Resin composition, resin sheet, cured film, method for producing cured film, semiconductor device, organic electroluminescence display device, and display device

A resin composition with polyimide, polybenzoxazole, and phenolic resin components addresses issues of pattern integrity and stripper resistance, enhancing reliability in semiconductor and display devices under varying environmental conditions.

JP7589547B2Active Publication Date: 2024-11-26TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020560423
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-29
Filing Date
2020-10-23
Publication Date
2024-11-26
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Conventional resin compositions used in semiconductor and display device applications have poor resistance to pattern shapes after low-temperature curing, are susceptible to strippers during wiring formation, and fail to withstand constant temperature and humidity tests.

Method used

A resin composition comprising polyimide, polybenzoxazole, or their precursors, combined with a phenolic resin and a thermal crosslinking agent, featuring specific structural units and ratios, which enhances resistance to strippers and maintains pattern integrity under heat and humidity.

Benefits of technology

The composition provides excellent resistance to strippers, maintains pattern shape after low-temperature curing, and withstands constant temperature and humidity tests, ensuring reliable performance in semiconductor and display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589547000046
    Figure 0007589547000046
  • Figure 0007589547000047
    Figure 0007589547000047
  • Figure 0007589547000048
    Figure 0007589547000048
Patent Text Reader

Abstract

Provided is a resin composition that can impart resistance to strippers for removing photoresist used during wiring formation and resistance to a temperature and humidity controlled test (HAST), and that excels in a pattern shape of the cured film after heat treatment when having the photosensitivity. The resin composition includes (A) one or more resins selected from the group consisting of a polyimide, a polybenzoxazole, a polyimide precursor, a polybenzoxazole precursor, and copolymers thereof, (B) a phenol resin, and (C) a thermal crosslinking agent, wherein the phenol resin (B) has a structural unit represented by a specific general formula (4), the structural unit represented by a general formula (4) has structural units represented by a specific general formula (5) and a specific general formula (6), and where the number of all structural units represented by the general formula (4) in the phenol resin (B) is 100, the ratio of the number of structural units represented by the general formula (5) and the general formula (6) is the general formula (5) : the general formula (6) = 60 : 40 to 90 : 10.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition used for a surface protective film or interlayer insulating film of a semiconductor element, an insulating layer of a display device such as an organic light-emitting element, or a planarizing film of a thin film transistor (hereinafter sometimes referred to as TFT) substrate. [Background technology]

[0002] Polyimide resins and polybenzoxazole resins, which have excellent heat resistance, electrical insulation properties, mechanical properties, etc., have been widely used in the past for surface protection films and interlayer insulating films of semiconductor elements, insulating layers of displays such as organic light-emitting elements, and planarizing films for thin film transistor (hereinafter sometimes referred to as TFT) substrates.

[0003] In recent years, in addition to the above-mentioned characteristics, polyimide resins and polybenzoxazole resins are required to have high sensitivity to g-line (436 nm), h-line (405 nm), i-line (365 nm), etc., which are used as exposure light sources, in order to improve productivity.

[0004] To date, methods for increasing sensitivity have been proposed, such as the inclusion of 101 parts by mass or more of novolac resin and / or polyhydroxystyrene resin per 100 parts by mass of polyimide precursor or polybenzoxazole precursor (see Patent Document 1), and the inclusion of a phenolic resin with a specific structure per 100 parts by mass of polyimide precursor or polybenzoxazole precursor (see Patent Documents 2 and 3).

[0005] In addition, in order to achieve high sensitivity and to satisfy the heat resistance required in the semiconductor manufacturing process, polybenzoxazole, polybenzoxazole precursor, polyimide, and polyimide precursor containing a phenolic resin with a specific structure (see Patent Document 4) have been proposed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-352004 A [Patent Document 2] JP 2018-22171 A [Patent Document 3] JP 2018-55124 A [Patent Document 4] International Publication No. 2014 / 069091 Summary of the Invention [Problem to be solved by the invention]

[0007] However, although the compositions described in the above documents have improved sensitivity to the exposure wavelength, there are problems with the pattern shape after curing at low temperatures, resistance to strippers used to remove photoresists used in wiring formation, and resistance to constant temperature and humidity testing (HAST). [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration. [1] A resin composition comprising: (A) one or more resins selected from the group consisting of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, and copolymers thereof; (B) a phenolic resin; and (C) a thermal crosslinking agent, wherein the (B) phenolic resin has a structural unit represented by general formula (4), and the structural unit represented by general formula (4) has structural units represented by general formulas (5) and (6), and when the number of all structural units represented by general formula (4) in the (B) phenolic resin is taken as 100, the ratio of the number of structural units represented by general formulas (5) and (6) is general formula (5):general formula (6)=60:40 to 90:10.

[0009] [ka]

[0010] In general formula (4), R 25 , R 27R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 , R 27 When there are multiple R, they may be the same or different. 26 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. j1 and j2 each independently represent an integer of 0 to 3.

[0011] [ka]

[0012] In general formula (5), R 25 R represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are multiple R, they may be the same or different. 26 R represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3; j3 represents an integer of 1 to 3.

[0013] [ka]

[0014] In general formula (6), R 25 R represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are multiple R, they may be the same or different. 26 R represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3. [2] A resin sheet formed on a substrate using the above resin composition. [3] A cured film obtained by curing the above-mentioned resin composition or the above-mentioned resin sheet. [4] A method for producing a cured film, comprising the steps of applying the above-mentioned resin composition to a substrate or laminating the above-mentioned resin sheet to a substrate, and then drying to form a resin film, exposing the dried resin film to light, developing the exposed resin film, and heat treating the developed resin film. [5] A semiconductor device having the above cured film. [6] An organic electroluminescence display device having at least a TFT substrate, a planarization layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode, wherein the planarization layer or the insulating layer contains the cured film described above. [7] A display device having at least metal wiring, the above-mentioned cured film, and a plurality of light-emitting elements, wherein the light-emitting elements have a pair of electrode terminals on either one surface, the pair of electrode terminals are connected to a plurality of the metal wirings extending into the cured film, and the plurality of the metal wirings maintain electrical insulation due to the cured film. A display device. Effect of the Invention

[0015] The resin composition of the present invention has resistance to a stripper used to remove a photoresist used in wiring formation, even when subjected to low-temperature heat treatment, and resistance to a constant temperature and humidity test (HAST). Furthermore, when the resin composition has photosensitivity, the cured film has an excellent pattern shape after heat treatment. [Brief description of the drawings]

[0016] [Figure 1] 1 is a front cross-sectional view showing one embodiment of a display device of the present invention. [Diagram 2] FIG. 2 is a front cross-sectional view showing one embodiment of a display device of the present invention in which a partition wall is provided. [Diagram 3] FIG. 2 is a front cross-sectional view of an opening pattern in a cured film. [Figure 4] FIG. 2 is a front cross-sectional view showing another embodiment of the display device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The resin composition of the present invention is a resin composition comprising (A) one or more resins selected from the group consisting of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, and copolymers thereof, (B) a phenolic resin, and (C) a thermal crosslinking agent, wherein the (B) phenolic resin has a structural unit represented by general formula (4), and the structural unit represented by general formula (4) has structural units represented by general formulas (5) and (6), and when the number of all structural units represented by general formula (4) in the (B) phenolic resin is taken as 100, the ratio of the number of structural units represented by general formulas (5) and (6) is general formula (5):general formula (6)=60:40 to 90:10.

[0018] [ka]

[0019] In general formula (4), R 25 , R 27 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 , R 27 When there are multiple R, they may be the same or different. 26 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. j1 and j2 each independently represent an integer of 0 to 3.

[0020] [ka]

[0021] In general formula (5), R 25 R represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are multiple R, they may be the same or different. 26 R represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3; j3 represents an integer of 1 to 3.

[0022] [ka]

[0023] In general formula (6), R 25 R represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are multiple R, they may be the same or different. 26 R represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3.

[0024] The (A) one or more resins selected from the group consisting of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, and copolymers thereof contained in the resin composition of the present invention will be described.

[0025] <(A) One or more resins selected from the group consisting of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, and copolymers thereof> (A) One or more resins selected from the group consisting of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, and copolymers thereof may hereinafter be referred to as component (A).

[0026] The polyimide is not particularly limited as long as it has an imide ring. The polyimide precursor is not particularly limited as long as it has a structure that becomes a polyimide having an imide ring by dehydration ring closure, and can contain polyamic acid, polyamic acid ester, etc. The polybenzoxazole is not particularly limited as long as it has an oxazole ring. The polybenzoxazole precursor is not particularly limited as long as it has a structure that becomes a polybenzoxazole having a benzoxazole ring by dehydration ring closure, and can contain polyhydroxyamide, etc.

[0027] The polyimide has a structural unit represented by general formula (1), the polyimide precursor and the polybenzoxazole precursor have a structural unit represented by the following general formula (2), and the polybenzoxazole has a structural unit represented by general formula (15). Two or more of these may be contained, or a resin in which the structural unit represented by general formula (1), the structural unit represented by general formula (2), and the structural unit represented by general formula (15) are copolymerized may be contained.

[0028] [ka]

[0029] In the general formula (1), V represents a 4-10 valent organic group having 4 to 40 carbon atoms, W represents a 2-8 valent organic group having 4 to 40 carbon atoms, a and b each represent an integer of 0 to 6. 1 and R 2 represents a group selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfonic acid group, and a thiol group, and a plurality of R 1 and R 2 may be the same or different.

[0030] [ka]

[0031] In the general formula (2), X and Y each independently represent a divalent to octavalent organic group having 4 to 40 carbon atoms.3 and R 4 each independently represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, c and d each represent an integer of 0 to 4, and e and f each represent an integer of 0 to 2.

[0032] [ka]

[0033] In formula (15), T and U each independently represent a divalent to octavalent organic group having 4 to 40 carbon atoms.

[0034] Specific examples of the (A) component include polyimide, polyimide precursor, polybenzoxazole precursor, and copolymers thereof. These resins may be contained alone or in combination. These resins have high heat resistance and have a small amount of outgassing under temperature conditions of 160°C or higher after heat treatment, so they are particularly suitable for use as planarizing films, insulating layers, partitions, protective films, and interlayer insulating films used in organic light-emitting devices, display devices, and semiconductor elements.

[0035] In addition, the component (A) is not particularly limited, but is preferably an alkali-soluble resin from the viewpoint of reducing the environmental load. The alkali solubility in the present invention will be explained. A solution in which a resin is dissolved in γ-butyrolactone is applied onto a silicon wafer, and the solution is prebaked at 120° C. for 4 minutes to form a prebaked film having a thickness of 10 μm±0.5 μm. Next, the prebaked film is immersed in a 2.38 mass % tetramethylammonium hydroxide aqueous solution at 23±1° C. for 1 minute, and then rinsed with pure water to determine the reduction in film thickness. A resin whose dissolution rate in the prebaked film is 50 nm / min or more is defined as being alkali-soluble.

[0036] In order to impart alkali solubility to component (A), it is preferable that a+b>0 in general formula (1). It is also preferable that c+d+e+f>0 in general formula (2). In the case of a polyimide precursor, it is preferable that X and Y in general formula (2) have aromatic groups. It is further preferable that X in general formula (2) has an aromatic group, e>0, has a carboxy group or a carboxy ester group at the ortho position of the aromatic amide group, and has a structure that forms an imide ring by dehydration ring closure.

[0037] In the case of a polybenzoxazole precursor in general formula (2), it is more preferable that X in general formula (2) has an aromatic group, d>0, has a hydroxyl group at the ortho position of the aromatic amide group, and has a structure that forms a benzoxazole ring by dehydration ring closure.

[0038] In the component (A), the repeat number n of the structural unit represented by general formula (1) or (2) is preferably 5 to 100,000, and more preferably 10 to 100,000.

[0039] In addition, the (A) component may have other structural units in addition to the structural units represented by general formula (1) or (2). Examples of the other structural units include, but are not limited to, cardo structures and siloxane structures. In this case, it is preferable that the structural units represented by general formula (1), (2), or (15) are the main structural units. Here, the main structural units refer to structural units represented by general formula (1), (2), or (15) that account for 50 mol% or more of the total number of structural units, and more preferably 70 mol% or more.

[0040] <Residue of the acid of component (A)> In the above general formula (1), V-(R 1 ) a In the above general formula (2), (OH) c -X-(COOR 3 ) eIn the above general formula (15), T represents an acid residue. V represents a tetravalent to decavalent organic group having 4 to 40 carbon atoms, and preferably an organic group having 4 to 40 carbon atoms containing an aromatic ring or a cyclic aliphatic group. X and T represent a divalent to octavalent organic group having 4 to 40 carbon atoms, and preferably an organic group having 4 to 40 carbon atoms containing an aromatic ring or an aliphatic group.

[0041] Examples of the acid components constituting the acid residue include dicarboxylic acids such as terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, triphenyl dicarboxylic acid, suberic acid, dodecafluorosuberic acid, azelaic acid, sebacic acid, hexadecafluorosebacic acid, 1,9-nonanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, and octadecane diacid. Examples of tricarboxylic acids include trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, and biphenyl tricarboxylic acid. Examples of tetracarboxylic acids include pyromellitic acid, 3,3',4,4'-biphenyl tetracarboxylic acid, and 2,3,3',4'-biphenyl tetracarboxylic acid. tetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-diphenylethertetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)propane, 2,2-bis(2,3-dicarboxyphenyl)propane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, bis(3,4-dicarboxyphenyl) 1,2,5,6-naphthalenetetracarboxylic acid, 9,9-bis(3,4-dicarboxyphenyl)fluorene, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 2,2-bis(3,Examples of the tetracarboxylic acid include, but are not limited to, 4-dicarboxyphenyl)hexafluoropropane and aromatic tetracarboxylic acids having the structures shown below, butane tetracarboxylic acid, cyclobutane tetracarboxylic acid, and 1,2,3,4-cyclopentane tetracarboxylic acid. Two or more of these may be used.

