Active energy ray curable composition and laminate using same
The active energy ray-curable composition with polyfunctional urethane (meth)acrylate and fine resin particles addresses the matte property and environmental issues of solvent-based and solvent-free varnishes, offering a cured layer with enhanced workability and aesthetic matte finish.
Patent Information
- Application Number
- JP2021062681
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-01
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Existing solvent-based matte coating varnishes for paper carton packages lack sufficient matte properties, workability, and environmental friendliness, while solvent-free alternatives do not meet the desired matte properties, and solvent-containing compositions affect workability and the environment.
An active energy ray-curable composition comprising polyfunctional urethane (meth)acrylate, monofunctional ethylenically unsaturated monomer, and fine resin particles, with specific molecular weight and viscosity ranges, and minimal organic solvent content, forming a cured layer with excellent substrate adhesion and matte properties.
The composition achieves a cured layer with excellent workability, environmental friendliness, and suitable matte properties, providing improved substrate adhesion and aesthetic appearance.
Smart Images

Figure 0007589626000001 
Figure 0007589626000002 
Figure 0007589626000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an active energy ray-curable composition and a laminate using the same. [Background technology]
[0002] In recent years, in the field of packaging using paper substrates (also called paper containers), research has been actively conducted on printing color inks on various substrates and then applying a coating varnish to them in order to impart durability and aesthetic appeal to the printed matter. With regard to paper container packaging, when it is displayed in stores after printing, there are cases where glossiness is required for aesthetic reasons, and cases where a matte finish is required. In particular, the demand for printed matter with a matte finish has been increasing in recent years.
[0003] Conventionally, solvent-based matte coating varnishes containing resin, matting agent, and solvent have been used for matte coating varnishes for paper packaging, usually for the purpose of imparting a high-class feel through high matte properties. In general, solvent-based matte coating varnishes have a high matte effect, but are inferior in workability and environmental friendliness, because the volume of the varnish film is reduced by the evaporation of the solvent components from the varnish film during the drying process after printing, and the matting agent is oriented on the surface of the varnish film. Furthermore, with solvent-based matte coating varnishes, the solid content of the ink changes due to the evaporation of the solvent components during printing, which causes concerns about viscosity changes during printing and the risk of environmental pollution due to the evaporated solvent.
[0004] In recent years, solvent-free activated energy ray-curable matte coating varnishes that improve workability and environmental friendliness have been developed. For example, Patent Document 1 proposes an activated energy ray-curable coating varnish that contains a photopolymerizable acrylate monomer, resin beads, and a photoinitiator, in which the resin beads are made of resin beads having two types of average particle diameters, and that produces printed matter with excellent matte finish and abrasion resistance.
[0005] Furthermore, Patent Document 2 proposes a solventless active energy ray-curable composition containing an active energy ray-curable compound, an inorganic matting agent, and an aluminum chelate compound, wherein the inorganic matting agent is silica having an average particle size of 1 to 15 μm, the thixotropic coefficient at 25° C. is 2 or less, and the viscosity at the coating environment temperature is 1000 mPa s or less.
[0006] Patent Document 3 proposes an active energy ray-curable resin composition comprising a urethane (meth)acrylate compound obtained by reacting a polyol compound, a hydroxyl group-containing (meth)acrylate compound, and a polyvalent isocyanate compound, and an organic filler, wherein the polyol compound comprises a polyol compound having a weight average molecular weight of 60 to 300 and a polyol compound having a weight average molecular weight of 3,000 to 20,000, and the organic filler is a combination of a polyurethane filler and a polyethylene filler.
[0007] However, while the technologies disclosed in Patent Documents 1 and 2 above are solvent-free and have excellent workability and environmental friendliness, they do not have sufficient matte properties compared to the solvent-based matte coating varnishes that have traditionally been mainstream, and issues remain for use in paper container packaging, where high matte properties are required in recent years.
[0008] In addition, the above-mentioned Patent Document 3 is considered to have a sufficient matte finish from the viewpoint of cosmetic appearance, but on the other hand, the composition contains a solvent to impart coatability, and is inferior in terms of workability and environmental friendliness. There were still issues to be addressed. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2010-241954 A [Patent Document 2] JP 2002-121210 A [Patent Document 3] JP 2015-101609 A Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide an active energy ray-curable composition for forming a cured layer which is excellent in workability, environmental friendliness, and suitability for printing and other coating processes, and which, when printed and cured, has excellent adhesion to a substrate and matte properties (beautiful cosmetic properties). [Means for solving the problem]
[0011] As a result of extensive research into the above-mentioned problems, the inventors have found that the problems can be solved by using the active energy ray-curable composition described below, and have thus completed the present invention.
[0012] That is, the present invention provides an active energy ray-curable composition containing a polyfunctional urethane (meth)acrylate, a monofunctional ethylenically unsaturated monomer, and resin fine particles, The weight average molecular weight of the polyfunctional urethane (meth)acrylate is 1,000 to 7,000; The composition does not contain an organic solvent or contains an organic solvent in an amount of 5% by mass or less of the total mass of the composition; The present invention relates to an active energy ray-curable composition, wherein the composition has a viscosity at 25° C. of 250 to 2500 mPa·s.
[0013] The present invention also relates to the above active energy ray-curable composition, which further contains a photopolymerization initiator.
[0014] The present invention also relates to the above active energy ray-curable composition, wherein the polyfunctional urethane (meth)acrylate has a structural unit derived from a polyether.
[0015] The present invention also relates to the above active energy ray-curable composition, wherein the monofunctional ethylenically unsaturated monomer contains a hydroxyalkyl (meth)acrylate.
[0016] The present invention also relates to the above active energy ray-curable composition, which has a viscosity at 25°C of 500 to 1500 mPa·s.
[0017] The present invention also relates to the above-mentioned active energy ray-curable composition, wherein the resin fine particles are urethane resin fine particles.
[0018] The present invention also relates to the above-mentioned active energy ray-curable composition for use on a paper substrate.
