Piezoelectric easily deformable aggregate, piezoelectric resin composition, piezoelectric film, and piezoelectric element

A piezoelectric resin composition with an inorganic-organic blend addresses the flexibility-piezoelectricity trade-off, creating a deformable piezoelectric film with comparable performance to conventional materials, suitable for wearable applications.

JP7589527B2Active Publication Date: 2024-11-26TOYO INK MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020200687
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-03
Publication Date
2024-11-26
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

Existing piezoelectric materials face a trade-off between flexibility and piezoelectric performance, with metal oxide-based materials being too rigid and resin-based materials having lower piezoelectricity, and combining them does not adequately address both properties.

Method used

A piezoelectric resin composition containing 100 parts by weight of an inorganic piezoelectric material with an average primary particle diameter of 0.1 to 10 μm and 0.1 to 30 parts by weight of an organic binder, forming an easily deformable aggregate with a compressive force of 5 mN or less for 10% deformation, which is used to create a piezoelectric film with both flexibility and piezoelectricity.

Benefits of technology

The composition achieves piezoelectric performance comparable to conventional films while providing flexibility, enabling applications that require deformability such as wearable sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589527000001
    Figure 0007589527000001
  • Figure 0007589527000002
    Figure 0007589527000002
  • Figure 0007589527000003
    Figure 0007589527000003
Patent Text Reader

Abstract

To provide an easily deformable aggregate and a piezoelectric resin composition capable of producing a piezoelectric film and a piezoelectric element having both piezoelectricity and flexibility.SOLUTION: An easily deformable aggregate includes 100 pts.wt. of spherical inorganic piezoelectric material (A) with an average primary particle size of 0.1 to 10 μm, and 0.1 to 30 pts.wt. of organic binder (B), and the average particle size is 2 to 100 μm, and the average compressive force required for a compression deformation rate of 10% is 5 mN or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piezoelectric easily deformable aggregate and a piezoelectric resin composition that can be suitably used for piezoelectric films and piezoelectric elements used in sensors and the like. [Background technology]

[0002] Metal oxides such as lead zirconate titanate are commonly known as piezoelectric materials and are used in a variety of piezoelectric devices such as ultrasonic sensors and actuators. While such metal oxide-based piezoelectric materials have high piezoelectric performance, they are very hard and inflexible. Therefore, they are not suitable for applications that require deformation of the sensor itself, such as wearable applications that have attracted attention in recent years. There are also piezoelectric materials made of resins such as polyvinylidene fluoride and its copolymers, but the piezoelectric performance of these materials is smaller than that of metal oxide-based piezoelectric materials.

[0003] In order to give piezoelectric materials flexibility, research is being conducted into combining metal oxide piezoelectric materials with resin (Patent Documents 1 and 2). However, this method does not provide sufficient piezoelectricity because the resin has a lower dielectric constant than the piezoelectric material, and it is necessary to apply a large voltage to the polarization process required to create the piezoelectric material. Reducing the resin content improves the piezoelectric performance, but it also greatly reduces flexibility. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-28323 A [Patent Document 2] Patent No. 6510148 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a piezoelectric film that has both piezoelectricity and flexibility. [Means for solving the problem]

[0006] The present invention relates to an easily deformable aggregate (C) comprising 100 parts by weight of an inorganic piezoelectric material (A) having an average primary particle size of 0.1 to 10 μm and 0.1 to 30 parts by weight of an organic binder (B), the aggregate having an average particle size of 2 to 100 μm and an average compressive force required for a compressive deformation rate of 10% of 5 mN or less.

[0007] The present invention also relates to a piezoelectric resin composition (F) comprising 20 to 90% by volume of the easily deformable aggregate (C) and 10 to 80% by volume of a binder resin (D).

[0008] The present invention also relates to a piezoelectric film (H) obtained by applying the piezoelectric resin composition (F) onto a substrate.

[0009] The present invention also relates to the piezoelectric film (H), wherein t is a thickness of the piezoelectric film (H) and DB is an average particle diameter of the easily deformable aggregate (C), and t / DB is 1 / 1 to 2.5 / 1.

[0010] The present invention also relates to a piezoelectric laminate (J) formed by stacking two or more types of piezoelectric films, the piezoelectric laminate (J) having a first piezoelectric film (L) containing the easily deformable aggregate (C) and a second piezoelectric film (K) containing an inorganic piezoelectric material (A) and a binder resin (D) but not containing the easily deformable aggregate (C), the first piezoelectric film (L) being stacked such that it is not located as the outermost layer of the piezoelectric laminate (J).

