Semiconductor Device

By integrating intermediate layers of magnesium and manganese oxides between the ceramic plate and metal layers in semiconductor devices, the bonding strength is enhanced, preventing substrate deterioration and maintaining device reliability under high temperature and voltage stress.

JP7589807B2Active Publication Date: 2024-11-26FUJI ELECTRIC CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023517029
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-28
Filing Date
2021-11-01
Publication Date
2024-11-26
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

The deterioration of the ceramic multilayer substrate in semiconductor devices due to heat generation and voltage application leads to a decrease in reliability, primarily caused by the degradation of bonding properties between the ceramic plate and metal layers.

Method used

Incorporation of intermediate layers containing oxides of magnesium and manganese between the ceramic plate and metal layers to enhance bonding strength and prevent deterioration, using methods such as coating with magnesium oxide powder and wet oxidation with a manganese-containing solution during the manufacturing process.

Benefits of technology

The intermediate layers effectively suppress the deterioration of the ceramic multilayer substrate, maintaining the bonding strength and reliability of the semiconductor device under high temperature and voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589807000001
    Figure 0007589807000001
  • Figure 0007589807000002
    Figure 0007589807000002
  • Figure 0007589807000003
    Figure 0007589807000003
Patent Text Reader

Abstract

This semiconductor device enables preventing deterioration of a ceramic laminate substrate. A ceramic board (20) is plate shape and has a front surface and a back surface on the side opposite of the front surface, and comprises a plurality of ceramic particles. A high-potential voltage is applied to a metal layer (30), the metal layer (30) is bonded to the front surface of the ceramic board (20), is electrically connected to a semiconductor chip, and contains copper. A low-potential voltage is applied to a metal layer (40), and the metal layer (40) is connected to the back surface of the ceramic plate (20), and contains copper. An intermediate layer (50b) is formed between the back surface of the ceramic plate (20) and the metal layer (40), and contains an oxide (51b) that has magnesium, which is an oxide having magnesium. By means of the oxides (51b) having magnesium included between the ceramic plate (20) and the metal layer (40), reduction in bonding of the metal layer (40) to the ceramic plate (20) is suppressed even when a high voltage is applied at high temperature to a ceramic laminate plate (10).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device. [Background technology]

[0002] The semiconductor device includes a power device and is used as a power conversion device. The power device is, for example, an IGBT (Insulated Gate Bipolar Transistor) or a power MOSFET (Metal Oxide Semiconductor Field Effect Transistor). The semiconductor device includes a semiconductor chip including the power device and a ceramic laminate substrate. The ceramic laminate substrate includes a ceramic plate, a plurality of metal layers formed on the front surface of the ceramic plate and constituting a circuit pattern, and a metal layer formed on the back surface of the ceramic plate. A semiconductor chip, a lead frame, etc. are bonded to the circuit pattern. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-147327 A Summary of the Invention [Problem to be solved by the invention]

[0004] In such a semiconductor device, when the semiconductor chip is driven, the semiconductor chip generates heat, and the area directly below the semiconductor chip is heated. Furthermore, in the semiconductor device, a large voltage is applied to the lead frame, so that a large voltage is applied to the metal layer between the front and back surfaces of the ceramic plate directly below the lead frame. If this situation continues, there is a risk that the bonding between the ceramic plate and the metal layer will deteriorate. If the ceramic laminate substrate deteriorates in this way, it may cause the semiconductor device to fail and the reliability of the semiconductor device may decrease.

[0005] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a semiconductor device in which deterioration of a ceramic laminate substrate is prevented. [Means for solving the problem]

[0006] According to one aspect of the present invention, there is provided a semiconductor chip, a bonding member, and a plate-shaped laminated substrate having a front surface and a back surface opposite to the front surface, the semiconductor chip being bonded to the front surface via the bonding member, the laminated substrate being plate-shaped and having a first main surface and a second main surface opposite to the first main surface, the laminated substrate comprising a ceramic plate having a plurality of ceramic particles, a high potential metal layer bonded to the first main surface and containing copper, a low potential metal layer bonded to the second main surface, containing copper and having a lower potential than the first main surface, and at least one of magnesium and manganese formed between the second main surface and the low potential metal layer. and formed on a part of the interface between the second main surface and the low potential metal layer. and an intermediate layer comprising a first oxide. Effect of the Invention

[0007] According to the disclosed technique, it is possible to prevent deterioration of the ceramic laminate substrate and suppress a decrease in the reliability of the semiconductor device.

[0008] The above and other objects, features and advantages of the present invention will become apparent from the following description taken in conjunction with the accompanying drawings illustrating preferred embodiments of the present invention. [Brief description of the drawings]

[0009] [Figure 1] 1 is a plan view of a semiconductor device according to a first embodiment. [Diagram 2] 1 is a side view of a semiconductor device according to a first embodiment. [Diagram 3] 2 is an equivalent circuit showing a function realized by the semiconductor device of the first embodiment. [Figure 4] 4 is a flowchart showing a method for manufacturing a ceramic laminate substrate included in the semiconductor device according to the first embodiment. [Diagram 5]1 is a schematic cross-sectional view of a ceramic laminate substrate of Comparative Example 1. FIG. [Figure 6] 4 is a schematic cross-sectional view of the ceramic laminate substrate of Comparative Example 1 under high temperature and high voltage conditions. FIG. [Figure 7] 1 is a schematic cross-sectional view of a ceramic laminate substrate according to a first embodiment (Example 1-1). [Figure 8] 1 is a schematic cross-sectional view of the ceramic laminate substrate according to the first embodiment (Example 1-1) at high temperature and high voltage. [Figure 9] 1 is a schematic cross-sectional view of a ceramic laminate substrate according to a first embodiment (Example 1-2). [Figure 10] 1 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-2) at high temperature and high voltage. [Figure 11] 1 is a schematic cross-sectional view of a ceramic laminate substrate according to a first embodiment (Example 1-3). [Figure 12] 3 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-3) at high temperature and high voltage. FIG. [Figure 13] 4 is a table summarizing test results of the ceramic laminate substrate according to the first embodiment. [Figure 14] 4 is a schematic cross-sectional view of a ceramic laminate substrate of Comparative Example 2. FIG. [Figure 15] 1 is a schematic cross-sectional view of the ceramic laminate substrate of Comparative Example 2 under high temperature and high voltage conditions. FIG. [Figure 16] FIG. 11 is a schematic cross-sectional view of a ceramic laminate substrate according to a second embodiment (Example 2-1). [Figure 17] 11 is a schematic cross-sectional view of the ceramic laminate substrate according to the second embodiment (Example 2-1) at high temperature and high voltage. FIG. [Figure 18] FIG. 11 is a schematic cross-sectional view of a ceramic laminate substrate according to a second embodiment (Example 2-2). [Figure 19] 13 is a schematic cross-sectional view of the ceramic laminate substrate according to the second embodiment (Example 2-2) at high temperature and high voltage. FIG. [Figure 20] FIG. 11 is a schematic cross-sectional view of a ceramic laminate substrate according to a second embodiment (Example 2-3). [Figure 21] 11 is a schematic cross-sectional view of the ceramic laminate substrate according to the second embodiment (Example 2-3) at high temperature and high voltage. FIG. [Figure 22] 13 is a diagram for explaining a region requiring an intermediate layer in a ceramic laminate substrate (with a rear surface metal layer at a low potential) according to a third embodiment. FIG. [Figure 23] 13 is a diagram for explaining an area requiring an intermediate layer in a ceramic laminate substrate (with a back metal layer at a high potential) according to a third embodiment. FIG. [Figure 24] 13 is a diagram for explaining a region requiring an intermediate layer in a ceramic laminate substrate (with a rear surface metal layer at a floating potential) according to a third embodiment. FIG. [Diagram 25] 13 is a diagram for explaining a region requiring an intermediate layer in the ceramic laminate substrate according to the third embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiment will be described with reference to the drawings. In the following description, the "front surface" and "upper surface" refer to the XY surface facing upward (+Z direction) in the semiconductor device 1 in the figure. Similarly, "up" refers to the upward (+Z direction) direction in the semiconductor device 1 in the figure. The "rear surface" and "lower surface" refer to the XY surface facing downward (-Z direction) in the semiconductor device 1 in the figure. Similarly, "lower" refers to the downward (-Z direction) direction in the semiconductor device 1 in the figure. Similar orientations are used in other figures as necessary. The terms "front surface", "upper surface", "upper", "rear surface", "lower surface", "lower", and "side surface" are merely convenient expressions for identifying relative positional relationships and do not limit the technical idea of ​​the present invention. For example, "upper" and "lower" do not necessarily mean a vertical direction relative to the ground. In other words, the directions of "upper" and "lower" are not limited to the direction of gravity. In the following description, the term "main component" refers to a case in which the component contains 80 vol% or more.

[0011] In the following description, the content may be expressed as "oxide equivalent". "Oxide equivalent" refers to a calculation in which each metal element confirmed by composition analysis is converted into its respective oxide. For example, all elements confirmed by composition analysis, such as aluminum, silicon, sodium, magnesium, manganese, zirconium, and yttrium, are converted into oxides such as aluminum oxide (Al2O3), silicon oxide (SiO2), sodium oxide (Na2O), magnesium oxide (MgO), manganese oxide (MnO), zirconium oxide (ZrO2), and yttrium oxide (Y2O3), and the ratio of the weight of each oxide to the total weight converted into oxides is expressed. Note that the composition analysis method may be, for example, XRF (X-ray fluorescence analysis), ICP (inductively coupled plasma) emission spectrometry, EPMA (electron beam microanalyzer), or EDX (energy dispersive X-ray spectroscopy).

[0012] In the following explanation, "not containing," "not confirmed," or "not formed" an element or compound means that it is below the measurement limit in the above composition analysis. For example, for manganese and magnesium, it means less than 0.01 wt% in terms of oxide. For example, for sodium, it means less than 0.001 wt% in terms of oxide.

[0013] [First embodiment] (Configuration of Semiconductor Device) A semiconductor device according to a first embodiment will be described with reference to Figs. 1 to 3. Fig. 1 is a plan view of the semiconductor device according to the first embodiment, and Fig. 2 is a side view of the semiconductor device according to the first embodiment. Fig. 3 is an equivalent circuit showing functions realized by the semiconductor device according to the first embodiment. Note that a sealing member is omitted in Fig. 1. Fig. 2 is a side view of the semiconductor device 1 of Fig. 1 as viewed in the +X direction.

[0014] The semiconductor device 1 includes at least a ceramic laminate substrate 10, semiconductor chips 60a, 60b, 65a, 65b, and external connection terminals 71 to 75. It may further include a case 90 and a sealing member 91 (see FIG. 2). In the semiconductor device 1, the external connection terminals 71 to 75 extend upward (in the +Z direction) from the front surface.

[0015] The ceramic laminate substrate 10 includes a ceramic plate 20, metal layers 30a-30f formed on the front surface of the ceramic plate 20, and a metal layer 40 formed on the back surface of the ceramic plate 20. In the following, the metal layers 30a-30f may be collectively referred to as the metal layer 30.

[0016] The ceramic plate 20 is mainly composed of ceramics that are insulating and have good thermal conductivity. Such ceramics may be composed of a material mainly composed of aluminum oxide (Al2O3) or zirconium oxide (ZrO2). Here, the ceramics mainly comprises aluminum oxide (Al2O3). In the second embodiment, zirconium oxide (ZrO2) is further included. The ceramics mainly comprises ceramic particles. The ceramic particles may be composed of a material mainly composed of aluminum oxide (Al2O3). The ceramic plate 20 may also include grain boundary material formed at grain boundaries and triple points of ceramic particles. Such grain boundary material may include, for example, an oxide containing silicon (second oxide). The ceramic plate 20 is rectangular in plan view. Furthermore, the corners may be R-chamfered or C-chamfered. The ceramic plate 20 has a thickness of 0.1 mm or more and 1.0 mm or less, for example, about 0.3 mm. The ceramic plate 20 will be described in detail later.

[0017] The metal layer 30 formed on the front surface of the ceramic plate 20 is mainly composed of a metal having excellent electrical conductivity. Examples of such metals include copper, aluminum, and alloys containing at least one of these. The metal layer 30 used here is mainly composed of copper. The surface of the metal layer 30 may be plated to improve corrosion resistance. Examples of plating materials used at this time include nickel, nickel-phosphorus alloy, and nickel-boron alloy. A plurality of metal layers 30 are formed on the front surface of the ceramic plate 20. For example, in the first embodiment, a plurality of metal layers 30a to 30f are formed on the front surface of the ceramic plate 20. Hereinafter, when the metal layers 30a to 30f are not distinguished from each other, they may be referred to as the metal layer 30. The metal layer 30 is electrically connected to the semiconductor chips 60a, 60b, 65a, and 65b. The metal layer 30 may be bonded to the semiconductor chips 60a, 60b, 65a, 65b and the external connection terminals 71 to 75 via a bonding member 35 such as solder. Each metal layer 30 may be polygonal. Furthermore, the corners may be R-chamfered or C-chamfered. The multiple metal layers 30 are formed on the inside of the ceramic plate 20. The thickness of each metal layer 30 is 0.1 mm or more and 0.5 mm or less, and may be about 0.3 mm.

[0018] The metal layer 40 formed on the back surface of the ceramic plate 20 is mainly composed of a metal having excellent thermal conductivity. Such a metal may be, for example, copper, aluminum, or an alloy containing at least one of these. The metal layer 40 used here is mainly composed of copper. The surface of the metal layer 40 may be plated to improve corrosion resistance. Examples of the plating material used at this time include nickel, a nickel-phosphorus alloy, and a nickel-boron alloy. The metal layer 40 is formed on the back surface of the ceramic plate 20 in correspondence with the metal layer 30. That is, the metal layer 40 includes the metal layers 30a to 30f formed on the front surface of the ceramic plate 20 in a plan view. The metal layer 40 may be connected to the heat dissipation member 92 via solder, brazing material, heat dissipation paste, or the like. The ceramic laminate substrate 10 can transfer heat generated in the semiconductor chips 60a, 60b, 65a, and 65b to the heat dissipation member 92 on the outside through the metal layer 30, the ceramic plate 20, and the metal layer 40. Therefore, when the semiconductor device 1 is in operation, the ceramic plate 20 is heated. The metal layer 40 is rectangular in plan view. Furthermore, the corners may be R-chamfered or C-chamfered. The metal layer 40 is formed on the inside of the ceramic plate 20. The metal layer 40 is formed to cover the area facing the metal layer 30. The thickness of the metal layer 40 is 0.1 mm or more and 0.5 mm or less, and may be about 0.3 mm.