[0019] The present invention also relates to a laminate having, on a paper substrate, a printed layer and a cured layer formed from the above-mentioned active energy ray-curable composition. Effect of the Invention
[0020] The present invention makes it possible to provide an active energy ray-curable composition for forming a cured layer which is excellent in workability, environmental friendliness, and suitability for printing and other coating processes, and which, when printed and cured, is excellent in adhesion to a substrate and matte property (beautiful cosmetic properties). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The following describes in detail the embodiments of the present invention. However, the description of the components described below is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to these contents as long as it does not go beyond the gist of the present invention.
[0022] The active energy ray-curable composition of the present invention is an active energy ray-curable composition containing a polyfunctional urethane (meth)acrylate, a monofunctional ethylenically unsaturated monomer, resin fine particles, and, if necessary, a photopolymerization initiator, The weight average molecular weight of the polyfunctional urethane (meth)acrylate is 1,000 to 7,000; The composition does not contain an organic solvent or contains an organic solvent in an amount of 5% by mass or less of the total mass of the composition; The viscosity of the composition at 25° C. is 250 to 2500 mPa·s. When the weight-average molecular weight of the polyfunctional urethane (meth)acrylate is within this range, the surface tackiness, blocking resistance, crease cracking resistance, etc. are good, and when the organic solvent in the total mass of the composition is 5 mass% or less, the viscosity stability is good, and when the viscosity of the composition at 25° C. is 250 to 2500 mPa·s, the smoothness, penetration prevention properties, etc. are good, and the printability and film properties of the printed matter are improved.
[0023] In the following description, (meth)acrylic and (meth)acrylate respectively mean methacrylic and / or acrylic, and methacrylate and / or acrylate. In addition, (meth)acryloyl means methacryloyl and / or acryloyl. In addition, the active energy ray curable composition may be simply referred to as "composition", but these terms have the same meaning.
[0024] (Multifunctional urethane (meth)acrylate) The weight average molecular weight of the polyfunctional urethane (meth)acrylate used in the present invention is 1000 to 7000. The viscosity of the composition is appropriately maintained to improve the coating suitability, and the cured layer formed by the active energy ray curable resin composition is uniform without excessive penetration into the paper substrate. Furthermore, the hardness of the cured layer is appropriately maintained and it does not crack. Furthermore, the polyfunctionality provides good blocking resistance. The weight average molecular weight is preferably 1500 to 5000, more preferably 1500 to 3500, and even more preferably 2000 to 3000. The number of functional groups of the polyfunctional urethane (meth)acrylate is preferably 2 to 4, more preferably 2 to 3, and even more preferably 2. Here, the number of functional groups refers to the number of polymerizable (meth)acrylate groups and other unsaturated double bond groups.
[0025] The weight average molecular weight is a value measured by gel permeation chromatography, and can be measured, for example, by using a GPC (gel permeation chromatography) "Shodex GPC System-21" manufactured by Showa Denko KK GPC is a liquid chromatography that separates and quantifies substances dissolved in a solvent based on the difference in their molecular size, and tetrahydrofuran is preferably used as the solvent, and the weight average molecular weight is preferably determined in terms of polystyrene.
[0026] The glass transition temperature (Tg) of the polyfunctional urethane (meth)acrylate is preferably 0 to 50° C., more preferably 5 to 40° C., further preferably 10 to 35° C., and particularly preferably 15 to 30° C. The glass transition temperature is a value measured by a differential scanning calorimeter (DSC), and the midpoint between the endothermic start temperature and end temperature due to the glass transition in the DSC curve is defined as the glass transition temperature.
[0027] The polyfunctional urethane (meth)acrylate is preferably in the following form, for example, a polyol and These include those obtained by reacting an isocyanate group-containing urethane prepolymer obtained by reacting a polyisocyanate under conditions of excess isocyanate groups with a (meth)acrylate having a hydroxyl group, and those obtained by reacting a polyisocyanate with a (meth)acrylate having a hydroxyl group, etc. Alternatively, they can also be obtained by reacting a hydroxyl group-containing urethane prepolymer obtained by reacting a polyol with a polyisocyanate under conditions of excess hydroxyl groups with a (meth)acrylate having an isocyanate group.
[0028] The polyol, the hydroxyl group-containing (meth)acrylate, and the polyisocyanate will now be described.
[0029] <Polyol> The polyol may be a known one, and suitable examples thereof include polyether polyol, polyester polyol, polyolefin polyol (polybutadiene polyol, polyisoprene polyol), polycarbonate polyol, polysiloxane polyol, and (meth)acrylic polyol, and may have an aliphatic structure or an alicyclic structure. Among these, polyether polyol is preferred. When polyether polyol is used, the multifunctional urethane (meth)acrylate has a structural unit derived from polyether. The polyether polyol is preferably, for example, polytetramethylene glycol, polyethylene glycol, polypropylene glycol, polytrimethylene glycol, or a copolymer thereof. When the multifunctional urethane (meth)acrylate has a structural unit derived from polyether, the viscosity and coating suitability of the composition can be improved.
[0030] <Polyisocyanate> As the polyisocyanate, known ones can be used, and examples thereof include aromatic diisocyanates, aliphatic diisocyanates, and alicyclic diisocyanates. Examples of aromatic diisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, xylylene diisocyanate, and 2,6-diisocyanate-benzyl chloride. Examples of the aliphatic diisocyanate include butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of alicyclic diisocyanates include cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, dimeryl diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, and dimer diisocyanate in which the carboxy group of a dimer acid is converted into an isocyanate group. These may be trimers to form an isocyanurate ring structure. These polyisocyanates may be used alone or in combination of two or more. Among these, tolylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, hexamethylene diisocyanate, and isocyanurates of hexamethylene diisocyanate are preferred.
[0031] <Hydroxyl group-containing (meth)acrylate> Examples of hydroxyl group-containing (meth)acrylates include trimethylolpropane di(meth)acrylate, trimethylolethane di(meth)acrylate, and pentaerythritol tri(meth)acrylate. (meth)acrylate, dipentaerythritol penta(meth)acrylate, 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, (meth)acrylate Examples of the hydroxyl group-containing (meth)acrylic acid ester include 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, ethyl-α-(hydroxymethyl) (meth)acrylate, monofunctional glycerol (meth)acrylate, or (meth)acrylic acid esters having a hydroxyl group at the end obtained by ring-opening addition of these (meth)acrylates and ε-caprolactone lactone, and alkylene oxide-added (meth)acrylic acid esters obtained by repeatedly adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to the above-mentioned hydroxyl group-containing (meth)acrylates. Among these, those containing at least one selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are preferred.