[0042] [ka]

[0043] In the formula, R 17 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 18 and R 19 represents a hydrogen atom or a hydroxyl group.

[0044] These acids can be used as they are, or as the acid anhydrides, halides, or active esters.

[0045] <Residue of diamine of component (A)> W-(R 2 ) b (OH) in the above general formula (2) d -Y-(COOR 4 ) f In the above general formula (15), U represents a diamine residue. W, Y, and U each represent a divalent to octavalent organic group having 4 to 40 carbon atoms, and among these, an organic group having 4 to 40 carbon atoms and containing an aromatic ring or a cyclic aliphatic group is preferred.

[0046] Specific examples of diamines constituting the diamine residue include 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 1,4-bis(4-aminophenoxy)benzene, and 2,2'-dimethyl-4,4'-diaminobiphenyl. , 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-di(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, or compounds in which at least a portion of the hydrogen atoms in these aromatic rings are substituted with alkyl groups or halogen atoms, aliphatic diamines, and diamines having the structures shown below. Two or more of these may be used.

[0047] [ka]

[0048] In the formula, R 20 R represents an oxygen atom, C(CF3)2, or C(CH3)2. 21 ~R 24 each independently represents a hydrogen atom or a hydroxyl group.

[0049] These diamines can be used as they are, or as diisocyanate compounds or trimethylsilylated diamines obtained by reacting the diamines with phosgene.

[0050] In addition, the component (A) preferably contains a group selected from an alkylene group and an alkylene ether group. These groups may contain an aliphatic ring. As the group selected from the alkylene group and the alkylene ether group, a group represented by general formula (3) is particularly preferred.

[0051] [ka]

[0052] In general formula (3), R 5 ~R 8 R each independently represents an alkylene group having 1 to 6 carbon atoms. 9 ~R 16 each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 6 carbon atoms. However, the structures represented in the parentheses are different. g, h, and i each independently represent an integer of 0 to 35, and g+h+i>0.

[0053] Examples of the group represented by formula (3) include an ethylene oxide group, a propylene oxide group, and a butylene oxide group, and the group may be linear, branched, or cyclic.

[0054] By containing a group selected from an alkylene group and an alkylene ether group, component (A) promotes imide ring-closing and benzoxazole ring-closing reactions even at low-temperature heat treatment, improving chemical resistance. In addition, alkylene groups and alkylene ether groups can obtain interactions such as coordinate bonds with metals, resulting in high adhesion to the substrate metal. Furthermore, by introducing alkylene groups and alkylene ether groups, polarity can be reduced, improving resistance to constant temperature and humidity testing (HAST).

[0055] The component (A) preferably contains a group selected from the alkylene group and the alkylene ether group in W in the general formula (1) or Y in the general formula (2), which can provide high chemical resistance by promoting ring closure in a cured film of the resin composition during low-temperature heat treatment, high adhesion to the substrate metal, and resistance to a constant temperature and humidity test (HAST).

[0056] Specific examples of diamines containing a group selected from an alkylene group and an alkylene ether group include ethylenediamine, 1,3-diaminopropane, 2-methyl-1,3-propanediamine, 1,4-diaminobutane, 1,5-diaminopentane, 2-methyl-1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 1,2-bis(aminomethyl)cyclohexane, 1,3 1,4-bis(aminomethyl)cyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), KH-511, ED-600, ED-900, ED-2003, EDR-148, EDR-176, D-200, D-400, D-2000, THF-100, THF-140, THF-170, RE-600, RE-900, RE-2000, RP-405, RP-409, RP-2005, RP-2009, RT-1000, HE-1000, HT-1100, HT-1700 (all trade names, manufactured by HUNTSMAN Co., Ltd.).

[0057] Furthermore, these diamines may contain bonds such as -S-, -SO-, -SO2-, -NH-, -NCH3-, -N(CH2CH3)-, -N(CH2CH2CH3)-, -N(CH(CH3)2)-, -COO-, -CONH-, -OCONH-, and -NHCONH-.

[0058] The diamine residue containing a group selected from an alkylene group and an alkylene ether group is preferably contained in an amount of 5 mol % or more, more preferably 10 mol % or more, of the total diamine residues. Also, the amount of the diamine residue is preferably 40 mol % or less, more preferably 30 mol % or less, of the total diamine residues. By containing the diamine residue in the above range, it is possible to improve the developability in an alkaline developer, and obtain high chemical resistance by promoting ring closure in a low-temperature heat treatment, high adhesion to the substrate metal, and resistance to a constant temperature and humidity test (HAST).

[0059] In addition, a diamine residue having an aliphatic polysiloxane structure may be copolymerized within a range that does not decrease heat resistance. By copolymerizing a diamine residue having an aliphatic polysiloxane structure, adhesion to a substrate can be improved. Specifically, as the diamine component, bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, etc., copolymerized at 1 to 15 mol % of the total diamine residues, etc., can be mentioned. Copolymerization within this range is preferable in terms of improving adhesion to a substrate such as a silicon wafer and not decreasing solubility in an alkaline solution.

[0060] In addition, a resin having an acidic group at the main chain end can be obtained by capping the terminals of the (A) component with a monoamine, acid anhydride, acid chloride, or monocarboxylic acid having an acidic group. Known monoamines, acid anhydrides, acid chlorides, and monocarboxylic acids having an acidic group may be used, or multiple monoamines, acid anhydrides, acid chlorides, and monocarboxylic acids may be used.

[0061] The content of the end-capping agent such as the monoamine, acid anhydride, acid chloride or monocarboxylic acid is preferably 2 to 25 mol % relative to 100 mol % of the total of the acid component and the amine component constituting the component (A).

[0062] The (A) component preferably has a weight average molecular weight of 10,000 or more and 100,000 or less. If the weight average molecular weight is 10,000 or more, the mechanical properties of the cured film after curing can be improved. More preferably, the weight average molecular weight is 20,000 or more. On the other hand, if the weight average molecular weight is 100,000 or less, the developability with various developers can be improved, and if the weight average molecular weight is 50,000 or less, the developability with an alkaline solution can be improved, which is preferable.

[0063] The weight average molecular weight (Mw) can be confirmed using gel permeation chromatography (GPC). For example, it can be measured using N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) as the developing solvent and calculated in terms of polystyrene.

[0064] The content of component (A) is preferably 3 to 55% by mass, and more preferably 5 to 40% by mass, based on 100% by mass of all components including the solvent. By keeping the content within this range, it is possible to obtain a viscosity suitable for spin coating or slit coating.

[0065] <Preparation of component (A)> The component (A) can be prepared by a known method.

[0066] In the case of a polyimide precursor, such as a polyamic acid or a polyamic acid ester, the first method is to react a tetracarboxylic dianhydride with a diamine compound at low temperature. The second method is to obtain a diester from a tetracarboxylic dianhydride and an alcohol, which is then reacted with an amine in the presence of a condensing agent. The third method is to obtain a diester from a tetracarboxylic dianhydride and an alcohol, which is then converted into an acid chloride of the remaining dicarboxylic acid, which is then reacted with an amine.

[0067] In the case of a polybenzoxazole precursor, such as polyhydroxyamide, it can be produced by a condensation reaction between a bisaminophenol compound and a dicarboxylic acid. Specifically, there is a method of reacting a dehydration condensation agent such as dicyclohexylcarbodiimide (DCC) with an acid and adding a bisaminophenol compound thereto, or a method of dropping a solution of a dicarboxylic acid dichloride into a solution of a bisaminophenol compound to which a tertiary amine such as pyridine has been added.

[0068] In the case of polyimide, for example, the polyimide precursor obtained by the above-mentioned method can be dehydrated and ring-closed by heating or chemical treatment with an acid or base to obtain the polyimide.

[0069] The resin composition of the present invention may contain other alkali-soluble resins in addition to the component (A). Specific examples of the other alkali-soluble resins include siloxane polymers, cyclic olefin polymers, and cardo resins. These resins may be used alone or in combination. In this case, it is preferable that the content of the other alkali-soluble resins is 1 to 50 parts by mass when the total of the component (A) and the other alkali-soluble resins is 100 parts by mass.

[0070] <(B) Phenolic resin> <Phenol resin containing a structural unit represented by general formula (4)> The resin composition of the present invention contains a (B) phenolic resin (hereinafter, may be referred to as component (B)), and the (B) phenolic resin has a structural unit represented by general formula (4).

[0071] [ka]

[0072] In general formula (4), R 25 , R 27 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 , R 27When there are multiple R, they may be the same or different. 26 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. j1 and j2 each independently represent an integer of 0 to 3.

[0073] As shown in the above general formula (4), by using a phenolic resin obtained from a phenolic compound and an aromatic aldehyde compound and / or an aromatic ketone compound, it is possible to provide excellent heat resistance and resistance to a stripper for removing a photoresist used in forming wiring. In addition, when the resin has photosensitivity, the contrast difference between the exposed and unexposed areas during development is large, and the glass transition temperature of the resin film is appropriately increased, so that the resin film after development and the cured film after heat treatment have excellent pattern shape with high taper.

[0074] Furthermore, the structural unit represented by the general formula (4) has structural units represented by the general formulas (5) and (6), and when the number of all structural units represented by the general formula (4) in the (B) phenol resin is taken as 100, the ratio of the number of structural units represented by the general formula (5) to the number of structural units represented by the general formula (6) is general formula (5):general formula (6)=60:40 to 90:10.

[0075] [ka]

[0076] In general formula (5), R 25 R represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are multiple R, they may be the same or different. 26 R represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3; j3 represents an integer of 1 to 3.

[0077] [ka]

[0078] In general formula (6), R 25 R represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are multiple R, they may be the same or different. 26 R represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3.

[0079] By setting the content within the above range, appropriate developability is imparted, and even in a low-temperature heat treatment, the composition has excellent resistance to a stripper for removing a photoresist used in wiring formation, and if the composition has photosensitivity, the composition has excellent pattern shapes of a resin film after development and a cured film after heat treatment.

[0080] <Phenol compounds> Examples of the phenolic compounds include alkylphenols such as phenol; meta-cresol, para-cresol, ortho-cresol, xylenol, ethylphenol, butylphenol, octylphenol, 2,3-dimethylphenol, 2,4-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2-methyl-3-ethyl-phenol, 2-methyl-3-methoxyphenol, 2,3,4-trimethylphenol, 2,3,5-trimethylphenol, 2,3,6-trimethylphenol, and the like; examples of polyhydric phenols include bisphenol A, bisphenol F, bisphenol S, resorcin, catechol, and the like; examples of other phenols include halogenated phenols, phenylphenol, and aminophenol. Among these, the phenolic compounds represented by the following formula (7) are more preferred. These phenolic compounds may be used alone or in combination of multiple phenolic compounds.

[0081] [ka]

[0082] <Aromatic aldehyde compounds> Examples of aromatic aldehyde compounds used in the structural unit represented by general formula (5) include 4-methoxybenzaldehyde, salicylaldehyde, 3-hydroxybenzaldehyde, 4-hydroxybenzaldehyde, 3-methylsalicylaldehyde, 4-methylsalicylaldehyde, 2-hydroxy-5-methoxybenzaldehyde, 2,4-dihydroxybenzaldehyde, 2,5-dihydroxybenzaldehyde, and 2,3,4-trihydroxybenzaldehyde. Among these, aromatic aldehyde compounds represented by the following formula (8) are more preferred. These aromatic aldehyde compounds may be used alone, or multiple aromatic aldehyde compounds may be used in combination.

[0083] [ka]

[0084] Examples of the aromatic aldehyde compound used in the structural unit represented by the general formula (6) include benzaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, 2,3-dimethylbenzaldehyde, 2,4-dimethylbenzaldehyde, 2,5-dimethylbenzaldehyde, 2,6-dimethylbenzaldehyde, 3,4-dimethylbenzaldehyde, and 3,5-dimethylbenzaldehyde. Benzaldehyde, 2,3,4-trimethylbenzaldehyde, 2,3,5-trimethylbenzaldehyde, 2,3,6-trimethylbenzaldehyde, 2,4,5-trimethylbenzaldehyde, 2,4,6-trimethylbenzaldehyde, 3,4,5-trimethylbenzaldehyde, 4-ethylbenzaldehyde, 4-tert-butylbenzaldehyde, 4-isobutylbenzaldehyde, and the like. Among them, the aromatic aldehyde compound represented by the following formula (9) is more preferable. These aromatic aldehyde compounds may be used alone or in combination of a plurality of aromatic aldehyde compounds.

[0085] [ka]

[0086] <Aromatic ketone compounds> Examples of the aromatic ketone compound used in the structural unit represented by the general formula (5) include p-hydroxyacetophenone, m-hydroxyacetophenone, 3',5'-dihydroxyacetophenone, p-hydroxypropiophenone, m-hydroxypropiophenone, p-hydroxyvalerophenone, 1'-hydroxy-2'-acetonaphthone, 2'-hydroxy-1'-acetonaphthone, 2'-hydroxy-5'-methylacetophenone, 4'-hydroxy-2'-methylacetophenone, and 4'-hydroxy-3'-methylacetophenone. acetophenone, 2',4'-dihydroxy-3'-methylacetophenone, 2'-hydroxy-4',5'-dimethylacetophenone, 4'-benzoyloxy-2'-hydroxy-3'-methylacetophenone, 4'-benzyloxy-2'-methoxy-3'-methylacetophenone, 2'-hydroxy-4'-methoxyacetophenone, 2'-hydroxy-5'-methoxyacetophenone, 2'-hydroxy-6'-methoxyacetophenone, 2-(phenylsulfonyl)acetophenone, 2-hydroxy-2-methylpropiophenone, 2',4' -Dihydroxy-3'-methylpropiophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2'-hydroxy-3-phenylpropiophenone, 4'-benzyloxy-2'-hydroxy-3'-methylpropiophenone, 2',4'-dihydroxy-3'-methylbutyrophenone, o-hydroxybenzophenone, p-hydroxybenzophenone, 2,4-dihydroxybenzophenone, 2,2'-dihydroxybenzophenone, 2,4-dihydroxybenzophenone, 4,4'-dihydroxy Benzophenone, 2,3,4-trihydroxybenzophenone, 2,4,4'-trihydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 4-fluoro-4'-hydroxybenzophenone, benzyl-4-hydroxyphenyl ketone, 2-hydroxy-5-methylbenzophenone, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 5-hydroxy-1-tetralone, and the like.Among these, aromatic ketone compounds represented by the following formula (10) are more preferred. These aromatic ketone compounds may be used alone or in combination of two or more aromatic ketone compounds.

