Quality control method for polymeric material, manufacturing method for resin composition, and quality control method for cable or tube
Raman spectroscopy is used to assess silicone content in polymeric materials, ensuring consistent slipperiness and improved performance of cables and tubes by evaluating peak intensities, addressing the inconsistency in silicone distribution.
Patent Information
- Application Number
- JP2021021475
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-02-15
AI Technical Summary
The challenge in polymeric materials containing silicone as a lubricant is the inconsistency in silicone content, leading to unpredictable slipperiness, which affects the performance of cables and tubes.
A quality control method using Raman spectroscopy to measure molecular vibrations from silicone, evaluating slipperiness based on peak intensities in the Raman spectrum, ensuring consistent silicone distribution and surface properties.
Enables accurate, non-destructive evaluation of slipperiness in polymeric materials, producing cables and tubes with enhanced surface properties and improved flexibility.
Smart Images

Figure 0007589575000005 
Figure 0007589575000006 
Figure 0007589575000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymeric material and a quality control method thereof, a method for producing a resin composition, a cable or tube and a quality control method thereof, and factory automation or a factory automation robot. [Background technology]
[0002] Conventionally, cables using polyester elastomer containing organic high molecular weight silicone polymer as the material of the insulation that covers the conductor are known (see Patent Document 1). According to the cable described in Patent Document 1, silicone has low affinity with other substances, prevents adhesion between surfaces, and provides releasability, so that the surfaces of the insulated core wires have good sliding properties. When the cable is subjected to stress such as bending or twisting, the twisted insulated core wires can move smoothly relative to each other, which contributes to improving the bending and twisting life. In addition, by improving the sliding properties between the insulated core wires, the flexibility of the cable itself can be improved.
[0003] In addition, polyester elastomers containing organic high molecular weight silicone polymers are cheaper than fluorine-based resins such as ethylene tetrafluoroethylene (ETFE), which have traditionally been used commonly as insulating materials with excellent surface slipperiness, thereby reducing cable manufacturing costs. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2008-218061 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when silicone is blended with a polymeric material such as polyester elastomer, the silicone content of the blended polymeric material may not match the blending ratio of the raw materials, and the desired slipperiness may not be obtained. Therefore, it is desirable to evaluate the actual slipperiness of the surface of an insulator that uses a polymeric material containing silicone as its material.
[0006] An object of the present invention is to provide a quality control method for polymeric materials that can evaluate the surface slipperiness of polymeric materials that contain silicone as a lubricant, a method for producing a resin composition that utilizes this quality control method for polymeric materials, a cable or tube and a quality control method therefor, and factory automation or a factory automation robot. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, the present invention provides a quality control method for a polymeric material, comprising a measurement step of irradiating a polymeric material containing silicone as a lubricant with a laser and measuring the Raman spectrum, and an evaluation step of evaluating the lubricity of the surface of the polymeric material based on the intensity of a peak in the Raman spectrum that is assigned to molecular vibrations derived from the silicone.
[0008] Furthermore, for the purpose of solving the above-mentioned problems, the present invention provides a quality control method for a cable or tube having an insulation made of a polymeric material containing silicone as a lubricant, which evaluates the lubricity of the surface of the insulation by the above-mentioned quality control method for polymeric material.
[0009] Furthermore, in order to solve the above-mentioned problems, the present invention provides a method for producing a resin composition, which comprises forming a resin composition using a polymeric material containing silicone as a lubricant, the polymeric material having a surface slipperiness evaluated by the above-mentioned quality control method for polymeric materials.
[0010] In addition, in order to solve the above-mentioned problems, the present invention provides a polymeric material made of polyethylene containing silicone as a lubricant, which satisfies at least one of the following conditions: a first condition that, in a Raman spectrum obtained by irradiating a laser, a ratio of a peak height of a first peak attributed to Si-O stretching vibration of the silicone to a peak height of a third peak attributed to CH2 rolling vibration of the polyethylene is 0.043 or more; a second condition that a ratio of an integrated intensity of the first peak to an integrated intensity of the third peak is 0.1 or more; a third condition that a ratio of a peak height of a second peak attributed to C-Si-C stretching vibration of the silicone to a peak height of the third peak is 0.014 or more; and a fourth condition that a ratio of an integrated intensity of the second peak to an integrated intensity of the third peak is 0.011 or more.
[0011] Further, in order to solve the above-mentioned problems, the present invention provides a cable or tube having an insulator made of the above-mentioned polymer material.