[0011] The present invention also relates to a piezoelectric element (M) including the piezoelectric film or the piezoelectric laminate. Effect of the Invention

[0012] The easily deformable aggregate of the present invention can impart piezoelectricity to a piezoelectric film at the same level as conventional ones even when a resin is blended to improve flexibility. Furthermore, since the piezoelectric resin composition of the present invention uses the easily deformable aggregate, it is possible to prepare a piezoelectric film that is compatible with flexibility and piezoelectricity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] <Easily deformable aggregate (C)> The easily deformable aggregate (C) of the present invention is characterized in that it contains 100 parts by weight of an inorganic piezoelectric material (A) having an average primary particle size of 0.1 to 10 μm, and 0.1 to 30 parts by weight of an organic binder (B), and has an average particle size of 2 to 100 μm and an average compressive force required for a compressive deformation rate of 10% of 5 mN or less. By using such a combination, a piezoelectric film that is compatible with flexibility and piezoelectricity can be produced.

[0014] In this specification, "easily deformable" means that the average compressive force required for a compressive deformation rate of 10% is 5 mN or less. The average compressive force required for a compressive deformation rate of 10% is the average value of the load required to deform the particles by 10% as measured by a compression test, and can be measured, for example, by a microcompression tester (MCT-210, manufactured by Shimadzu Corporation). Specifically, a very small amount of the sample to be measured is magnified under a microscope, an arbitrary particle is selected, the particle to be measured is moved to the lower part of the pressure indenter, a load is applied to the pressure indenter, and the particle to be measured is compressed and deformed. The tester is provided with a detector for measuring the compressive displacement of the particle to be measured, located above the pressure indenter. The detector measures the compressive displacement of the particle to be measured to obtain the deformation ratio. Then, the compressive force required to compress and deform the particle to be measured by 10% (hereinafter also abbreviated as "10% compressive deformation force"). The "10% compressive deformation force" is obtained in the same manner for any other particle to be measured, and the average value of the "10% compressive deformation force" for 10 particles to be measured is defined as the "average compressive force required for a compressive deformation ratio of 10%". Note that the easily deformable aggregate (C) of the present invention is in a state in which a plurality of small inorganic piezoelectric materials (A) are aggregated as described later, but in the measurement of the compressive deformation ratio, the aggregate is taken as a unit of one particle.

[0015] <Inorganic Piezoelectric Materials (A)> The inorganic piezoelectric material (A) is not particularly limited as long as it has an average primary particle diameter of 0.1 to 10 μm and has piezoelectricity, and examples thereof include barium titanate, lead titanate, bismuth titanate, sodium bismuth titanate, lead zirconate titanate, lithium niobate, sodium niobate, potassium sodium niobate, lithium tantalate, sodium tungstate, and zinc oxide. These may be used alone or in combination of two or more. From the viewpoints of toxicity and production stability, those that do not contain lead are preferred.

[0016] The inorganic piezoelectric material (A) used to obtain the easily deformable aggregate (C) has an average primary particle diameter of 0.1 to 10 μm, preferably 0.3 to 5 μm. When using an inorganic piezoelectric material (A) of one size, it is preferable to use one having an average primary particle diameter of 0.3 to 5 μm. A plurality of types of inorganic piezoelectric materials (A) of different sizes can also be used, and in this case, it is preferable to use a combination of relatively small and relatively large ones in terms of reducing the void ratio within the aggregate. If the average primary particle diameter is too small, it is difficult to align the polarity of the piezoelectric material, and the piezoelectricity tends to decrease. On the other hand, if the average primary particle diameter is too large, the aggregate is easily broken down even if an attempt is made to form it, and the aggregate itself is difficult to form. In this specification, the average primary particle size of the inorganic piezoelectric material (A) is a value measured by a particle size distribution meter (for example, Mastersizer 2000 manufactured by Malvern Instruments). The fact that the easily deformable aggregate (C) of the present invention is not easily disintegrated is also supported by the fact that, for example, even if the easily deformable aggregate (C) is placed in a glass sample tube so that the porosity is 70% and shaken in a shaker for 2 hours, the average particle size after shaking is 80% or more of the average particle size before shaking.