[0087] [ka]

[0088] Examples of the aromatic ketone compound used in the structural unit represented by the general formula (6) include acetophenone, propiophenone, butyrophenone, isobutyrophenone, valerophenone, hexanophenone, 2,2-dimethylpropiophenone, 2-phenylbutyrophenone, phenyl vinyl ketone, cyclohexyl phenyl ketone, p-methylacetophenone, m-methylacetophenone, o-methylacetophenone, p-ethylacetophenone, p-propylacetophenone, p-isobutylacetophenone, p-butylacetophenone, pt- Butylacetophenone, 2',4'-dimethylacetophenone, 3',4'-dimethylacetophenone, 2',4',6'-trimethylacetophenone, p-methylpropiophenone, m-methylpropiophenone, o-methylpropiophenone, p-ethylpropiophenone, m-ethylpropiophenone, o-ethylpropiophenone, pt-butylpropiophenone, 1'-acetonaphthone, 2'-acetonaphthone, 6'-methyl-2'-acetonaphthone, 4-acetylbiphenyl, t-butyl-4-phenoxyphenyl ketone, 1-(2- naphthyl)-3-phenyl-2-propen-1-one, 2-fluoroacetophenone, p-fluoroacetophenone, m-fluoroacetophenone, o-fluoroacetophenone, m-trifluoromethylacetophenone, 2-fluoropropiophenone, 3-fluoropropiophenone, p-fluoropropiophenone, m-fluoropropiophenone, o-fluoropropiophenone, p-methoxyacetophenone, m-methoxyacetophenone, o-methoxyacetophenone, 2-methoxyacetophenone, p-ethoxyacetophenone, p-Phenoxyacetophenone, 2',2'-diethoxyacetophenone, 2',4'-dimethoxyacetophenone, 2',5'-dimethoxyacetophenone, 2',6'-dimethoxyacetophenone, 3',4'-dimethoxyacetophenone, 3',5'-dimethoxyacetophenone, 3',4'-(methylenedioxy)acetophenone, 3',4'-(methylenedioxy)propiophenone, 6'-methoxy-2'-acetonaphthone, 6'-methoxy-2'-propiononaphthone, 2',4'-dimethoxy-3'-methylacetophenone, 2,2-Dimethoxy-2-phenylacetophenone, 5'-fluoro-2'-hydroxyacetophenone, 3',5'-dimethoxy-4'-hydroxyacetophenone, 2-fluoro-p-methoxyacetophenone, 2-fluoro-m-methoxyacetophenone, 2-fluoro-o-methoxyacetophenone, 2'-fluoro-4'-methoxyacetophenone, 3'-fluoro-4'-methoxyacetophenone, 2',4'-dimethoxy-3'-methylpropiophenone, benzophenone, anthraquinone, p-methylbenzophenone, m-methylbenzophenone, o-methylbenzophenone, p-ethylbenzophenone, m-ethylbenzophenone, o-ethylbenzophenone, 2,5-dimethylbenzophenone, 2,4-di Examples of the aromatic ketone compounds include methylbenzophenone, 3,4-dimethylbenzophenone, p-morpholinobenzophenone, p-phenylbenzophenone, o-fluorobenzophenone, p-fluorobenzophenone, 2,4'-difluorobenzophenone, p-methoxybenzophenone, 4,4'-dimethoxybenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4-(p-triylthio)benzophenone, 1-indanone, 2-methyl-1-indanone, 3-methyl-1-indanone, 4-methoxy-1-indanone, 5-methoxy-1-indanone, 6-methoxy-1-indanone, 4-hydroxy-1-indanone, α-tetralone, and 1-benzosuberone. Among these, aromatic ketone compounds represented by the following formula (11) are more preferred. These aromatic ketone compounds may be used alone or in combination with one another.

[0089] [ka]

[0090] In the present invention, the aromatic aldehyde compound and aromatic ketone compound may be used alone or in combination. The ratio of the phenol compound to the aromatic aldehyde compound and / or aromatic ketone compound is preferably in the range of 0.5-2.0 in molar ratio (aromatic aldehyde compound and / or aromatic ketone compound) / (phenol compound) since it is possible to obtain a novolac type phenolic resin with a sufficiently high molecular weight with less unreacted phenols, and more preferably in the range of 0.7-1.8.

[0091] In the present invention, the polycondensation reaction of component (B) is preferably carried out using an acid catalyst, such as inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, and boric acid, and organic acids such as oxalic acid, acetic acid, and p-toluenesulfonic acid.

[0092] The weight average molecular weight of component (B) is preferably from 500 to 10,000, and more preferably from 500 to 5,000. When the weight average molecular weight is within the above range, compatibility with component (A) and the like, heat resistance, appropriate developability, and photosensitivity can be achieved, resulting in an excellent pattern shape of the resin film after development and the cured film after heat treatment, and resistance to a stripper for removing the photoresist used in forming wiring.

[0093] The weight average molecular weight (Mw) can be confirmed using gel permeation chromatography (GPC). For example, it can be measured using N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) as the developing solvent and calculated in terms of polystyrene.

[0094] <Preparation of component (B)> The component (B) can be prepared by a known method, but is usually prepared by polycondensation reaction. The polycondensation reaction proceeds by stirring for several hours under heating in the presence of the acid catalyst. The reaction temperature is preferably 50°C to 140°C. The reaction can also be carried out in a solvent by adding a solvent during the reaction. Examples of reaction solvents include alcohol solvents such as methanol, ethanol, and propanol, polyol solvents such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, trimethylene glycol, diethylene glycol, polyethylene glycol, and glycerin, and glycol ether solvents such as 2-ethoxyethanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ...ethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl Examples of the solvent include, but are not limited to, ethanol monobutyl ether, ethylene glycol monopentyl ether, ethylene glycol dimethyl ether, ethylene glycol ethyl methyl ether, ethylene glycol monophenyl ether, etc., cyclic ether solvents include 1,3-dioxane, 1,4-dioxane tetrahydrofuran, dioxane, etc., glycol ester solvents include ethylene glycol acetate, diethylene glycol monomethyl ether acetate, etc., ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, etc., aromatic hydrocarbons include toluene, xylene, etc., and other solvents include γ-butyrolactone, pure water, etc. These solvents can be used alone or in combination of two or more.

[0095] The amount of the solvent added is preferably 10 parts by mass or more and 300 parts by mass or less based on 100 parts by mass of the phenol compound.

[0096] After the reaction is completed, the acid catalyst is neutralized using a base such as pyridine, triethylamine, or sodium hydroxide, and if necessary, the neutralized salt is removed by extraction into the aqueous layer, followed by dehydration and monomer removal steps for recovery.

[0097] After synthesis of the phenolic resin (B), a monomer removal step is usually performed. The monomer removal method can be selected from a solvent fractionation method in which a solvent and water are added and the aqueous layer is removed, a method in which the monomer is volatilized by heating under reduced pressure, and the like.

[0098] Alternatively, the component (B) may be prepared by a method comprising the following three steps:

[0099] <Process 1> The phenol compound and the aromatic aldehyde compound or aromatic ketone compound are heated in the presence of the acid catalyst, optionally using a solvent, at a temperature in the range of 60 to 140°C to polycondense, thereby obtaining a phenolic trinuclear compound.

[0100] <Process 2> The phenolic trinuclear compound obtained in step 1 is isolated from the reaction solution.

[0101] <Process 3> The phenolic trinuclear compound isolated in step 2 and the aromatic aldehyde compound and / or aromatic ketone compound are heated in the presence of the acid catalyst, optionally using a solvent, at a temperature in the range of 60 to 140°C to polycondense, thereby obtaining a phenolic resin.

[0102] Use of a phenolic trinuclear compound is preferred because it narrows the molecular weight distribution, and therefore has excellent resistance to strippers used to remove photoresists used in wiring formation, even with low-temperature heat treatment, and, if photosensitive, provides excellent resin film after development and excellent pattern shapes of the cured film after heat treatment.

[0103] After the reaction in steps 1 and 3 is completed, the acid catalyst is neutralized using a base such as pyridine, triethylamine, or sodium hydroxide, and if necessary, the neutralized salt is removed by extraction into the aqueous layer, followed by dehydration, monomer removal, isolation, and other steps for recovery.

[0104] The charging ratio of the phenol compound to the aromatic aldehyde compound or aromatic ketone compound in step 1 [phenol compound / (aromatic aldehyde compound or aromatic ketone compound)] is preferably in the range of 1 / 0.2 to 1 / 0.5, and more preferably in the range of 1 / 0.25 to 1 / 0.45, in terms of molar ratio, because this provides excellent removability of the unreacted phenol compound, product yield, and purity of the reaction product.

[0105] An example of a method for isolating the phenol trinuclear compound from the reaction solution in step 2 is to add the reaction solution to a poor solvent in which the reaction product is insoluble or poorly soluble, filter off the resulting precipitate, dissolve the reaction product in a solvent that dissolves the reaction product and is miscible in the poor solvent, and add the solution to the poor solvent again to filter off the resulting precipitate. Examples of the poor solvent used in this case include water, monoalcohols such as methanol, ethanol, and propanol, aliphatic hydrocarbons such as n-hexane, n-heptane, n-octane, and cyclohexane, and aromatic hydrocarbons such as toluene and xylene. Among these poor solvents, water and methanol are preferred because they can efficiently remove the acid catalyst at the same time. On the other hand, examples of the solvent include polyol solvents such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, trimethylene glycol, diethylene glycol, polyethylene glycol, and glycerin; glycol ether solvents such as 2-ethoxyethanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ... Examples of the solvents include ethylene glycol monobutyl ether, ethylene glycol monopentyl ether, ethylene glycol dimethyl ether, ethylene glycol ethyl methyl ether, and ethylene glycol monophenyl ether; cyclic ether solvents include 1,3-dioxane, 1,4-dioxane tetrahydrofuran, and dioxane; glycol ester solvents include ethylene glycol acetate and diethylene glycol monomethyl ether acetate; ketone solvents include acetone, methyl ethyl ketone, and methyl isobutyl ketone; and other solvents include γ-butyrolactone. Each of these solvents can be used alone or in combination of two or more. The isolation method of step 2 above can provide a phenol trinuclear compound.

[0106] The ratio of the phenolic trinuclear compound to the aromatic aldehyde compound and / or aromatic ketone compound in step 3 is preferably in the range of 1 / 0.5 to 1 / 1.2, more preferably 1 / 0.6 to 1 / 0.9, in terms of molar ratio (phenolic trinuclear compound) / (aromatic aldehyde compound and / or aromatic ketone compound), since excessive polymerization (gelation) can be suppressed and a compound with an appropriate molecular weight can be obtained.

[0107] Examples of the solvents used as necessary in the above steps 1 and 3 include alcohol solvents such as methanol, ethanol, and propanol; polyol solvents such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, trimethylene glycol, diethylene glycol, polyethylene glycol, and glycerin; and glycol ether solvents such as 2-ethoxyethanol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and ethylene glycol monopropyl ether. Examples of the solvent include, but are not limited to, ether, ethylene glycol monobutyl ether, ethylene glycol monopentyl ether, ethylene glycol dimethyl ether, ethylene glycol ethyl methyl ether, ethylene glycol monophenyl ether, and the like; cyclic ether solvents include 1,3-dioxane, 1,4-dioxane tetrahydrofuran, dioxane, and the like; glycol ester solvents include ethylene glycol acetate, diethylene glycol monomethyl ether acetate, and the like; ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, and the like; aromatic hydrocarbons include toluene, xylene, and the like; and other solvents include γ-butyrolactone, pure water, and the like. These solvents can be used alone or in combination of two or more. The content of the (B) component is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, per 100 parts by mass of the (A) component, from the viewpoints of excellent pattern shape of the cured film after heat treatment, resistance to a stripper for removing the photoresist used in wiring formation, etc. Also, from the viewpoints of compatibility with the (A) component, etc., the content of the (B) component is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, per 100 parts by mass of the (A) component.

[0108] <(C) Thermal crosslinking agent> The resin composition of the present invention contains (C) a thermal crosslinking agent. The thermal crosslinking agent refers to a resin or compound having at least two thermally reactive functional groups, which are thermal crosslinking groups, in the molecule.

[0109] Specific examples of the thermal crosslinking group include a cyclic ether group, an alkoxymethyl group, and a methylol group.

[0110] The (C) thermal crosslinking agent preferably contains a thermal crosslinking agent having a biphenyl structure which may have a substituent and / or a thermal crosslinking agent having a structural unit represented by general formula (14) which will be described later.

[0111] <Thermal Crosslinking Agent Having a Biphenyl Structure Which May Have a Substituent> The resin composition of the present invention preferably contains, as the (C) thermal crosslinking agent, a thermal crosslinking agent having a biphenyl structure which may have a substituent.

[0112] By having a biphenyl structure which may have a substituent, it is possible to improve the chemical resistance of the cured film against strippers, etc., and furthermore, it is possible to impart low water absorption, thereby improving the resistance against a constant temperature and humidity test (HAST), etc. Furthermore, it is possible to appropriately lower the glass transition temperature of the resin film or the cured film, thereby imparting fluidity, and therefore it is excellent in controlling the pattern shape of the resin film after development and the cured film after heat treatment.