[0012] In addition, in order to solve the above-mentioned problems, the present invention provides a factory automation or a factory automation robot equipped with the above-mentioned cable or tube. Effect of the Invention
[0013] According to the present invention, it is possible to provide a quality control method for polymeric materials that can evaluate the surface slipperiness of polymeric materials that contain silicone as a lubricant, a method for producing a resin composition that utilizes this quality control method for polymeric materials, a cable or tube and a quality control method thereof, and factory automation or a factory automation robot. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a radial cross-sectional view of a cable for an FA robot, which is an example of a cable according to the present embodiment. [Diagram 2] FIG. 2 is a graph showing Raman spectra of polyethylene containing no silicone and polyethylene containing silicone added in amounts of 0.99 to 6.54 mass %. [Diagram 3] Fig. 3(a) is a graph showing an enlargement of the vicinity of peak A1 and peak A2 in the Raman spectrum shown in Fig. 2. Fig. 3(b) is a graph showing an enlargement of the vicinity of peak A3 in the Raman spectrum shown in Fig. 2. [Figure 4] Fig. 4(a) is a graph showing the relationship between the ratio of the peak height of peak A1 to the peak height of peak A3 (peak height ratio) and the concentration of silicone added. Fig. 4(b) is a graph showing the relationship between the ratio of the integrated intensity of peak A1 to the integrated intensity of peak A3 (integral intensity ratio) and the concentration of silicone added. [Diagram 5] Fig. 5(a) is a graph showing the relationship between the ratio of the peak height of peak A2 to the peak height of peak A3 (peak height ratio) and the concentration of silicone added. Fig. 5(b) is a graph showing the relationship between the ratio of the integrated intensity of peak A2 to the integrated intensity of peak A3 (integral intensity ratio) and the concentration of silicone added. [Figure 6] Fig. 6(a) is a graph showing the relationship between the peak height ratio of peak A1 and the surface static friction coefficient of polyethylene containing 0 to 6.54 mass% silicone, measured under temperature conditions of 25° C., 50° C., and 75° C. Fig. 6(b) is a graph enlarging the range of peak height ratios of 0 to 0.2 in Fig. 6(a), and includes a straight line showing 0.351, which is the static friction coefficient of ETFE, measured under a temperature condition of 25° C. [Figure 7] Fig. 7(a) is a graph showing the relationship between the integrated intensity ratio of peak A1 and the static friction coefficient of the surface of polyethylene containing 0 to 6.54 mass% silicone, measured under temperature conditions of 25° C., 50° C., and 75° C. Fig. 7(b) is a graph enlarging the range of integrated intensity ratios of 0 to 0.4 in Fig. 7(a), and includes a straight line showing 0.351, which is the static friction coefficient of ETFE measured under a temperature condition of 25° C. [Figure 8]Fig. 8(a) is a graph showing the relationship between the peak height ratio of peak A2 and the surface static friction coefficient of polyethylene containing 0 to 6.54 mass% silicone, measured under temperature conditions of 25° C., 50° C., and 75° C. Fig. 8(b) is a graph enlarging the range of peak height ratios of 0 to 0.08 in Fig. 8(a), and includes a straight line showing 0.351, which is the static friction coefficient of ETFE, measured under a temperature condition of 25° C. [Figure 9] Fig. 9(a) is a graph showing the relationship between the integrated intensity ratio of peak A2 and the static friction coefficient of the surface of polyethylene containing 0 to 6.54 mass% silicone, measured under temperature conditions of 25° C., 50° C., and 75° C. Fig. 9(b) is a graph enlarging the range of integrated intensity ratios of 0 to 0.08 in Fig. 9(a), and includes a straight line showing 0.351, which is the static friction coefficient of ETFE measured under a temperature condition of 25° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Embodiment] (Quality control method for polymer materials) Polymer materials such as polyester elastomers that contain silicone as a lubricant have excellent surface slip properties and can be used, for example, as insulating materials for cables or tubes used in factory automation (FA), FA robots, medical ultrasound probes, etc.
[0016] According to the quality control method for a polymer material of this embodiment, Raman scattering measurement can be used to evaluate the surface slipperiness in a non-destructive, non-contact manner while maintaining the original state of the polymer material.
[0017] The quality control method for a polymeric material according to the present embodiment includes, for example, a measurement step of irradiating a polymeric material containing silicone as a lubricant with a laser and measuring a Raman spectrum, and an evaluation step of evaluating the lubricity of the surface of the polymeric material based on the intensity of a peak in the Raman spectrum that is attributable to molecular vibration derived from silicone. Here, the intensity of the peak in the Raman spectrum in the present embodiment means the peak height or integrated intensity.