[0032] <Monofunctional ethylenically unsaturated monomer> Examples of the monofunctional ethylenically unsaturated monomers used in the present invention include (alkyl)(meth)acrylates having 1 to 18 carbon atoms, such as methyl(meth)acrylate, ethyl(meth)acrylate, butyl(meth)acrylate, hexyl(meth)acrylate, octyl(meth)acrylate, dodecyl(meth)acrylate, and stearyl(meth)acrylate, and further include alkylphenols such as benzyl(meth)acrylate, butylphenol, octylphenol, nonylphenol, and dodecylphenol, (meth)acrylates of ethylene oxide adducts, isobornyl(meth)acrylate, cyclohexyl(meth)acrylate, tricyclodecane monomethylol(meth)acrylate, 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, hydroxypentyl(meth)acrylate, 2-hydroxypropyl ... 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-hydroxy-3-butoxypropyl (meth)acrylate, 2-hydroxy-3-methoxypropyl (meth)acrylate, diethylene glycol mono(meth)acrylate, triethylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, dipropylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, glycerin mono(meth)acrylate, acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, 2-(meth)acryloyloxypropyl phthalate, β-carboxyethyl (meth)acrylate, (meth)acrylic acid dimer, ω-carboxy-polycaprolactone mono(meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, N-vinylpyrrolidone, N-vinylformamide, (meth)acryloylmorpholine, and the like. Among them, it is preferable to include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc. The number of carbon atoms in the alkyl group is preferably 2 to 10 or 2 to 6, and more preferably 2 to 4. The monofunctional ethylenically unsaturated monomer has the effect of significantly reducing the viscosity of the active energy ray-curable composition and improving the smoothness of the coating film. The monofunctional ethylenically unsaturated monomer is preferably contained in an amount of 30 to 60 mass %, more preferably 35 to 55 mass %, and even more preferably 40 to 50 mass %, based on the total mass of the active energy ray-curable composition. The mass ratio of the polyfunctional urethane (meth)acrylate to the monofunctional ethylenically unsaturated monomer is preferably 10:90 to 40:60, and more preferably 15:85 to 30:70.The hydroxyalkyl (meth)acrylate is preferably contained in an amount of 70 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 85 to 100 mass%, based on the total mass of the monofunctional ethylenically unsaturated monomer.
[0033] <Difunctional ethylenically unsaturated monomer> The composition of the present invention is also preferably a case where it contains a bifunctional ethylenically unsaturated monomer. The bifunctional ethylenically unsaturated monomer is, for example, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, octanediol di(meth)acrylate and other alkylene glycol di(meth)acrylates, polyethylene glycol 200 di(meth)acrylate (numbers indicate molecular weight), polyethylene glycol 300 di(meth)acrylate, polyethylene glycol 400 di(meth)acrylate, polyethylene glycol 600 di(meth)acrylate, polyethylene glycol 1000 di(meth)acrylate and other polyethylene glycol di(meth)acrylates, as well as tetraethylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, etc., and is preferably one containing a polyether structure. The amount of the bifunctional ethylenically unsaturated monomer is preferably 15% by mass or less, more preferably 7% by mass or less, based on the total mass of the composition. The difunctional ethylenically unsaturated monomer does not include the above-mentioned polyfunctional urethane (meth)acrylate.
[0034] <Resin fine particles> In the present invention, the resin fine particles have a matte function. The resin fine particles preferably have an average particle diameter of 1 to 10 μm, more preferably 1.5 to 8 μm, further preferably 2 to 6 μm, and even more preferably 2 to 3 μm. The average particle diameter here refers to the volume average particle diameter measured by a laser diffraction method, and can be measured, for example, using a Microtrack Bell T330EXII. Specific examples of suitable resin particles include urethane resin particles, silicone resin particles, melamine resin particles, melamine-benzoguanamine resin particles, acrylic resin particles (e.g., polymethyl methacrylate resin particles), acrylic-styrene copolymer resin particles, polycarbonate resin particles, polyethylene resin particles, polystyrene resin particles, and benzoguanamine resin particles. These may be used alone or in combination of two or more. Among these, urethane resin particles are more preferred. The above resin particles may be used in combination of two or more as needed.
[0035] The resin fine particles are contained in an amount of preferably 15 to 35% by mass, more preferably 20 to 30% by mass, and even more preferably 23 to 27% by mass, based on the total mass of the composition. The glass transition temperature of the resin fine particles is preferably -30 to 40°C, more preferably -20 to 30°C, and even more preferably -15 to 25°C. The glass transition temperature is a value measured by a differential scanning calorimeter (DSC), and the midpoint between the endothermic start temperature and end temperature based on the glass transition in the DSC curve is taken as the glass transition temperature.
[0036] Specific examples of urethane resin microparticles include crosslinked urethane beads such as Art Pearl C-1000 transparent, Art Pearl C-600 transparent, Art Pearl C-400 transparent, Art Pearl C-800, Art Pearl MM-120T, Art Pearl JB-800T, Art Pearl JB-600T, Art Pearl P-800T, and Art Pearl P-400T (manufactured by Negami Chemical Industries Co., Ltd.).
[0037] Specific examples of silicone resin particles include KMP-594, KMP-597, and KMP- 598, KMP-600, KMP-601, KMP-602 (manufactured by Shin-Etsu Chemical Co., Ltd.), Trefil E-506S, EP-9215 (manufactured by Dow Corning Toray Co., Ltd.), etc.
[0038] Specific examples of melamine resin fine particles include Eposter SS, Eposter S, Eposter FS, Eposter S6, and Eposter S12 (manufactured by Nippon Shokubai Co., Ltd.). A specific example of the melamine-benzoguanamine resin fine particles is Eposter M30 (manufactured by Nippon Shokubai Co., Ltd.).
[0039] Specific examples of acrylic resin microparticles include Eposter MA1002, Eposter MA1004, Eposter MA1006, and Eposter MA1010 (manufactured by Nippon Shokubai Co., Ltd.), Tuftic FH-S005, Tuftic FH-S008, Tuftic FH-S010, Tuftic FH-S015, and Tuftic FH-S020 (manufactured by Toyobo Co., Ltd.), and Chemisnow M. X-80H3wT, MX-150, MX-180TA, MX-300, MX-500, MX-1000, MX-1500H, MX-2000, MX-3000 (manufactured by Soken Chemical Engineering Co., Ltd.), etc.
