional processing of the sample, is an obstacle in image analysis, so secondary electron images with strong contrast caused by unevenness due to edge effects are undesirable. Therefore, when performing image analysis, it is desirable to observe images that are made up of backscattered electrons.

[0038] In the case of TEM, the higher the accelerating voltage, the greater the spatial resolution. However, depending on the sample, damage may occur due to electron beam irradiation. When handling such samples, it is acceptable to make adjustments such as reducing the accelerating voltage or current value.

[0039] [Image Analysis] <3D construction> A 3D image may be constructed using the method described above in [Acquisition of observation image]. In general, the axes of a 3D constructed image are defined as the horizontal direction of the 2D observation image as the X-axis, the vertical direction as the Y-axis, and, when using an SEM, the FIB cross-section processing direction as the Z-axis.

[0040] Two-dimensional observation images are often affected by stage drift during observation and have slight misalignment in X and Y positions, so when overlaying the images, least-squares fitting can be performed between adjacent images to align the X and Y positions.

[0041] In the case of TEM, a 3D image may be constructed by tomography. Specifically, 2D observation images are taken at different tilt angles. In this case, Au nanopowder or the like is added to the sample in advance. Then, position information of the markings is stored in the sample. A 3D image may be constructed by performing position alignment using least squares fitting based on this position information in the sample, as in SEM.

[0042] <Pixel size equalization process> Prior to the binarization process described below, a pixel size equalization process may be performed on the observed image of the sample to equalize the pixel sizes in the X-axis and Y-axis or the X-axis, Y-axis, and Z-axis, taking into account the incident angle of the electron beam of the electron microscope used to obtain the observed image with respect to the porous secondary particles.

[0043] <Noise removal process> Noise contained in the observation image (hereinafter also referred to as "image") with the pixel size equalized may become an obstacle in the subsequent binarization process. Therefore, a noise removal process may be performed as necessary. As a specific method for the noise removal process, a known noise removal technique employed in general image processing techniques may be used.

[0044] <Binarization process> FIG. 1 is a schematic diagram showing an example of the binarization process. In this process, a binarized image is obtained by binarizing the observation image of the sample after the size equalization process. Specifically, the binarization process separates the material to be analyzed from other materials. The binarization process is a process in which, for example, a range of gray scale values ​​is set for each pixel of a monochrome image to separate the materials.

[0045] Instead of the binarization process, a ternary process, a four-level process, or the like may be performed. Even in this case, it is preferable to divide the image after the ternary process into two types, a region recognized as the substance to be analyzed and the other region, and then perform the subsequent process. The binarization process of the present invention includes both performing the binarization process from the beginning and dividing the region into two types in this way after performing the ternary process or the like.

[0046] <Binarized image smoothing process> In this step, the binary image is subjected to morphology processing. In this specification, "morphology processing" refers to processing that combines several times the expansion and contraction of pixels in the island (or sea) parts of a sea-island structure when the particle images are islands and the image of the other parts is the sea, and is intended to smooth the binary image and / or remove isolated points (fill holes).

[0047] <Connection definition process using watershed algorithm> FIG. 2 is a schematic diagram illustrating an example of a junction definition process using the watershed algorithm. In this step, a watershed algorithm is used to define connections between primary particles in the binarized image. The watershed algorithm is a well-known technique in image processing, and is a method for dividing image regions having ambiguous boundaries. Specifically, in a binarized image with an island-sea structure, if the area where the island is far from the sea (i.e., the center of the island or its vicinity) is considered to be high brightness, the method sets a boundary between high brightness areas at an appropriate position according to each brightness.

[0048] In this embodiment, an example is given in which if there is even one pixel (one pixel or one voxel) of a portion having the above brightness, that portion is recognized as a high brightness portion. However, the present invention is not limited to this example, and a portion may be recognized as a high brightness portion only when there are multiple pixels of the portion having the above brightness, depending on the type of target sample, the conditions for acquiring the observation image, and other reasons.

[0049] As described above in [Acquisition of Observation Image], in this embodiment, the observation image to be acquired first is an observation image of a tertiary particle formed by connecting a plurality of porous secondary particles, observed by an electron microscope. That is, in this embodiment, it is preferable to perform the pixel size equalization process, the noise removal process, the binarization process, the binarized image smoothing process, and the connection part definition process on the observation image of the tertiary particle formed by connecting a plurality of porous secondary particles. Through these processes, porous secondary particles separated by the connection parts are extracted from the binarized tertiary particle image. Then, in this embodiment, the degree of connection of the primary particles in this porous secondary particle is evaluated.

[0050] When evaluating the degree of connectivity of primary particles in porous secondary particles, it is preferable to carry out the pixel size equalization process, the noise removal process, the binarization process, and the connection portion definition process on the observation image of the porous secondary particle, in the same manner as the observation image of the tertiary particle.