[0018] The slipperiness of the surface of a polymeric material depends on the concentration of silicone, and the intensity of the peaks attributable to molecular vibrations derived from silicone in the Raman spectrum changes depending on the silicone content of the polymeric material, so the slipperiness of the surface of the polymeric material can be evaluated based on this intensity. In particular, the peak attributable to the Si-O stretching vibration of silicone (referred to as the first peak) and the peak attributable to the C-Si-C stretching vibration of silicone (referred to as the second peak) are easy to read the change in intensity depending on the silicone content of the polymeric material, so in the above evaluation step, it is preferable to evaluate the slipperiness of the surface of the polymeric material based on at least one of the intensity of the first peak and the intensity of the second peak.
[0019] The first peak is at 460 cm in the Raman spectrum. -1 More than 520cm -1 The second peak is at 700 cm in the Raman spectrum. -1 More than 720cm -1 The peaks have the maximum intensity within the following range: Note that the positions of the first and second peaks may shift within the above wavenumber range depending on factors such as the temperature of the polymer material during measurement.
[0020] In addition, if the polymeric material contains a contaminant containing Si, such as mud, the intensity of the first peak or the second peak increases due to the Si contained in the contaminant, and the slipperiness of the surface of the polymeric material may not be accurately evaluated. Even in this case, since there is little possibility that both the first peak and the second peak will change depending on the amount of Si contained in the contaminant, the slipperiness of the surface of the polymeric material according to the silicone content can be accurately evaluated by performing an evaluation based on both the first peak and the second peak.
[0021] Furthermore, by investigating in advance the correlation between the intensity of the peaks attributable to molecular vibrations derived from silicone, such as Si-O stretching vibration and C-Si-C stretching vibration, and the concentration of silicone in the polymer material, it is also possible to determine the specific concentration of silicone in the polymer material from the intensity of the peaks attributable to molecular vibrations derived from silicone.
[0022] Furthermore, when the polymeric material is polyethylene, in the above evaluation step, among the peaks attributable to molecular vibrations originating from the polyethylene base material, for example, a peak attributable to the CH2 rolling vibration of polyethylene (referred to as the third peak) can be used as a criterion for the intensities of the first and second peaks. That is, the slipperiness of the surface of the polymeric material can be evaluated based on at least one of the ratio of the intensity of the first peak to the intensity of the third peak in the Raman spectrum and the ratio of the intensity of the second peak to the intensity of the third peak. The third peak is located at 1150 cm -1 More than 1200cm -1 Maximum strength is achieved within the following range.
[0023] Specifically, for example, when evaluating the slipperiness of the surface of a polymeric material based on the intensity of the first peak, the slipperiness of the surface of the polymeric material can be evaluated based on at least one of the results of whether or not the ratio of the peak height of the first peak to the peak height of the third peak is 0.043 or more, and whether or not the ratio of the integrated intensity of the first peak to the integrated intensity of the third peak is 0.1 or more.
[0024] The inventors have confirmed that when the ratio of the peak height of the first peak to the peak height of the third peak is 0.043 or more, or when the ratio of the integrated intensity of the first peak to the integrated intensity of the third peak is 0.1 or more, the static friction coefficient of the surface of polyethylene (25 to 50°C) as a polymer material is equal to or less than the static friction coefficient of the surface of ETFE (25°C), thereby exhibiting excellent slip properties.
[0025] In addition, when evaluating the slipperiness of the surface of a polymeric material based on the intensity of the second peak, the slipperiness of the surface of the polymeric material can be evaluated based on at least one of the results of whether the ratio of the peak height of the second peak to the peak height of the third peak is 0.014 or more and whether the ratio of the integrated intensity of the second peak to the integrated intensity of the third peak is 0.011 or more.
[0026] The inventors have confirmed that when the ratio of the peak height of the second peak to the peak height of the third peak is 0.014 or more, or when the ratio of the integrated intensity of the second peak to the integrated intensity of the third peak is 0.011 or more, the static friction coefficient of the surface of polyethylene (25 to 50°C) as a polymer material is equal to or less than the static friction coefficient of the surface of ETFE (25°C), thereby exhibiting excellent slip properties.
[0027] Here, the integrated intensity and peak height of the first to third peaks are calculated using a peak profile obtained by fitting analysis using statistical distribution functions such as a Pseudo-Voigt function, a Lorentz function, and a Gauss distribution function, and are obtained after background correction of the peak profile. The background correction is performed to remove the influence of background thought to be caused by unavoidable light such as generated fluorescence, Rayleigh and Mie scattered light originating from the irradiated laser light, and disturbing light other than the irradiated laser light, which is not caused by the molecular structure of the polymer material and silicone, and is performed by subtracting a background profile (baseline) obtained by fitting analysis using a polynomial function, a spline function, etc. from the above-mentioned peak profile. In addition, the integral range when obtaining the integrated intensity of the first to third peaks is the range between the two intersection points of the above-mentioned peak profile and the background profile.