[0017] <Organic binder (B)> The organic binder (B) in this specification plays the role of a "binder" that binds the inorganic piezoelectric material (A). The organic binder (B) is not particularly limited, and for example, the molecular weight does not matter as long as it can play the role of a "binder", and examples thereof include surfactants, polyether resins, polyurethane resins, (unsaturated) polyester resins, alkyd resins, butyral resins, acetal resins, polyamide resins, (meth)acrylic resins, styrene / (meth)acrylic resins, polystyrene resins, nitrocellulose, benzyl cellulose, cellulose (tri)acetate, casein, shellac, gelatin, Gilsonite, rosin, rosin esters, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl cellulose, hydroxypropyl ... Examples of the organic binder include, but are not limited to, dimethyl cellulose, carboxymethyl cellulose, carboxymethyl ethyl cellulose, carboxymethyl nitrocellulose, ethylene / vinyl alcohol resin, styrene / maleic anhydride resin, polybutadiene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinylidene fluoride resin, polyvinyl acetate resin, ethylene / vinyl acetate resin, vinyl chloride / vinyl acetate resin, vinyl chloride / vinyl acetate / maleic acid resin, fluororesin, silicone resin, epoxy resin, phenoxy resin, phenol resin, maleic acid resin, urea resin, melamine resin, benzoguanamine resin, ketone resin, petroleum resin, chlorinated polyolefin resin, modified chlorinated polyolefin resin, chlorinated polyurethane resin, etc. The organic binder (B) may be used alone or in combination of two or more. (Meth)acrylic resin, styrene / (meth)acrylic resin, polyvinyl alcohol, and carboxymethyl cellulose are preferred.

[0018] In addition, the organic binder (B) is preferably non-curable since it also affects the deformability of the resulting easily deformable aggregate (C). The term "non-curable" means that the organic binder (B) does not self-crosslink at 25° C. It is preferable not to use a component that functions as a curing agent for the organic binder (B).

[0019] The easily deformable aggregate (C) of the present invention contains 0.1 to 30 parts by weight of the organic binder (B) relative to 100 parts by weight of the inorganic piezoelectric material (A), and preferably contains 0.1 to 10 parts by weight. If the amount is less than 0.1 part by weight, the inorganic piezoelectric material (A) cannot be sufficiently bound, and sufficient strength cannot be obtained to maintain the shape, which is not preferable. If the amount is more than 30 parts by weight, the effect of binding the inorganic piezoelectric material (A) is large, but the binder may get between the inorganic piezoelectric material (A) more than necessary, which is not preferable, as there is a risk of inhibiting piezoelectricity.

[0020] The average particle size of the easily deformable aggregate (C) of the present invention is 2 to 100 μm, preferably 5 to 50 μm. If the average particle size is smaller than 2 μm, the number of inorganic piezoelectric materials (A) constituting the easily deformable aggregate (C) is small, and the effect as an aggregate is low and the deformability is also poor, which is not preferred. If the average particle size exceeds 100 μm, the weight of the easily deformable aggregate (C) per unit volume becomes large, which is not preferred because it causes problems such as settling when used as a dispersion or loss of freedom in the thickness of the piezoelectric film to be formed. The average particle size of the easily deformable aggregate (C) in the present invention is a value measured by a particle size distribution meter (for example, Mastersizer 2000 manufactured by Malvern Instruments).

[0021] <Method for producing easily deformable aggregate (C)> The easily deformable aggregate (C) of the present invention can be obtained, for example, by spraying an organic binder solution containing 100 parts by weight of inorganic piezoelectric material (A), 0.1 to 30 parts by weight of organic binder (B), and a solvent, and then removing the solvent while spraying. In order to obtain easily deformable aggregates (C) having a uniform composition, it is preferable to preliminarily mix the inorganic piezoelectric material (A) and the organic binder (B) in a solvent to form a slurry, and then remove the solvent.

[0022] The method for removing the solvent from the slurry is not particularly limited, and the easily deformable aggregate (C) can be produced using a commercially available device. For example, the method can be selected from spray drying, stirring drying, static drying, and the like. Among them, spray drying can be preferably used because it can produce easily deformable aggregates (C) that are relatively close to a perfect sphere and have a uniform particle size with good productivity, and can be dried quickly and easily deformed. Specifically, the solvent may be volatilized and removed while spraying the slurry in a mist form. The spraying conditions and volatilization conditions may be appropriately selected.

[0023] <Piezoelectric resin composition (F), piezoelectric film (H)> The piezoelectric resin composition (F) of the present invention preferably contains 20 to 90 volume % of the easily deformable aggregate (C) of the present invention, 10 to 80 volume % of a binder resin (D), and a solvent (E). The volume % of each component in the piezoelectric resin composition is calculated by the calculation method described below.