[0040] Specific examples of acrylic-styrene copolymer resin fine particles include Eposter MA2003 (manufactured by Nippon Shokubai Co., Ltd.), FS-102, FS-201, FS-301, MG-451, MG-351 (manufactured by Nippon Paint Industrial Coatings Co., Ltd.), and the like.
[0041] Specific examples of polycarbonate resin fine particles include fine particles described in JP-A-2014-125495, fine particles obtained by the production method described in JP-A-2011-26471, and fine particles obtained by the method described in JP-A-2001-213970.
[0042] Specific examples of polyethylene resin fine particles include Mipelon XM-220 and XM221U (manufactured by Mitsui Chemicals, Inc.), Flow Beads LE-1080 (manufactured by Sumitomo Seika Chemicals, Inc.), and the like. Specific examples of polystyrene-based fine particles include Chemisnow SX-130H, SX-350H, and SX-500H (manufactured by Soken Chemical & Engineering Co., Ltd.).
[0043] Specific examples of benzoguanamine resin fine particles include Eposter MS, Eposter M05, and Eposter L15 (manufactured by Nippon Shokubai Co., Ltd.).
[0044] <Photopolymerization initiator> The active energy ray curable composition of the present invention may contain a photopolymerization initiator. The photopolymerization initiator generates radicals by irradiation with active energy rays such as light, and initiates a crosslinking reaction and a polymerization reaction of the acrylate group of the polyfunctional urethane (meth)acrylate or the monofunctional ethylenically unsaturated monomer. Suitable examples of the photopolymerization initiator include acetophenone-based photopolymerization initiators, alkylphenone-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzophenone-based photopolymerization initiators, and acylphosphine oxide-based photopolymerization initiators. Among them, acetophenone-based photopolymerization initiators and acylphosphine oxide-based photopolymerization initiators are preferred. The photopolymerization initiator is preferably contained in an amount of 1 to 10% by mass, more preferably 2 to 7% by mass, and even more preferably 3 to 5% by mass in the total mass of the composition.
[0045] Examples of the acetophenone-based photopolymerization initiator include 4-phenoxydichloroacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 4-(2-hydroxyethoxy Examples of photopolymerization initiators include acetophenone-based photopolymerization initiators such as 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2,2-dimethoxy-2-phenylacetophenone, etc.
[0046] Examples of the alkylphenone photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and the like.
[0047] Examples of the benzoin-based photopolymerization initiator include benzoin, benzoin methyl ether, benzoin isoethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0048] Examples of the benzophenone-based photopolymerization initiator (d-1) include benzophenone, 4-methylbenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, methyl-o-benzoylbenzoate, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3-dimethyl-4-methoxybenzophenone, etc. Among these, 4-methylbenzophenone is preferred.
[0049] Examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-chlorothioxanthone, 2,4-dichlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, isopropylthioxanthone, and 2,4-diisopropylthioxanthone.
[0050] Examples of anthraquinone-based photopolymerization initiators include α-acyloxime ester, benzil, methylbenzoyl formate ("Biacure 55"), 2-ethylanthraquinone, and the like.
[0051] Examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyldiphenylphosphine oxide ("OmniradTPO"), bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide ("IRGACURE819"), and the like.
[0052] The photopolymerization initiators may be used alone or in combination of two or more.
[0053] <Organic solvent in the composition> In order to solve the problems of the present invention, it is essential that the composition does not contain an organic solvent or that the organic solvent content is 5% by mass or less of the total mass of the composition. It is preferably 3% by mass or less, and more preferably 1.5% by mass or less. This is because printability is improved within this range. Usable organic solvents include known solvents used in coating varnishes.
[0054] <Viscosity of Composition> The viscosity of the composition is 250 to 2500 mPa·s at 25°C, which solves the problem of the present invention. It is essential to determine the viscosity of the composition. If the viscosity is within the range, excessive penetration into paper substrates and the like after coating by printing or the like is suppressed. In addition, the surface of the cured layer becomes a uniform film, and no spots or the like occur. The viscosity referred to here is a measured value according to the method described in JIS K5600-2, and can be measured, for example, using a cone-plate type viscometer using a cone with a cone diameter of 35 mm and a cone angle of 2° at a shear rate of 100 per second in an environment of 25°C. The viscosity of the composition at 25°C is preferably 300 to 2000 mPa·s, and more preferably 500 to 1500 mPa·s.
[0055] (Additives) The active energy ray-curable composition of the present invention can appropriately contain known additives. For example, a leveling agent, a polymerization inhibitor, an ultraviolet absorber, a light stabilizer, a sensitizer, a curing agent, a plasticizer, a wetting agent, an adhesion aid, an antifoaming agent, an antistatic agent, etc. can be used, and there are no particular limitations.
[0056] (Production of active energy ray-curable composition) The active energy ray curable composition can be produced by stirring a polyfunctional urethane (meth)acrylate having a weight average molecular weight of 1000 to 7000, a monofunctional ethylenically unsaturated monomer, resin fine particles, and a photopolymerization initiator for about 30 minutes to 3 hours using a bladed stirrer (disper), etc. If mixing is difficult and the viscosity, etc., tends to become non-uniform, a roller mill, ball mill, pebble mill, attritor, sand mill, etc. may be used.
[0057] When the active energy ray-curable composition of the present invention contains air bubbles or unexpectedly large particles, these particles deteriorate the quality of the printed matter, and therefore it is preferable to remove them by filtration, etc. As the filter, a conventionally known filter can be used.
[0058] (Manufacture of laminates) The method for producing the laminate of the present invention is not particularly limited, but it is preferably produced by printing / coating the active energy ray-curable composition on a paper substrate or a film substrate and curing it. Note that a printed layer made of a printing ink composition may be formed on the substrate, and the active energy ray-curable composition of the present invention may be printed / coated on the printed layer and cured to form a laminate.