[0051] In addition, when evaluating the degree of connectivity of primary particles in porous secondary particles, the above-mentioned binary image smoothing step may or may not be performed. If it is performed, the image is smoothed, and if it is not performed, the loss of information due to image smoothing is not caused. In particular, considering that the connection parts of the primary particles are displayed in units of several pixels, the above-mentioned binary image smoothing step may not be performed.

[0052] <Number evaluation process> FIG. 3 is a schematic diagram showing an example of the number evaluation step. In this process, the number of primary particles in the binarized image after separating the primary particles at the boundary of the connection part is evaluated. There is no specific limitation on the specific method of evaluating this number, and for example, as shown in Figure 3, clustering may be performed in which a cluster surrounded by a part where pixels are not in contact with each other is regarded as one cluster, i.e., one primary particle. Furthermore, each primary particle may be numbered so that it can be distinguished later, or the total number of each primary particle may simply be obtained.

[0053] <Connectivity evaluation process> In this step, the degree of connectivity of the primary particles in the porous secondary particles is evaluated from the area or volume of the connection portion defined in the above-mentioned connection portion defining step.

[0054] There is no limitation on the method for obtaining the area or volume of the connection portion, but one example will be given below. FIG. 4 is a schematic diagram showing an example of a method for acquiring the area or volume of a connected portion in the connection degree evaluation step. First, in the number evaluation step, a post-separation primary particle image is obtained, which is separated at the connection portion. The area of ​​the connection portion may be obtained by subtracting the area of ​​the post-separation primary particle image from the area of ​​the primary particle before separation in the binarized image before the connection portion defining step. In the case of volume, the area of ​​the connection portion obtained from the primary particle image before separation in the binarized image before the connection portion defining step according to the depth in the Z-axis direction and the post-separation primary particle image may be added together to obtain the volume of the connection portion. In other words, the volume of the connection portion may be obtained by subtracting the volume of the post-separation primary particle image from the volume of the primary particle before separation in the binarized image before the connection portion defining step. As another method, the connecting portions may be specified in the above-mentioned connecting portion defining step, and the area or volume of the connecting portions may be obtained by adding up the number of pixels of the specified connecting portions.

[0055] Furthermore, in this step, it is preferable to obtain a value by dividing the area or volume of the connection part obtained in the connection part definition step by the number of primary particles obtained in the number evaluation step. Even without dividing by the number of primary particles, the area or volume of the connection part can be obtained from the total number of pixels of the connection part and the information on "what size one pixel has in real space" described in the above [Acquisition of observation image] <Magnification and number of pixels in observation image>. On the other hand, since the area of ​​the connection part is greatly affected by the number of primary particles, if it is desired to evaluate the degree of crushing strength of the porous secondary particles in more detail, it is preferable to divide the area or volume of the connection part by the number of primary particles to eliminate the effect of the number of primary particles.

[0056] The technical scope of the present invention is not limited to the present embodiment, but includes various modifications and improvements within the scope of the specific effects that can be obtained by the constituent elements of the invention and their combinations.

[0057] For example, if the porous secondary particles can be evaluated individually, there is no need to extract the porous secondary particles from the tertiary particles.

[0058] In addition, although the present embodiment has been described as an example of evaluating the degree of connectivity for a three-dimensional observation image, the technical idea of ​​the present invention can of course also be applied to a two-dimensional observation image. However, since the connection network exists in three dimensions, it is preferable to evaluate the degree of connectivity for a three-dimensional observation image, as exemplified in the present embodiment.

[0059] In addition, although the present embodiment has been described as an example in which the volume of the connecting portion is evaluated, it is of course possible to evaluate the degree of connection from the area of ​​the connecting portion. For example, it is possible to compare the areas of the connecting portions of different samples before evaluating the volume of the connecting portions, and to roughly evaluate the magnitude of the crushing strength. However, since the connecting network exists in three dimensions, it is preferable to evaluate the volume of the connecting portion, as exemplified in this embodiment.

[0060] The degree of connectivity of primary particles in porous secondary particles can be evaluated by at least carrying out the binarization step, the connection portion definition step, and the connectivity evaluation step.

[0061] The present embodiment relates to a method for evaluating the degree of connectivity of primary particles in porous secondary particles. The evaluation includes grasping the degree of connectivity and also includes comparing the degree of connectivity with the degree of connectivity in another sample.