[0024] A piezoelectric film (H) can be obtained by applying the piezoelectric resin composition (F) onto a substrate to form a coating film. Furthermore, the piezoelectricity of the piezoelectric film (H) can be improved by applying pressure to the piezoelectric film (H) to deform the easily deformable aggregates (C) contained therein.

[0025] By the way, to achieve high piezoelectric performance, it is important to have a small ratio of low dielectric layers. Normally, when a piezoelectric material is mixed with a resin to create a highly flexible piezoelectric film, when an electric field is applied from the outside, most of the electric field is consumed in the low dielectric parts, and almost no electric field is applied to the desired piezoelectric part. The easily deformable aggregate (C) of the present invention is expected to have high piezoelectric performance because the inorganic piezoelectric material (A) is aggregated, the distance between particles is short, and it contains almost no low dielectric components. In addition, since the aggregate part containing a large amount of piezoelectric material and the flexible resin part are separated within the film, it is expected that the film as a whole will have both properties. Moreover, the easily deformable aggregate (C) of the present invention can achieve high piezoelectric performance because it is "easily deformable". In other words, when a force is applied to the easily deformable aggregate (C), the easily deformable aggregate (C) does not collapse, and the adhesion between the inorganic piezoelectric materials (A) in the easily deformable aggregate (C) is improved, so that the inhibition of the electric field caused by the low dielectric components can be further suppressed.

[0026] The piezoelectric resin composition (F) contains a readily deformable aggregate (C), a binder resin (D), and a solvent (E). The readily deformable aggregate (C) may be used alone or in combination with a plurality of aggregates having different average particle sizes, different types or average primary particle sizes of the constituent inorganic piezoelectric materials (A), or different types or amounts of the constituent organic binders (B).

[0027] <Binder resin (D)> Examples of the binder resin (D) used in obtaining the piezoelectric resin composition (F) include polyurethane resin, polyester resin, polyester urethane resin, alkyd resin, butyral resin, acetal resin, polyamide resin, acrylic resin, styrene-acrylic resin, styrene resin, nitrocellulose, benzyl cellulose, cellulose (tri)acetate, casein, shellac, Gilsonite, gelatin, styrene-maleic anhydride resin, polybutadiene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinylidene fluoride resin, polyvinyl acetate resin, ethylene vinyl acetate resin, vinyl chloride / vinyl acetate copolymer resin, vinyl chloride / vinyl acetate / maleic acid copolymer resin, fluororesin, silicone resin, epoxy resin, phenoxy resin, and the like. One or more types selected from the group consisting of silicone resins, phenolic resins, maleic acid resins, urea resins, melamine resins, benzoguanamine resins, ketone resins, petroleum resins, rosin, rosin esters, polyvinyl alcohol, polyvinylpyrrolidone, polyacrylamide, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, carboxymethyl ethyl cellulose, carboxymethyl nitrocellulose, ethylene / vinyl alcohol resins, polyolefin resins, chlorinated polyolefin resins, modified chlorinated polyolefin resins, and chlorinated polyurethane resins can be used as appropriate depending on the application. (Meth)acrylic resin, styrene / (meth)acrylic resin, polyvinyl alcohol, polyvinylidene fluoride resin, and epoxy resin are preferred.

[0028] <Solvent (E)> The piezoelectric resin composition of the present invention preferably further contains a solvent. The solvent (E) is not particularly limited as long as it dissolves the binder resin (D), and for example, one or more solvents selected from the group consisting of water, ethyl acetate, methanol, ethanol, propanol, acetone, methyl ethyl ketone, toluene, dichloromethane, and chloroform can be appropriately used depending on the application. It is preferable to use water, acetone, or toluene.

[0029] In order to ensure the deformability, the organic binder (B) constituting the easily deformable aggregate (C) is preferably non-curable. However, the binder resin (D) contained in the piezoelectric resin composition (F) or the piezoelectric film (H) may be a binder resin (D) that cures by itself or that cures by reaction with a suitable curing agent.