[0113] Of the (C) thermal crosslinking agents, the thermal crosslinking agent having a biphenyl structure which may have a substituent preferably contains a structure of general formula (12) or general formula (13).

[0114] As the biphenyl structure which may have a substituent, the structures represented by the general formula (12) and the general formula (13) are preferred from the viewpoints of improving chemical resistance and improving resistance to a constant temperature and humidity test (HAST) and the like.

[0115] [ka]

[0116] In general formula (12), R 29 and R 30 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 29 , R 30 When there are multiple R, they may be the same or different. 31 , R 32 represents a thermal crosslinking group. m1 and m2 each independently represent an integer of 0 to 4, and m3 and m4 each independently represent an integer of 1 to 3, providing that 1≦m1+m3≦5 and 1≦m2+m4≦5 are satisfied.

[0117] [ka]

[0118] In general formula (13), R 33 , R 34 , R 35 and R 36 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 33 , R 34 , R 35 and R 36 When there are multiple R, they may be the same or different. 37 , R 38 , R 39 and R 40 represents a thermal crosslinking group. 41represents a monovalent organic group having 1 to 10 carbon atoms. n1, n4, n5, and n8 each independently represent an integer of 1 to 3, n2, n3, n6, and n7 each independently represent an integer of 0 to 4, n9 represents a repeating unit and is an integer of 1 to 10, and n10 represents an integer of 0 or 1.

[0119] Specific examples of the structures represented by general formula (12) and general formula (13) include, but are not limited to, the following cyclic ether group compounds, methylol compounds, and alkoxymethyl compounds in which the hydrogen atom of the methylol group is substituted with a methyl group or an alkyl group having 2 to 10 carbon atoms. Copolymers are also acceptable.

[0120] [ka]

[0121] [ka]

[0122] n9 represents a repeating unit and is an integer of 1 to 10.

[0123] In the present invention, known cyclic ether group compounds, alkoxymethyl compounds and methylol compounds may be contained as other thermal crosslinking agents.

[0124] <Thermal crosslinking agent having a structural unit represented by general formula (14)> The resin composition of the present invention preferably contains a thermal crosslinking agent having a structural unit represented by general formula (14).

[0125] [ka]

[0126] In general formula (14), R 42 is a divalent organic group having an alkylene group or an alkylene ether group having 1 to 15 carbon atoms; R 43 and R 44each independently represents a hydrogen atom or a methyl group.

[0127] Thermal crosslinking agents having a structural unit represented by general formula (14) have a flexible alkylene group and a rigid aromatic group, and therefore can improve the chemical resistance of the cured film against strippers and the like, and can impart low water absorption, thereby improving resistance to constant temperature and humidity testing (HAST), etc. Furthermore, they can appropriately lower the glass transition temperature of the resin film or cured film to impart fluidity, and therefore are excellent in controlling the pattern shape of the resin film after development and the cured film after heat treatment.

[0128] Examples of the crosslinking group contained in the thermal crosslinking agent having a structural unit represented by general formula (14) include, but are not limited to, an acrylic group, a methylol group, an alkoxymethyl group, a cyclic ether group, etc. Among these, a cyclic ether group is preferred because it can react with the hydroxyl group of component (A) to improve the heat resistance of the cured film and can react without dehydration.

[0129] Specific examples of the compound containing the structural unit represented by general formula (14) include, but are not limited to, the following structures.

[0130] [ka]

[0131] During the ceremony o 2 is an integer between 1 and 5, o 1 is 1 to 20, and from the viewpoints of chemical resistance, low water absorption, and control of pattern shape, 2 is 1~2,o 1 is preferably 3 to 7.

[0132] As the thermal crosslinking agent (C), a thermal crosslinking agent having a biphenyl structure which may have a substituent and / or a thermal crosslinking agent having a structural unit represented by general formula (14), other thermal crosslinking agents may be contained in combination of two or more kinds.

[0133] When the total amount of the (C) thermal crosslinking agent is taken as 100 mass%, the content ratio of the thermal crosslinking agent having a biphenyl structure which may have a substituent and the thermal crosslinking agent having a structural unit represented by general formula (14) is preferably 15 mass% or more and 80 mass% or less. This can improve the chemical resistance of the cured film against strippers and the like, and furthermore, can impart low water absorption, thereby improving resistance to constant temperature and humidity tests (HAST) and the like. Furthermore, since the glass transition temperature of the resin film or the cured film is appropriately lowered, the pattern shape of the cured film is excellent when it has photosensitivity.

[0134] In the resin composition of the present invention, the (C) thermal crosslinking agent contains the thermal crosslinking agent having a biphenyl structure which may have a substituent, and the content of the thermal crosslinking agent having a biphenyl structure which may have a substituent is preferably 30 parts by mass or more and 150 parts by mass or less relative to 100 parts by mass of the (B) phenolic resin.

[0135] The content of the (C) thermal crosslinking agent having a biphenyl structure which may have a substituent is preferably 30 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more, relative to 100 parts by mass of the (B) phenolic resin, from the viewpoint of improving resistance to a stripper for removing a photoresist used in wiring formation, resistance to a constant temperature and humidity test (HAST), etc., while maintaining the pattern shape, the content is preferably 150 parts by mass or less, more preferably 120 parts by mass or less, and even more preferably 100 parts by mass or less, relative to 100 parts by mass of the (B) phenolic resin, from the viewpoint of improving resistance to a stripper for removing a photoresist used in wiring formation, resistance to a constant temperature and humidity test (HAST), etc.

[0136] <(D) Photosensitive compound> The resin composition of the present invention preferably contains (D) a photosensitive compound (hereinafter, may be referred to as component (D)).

[0137] The inclusion of component (D) can impart photosensitivity to the resin composition. Component (D) is a compound whose chemical structure changes in response to ultraviolet light, and examples thereof include a photoacid generator, a photobase generator, and a photopolymerization initiator. When a photoacid generator is used as component (D), acid is generated in the light-irradiated portion of the photosensitive resin composition, and the solubility of the light-irradiated portion in an alkaline developer increases, so that a positive pattern in which the light-irradiated portion dissolves can be obtained.

[0138] When a photobase generator is used as component (D), a base is generated in the irradiated parts of the resin composition, which reduces the solubility of the irradiated parts in an alkaline developer, thereby making it possible to obtain a negative pattern in which the irradiated parts are insolubilized.

[0139] When a photopolymerization initiator is used as component (D), radicals are generated in the light-irradiated portion of the resin composition, radical polymerization proceeds, and the resin composition becomes insoluble in an alkaline developer, forming a negative pattern. In addition, UV curing during exposure is promoted, improving sensitivity.

[0140] Among the above-mentioned (D) components, photoacid generators are preferred because they provide high-resolution patterns with high sensitivity. Examples of photoacid generators include quinone diazide compounds, sulfonium salts, phosphonium salts, diazonium salts, and iodonium salts. Furthermore, sensitizers and the like can be included as necessary.

[0141] As the quinone diazide compound, a compound having a phenolic hydroxyl group and a sulfonic acid of naphthoquinone diazide bonded by ester is preferable. The compound having a phenolic hydroxyl group used here is Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, TrisP-SA, TrisOCR-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, methylenetris-FR-CR, BisRS-26 X, DML-MBPC, DML-MBOC, DML-OCHP, DML-PCHP, DML-PC, DML-PTBP, DML-34X, DML-EP, DML-POP, Dimethylol-BisOC-P, DML-PFP , DML-PSBP, DML-MTrisPC, TriML-P, TriML-35XL, TML-BP, TML-HQ, TML-pp-BPF, TML-BPA, TMOM-BP, HML-TPPHBA, HML-TP Examples of preferred compounds include HAP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.), BIR-OC, BIP-PC, BIR-PC, BIR-PTBP, BIR-PCHP, BIP-BIOC-F, 4PC, BIR-BIPC-F, TEP-BIP-A, 46DMOC, 46DMOEP, TM-BIP-A (trade name, manufactured by Asahi Organic Chemical Industry Co., Ltd.), 2,6-dimethoxymethyl-4-tert-butylphenol, 2,6-dimethoxymethyl-p-cresol, 2,6-diacetoxymethyl-p-cresol, naphthol, tetrahydroxybenzophenone, methyl gallate, bisphenol A, bisphenol E, methylene bisphenol, and BisP-AP (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) to which 4-naphthoquinone diazide sulfonic acid or 5-naphthoquinone diazide sulfonic acid has been introduced via an ester bond, but other compounds can also be used.

[0142] In addition, it is preferable that 50 mol % or more of the functional groups of the compound having a phenolic hydroxyl group are substituted with quinone diazide. By using a quinone diazide compound substituted with 50 mol % or more, the affinity of the quinone diazide compound to an alkaline aqueous solution is reduced. As a result, the solubility of the resin composition in an alkaline aqueous solution of the unexposed portion is greatly reduced. Furthermore, the quinone diazide sulfonyl group is converted to an indene carboxylic acid by exposure, and a high dissolution rate of the photosensitive resin composition in an alkaline aqueous solution of the exposed portion can be obtained. That is, as a result, the dissolution rate ratio of the exposed portion and the unexposed portion of the composition can be increased, and a pattern with high resolution can be obtained.

[0143] By containing such a quinone diazide compound, it is possible to obtain a resin composition having positive photosensitivity that is sensitive to the i-line (365 nm), h-line (405 nm), and g-line (436 nm) of a general mercury lamp, or to a broad band including these rays. Also, the (D) component may be contained alone or in combination of two or more kinds, and a highly sensitive resin composition may be obtained.

[0144] Examples of quinone diazides include a 5-naphthoquinone diazide sulfonyl group, a 4-naphthoquinone diazide sulfonyl group, and a group containing a 4-naphthoquinone diazide sulfonyl group and a 5-naphthoquinone diazide sulfonyl group in the same molecule.

[0145] The naphthoquinone diazide sulfonyl ester compound preferably contains a 5-naphthoquinone diazide sulfonyl ester compound (D-1). The absorption of the (D-1) component extends to the g-line region of a mercury lamp, making it suitable for g-line exposure and full-wavelength exposure. In addition, it forms a crosslinked structure by reacting with the (A) and (B) components during curing, improving chemical resistance.

[0146] The naphthoquinone diazide sulfonyl ester compound has a 5-naphthoquinone diazide sulfonyl ester compound (D-1) and a 4-naphthoquinone diazide sulfonyl ester compound (D-2), and the content ratio thereof is preferably (D-2) / (D-1)=0.3-3. The (D-2) component has absorption in the i-line region of a mercury lamp, and is suitable for i-line exposure. In addition, since the acid generated by exposure is a strong sulfonic acid, the alkali dissolution of the entire exposed area increases during development, and the pattern shape after development and heat treatment can be improved. Therefore, by making the content ratio (D-2) / (D-1)=0.3-3, both chemical resistance and pattern shape after heat treatment can be achieved.

[0147] The quinone diazide compound can be synthesized by a known method through an esterification reaction between a compound having a phenolic hydroxyl group and a quinone diazide sulfonic acid compound. The use of the quinone diazide compound improves the resolution, sensitivity, and film remaining rate.

[0148] The molecular weight of component (D) is preferably 300 or more, more preferably 350 or more, and is preferably 3,000 or less, more preferably 1,500 or less, from the standpoint of heat resistance, mechanical properties and adhesiveness of the film obtained by heat treatment.

[0149] Of the components (D), sulfonium salts, phosphonium salts, and diazonium salts are preferred because they appropriately stabilize the acid components generated by exposure to light, with sulfonium salts being particularly preferred.

[0150] The content of component (D) is preferably 0.1 to 100 parts by mass per 100 parts by mass of component (A). When the content of component (D) is 0.1 to 100 parts by mass, photosensitivity can be imparted while maintaining the heat resistance, chemical resistance, and mechanical properties of the film after heat treatment.

[0151] When the (D) component contains a quinone diazide compound, the content of the (D) component is more preferably 1 part by mass or more, and even more preferably 3 parts by mass or more, relative to 100 parts by mass of the (A) component. Also, it is more preferably 100 parts by mass or less, and even more preferably 80 parts by mass or less. If it is 1 part by mass or more and 100 parts by mass or less, it is possible to impart photosensitivity while maintaining the heat resistance, chemical resistance, and mechanical properties of the film after heat treatment.

[0152] When the (D) component contains a sulfonium salt, a phosphonium salt, or a diazonium salt, the content of the (D) component is more preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and particularly preferably 3 parts by mass or more, based on 100 parts by mass of the (A) component. Also, it is more preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and particularly preferably 50 parts by mass or less. If it is 0.1 parts by mass or more and 100 parts by mass or less, it is possible to impart photosensitivity while maintaining the heat resistance, chemical resistance, and mechanical properties of the film after heat treatment.

[0153] When a photobase generator is contained as the component (D), specific examples of the photobase generator include amide compounds and ammonium salts.

[0154] Examples of the amide compound include 2-nitrophenylmethyl-4-methacryloyloxypiperidine-1-carboxylate, 9-anthrylmethyl-N,N-dimethylcarbamate, 1-(anthraquinone-2yl)ethyl imidazole carboxylate, (E)-1-[3-(2-hydroxyphenyl)-2-propenoyl]piperidine, and the like.

[0155] Examples of ammonium salts include 1,2-diisopropyl-3-(bisdimethylamino)methylene)guanidinium 2-(3-benzoylphenyl)propionate, (Z)-{[bis(dimethylamino)methylidene]amino}-N-cyclohexylamino)methaniminium tetrakis(3-fluorophenyl)borate, and 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidinium n-butyltriphenylborate.

[0156] When the photobase generator is contained as the (D) component, the content of the (D) component in the resin composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.7 parts by mass or more, and particularly preferably 1 part by mass or more, relative to 100 parts by mass of the (A) component. When the content is within the above range, the sensitivity during exposure can be improved. On the other hand, the content is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 17 parts by mass or less, and particularly preferably 15 parts by mass or less. When the content is within the above range, the resolution after development can be improved.