[0028] The ratio of the peak height of the first peak to the peak height of the third peak, the ratio of the integrated intensity of the first peak to the integrated intensity of the third peak, the ratio of the peak height of the second peak to the peak height of the third peak, and the ratio of the integrated intensity of the second peak to the integrated intensity of the third peak each reach their upper limit when silicone is added to the polymer material up to the limit.
[0029] In the Raman scattering measurement in the quality control method of the polymer material according to the present embodiment, the spot diameter of the laser irradiated on the surface of the polymer material is the measurement area, so that evaluation can be performed within a micro area with a diameter of 1 μm or less (for example, 0.4 to 1.0 μm). That is, not only average information on the magnitude of the silicone concentration of the polymer material, but also information for each micro area can be obtained. Therefore, for example, the disproportionation state accompanying the aggregation of silicone in the polymer material can be clarified, and the quality of the polymer material can be controlled to a higher degree. Note that the aforementioned value is not the limit value for the laser spot diameter. In principle, the laser spot diameter is determined by the wavelength of the laser light source and the numerical aperture of the objective lens. Therefore, when a Raman spectroscopic analysis is performed on the polymer material according to the present embodiment using a laser with a shorter wavelength and an objective lens with a larger numerical aperture, it becomes possible to measure even smaller micro areas of less than 0.4 μm.
[0030] (polymer material) According to the present embodiment, a polymer material having excellent surface slipperiness can be provided by selecting a polymer material having excellent surface slipperiness from polymer materials whose surface slipperiness has been evaluated by the above-mentioned quality control method for polymer materials.
[0031] The polymeric material according to the present embodiment is, for example, a polymeric material made of polyethylene containing silicone as a lubricant, and satisfies at least one of the following conditions: a first condition that the ratio of the peak height of the first peak to the peak height of the third peak in a Raman spectrum obtained by irradiating a laser is 0.043 or more; a second condition that the ratio of the integrated intensity of the first peak to the integrated intensity of the third peak is 0.1 or more; a third condition that the ratio of the peak height of the second peak to the peak height of the third peak is 0.014 or more; and a fourth condition that the ratio of the integrated intensity of the second peak to the integrated intensity of the third peak is 0.011 or more.
[0032] (Quality control method for cables and tubes) According to this embodiment, as a quality control method for a cable or tube having an insulation made of a polymeric material containing silicone as a lubricant, a method for evaluating the lubricity of the surface of the insulation can be provided by the above-mentioned quality control method for the polymeric material.
[0033] According to this cable or tube quality control method, it is possible to control the quality of cables or tubes for which surface smoothness is important, such as cables or tubes used in FA, FA robots, medical ultrasound probes, etc.
[0034] 1 is a radial cross-sectional view of a cable 1 for an FA robot, which is an example of a cable according to the present embodiment. The cable 1 includes a linear conductor 10 covered with a plurality of insulators 11, a pressure winding tape 12 wound around the conductor 10 covered with a bundle of insulators 11, a braided shield 13 provided around the pressure winding tape 12, and a sheath 14 provided around the braided shield 13.
[0035] The conductor 10 is made of a conductor such as copper. The number of conductors 10 included in the cable 1 is not particularly limited and is set appropriately depending on the application of the cable 1, etc. As described above, the insulator 11 is made of a polymer material containing silicone as a lubricant. The pressure winding tape 12 is made of a resin tape or the like. The braided shield 13 is made of a braided conductor wire or the like. The sheath 14 is made of polyvinyl chloride (PVC) or the like.
[0036] If the surface of the insulator 11 has excellent slipperiness, the insulator 11 can move easily inside the cable 1, thereby increasing the resistance of the insulator 11 to bending and twisting of the cable 1 and increasing the flexibility of the cable 1.
[0037] When diagnosing an insulator exposed on the surface of a cable or tube (for example, the insulator 11 exposed from the end of the cable 1), the cable or tube can be set in the Raman scattering measurement device as is and the measurement can be performed non-destructively. When diagnosing an insulator not exposed on the surface of a cable or tube, for example, the cable or tube is cut open and the measurement is performed.
[0038] In addition, by using a gun-type Raman scattering measurement device in which the laser irradiation part and the scattered light receiving part can be freely moved, it is possible to measure cables or tubes in their original state, even if the cables or tubes are difficult to measure using normal measurement devices, such as long, unprocessed cables or tubes.
[0039] (cable or tube) According to this embodiment, it is possible to provide a cable or tube having an insulator made of the above-mentioned polymer material and having an excellent surface slipperiness of the insulator. This cable or tube can be obtained by selecting a cable or tube having an excellent surface slipperiness of the insulator from cables or tubes whose surface slipperiness of the insulator has been evaluated by the above-mentioned cable or tube quality control method. Also, this cable or tube can be obtained by forming an insulator using a polymer material having an excellent surface slipperiness selected from polymer materials whose surface slipperiness has been evaluated by the above-mentioned polymer material quality control method.