[0030] In this case, the content of the easily deformable aggregate (C) can be appropriately selected according to the target piezoelectricity and application, but is preferably 20 to 90 volume % based on the solid content of the piezoelectric resin composition (F). More preferably, it is in the range of 40 to 90 volume %. If the content is less than 20 volume %, the effect of adding the easily deformable aggregate (C) is weak and sufficient piezoelectricity cannot be obtained. On the other hand, if the content exceeds 90 volume %, the content of the binder resin (D) becomes relatively small, and the flexibility of the formed piezoelectric film (H) decreases and becomes brittle, or voids are generated in the piezoelectric film (H), and there is a risk of dielectric breakdown when a high voltage is applied. The volume % here indicates a theoretical value calculated based on the weight ratio and specific gravity of the inorganic piezoelectric material (A), the organic binder (B), and the binder resin (D) relative to the solid content in the piezoelectric resin composition (F).

[0031] The piezoelectric resin composition (F) can also be used in combination with a non-aggregated inorganic piezoelectric material. By using a non-aggregated inorganic piezoelectric material in combination, the gaps between the easily deformable aggregates (C) can be filled, and when gaps are generated when the easily deformable aggregates (C) are deformed, the gaps between the inorganic piezoelectric materials (A) can be filled, and thus a further improvement in piezoelectricity can be expected. Examples of inorganic piezoelectric materials that can be used in combination include those exemplified as inorganic piezoelectric material (A).

[0032] <Method for producing piezoelectric resin composition (F) and piezoelectric film (H)> The piezoelectric resin composition (F) is preferably produced by stirring and mixing the easily deformable aggregate (C), the binder resin (D), and, if necessary, the solvent (E). A general stirring method can be used for stirring and mixing, and examples of such methods include a Scandex, a paint conditioner, a sand mill, a mortar mill, a media-less disperser, a three-roll mill, and a bead mill, and these can be combined to produce the composition.

[0033] After stirring and mixing, it is preferable to perform a defoaming step in order to remove air bubbles from the piezoelectric resin composition (F). The defoaming method is not particularly limited and can be performed using a general method, for example, vacuum defoaming, ultrasonic defoaming, etc.

[0034] The method for producing the piezoelectric film (H) of the present invention includes a step of applying the piezoelectric resin composition (F) onto a substrate to form a coating film, and a step of removing the solvent (E) from the coating film to form the piezoelectric film (H). As described above, the piezoelectric performance of the produced piezoelectric film (H) can be further improved by applying pressure to the produced piezoelectric film (H).

[0035] The substrate can be a resin film such as a PET (polyethylene terephthalate) film or a polyimide film. It is preferable to use a film that has been treated to be easily peeled off, in order to make it easier to handle when attaching electrodes to the piezoelectric film (H) in a later process. By using a metal material such as foil or plate-shaped copper, silver, gold, or SUS as the substrate, it can also be used as an electrode as is.

[0036] Examples of methods for applying the piezoelectric resin composition (F) to a substrate include knife coating, die coating, lip coating, roll coating, curtain coating, bar coating, gravure coating, flexo coating, dip coating, spray coating, and spin coating.

[0037] The relationship between the thickness t of the piezoelectric film (H) and the average particle diameter DB of the easily deformable aggregate (C) is preferably t / DB, which is 2.5 / 1 to 1 / 1. If the thickness t of the piezoelectric film (H) is such that t / DB is greater than 2.5, the piezoelectric film (H) will be too large for the size of the aggregate, and there is a high possibility that a resin component with a low dielectric constant will get between the electrodes, resulting in a decrease in piezoelectric performance. In addition, since the thickness of the piezoelectric film (H) greatly affects its resonance frequency, it is preferable to select the thickness appropriately according to the application.

[0038] After producing a piezoelectric film on any substrate, it can be laminated with any other member to produce a piezoelectric laminate (J). In this case, the piezoelectric laminate (J) has a first piezoelectric film (L) containing a piezoelectric resin composition (F) and a second piezoelectric film (K) containing a piezoelectric material composition that contains an inorganic piezoelectric material (A) and a binder resin (D) and does not contain the easily deformable aggregate (C), and it is preferable that the first piezoelectric film (L) is laminated so as not to be located as the outermost layer of the piezoelectric laminate (J). By adopting such a layered structure, it is possible to prevent aggregates from being placed in the outermost layer and to arrange the inorganic piezoelectric material (A) so as to fill the gap between the substrate and the aggregates, thereby suppressing the occurrence of voids and expected to improve the piezoelectric performance.