[0019] In addition, intermediate layers 50a, 50b are formed between the ceramic plate 20 and the metal layers 30, 40. The intermediate layers 50a, 50b contain an oxide (first oxide) containing at least one of magnesium and manganese. The oxide may be, for example, magnesium oxide (MgO), manganese oxide (MnO), (Mg, Mn)O, or (Mg, Mn)Mn2O4. These oxides are contained in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a, 50b.

[0020] In addition, the oxides contained in the intermediate layers 50a and 50b may contain aluminum. Such oxides may include a spinel crystal system containing aluminum. Examples of the spinel crystal system include MgAl2O4, MnAl2O4, (Mg, Mn)Al2O4, and (Mg, Mn)(Al, Mn)2O4. The ceramic laminate substrate 10 may include at least one of the intermediate layer 50a and the intermediate layer 50b.

[0021] For example, a direct copper bonding (DCB) substrate or an active metal brazed (AMB) substrate may be used as the ceramic laminate substrate 10 having such a configuration. The manufacturing method and details of the ceramic laminate substrate 10 will be described later.

[0022] The semiconductor chips 60a, 60b, 65a, and 65b are mainly composed of silicon or silicon carbide. The semiconductor chips 60a and 60b are switching elements. The switching elements are, for example, IGBTs and power MOSFETs. The semiconductor chips 60a and 60b have a drain electrode or a collector electrode as an input electrode (main electrode) on the back surface. The semiconductor chips 60a and 60b also have a gate electrode as a control electrode 61a and 61b and a source electrode or an emitter electrode as an output electrode 62a and 62b (main electrode) on the front surface. The back surfaces of the semiconductor chips 60a and 60b are bonded to the metal layers 30b and 30c by solder (not shown).

[0023] The semiconductor chips 65a and 65b are diode elements. The diode elements are, for example, FWD (Free Wheeling Diodes) such as SBD (Schottky Barrier Diodes) and PiN (P-intrinsic-N) diodes. Such semiconductor chips 65a and 65b each have a cathode electrode as an output electrode (main electrode) on the back surface and an anode electrode as input electrodes 66a and 66b (main electrodes) on the front surface. The back surfaces of the semiconductor chips 65a and 65b are bonded to the metal layers 30b and 30c by the above-mentioned solder (not shown). The semiconductor chips 60a, 60b, 65a and 65b are RC (Reverse Conductive)-IGBT elements and RB (Reverse Blocking) elements, which are semiconductor chips each including a switching element and a diode element. g) The element may be an IGBT element.

[0024] The joining member 35 that joins the semiconductor chips 60a, 60b, 65a, 65b to the metal layers 30b, 30c may be solder. Lead-free solder is used as the solder. The lead-free solder is mainly composed of an alloy containing at least two of tin, silver, copper, zinc, antimony, indium, and bismuth. Furthermore, the solder may contain additives. The joining member 35 may be a metal sintered body instead of solder. The material of the metal sintered body is mainly composed of silver or a silver alloy. In addition, such solder and metal sintered body may be used not only for joining the semiconductor chips 60a, 60b to the metal layers 30b, 30c, but also for joining the metal layers 30a, 30e, 30c, 30f, 30d of the external connection terminals 71 to 75 described later.

[0025] Each of the external connection terminals 71 to 75 has a plate shape, a prismatic shape, or a cylindrical shape. In this embodiment, a prismatic shape is illustrated. One end of each of the external connection terminals 71 to 75 is electrically and mechanically joined to the metal layers 30a, 30e, 30c, 30f, and 30d of the ceramic laminate substrate 10. The other end of each of the external connection terminals 71 to 75 extends from the sealing member 91. The other end may be connected to an external device (not shown).

[0026] The external connection terminals 71 to 75 are mainly composed of a metal having excellent electrical conductivity. Examples of such metals include aluminum, copper, iron, nickel, and alloys containing at least one of these. The surfaces of the external connection terminals 71 to 75 may also be plated to improve corrosion resistance. Examples of plating materials used in this case include nickel, nickel-phosphorus alloys, and nickel-boron alloys. The external connection terminals 71 to 75 and the metal layers 30a, 30e, 30c, 30f, and 30d may be bonded to each other using solder and a metal sintered body, as in the case of bonding the semiconductor chips 60a, 60b, 65a, and 65b. The external connection terminals 71 to 75 and the metal layers 30a, 30e, 30c, 30f, and 30d may also be bonded to each other directly using ultrasonic waves or lasers.

[0027] The bonding wires 80a to 80e are mainly composed of a metal having excellent electrical conductivity. Such metal is composed of aluminum, copper, or an alloy containing at least one of them. The bonding wire 80a mechanically and electrically connects the metal layers 30a and 30b. The bonding wire 80d mechanically and electrically connects the metal layer 30e and the control electrode 61a of the semiconductor chip 60a. The bonding wire 80b mechanically and electrically connects the output electrode 62a of the semiconductor chip 60a, the input electrode 66a of the semiconductor chip 65a, and the metal layer 30c. The bonding wire 80e mechanically and electrically connects the metal layer 30f and the control electrode 61b of the semiconductor chip 60b. The bonding wire 80c mechanically and electrically connects the output electrode 62b of the semiconductor chip 60b, the input electrode 66b of the semiconductor chip 65b, and the metal layer 30d. The diameter of the control bonding wires 80d, 80e is, for example, 25 μm or more and 400 μm or less, and the diameter of the main current bonding wires 80a to 80c is, for example, 250 μm or more and 600 μm or less.

[0028] The case 90 houses the metal layer 30 on the front surface of the ceramic laminate substrate 10, the semiconductor chips 60a, 60b, 65a, 65b, and one end of the external connection terminals 71-75. The other ends of the external connection terminals 71-75 may extend upward (in the +Z direction) from the front surface of the case. The case 90 is made of resin. Such resin is mainly composed of thermoplastic resin. The thermoplastic resin is, for example, polyphenylene sulfide resin, polybutylene terephthalate resin, polybutylene succinate resin, polyamide resin, or acrylonitrile butadiene styrene resin.

[0029] The sealing member 91 may seal the inside of the case 90. That is, the sealing member 91 seals the metal layer 30 on the front surface of the ceramic laminate substrate 10, the semiconductor chips 60a, 60b, 65a, 65b, and one end of the external connection terminals 71 to 75. The sealing member 91 contains, for example, a thermosetting resin and a filler contained in the thermosetting resin. The thermosetting resin is, for example, an epoxy resin, a phenolic resin, or a maleimide resin. An example of such a sealing member is an epoxy resin containing a filler. An inorganic material is used as the filler. Examples of the inorganic material include silicon oxide, aluminum oxide, boron nitride, or aluminum nitride. In addition to the materials already described, the sealing member 91 may be a silicone gel.

[0030] As shown in FIG. 3, the semiconductor device 1 configures a half-bridge circuit including an upper arm portion A and a lower arm portion B. The connection point P is connected to the positive electrode of an external power supply (not shown). The connection point P and the connection point C1 of the collector electrode of the semiconductor chip 60a are connected by a wiring 81. The connection point M is connected to a load (not shown). The connection point M and the connection point E1C2 of the emitter electrode of the semiconductor chip 60a and the collector electrode of the semiconductor chip 60b are connected by a wiring 83. The connection point N is connected to the negative electrode of an external power supply (not shown). The connection point N and the connection point E2 of the emitter electrode of the semiconductor chip 60b are connected by a wiring 85. Here, during operation of the semiconductor device 1, the connection point P has a higher potential than the connection point M. Therefore, the wiring 81 has a higher potential than the wiring 83. Furthermore, the connection point M has a higher potential than the connection point N. Therefore, the wiring 83 has a higher potential than the wiring 85. The potential of the wiring 81 may be higher than the potential of the wiring 83 by 250 V or more and less than 1000 V. The potential of the wiring 83 may be higher than the potential of the wiring 85 by 250 V or more and less than 1000 V.

[0031] The connection points G1 and G2 are connected to a control power supply (not shown). The connection point G1 is connected to a control electrode 61a (not shown in FIG. 3, see FIG. 1) of the semiconductor chip 60a by a wiring 82. The connection point G2 is connected to a control electrode 61b (not shown in FIG. 3, see FIG. 1) of the semiconductor chip 60b by a wiring 84.

[0032] The upper arm portion A of the semiconductor device 1 includes the metal layers 30a, 30b, and 30e of the ceramic laminate substrate 10, the semiconductor chips 60a and 65a, the external connection terminals 71, 73, and 72, and the bonding wires 80a, 80b, and 80d that connect them. The lower arm portion B of the semiconductor device 1 includes the metal layers 30d, 30c, and 30f of the ceramic laminate substrate 10, the semiconductor chips 60b and 65b, the external connection terminals 75, 73, and 74, and the bonding wires 80c and 80e that connect them. The metal layers 30b and 30c are electrically connected by the bonding wire 80b, so that the upper arm portion A and the lower arm portion B are connected. In this way, the semiconductor device 1 can function as a half-bridge circuit including the upper arm portion A and the lower arm portion B.

[0033] The wiring 81 includes an external connection terminal 71, which is a P terminal (positive electrode), a metal layer 30a to which the external connection terminal 71 is connected, a metal layer 30b on which the semiconductor chips 60a and 65a are arranged, and a bonding wire 80a connecting the metal layer 30a and the metal layer 30b. The wiring 83 includes an external connection terminal 73, which is an M terminal, a metal layer 30c on which the external connection terminal 73 and the semiconductor chips 60b and 65b are arranged, and a bonding wire 80b connecting the metal layer 30c and the semiconductor chips 60a and 65a. The wiring 85 includes an external connection terminal 75, which is an N terminal (negative electrode), a metal layer 30d on which the external connection terminal 75 is arranged, and a bonding wire 80c connecting the metal layer 30d and the semiconductor chips 60b and 65b.

[0034] Therefore, when the semiconductor device 1 is in operation, if the metal layer 40 formed on the back surface of the ceramic plate 20 is grounded to have the same potential as the N terminal, the metal layer 40 has a lower potential than the metal layers 30a, 30b, and 30c corresponding to the wirings 81 and 83. That is, in this case, the metal layer with a low potential is the metal layer 40 formed on the back surface of the ceramic plate 20, and the metal layer with a high potential is the metal layers 30a, 30b, and 30c formed on the front surface of the ceramic plate 20. For example, the metal layer 40 has a lower potential than the metal layers 30a and 30b by 500V or more and less than 2000V. Also, the metal layer 40 has a lower potential than the metal layer 30c by 250V or more and less than 1000V.

[0035] In addition, during operation of the semiconductor device 1, when the metal layer 40 formed on the back surface of the ceramic plate 20 is grounded to have the same potential as the M terminal, or when it is not grounded and is floating, the metal layer 40 has a lower potential than the metal layers 30a and 30b corresponding to the wiring 81. That is, in this case, the low-potential metal layer is the metal layer 40 formed on the back surface of the ceramic plate 20, and the high-potential metal layer is the metal layers 30a and 30b formed on the front surface of the ceramic plate 20. For example, the metal layer 40 has a lower potential than the metal layers 30a and 30b by 250V or more and less than 1000V. In addition, the metal layer 30d corresponding to the wiring 85 has a lower potential than the metal layer 40. That is, in this case, the low-potential metal layer is the metal layer 30d formed on the front surface of the ceramic plate 20, and the high-potential metal layer is the metal layer 40 formed on the back surface of the ceramic plate 20. For example, the metal layer 30d has a lower potential than the metal layer 40 by 250 V or more and less than 1000 V.

[0036] (Method of manufacturing a semiconductor device) Next, a method for manufacturing the ceramic laminated substrate 10 included in the semiconductor device 1 will be described with reference to Fig. 4. Fig. 4 is a flow chart showing a method for manufacturing the ceramic laminated substrate included in the semiconductor device of the first embodiment. In manufacturing the ceramic laminated substrate 10, first, a ceramic plate and a metal foil are prepared (steps S1a and S1b). Note that either step S1a or S1b may be performed first.

[0037] The preparation of the ceramic plate will be described (Step S1a). First, aluminum oxide (Al2O3) powder is added with silicon oxide (SiO2) powder, and the mixture is stirred with a binder and formed into a plate shape. Magnesium oxide (MgO) powder is applied to the surface of the plate-shaped molded product, and the product is fired at a predetermined temperature for a predetermined time. The ceramic plate thus fired contains aluminum oxide as ceramic particles, and contains an oxide (second oxide) containing silicon at the grain boundaries and triple junctions of the ceramic particles, and an oxide containing magnesium is formed on the surface. Also, an oxide containing magnesium may be formed at the grain boundaries and triple junctions of the ceramic particles. In addition, the coating of magnesium oxide powder at this time may be omitted. The average particle size of the ceramic particles is 0.5 μm or more and 25 μm or less. More preferably, it is 1 μm or more and 10 μm or less.

[0038] In the ceramic plate 20, the content of aluminum oxide is 90 wt% or more and 99 wt% or less, more preferably 92 wt% or more and 98 wt% or less, calculated as oxide. The content of silicon-containing oxide in the ceramic plate 20 is 90 wt% or more and 99 wt% or less, more preferably 92 wt% or more and 98 wt% or less, based on the total amount calculated as oxide. 、 The content of the oxide containing silicon is 0.01wt% or more and 3.0wt% or less, and more preferably 1.0wt% or more and 3.0wt% or less, calculated as silicon oxide (SiO2). If the content of the oxide containing silicon is too small, many voids remain in the ceramic plate, which makes it easy to crack. If the content of the oxide containing silicon is too large, the conduction of ions in the ceramic plate increases during operation of the semiconductor device 1, which makes it easy for the insulation property and the bonding property of the copper foil to decrease.

[0039] In addition, the ceramic plate 20 contains various materials used in its manufacture in addition to ceramic particles, oxides containing magnesium, and oxides containing silicon. One example of such a material is an oxide containing sodium. For example, there is sodium oxide (Na2O). The content of the oxide containing sodium in the ceramic plate 20 is calculated as follows: 、The content is 0.001wt% or more and 0.2wt% or less, and more preferably 0.002wt% or more and 0.2wt% or less, calculated as sodium oxide (Na2O). If the content of the oxide containing sodium is too low, it becomes difficult to refine the ceramic raw material powder. If the content is too high, β-alumina (Na2O·11Al2O3) is formed, which tends to cause a decrease in insulation and strength. The ceramic plate 20 preferably does not contain β-alumina.