[0157] When a photopolymerization initiator is contained as the component (D), the photopolymerization initiator is preferably, for example, a benzyl ketal-based photopolymerization initiator, an α-hydroxyketone-based photopolymerization initiator, an α-aminoketone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, an oxime ester-based photopolymerization initiator, an acridine-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an aromatic ketoester-based photopolymerization initiator or a benzoic acid ester-based photopolymerization initiator, or a titanocene-based photopolymerization initiator. From the viewpoint of improving the sensitivity during exposure, an α-hydroxyketone-based photopolymerization initiator, an α-aminoketone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, an oxime ester-based photopolymerization initiator, an acridine-based photopolymerization initiator, or a benzophenone-based photopolymerization initiator is more preferable, and an α-aminoketone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, or an oxime ester-based photopolymerization initiator is even more preferable.

[0158] Examples of the α-aminoketone photopolymerization initiator include 2-dimethylamino-2-methyl-1-phenylpropan-1-one, 2-diethylamino-2-methyl-1-phenylpropan-1-one, 2-methyl-2-morpholino-1-phenylpropan-1-one, 2-dimethylamino-2-methyl-1-(4-methylphenyl)propan-1-one, 2-dimethylamino-1-(4-ethylphenyl)-2-methylpropan-1-one, 2-dimethylamino-1-(4-isopropylphenyl)-2-methylpropan-1-one, and 1-(4-butylphenyl)-2-dimethylamino-2-methylpropan-1-one. 1-(4-methylphenyl)-2-morpholinopropan-1-one, 2-dimethylamino-1-(4-methoxyphenyl)-2-methylpropan-1-one, 2-dimethylamino-2-methyl-1-(4-methylthiophenyl)propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-benzyl-2-dimethylamino-1-(4-dimethylaminophenyl)-butan-1-one, 2-dimethylamino-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone.

[0159] Examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)phosphine oxide.

[0160] Examples of the oxime ester photopolymerization initiator include 1-phenylpropane-1,2-dione-2-(O-ethoxycarbonyl)oxime, 1-phenylbutane-1,2-dione-2-(O-methoxycarbonyl)oxime, 1,3-diphenylpropane-1,2,3-trione-2-(O-ethoxycarbonyl)oxime, 1-[4-(phenylthio)phenyl]octane-1,2-dione-2-(O-benzoyl)oxime, 1-[4-[4-(carboxyphenyl)thio]phenyl] 1-[9-ethyl-6-[2-methyl-4-[1-(2,2-dimethyl-1,3-dioxolan-4-yl)methyloxy]benzoyl]-9H-carbazol-3-yl]ethanone-1-(O-acetyl)oxime, 1-[9-ethyl-6-[2-methyl-4-[1-(2,2-dimethyl-1,3-dioxolan-4-yl)methyloxy]benzoyl]-9H-carbazol-3-yl]ethanone-1-(O-acetyl)oxime or “ADEKA ARCLES”® NCI-831.

[0161] When the photopolymerization initiator is contained as the (D) component, the content of the (D) component in the resin composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.7 parts by mass or more, and particularly preferably 1 part by mass or more, relative to 100 parts by mass of the (A) component. When the content is within the above range, the sensitivity during exposure can be improved. On the other hand, the content is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 17 parts by mass or less, and particularly preferably 15 parts by mass or less. When the content is within the above range, the resolution after development can be improved.

[0162] <Other> The resin composition of the present invention may contain, as necessary, other components such as a radical polymerizable compound, an antioxidant, a solvent, a compound having a phenolic hydroxyl group, an adhesion improver, an adhesion promoter, and a surfactant.

[0163] <Method of producing resin composition> Next, the method for producing the resin composition of the present invention will be described. For example, the resin composition can be obtained by mixing and dissolving each of the components (A), (B), and (C) and, if necessary, the component (D), a radical polymerizable compound, an antioxidant, a solvent, a compound having a phenolic hydroxyl group, an adhesion improver, an adhesion improver, a surfactant, etc.

[0164] The dissolution method may be a known method such as heating or stirring.

[0165] The viscosity of the resin composition is preferably 2 to 5,000 mPa·s. By adjusting the solid content concentration so that the viscosity is 2 mPa·s or more, it is easy to obtain a desired film thickness. On the other hand, if the viscosity is 5,000 mPa·s or less, it is easy to obtain a highly uniform coating film. A resin composition having such a viscosity can be easily obtained, for example, by setting the solid content concentration to 5 to 60 mass%. Here, the solid content concentration refers to the components other than the solvent.

[0166] The obtained resin composition is preferably filtered using a filter to remove dust and particles. The filter material may be polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc., with polyethylene and nylon being preferred.

[0167] <Resin sheet> The resin sheet of the present invention is a resin sheet formed on a substrate using the above-mentioned resin composition. Specifically, it refers to a sheet obtained by applying the resin composition to a substrate and drying it.

[0168] A film such as polyethylene terephthalate (PET) can be used as the substrate to which the resin composition is applied. When the resin sheet is used by laminating it to a substrate such as a silicon wafer, if it is necessary to peel and remove the substrate, it is preferable to use a substrate whose surface is coated with a release agent such as silicone resin, since this allows the resin sheet to be easily peeled from the substrate.

[0169] <Method of manufacturing the cured film> Next, the cured film of the present invention obtained by curing the resin composition of the present invention or the resin sheet of the present invention, and the method for producing the same will be described.

[0170] Hereinafter, the term "resin film" refers to a film obtained by applying the resin composition of the present invention to a substrate and drying it, and the term "cured film" refers to a resin film or a film obtained by curing a resin sheet.

[0171] The method for producing a cured film of the present invention preferably includes a step of applying the resin composition to a substrate or laminating a resin sheet to a substrate, and then drying to form a resin film, an exposure step of exposing the dried resin film to light, a development step of developing the exposed resin film, and a heat treatment step of heat treating the developed resin film.

[0172] First, the resin composition of the present invention is applied to a substrate to obtain a coating film of the resin composition. The substrate may be, but is not limited to, a silicon wafer, ceramics, gallium arsenide, an organic circuit board, an inorganic circuit board, or a substrate on which a circuit component is arranged. Coating methods include spin coating, slit coating, dip coating, spray coating, and printing. The coating thickness varies depending on the coating method, the solid content concentration of the composition, and the viscosity, but is usually applied so that the coating thickness after drying is 0.1 to 150 μm.

[0173] Prior to coating, the substrate to which the resin composition is to be applied may be pretreated with the adhesion improver described above. For example, the substrate surface may be treated by spin coating, slit die coating, bar coating, dip coating, spray coating, steam treatment, or the like using a solution in which the adhesion improver is dissolved in a solvent such as isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, or diethyl adipate at 0.5 to 20% by mass. After the substrate surface is treated, a reduced pressure drying treatment may be performed as necessary. In addition, the reaction between the substrate and the adhesion improver may be promoted by subsequent heat treatment at 50°C to 280°C.

[0174] Next, the coating film of the resin composition is dried to obtain a resin film, which is preferably dried at a temperature in the range of 50° C. to 140° C. for one minute to several hours using an oven, a hot plate, infrared rays, etc.

[0175] On the other hand, when using a resin sheet formed from the resin composition of the present invention, if the resin sheet has a protective film, the protective film is peeled off, the resin sheet is placed opposite the substrate, and the two are bonded by thermocompression (the process of placing the resin sheet opposite the substrate and bonding them by thermocompression is sometimes referred to as laminating the resin sheet to the substrate). Next, the resin sheet laminated to the substrate is dried in the same manner as in obtaining the resin film to form a resin film. The resin sheet can be obtained by applying the resin composition of the present invention to a support film made of polyethylene terephthalate or the like, which is a peelable substrate, and drying the film.

[0176] Thermocompression bonding can be performed by heat pressing, heat lamination, heat vacuum lamination, etc. The lamination temperature is preferably 40°C or higher in terms of adhesion to the substrate and embeddability. In addition, when the resin sheet has photosensitivity, the lamination temperature is preferably 140°C or lower in order to prevent the resin sheet from curing during lamination, which may result in a decrease in the resolution of the pattern formation in the exposure and development process.

[0177] In the exposure step, the photosensitive resin film is irradiated with actinic radiation through a mask having a desired pattern. Actinic radiation used for exposure includes ultraviolet rays, visible rays, electron beams, X-rays, etc., but in the present invention, it is preferable to use g-rays (436 nm), h-rays (405 nm), or i-rays (365 nm), which are common exposure wavelengths. In the case of a resin film that does not have photosensitivity, a photoresist is formed after the resin film is formed, and then the actinic radiation is irradiated.

[0178] Next, the exposed photosensitive resin film is developed. As the developer, an aqueous solution of an alkaline compound such as tetramethylammonium, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and hexamethylenediamine is preferable. In some cases, polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, γ-butyrolactone, and dimethylacrylamide, alcohols such as methanol, ethanol, and isopropanol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, and ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, and methyl isobutyl ketone may be added to these alkaline aqueous solutions. After development, rinsing with water is generally performed. Here too, rinsing treatment may be carried out by adding alcohols such as ethanol and isopropyl alcohol, or esters such as ethyl lactate and propylene glycol monomethyl ether acetate to water.

[0179] The resin film thus obtained is heated to advance the thermal crosslinking reaction, and the cured film of the present invention is obtained. The cured film has improved heat resistance and chemical resistance due to crosslinking. This heat treatment may be performed by increasing the temperature stepwise or continuously. The heat treatment is preferably performed for 5 minutes to 5 hours. An example is a case where the heat treatment is performed at 100°C for 30 minutes, and then further at 230°C for 60 minutes. The heat treatment conditions are preferably 140°C or higher and 400°C or lower. The heat treatment conditions are preferably 140°C or higher and more preferably 160°C or higher in order to advance the thermal crosslinking reaction. In addition, the heat treatment conditions are preferably 300°C or lower and more preferably 250°C or lower in order to provide an excellent cured film and improve the reliability of semiconductor devices and display devices.

[0180] The cured film of the present invention thus obtained has an opening pattern, and the angle of the inclined side in the cross section of the opening pattern is preferably 40° or more and 80° or less.

[0181] Fig. 3 shows a front cross-sectional view of the opening pattern of the cured film. In Fig. 3, the angle of the inclined side 14 of the opening pattern formed in the cured film 3 is 15. The inclined side is a straight line connecting the upper opening pattern and the lower opening pattern.

[0182] By setting the angle of the inclined side in the cross section of the opening pattern of the cured film within this range, semiconductor devices and display devices described below to which this cured film is applied are less likely to suffer from problems such as wiring defects such as wiring short circuits, and are highly reliable.

[0183] <Semiconductor device> The cured film of the present invention obtained by curing the resin composition of the present invention or the resin sheet of the present invention can be used in electronic components such as known semiconductor devices. That is, the semiconductor device of the present invention has the cured film of the present invention. The semiconductor device of the present invention has metal wiring and an insulating film, and has the cured film of the present invention as an insulating film. The semiconductor device generally refers to a device that includes a semiconductor element or an integrated circuit that integrates the semiconductor element as a component. The semiconductor device of the present invention includes not only a device that includes a semiconductor element, but also components for a semiconductor device such as a wiring board. In addition, the semiconductor device of the present invention also includes a semiconductor package in which a semiconductor element or the like is protected by a sealing resin and further has a function of electrically connecting to the outside. Specifically, the cured film of the present invention is suitably used for applications such as a passivation film for a semiconductor, a protective film for a semiconductor element, and an interlayer insulating film for multilayer wiring for high-density packaging.

[0184] In particular, in recent semiconductor devices, with the further miniaturization of electrodes of semiconductor elements and metal wiring of substrates, semiconductor devices having electrodes, metal wiring, and bumps using gold, silver, copper, nickel, aluminum, etc. have become mainstream, and in the etching process of metal wiring and barrier metal and the pattern formation process of resist during the formation of these, they come into contact with many chemicals such as flux and strippers for removing photoresist. When the cured film made of the resin composition or resin sheet of the present invention is used as a protective film for such electrodes and metal wiring, it is particularly preferably used because it has high resistance to these chemicals. Note that copper wiring may be subjected to oxidation treatment in the manufacturing process. Even in such cases, the cured film of the present invention can be preferably used.

[0185] Preferred examples of semiconductor devices having the cured film of the present invention (hereinafter, sometimes referred to as a cured film made of the resin composition or resin sheet of the present invention) obtained by curing the resin composition of the present invention or the resin sheet of the present invention include logic devices such as CPUs and GPUs described in International Publication No. 2018 / 066395, memories such as MRAM and promising polymer memories (Polymer Ferroelectric RAM: PFRAM) and phase change memories (Phase Change RAM: PCRAM, or Ovonic Unified Memory: OUM), semiconductor devices having bumps, fan-out wafer level packages (fan-out WLPs) or fan-out panel level packages (fan-out PLPs), coil components of inductor devices, mini LEDs with a chip size of 100 to 700 μm, and micro LEDs with a chip size of 100 μm or less.

[0186] In a semiconductor device having bumps, a fan-out wafer level package (fan-out WLP) or a fan-out panel level package (fan-out PLP), or a coil component of an inductor device, a cured film made of the resin composition or resin sheet of the present invention may be formed as an insulating film, and then a metal wiring (so-called rewiring) may be formed thereon. By repeating the above steps, a multilayer wiring structure can be formed in which two or more layers of rewiring are separated by an insulating film made of the cured product of the resin composition or resin sheet of the present invention. The insulating film separating the rewiring is called an interlayer insulating film. In this case, the formed insulating film will come into contact with various chemical solutions multiple times, but since the insulating film made of the cured product of the resin composition or resin sheet of the present invention has excellent adhesion and chemical resistance, a good multilayer wiring structure can be formed. Furthermore, when the resin composition or resin sheet of the present invention has photosensitivity, it has an excellent taper shape after curing, which improves the degree of freedom in the layout design of copper wiring when forming multilayer metal wiring, and therefore it can be particularly preferably used as a protective film for multilayer metal wiring. There is no upper limit to the number of layers in a multilayer wiring structure, but one having 10 layers or less is often used.