[0062] This embodiment has exemplified a method for evaluating the degree of connectivity of primary particles in porous secondary particles, but as described above, a method similar to the method for separating primary particles from porous secondary particles is also adopted for separating porous secondary particles from tertiary particles. Therefore, the present invention can be expressed as follows: "A method for evaluating the degree of connectivity of n-th order particles in a porous (n+1)-th order particle formed by connecting a plurality of n-th order particles, a binarization step of binarizing the observation image of the porous (n+1) primary particles to obtain a binarized image; defining connections between n-th order particles in the binarized image using a watershed algorithm; a connectivity evaluation step of evaluating the connectivity of n-order particles in the porous (n+1)-order particles based on the area or volume of the connected portions; A method for evaluating the degree of connectivity of n-order particles in porous (n+1)-order particles (where n is a natural number).

[0063] The technical idea of ​​the present invention is also applied to the following configuration for separating n-order particles from porous (n+1)-order particles: "A method for evaluating the degree of connectivity of n-order particles in porous (n+1)-order particles formed by the connectivity of a plurality of n-order particles, a binarization step of binarizing the observation image of the porous (n+1) primary particles to obtain a binarized image; a connector defining step of defining connectors between n-th order particles in the binarized image using a watershed algorithm; A step of separating and extracting the n-th order particles at the connection portion; A method for extracting n-order particles from porous (n+1)-order particles.

[0064] The image processing in each of the above steps can be realized by using known software. One example is AVIZO (image analysis software manufactured by Japan FI Inc.), which will be described in the Examples section below. However, the present invention is not limited to using this software, and for example, each step related to the above [image analysis] may be handled by multiple different software. EXAMPLES

[0065] Hereinafter, the present invention will be specifically described using examples, but the present invention is not limited to the following examples at all.

[0066] First, as samples, two types of composite oxide particles were prepared. Sample A is composite oxide particles containing porous secondary particles with a relatively high porosity (porosity 45.0%), and the composite oxide particles have a relatively low crushing strength. Sample B is composite oxide particles containing porous secondary particles with a relatively low porosity (porosity 37.2%), and the composite oxide particles have a relatively high crushing strength. For each sample, based on the method described in this embodiment, the volume of the connection part of the primary particles was obtained, and after evaluating the degree of connection, when comparing the degree of connection in each sample, if the degree of connection of Sample B is greater than that of Sample A, it is consistent with the tendency of the actual crushing strength to be high or low. In that case, this example serves as evidence for obtaining the actual degree of connection, and this example becomes a material showing the validity of the present invention. Note that the numerical values (including the above porosity) related to Samples A and B shown in the items of the examples represent the average values of the test results for five lots.

[0067] After embedding Samples A and B in a thermosetting resin respectively, three-dimensional SEM observation was carried out under the following conditions.

[0068] [Three-dimensional SEM measurement conditions] · Dual Beam SEM-FIB device Scios manufactured by FEI Company, Japan <SEM observation conditions> · Acceleration voltage: 2 kV · Current value: 0.1 nA · Working distance: 7 mm · Magnification: 10 k (HFW: 20.7 μm) · Number of pixels: X: 1536 × Y: 1024 (pixel size: X: 4.56 nm × Y: 4.56 nm) · Tilt Angle: 52° · Dwell Time: 30 μs (1 Scan) ·Detector: Backscattered electron detector <FIB processing conditions> ·Acceleration voltage: 30 kV ·Current value: 100 pA ·Working distance: 19 mm ·Processing pitch: 30 nm

[0069] For the obtained set of two-dimensional images, the above AVIZO was used to perform three-dimensional construction (specifically, Y-axis tilt angle correction, XY alignment, trimming of unnecessary regions, and upper and lower brightness adjustment) to obtain a three-dimensional constructed image.

[0070] Note that the voxel size of the obtained three-dimensional constructed image is X: 13.49 nm, Y: 17.12 nm, Z: 30 nm.

[0071] For the obtained three-dimensional constructed image, the following analysis was performed to evaluate the connectivity. Contents not described below are the same as those described in this embodiment.

[0072] [Image analysis conditions] <Equivalent pixel size process for the image of tertiary particles observation> Pixel recalculation was performed so that the pixel sizes of the X-axis, Y-axis, and Z-axis became equivalent. The voxel size after recalculation is X: 13.49 nm, Y: 13.49 nm, Z: 13.49 nm.

[0073] <Binarization process for the image of tertiary particles observation> The porous particle region and the rest (the resin region used for embedding) were binarized and separated using the brightness difference.

[0074] <Smoothing process for the binarized image, process for defining connected components> By the method described in this embodiment, each of the above steps was performed. Then, porous secondary particles were extracted from the tertiary particles.

[0075] <Binarization process> For the extracted porous secondary particles, this step was performed by the method described in the binarization process for the image of tertiary particles observation.

[0076] <Connection section specified process> This process gave the area of ​​the connection part (number of pixels: pixels).Then, the areas of the connection parts according to the depth in the Z-axis direction were summed up to give the volume of the connection part (number of pixels: voxels).