[0040] The preparation of the metal foil will be described (Step S1b). A metal foil containing copper as a main component is prepared, and its surface is oxidized. As a result, copper oxide (Cu x O) is formed. In this oxidation step, a wet oxidation method or a dry oxidation method may be used. In the wet oxidation method, for example, a metal foil mainly composed of copper can be immersed in a manganese-containing solution to be oxidized. By the wet oxidation method using a manganese-containing solution, copper oxide is formed on the surface of the metal foil, and an oxide containing manganese is also formed. In the dry oxidation method, for example, a metal foil mainly composed of copper is heated in the air or an oxygen gas atmosphere. As a result, in the dry oxidation method, copper oxide is formed on most of the surface of the metal foil, and other metals including manganese are not formed.

[0041] Next, the metal foil formed in step S1b is bonded to the front and back surfaces of the ceramic plate formed in step S1a (step S2). That is, the metal foil formed in step S1b is superimposed on the front and back surfaces of the ceramic plate formed in step S1a, and heat treatment is performed at a predetermined temperature for a predetermined time. At this time, the metal layer formed on the front and back surfaces of the ceramic plate is made of metal foil made by either a wet oxidation method or a dry oxidation method. That is, the metal foil made by the wet oxidation method is superimposed on the front and back surfaces of the ceramic plate, respectively. The metal foil made by the dry oxidation method is superimposed on the front and back surfaces of the ceramic plate 20, respectively.

[0042] When the ceramic plate and the metal layer are laminated and heat treated in this way, copper oxide (Cu x O) is formed. In addition, intermediate layers 50a, 50b containing an oxide having at least one of magnesium and manganese can be formed at the contact interface between the ceramic plate and the metal layer by a predetermined method. The predetermined method may be at least one of coating magnesium oxide when firing the ceramic plate, or forming the metal layer by a wet oxidation method using a manganese-containing solution.

[0043] The ceramic laminate substrate 10 of Example 1-1 described below is one in which magnesium oxide is applied during firing of the ceramic plate 20. Therefore, intermediate layers 50a, 50b containing an oxide having magnesium as a first oxide are formed at the contact interfaces between the ceramic plate 20 and the metal layers 30, 40.

[0044] The ceramic laminate substrate 10 of Example 1-2 described below is obtained by coating magnesium oxide during firing of the ceramic plate 20, and forming the metal layers 30, 40 by a wet oxidation method using a manganese-containing solution. As a result, intermediate layers 50a, 50b containing oxides having both magnesium and manganese as first oxides are formed at the contact interfaces between the ceramic plate 20 and the metal layers 30, 40.

[0045] In the ceramic laminate substrate 10 of Examples 1-3 described below, the metal layers 30, 40 are formed by a wet oxidation method using a manganese-containing solution during firing of the ceramic plate 20. As a result, intermediate layers 50a, 50b containing an oxide having manganese as the first oxide are formed at the contact interface between the ceramic plate 20 and the metal layers 30, 40. This allows the ceramic plate 20 and the metal layers 30, 40 to be suitably bonded to each other.

[0046] Next, the metal layer formed on the ceramic plate in step S2 is etched (step S3). That is, the metal layer formed on the front surface of the ceramic plate is etched into a predetermined shape to form metal layers 30a-30f. Also, the metal layer formed on the back surface of the ceramic plate is etched to form metal layer 40. Note that the surfaces of metal layers 30a-30f and the surface of metal layer 40 are doped with copper oxide (Cu x O) film must not be formed. x The coating (O) can be removed by heat treatment in a reducing atmosphere during bonding (step S2) or by surface polishing after bonding or etching. The ceramic plate 20 has a thickness of about 0.32 mm. The metal layers 30 and 40 have a thickness of about 0.3 mm.

[0047] As a result, a ceramic laminate substrate 10 is manufactured in which the intermediate layers 50a, 50b are included between the ceramic plate 20 and the metal layers 30, 40. In such a ceramic laminate substrate 10, the intermediate layers 50a, 50b suppress a decrease in the bonding strength between the metal layers 30, 40 and the ceramic plate 20. When magnesium oxide powder is applied in step S1a, the ceramic laminate substrate 10 has a magnesium oxide (MgO) content of the ceramic plate 20 and the intermediate layers 50a, 50b of the ceramic laminate substrate 10 that is 0.1 wt% or more and 1.5 wt% or less of the total amount calculated as oxide. Furthermore, in this case, the magnesium content calculated as magnesium oxide (MgO) is 10 wt% or more and 50 wt% or less of the silicon content calculated as silicon oxide (SiO2). In the case where the coating of magnesium oxide powder is not performed in step S1a, the ceramic laminate substrate 10 does not contain magnesium (it is less than the measurement lower limit of 0.01 wt%). In addition, in the case where the wet oxidation method using the manganese-containing solution is performed in step S1b, the content of the oxide containing manganese in the ceramic plate 20 and the intermediate layers 50a, 50b in the ceramic laminate substrate 10 is 0.01 wt% or more and 0.15 wt% or less in terms of manganese oxide (MnO) with respect to the total amount calculated as oxide. Furthermore, in this case, the content of manganese calculated as manganese oxide (MnO) is 1.0 wt% or more and 5.0 wt% or less with respect to the content of silicon calculated as silicon oxide (SiO2). In the case where the wet oxidation method using the manganese-containing solution is not performed in step S1b, the ceramic laminate substrate 10 does not contain manganese (it is less than the measurement lower limit of 0.01 wt%).

[0048] The ceramic laminate substrate 10 of Example 1-1 described later is a case where magnesium oxide powder was applied, but the wet oxidation method using a manganese-containing solution was not performed. In this case, the ceramic laminate substrate 10 teeth, contains an oxide containing magnesium, but does not contain an oxide containing manganese. The ceramic laminate substrate of Example 1-2 described later is a case where both the coating of magnesium oxide powder and the wet oxidation method using a manganese-containing solution are performed. Therefore, the ceramic laminate substrate 10 contains both an oxide containing magnesium and an oxide containing manganese. The ceramic laminate substrate 10 of Example 1-3 described later is a case where the coating of magnesium oxide powder is not performed, and the wet oxidation method using a manganese-containing solution is performed. Therefore, the ceramic laminate substrate 10 does not contain an oxide containing magnesium, but contains an oxide containing manganese. Note that the ceramic laminate substrate 100 of the comparative example described later is a case where both the coating of magnesium oxide powder and the wet oxidation method using a manganese-containing solution are not performed. Therefore, the ceramic laminate substrate 100 does not contain either an oxide containing magnesium or an oxide containing manganese.

[0049] (Ceramic laminate substrate of comparative example 1) In the following, in order to explain the suppression of the decrease in the bonding strength of the metal layers 30, 40 by the intermediate layers 50a, 50b, a ceramic laminate substrate not including the intermediate layers 50a, 50b will be described as Comparative Example 1 with reference to Figs. 5, 6, and 13. Fig. 5 is a schematic cross-sectional view of the ceramic laminate substrate of Comparative Example 1, and Fig. 6 is a schematic cross-sectional view of the ceramic laminate substrate of Comparative Example 1 at high temperature and high voltage. Fig. 13 is a table summarizing the test results of the ceramic laminate substrate. Fig. 5 typically shows the micro state in the area surrounded by the dashed line in Fig. 2. Fig. 6 also typically shows the micro state when a high voltage is applied between the metal layers 30, 40 at high temperature in Fig. 5. Fig. 13 also shows the micro state of Comparative Example 1, which will be described below together with Comparative Example 1. Examples 1-1 to 1-3 The test results are also shown.

[0050] The ceramic plate 120 included in the ceramic laminate substrate of Comparative Example 1 was produced without coating with magnesium oxide in step S1a of FIG. 4. This ceramic plate contains aluminum oxide as a main component, and also contains an oxide containing silicon and an oxide containing sodium. The metal layer included in the ceramic laminate substrate of Comparative Example 1 was produced by the dry oxidation method in step S1b of FIG. 4. The ceramic plate and the metal layer are subjected to the processes of steps S2 and S3 of FIG. 4 to produce the ceramic laminate substrate 100 of Comparative Example 1. The ceramic laminate substrate 100 does not contain magnesium and manganese. That is, the ceramic laminate substrate 100 produced in this manner does not have the intermediate layers 50a and 50b containing an oxide containing at least one of magnesium and manganese.

[0051] The ceramic laminated substrate 100 thus manufactured is constructed by laminating a metal layer 40, a ceramic plate 120, and a metal layer 30 in this order from the bottom, as shown in Fig. 5. The ceramic plate 120 contains at least aluminum oxide 21 (Al2O3) particles, and oxides 22 (Si-O) and sodium oxide 23 (Na2O) that contain silicon at the grain boundaries and triple points. The metal layers 30 and 40 are mainly composed of copper (Cu) and do not contain oxygen. At the boundaries between the metal layers 30 and 40 and the ceramic plate 120, oxides 31 and 41 (Cu-O) that contain copper are formed, respectively.

[0052] The results of an evaluation test of the peel strength of the ceramic laminate substrate 100 are described below. The peel strength evaluation test measures the peel strength of the metal layers 30, 40 from the ceramic plate 120 of the ceramic laminate substrate 100 before and after a reliability test. Next, the bonding strength of the metal layers 30, 40 to the ceramic plate 120 is evaluated from the measurement results. The peel strength value was calculated as the average value of the measurements at 40 points.

[0053] First, the reliability test is performed by continuously operating the half-bridge circuit in a predetermined on / off pattern for a predetermined time in a high-temperature environment. 1 The metal layer 40 formed on the back surface of the ceramic plate 20 was grounded so as to have the same potential as the N terminal. 1 The metal layer 30 formed on the front surface of the ceramic laminate substrate 20 is a high-potential metal layer, and the metal layer 40 formed on the back surface is a low-potential metal layer.

[0054] The peel strength is measured as follows: In the ceramic laminate substrate 100, a rectangular pattern having a predetermined width is processed in a part of the metal layers 30, 40, one end of the rectangular metal layers 30, 40 is peeled off from the ceramic plate 120, and the peeled end is pulled at a constant speed in a direction perpendicular to the main surface of the ceramic laminate substrate 100 for a predetermined length or more. The load applied during this pulling is measured.

[0055] The evaluation is performed based on the change in peel strength of the metal layers 30, 40 included in the ceramic laminate substrate 100 before and after the reliability test. If the peel strength after the reliability test is 95% or more of the peel strength before the reliability test, it is evaluated as "Excellent", if it is less than 95% and 90% or more, it is evaluated as "Very Good", if it is less than 90% and 60% or more, it is evaluated as "Good", and if it is less than 60%, it is evaluated as "Not Good" (see FIG. 13). Note that FIG. 13 shows the ceramic plate, metal layer, and intermediate layer used in the evaluation and the test results for Examples 1-1 to 1-3 and Comparative Example 1.

[0056] 13 (rightmost column), the evaluation result for Comparative Example 1 is "Excellent" for the front surface of the ceramic laminate substrate 100, but "Not Good" for the back surface. That is, the ceramic laminate substrate 100 is in a state where the bonding strength of the metal layer 40 to the back surface of the ceramic plate 120 has decreased due to the reliability test. The reason for this has not yet been fully elucidated at present, and while not being bound by any theory, it can be considered as follows.

[0057] The ceramic laminate substrate 100 after the reliability test has a composition as shown in Fig. 6. When a high potential (positive electrode) and a low potential (negative electrode) voltage are applied to the metal layers 30 and 40 at a high temperature, the sodium oxide 23 (see Fig. 5) is converted into sodium ions 24 (Na + ) and oxygen ion 25 (O 2- ) The sodium ions 24 pass through the oxide 22 containing silicon at the grain boundaries of the aluminum oxide 21 and move to the negative electrode, low potential metal layer 40 side. The oxygen ions 25 pass through the oxide 22 containing silicon at the grain boundaries of the aluminum oxide 21 and move to the positive electrode, high potential metal layer 30 side.

[0058] The oxygen ions 25 that have migrated to the positive electrode react with the copper contained in the metal layer 30 to form an oxide containing copper 31. At the positive electrode, the oxide containing copper 31 increases, and the bonding strength to each of the aluminum oxide 21 and the oxide containing silicon 22 improves.

[0059] On the other hand, the sodium ions 24 that have moved to the negative electrode react with the copper-containing oxide 41 (see FIG. 5) to reduce the copper oxide, and the copper-containing oxide 41 of the negative electrode that has reacted with the sodium ions 24 becomes Cu and is included in the metal layer 40. The sodium ions 24 are also oxidized to sodium oxide. In this way, the copper-containing oxide 41, which has a large bonding strength to both the aluminum oxide 21 and the silicon-containing oxide 22, decreases. In addition, the concentration of sodium ions (sodium oxide 23) increases in the ceramic plate 120 near the boundary with the metal layer 40 of the negative electrode, making it easier for particles of the aluminum oxide 21 to detach. This reduces the bonding strength of the metal layer 40 to the ceramic plate 120.

[0060] When such a ceramic laminate substrate 100 is used in place of the ceramic laminate substrate 10 of the semiconductor device 1, when the metal layer 40 is grounded, the metal layer 40 has a low potential (reference potential), the metal layer 30a has a high potential, and the metal layer 30c has an intermediate potential. This reduces the bonding strength in the portions of the metal layer 40 facing the metal layers 30a and 30c (particularly the high-potential metal layer 30).

[0061] The metal layer 40 may be at a floating potential without being grounded, or may be at a midpoint ground (grounded to the same potential as the metal layer 30c). In these cases, the metal layers 30a and 30b on the collector side of the upper arm portion are at a high potential, and the metal layer 40 is at a low potential. This reduces the bonding strength of the portion of the metal layer 40 facing the metal layers 30a and 30b. On the other hand, the metal layer 30d on the emitter side of the lower arm portion is at a low potential, and the metal layer 40 facing the metal layer 30d is at a high potential, which reduces the bonding strength of the metal layer 30d.

[0062] In the following, examples 1-1 to 1-3 will be described according to the intermediate layers 50a, 50b in a ceramic laminate substrate 10 including a ceramic plate 20 containing aluminum oxide as a main component.

[0063] (Ceramic laminate substrate of Example 1-1) Next, the ceramic laminate substrate 10 including the intermediate layers 50a, 50b will be described with reference to Figs. 7, 8, and 13. Fig. 7 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-1), and Fig. 8 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-1) at high temperature and high voltage. Fig. 7 typically shows the micro state in the area surrounded by the dashed line in Fig. 2. Fig. 8 also typically shows the micro state when a high voltage is applied between the metal layers 30, 40 at high temperature in Fig. 2.

[0064] As shown in FIG. 7, the ceramic laminate substrate 10 of Example 1-1 is configured by laminating a metal layer 40, an intermediate layer 50b, a ceramic plate 20, an intermediate layer 50a, and a metal layer 30 in this order from the bottom.