[0040] The cable or tube of this embodiment is provided with an insulator made of a polymeric material, for example, polyethylene containing silicone as a lubricant, and satisfies at least one of the following conditions: a first condition that in a Raman spectrum obtained by irradiating a laser, the ratio of the peak height of the first peak to the peak height of the third peak is 0.043 or more; a second condition that the ratio of the integrated intensity of the first peak to the integrated intensity of the third peak is 0.1 or more; a third condition that the ratio of the peak height of the second peak to the peak height of the third peak is 0.014 or more; and a fourth condition that the ratio of the integrated intensity of the second peak to the integrated intensity of the third peak is 0.011 or more.
[0041] (Devices and systems equipped with cables or tubes) According to the present embodiment, it is possible to provide devices and systems such as FA, FA robots, and medical ultrasonic probes, which are provided with the above-mentioned cable or tube having an insulating surface with excellent slipperiness.
[0042] (Method of producing resin composition) According to an embodiment of the present invention, a resin composition can be produced by using a polymer material whose quality has been controlled by the above-mentioned quality control method for a polymer material. According to this method for producing a resin composition, a polymer material having excellent surface slip properties can be selected and used as a material for the resin composition.
[0043] Here, the form of the resin composition is not particularly limited as long as it contains a polymer material, and can be applied to, for example, fibers made of a polymer material woven into fibers made of thread-like materials processed and shaped from transition elements, precious metals such as gold, silver, and platinum, and carbon, or to a film made of a polymer material laminated on a base material made of a material with a large friction coefficient, such as ceramics or metal materials that are subject to significant wear during sliding.
[0044] (Effects of the embodiment) According to the above embodiment, by using Raman scattering measurement, it is possible to evaluate the slipperiness of the surface of a polymer material containing silicone as a lubricant and to control its quality. In addition, it is possible to evaluate the slipperiness of the surface of an insulator made of a polymer material containing silicone as a lubricant, such as a cable or tube, and to control its quality. In addition, it is possible to manufacture a resin composition containing a polymer material having excellent surface slipperiness by utilizing this quality control method for polymer materials.
[0045] Furthermore, by carrying out quality control of this polymer material and cable or tube, it is possible to provide a polymer material with excellent surface slipperiness, a cable or tube having an insulator with excellent surface slipperiness, and even factory automation or a factory automation robot equipped with this cable or tube.
[0046] In addition, the quality control method for polymer materials, the quality control method for cables or tubes, and the manufacturing method for resin compositions according to the above-mentioned embodiments can also be applied to material development using materials informatics (MI), which analyzes data using machine learning, artificial intelligence (AI), etc.
[0047] Furthermore, similarly to the quality control method for polymeric materials according to the above-described embodiment, Raman scattering measurement can also be used to control the quality of polymeric materials to which microparticles made of fluororesins such as PTFE, or microparticles made of inorganic substances such as oxides and metals, have been added and dispersed, or of silicone slipping layers such as silicone rubber in which microparticles containing Si have been dispersed. EXAMPLES
[0048] Polyethylene was prepared as a polymeric material containing silicone as a lubricant and processed into a sheet, and Raman scattering measurements were performed. The Raman scattering measurements were performed using Nanophoton's RAMANforce Standard VIS-NIR-HS under the following measurement conditions: laser wavelength 532 nm, spectrometer entrance slit width 50 μm, diffraction grating groove count 300 gr / mm, ND filter laser maximum light amount to attenuated light amount ratio (attenuation ratio) 250 / 255, objective lens magnification, numerical aperture (NA), and theoretical measurement diameter 5 times, 0.15, and 2.2 μm, respectively, and counting time 1 second × 20 cycles. The Raman scattering measurements were performed under the following conditions: temperature 20°C (average value of two-point measurements in the analysis room), humidity 28 RH% (average value of three-point measurements in the analysis room), and atmospheric pressure (so-called atmospheric pressure).
[0049] 2 is a graph showing the Raman spectra of polyethylene that does not contain silicone and polyethylene that contains silicone added at 0.99 to 6.54 mass %. -1 More than 520cm -1 The peak A1 with the maximum intensity in the following range is a peak assigned to the Si-O stretching vibration of silicone, and is located at 700 cm -1 More than 720cm -1 The peak A2 with the maximum intensity in the following range is a peak assigned to the C-Si-C stretching vibration of silicone, and has a peak at 1150 cm -1 More than 1200cm -1 Peak A3, which has the maximum intensity within the following range, is the peak assigned to the CH2 rolling vibration of polyethylene.