[0077] <Number evaluation process> This step was carried out by the method described in this embodiment. Each primary particle was numbered so that it could be distinguished later, and the number of particles was counted. The center figure in Figure 4 is a binarized image after this step.

[0078] <Connectivity evaluation process> This step was carried out by the method described in this embodiment. In the number evaluation step, an image of the primary particles separated at the connection part was obtained, and the volume of the connection part was obtained by subtracting the image of the primary particles after separation. Then, the volume of the connection part was divided by the number of primary particles to obtain a value.

[0079] The number of primary particles in sample A after separation was 481, and the volume of the connected parts was 1.14 × 10 9 nm 3 and the (volume of the connecting part) / (number of primary particles) is 2.64×10 6 (nm 3 / number). The number of primary particles after separation in sample B was 396, and the volume of the connected parts was 1.44 × 10 9 nm 3 and the volume of the connected parts / number of primary particles is 3.74 × 10 6 (nm 3 / number). In other words, the degree of connectivity of sample B was greater than that of sample A, which coincided with the tendency of the actual crushing strength. As a result, it was found that the actual degree of connectivity can be determined by this example. In detail, when the degree of connectivity obtained in the connectivity evaluation step is large, the crushing strength of the sample (porous secondary particles) can be evaluated as being large, and when the degree of connectivity obtained in the connectivity evaluation step is small, the crushing strength of the sample (porous secondary particles) can be evaluated as being small. This crushing strength evaluation step may be performed after the connectivity evaluation step as part of the method for evaluating primary particles in porous secondary particles, which is the present invention.

Claims

1. A method for evaluating primary particles in porous secondary particles formed by connecting a plurality of primary particles, comprising the steps of: a binarization step of binarizing the observation image of the porous secondary particles to obtain a binarized image; defining connections between primary particles in the binarized image using a watershed algorithm; a step of evaluating a degree of connectivity of primary particles in the porous secondary particles based on the volume of the connected portions; The method for evaluating primary particles in porous secondary particles has the following feature.

2. The method for evaluating primary particles in porous secondary particles according to claim 1, wherein the observation image is a three-dimensional observation image obtained by acquiring two-dimensional observation images in the depth direction obtained by cross-sectional processing of the porous secondary particles using a focused ion beam processing and observation device (FIB) and image observation using a scanning electron microscope (SEM), or a three-dimensional observation image obtained by a tomography method of a transmission electron microscope (TEM) on the porous secondary particles.

3. a number evaluation step of evaluating the number of primary particles after separating the primary particles at the connection portion in the binarized image, 3. The method for evaluating primary particles in porous secondary particles according to claim 1 or 2, wherein in the connectivity evaluation step, a value is obtained by dividing the volume of the connected parts obtained in the connected part definition step by the number of primary particles obtained in the number evaluation step.

4. In the number evaluation step, an image of primary particles separated at the connecting portion is obtained, 4. The method for evaluating primary particles in porous secondary particles according to claim 3, wherein the volume of the connection portion is obtained by subtracting the volume of the post-separation primary particle image from the volume of the primary particle before separation in the binarized image before the connection portion defining step.

5. The method for evaluating primary particles in porous secondary particles according to any one of claims 1 to 4, further comprising a pixel size equalization step of equalizing pixel sizes in the X-axis and Y-axis or the X-axis, Y-axis and Z-axis of an observation image of the porous secondary particles, taking into account an incident angle of an electron beam of an electron microscope used to obtain the observation image with respect to the porous secondary particles, prior to the binarization step.

6. a tertiary particle observation image pixel size equalization step of equalizing pixel sizes in the X-axis and Y-axis or the X-axis, Y-axis, and Z-axis directions of an observation image of a tertiary particle formed by connecting a plurality of porous secondary particles, taking into account an incident angle of an electron beam of an electron microscope used to obtain the observation image of the tertiary particle with respect to the tertiary particle; a tertiary particle observation image binarization step of obtaining a binarized image by binarizing the observation image of the tertiary particles after the size equalization step; a binary image smoothing step of performing morphology processing on the binary tertiary particle image; a connection portion defining step of defining connections between secondary particles in the tertiary particle binary image after the binary image smoothing step using a watershed algorithm; and The method for evaluating primary particles in porous secondary particles according to any one of claims 1 to 5, wherein porous secondary particles separated at the connection portion in the binary image of the tertiary particles are subject to evaluation of the degree of connection of the primary particles.

7. The method for evaluating primary particles in porous secondary particles according to any one of claims 1 to 6, further comprising a crushing strength evaluation step of evaluating the crushing strength of the porous secondary particles as being high when the degree of connectivity obtained in the connection degree evaluation step is high, and evaluating the crushing strength of the porous secondary particles as being low when the degree of connectivity obtained in the connection degree evaluation step is low.

Citation Information

Patent Citations

  • Charged particle beam device

    JP2014135214A