[0065] The ceramic plate 20 is manufactured by applying magnesium oxide powder in step S1a of Fig. 4. The metal layers 30 and 40 are manufactured by a dry oxidation method in step S1b of Fig. 4. The ceramic plate 20 contains, as a second oxide, an oxide 22 having silicon between particles (grain boundaries and triple points) of the aluminum oxide 21 and sodium oxide 23. The ceramic plate 20 may further contain magnesium oxide.

[0066] The intermediate layers 50a and 50b contain magnesium-containing oxides 51a and 51b (Mg-O) as the first oxide. The magnesium-containing oxides 51a and 51b are formed in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a and 50b. Furthermore, copper-containing oxides 31 and 41 are formed at the boundaries between the metal layers 30 and 40 and the ceramic plate 20, and at the boundaries between the magnesium-containing oxides 51a and 51b, the metal layers 30 and 40, and the ceramic plate 20.

[0067] In the ceramic laminate substrate 10 (before reliability testing), if the magnesium-containing oxides 51a, 51b are too large, the bonding strength between the ceramic plate 20 and the metal layers 30, 40 decreases. For this reason, the intermediate layers 50a, 50b containing the magnesium-containing oxides 51a, 51b are preferably formed to cover 10% or more and 80% or less of the bonding surface between the ceramic plate 20 and the metal layers 30, 40, and more preferably 20% or more and 50% or less.

[0068] A peel strength evaluation test was also conducted on such a ceramic laminate substrate 10. As shown in FIG. 13, the evaluation results for Example 1-1 were "Excellent" for the front surface of the ceramic laminate substrate 10 and "Good" for the back surface. That is, even after the reliability test was conducted on the ceramic laminate substrate 10, the bonding strength of the metal layer 40 to the back surface of the ceramic plate 20 was somewhat improved and the decrease in bonding was suppressed compared to Comparative Example 1. The reason for this has not yet been fully elucidated, and the present invention is not limited to any theory, but it can be considered as follows.

[0069] The ceramic laminate substrate 10 after the reliability test has a composition as shown in Fig. 8. When a high potential (positive electrode) and a low potential (negative electrode) voltage are applied to the metal layers 30 and 40 at a high temperature, the sodium oxide 23 (see Fig. 7) is converted into sodium ions 24 (Na + ) and oxygen ion 25 (O 2- ) The sodium ions 24 pass through the grain boundaries of the aluminum oxide 21 and the oxide 22 containing silicon at the triple junctions, and move to the low-potential metal layer 40 side, which is the negative electrode. The oxygen ions 25 pass through the grain boundaries of the aluminum oxide 21 and the oxide 22 containing silicon at the triple junctions, and move to the high-potential metal layer 30 side, which is the positive electrode.

[0070] The oxygen ions 25 that have migrated to the positive electrode react with the copper of the metal layer 30 to form an oxide containing copper 31. Thus, the amount of the oxide containing copper 31 increases in the positive electrode, improving the bonding strength with the aluminum oxide 21 and the oxide containing silicon 22.

[0071] On the other hand, the sodium ions 24 that have migrated to the negative electrode react with the copper-containing oxide 41 (see FIG. 7) in the areas where there is no magnesium-containing oxide 51b, reducing the copper oxide, and the copper-containing oxide 41 of the negative electrode that has reacted with the sodium ions 24 becomes Cu and is included in the metal layer 40. The sodium ions 24 are also oxidized to sodium oxide. In this way, the copper-containing oxide 41, which has a large adhesive force to both the aluminum oxide 21 and the silicon-containing oxide 22, is reduced. Also, the ceramics near the boundary of the metal layer 40 of the negative electrode board 2 At 0, the concentration of sodium ions (sodium oxide 23) increases, making it easier for aluminum oxide 21 particles to detach.

[0072] However, unlike Comparative Example 1, the ceramic laminate substrate 10 has magnesium oxide 26 disposed in the intermediate layers 50a and 50b. This blocks the reaction of sodium ions 24 with the copper-containing oxide 41. Therefore, in the area where the magnesium-containing oxide 51b is formed, the copper-containing oxide 41 exists without becoming Cu. In addition, magnesium oxide 26 exists at the grain boundaries and triple points of the aluminum oxide 21. This blocks the migration route of part of the silicon-containing oxide 22 at the grain boundaries, blocking the migration of part of the sodium ions 24. This suppresses the reaction of the sodium ions 24 with the copper-containing oxide 41. Therefore, in this area, the bonding strength between the ceramic plate 20 and the metal layer 40 is maintained.

[0073] As a result, in the ceramic laminate substrate 10 of Example 1-1, the decrease in the bonding strength from the ceramic plate 20 to the metal layer 40 is suppressed, and the bonding strength of the metal layer 40 to the ceramic plate 20 is improved, compared to Comparative Example 1.

[0074] According to Comparative Example 1, even without the intermediate layers 50a and 50b, the bonding strength of the metal layer 30 on the front surface (high potential side) of the ceramic plate 120 can be maintained to a certain degree, and the bonding strength of the metal layer 40 on the back surface (low potential side) of the ceramic plate 120 decreases. The intermediate layer 50b between the back surface (low potential side) of the ceramic plate 20 and the metal layer 40 of the ceramic laminate substrate 10 of the first embodiment suppresses the decrease in bonding strength of the metal layer 40. Therefore, in the ceramic laminate substrate 10, as long as there is at least the intermediate layer 50b between the back surface (low potential side) of the ceramic plate 20 and the metal layer 40, the decrease in bonding strength of the metal layer 40 is suppressed, and deterioration of the ceramic laminate substrate 10 can be prevented.

[0075] The semiconductor device 1 includes semiconductor chips 60a, 60b, 65a, and 65b, a bonding member 35, and a ceramic laminate substrate 10 having a plate shape, a front surface, and a back surface opposite to the front surface, and the semiconductor chips 60a, 60b, 65a, and 65b are bonded to the front surface via the bonding member 35. The ceramic laminate substrate 10 includes a ceramic plate 20, metal layers 30 and 40, and an intermediate layer 50b. The ceramic plate 20 is plate-shaped, has a first main surface (the front surface in the first embodiment) and a second main surface (the back surface in the first embodiment) opposite to the first main surface, and includes ceramic particles. The metal layer 30 is bonded to the first main surface of the ceramic plate 20 by applying a high potential voltage, and contains copper. The metal layer 40 is bonded to the second main surface of the ceramic plate 20 by applying a low potential voltage, and contains copper. The intermediate layer 50b is formed between the second main surface of the ceramic plate 20 and the low-potential metal layer 40, and contains an oxide 51b containing magnesium. In the ceramic laminate substrate 10, even when a high voltage is applied at high temperature, the oxide 51b containing magnesium prevents a decrease in the bondability of the metal layer 40 to the ceramic plate 20 due to the application of the oxide 51b containing magnesium between the ceramic plate 20 and the low-potential metal layer 40. This prevents deterioration of the ceramic laminate substrate 10, and prevents a decrease in the reliability of the semiconductor device 1.

[0076] In the first and second embodiments, when the metal layer 40 formed on the back surface of the ceramic plate 20 is grounded to have the same potential as the N terminal, the metal layer with a high potential is the metal layers 30a, 30b, and 30c formed on the front surface of the ceramic plate 20. The metal layer with a low potential is the metal layer 40 formed on the back surface of the ceramic plate 20.

[0077] In the first and second embodiments, when the metal layer 40 formed on the back surface of the ceramic plate 20 is grounded to have the same potential as the M terminal, or ground When the ceramic plate 20 is not fixed but floats, the high-potential metal layer is the metal layers 30a and 30b formed on the front surface of the ceramic plate 20, and the low-potential metal layer is the metal layer 40 formed on the rear surface of the ceramic plate 20 facing the metal layers 30a and 30b. In this case, the low-potential metal layer is the metal layer 30d formed on the front surface of the ceramic plate 20, and the high-potential metal layer is the metal layer 40 formed on the rear surface of the ceramic plate 20 facing the metal layer 30d.

[0078] The region (position) where the intermediate layer is required depending on the potential between the metal layer 30 and the metal layer 40 of the ceramic plate 20 when the semiconductor device 1 is operating or stopped will be described in the third embodiment.

[0079] In the present embodiment, the method of forming an oxide containing magnesium in the intermediate layers 50a, 50b has been described as coating the surface of a plate-shaped product with magnesium oxide powder in the ceramic plate preparation step (step S1a) and firing the product at a predetermined temperature for a predetermined time. However, the present invention is not limited to this method, and the surface of the plate-shaped product may be coated with a solution containing manganese and fired in the ceramic plate preparation step (step S1a). The intermediate layers 50a, 50b can also be formed with an oxide containing magnesium by sputtering or vapor deposition on the ceramic plate or metal foil during the ceramic plate preparation step (step S1a) and the metal foil preparation step (step S1b).

[0080] In the present embodiment, the method of forming an oxide containing manganese in the intermediate layers 50a, 50b has been described as being such that the metal foil is immersed in a manganese-containing solution and oxidized in the metal foil preparation step (step S1b). However, the present invention is not limited to this method, and the surface of the plate-shaped molded product may be coated with a powder or solution containing manganese and then fired in the ceramic plate preparation step (step S1a). The oxide containing manganese can also be formed in the intermediate layers 50a, 50b by forming manganese or an oxide containing manganese on the ceramic plate or metal foil by sputtering or vapor deposition during the ceramic plate preparation step (step S1a) or the metal foil preparation step (step S1b).

[0081] (Ceramic laminate substrate of Example 1-2) In the embodiment of Example 1-2, the ceramic plate 20 of the ceramic laminate substrate 10 is manufactured by coating magnesium oxide powder in step S1a of FIG. 4, and the metal layers 30, 40 are manufactured by a wet oxidation method. This will be described with reference to FIG. 9, FIG. 10, and FIG. 13. FIG. 9 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-2), and FIG. 10 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-2) at high temperature and high voltage. FIG. 9 shows a schematic microscopic state at a location corresponding to the area surrounded by the dashed line in FIG. 2. FIG. 10 also shows a schematic microscopic state when a high voltage is applied between the metal layers 30, 40 at high temperature in FIG. 2.

[0082] As shown in FIG. 9, the ceramic laminate substrate 10 of Example 1-2 is configured by laminating a metal layer 40, an intermediate layer 50b, a ceramic plate 20, an intermediate layer 50a, and a metal layer 30 in this order from the bottom.

[0083] The ceramic plate 20 is manufactured by applying magnesium oxide powder in step S1a of Fig. 4, similar to Example 1-1. Meanwhile, the metal layers 30, 40 are manufactured by a wet oxidation method in step S1b of Fig. 4, unlike Example 1-1. The ceramic plate 20 contains, as a second oxide, an oxide 22 having silicon between particles (grain boundaries and triple points) of the aluminum oxide 21, and sodium oxide 23. It may further contain magnesium oxide.

[0084] The metal layers 30 and 40 are mainly composed of copper. The intermediate layers 50a and 50b contain oxides 52a and 52b (Mg-Mn-O) containing magnesium and manganese as the first oxide. The oxides 52a and 52b containing magnesium and manganese are formed in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a and 50b. Furthermore, oxides 31 and 41 containing copper are formed at the boundaries between the metal layers 30 and 40, the ceramic plate 20, and the oxides 52a and 52b containing magnesium and manganese.

[0085] In Example 1-1, in the ceramic laminate substrate 10 (before the reliability test), the area covered by the intermediate layers 50a, 50b was limited, and it was not possible to increase the bonding strength between the ceramic plate 20 and the metal layers 30, 40. In Example 1-2, the intermediate layers 50a, 50b containing the oxides 52a, 52b containing magnesium and manganese can be formed widely. This makes it possible to increase the bonding strength between the ceramic plate 20 and the metal layers 30, 40 compared to Example 1-1. It is preferable that such intermediate layers 50a, 50b are formed so as to cover 20% or more and 80% or less of the bonding surface between the ceramic plate 20 and the metal layers 30, 40.

[0086] A peel strength evaluation test was also conducted on such a ceramic laminate substrate 10. The evaluation result for Example 1-2 was "Excellent" for both the front and back surfaces of the ceramic laminate substrate 10, as shown in FIG. 13. That is, even when the ceramic laminate substrate 10 was subjected to a reliability test, the bonding strength of the metal layer 40 to the back surface of the ceramic plate 20 was improved and the decrease in bonding was suppressed, compared to Example 1-1. The reason for this has not yet been fully elucidated, and although we are not bound by any theory, it can be considered as follows.

[0087] The ceramic laminate substrate 10 after the reliability test has a composition as shown in Fig. 10. When high potential (positive electrode) and low potential (negative electrode) voltages are applied to the metal layers 30 and 40 at high temperature, sodium oxide 23 (see Fig. 9) separates into sodium ions 24 and oxygen ions 25. The sodium ions 24 pass through the oxide 22 containing silicon at the grain boundaries and triple points of the aluminum oxide 21, and move to the low potential metal layer 40 side, which is the negative electrode. The oxygen ions 25 pass through the oxide 22 containing silicon at the grain boundaries of the aluminum oxide 21, and move to the high potential metal layer 30 side, which is the positive electrode.

[0088] The oxygen ions 25 that have migrated to the positive electrode react with the copper of the metal layer 30 to form an oxide containing copper 31. Thus, the amount of the oxide containing copper 31 increases in the positive electrode, improving the bonding strength with the aluminum oxide 21 and the oxide containing silicon 22.

[0089] In the ceramic laminate substrate 10 in Example 1-2, the magnesium oxide 26 is disposed at the grain boundaries and triple junctions of the aluminum oxide 21. Furthermore, the oxide 52b containing magnesium and manganese is formed at the boundary and triple junctions between the aluminum oxide 21 of the negative electrode and the metal layer 40 of the low potential. In particular, the region in which the oxide 52b containing magnesium and manganese is formed is wider than the oxide 51b containing magnesium in Example 1-1. Therefore, the sodium ions 24 that have moved to the negative electrode are blocked from moving to the oxide 52b containing magnesium and manganese. Therefore, the reaction between the sodium ions 24 and the oxide 41 containing copper is more inhibited than in Example 1-1. Therefore, the oxide 41 containing copper exists at the boundary between the aluminum oxide 21, the metal layer 40, and the oxide 52b containing magnesium and manganese without becoming Cu. Therefore, the bonding strength between the ceramic plate 20 and the metal layer 40 is maintained more than in Example 1-1.

[0090] As a result, in the ceramic laminate substrate 10 of Example 1-2, the decrease in the bonding strength from the ceramic plate 20 to the metal layer 40 is suppressed and the bonding strength of the metal layer 40 to the ceramic plate 20 is improved compared to the case of Example 1-1.