[0050] Figure 3(a) is a graph showing an enlargement of the vicinity of peak A1 and peak A2 in the Raman spectrum shown in Figure 2. As shown in Figures 2 and 3(a), the intensity of both peak A1 attributed to the Si-O stretching vibration of silicone and peak A2 attributed to the C-Si-C stretching vibration of silicone increases with an increase in the concentration of silicone added. Figure 3(b) is a graph showing an enlargement of the vicinity of peak A3 in the Raman spectrum shown in Figure 2.
[0051] Fig. 4(a) is a graph showing the relationship between the ratio of the peak height of peak A1 to the peak height of peak A3 (peak height ratio) and the concentration of silicone added. Fig. 4(b) is a graph showing the relationship between the ratio of the integrated intensity of peak A1 to the integrated intensity of peak A3 (integral intensity ratio) and the concentration of silicone added.
[0052] Table 1 below shows the peak height ratio and integrated intensity ratio of peak A1 for each concentration of silicone added, which correspond to the numerical values of each plot point in Figures 4(a) and (b), as well as the peak height and integrated intensity of peak A1 and the peak height and integrated intensity of peak A3 for each concentration of silicone added, which were used to calculate these ratios.
[0053] [Table 1]
[0054] Fig. 5(a) is a graph showing the relationship between the ratio of the peak height of peak A2 to the peak height of peak A3 (peak height ratio) and the concentration of silicone added. Fig. 5(b) is a graph showing the relationship between the ratio of the integrated intensity of peak A2 to the integrated intensity of peak A3 (integral intensity ratio) and the concentration of silicone added.
[0055] Table 2 below shows the peak height ratio and integrated intensity ratio of peak A2 for each concentration of silicone added, which correspond to the numerical values of each plot point in Figures 5(a) and (b), as well as the peak height and integrated intensity of peak A2 and the peak height and integrated intensity of peak A3 for each concentration of silicone added, which were used to calculate these ratios.
[0056] [Table 2]
[0057] FIG. 6(a) is a graph showing the relationship between the peak height ratio of peak A1 and the surface static friction coefficient of polyethylene containing 0 to 6.54 mass % silicone, measured under temperature conditions of 25°C, 50°C, and 75°C.
[0058] FIG. 7(a) is a graph showing the relationship between the integrated intensity ratio of peak A1 and the surface static friction coefficient of polyethylene containing 0 to 6.54 mass % silicone, measured under temperature conditions of 25°C, 50°C, and 75°C.
[0059] FIG. 8(a) is a graph showing the relationship between the peak height ratio of peak A2 and the surface static friction coefficient of polyethylene containing 0 to 6.54 mass % silicone, measured under temperature conditions of 25°C, 50°C, and 75°C.
[0060] FIG. 9(a) is a graph showing the relationship between the integrated intensity ratio of peak A2 and the surface static friction coefficient of polyethylene containing 0 to 6.54 mass % silicone, measured under temperature conditions of 25° C., 50° C., and 75° C.
[0061] Here, the method of measuring the static friction coefficients in Fig. 6(a), Fig. 7(a), Fig. 8(a), and Fig. 9(a) will be described. The static friction coefficients were measured using a friction and wear tester based on Orientec's "EMF-3-F" in accordance with the test method compliant with the Japanese Industrial Standard JIS K 7218. The measurement format was ring-on-ring (circular sliding with ring-shaped samples in contact with each other), and the radius "r" of the ring-shaped sample was 11.4 mm. The measurement conditions were a load "W" of 0.8 kgw, a rotational peripheral speed of 10 mm / s, and a test time of 1 min.
[0062] Then, "F" (torque) was measured at a point where the distance "R" from the center of the ring-shaped sample was 100 mm, and the friction coefficient when the maximum force F (maximum torque) was measured during the test time was defined as the "static friction coefficient μ." The calculation formula used to derive the static friction coefficient μ is shown below as Equation 1.
[0063]
number
[0064] Table 3 below shows the relationship between the peak height ratio and integrated intensity ratio of peak A1, the peak height ratio and integrated intensity ratio of peak A2, and the static friction coefficient measured under temperature conditions of 25°C, 50°C, and 75°C, which relate to the numerical values of each plot point in Figures 6(a), 7(a), 8(a), and 9(a).
[0065] [Table 3]
[0066] Figure 6(b) is a graph that expands the range of peak height ratios of 0 to 0.2 in Figure 6(a), and includes a straight line indicating 0.351, which is the static friction coefficient of ETFE measured at a temperature of 25°C. As shown in Figure 6(b), the static friction coefficient of silicone-containing polyethylene decreases as the temperature decreases, and when the peak height ratio of peak A1 is approximately 0.043 or more, the static friction coefficient of the silicone-containing polyethylene at 50°C or less becomes equal to or less than the static friction coefficient of ETFE at 25°C.