[0039] The film thickness t of the first piezoelectric film (L) is preferably in the range of 2.5 / 1 to 1 / 1 with respect to the average particle diameter DB of the easily deformable aggregate (C), similarly to the piezoelectric film (H). The second piezoelectric film (K) is preferably in the range of 1 to 20 μm. In addition, since the film thickness of the piezoelectric laminate (J) greatly affects its resonant frequency, it is preferable to select the film thickness appropriately according to the application.

[0040] The second piezoelectric film (K) preferably contains an inorganic piezoelectric material (A) and a binder resin (D). In order to achieve both flexibility and piezoelectric performance of the film, it is preferable that the inorganic piezoelectric material (A) occupies 50 to 90 volume % in the film and the binder resin (D) occupies 50 to 10 volume % in the film.

[0041] The piezoelectric laminate (J) is preferably produced by a press. The press treatment is not particularly limited, and a known press machine can be used. The temperature during pressing can be appropriately selected, but if it is to be used as a thermosetting adhesive sheet, it is preferable to heat the laminate to a temperature at which the binder resin (D) is thermally cured or higher.

[0042] The pressure during pressing can be appropriately selected as long as it is possible to apply a pressure that can deform the easily deformable aggregate (C), but it is preferably 1 MPa or more.

[0043] <Piezoelectric element (M)> A piezoelectric element (M) can be produced by placing two electrodes on either side of the produced piezoelectric film (H) or piezoelectric laminate (J).

[0044] The electrodes may be made of, for example, gold, silver, copper, stainless steel, silver paste, conductive carbon paste, etc. The two electrodes may be the same or different. EXAMPLES

[0045] <Creation of easily deformable aggregate (C-1)> Example 1 100 parts by weight of barium titanate powder (manufactured by Kojundo Chemical Laboratory Co., Ltd., average primary particle size: about 1 μm) as inorganic piezoelectric material (A), 2 parts by weight of polyvinyl alcohol (PVA) (Gohsenol NL-05, manufactured by Mitsubishi Chemical Corporation) as organic binder (B), and 150 parts by weight of ion-exchanged water were stirred at 1000 rpm for 1 hour in a disperser to obtain a slurry. This slurry was spray-dried in a mini spray dryer (manufactured by Nippon Buchi Co., Ltd., "B-290") in an atmosphere of 125°C to obtain an easily deformable aggregate (C-1).

[0046] <Preparation of easily deformable aggregates (C-2)~(C-14)> (Examples 2 to 9, Comparative Examples 1 to 5) Easily deformable aggregates (C-2) to (C-14) were prepared in the same manner as the easily deformable aggregate (C-1), except that the inorganic piezoelectric material (A), organic binder (B), and their amounts used were changed to those shown in Table 1.

[0047] <Evaluation of easily deformable aggregates (C)> <Average primary particle size, average particle size> The measurement was performed using a particle size distribution analyzer, Mastersizer 2000, manufactured by Malvern Instruments, Inc. The measurement conditions were an air pressure of 2.5 bar using a dry unit, and the feed rate was optimized depending on the sample.

[0048] <Average compression force required for 10% compression deformation> The average compression force required for a compression deformation rate of 10% was calculated by measuring the load required to deform the particles by 10% using a micro-compression tester (MCT-210, manufactured by Shimadzu Corporation) for 10 particles randomly selected within the measurement area, and taking the average value.

[0049] <Disintegration resistance: retention rate of average particle size after shaking test> The easily deformable aggregate (C) was placed in a glass sample tube so that the porosity was 70%, and after shaking for 2 hours in a shaker, the particle size distribution was measured and it was confirmed that the particle size after treatment was 80% or more of the average particle size before treatment.

[0050] <Preparation of Piezoelectric Resin Composition (F-1), Piezoelectric Film (H-1), and Piezoelectric Element (M-1)> Example 10 100 parts by weight of the easily deformable aggregate (C-1) (average particle diameter 10 μm) obtained in Example 1, 5 parts by weight of potassium sodium niobium powder (manufactured by Kyoritsu Material Co., Ltd., average primary particle diameter: approximately 1 μm) as the inorganic piezoelectric material (A), 10 parts by weight of polyvinyl alcohol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as the binder resin (D), and 30 parts by weight of toluene as the solvent (E) were stirred with a disperser and ultrasonically degassed to obtain a piezoelectric resin composition (F-1). The obtained piezoelectric resin composition (F-1) was applied to a release-treated sheet (a 75 μm-thick release-treated polyethylene terephthalate film) using a comma coater, and then heated and dried at 100°C for 10 minutes to obtain a piezoelectric film (H-1) with a thickness of 50 μm. This piezoelectric film (H-1) was used as an electrode and sandwiched between two pieces of stainless steel (SUS430) manufactured by Kyuho Metal Works, and pressed at 150°C and 2 MPa for 1 hour to obtain a piezoelectric element (M-1) equipped with the piezoelectric film (H-1).