[0091] (Ceramic laminate substrates of Examples 1-3) In Example 1-3, a case where the ceramic plate 20 of the ceramic laminate substrate 10 is manufactured without coating magnesium oxide powder in step S1a of FIG. 4, and the metal layers 30, 40 are manufactured by a wet oxidation method will be described with reference to FIGS. 11, 12, and 13. FIG. 11 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-3), and FIG. 12 is a schematic cross-sectional view of the ceramic laminate substrate of the first embodiment (Example 1-3) at high temperature and high voltage. FIG. 11 shows a schematic microscopic state in the area surrounded by the dashed line in FIG. 2. FIG. 12 shows a schematic microscopic state when a high voltage is applied between the metal layers 30, 40 at high temperature in FIG. 2.

[0092] As shown in FIG. 11, the ceramic laminate substrate 10 of Example 1-3 is configured by laminating a metal layer 40, an intermediate layer 50b, a ceramic plate 20, an intermediate layer 50a, and a metal layer 30 in this order from the bottom.

[0093] Unlike Examples 1-1 and 1-2, the ceramic plate 20 was manufactured without coating magnesium oxide powder in step S1a of Fig. 4. Similarly to Example 1-2, the metal layers 30 and 40 were manufactured by a wet oxidation method in step S1b of Fig. 4. The ceramic plate 20 contains, as the second oxide, an oxide 22 having silicon between particles (grain boundaries and triple points) of the aluminum oxide 21 and sodium oxide 23.

[0094] The metal layers 30 and 40 are mainly composed of copper. The intermediate layers 50a and 50b contain manganese-containing oxides 53a and 53b (Mn-O) as the first oxide. The manganese-containing oxides 53a and 53b are formed in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a and 50b. Furthermore, copper-containing oxides 31 and 41, which are oxides containing copper, are formed at the boundaries between the metal layers 30 and 40, the ceramic plate 20, and the manganese-containing oxides 53a and 53b.

[0095] In the ceramic laminate substrate 10 (before reliability testing), if there is too much manganese-containing oxide 53a, 53b, the bonding strength between the ceramic plate 20 and the metal layers 30, 40 decreases. For this reason, the intermediate layers 50a, 50b containing the manganese-containing oxide 53a, 53b are preferably formed to cover 10% or more and 80% or less of the bonding surface between the ceramic plate 20 and the metal layers 30, 40, and more preferably 20% or more and 50% or less.

[0096] A peel strength evaluation test was also conducted on the ceramic laminate substrate 10. As shown in FIG. 13, the evaluation results for Example 1-3 were "Excellent" on the front surface of the ceramic laminate substrate 10 and "Very Good" on the back surface. In other words, even when the ceramic laminate substrate 10 was subjected to a reliability test, Example 1-1 Compared to the above, the bonding strength of the metal layer 40 to the rear surface of the ceramic plate 20 is somewhat improved, and the deterioration of the bonding property is suppressed. The reason for this has not yet been fully elucidated at present, and while not being bound by theory, it can be considered as follows.

[0097] The ceramic laminate substrate 10 after the reliability test has a composition as shown in Fig. 12. When high potential (positive electrode) and low potential (negative electrode) voltages are applied to the metal layers 30 and 40 at high temperature, sodium oxide 23 (see Fig. 11) separates into sodium ions 24 and oxygen ions 25. The sodium ions 24 pass through the oxide 22 containing silicon at the grain boundaries and triple points of the aluminum oxide 21, and move to the low potential metal layer 40 side, which is the negative electrode. The oxygen ions 25 pass through the oxide 22 containing silicon at the grain boundaries of the aluminum oxide 21, and move to the high potential metal layer 30 side, which is the positive electrode.

[0098] The oxygen ions 25 that have migrated to the positive electrode react with the copper of the metal layer 30 to form an oxide containing copper 31. Thus, the amount of the oxide containing copper 31 increases in the positive electrode, improving the bonding strength with the aluminum oxide 21 and the oxide containing silicon 22.

[0099] On the other hand, the sodium ions 24 that have migrated to the negative electrode react with the copper-containing oxide 41 (see FIG. 11) in the area where the manganese-containing oxide 53b is not present, reducing the copper oxide, and the copper-containing oxide 41 of the negative electrode that has reacted with the sodium ions 24 becomes Cu and is included in the metal layer 40. The sodium ions 24 are also oxidized to sodium oxide. In this way, the copper-containing oxide 41, which has a large adhesive force to both the aluminum oxide 21 and the silicon-containing oxide 22, decreases. In addition, the concentration of sodium ions (sodium oxide 23) increases at the grain boundaries and triple points of the silicon-containing oxide 22 near the boundary of the metal layer 40 of the negative electrode, making it easier for particles of the aluminum oxide 21 to detach.

[0100] However, in the ceramic laminate substrate 10 of Example 1-3, manganese oxide 27 is disposed in the intermediate layers 50a and 50b. Therefore, it blocks the reaction of sodium ions 24 with the copper-containing oxide 41. Therefore, in the area where the manganese-containing oxide 53b is formed, the copper-containing oxide 41 exists without becoming Cu. In addition, manganese oxide 27 is disposed in the grain boundaries and triple junctions of the aluminum oxide 21. Therefore, the migration route of part of the silicon-containing oxide 22 at the grain boundaries is blocked, and the migration of part of the sodium ions 24 is blocked. Therefore, the reaction between the sodium ions 24 and the copper-containing oxide 41 is suppressed. Therefore, in this area, the bonding strength between the ceramic plate 20 and the metal layer 40 is maintained. Also, the bonding strength at this time is the same as that in Example 1- 1 It is possible that it is larger than that.

[0101] As a result, in the ceramic laminate substrate 10 of Example 1-3, the decrease in the bonding strength from the ceramic plate 20 to the metal layer 40 is suppressed and the bonding strength of the metal layer 40 to the ceramic plate 20 is improved compared to the case of Example 1-1.

[0102] [Second embodiment] The ceramic plate 20 included in the ceramic laminate substrate 10 of the second embodiment further contains zirconium oxide (ZrO2) in comparison with the ceramic plate 20 of the first embodiment. Note that the second embodiment will also be described based on the semiconductor device 1 of the first embodiment (FIGS. 1 and 2).

[0103] (Method of manufacturing a semiconductor device) The ceramic laminate substrate 10 of the second embodiment is also manufactured according to the flowchart of the manufacturing method of the first embodiment shown in Fig. 4. In the second embodiment, when manufacturing the ceramic laminate substrate 10, first, a ceramic plate and a metal foil are prepared (steps S1a and S1b). Either step S1a or S1b may be performed first.

[0104] The preparation of the ceramic plate will be described (Step S1a). First, zirconium oxide (ZrO2) powder is added to aluminum oxide (Al2O3) powder together with silicon oxide (SiO2) powder, and the mixture is stirred with a binder and formed into a plate. Magnesium oxide (MgO) powder is applied to the surface of the plate-shaped molded product, and the product is fired at a predetermined temperature for a predetermined time. The ceramic plate thus fired contains aluminum oxide as ceramic particles, and contains an oxide containing zirconium and an oxide containing silicon (second oxide) at the grain boundaries and triple points of the ceramic particles, and an oxide containing magnesium is formed on the surface. In addition, an oxide containing magnesium may be formed at the grain boundaries and triple points of the ceramic particles. The presence of an oxide containing zirconium can increase the flexural strength compared to the case where there is no oxide containing zirconium.

[0105] To manufacture the ceramic plate 20 of the second embodiment, in addition to zirconium oxide (ZrO2) powder, powder of yttrium oxide (Y2O3), magnesium oxide (MgO) or calcium oxide (CaO) may be added. Alternatively, powder of partially stabilized zirconia may be added instead of powder of zirconium oxide (ZrO2). In this way, the ceramic plate 20 contains aluminum oxide as ceramic particles, and partially stabilized zirconia and an oxide containing silicon (second oxide) are contained at the grain boundaries and triple points of the ceramic particles. In this case, the partially stabilized zirconia is preferably calculated as zirconium oxide (ZrO2) zirconium The zirconium oxide (Y2O3) content is 2.5 mol% or more and 3.5 mol% or less. This makes it possible to further increase the flexural strength compared to the case where only zirconium oxide is used. The average particle size of the ceramic particles is 0.5 μm or more and 25 μm or less. More preferably, it is 1 μm or more and 10 μm or less.

[0106] In the ceramic plate 20, the content of aluminum oxide is 80 wt% or more and 95 wt% or less, more preferably 84 wt% or more and 92 wt% or less, calculated as oxide, based on the total amount of oxide. 、 The content of the oxide having silicon in the ceramic plate 20 is 5.0 wt% or more and 20.0 wt% or less, more preferably 8 wt% or more and 16 wt% or less, calculated as zirconium oxide (ZrO2) based on the total amount of the oxide. 、 The content is 0.01wt% or more and 3.0wt% or less, calculated as silicon oxide (SiO2), and more preferably 1.0wt% or more and 3.0wt% or less. If the content of silicon-containing oxide is too low, many voids remain in the ceramic plate, making it prone to cracking. On the other hand, if the content is too high, the thermal conductivity of the ceramic plate decreases, and the heat dissipation performance deteriorates.

[0107] Furthermore, the ceramic plate 20 of the second embodiment also contains various materials used in manufacturing in addition to ceramic particles, oxides containing magnesium, oxides containing silicon, and oxides containing zirconium. One example of such a material is an oxide containing sodium. For example, sodium oxide. The content of the oxide containing sodium in the ceramic plate 20 is 1.0% of the total amount calculated as oxide. 、 The content of the oxide containing sodium is 0.001wt% or more and 0.2wt% or less, and more preferably 0.002wt% or more and 0.2wt% or less, calculated as sodium oxide (Na2O). If the content of the oxide containing sodium is too small, it becomes difficult to refine the ceramic raw material powder. If the content is too large, β-alumina is formed, which tends to cause a decrease in insulation and strength. The ceramic plate 20 preferably does not contain β-alumina.

[0108] The preparation of the metal foil in step S1b is performed in the same manner as in the first embodiment. Moreover, the manufacturing method from step S2 onwards is performed in the same manner as in the first embodiment, using the ceramic plate prepared in step S1a of the second embodiment.

[0109] As a result, a ceramic laminate substrate 10 is manufactured in which the intermediate layers 50a, 50b are included between the ceramic plate 20 and the metal layers 30, 40. In such a ceramic laminate substrate 10, the intermediate layers 50a, 50b suppress the deterioration of the bonding between the metal layers 30, 40 and the ceramic plate 20. When the magnesium oxide powder is applied in step S1a of the second embodiment, the content of the oxide containing magnesium in the ceramic plate 20 and the intermediate layers 50a, 50b in the ceramic laminate substrate 10 is 0.1 wt% or more and 1.5 wt% or less in terms of magnesium oxide (MgO) with respect to the total amount calculated as oxide. Furthermore, in this case, the content of magnesium calculated as magnesium oxide (MgO) is 2.0 wt% or more and 20.0 wt% or less with respect to the content of zirconium calculated as zirconium oxide (ZrO2), and more preferably 7.5 wt% or more and 15 wt% or less. In the case where the coating of magnesium oxide powder is not performed in step S1a of the second embodiment, the ceramic laminate substrate 10 does not contain magnesium (it is less than the measurement lower limit of 0.01 wt%). In addition, in the case where the wet oxidation method using the manganese-containing solution is performed in step S1b, the content of manganese oxide in the ceramic plate 20 and the intermediate layers 50a, 50b in the ceramic laminate substrate 10 is 0.01 wt% or more and 0.15 wt% or less. Furthermore, in this case, the content of manganese calculated as manganese oxide is 0.05 wt% or more and 2 wt% or less, more preferably 0.2 wt% or more and 0.8 wt% or less, relative to the content of zirconium calculated as zirconium oxide. In the case where the wet oxidation method using the manganese-containing solution is not performed in step S1b, the content of manganese is not confirmed in the ceramic laminate substrate 10, and is less than the measurement lower limit of 0.01 wt%.

[0110] Also, in the second embodiment, without being limited thereto, when preparing the ceramic plate (step S1a) and the metal foil (step S1b), magnesium or an oxide containing magnesium can be formed on the intermediate layers 50a, 50b by forming magnesium or an oxide containing magnesium on the ceramic plate or the metal foil by sputtering or vapor deposition. In the ceramic plate preparation step (step S1a), magnesium or a powder or solution containing magnesium may be applied to the surface of the plate-shaped molded product, and then fired.

[0111] In the following, examples 2-1 to 2-3 corresponding to the intermediate layers 50a, 50b in the ceramic laminate substrate 10 including ceramic plates mainly composed of aluminum oxide and zirconium oxide will be described. In the second embodiment, the same reliability test as in the first embodiment is performed.

[0112] (Ceramic laminate substrate of comparative example 2) In the following, in order to explain the suppression of the decrease in the bonding strength of the metal layers 30, 40 by the intermediate layers 50a, 50b in the ceramic plate 20 of the second embodiment, a ceramic laminate substrate 10 not including the intermediate layers 50a, 50b will be described as Comparative Example 2 with reference to Figs. 14 and 15. Fig. 14 is a schematic cross-sectional view of the ceramic laminate substrate of Comparative Example 2, and Fig. 15 is a schematic cross-sectional view of the ceramic laminate substrate of Comparative Example 2 at high temperature and high voltage. Fig. 14 shows a schematic microscopic state in the area surrounded by the dashed line in Fig. 2. Fig. 15 shows a schematic microscopic state when a high voltage is applied between the metal layers 30, 40 at high temperature in Fig. 2.

[0113] The ceramic plate 120 of Comparative Example 2 was manufactured without coating magnesium oxide powder in step S1a (second embodiment) of Fig. 4. The metal layers 30 and 40 were manufactured by a dry oxidation method in step S1b of Fig. 4.

[0114] The ceramic laminated substrate 100 thus manufactured is configured by laminating a metal layer 40, a ceramic plate 120, and a metal layer 30 in this order from the bottom, as shown in FIG. 14. The ceramic plate 120 contains, as a second oxide, an oxide 22 containing silicon between particles (grain boundaries and triple points) of an aluminum oxide 21, and zirconium oxide 28. It may further contain sodium oxide 23. Note that instead of zirconium oxide 28, an oxide containing zirconium may be used, for example, partially stabilized zirconia. Also, the metal layers 30 and 40 are configured with copper as the main component, similarly to the first embodiment.

[0115] The comparative ceramic laminate substrate 100 does not contain magnesium or manganese. That is, the ceramic laminate substrate 100 thus manufactured does not have the intermediate layers 50a, 50b containing an oxide having at least one of magnesium and manganese.

[0116] The ceramic laminate substrate 100 was also subjected to the peel strength evaluation test similar to that of the first embodiment. The evaluation results were "Not Good" on both the front and back surfaces of the ceramic plate (table not shown). The reason for this has not yet been fully elucidated, and while not being bound by any theory, it can be considered as follows.