[0059] The printing / coating method of the active energy ray-curable composition is not particularly limited, and examples thereof include wet coating methods such as spraying, showering, dipping, flow coating, gravure printing, flexographic printing, rolling, spinning, dispenser, inkjet printing, and screen printing.
[0060] Examples of active energy rays include ultraviolet rays such as far ultraviolet rays, ultraviolet rays, and near ultraviolet rays. On the other hand, it is also possible to use electron beams or proton beams, in which case curing can be achieved without using a photopolymerization initiator, but curing by ultraviolet irradiation is preferred in terms of curing speed, availability of an irradiation device, cost, and the like.
[0061] The method of curing by ultraviolet irradiation uses a high-pressure mercury lamp, ultra-high-pressure mercury lamp, carbon arc lamp, metal halide lamp, xenon lamp, chemical lamp, electrodeless discharge lamp, LED, etc. that emits light in the 150 to 450 nm wavelength range, with an accumulated light quantity of 30 to 5000 mJ / cm. 2 , preferably 100 to 1000 mJ / cm 2 After the ultraviolet irradiation, heating may be carried out as necessary to ensure complete curing.
[0062] The active energy ray-curable composition can be printed or coated to form a layer, and then irradiated with active energy rays to form a cured layer. The film thickness (film thickness after curing) when the active energy ray-curable composition is printed or coated is usually preferably 1 to 50 μm, more preferably 1 to 30 μm, even more preferably 1 to 20 μm, further preferably 1 to 10 μm, and particularly preferably 1 to 5 μm.
[0063] <Paper base material> The paper substrate used in the present invention is preferably ordinary paper or cardboard, and although there is no particular designation for the thickness, a substrate having a thickness of 0.2 mm to 1.0 mm can be preferably used, and the printed surface may be corona-treated. In addition, the surface of the paper substrate may be vapor-deposited with a metal such as aluminum for the purpose of providing design, and may further be surface-coated with acrylic resin, urethane resin, polyester resin, polyolefin resin, or other resin, and may further be surface-treated, such as corona treatment. For example, coated cardboard and Marie-coated paper are preferably used.
[0064] <Film substrate> The film substrate used in the present invention is preferably a normal PET (polyethylene terephthalate) or PVC (polyvinyl chloride), and is not particularly limited. The film thickness is preferably 0.02 mm to 1.0 mm, and the surface of the substrate may be corona-treated. The film substrate may be surface-coated with acrylic resin, urethane resin, polyester resin, polyolefin resin, or other resin, and may further be surface-treated, such as corona treatment. Examples include Cosmoshine A4300 (manufactured by Toyobo), E5101 (manufactured by Toyobo), and Crisper K2323 (manufactured by Toyobo).
[0065] <Printing ink composition> Examples of the printing ink composition include known gravure ink compositions, flexographic ink compositions, ultraviolet-curable flexographic ink compositions, offset ink compositions, ultraviolet-curable offset ink compositions, and other ink compositions, and any printing ink composition may be used. Among them, when an ultraviolet-curable offset ink composition or an ultraviolet-curable flexographic ink composition is used, if an active energy ray-curable composition is laminated, a curing reaction caused by ultraviolet light or the like occurs between the layers, improving adhesion. Therefore, as the printing ink composition, an ultraviolet-curable offset ink composition or an ultraviolet-curable flexographic ink composition is more preferable.
[0066] <Printing ink> A known method can be used as a printing method for the printing ink composition. Examples include gravure printing, flexographic printing, offset printing, and screen printing. The thickness of the ink layer is preferably 0.1 to 15 μm. It is more preferably 0.5 to 12 μm. The printing ink composition may be either an organic solvent-based or water-based ink composition, or may be an ultraviolet-curable ink composition. The ink layer may be formed by combining the above printing ink compositions, and the printing layer can be formed by drying or ultraviolet curing after printing. EXAMPLES
[0067] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts and % represent parts by mass and % by mass unless otherwise noted.
[0068] (Weight average molecular weight) The weight average molecular weight was determined by measuring the molecular weight distribution using a GPC (gel permeation chromatography) device (HLC-8220 manufactured by Tosoh Corporation) and converting it into a molecular weight using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min
[0069] (glass transition temperature) The glass transition temperature (Tg) was determined by DSC (differential scanning calorimetry) using a Rigaku Corporation DSC8231 measuring device, with a measurement temperature range of -70 to 150°C, a heating rate of 10°C / min, and the midpoint between the endothermic start and end temperatures based on the glass transition in the DSC curve being taken as the glass transition temperature.
[0070] [Synthesis Example 1: Synthesis of urethane acrylate UA1] In a 4L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 262 parts (1 mole) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodur W, manufactured by Sumika Covestro Urethane Co., Ltd.), 2000 parts (2 moles) of polytetramethylene ether glycol (product name: PTMG1000, manufactured by Mitsubishi Chemical Corporation), 232 parts (2 moles) of 2-hydroxyethyl acrylate (product name: Hydroxyethyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 1.247 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while blowing in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum and terminating the reaction, the mixture was cooled to 40°C, and 2262 parts of a pale yellow liquid (UA1) was obtained. The weight average molecular weight of the urethane acrylate UA1 was 2200, the Tg was 25°C, and the number of functional groups was 2.
[0071] [Synthesis Example 2: Synthesis of urethane acrylate UA2] In a 4L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 79 parts (0.3 mol) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodur W, manufactured by Sumika Covestro Urethane Co., Ltd.), 11750 parts (0.6 mol) of polytetramethylene ether glycol (product name: PTMG3000, manufactured by Mitsubishi Chemical Corporation), 70 parts (0.6 mol) of 2-hydroxyethyl acrylate (product name: Hydroxyethyl Acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 0.97 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while blowing in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum and terminating the reaction, the mixture was cooled to 40°C, and 1949 parts of a pale yellow liquid (UA2) was obtained. The weight average molecular weight of the urethane acrylate UA2 was 6200, the Tg was 9°C, and the number of functional groups was 2.