[0051] <Preparation of Piezoelectric Resin Composition (F), Piezoelectric Film (H), and Piezoelectric Element (M)> (Examples 11 to 30, Comparative Examples 6 to 8) Except for changing the inorganic piezoelectric material (A), easily deformable aggregate (C), binder resin (D) and their blending amounts to those shown in Table 2, piezoelectric resin compositions (F-2) to (F-24), piezoelectric films (H-2) to (H-24), and piezoelectric elements (M-2) to (M-24) were prepared in the same manner as piezoelectric resin composition (F-1), piezoelectric film (H-1), and piezoelectric element (M-1).

[0052] <Evaluation of piezoelectric resin composition, piezoelectric film, and piezoelectric element> <Calculation of volume percentage of each component contained in piezoelectric resin composition (F)> The theoretical density of the easily deformable aggregate (C) present in the piezoelectric resin composition (F-1) is (Dry volume of easily deformable aggregate (C-1) / Sum of dry volumes of each component of piezoelectric resin composition (F-1)) = (Mass of easily deformable aggregate (C-1) / Density of easily deformable aggregate (C-1)) / [(mass of easily deformable aggregate (C-1) / density of easily deformable aggregate (C-1)) + (Mass of inorganic piezoelectric material (A) / Density of inorganic piezoelectric material (A)) + (mass of binder resin (D) / density of binder resin (D))] =(100 / 5.93) / (100 / 5.93+5 / 6.02+16 / 1.01) =50%. The other components and examples can be calculated in a similar manner.

[0053] <Film thickness> The film thickness at the four corners and the center of the piezoelectric film (H) from which the release treatment sheet had been peeled off was measured using a Nikon Corporation "DIGIMICROSTANDMS-5C," and the average was taken as the film thickness.

[0054] <Evaluation of piezoelectric performance> The piezoelectric element (M) was heated to 100° C. in an oil bath and a voltage of 200 V was applied to it for 1 hour using a DC power supply, thereby carrying out a polarization treatment. After polarization, the piezoelectric element (M) was given an AC current with an amplitude of 10 V and a frequency of 42 kHz using a multifunction generator WF1943 (NF Corporation), causing ultrasonic waves to oscillate. An airborne ultrasonic sensor MA40S4R (Murata Manufacturing Co., Ltd.) was fixed 1 cm away from the piezoelectric element (M) to observe the ultrasonic waves. The ultrasonic sensor was connected to an oscilloscope DPO3052 (Tektronix), and the piezoelectric performance was confirmed from the frequency and amplitude of the observed signal. Evaluation criteria ◎: Observed amplitude is 25mV or more (excellent) ○: Observed amplitude is 20mV or more but less than 25mV (good) △: The observed amplitude is between 10mV and 20mV (no problem in practical use) ×: Observed amplitude is less than 10mV (not practical)

[0055] <Flexibility assessment> A bending test was conducted to evaluate the flexibility of the piezoelectric film (H). The bending test was conducted using a 20 mm diameter mandrel in a bending resistance tester (Coating Tester, cylindrical mandrel method). The piezoelectric film (H) was set in the device and folded 5 times at a rate of 1 folding per 10 seconds. The flexibility was evaluated from the properties of the piezoelectric film (H) after folding. Evaluation criteria ◎: No change (excellent) ○: Cracks occurred, but no chipping occurred (good) ×: Chips occurred and the film could not be maintained (not practical)

[0056] <Creating the piezoelectric laminate (J)> (Examples 31 to 34) Except for changing the inorganic piezoelectric material (A), easily deformable aggregate (C), binder resin (D) and their blending amounts to those shown in Table 3, the first piezoelectric films (L-25) to (L-26) and the second piezoelectric films (K-27) to (K-28) were prepared in the same manner as the piezoelectric resin composition (F-1) and the piezoelectric film (H-1).