[0187] In fan-out WLP or fan-out PLP, the rewiring is becoming finer. The cured film of the present invention has high metal adhesion even to metal wiring with a width of the metal wiring and a distance between adjacent metal wirings of 5 μm or less, and is therefore suitable for use in fine rewiring. Here, the width of the metal wiring and the distance between adjacent metal wirings of 5 μm or less means that the width of the metal wiring is 5 μm or less, and the distance between adjacent metal wirings is also 5 μm or less.

[0188] In the fan-out WLP or fan-out PLP having such a fine structure, it is preferable that the width of the metal wiring and the interval between adjacent metal wirings in the rewiring layer closer to the semiconductor chip among the adjacent rewiring layers are the same or narrower than the width of the metal wiring and the interval between adjacent metal wirings in the rewiring layer farther from the semiconductor chip. Here, the rewiring layer refers to a layer consisting of a set of rewirings and an interlayer insulating film formed thereon in a multilayer wiring structure in which multiple rewirings are separated by multiple interlayer insulating films. Note that there are also cases where the rewiring layer consists of only one layer. Moreover, the width of the metal wiring and the interval between adjacent metal wirings in the rewiring layer being the same or narrower means that the width of the metal wiring in the rewiring layer closer to the semiconductor chip is the same or narrower than the width of the metal wiring in the rewiring layer farther from the semiconductor chip, and the interval between adjacent metal wirings in the rewiring layer closer to the semiconductor chip is the same or narrower than the interval between adjacent metal wirings in the rewiring layer farther from the semiconductor chip.

[0189] Furthermore, in these structures, it is preferable that the thickness of the interlayer insulating film of the redistribution layer closer to the semiconductor chip, among adjacent redistribution layers, is the same as or thinner than the thickness of the interlayer insulating film of the redistribution layer farther from the semiconductor chip.

[0190] <Display device> The cured film obtained by curing the resin composition or the resin sheet of the present invention is suitably used in a display device including a first electrode formed on a substrate and a second electrode provided opposite the first electrode, specifically, for example, a display device using an LCD, an ECD, an ELD, or an organic EL.

[0191] The organic EL display device of the present invention has at least a TFT substrate, a planarizing layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode, and it is preferable that the planarizing layer or the insulating layer contains the cured film of the present invention.

[0192] Furthermore, it is preferable that the display device has at least metal wiring, the cured film of the present invention, and a plurality of light-emitting elements, wherein the light-emitting elements have a pair of electrode terminals on either one surface, the pair of electrode terminals are connected to a plurality of the metal wirings extending in the cured film, and the plurality of the metal wirings maintain electrical insulation due to the cured film.

[0193] The display device will be described with reference to FIG. 1 as an example of one embodiment.

[0194] In FIG. 1, the display device 1 has a plurality of light-emitting elements 2 arranged on a counter substrate 5, and a cured film 3 arranged on the light-emitting elements 2. The term "on the light-emitting elements" may refer not only to the surface of the light-emitting elements, but also to the upper side of the support substrate or the light-emitting elements. In the embodiment shown in FIG. 1, a configuration is illustrated in which a plurality of cured films 3 are further laminated on the cured film 3 arranged so as to contact at least a part of the light-emitting elements 2, resulting in a total of three layers, but this is not limited thereto, and the cured film 3 may be a single layer. The light-emitting element 2 has a pair of electrode terminals 6 on the surface opposite to the surface in contact with the counter substrate 5, and each electrode terminal 6 is connected to a metal wiring 4 extending in the cured film 3. The multiple metal wirings 4 extending in the cured film 3 are covered by the cured film 3, and the cured film 3 also functions as an insulating film, so that the configuration maintains electrical insulation. Furthermore, the light-emitting element 2 is electrically connected to a driving element 8 added to a light-emitting element driving substrate 7 provided at a position opposite to the counter substrate 5 through the metal wiring 4 or 4c, so that the light emission of the light-emitting element 2 can be controlled. Furthermore, the light-emitting element driving substrate 7 is electrically connected to the metal wiring 4 via, for example, solder bumps 10. Furthermore, a barrier metal 9 may be disposed to prevent diffusion of metal such as the metal wiring 4. Note that, hereinafter, the metal wiring 4c in the figures may penetrate the light-emitting element driving substrate 7 and be connected to the driving element 8.

[0195] The cured film 3 is a cured film obtained by curing the resin composition or resin sheet of the present invention.

[0196] There are no particular limitations on the material of the metal wiring 4, and any known material can be used. Examples include gold, silver, copper, aluminum, and nickel, with copper being preferred. As another embodiment of the display device, as shown in Fig. 4, a configuration is exemplified in which a cured film 16 is provided in the display device of Fig. 1 so as to be in contact with at least a part of the light-emitting element 2. The cured film 16 arranged in contact with at least a part of the light-emitting element 2 may be composed of a cured film obtained by curing the resin composition or resin sheet of the present invention, or may be composed of a material other than the cured film obtained by curing the resin composition or resin sheet of the present invention, and known materials such as epoxy resin, silicone resin, and fluororesin may be used.

[0197] In the present invention, the total thickness of the cured film is preferably from 5 μm to 100 μm.

[0198] By making the total thickness of the cured film 5 μm to 100 μm, it is possible to reduce the height of the display device having the light-emitting element itself, suppress wiring defects such as short circuits due to shortening the wiring distance, suppress loss, and improve high-speed response.

[0199] The total thickness of the cured film refers to the total thickness of the continuous cured film layer in which at least a part of one cured film is in contact with another cured film. For example, when a plurality of cured films 3 are laminated as shown in FIG. 1, the region indicated by 12 in FIG. 1 is the total thickness of the cured film layer. The total thickness is preferably 7 to 70 μm, more preferably 8 to 60 μm. If it is less than 5 μm, there is a concern of wiring defects such as short circuit of wiring due to insufficient protection of metal wiring, and if it exceeds 100 μm, there may be inconveniences in terms of reducing the height of the display device itself, suppressing wiring defects such as short circuit of wiring due to shortening the wiring distance, suppressing loss reduction, and improving high-speed response.

[0200] In addition, when a plurality of cured films are laminated, the number of layers of the cured films is preferably 2 to 10.

[0201] From the viewpoint of arranging a plurality of light-emitting elements, the cured film preferably has one or more layers. Furthermore, by having two or more layers, the number of metal wirings that can be connected to the light-emitting elements can be increased, so that a plurality of light-emitting elements can be arranged. Also, from the viewpoints of suppressing wiring defects such as short circuits due to a low package height and a short wiring distance, reducing loss, and improving high-speed responsiveness, the cured film preferably has 10 layers or less.

[0202] This configuration allows the application of minute light-emitting elements, and also allows for high-density mounting of multiple light-emitting elements, making it possible to obtain a display device having light-emitting elements with high resolution in a wide range of sizes.Furthermore, it becomes possible to form fine metal wiring, and since the number of wirings that can be formed in a unit area increases, the overall thickness of the cured film can be reduced, and it becomes possible to reduce the height of the display device having the light-emitting elements, suppress wiring defects such as short circuits due to shortening the wiring distance, suppress loss, and improve high-speed response.

[0203] From the viewpoint of application of minute light-emitting elements and high-density mounting of light-emitting elements, the maximum length of the bottom part of the metal wiring is preferably 2 to 15 μm, more preferably 2 to 10 μm, and further preferably 2 to 5 μm. If it is less than 2 μm, poor connection with the light-emitting element 2 may occur, and if it exceeds 20 μm, it may be detrimental to application of minute light-emitting elements and high-density mounting.

[0204] Moreover, the light emitting element is preferably an LED having a side length of 5 μm or more and 700 μm or less, and more preferably, the light emitting element is an LED having a side length of 5 μm or more and 100 μm or less.

[0205] In the present invention, a partition wall having a thickness equal to or greater than the thickness of the light emitting elements and made of a cured film obtained by curing a resin composition containing the (A) resin may be provided between the plurality of light emitting elements.

[0206] 2, it is preferable to have partition walls 11 in a repeating pattern according to the number of pixels of a display device 1 having light-emitting elements 2, i.e., between or around each light-emitting element 2. This configuration is preferable because it makes it easier to attach the display device to the counter substrate 5.

[0207] The thickness of the partition is preferably larger than the thickness of each light emitting element, and specifically, is preferably 5 μm to 120 μm.

[0208] The partition wall may be a cured film obtained by curing the resin composition or the resin sheet of the present invention, or may be made of other materials, such as known materials including epoxy resins, (meth)acrylic polymers, polyurethanes, polyesters, polyolefins, and polysiloxanes.

[0209] In addition, it is preferable that a partition wall having a thickness equal to or greater than the thickness of the light emitting element is disposed between the plurality of light emitting elements in the cured film covering the light emitting elements. EXAMPLES

[0210] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. The resin compositions and resin sheets in the examples were evaluated by the following methods. For the evaluation, a resin composition (hereinafter referred to as varnish) that had been previously filtered through a 1 μm polytetrafluoroethylene filter (manufactured by Sumitomo Electric Industries, Ltd.) was used.

[0211] <Evaluation of resin composition without photosensitivity> (1) Evaluation of the opening pattern shape of a cured film made of a resin composition that does not have photosensitivity A varnish was prepared and applied to an 8-inch silicon wafer by spin coating using a coater / developer ACT-8 (Tokyo Electron Ltd.) so that the film thickness after heating would be 7 μm, followed by pre-baking to prepare a pre-baked film. Pre-baking was performed at 110°C for 3 minutes. Thereafter, a positive photoresist OFPR-800 (Tokyo Ohka Kogyo Co., Ltd.) was applied onto the pre-baked film and pre-baked at 100°C for 10 minutes. Next, an i-line stepper (Nikon Corporation, NSR-2205i14) was used to apply 100 to 800 mJ / cm2. 2The exposure was performed at an exposure dose of 1.5 μm. The size of the circular pattern used for exposure was 30 μm. After exposure, the film was developed using a 2.38% by mass tetramethylammonium (TMAH) aqueous solution (manufactured by Tama Chemicals) under conditions such that the change in film thickness in the unexposed area before and after development was 1.5 μm, and then rinsed with pure water and spun dry to obtain a patterned film. The film thickness after pre-baking and after development was measured using an optical interference film thickness measuring device Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd., with a refractive index of 1.629.

[0212] Next, the temperature was increased from 50° C. to 100° C. at 3.5° C. / min, and then a heat treatment was performed at 100° C. for 30 minutes. After that, the temperature was increased to 160° C. at 3.5° C. / min, and then a baking was performed at 160° C. for 10 minutes, and then the photoresist film was removed by immersing in a stripping solution 106 (manufactured by Tokyo Ohka Kogyo Co., Ltd.) for 3 minutes and rinsing with pure water.

[0213] Thereafter, using an inert oven CLH-21CD-S (manufactured by Koyo Thermo Systems Co., Ltd.), the temperature was raised from 50° C. to 100° C. at a rate of 3.5° C. / min under a nitrogen stream with an oxygen concentration of 20 ppm or less, and then heat treatment was performed for 30 minutes at 100° C. Thereafter, the temperature was raised at a rate of 3.5° C. / min to a cure temperature of 200° C., 230° C., or 250° C. as shown in Table 3, and then heat treatment was performed for 1 hour at the cure temperature after the temperature increase as shown in Table 3, thereby curing the pattern-forming film to obtain a cured film.

[0214] When the temperature dropped below 50°C, the wafer was removed, and then the wafer was cut and the cross-sectional shape of the 5 μm circular pattern was observed and measured using a scanning electron microscope S-4800 (Hitachi High-Technologies Corporation). The angle of the inclined side was calculated by connecting the upper opening pattern and the lower opening pattern with a straight line.

[0215] As a result, when the angle of the inclined side was between 40° and 80° and below, it was rated as good, with a rating of 2, and when it was less than 40° or more than 80°, it was rated as poor, with a rating of 1.

[0216] (2) Evaluation of chemical resistance of non-photosensitive resin compositions A varnish was prepared and applied to an 8-inch silicon wafer by spin coating using a coating and developing apparatus ACT-8 (manufactured by Tokyo Electron Ltd.) so that the film thickness after heating would be 7 μm, followed by pre-baking to produce a pre-baked film. Pre-baking was performed at 110°C for 3 minutes in each case. Thereafter, development was performed using a 2.38 mass% aqueous solution of tetramethylammonium (TMAH) (manufactured by Tama Chemicals Co., Ltd.) under conditions such that the change in film thickness in the unexposed areas before and after development would be 1.5 μm, followed by rinsing with pure water and shaking off to dry, yielding a developed resin film.

[0217] Thereafter, the coating film was heated in an inert oven (manufactured by Koyo Thermo Systems Co., Ltd., CLH-21CD-S) from 50°C to 100°C at a rate of 3.5°C / min under a nitrogen stream with an oxygen concentration of 20 ppm or less, and then heat-treated at 100°C for 30 minutes. Thereafter, the temperature was raised at a rate of 3.5°C / min to 200°C, 230°C or 250°C, which are the curing temperatures listed in Table 3, and then heat-treated for 1 hour at the curing temperature after the temperature increase listed in Table 3, to harden the coating film and obtain a cured film. The thickness of the coating film after pre-baking and development was measured using an optical interference film thickness measuring device Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd., with a refractive index of 1.629, and the thickness of the cured film was measured with a refractive index of 1.629.

[0218] When the temperature dropped below 50° C., the silicon wafer was removed, and the resulting cured film was immersed in a stripper consisting of NMP / DMSO / ethanolamine=70 / 20 / 10 and treated at 70° C. for 30 minutes. Thereafter, the presence or absence of peeling or elution was observed, and the rate of change in film thickness was measured.