[0067] Figure 7(b) is a graph that expands the range of integrated intensity ratios of 0 to 0.4 in Figure 7(a), and includes a straight line indicating 0.351, which is the static friction coefficient of ETFE measured at a temperature of 25°C. As shown in Figure 7(b), the static friction coefficient of silicone-containing polyethylene decreases as the temperature decreases, and when the integrated intensity ratio of peak A1 is approximately 0.1 or more, the static friction coefficient of silicone-containing polyethylene at 50°C or less becomes equal to or less than the static friction coefficient of ETFE at 25°C.
[0068] Figure 8(b) is a graph in which the range of peak height ratios of 0 to 0.08 in Figure 8(a) is enlarged, and includes a straight line indicating 0.351, which is the static friction coefficient of ETFE measured at a temperature of 25°C. As shown in Figure 8(b), the static friction coefficient of silicone-containing polyethylene decreases as the temperature decreases, and when the peak height ratio of peak A2 is approximately 0.014 or more, the static friction coefficient of the silicone-containing polyethylene at 50°C or less becomes equal to or less than the static friction coefficient of ETFE at 25°C.
[0069] Figure 9(b) is a graph that expands the range of integrated intensity ratios of 0 to 0.08 in Figure 9(a), and includes a straight line indicating 0.351, which is the static friction coefficient of ETFE measured at a temperature of 25°C. As shown in Figure 9(b), the static friction coefficient of silicone-containing polyethylene decreases as the temperature decreases, and when the integrated intensity ratio of peak A2 is approximately 0.011 or more, the static friction coefficient of silicone-containing polyethylene at 50°C or less becomes equal to or less than the static friction coefficient of ETFE at 25°C.
[0070] (Summary of the embodiment) Next, the technical ideas grasped from the above-described embodiment will be described by using the reference numerals and the like in the embodiment. However, the reference numerals and the like in the following description do not limit the components in the claims to the members and the like specifically shown in the embodiment.
[0071] [1] A quality control method for a polymeric material, comprising: a measuring step of irradiating a polymeric material containing silicone as a lubricant with a laser and measuring the Raman spectrum; and an evaluation step of evaluating the lubricity of the surface of the polymeric material based on the intensity of a peak in the Raman spectrum that is attributable to molecular vibrations derived from the silicone.
[0072] [2] The quality control method for a polymer material according to the above-mentioned [1], wherein in the evaluation step, the slipperiness of the surface of the polymer material is evaluated based on at least one of the intensity of a first peak in the Raman spectrum, which is attributed to the Si-O stretching vibration of the silicone, and the intensity of a second peak in the Raman spectrum, which is attributed to the C-Si-C stretching vibration of the silicone.
[0073] [3] The quality control method for a polymeric material described in [2] above, wherein the polymeric material is polyethylene, and in the evaluation step, the slipperiness of the surface of the polymeric material is evaluated based on at least one of the ratio of the intensity of the first peak to the intensity of the third peak assigned to the CH2 rolling vibration of the polyethylene in the Raman spectrum and the ratio of the intensity of the second peak to the intensity of the third peak.
[0074] [4] The first peak is 460 cm in the Raman spectrum. -1 More than 520cm -1 and the second peak is a peak having a maximum intensity within the range of 700 cm or less in the Raman spectrum. -1 More than 720cm -1 and the third peak is a peak having a maximum intensity within the range of 1150 cm -1 More than 1200cm -1 The quality control method for a polymer material according to the above [3], wherein the peak has a maximum intensity within the following range.
[0075] [5] A quality control method for a polymer material described in [3] or [4] above, wherein in the evaluation step, the slipperiness of the surface of the polymer material is evaluated based on at least one of the results of whether or not the ratio of the peak height of the first peak to the peak height of the third peak is 0.043 or more and whether or not the ratio of the integrated intensity of the first peak to the integrated intensity of the third peak is 0.1 or more.
[0076] [6] A quality control method for a polymer material described in any one of [3] to [5] above, wherein in the evaluation step, the slipperiness of the surface of the polymer material is evaluated based on at least one of the results of whether or not the ratio of the peak height of the second peak to the peak height of the third peak is 0.014 or more and whether or not the ratio of the integrated intensity of the second peak to the integrated intensity of the third peak is 0.011 or more.
[0077] [7] A quality control method for a cable (1) or a tube having an insulation (11) made of a polymeric material containing silicone as a lubricant, comprising evaluating the lubricity of a surface of the insulation (11) by the quality control method for a polymeric material according to any one of the above items [1] to [6].