[0057] (Example 35) One piece measuring 1 cm x 1 cm was cut out from the first piezoelectric film (L-25), and two pieces measuring 1 cm x 1 cm were cut out from the second piezoelectric film (K-27). The side opposite the release sheet of the second piezoelectric film (K-27) was placed against the side opposite the release sheet of the first piezoelectric film (L-25), and they were laminated together using a roll laminator. Next, the release sheet on the first piezoelectric film (L-25) side was peeled off, and the side opposite the release sheet of the other second piezoelectric film (K-27) was similarly laminated to the exposed surface of the piezoelectric film (H-25), to obtain a piezoelectric laminate (J-28) with both sides covered with release sheets. The laminate of piezoelectric films, with the release sheets removed from both sides, was sandwiched between two sheets of stainless steel (SUS430) manufactured by Kyuho Metal Works as electrodes, and pressed at 150°C and 2 MPa for 1 hour to obtain a piezoelectric element (M-28).

[0058] (Examples 36 to 38) Except for changing the first piezoelectric film (L) and the second piezoelectric film (K) used to those shown in Table 4, piezoelectric laminates (J-29) to (J-31) and piezoelectric elements (M-29) to (M-31) were produced in the same manner as the piezoelectric laminate (J-28) and the piezoelectric element (M-28).

[0059] From the results in Tables 1 to 4, it was confirmed that by using the easily deformable aggregate (C) of the present invention, a piezoelectric film and a piezoelectric element that have both flexibility and piezoelectric performance can be produced.

[0060] [Table 1]

[0061] BaTiO3(1): BAF15PB (manufactured by Kojundo Chemical Laboratory Co., Ltd., average primary particle diameter 1 μm) BaTiO3(2): BT-50nm (Nippon Chemical Industry Co., Ltd., average primary particle size 50nm) BaTiO3(3): BTE-UP (Nihon Kagaku Kogyo Co., Ltd., average primary particle size 14μm) KNN: Potassium sodium niobium powder (Kyoritsu Material Co., Ltd., average primary particle diameter 1 μm) PVA: Gohsenol NL-05 (manufactured by Mitsubishi Chemical Corporation) PVP: K-85W (manufactured by Nippon Shokubai Co., Ltd.) PEI: Epomin SP-200 (manufactured by Nippon Shokubai Co., Ltd.)

[0062] [Table 2]

[0063] Epoxy resin: jER1256 (Mitsubishi Chemical Corporation) Cellulose ester: CAB-551-0.2 (manufactured by EASTMAN CHEMICAL)

[0064] [Table 3]

[0065] [Table 4]

Claims

1. The easily deformable aggregate (C) comprises 100 parts by weight of an inorganic piezoelectric material (A) having an average primary particle size of 0.3 to 5 μm, and 0.1 to 30 parts by weight of an organic binder (B) which is at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, and polyethyleneimine, and is characterized in that the aggregate (C) has an average particle size of 5 to 100 μm and an average compressive force required for a compressive deformation rate of 10% is 0.6 mN or more and 5 mN or less.

2. A piezoelectric resin composition (F), comprising 20 to 90 volume % of the easily deformable aggregate (C) according to claim 1 and 10 to 80 volume % of a binder resin (D) which is at least one selected from the group consisting of polyvinyl alcohol, an epoxy resin, and a cellulose ester.

3. A piezoelectric film (H) obtained by applying the piezoelectric resin composition (F) according to claim 2 onto a substrate.

4. 4. The piezoelectric film (H) according to claim 3, wherein t is a thickness of the piezoelectric film (H) and DB is an average particle diameter of the easily deformable aggregate (C), and t / DB is 1 / 1 to 2.5 / 1.

5. A piezoelectric laminate (J) formed by stacking two or more types of piezoelectric films, comprising a first piezoelectric film (L) containing the easily deformable aggregate (C) described in claim 1, and a second piezoelectric film (K) containing an inorganic piezoelectric material (A) and a binder resin (D) but not containing the easily deformable aggregate (C), wherein the first piezoelectric film (L) is stacked so as not to be located as the outermost layer of the piezoelectric laminate (J).

6. A piezoelectric element (M) comprising the piezoelectric film (H) according to claim 3 or 4, or the piezoelectric laminate (J) according to claim 5.

Citation Information

Patent Citations

  • Piezoelectric body device and its manufacturing method

    JP1998335713A

  • Method of manufacturing laminated type piezoelectric element

    JP2010245321A

  • Piezoelectric ceramic, method for manufacturing the same, piezoelectric element, liquid discharge head, and ultrasonic motor

    JP2011132121A

  • Piezoelectric sensor

    JP2017028323A

  • Piezoelectric element, method of manufacturing piezoelectric element, piezoelectric actuator and electronic apparatus

    JP2017108125A