[0072] [Synthesis Example 3: Synthesis of urethane acrylate UA3] In a 3L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 500 parts (1 mole) of hexamethylene diisocyanate trimer (product name: Sumidur N3390 manufactured by Sumika Bayer Urethane Co., Ltd.), 675 parts (3 moles) of polytetramethylene ether glycol (product name: PTMG250 manufactured by Mitsubishi Chemical Co., Ltd.), 348 parts (3 moles) of 2-hydroxyethyl acrylate (product name: Hydroxyethyl Acrylate manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 0.76 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while blowing in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum, the reaction was completed, and the mixture was cooled to 40°C to obtain 1523 parts of a pale yellow liquid (UA3). The weight average molecular weight of the urethane acrylate UA3 was 1 200, Tg was 35°C, and the number of functional groups was 3.
[0073] [Synthesis Example 4: Synthesis of urethane acrylate UA4] In a 4L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 158 parts (0.6 mol) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodur W manufactured by Sumika Covestro Urethane Co., Ltd.), 1680 parts (1.2 mol) of polybutadiene with hydroxyl groups at both ends (product name: NISSO-PBG-1000 manufactured by Nippon Soda Co., Ltd.), 139 parts (1.2 mol) of 2-hydroxyethyl acrylate (product name: hydroxyethyl acrylate manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 0.99 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while blowing in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum as the reaction was completed, the mixture was cooled to 40°C to obtain 1977 parts of a pale yellow liquid (UA4). The urethane acrylate UA4 had a weight average molecular weight of 3,000, a Tg of 21° C., and two functional groups.
[0074] [Synthesis Example 5: Synthesis of urethane acrylate UA5] In a 4L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 131 parts (0.5 mol) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodur W manufactured by Sumika Covestro Urethane Co., Ltd.), 2000 parts (1.0 mol) of polytetramethylene ether glycol (product name: PTMG2000 manufactured by Mitsubishi Chemical Corporation), 116 parts (1.0 mol) of 2-hydroxyethyl acrylate (product name: hydroxyethyl acrylate manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 1.12 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while feeding in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum as the reaction was completed, the mixture was cooled to 40°C to obtain 1977 parts of a pale yellow liquid (UA4). The urethane acrylate UA5 had a weight average molecular weight of 3,500, a Tg of 19° C., and two functional groups.
[0075] [Comparative Synthesis Example 1: Synthesis of urethane acrylate UA6] In a 4L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 66 parts (0.25 mol) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodur W manufactured by Sumika Covestro Urethane Co., Ltd.), 2000 parts (0.5 mol) of polytetramethylene ether glycol (product name: PTMG4000 manufactured by Mitsubishi Chemical Corporation), 58 parts (0.5 mol) of 2-hydroxyethyl acrylate (product name: hydroxyethyl acrylate manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 1.04 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while blowing in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum and terminating the reaction, the mixture was cooled to 40°C to obtain 2077 parts of a pale yellow liquid (UA5). The urethane acrylate UA6 had a weight average molecular weight of 9,000, a Tg of -9°C, and two functional groups.
[0076] [Comparative Synthesis Example 2: Synthesis of urethane acrylate UA7] In a 4L separable 4-neck flask equipped with a stirrer, thermometer, and cooling tube, 576 parts (2.2 moles) of dicyclohexylmethane 4,4'-diisocyanate (product name: Desmodur W, manufactured by Sumika Covestro Urethane Co., Ltd.), 990 parts (4.4 moles) of polytetramethylene ether glycol (product name: PTMG250, manufactured by Mitsubishi Chemical Corporation), 511 parts (4.4 moles) of 2-hydroxyethyl acrylate (product name: Hydroxyethyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 1.06 parts (500 ppm) of p-methoxyphenol were charged, and the mixture was stirred while blowing in air and reacted at 80°C for 4 hours. After confirming the disappearance of the peak due to the isocyanate group in the IR spectrum and terminating the reaction, the mixture was cooled to 40°C, and 2124 parts of a pale yellow liquid (UA6) were obtained. The weight average molecular weight of the urethane acrylate UA7 was 700, the Tg was 44°C, and the number of functional groups was 2. Table 1 summarizes the urethane (meth)acrylates synthesized above.
[0077] (Example 1: Preparation of active energy ray-curable composition S1) 12 parts of urethane acrylate UA1, 47 parts of 4-HBA (4-hydroxybutyl acrylate, manufactured by Osaka Organic Chemicals), 25 parts of ART PEARL MM-120T (urethane-based fine particles, average particle diameter 2 μm, glass transition temperature “Tg” 22° C., manufactured by Negami Chemical Industries, Ltd.), 4 parts of Omnirad TPO (2,4,6-trimethylbenzoyldiphenylphosphine oxide, manufactured by IGM) as a photopolymerization initiator, and 12 parts of a silicone-based defoamer as an additive were mixed and stirred for 90 minutes with a bladed stirrer to obtain an active energy ray-curable composition S1.
[0078] (Examples 2 to 21: Preparation of active energy ray-curable compositions S2 to S21) Active energy ray-curable compositions S2 to S21 were obtained in the same manner as in Example 1, except that the raw materials shown in Table 2-1 were used in the blending ratios shown therein.
[0079] (Comparative Examples 1 to 6: Preparation of Active Energy Ray-Curable Compositions T1 to T6) Active energy ray-curable compositions T1 to T6 were obtained in the same manner as in Example 1, except that the raw materials shown in Table 2-2 were used in the blending ratios shown therein.
[0080] The abbreviations of the raw materials in Tables 2-1 and 2-2 are as follows. <Monofunctional ethylenically unsaturated monomer> ·HEA (2-hydroxyethyl acrylate, manufactured by Osaka Organic Co., Ltd.) ·LA (Lauryl acrylate, manufactured by Osaka Organic Co., Ltd.) <Difunctional ethylenically unsaturated monomer> TEGDA (Tetraethylene glycol diacrylate, manufactured by Osaka Organic Co., Ltd.) <Resin fine particles> ·ART PEARL C-800 transparent (urethane resin fine particles, average particle size 6μm, Tg=-13℃, manufactured by Negami Kogyo Co., Ltd.) ·ART PEARL C-1000 transparent (urethane resin fine particles, average particle size 3μm, Tg=-13℃, manufactured by Negami Kogyo Co., Ltd.) ·ART PEARL J-4P (acrylic resin fine particles, average particle size 2.2μm, manufactured by Negami Kogyo Co., Ltd.) · Silosphere C-1504 (spherical silica, average particle size 4.5 μm, manufactured by Fuji Silysia) <Photopolymerization initiator> Omnirad 1173 (2,4,6-trimethylbenzoyldiphenylphosphine oxide, manufactured by IGM) <Organic solvent> · PGM-AC (Propylene glycol monomethyl ether acetate, manufactured by Toyo Petrochemical Co., Ltd.)