[0078] [8] A method for producing a resin composition, comprising forming a resin composition using a polymer material containing silicone as a lubricant, the polymer material having a surface slipperiness evaluated by the quality control method for polymer material according to any one of [1] to [6] above.
[0079] [9] A polymeric material made of polyethylene containing silicone as a lubricant, which satisfies at least one of the following conditions: a first condition that a ratio of a peak height of a first peak attributed to Si-O stretching vibration of the silicone to a peak height of a third peak attributed to CH rolling vibration of the polyethylene in a Raman spectrum obtained by irradiating a laser is 0.043 or more; a second condition that a ratio of an integrated intensity of the first peak to an integrated intensity of the third peak is 0.1 or more; a third condition that a ratio of a peak height of a second peak attributed to C-Si-C stretching vibration of the silicone to a peak height of the third peak is 0.014 or more; and a fourth condition that a ratio of an integrated intensity of the second peak to an integrated intensity of the third peak is 0.011 or more.
[0080]
[10] A cable (1) or tube having an insulator (11) made of the polymer material described in [9] above.
[0081]
[11] A factory automation or a factory automation robot comprising the cable (1) or tube described in
[10] above.
[0082] Although the embodiment and examples of the present invention have been described above, the present invention is not limited to the above embodiment and examples, and various modifications can be made within the scope of the gist of the invention. Furthermore, the above-described embodiment and examples do not limit the invention according to the claims. Furthermore, it should be noted that not all of the combinations of features described in the embodiment and examples are essential to the means for solving the problems of the invention. [Explanation of symbols]
[0083] 1 Cable 10 Conductors 11 Insulators 12. Holding Tape 13 Braided Shield 14 Sheath
Claims
1. a measuring step of irradiating a polymer material made of polyethylene containing silicone as a lubricant with a laser and measuring a Raman spectrum; an evaluation step of evaluating the slipperiness of the surface of the polymer material based on the intensity of a first peak attributable to the Si-O stretching vibration of the silicone and the intensity of a third peak attributable to the CH 2 rolling vibration of the polyethylene in the Raman spectrum; Including, In the evaluation step, the slipperiness of the surface of the polymer material is evaluated based on at least one of the results of whether or not a ratio of the peak height of the first peak to the peak height of the third peak is 0.043 or more and whether or not a ratio of the integrated intensity of the first peak to the integrated intensity of the third peak is 0.1 or more. Quality control methods for polymeric materials.
2. The first peak is at 460 cm in the Raman spectrum. -1 520cm or more -1 The peak with the maximum intensity is within the following range: The third peak is at 1150 cm in the Raman spectrum. -1 More than 1200cm -1 The peak with the maximum intensity is within the following range: The method for quality control of a polymeric material according to claim 1.
3. A measuring step of irradiating a polymer material made of polyethylene containing silicone as a lubricant with a laser and measuring a Raman spectrum; an evaluation step of evaluating the slipperiness of the surface of the polymer material based on the intensity of a second peak attributable to the C-Si-C stretching vibration of the silicone and the intensity of a third peak attributable to the CH 2 rolling vibration of the polyethylene in the Raman spectrum; Including, In the evaluation step, the slipperiness of the surface of the polymer material is evaluated based on at least one of the results of whether or not a ratio of the peak height of the second peak to the peak height of the third peak is 0.014 or more and whether or not a ratio of the integrated intensity of the second peak to the integrated intensity of the third peak is 0.011 or more. Quality control methods for polymeric materials.
4. The second peak is a peak having a maximum intensity in the range of 700 cm −1 to 720 cm −1 in the Raman spectrum, the third peak is a peak having a maximum intensity in the range of 1150 cm −1 to 1200 cm −1 in the Raman spectrum; The method for quality control of a polymeric material according to claim 3.
5. A quality control method for a cable or tube having an insulation made of a polymeric material consisting of polyethylene containing silicone as a lubricant, comprising the steps of: The slipperiness of the surface of the insulator is evaluated by the quality control method for a polymer material according to any one of claims 1 to 4. A method for quality control of cables or tubes.
6. A step of evaluating the slipperiness of a surface by the quality control method for a polymer material according to any one of claims 1 to 4, and forming a resin composition using a polymer material made of polyethylene containing silicone as a lubricant. A method for producing a resin composition.
Citation Information
Patent Citations
Lubricant composition for use at high temperature
JP1985141796A
Thresher
JP1990057117A
Lubricant composition for warm and hot forging
JP1991250098A
Insulated wire
JP2000357418A
Organopolysiloxane-siliceous material complex and application
JP2002146190A