[0117] 15, in the ceramic laminate substrate 100 of Comparative Example 2, a high potential (positive electrode) and a low potential (negative electrode) voltage are applied to the metal layers 30, 40 at high temperatures. This reduces the copper-containing oxide 41 (Cu-O) formed at the boundary between the negative metal layer 40 and the zirconium oxide 28 of the ceramic plate 120. For example, CuO+2e (electrons)→Cu+O 2- As a result, the copper-containing oxide 41 is reduced on the negative electrode side, and the metal layer 40 and the ceramic Board 120The bonding strength between the two electrodes is reduced. Oxygen ions 25 generated by the reduction of the copper-containing oxide 41 (Cu-O) pass through the grain boundaries of the aluminum oxide 21 and the zirconium oxide 28 at the triple point, and move to the positive electrode, that is, the high-potential metal layer 30 side. The oxygen ions 25 that have moved to the positive electrode react with the copper of the metal layer 30, and grow the copper-containing oxide 31. For example, Cu+O 2- →CuO+2e (electrons) reaction occurs. Therefore, in the positive electrode, the oxide 31 containing copper increases excessively, and the metal layer 30 and the ceramic Board 120 The bonding strength decreases.

[0118] In the ceramic plate 120 of the ceramic laminate substrate 100 of Comparative Example 2 in the second embodiment, as described above, the movement of oxygen ions is promoted by zirconium oxide. Therefore, reduction proceeds on the negative electrode side, and oxidation proceeds on the positive electrode side. Therefore, the ceramic plate 120 of Comparative Example 2 in the first embodiment is further improved than that of Comparative Example 1 in the first embodiment. Board 120 The bonding strength of the metal layers 30 and 40 to the metal layer 30 and 40 decreases.

[0119] (Ceramic laminate substrate of Example 2-1) Next, the ceramic laminate substrate 10 including the intermediate layers 50a, 50b will be described with reference to Figs. 16 and 17. Example 2-1 corresponds to Example 1-1. Fig. 16 is a schematic cross-sectional view of the ceramic laminate substrate of the second embodiment (Example 2-1), and Fig. 17 is a schematic cross-sectional view of the ceramic laminate substrate of the second embodiment (Example 2-1) at high temperature and high voltage. Fig. 16 shows a schematic microscopic state in the area surrounded by the dashed line in Fig. 2. Fig. 17 shows a schematic microscopic state when a high voltage is applied between the metal layers 30, 40 at high temperature in Fig. 2.

[0120] As shown in FIG. 16, the ceramic laminate substrate 10 of Example 2-1 is configured by laminating a metal layer 40, an intermediate layer 50b, a ceramic plate 20, an intermediate layer 50a, and a metal layer 30 in this order from the bottom.

[0121] The ceramic plate 20 is produced by applying magnesium oxide powder in step S1a (second embodiment) of Fig. 4. The metal layers 30 and 40 are produced by a dry oxidation method in step S1b of Fig. 4.

[0122] The ceramic plate 20 contains, as the second oxide, an oxide 22 containing silicon between particles (grain boundaries and triple points) of the aluminum oxide 21, and zirconium oxide 28. It may further contain sodium oxide 23 and magnesium oxide. Note that instead of the zirconium oxide 28, an oxide containing zirconium may be used, for example, partially stabilized zirconia.

[0123] Similarly to the first embodiment, the metal layers 30 and 40 are mainly composed of copper. The intermediate layers 50a and 50b contain magnesium-containing oxides 51a and 51b as the first oxide. The magnesium-containing oxides 51a and 51b are formed in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a and 50b. Furthermore, copper-containing oxides 31 and 41 are formed at the boundaries between the metal layers 30 and 40 and the ceramic plate 20, and at the boundaries between the magnesium-containing oxides 51a and 51b, the metal layers 30 and 40, and the ceramic plate 20.

[0124] In the ceramic laminate substrate 10 (before reliability testing), if the magnesium-containing oxides 51a, 51b are too large, the bonding strength between the ceramic plate 20 and the metal layers 30, 40 decreases. For this reason, the intermediate layers 50a, 50b containing the magnesium-containing oxides 51a, 51b are preferably formed to cover 10% or more and 80% or less of the bonding surface between the ceramic plate 20 and the metal layers 30, 40, and more preferably 20% or more and 50% or less.

[0125] A peel strength evaluation test was also conducted on this ceramic laminate substrate 10. The evaluation results for Example 2-1 were "Good" for the front surface of the ceramic laminate substrate 10 and "Good" for the back surface. That is, in the ceramic laminate substrate 10, the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is somewhat improved compared to the comparative example, and the decrease in bonding is suppressed. The reason for this has not yet been fully elucidated, and while not being bound by theory, it can be considered as follows.

[0126] As shown in FIG. 17, in the ceramic laminate substrate 10 of Example 2-1, a high potential (positive electrode) and a low potential (negative electrode) voltage are applied to the metal layers 30 and 40 at high temperature. In the area where the intermediate layer 50b containing the magnesium-containing oxide 51b is not present, the copper-containing oxide 41 (Cu-O) is reduced at the boundary between the metal layer 40 on the negative electrode side and the zirconium oxide 28 of the ceramic plate 20. However, unlike Comparative Example 2, the ceramic laminate substrate 10 has the intermediate layer 50b containing the magnesium-containing oxide 51b arranged on the negative electrode side. Therefore, in the area where the intermediate layer 50b is formed on the negative electrode side, the zirconium oxide 28 and the copper-containing oxide 41 (Cu-O) do not come into direct contact with each other, and the reduction of the copper-containing oxide 41 is suppressed. In other words, the intermediate layer 50b blocks the reduction of the copper-containing oxide 41. Therefore, in the area where the intermediate layer 50b is formed, the oxide 41 containing copper is present without becoming copper. In addition, since reduction at the negative electrode is suppressed, the generation of oxygen ions is reduced, and excessive oxidation of copper at the boundary between the metal layer 30 and the ceramic plate 20 on the positive electrode side is suppressed. Therefore, since the intermediate layer 50b containing the oxide 51b containing magnesium is formed on the negative electrode side, the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is somewhat improved compared to Comparative Example 2, and a decrease in bonding property is suppressed.

[0127] The magnesium oxide 26 may be present at the grain boundaries and triple junctions. This partially blocks the migration route of oxygen ions at the grain boundaries. This also suppresses the oxidation-reduction reaction at the positive and negative electrodes. The ceramic laminate substrate 10 may have an intermediate layer 50a including an oxide 51a containing magnesium formed on the positive electrode side. This prevents direct contact between the zirconium oxide 28 and the oxide 31 (Cu-O) containing copper in the portion where the intermediate layer 50b is formed on the positive electrode side, suppressing oxidation of the metal layer 30. In other words, the intermediate layer 50a blocks oxidation of the metal layer 30. This further improves the bonding strength of the metal layers 30 and 40 to the ceramic plate 20, suppressing a decrease in bonding strength.

[0128] As described above, in the ceramic laminate substrate 10 of Example 2-1, similar to Example 1-1, a decrease in the bonding strength from the ceramic plate 20 to the metal layer 40 is suppressed, and the bonding strength of the metal layer 40 to the ceramic plate 20 is improved. In the ceramic laminate substrate 10 of Example 2-1, similar to Example 1-1, as long as there is at least an intermediate layer 50b between the rear surface (low potential side) of the ceramic plate 20 and the metal layer 40, a decrease in the bonding property of the metal layer 40 is suppressed, and deterioration of the ceramic laminate substrate 10 can be prevented.

[0129] (Ceramic laminate substrate of Example 2-2) In Example 2-2, a case where the ceramic plate 20 of the ceramic laminate substrate 10 is manufactured by coating magnesium oxide powder in step S1a (second embodiment) of FIG. 4, and the metal layers 30, 40 are manufactured by a wet oxidation method will be described with reference to FIG. 18 and FIG. 19. FIG. 18 is a schematic cross-sectional view of the ceramic laminate substrate of the second embodiment (Example 2-2), and FIG. 19 is a schematic cross-sectional view of the ceramic laminate substrate of the second embodiment (Example 2-2) at high temperature and high voltage. FIG. 18 shows a schematic microscopic state at a location corresponding to the area surrounded by the dashed line in FIG. 2. FIG. 19 shows a schematic microscopic state when a high voltage is applied between the metal layers 30, 40 at high temperature in FIG. 2.

[0130] As shown in FIG. 18, the ceramic laminate substrate 10 of Example 2-2 is configured by laminating a metal layer 40, an intermediate layer 50b, a ceramic plate 20, an intermediate layer 50a, and a metal layer 30 in this order from the bottom.

[0131] The ceramic plate 20 was produced by applying magnesium oxide powder in step S1a (second embodiment) of Fig. 4, similarly to Example 2-1. Moreover, unlike Example 2-1, the metal layers 30 and 40 were produced by a wet oxidation method in step S1b of Fig. 4.

[0132] The ceramic plate 20 contains, as the second oxide, an oxide 22 containing silicon between particles (grain boundaries and triple points) of the aluminum oxide 21, and zirconium oxide 28. It may further contain sodium oxide 23 and magnesium oxide. Note that instead of the zirconium oxide 28, an oxide containing zirconium may be used, for example, partially stabilized zirconia.

[0133] The metal layers 30 and 40 are mainly composed of copper. The intermediate layers 50a and 50b contain, as the first oxide, oxides 52a and 52b containing magnesium and manganese, respectively, as in Example 1-2. The oxides 52a and 52b containing magnesium and manganese are formed in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a and 50b. Furthermore, oxides 31 and 41 containing copper are formed at the boundaries between the metal layers 30 and 40, the ceramic plate 20, and the oxides 52a and 52b containing magnesium and manganese, respectively.

[0134] In Example 2-1, in the ceramic laminate substrate 10 (before the reliability test), the area covered by the intermediate layers 50a, 50b was limited, and it was not possible to increase the bonding strength between the ceramic plate 20 and the metal layers 30, 40. In Example 2-2, the intermediate layers 50a, 50b containing the oxides 52a, 52b containing magnesium and manganese can be formed widely. This makes it possible to increase the bonding strength between the ceramic plate 20 and the metal layers 30, 40 compared to Example 2-1. It is preferable that such intermediate layers 50a, 50b are formed so as to cover 20% or more and 80% or less of the bonding surface between the ceramic plate 20 and the metal layers 30, 40.

[0135] A peel strength evaluation test was also conducted on such a ceramic laminate substrate 10. The evaluation result for Example 2-2 was "Excellent" for the front surface of the ceramic laminate substrate 10 and "Excellent" for the back surface. That is, in the ceramic laminate substrate 10, the decrease in the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is significantly suppressed compared to the comparative example. Furthermore, the decrease in the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is suppressed more than in Example 2-1. The reason for this has not yet been fully elucidated, and although we are not bound by any theory, it can be considered as follows.

[0136] As shown in FIG. 19, in the ceramic laminate substrate 10 of Example 2-2, a high potential (positive electrode) and a low potential (negative electrode) voltage are applied to the metal layers 30, 40 at high temperature. In the ceramic laminate substrate 10, an intermediate layer 50b including an oxide 52b containing magnesium and manganese is arranged on the negative electrode side. Therefore, in the portion on the negative electrode side where the intermediate layer 50b is formed, the zirconium oxide 28 and the oxide 41 containing copper (Cu-O) do not come into direct contact with each other, and the reduction of the oxide 41 containing copper is suppressed. That is, the intermediate layer 50b blocks the reduction of the oxide 41 containing copper. Therefore, in the portion where the intermediate layer 50b is formed, the oxide 41 containing copper exists without becoming copper. In addition, since the reduction at the negative electrode is suppressed, the generation of oxygen ions is small, and the excessive oxidation of copper at the boundary between the metal layer 30 and the ceramic plate 20 on the positive electrode side is suppressed. Therefore, by forming the intermediate layer 50b including the oxide 52b having magnesium and manganese on the negative electrode side, the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is significantly improved and the decrease in bonding property is suppressed compared to Comparative Example 2. Furthermore, it is considered that the decrease in the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is suppressed more than in Examples 2-1 and 2-3 described later because reduction is blocked more than in Example 2-1 and Example 2-3 described later.

[0137] Magnesium oxide 26 may also be present at grain boundaries and triple junctions. This will partially block the migration route of oxygen ions at the grain boundaries. This will also suppress the oxidation-reduction reaction at the positive and negative electrodes. The ceramic laminate substrate 10 may also have an intermediate layer 50a formed on the positive electrode side, which includes an oxide 52a containing magnesium and manganese. This will allow the intermediate layer 50 to be formed on the positive electrode side. a In the portion where the intermediate layer 50a is formed, the zirconium oxide 28 and the copper-containing oxide 31 (Cu-O) are not in direct contact with each other, and oxidation of the metal layer 30 is suppressed. In other words, the intermediate layer 50a blocks oxidation of the metal layer 30. This further improves the bonding strength of the metal layers 30, 40 to the ceramic plate 20, and suppresses deterioration of the bondability.

[0138] As a result, in the ceramic laminate substrate 10 of Example 2-2, the decrease in the bonding strength from the ceramic plate 20 to the metal layer 40 is further suppressed, and the bonding strength of the metal layer 40 to the ceramic plate 20 is improved, compared to Example 2-1 and Example 2-3 described below.

[0139] (Ceramic laminate substrate of Example 2-3) In Example 2-3, a case where the ceramic plate 20 of the ceramic laminate substrate 10 is manufactured without coating magnesium oxide powder in step S1a (second embodiment) of FIG. 4, and the metal layers 30, 40 are manufactured by a wet oxidation method will be described with reference to FIG. 20 and FIG. 21. FIG. 20 is a schematic cross-sectional view of the ceramic laminate substrate of the second embodiment (Example 2-3), and FIG. 21 is a schematic cross-sectional view of the ceramic laminate substrate of the second embodiment (Example 2-3) at high temperature and high voltage. FIG. 20 shows a schematic microscopic state in the area surrounded by the dashed line in FIG. 2. FIG. 21 shows a schematic microscopic state when a high voltage is applied between the metal layers 30, 40 at high temperature in FIG. 2.

[0140] As shown in FIG. 20, the ceramic laminate substrate 10 of Example 2-3 is configured by laminating a metal layer 40, an intermediate layer 50b, a ceramic plate 20, an intermediate layer 50a, and a metal layer 30 in this order from the bottom.

[0141] Unlike Examples 2-1 and 2-2, the ceramic plate 20 was manufactured without coating magnesium oxide powder in step S1a (second embodiment) of Fig. 4. Moreover, the metal layers 30 and 40 were manufactured by the wet oxidation method in step S1b of Fig. 4, similar to Example 2-2.