[0219] As a result, when the rate of change in film thickness before and after immersion was 5% or less, it was rated as extremely good (3), when the rate of change in film thickness was more than 5% but less than 10%, it was rated as good (2), and when the rate of change in film thickness was more than 10% or peeling or dissolution was observed, it was rated as poor (1). The smaller the rate of change in film thickness, the better the chemical resistance.

[0220] (3) HAST resistance evaluation of non-photosensitive resin composition on copper wiring board To evaluate peeling in copper wiring, the following evaluation substrate was prepared. Copper wiring with a thickness of 3 μm, width of 50 μm, and wiring interval of 100 μm was created on an 8-inch silicon wafer. This was used as the evaluation substrate.

[0221] The varnish was applied to the evaluation substrate by spin coating using a coating and developing apparatus ACT-8 (manufactured by Tokyo Electron Co., Ltd.) so that the film thickness after heating would be 7 μm, and prebaked to prepare a prebaked film. The prebaking was performed at 110°C for 3 minutes. Then, using an inert oven CLH-21CD-S (manufactured by Koyo Thermo Systems Co., Ltd.), the temperature was raised from 50°C to 100°C at a rate of 3.5°C / min under a nitrogen flow with an oxygen concentration of 20 ppm or less, and then heat treatment was performed at 100°C for 30 minutes. Then, the temperature was raised at a rate of 3.5°C / min to 200°C, 230°C, or 250°C, which are the cure temperatures listed in Table 3, and then heat treatment was performed for 1 hour at the cure temperature after heating listed in Table 3, and the prebaked film was cured to obtain a cured film. When the temperature reached 50°C or less, the evaluation substrate (hereinafter referred to as a sample) was taken out.

[0222] Next, the sample was placed in a HAST device and treated for 168 hours at a temperature of 130°C and a humidity of 85%. After that, the sample was removed and cut and the cross section was observed at a magnification of 50,000 times using a scanning electron microscope Versa 3D Dual Beam (manufactured by FEI Corporation) with a focused ion beam processing device in order to observe peeling between the resin composition and the copper wiring.

[0223] As a result, those with no peeling between the resin composition and the copper wiring were rated as extremely good (2), those with some defects such as peeling or cavities were rated as fair (1), and those with defects such as peeling or cavities were rated as poor (0). The fewer peeling or cavities, the better the HAST resistance.

[0224] <Evaluation of photosensitive resin composition> (4) Evaluation of the opening pattern shape of a cured film made of a photosensitive resin composition The varnish was prepared and applied to an 8-inch silicon wafer by spin coating using a coating and developing apparatus ACT-8 (Tokyo Electron Ltd.) so that the film thickness after heating would be 7 μm. The wafer was then prebaked to produce a prebaked film. Prebaking was performed at 110°C for 3 minutes. Then, an i-line stepper (Nikon Corporation, NSR-2205i14) was used to apply 100 to 800 mJ / cm2. 2 The exposure was performed at an exposure dose of 1.5 μm. The size of the circular pattern used for exposure was 5 μm. After exposure, the film was developed using a 2.38% by mass tetramethylammonium (TMAH) aqueous solution (manufactured by Tama Chemicals) under conditions such that the change in film thickness in the unexposed area before and after development was 1.5 μm, and then rinsed with pure water and spun dry to obtain a patterned film. The film thickness after pre-baking and after development was measured using an optical interference film thickness measuring device Lambda Ace STM-602 manufactured by Dainippon Screen Mfg. Co., Ltd., with a refractive index of 1.629.

[0225] After development, the film was heated from 50° C. to 100° C. at a rate of 3.5° C. / min under a nitrogen stream with an oxygen concentration of 20 ppm or less using an inert oven CLH-21CD-S (manufactured by Koyo Thermo Systems Co., Ltd.), and then heated for 30 minutes at 100° C. After that, the film was heated at a rate of 3.5° C. / min to a cure temperature of 200° C., 230° C., or 250° C. as shown in Table 4, and then heated for 1 hour at the cure temperature after the temperature increase as shown in Table 4, to cure the pattern-forming film and obtain a cured film.

[0226] When the temperature dropped below 50°C, the wafer was removed, and then the wafer was cut and the cross-sectional shape of the 5 μm circular pattern was observed and measured using a scanning electron microscope S-4800 (Hitachi High-Technologies Corporation). The angle of the inclined side was calculated by connecting the upper opening pattern and the lower opening pattern with a straight line.

[0227] As a result, when the angle of the inclined side was between 40° and 80° and below, it was rated as good, with a rating of 2, and when it was less than 40° or more than 80°, it was rated as poor, with a rating of 1.

[0228] (5) Evaluation of chemical resistance of photosensitive resin composition The same as (2) above except as shown in Table 4.

[0229] (6) HAST resistance evaluation of photosensitive resin composition on copper wiring board The same as (3) above except as shown in Table 4.

[0230] <Synthesis Example 1: Synthesis of hydroxyl group-containing diamine compound> 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (manufactured by Central Glass Co., Ltd., hereinafter referred to as BAHF) was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide (manufactured by Tokyo Chemical Industry Co., Ltd.), and cooled to -15°C. A solution of 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride (manufactured by Tokyo Chemical Industry Co., Ltd.) dissolved in 100 mL of acetone was added dropwise to the solution. After the dropwise addition, the mixture was stirred at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was filtered and dried in vacuum at 50°C.

[0231] 30 g of the obtained white solid was placed in a 300 mL stainless steel autoclave and dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon (Wako Pure Chemical Industries, Ltd.) was added. Hydrogen was introduced into the mixture using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, the reaction was terminated when it was confirmed that the balloon was no longer deflating. After the reaction was completed, the mixture was filtered to remove the palladium compound catalyst, and the mixture was concentrated using a rotary evaporator to obtain a hydroxyl group-containing diamine compound represented by the following formula.

[0232] [ka]

[0233] <Synthesis Example 2: Synthesis of phenol trinuclear compounds> In a 100mL two-neck flask equipped with a condenser and a thermometer, 3.2g (30mmol) of m-cresol and 1.2g (10mmol) of p-hydroxybenzaldehyde were charged and dissolved in 10mL of 2-ethoxyethanol. After adding 1mL of sulfuric acid while cooling in an ice bath, the mixture was heated and stirred at 100°C for 2 hours to react. After the reaction, the resulting solution was reprecipitated with water to obtain a crude product. The crude product was redissolved in acetone and further reprecipitated with water, and the resulting product was filtered and dried in vacuum to obtain a phenol trinuclear compound represented by the following formula.

[0234] [ka]

[0235] <Synthesis Example 3: Synthesis of phenol trinuclear compounds> In a 100mL two-neck flask equipped with a condenser and a thermometer, 3.2g (30mmol) of m-cresol and 1.4g (10mmol) of p-hydroxyacetophenone were charged and dissolved in 10mL of 2-ethoxyethanol. After adding 1mL of sulfuric acid while cooling in an ice bath, the mixture was heated and stirred at 100°C for 2 hours to react. After the reaction, the resulting solution was reprecipitated with water to obtain a crude product. The crude product was redissolved in acetone and further reprecipitated with water, and the resulting product was filtered and dried in vacuum to obtain a phenol trinuclear compound represented by the following formula.

[0236] [ka]

[0237] <Synthesis Example 4: Synthesis of polybenzoxazole precursor (A-1)> Under a dry nitrogen stream, 1.5 g (0.0075 mol) of 4,4'-diaminodiphenyl ether (hereinafter referred to as 4,4'-DAE), 12.8 g (0.035 mol) of BAHF, and 5.0 g (0.0050 mol) of RT-1000 (HUNTSMAN Co., Ltd.) were dissolved in 100 g of NMP. To this, dodecanoic acid diimidazole (7.4 g, 0.023 mol) and PBOM (8.1 g, 0.023 mol) were added together with 25 g of NMP, and the mixture was reacted at 85°C for 3 hours. Next, 0.6 g (0.0025 mol) of SiDA, 0.8 g (0.0025 mol) of ODPA, and 0.8 g (0.0050 mol) of NA were added together with 25 g of NMP, and the mixture was reacted at 85°C for 1 hour. After the reaction was completed, the mixture was cooled to room temperature, and 13.2 g (0.25 mol) of acetic acid was added together with 25 g of NMP, followed by stirring at room temperature for 1 hour. After stirring was completed, the solution was poured into 1.5 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and then dried in a 50°C ventilated dryer for three days to obtain a powder of polybenzoxazole precursor (A-1).

[0238] <Synthesis Example 5: Synthesis of polybenzoxazole precursor (A-2)> Under a dry nitrogen stream, 27.5 g of BAHF (0.075 mol) was dissolved in 257 g of NMP. 17.2 g (0.048 mol) of PBOM was added together with 20 g of NMP, and the mixture was reacted at 85 ° C for 3 hours. Next, 20.0 g (0.02 mol) of RT-1000 (HUNTSMAN Co., Ltd.), 1.2 g (0.005 mol) of SiDA, and 14.3 g (0.04 mol) of PBOM were added together with 50 g of NMP, and the mixture was reacted at 85 ° C for 1 hour. Furthermore, 3.9 g (0.024 mol) of 5-norbornene-2,3-dicarboxylic anhydride was added together with 10 g of NMP as a terminal blocking agent, and the mixture was reacted at 85 ° C for 30 minutes. After the reaction was completed, the mixture was cooled to room temperature, and 52.8 g (0.50 mol) of acetic acid was added together with 87 g of NMP, and the mixture was stirred at room temperature for 1 hour. After stirring, the solution was poured into 3 L of water to obtain a white precipitate, which was collected by filtration, washed three times with water, and then dried in a 50°C ventilated dryer for three days to obtain a powder of polybenzoxazole precursor (A-2).

[0239] <Synthesis Example 6: Synthesis of polyimide precursor (A-3)> Under a dry nitrogen stream, 51.9 g (0.086 mol) of the hydroxyl group-containing diamine obtained in Synthesis Example 1 and 1.0 g (0.004 mol) of 1,3-bis(3-aminopropyl)tetramethyldisiloxane (hereinafter referred to as SiDA) were dissolved in 200 g of NMP. 31.0 g (0.10 mol) of 4,4'-oxydiphthalic anhydride (hereinafter referred to as ODPA) was added thereto, and the mixture was stirred at 40°C for 2 hours. Then, 1.1 g (0.01 mol) of 3-aminophenol (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an end-capping agent together with 10 g of NMP, and the mixture was reacted at 40°C for 1 hour. Then, a solution obtained by diluting 7.1 g (0.06 mol) of dimethylformamide dimethylacetal (manufactured by Mitsubishi Rayon Co., Ltd., hereinafter referred to as DFA) with 5 g of NMP was added dropwise. After the dropwise addition, the mixture was stirred at 40°C for 2 hours. After stirring, the solution was poured into 2 L of water, and the precipitate of the polymer solid was collected by filtration. The polymer solid was washed three times with 2 L of water, and then dried in a vacuum dryer at 50° C. for 72 hours to obtain a polyimide precursor (A-3).

[0240] <Synthesis Example 7 Synthesis of polyimide precursor (A-4)> Under a dry nitrogen stream, 41.1 g (0.068 mol) of the hydroxyl group-containing diamine obtained in Synthesis Example 1, 18.0 g (0.018 mol) of a diamine containing propylene oxide and tetramethylene ether glycol structures (RT-1000, manufactured by HUNTSMAN Co., Ltd.), and 1.0 g (0.004 mol) of SiDA were dissolved in 200 g of NMP. 31.0 g (0.10 mol) of ODPA was added thereto, and the mixture was stirred at 40° C. for 2 hours. Then, 1.1 g (0.01 mol) of 3-aminophenol was added as an end-capping agent together with 10 g of NMP, and the mixture was reacted at 40° C. for 1 hour. Then, a solution in which 6.0 g (0.05 mol) of DFA (manufactured by Mitsubishi Rayon Co., Ltd.) was diluted with 5 g of NMP was added dropwise. After the dropwise addition, the mixture was stirred for 2 hours at 40° C. After the stirring was completed, the solution was poured into 2 L of water, and the precipitate of the polymer solid was collected by filtration. The polymer was further washed three times with 2 L of water, and the collected polymer solid was dried in a vacuum dryer at 50° C. for 72 hours to obtain a polyimide precursor (A-4).

[0241] <Synthesis Example 8: Synthesis of polyimide (A-5)> Under a dry nitrogen stream, 29.3 g (0.08 mol) of BAHF, 1.2 g (0.005 mol) of SiDA, and 3.3 g (0.03 mol) of 3-aminophenol as a terminal blocking agent were dissolved in 80 g of NMP. 31.2 g (0.1 mol) of ODPA was added together with 20 g of NMP, and the mixture was reacted at 60°C for 1 hour, and then stirred at 180°C for 4 hours. After stirring, the solution was poured into 3 L of water to obtain a white precipitate. The precipitate was collected by filtration, washed three times with water, and then dried in a vacuum dryer at 80°C for 20 hours to obtain a powder of polyimide (A-5).

[0242] <Synthesis Example 9: Synthesis of phenolic resin (B-1)> Under a dry nitrogen stream, 108.1g (1.0 mol) of m-cresol, 34.0g (0.32 mol) of benzaldehyde, 90.4g (0.74 mol) of salicylaldehyde, 200g of ethanol, and 8.6g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain phenolic resin (B-1). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 70:30.

[0243] <Synthesis Example 10: Synthesis of phenolic resin (B-2)> Under a dry nitrogen stream, 108.1g (1.0 mol) of m-cresol, 11.7g (0.11 mol) of benzaldehyde, 116.0g (0.95 mol) of salicylaldehyde, 200g of ethanol, and 8.6g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain phenolic resin (B-2). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 90:10.

[0244] <Synthesis Example 11 Synthesis of phenolic resin (B-3)> Under a dry nitrogen stream, 108.1g (1.0 mol) of m-cresol, 44.6g (0.42 mol) of benzaldehyde, 76.9g (0.63 mol) of salicylaldehyde, 200g of ethanol, and 8.6g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain phenolic resin (B-3). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 60:40.