[0081] Example 22 <Coating of active energy ray-curable composition S1> Using a sheet-fed printing press "Lithrone 26 (manufactured by Komori Corporation)," a UV-curable offset ink "FD Carton X Ink M (manufactured by Toyo Ink Co., Ltd., containing multifunctional (meth)acrylic monomers with three or more functionalities)" was printed on the paper substrate Aurora Coat (coated paper high gloss type, paper thickness 81 μm, manufactured by Nippon Paper Industries Co., Ltd.) so that the ink density was 1.75 (measuring device: X-Rite eXact (manufactured by X-Rite Co., Ltd.), conditions: Illuminant D50, standard observer 2°, density status E, no filter), and cured with a UV lamp. The printing speed of the above printing was 8000 sheets / hour, the types of UV lamps were two air-cooled metal halide lamps and one high-pressure mercury lamp, and the intensity of the UV lamps was 160 W / cm for all three lamps (accumulated light quantity 450 mJ / cm 2 ). Next, the active energy ray curable composition S1 was applied onto the printed matter of FD Carton X Ink M obtained above using a flexographic coating unit of Lithrone 26, and cured with a UV lamp to obtain a laminate G1. The anilox roll of the coating unit had a trihelical engraved pattern, a line count of 90 lines / inch, and a cell volume of 25 ml / m 2 During flexo coating, the printing speed was 8000 sheets / hour, and the temperature of the S1 liquid was controlled to 25°C. The type, number, and intensity of the UV lamps were the same as those used for the curing conditions of FD Karton X Ink M described above.
[0082] (Examples 23 to 43) In the same manner as in Example 22, laminates G2 to G22 (Examples) were obtained using the active energy ray-curable compositions S2 to S23 shown in Table 2-1.
[0083] (Example 43) A laminate G22 was obtained in the same manner as in Example 22, except that the paper substrate (Aurora Coat, (coated paper high gloss type, paper thickness 81 μm, manufactured by Nippon Paper Industries Co., Ltd.) used in Example 22 was changed to the paper substrate (U-Lite, (coated paper matte type, paper thickness 79 μm, manufactured by Nippon Paper Industries Co., Ltd.) shown in Table 3-1.
[0084] (Example 45) A laminate G23 was obtained in the same manner as in Example 22, except that the paper substrate (Aurora Coat, (coated paper high gloss type, paper thickness 81 μm, manufactured by Nippon Paper Industries Co., Ltd.) used in Example 22 was changed to a film substrate (Crisper K2323, polyester film, thickness 75 μm, manufactured by Toyobo Co., Ltd.) described in Table 3-1.
[0085] (Comparative Examples 7 to 12) Laminates H1 to H6 (Comparative Examples) were obtained in the same manner as in Example 22, except that active energy ray-curable compositions T1 to T6 shown in Table 2-2 were used.
[0086] (evaluation) The active energy ray curable compositions and laminates obtained in the Examples and Comparative Examples were evaluated for viscosity stability, penetration prevention, smoothness, matte finish, surface tackiness, blocking resistance, and adhesion as described below. The evaluation results are shown in Tables 3-1 and 3-2.
[0087] <Viscosity stability> The viscosity change rate was measured for the active energy ray curable compositions obtained in the examples and comparative examples. The viscosity change rate is a value obtained by measuring the viscosity before and after heating, dividing the viscosity after heating by the viscosity before heating, and expressing the value as a percentage (%). The above-mentioned heating is a process in which the active energy ray curable composition is poured into a cylindrical metal container with an inner diameter of 9.6 cm and a height of 3.0 cm to a thickness of 1 cm, and then left in a 40°C environment for 30 minutes. The viscosity was measured using a cone-plate type viscometer under a liquid temperature condition of 25°C. The evaluation criteria are as follows. 5 (Excellent): Viscosity change rate 0% to less than 3% 4 (Good): Viscosity change rate is 3% or more but less than 6% 3 (Acceptable): Viscosity change rate is 6% or more but less than 9% 2 (Not acceptable): Viscosity change rate is 9% or more but less than 12% 1 (Poor): Viscosity change rate 12% or more The practical usable ratings are 3, 4 and 5.
[0088] <Seeping prevention> A laminate was prepared using the active energy ray curable compositions obtained in the examples and comparative examples. When applying the UV offset ink, the composition was applied not to the image areas of the ink but to the non-image areas, and the printed matter having a cured layer was discharged without being irradiated with a UV lamp. The time required for a mottled pattern to appear due to the active energy ray curable composition soaking into the substrate was measured. Note that, since the soaking phenomenon stops at that point if the composition is irradiated with a UV lamp after coating in the coating unit, the UV lamp was not irradiated in this evaluation. The evaluation criteria are as follows: 5 (Excellent): 15 seconds or more 4 (Good): 12 to 15 seconds 3 (OK): 9 to 12 seconds 2 (Not allowed): Between 6 and 9 seconds 1 (Poor): Less than 6 seconds The practical usable ratings are 3, 4 and 5.
[0089] <Smoothness> The arithmetic mean roughness Ra of the cured layer surface of the laminates obtained in the examples and comparative examples was measured. The measurement of Ra was performed using a laser microscope (VK-X100 manufactured by Keyence Corporation, magnification 1000 times). The evaluation criteria are as follows. 5 (Excellent): Ra less than 1.0 μm 4 (Good): Ra 1.0μm or more and less than 1.5μm 3 (Acceptable): Ra 1.5μm or more and less than 2.0μm 2 (Not acceptable): Ra 2.0μm or more and less than 2.5μm 1 (poor): Ra 2.5μm or more The practical usable ratings are 3, 4 and 5.
[0090] <Matte finish> The gloss of the cured layer surface was measured for the laminates obtained in the examples and comparative examples. The gloss was measured at an incident angle of 60 degrees. The evaluation criteria were as follows. The gloss was measured using Micro Trigloss manufactured by BYK. 5 (Excellent): Gloss value less than 6 4 (Good): Gloss value 6 or more but less than 8 3 (Acceptable): Gloss value 8 or more but less than 10 2 (unacceptable): Gloss value between 10 and 12 1 (poor): Gloss value 12 or more The practical usable ratings are 3, 4 and 5.