[0142] The ceramic plate 20 contains, as the second oxide, an oxide 22 containing silicon between particles (grain boundaries and triple points) of the aluminum oxide 21, and zirconium oxide 28. It may further contain sodium oxide 23. Note that instead of the zirconium oxide 28, an oxide containing zirconium may be used, for example, partially stabilized zirconia.

[0143] The metal layers 30 and 40 are mainly composed of copper. The intermediate layers 50a and 50b contain manganese-containing oxides 53a and 53b, respectively, as the first oxide. The manganese-containing oxides 53a and 53b are formed in large amounts on the front and back sides of the ceramic plate 20 in the intermediate layers 50a and 50b. Furthermore, at the boundaries between the metal layers 30 and 40, the ceramic plate 20, and the manganese-containing oxides 53a and 53b, Copper In the present embodiment, oxides 31 and 41 having the following properties are formed.

[0144] In the ceramic laminate substrate 10 (before reliability testing), if there is too much manganese-containing oxide 53a, 53b, the bonding strength between the ceramic plate 20 and the metal layers 30, 40 decreases. For this reason, the intermediate layers 50a, 50b containing the manganese-containing oxide 53a, 53b are preferably formed to cover 10% or more and 80% or less of the bonding surface between the ceramic plate 20 and the metal layers 30, 40, and more preferably 20% or more and 50% or less.

[0145] A peel strength evaluation test was also conducted on such a ceramic laminate substrate 10. The evaluation result for Example 2-2 was "Excellent" for the front surface of the ceramic laminate substrate 10 and "Very Good" for the back surface. That is, in the ceramic laminate substrate 10, the decrease in the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is suppressed compared to Comparative Example 2. Furthermore, the decrease in the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is suppressed more than in Example 2-1. The reason for this has not yet been fully elucidated at this point in time, and although we are not bound by any theory, it can be considered as follows.

[0146] As shown in FIG. 21, in the ceramic laminate substrate 10 of Example 2-3, a high potential (positive electrode) and a low potential (negative electrode) voltage are applied to the metal layers 30, 40 at high temperature. The ceramic laminate substrate 10 has an intermediate layer 50b including a manganese-containing oxide 53b arranged on the negative electrode side. Therefore, in the portion on the negative electrode side where the intermediate layer 50b is formed, the zirconium oxide 28 and the copper-containing oxide 41 (Cu-O) do not come into direct contact with each other, and the reduction of the copper-containing oxide 41 is suppressed. That is, the intermediate layer 50b blocks the reduction of the copper-containing oxide 41. Therefore, in the portion where the intermediate layer 50b is formed, the copper-containing oxide 41 exists without becoming copper. In addition, since the reduction at the negative electrode is suppressed, the generation of oxygen ions is small, and the excessive oxidation of copper at the boundary between the metal layer 30 and the ceramic plate 20 is suppressed even on the positive electrode side. Therefore, the manganese-containing oxide 53b on the negative electrode side is not directly contacted with the zirconium oxide 28 and the copper-containing oxide 41 (Cu-O) is suppressed. 53b By forming the intermediate layer 50b including the above, the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is improved and the decrease in bonding property is suppressed compared to Comparative Example 2. Furthermore, it is considered that the decrease in the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is suppressed more than in Example 2-1 because the reduction is blocked more than in Example 2-1.

[0147] Furthermore, the ceramic laminate substrate 10 may have an intermediate layer 50a including an oxide 53a containing manganese formed on the positive electrode side. In this way, in the portion on the positive electrode side where the intermediate layer 50b is formed, the zirconium oxide 28 and the oxide 31 containing copper (Cu-O) are not in direct contact with each other, and oxidation of the metal layer 30 is suppressed. In other words, the intermediate layer 50a blocks oxidation of the metal layer 30. In this way, the bonding strength of the metal layers 30, 40 to the ceramic plate 20 is further improved, and a decrease in bonding property is suppressed.

[0148] As a result, in the ceramic laminate substrate 10 of Example 2-3, the decrease in the bonding strength from the ceramic plate 20 to the metal layer 40 is further suppressed compared to Example 2-1, and the bonding strength of the metal layer 40 to the ceramic plate 20 is improved.

[0149] [Third embodiment] As described in the first and second embodiments, in the ceramic laminate substrate 10, layer One of 30 and 40 is at a high potential, and the other is a metal layer When the other of 30 and 40 is at a low potential, at least one metal having a low potential is layer An intermediate layer is formed between the metal (with the intermediate layer) and the ceramic plate 20. layer Peeling off is suppressed.

[0150] In the third embodiment, in the semiconductor device 1 shown in FIGS. 1 to 3, the metal of the ceramic laminate substrate 10 when the semiconductor device 1 is in operation and when it is stopped is layer Based on the potential difference across 30 and 40, the region where the intermediate layer is required will be described.

[0151] First, the semiconductor device 1 will be described when it is stopped. When the semiconductor device 1 is stopped, the control signals input to the control electrodes 61a, 61b of the semiconductor chips 60a, 60b are each off. Therefore, in the ceramic laminate substrate 10, the metal layers 30a, 30b are at a high potential, and the metal layer 30d is at a low potential. The upper arm portion A and the lower arm portion B at this time are each called a stopped state. The stopped state of the semiconductor device 1 corresponds to FIGS. 22(A), 23(A), and 24(A), respectively, which will be described later.

[0152] The operation of the semiconductor device 1 will now be described. When the semiconductor device 1 is operated, the control signal input to the control electrode 61a of the semiconductor chip 60a is on, and the control signal input to the control electrode 61b of the semiconductor chip 60b is off. Therefore, in the ceramic laminate substrate 10, the metal layers 30a, 30b, and 30c are at high potential, and the metal layer 30d is at low potential. In this case, the upper arm portion A is called the operating state, and the lower arm portion B is called the stopped state. The operation of the semiconductor device 1 corresponds to the cases of Figures 22(B), 23(B), and 24(B) described later.

[0153] When the semiconductor device 1 is driven in another manner, the control electrode 61a of the semiconductor chip 60a The control signal input to is off, and the control electrode 61b of the semiconductor chip 60b The control signal input to is on. Therefore, in the ceramic laminate substrate 10, the metal layers 30a and 30b are at a high potential, and the metal layers 30c and 30d are at a low potential. In this case, the upper arm portion A is called a stopped state, and the lower arm portion B is called a driven state. The driving states of the semiconductor device 1 correspond to the cases shown in Figs. 22(C), 23(C), and 24(C) described later.

[0154] Next, the metal of the ceramic laminate substrate 10 layer The regions requiring an intermediate layer for each of the potentials 30 and 40 will be described with reference to Figs. 22 to 25. Fig. 22 is a diagram for explaining the region requiring an intermediate layer in the ceramic laminate substrate (back metal layer is at a low potential) of the third embodiment. Fig. 23 is a diagram for explaining the region requiring an intermediate layer in the ceramic laminate substrate (back metal layer is at a high potential) of the third embodiment. Fig. 24 is a diagram for explaining the region requiring an intermediate layer in the ceramic laminate substrate (back metal layer is at a floating potential) of the third embodiment. Fig. 25 is a diagram for explaining the region requiring an intermediate layer in the ceramic laminate substrate of the third embodiment.

[0155] 22 to 24 show simplified views of the ceramic laminate substrate 10, the semiconductor chips 60a and 60b, and the external connection terminals 71 to 75 shown in FIG. 2. Only components necessary for the explanation are labeled with reference numerals. Upper A Group A and Lower A This corresponds to the case where the arm B is in a stopped state. Upper A Arm section A is in the driving state, Lower A This corresponds to the case where the arm B is in a stopped state. Upper A When the A part is stopped, Lower A This corresponds to the case where arm portion B is in a driving state. Figures 22(D), 23(D), and 24(D) respectively show the formation region of the intermediate layer.

[0156] With reference to FIG. 22, a case where the metal layer 40, which is the back metal layer in the ceramic laminate substrate 10, is at a low potential will be described. At this time, when the upper arm portion A and the lower arm portion B are in a stopped state, as shown in FIG. 22(A), the metal layers 30a and 30b are at a high potential, and the metal layer 30d is at a low potential. The metal layer 30c is at a floating potential. A potential difference occurs between the high potential metal layers 30a and 30b and the low potential metal layer 40 in the ceramic plate 20 (P1 and P2 regions shown by the dashed lines). For this reason, it is considered that peeling of the metal layer 40 occurs between the ceramic plate 20 in the P1 region and the region of the metal layer 40 facing the metal layer 30a. It is also considered that peeling of the metal layer 40 occurs between the ceramic plate 20 in the P2 region and the region of the metal layer 40 facing the metal layer 30b.

[0157] Next, when the upper arm section A is in a driving state and the lower arm section B is in a stopped state, as shown in FIG. 22(B), the metal layers 30a, 30b, and 30c are at a high potential, and the metal layer 30d is at a low potential. In the ceramic plate 20, a potential difference occurs between the high-potential metal layers 30a, 30b, and 30c and the low-potential metal layer 40 (areas P1 to P3 shown by dashed lines). For this reason, peeling of the metal layer 40 may occur between the ceramic plate 20 in the P1 region and the region of the metal layer 40 facing the metal layer 30a. Peeling of the metal layer 40 may occur between the ceramic plate 20 in the P2 region and the region of the metal layer 40 facing the metal layer 30b. Peeling of the metal layer 40 may occur between the ceramic plate 20 in the P3 region and the region of the metal layer 40 facing the metal layer 30c.

[0158] Next, when the upper arm section A is in a stopped state and the lower arm section B is in a driven state, as shown in FIG. 22(C), the metal layers 30a and 30b are at a high potential and the metal layers 30c and 30d are at a low potential. A potential difference occurs between the high potential metal layers 30a and 30b and the low potential metal layer 40 (areas P1 and P2 shown by dashed lines) in the ceramic plate 20. For this reason, it is considered that peeling of the metal layer 40 occurs between the ceramic plate 20 in the P1 area and the area of ​​the metal layer 40 facing the metal layer 30a. It is also considered that peeling of the metal layer 40 occurs between the ceramic plate 20 in the P2 area and the area of ​​the metal layer 40 facing the metal layer 30b.

[0159] In the above-mentioned FIG. 22(A)-FIG. 22(C), it is necessary to form an intermediate layer in the L1-L3 regions shown in FIG. 22(D) based on the potential difference generated when the semiconductor device 1 is stopped and driven. The L1 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30a. The L2 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30b. The L3 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30c. In particular, according to FIG. 22(A)-FIG. 22(C), it is considered that the potential difference occurs frequently between the ceramic plate 20 and the region of the metal layer 40 facing the metal layers 30a and 30b. For this reason, it is necessary to form an intermediate layer at least in the L1 and L2 regions.

[0160] 23, a case will be described in which the metal layer 40, which is the back metal layer in the ceramic laminate substrate 10, is at a high potential. In this case, when the upper arm portion A and the lower arm portion B are in a stopped state, as shown in FIG. 23(A), the metal layers 30a and 30b are at a high potential, and the metal layer 30d is at a low potential. The metal layer 30c is at a floating potential. In the ceramic plate 20, a potential difference occurs between the low potential metal layer 30d and the high potential metal layer 40 (region P4 indicated by the dashed line). For this reason, it is considered that the metal layer 30d may peel off between the ceramic plate 20 and the metal layer 30d in the P4 region.

[0161] Next, when the upper arm portion A is in a driving state and the lower arm portion B is in a stopped state, as shown in Fig. 23(B), the metal layers 30a, 30b, and 30c are at a high potential, and the metal layer 30d is at a low potential. A potential difference is generated between the low-potential metal layer 30d and the high-potential metal layer 40 in the ceramic plate 20 (region P4 indicated by the dashed line). This may cause peeling of the metal layer 30d between the ceramic plate 20 and the metal layer 30d in the P4 region.

[0162] Next, when the upper arm portion A is in a stopped state and the lower arm portion B is in a driven state, as shown in FIG. 23(C), the metal layers 30a and 30b are at a high potential and the metal layers 30c and 30d are at a low potential. A potential difference occurs between the low potential metal layers 30c and 30d and the high potential metal layer 40 in the ceramic plate 20 (areas P3 and P4 shown by dashed lines). For this reason, it is considered that the metal layer 30c may peel off between the ceramic plate 20 and the metal layer 30c in the P3 area. It is also considered that the metal layer 30d may peel off between the ceramic plate 20 and the metal layer 30d in the P4 area.

[0163] 23(A) to 23(C), based on the potential difference that occurs when the semiconductor device 1 is stopped and driven, it is necessary to form an intermediate layer in the L4 and L5 regions shown in FIG. 23(D). The L4 region is the boundary between the ceramic plate 20 and the metal layer 30c. The L5 region is the boundary between the ceramic plate 20 and the metal layer 30d. In particular, according to FIG. 23(A) to FIG. 23(C), it is considered that the potential difference occurs frequently between the ceramic plate 20 and the metal layer 30d. For this reason, it is necessary to form an intermediate layer at least in the L5 region.

[0164] With reference to FIG. 24, a case will be described where the metal layer 40, which is the back metal layer in the ceramic laminate substrate 10, is at a floating potential. That is, when the semiconductor device 1 is not operating, no potential is applied to the metal layer 40. At this time, when the upper arm portion A and the lower arm portion B are in a stopped state, as shown in FIG. 24(A), the metal layers 30a and 30b are at a high potential, and the metal layer 30d is at a low potential. At this time, the metal layer 40, which is the back metal layer, is at a potential according to the area ratio of the potential on the front surface. In this embodiment, the area of ​​the high potential is larger than the area of ​​the low potential (see FIG. 1). Therefore, the metal layer 40 is at a potential closer to the high potential than to the low potential. Therefore, in the ceramic plate 20, the low potential metal layer 30d and the metal layer A potential difference occurs between the ceramic plate 20 and the metal layer 30d in the P4 region (region P4 indicated by the dashed line).

[0165] Next, when upper arm portion A is in a driven state and lower arm portion B is in a stopped state, as shown in FIG. 24(B), metal layers 30a, 30b, and 30c are at a high potential, and metal layer 30d is at a low potential. At this time, metal layer 40, which is the back surface metal layer, is at a potential according to the area ratio of the potential on the front surface. In this embodiment, the area of ​​the high potential is much larger than the area of ​​the low potential (see FIG. 1). Therefore, metal layer 40 is at a potential approximately equal to the high potential. Therefore, genus The layer 40 has a potential substantially equal to that of the metal layers 30a, 30b, and 30c. A potential difference occurs between the low-potential metal layer 30d and the high-potential metal layer 40 (area P4 indicated by the dashed line) in the ceramic plate 20. This may cause peeling of the metal layer 30d between the ceramic plate 20 and the metal layer 30d in the area P4.