[0245] <Synthesis Example 12: Synthesis of phenolic resin (B-4)> Under a dry nitrogen stream, 108.1g (1.0 mol) of m-cresol, 128.2g (1.05 mol) of salicylaldehyde, 200g of ethanol, and 8.6g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain phenolic resin (B-4). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5):general formula (6)=100:0.

[0246] <Synthesis Example 13: Synthesis of phenolic resin (B-5)> Under a dry nitrogen stream, 108.1g (1.0 mol) of m-cresol, 56.2g (0.53 mol) of benzaldehyde, 64.7g (0.53 mol) of salicylaldehyde, 200g of ethanol, and 8.6g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain phenolic resin (B-5). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5):general formula (6)=50:50.

[0247] <Synthesis Example 14: Synthesis of phenolic resin (B-6)> Under a dry nitrogen stream, 108.1g (1.0 mol) of m-cresol, 38.4g (0.32 mol) of acetophenone, 100.8g (0.74 mol) of 4-hydroxyacetophenone, 200g of 2-ethoxyethanol, and 8.6g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted at 120°C for 18 hours. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain phenolic resin (B-6). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5):general formula (6)=70:30.

[0248] <Synthesis Example 15: Synthesis of phenolic resin (B-7)> Under a dry nitrogen stream, 320.4 g (1.0 mol) of the trinuclear phenol compound obtained in Synthesis Example 2, 34.0 g (0.32 mol) of benzaldehyde, 90.4 g (0.74 mol) of salicylaldehyde, 200 g of ethanol, and 8.6 g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain a phenolic resin (B-7). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 70:30.

[0249] <Synthesis Example 16: Synthesis of phenolic resin (B-8)> Under a dry nitrogen stream, 320.4 g (1.0 mol) of the trinuclear phenol compound obtained in Synthesis Example 2, 11.7 g (0.11 mol) of benzaldehyde, 116.0 g (0.95 mol) of salicylaldehyde, 200 g of ethanol, and 8.6 g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain a phenolic resin (B-8). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 90:10.

[0250] <Synthesis Example 17: Synthesis of phenolic resin (B-9)> Under a dry nitrogen stream, 320.4 g (1.0 mol) of the trinuclear phenol compound obtained in Synthesis Example 2, 44.6 g (0.42 mol) of benzaldehyde, 76.9 g (0.63 mol) of salicylaldehyde, 200 g of ethanol, and 8.6 g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted for 18 hours under reflux at 65°C. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain a phenolic resin (B-9). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 60:40.

[0251] <Synthesis Example 18: Synthesis of phenolic resin (B-10)> Under a dry nitrogen stream, 320.4 g (1.0 mol) of the trinuclear phenol compound obtained in Synthesis Example 2, 38.4 g (0.32 mol) of acetophenone, 100.8 g (0.74 mol) of 4-hydroxyacetophenone, 200 g of 2-ethoxyethanol, and 8.6 g (0.05 mol) of paratoluenesulfonic acid were charged into a reaction vessel and reacted at 120°C for 18 hours. After neutralizing the reaction system with caustic soda, methyl isobutyl ketone and water were added, and washing was performed five times by separation. Methyl isobutyl ketone was distilled off under reduced pressure at 100°C using an evaporator to obtain a phenolic resin (B-10). The ratio of the number of structural units represented by general formula (5) and general formula (6) was general formula (5): general formula (6) = 70:30.

[0252] <Synthesis Example 19: Synthesis of phenolic resin (B-11)> Under a dry nitrogen stream, 70.2g (0.65 mol) of m-cresol, 37.8g (0.35 mol) of p-cresol, 37% by weight, 75.5g of aqueous formaldehyde solution (0.93 mol of formaldehyde), 0.63g (0.005 mol) of oxalic acid dihydrate, and 264g of methyl isobutyl ketone were charged into a flask, which was then immersed in an oil bath and subjected to a polycondensation reaction for 4 hours while refluxing the reaction solution. The temperature of the oil bath was then raised over a period of 3 hours, after which the pressure in the flask was reduced to 40-67hPa to remove the volatile matter, and the flask was cooled to room temperature to obtain a polymer solid of phenolic resin (B-11). The weight average molecular weight determined by GPC was 3500.

[0253] <Synthesis Example 20: Synthesis of photosensitizer (quinone diazide compound) (D-1)> Under a dry nitrogen stream, 21.2 g (0.05 mol) of 4,4'-[1-[4-[1-(4-hydroxyphenyl-1)-1-methylethyl]phenyl]ethylidene]bisphenol (Honshu Chemical Industry Co., Ltd., hereinafter referred to as TrisP-PA) and 37.5 g (0.14 mol) of 5-naphthoquinone diazide sulfonic acid chloride (Toyo Gosei Co., Ltd., NAC-5) were dissolved in 450 g of γ-butyrolactone at room temperature. 12.7 g of triethylamine mixed with 50 g of γ-butyrolactone was added dropwise so that the temperature in the system did not exceed 35°C. After the dropwise addition, the mixture was stirred at 40°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The precipitate was then collected by filtration and washed with 1 L of 1% hydrochloric acid. Then, it was washed twice with 2 L of water. This precipitate was dried in a vacuum dryer to obtain a quinone diazide compound (D-1) represented by the following formula.

[0254] [ka]

[0255] <Synthesis Example 21: Synthesis of photosensitizer (quinone diazide compound) (D-2)> Under a dry nitrogen stream, 21.2 g (0.05 mol) of 4,4'-[1-[4-[1-(4-hydroxyphenyl-1)-1-methylethyl]phenyl]ethylidene]bisphenol (Honshu Chemical Industry Co., Ltd., hereinafter referred to as TrisP-PA) and 37.5 g (0.14 mol) of 4-naphthoquinone diazide sulfonic acid chloride (Toyo Gosei Co., Ltd., NAC-5) were dissolved in 450 g of γ-butyrolactone at room temperature. 12.7 g of triethylamine mixed with 50 g of γ-butyrolactone was added dropwise so that the temperature in the system did not exceed 35°C. After the dropwise addition, the mixture was stirred at 40°C for 2 hours. The triethylamine salt was filtered, and the filtrate was poured into water. The precipitate was then collected by filtration and washed with 1 L of 1% hydrochloric acid. Then, it was washed twice with 2 L of water. This precipitate was dried in a vacuum dryer to obtain a quinone diazide compound (D-2) represented by the following formula.

[0256] [ka]

[0257] The structures and solvents of the components (C-1), (C-2), (C-3), (C-4) and (C-5) used in the examples and comparative examples are shown below.

[0258] [ka]

[0259] [ka]

[0260] (C-1): YX-4000HK [biphenyl-type cyclic ether type thermal crosslinking agent] (manufactured by Mitsubishi Chemical Corporation) (C-3): TMOM-BP [biphenyl-type alkoxymethyl-type thermal crosslinking agent] (manufactured by Honshu Chemical Industry Co., Ltd.) (C-4): HMOM-TPHAP [triphenylmethane type alkoxymethyl type thermal crosslinking agent] (manufactured by Honshu Chemical Industry Co., Ltd.) Solvent: gamma-butyrolactone (GBL) [Examples 1 to 23, 26 ~43, Comparative Examples 1 to 16 , Reference example 25 ] To the (A) resins (A-1) to (A-5) obtained in Synthesis Examples 4 to 8, the (B) phenolic resins (B-1) to (B-11) obtained in Synthesis Examples 9 to 19, the (C) thermal crosslinking agents (C-1) to (C-5), and the photosensitive compounds (D-1) and (D-2) obtained in Synthesis Examples 20 to 21 were added in the amounts shown in Tables 1 to 2, and a varnish was prepared using GBL as a solvent. The properties of these were measured using the above-mentioned evaluation methods. The components and measurement results are shown in Tables 3 to 4. In the table, Example 25 should be read as Reference Example 25.

[0261] [Table 1]

[0262] [Table 2-1]

[0263] [Table 2-2]

[0264] [Table 3]

[0265] [Table 4-1]

[0266] [Table 4-2] [Explanation of symbols]

[0267] 1 Display device 2 Light emitting element 3 Cured film 4, 4c metal wiring 5 Opposing substrate 6 electrode terminal 7 Light emitting element driving board 8 Driving element 9. Barrier Metal 10 Solder Bumps 11 Bulkhead 12 Total thickness of the cured film 13 Substrate 14 Slanted Edge 15 Angle of inclined side 16 Cured film

Claims

1. (A) one or more resins selected from the group consisting of polyimide, polybenzoxazole, polyimide precursor, polybenzoxazole precursor, and copolymers thereof; (B) a phenolic resin, (C) Thermal crosslinking agent A resin composition comprising: The (B) phenol resin has a structural unit represented by general formula (4), and the structural unit represented by general formula (4) has structural units represented by general formulas (5) and (6), A resin composition in which, when the number of all structural units represented by general formula (4) in the (B) phenol resin is taken as 100, the ratio of the numbers of structural units represented by general formula (5) and general formula (6) is general formula (5):general formula (6)=60:40 to 90:

10. 【Chemistry 1】 (In general formula (4), R 25 , R 27 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 , R 27 When there are a plurality of R, they may be the same or different. 26 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. j1 and j2 each independently represent an integer of 0 to 3. 【Chemistry 2】 (In general formula (5), R 25 represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are a plurality of R, they may be the same or different. 26 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3, and j3 represents an integer of 1 to 3. 【Chemistry 3】 (In general formula (6), R 25 represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 25 When there are a plurality of R, they may be the same or different. 26 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 28 R represents a monovalent organic group having 1 to 10 carbon atoms. 28 When a plurality of j1 and j4 are present, they may be the same or different. j1 and j4 each independently represent an integer of 0 to 3. However, the sum of j3 and j4 is always j2.

2. The resin composition according to claim 1, wherein the (C) thermal crosslinking agent contains a thermal crosslinking agent having a biphenyl structure which may have a substituent and / or a thermal crosslinking agent having a structural unit represented by general formula (14). 【Chemistry 4】 (In general formula (14), R 42 represents a divalent organic group having an alkylene group or an alkylene ether group having 1 to 15 carbon atoms; R 43 and R 44 each independently represents a hydrogen atom or a methyl group.

3. The resin composition according to claim 2, wherein a content ratio of the thermal crosslinking agent having a biphenyl structure which may have a substituent and the thermal crosslinking agent having a structural unit represented by general formula (14) is 15 mass% or more and 80 mass% or less, when the entire thermal crosslinking agent (C) is 100 mass%.

4. The resin composition according to claim 2 or 3, wherein the thermal crosslinking agent having a biphenyl structure which may have a substituent contains a structure represented by general formula (12) or general formula (13). 【Chemistry 5】 (In general formula (12), R 29 and R 30 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 29 , R 30 When there are a plurality of R, they may be the same or different. 31 , R 32 represents a thermal crosslinking group. m1 and m2 each independently represent an integer of 0 to 4, and m3 and m4 each independently represent an integer of 1 to 3, and satisfy 1≦m1+m3≦5 and 1≦m2+m4≦5. 【Chemistry 6】 (In general formula (13), R 33 , R 34 , R 35 and R 36 R each independently represents a hydroxyl group or a monovalent organic group having 1 to 10 carbon atoms. 33 , R 34 , R 35 and R 36 When there are a plurality of R, they may be the same or different. 37 , R 38 , R 39 and R 40 represents a thermal crosslinking group. 41 represents a monovalent organic group having 1 to 10 carbon atoms; n1, n4, n5, and n8 each independently represent an integer of 1 to 3; n2, n3, n6, and n7 each independently represent an integer of 0 to 4; n9 represents a repeating unit and is an integer of 1 to 10; and n10 represents an integer of 0 or 1. However, n1+n5≦5, n2+n6≦4, n3+n7≦4, and n4+n8≦4.

5. The resin composition according to any one of claims 2 to 4, wherein the (C) thermal crosslinking agent contains the thermal crosslinking agent having a biphenyl structure which may have a substituent, and the content of the thermal crosslinking agent having a biphenyl structure which may have a substituent is 30 parts by mass or more and 150 parts by mass or less relative to 100 parts by mass of the (B) phenolic resin.

6. The resin composition according to any one of claims 1 to 5, further comprising (D) a photosensitive compound.

7. A resin sheet formed on a substrate using the resin composition according to any one of claims 1 to 6.

8. A cured film obtained by curing the resin composition according to any one of claims 1 to 6 or the resin sheet according to claim 7.

9. The cured film according to claim 8 , wherein the cured film has an opening pattern, and an angle of an inclined side in a cross section of the opening pattern is 40° or more and 80° or less.

10. The resin composition according to any one of claims 1 to 6 is applied to a substrate, or the resin sheet according to claim 7 is laminated to a substrate, and then A method for producing a cured film, comprising: a step of drying to form a resin film; an exposure step of exposing the dried resin film to light; a development step of developing the exposed resin film; and a heat treatment step of heat treating the developed resin film.

11. A semiconductor device comprising the cured film according to claim 8.

12. An organic electroluminescence display device having at least a TFT substrate, a planarization layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode, wherein the planarization layer or the insulating layer comprises the cured film according to claim 8.

13. 9. A display device having at least metal wiring, the cured film according to claim 8, and a plurality of light-emitting elements, wherein the light-emitting elements are provided with a pair of electrode terminals on either one surface thereof, the pair of electrode terminals are connected to a plurality of the metal wirings extending in the cured film, and the plurality of the metal wirings are configured to maintain electrical insulation due to the cured film.

Citation Information

Patent Citations

  • Photoresist of mixture of photoactive compounds

    JP1996286370A

  • Positive photosensitive resin precursor composition

    JP2005352004A

  • Photosensitive resin composition

    JP2010197748A

  • Positive photosensitive resin composition, cured film, protective film, insulating film, semiconductor device, and display device

    JP2014211517A

  • Method for producing novolak-type phenol resin and photoresist composition