[0091] <Surface tackiness> The laminates obtained in the Examples and Comparative Examples were evaluated for the presence or absence of surface tack (stickiness) of the cured film (cured layer). A finger was pressed firmly against the cured film for 10 seconds, and then the finger was removed from the film surface. Thereafter, the degree of fingerprint adhesion to the cured layer surface and stickiness to the touch of the finger were measured. The evaluation criteria were as follows: 5 (Excellent): No fingerprints and no sticky feeling 4 (Good): Fingerprints are slightly visible, but the surface does not feel sticky. 3 (Acceptable): Fingerprints remain, but the surface does not feel sticky. 2 (No good): Fingerprints remain and it feels slightly sticky. 1 (Poor): Fingerprints stick and it feels sticky. The practical usable ratings are 3, 4 and 5.
[0092] <Blocking resistance> The laminates obtained in the examples and comparative examples were stacked so that the cured layers were in contact with each other, and subjected to a pressure of 10 kgf / cm 2 The specimen was left in an environment of 40℃ and 80% RH for 24 hours. After peeling, the state of blocking (the phenomenon in which one hardened layer adheres to the other hardened layer and transfers when the hardened layers are pulled apart from each other when they are in contact with each other) was evaluated. Regarding peel resistance, a test piece of 25 mm x 100 mm was prepared and left for 30 minutes in an atmosphere of 23°C and 50% RH, and then the 180°C peel strength (N / 25 mm) was measured at a peel speed of 30 mm / min. The evaluation criteria are as follows: 5 (Excellent): No blocking (no metastasis) Peel resistance: less than 0.01N / 25mm 4 (Good): No blocking (no metastasis) Peel resistance: 0.01N / 25mm or more, less than 0.03N / 25mm 3 (OK): No blocking (no metastasis) Peel resistance: 0.03N / 25mm or more, less than 0.05N / 25mm 2 (Not possible): Blocking occurs (transition possible) Peel resistance: 0.05N / 25mm or more 1 (Poor): Blocking occurs and the substrate is damaged during peeling. Peel resistance: 0.05N / 25mm or more The practical usable ratings are 3, 4 and 5.
[0093] <Crack resistance> For the laminates obtained in the examples and comparative examples, the cured layer was folded in a mountain shape with a bending radius of 2 mm, and then a peeling test was performed on the folded portion using a 100 mm long adhesive tape (LP12, manufactured by Nichiban Co., Ltd.), and the total length of the portion where the cured layer peeled off was measured. The evaluation criteria are as follows. 5 (Excellent): Peel length less than 1 mm 4 (Good): Peel length 1mm or more but less than 5mm 3 (Acceptable): Peel length 5mm or more and less than 9mm 2 (Not acceptable): Peel length 9mm or more and less than 13mm 1 (Poor): Peel length 13mm or more The practical usable ratings are 3, 4 and 5.
[0094] <Adhesiveness> For the laminates obtained in the examples and comparative examples, a checkerboard peel test tool was used to test the hardened layer against a 1 mm 2 Then, adhesive tape (LP24, manufactured by Nichiban Co., Ltd.) was applied to the cross-cuts and peeled off at a 90-degree angle, and the number of remaining squares in the cured layer was counted. The evaluation criteria were as follows: 5 (Excellent): Number of remaining squares = 96-100 4 (Good): Number of remaining squares = 91-95 3 (Acceptable): Number of remaining squares = 86-90 2 (Not acceptable): Number of remaining squares = 81-85 1 (Poor): Number of remaining squares = 80 or less The practical usable ratings are 3, 4 and 5.
[0095] A practically usable active energy ray-curable composition is one that simultaneously satisfies stable printability and good film properties, i.e., one that simultaneously satisfies a rating of 3 or more in viscosity stability and a rating of 3 or more in all of the following properties: penetration inhibition, smoothness, matte finish, surface tackiness, blocking resistance, crease cracking resistance, and adhesion.
[0096] From the above examples, a method was found in which sufficient viscosity stability and stable printability could be imparted by reducing the amount of solvent in the active energy ray curable composition. In addition, excellent cured film properties could be obtained by setting the molecular weight of the urethane (meth)acrylate to 1000 to 7000.
[0097] [Table 1]
[0098] [Table 2-1]
[0099] [Table 2-2]
[0100] [Table 3-1]
[0101] [Table 3-2] [Industrial Applicability]
[0102] Since no organic solvent is blended or the amount of organic solvent can be reduced, the present active energy ray-curable composition is useful as a low-gloss coating agent with low environmental impact.
Claims
1. An active energy ray-curable composition comprising a polyfunctional urethane (meth)acrylate, a monofunctional ethylenically unsaturated monomer, and resin fine particles, The weight average molecular weight of the polyfunctional urethane (meth)acrylate is 1,000 to 7,000; The composition does not contain an organic solvent or contains an organic solvent in an amount of 5% by mass or less based on the total mass of the composition; The viscosity of the composition at 25°C is 250 to 2500 mPa s, An active energy ray-curable composition for use on a paper substrate.
2. The active energy ray-curable composition according to claim 1 , further comprising a photopolymerization initiator.
3. The active energy ray-curable composition according to claim 1 or 2, wherein the polyfunctional urethane (meth)acrylate has a structural unit derived from a polyether.
4. The active energy ray-curable composition according to any one of claims 1 to 3, having a viscosity at 25°C of 500 to 1500 mPa·s.
5. 5. The active energy ray-curable composition according to claim 1, wherein the resin fine particles are urethane resin fine particles.
6. A laminate having a printed layer and a cured layer formed from the active energy ray-curable composition according to any one of claims 1 to 5 on a paper substrate.
Citation Information
Patent Citations
Heat pump type air-conditioning hot-water supply device
JP1985086358A
Active energy ray-curable composition
JP2002121210A
Solvent-free photocurable coating composition for forming flat coating film
JP2003261815A
Active energy ray-curable coating varnish composition and printed material thereof
JP2010241954A
Active energy ray-curable black resin composition
JP2013082924A