[0166] Next, when the upper arm portion A is in a stopped state and the lower arm portion B is in a driven state, as shown in FIG. 24(C), the metal layers 30a and 30b are at a high potential, and the metal layers 30c and 30d are at a low potential. At this time, the metal layer 40, which is the back metal layer, is at a potential according to the area ratio of the potential on the front surface. In this embodiment, the area of ​​the high potential and the area of ​​the low potential are almost the same (see FIG. 1). Therefore, the metal layer 40 is at a potential almost intermediate between the high potential and the low potential. In the ceramic plate 20, a potential difference of half the difference between the high potential and the low potential is generated between the high potential metal layers 30a and 30b and the metal layer 40 (areas P1 and P2 shown by dashed lines). In addition, a potential difference of half the difference between the high potential and the low potential is generated between the low potential metal layers 30c and 30d and the metal layer 40 (areas P3 and P4 shown by dashed lines). For this reason, peeling may occur between the ceramic plate 20 in the P1 and P2 regions and the metal layer 40. Also, peeling may occur between the ceramic plate 20 in the P3 and P4 regions and the metal layers 30c and 30d.

[0167] In the above-mentioned FIG. 24(A) to FIG. 24(C), based on the potential difference occurring when the semiconductor device 1 is stopped and driven, it is necessary to form an intermediate layer in the L1, L2 and L5 regions shown in FIG. 24(D). The L1 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30a. The L2 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30b. The L5 region is the boundary between the ceramic plate 20 and the metal layer 30d. In particular, according to FIG. 24(A) to FIG. 24(C), it is considered that the potential difference occurs frequently between the ceramic plate 20 and the metal layer 30d. For this reason, it is necessary to form an intermediate layer at least in the L5 region.

[0168] Considering the above FIG. 22(D), FIG. 23(D), and FIG. 24(D), the ceramic laminate substrate 10 requires intermediate layers to be formed in the L1 to L5 regions indicated by the broken lines as shown in FIG. 25. The L1 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30a. The L2 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30b. The L3 region is the boundary between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30c. The L4 region is the boundary between the ceramic plate 20 and the metal layer 30c. The L5 region is the boundary between the ceramic plate 20 and the metal layer 30d. In addition, considering the frequency of occurrence of the potential difference in FIG. 22 to FIG. 24, it is necessary to form intermediate layers at least in the L1 region, the L2 region, and the L5 region.

[0169] On the other hand, there may be no intermediate layer at the boundaries between the ceramic plate 20 and the metal layers 30a and 30b, and there may also be no intermediate layer at the boundaries between the ceramic plate 20 and the region of the metal layer 40 facing the metal layer 30d.

[0170] The above merely illustrates the principles of the present invention. Furthermore, numerous modifications and variations are possible for those skilled in the art, and the present invention is not limited to the exact configurations and applications shown and described above, and all corresponding modifications and equivalents are deemed to be within the scope of the present invention by the appended claims and their equivalents. For example, the ceramic plate 20 may be made of a ceramic that is insulating and has good thermal conductivity as its main component. Such ceramics are not limited to aluminum oxide or zirconium oxide. For example, aluminum nitride (AlN) or silicon nitride (Si3N4) may be used as the main component. Furthermore, zirconium oxide may be added to such aluminum nitride or silicon nitride. The ceramic plate 20 may also include grain boundary materials formed at the grain boundaries and triple points of ceramic particles. Such grain boundary materials may include, for example, oxides (second oxides) having aluminum or silicon. [Explanation of symbols]

[0171] 1 Semiconductor device 10. Ceramic laminate substrate 20 Ceramic plate 21 Aluminum Oxide 22 Silicon-containing oxide 23 Sodium oxide 24 Sodium ion 25 Oxygen ion 26 Magnesium Oxide 27 Manganese oxide 30,30a~30f Metal layer (high potential metal layer) 35 Joint materials 31,41 Copper-containing oxide 40 Metal layer (low potential metal layer) 50a,50b middle class 51a, 51b Magnesium-containing oxide 52a, 52b Oxide containing magnesium and manganese 53a, 53b Manganese-containing oxide 60a, 60b, 65a, 65b Semiconductor chip 61a, 61b Control electrodes 62a, 62b Output electrodes 66a, 66b Input electrodes 71~75 External connection terminals 80a~80e Bonding wire 81~85 Wiring 90 cases 91 Sealing member 92 Heat dissipation materials

Claims

1. A semiconductor chip; A joining member; a plate-shaped laminated substrate having a front surface and a back surface opposite to the front surface, the semiconductor chip being bonded to the front surface via the bonding member; Equipped with The laminated substrate comprises: A ceramic plate having a plate shape, a first main surface and a second main surface opposite to the first main surface, and including a plurality of ceramic particles; a high potential metal layer including copper bonded to the first major surface; a low potential metal layer bonded to the second main surface, the low potential metal layer including copper and having a lower potential than the first main surface; an intermediate layer including a first oxide formed between the second main surface and the low potential metal layer, the intermediate layer including at least one of magnesium and manganese, and the first oxide formed at a part of an interface between the second main surface and the low potential metal layer; A semiconductor device having the above structure.

2. the first oxide is in contact with both the second principal surface and the low potential metal layer; The semiconductor device according to claim 1 .

3. The first main surface is a front surface side of the laminated substrate, the second main surface is a rear surface side of the laminated substrate, the semiconductor chip is electrically connected to the high potential metal layer; 3. The semiconductor device according to claim 1 or 2.

4. the first main surface is a rear surface side of the laminated substrate, The second main surface is a front surface side of the laminated substrate, the semiconductor chip is electrically connected to the low potential metal layer; 3. The semiconductor device according to claim 1 or 2.

5. The ceramic plate and the intermediate layer contain magnesium in an oxide equivalent of 0.1 wt % or more and 1.5 wt % or less, or Manganese, calculated as oxide, is 0.01 wt% or more and 0.15 wt% or less. At least one of 5. The semiconductor device according to claim 1.

6. The intermediate layer covers 10% or more and 80% or less of the joint surface between the ceramic plate and the low potential metal layer. The semiconductor device according to claim 1 .

7. The plurality of ceramic particles and the first oxide are respectively disposed on the joint surface between the ceramic plate and the low potential metal layer, and on the joint surface, the first oxide is further disposed between the plurality of ceramic particles on the second main surface side. The semiconductor device according to claim 6.

8. The first oxide is formed in a larger amount on the second main surface side of the intermediate layer. The semiconductor device according to claim 7.

9. The first oxide further includes an oxide comprising aluminum.

9. The semiconductor device according to claim 1.

10. The first oxide is MgO, MnO, (Mg, Mn)O, (Mg, Mn)Mn 2 O 4 Contains any of the following:

10. The semiconductor device according to claim 1.

11. The first oxide includes a spinel crystal system having aluminum. The semiconductor device according to claim 9.

12. The ceramic plate further includes a second oxide having silicon at at least one of grain boundaries and triple points of the plurality of ceramic particles. The semiconductor device according to claim 1 .

13. The content of the silicon in the ceramic plate is 0.01 wt % or more and 3.0 wt % or less in terms of oxide. The semiconductor device according to claim 12.

14. The content of the silicon in the ceramic plate is 1.0 wt % or more and 3.0 wt % or less in terms of oxide. The semiconductor device according to claim 12.

15. The laminated substrate includes an oxide containing magnesium, and the magnesium, calculated as magnesium oxide (MgO), is converted into silicon oxide (SiO 2 ) The silicon content is 10 wt % or more and 50 wt % or less, or The manganese oxide is calculated as manganese oxide (MnO) and is calculated as silicon oxide (SiO 2 % or more and 5.0 wt % or less relative to the silicon content calculated as a carbon black. At least one of the following is included:

15. The semiconductor device according to claim 12.

16. The ceramic plate further includes the second oxide including sodium oxide at at least one of grain boundaries and triple points of the plurality of ceramic particles, The content of the sodium oxide in the ceramic plate is 0.001 wt % or more and 0.2 wt % or less in terms of oxide.

15. The semiconductor device according to claim 12.

17. The ceramic particles include aluminum oxide.

17. The semiconductor device according to claim 1.

18. The content of the aluminum oxide in the ceramic plate is 90 wt % or more and 99 wt % or less. The semiconductor device according to claim 17.

19. The ceramic plate further includes an oxide having zirconium at at least one of grain boundaries and triple points of the plurality of ceramic particles.

19. The semiconductor device according to claim 17 or 18.

20. The ceramic plate further includes an oxide containing zirconium and an oxide containing yttrium at at least one of grain boundaries and triple points of the plurality of ceramic particles.

19. The semiconductor device according to claim 17 or 18.

21. The content of the oxide containing zirconium in the ceramic plate is 5.0 wt % or more and 20.0 wt % or less in terms of oxide.

21. The semiconductor device according to claim 19 or 20.

22. The zirconium-containing oxide and the yttrium-containing oxide are zirconium oxide (ZrO 2 ) to yttrium oxide (Y 2 O 3 ) contains 2.5 mol% or more and 3.5 mol% or less of yttrium, The semiconductor device according to claim 20.

23. The laminated substrate contains an oxide containing magnesium, and magnesium calculated as magnesium oxide (MgO) is converted to zirconium oxide (ZrO 2 ) Containing 2.0 wt% or more and 20.0 wt% or less of zirconium converted into 23. The semiconductor device according to claim 19.

24. The laminated substrate contains an oxide containing manganese, and manganese calculated as manganese oxide (MnO) is converted into zirconium oxide (ZrO 2 ) Containing 0.05 wt% or more and 2.0 wt% or less of zirconium converted into 24. The semiconductor device according to claim 19.

25. The semiconductor chip includes a first semiconductor chip and a second semiconductor chip, The high potential metal layer is a positive electrode metal layer to which a positive electrode terminal is connected; a chip metal layer to which the first semiconductor chip is bonded; an output metal layer to which the second semiconductor chip is bonded and to which an output terminal is connected; a negative electrode metal layer to which a negative electrode terminal is connected; Including, The intermediate layer is included in a region of the second main surface facing the positive electrode metal layer. The semiconductor device according to claim 3 .

26. the intermediate layer is further included in a region of the second main surface facing the chip metal layer; The semiconductor device according to claim 25.

27. The semiconductor chip includes a first semiconductor chip and a second semiconductor chip, The low potential metal layer is A positive electrode metal layer to which a positive electrode terminal is connected; a chip metal layer to which the first semiconductor chip is bonded; an output metal layer to which the second semiconductor chip is bonded and to which an output terminal is connected; a negative electrode metal layer to which a negative electrode terminal is connected; Including, The intermediate layer is included in a region of the second main surface facing the negative electrode metal layer. The semiconductor device according to claim 4.

28. The intermediate layer is further included in a region of the second main surface facing the output metal layer.

28. The semiconductor device according to claim 27.

29. The first main surface is a front surface side of the laminated substrate, the second main surface is a back surface side of the laminated substrate, and the low potential metal layer is at a floating potential; the semiconductor chip is electrically connected to the high potential metal layer; 3. The semiconductor device according to claim 1 or 2.

30. The semiconductor chip includes a first semiconductor chip and a second semiconductor chip, The high potential metal layer is A positive electrode metal layer to which a positive electrode terminal is connected; a chip metal layer to which the first semiconductor chip is bonded; an output metal layer to which the second semiconductor chip is bonded and to which an output terminal is connected; a negative electrode metal layer to which a negative electrode terminal is connected; Including, The intermediate layer is included in a region of the first main surface facing the negative electrode metal layer.

30. The semiconductor device according to claim 29.

31. The intermediate layer is further included in a region of the second main surface facing the positive electrode metal layer and the chip metal layer. The semiconductor device according to claim 30.

32. a first semiconductor chip and a second semiconductor chip; A joining member; a plate-shaped laminated substrate having a front surface and a back surface opposite to the front surface, the first semiconductor chip and the second semiconductor chip being bonded to the front surface via the bonding member; Equipped with The laminated substrate comprises: A ceramic plate having a plate shape, a first main surface and a second main surface opposite to the first main surface, and including a plurality of ceramic particles; a first metal layer bonded to the first major surface and including copper; a second metal layer bonded to the second major surface and comprising copper; an intermediate layer including a first oxide having at least one of magnesium and manganese; having The first metal layer A positive electrode metal layer to which a positive electrode terminal is connected; a chip metal layer to which the first semiconductor chip is bonded; an output metal layer to which the second semiconductor chip is bonded and to which an output terminal is connected; a negative electrode metal layer to which a negative electrode terminal is connected; Including, the intermediate layer is included in a part of an area of ​​the second main surface facing the positive metal layer and the chip metal layer, and in an area of ​​the first main surface facing the negative metal layer; Semiconductor device.

33. The intermediate layer is further included in a region of the second main surface facing the output metal layer and a region of the first main surface facing the output metal layer. The semiconductor device according to claim 32.

34. A semiconductor chip; A joining member; a plate-shaped laminated substrate having a front surface and a back surface opposite to the front surface, the semiconductor chip being disposed on the front surface via the bonding member; Equipped with The laminated substrate comprises: A ceramic plate containing ceramic particles; A metal layer bonded to a main surface of the ceramic plate; an intermediate layer including a first oxide containing manganese, the first oxide being formed in a portion between the main surface and the metal layer; A semiconductor device having the above structure.

35. The ceramic plate further includes a second oxide having silicon at at least one of grain boundaries and triple points of the plurality of ceramic particles, The manganese content calculated as manganese oxide is 1.0 wt % or more and 5.0 wt % or less based on the silicon content calculated as silicon oxide. The semiconductor device according to claim 34.

36. The ceramic plate further includes a second oxide having silicon at at least one of grain boundaries and triple points of the plurality of ceramic particles, The manganese content calculated as manganese oxide is 0.05 wt % or more and 2 wt % or less with respect to the zirconium content calculated as zirconium oxide. The semiconductor device according to claim 34.

37. The first oxide further includes magnesium, The ceramic plate and the intermediate layer contain magnesium in an oxide equivalent of 0.1 wt % or more and 1.5 wt % or less, and Manganese, calculated as oxide, is 0.01 wt% or more and 0.15 wt% or less. At least one of The semiconductor device according to claim 34.

Citation Information

Patent Citations

  • Semiconductor power module and inverter device using the same

    JP2000031325A

  • Ceramic base body, heat dissipating base body and electronic device

    JP2010030280A

  • Laminate, insulating cooling plate, power module and method for producing laminate

    JP2015086085A

  • Semiconductor device and manufacturing method

    JP2017147327A

  • Copper / ceramic joint, insulation circuit board, and manufacturing method for copper / ceramic joint, manufacturing method for insulation circuit board

    JP2019127432A