Bonded body and semiconductor device including the bonded body
By forming dendritic structures on metal surfaces for resin impregnation, the method enhances bonding strength and durability between metal and resin parts, addressing efficiency and cost issues in existing techniques.
Patent Information
- Application Number
- JP2023566917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-16
- Filing Date
- 2023-02-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-13
AI Technical Summary
Existing methods for improving bonding between metal and resin parts, such as using silane coupling agents, are costly and complex due to the need for separate functional molecule preparation and masking, while laser-based techniques struggle to form deep recesses efficiently, limiting production efficiency and bonding effectiveness.
A method involving a metal member with a dendritic structure on its surface, where the resin member is impregnated into nanometer-scale recesses and dendritic structures, including alternating and angled recesses, to enhance bonding strength without separate functional molecules.
This approach secures a sufficient contact area and ensures firm bonding between metal and resin, achieving high strength and durability with improved production efficiency.
Smart Images

Figure 0007589835000001 
Figure 0007589835000002 
Figure 0007589835000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a conjugate. and a semiconductor device including the joint body. This is regarding. [Background technology]
[0002] Conventionally, a technique for improving the bonding performance between a metal member and a resin member is known in which a thin film of functional molecules such as a silane coupling agent is formed on the surface of the metal member by a deposition process or the like to improve adhesion with the resin. However, this method requires separate preparation of the functional molecules, and furthermore, in order to form a thin film of the functional molecules only on the required parts, it is necessary to prevent contamination by masking, which makes the processing process complicated. Therefore, the dissimilar material bonded body of a metal member and a resin member obtained by improving the bonding performance using functional molecules is expensive. Therefore, as a method that does not require separate functional molecule raw materials or masks, many direct bonding techniques have been proposed that use the anchor effect to impregnate a resin material into the unevenness formed on a metal member. Specifically, a laser is irradiated onto a metal member or a plated surface, and the metal molecules on the surface are evaporated and removed by the energy of the laser, forming an uneven shape. By making the resin material bite into the recessed shape thus formed, a dissimilar material bonded body with high bonding strength can be obtained. Therefore, since there is no need to separately prepare functional molecule raw materials or masks, and the processing steps are simple, a dissimilar material bonded body with high bonding strength can be produced at a lower cost than before. For example, as one of the conventional techniques, Patent Document 1 discloses a bonding technique in which recesses on the order of micrometers are provided on the surface of a metal to be bonded to a polymeric material, protrusions are provided on the inner walls of the recesses, and pores or recesses on the order of nanometers are formed on the surfaces of the protrusions, thereby achieving an anchor effect and a covalent bond effect. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2019-528182 Summary of the Invention [Problem to be solved by the invention]
[0004] However, although the recesses on the metal surface require a depth of at least five times the width of the recesses, the short-pulse or ultrashort-pulse laser used for processing is not suitable for forming deep recesses, and processing takes time, making it unrealistic in terms of production efficiency. In addition, although it is said that the effect of covalent bonding can be obtained by the nanometer-order pores or recesses formed on the protrusion surface, it is not unusual for the surface roughness of the metal to be formed by nanometer-order irregularities. Rather, the problem is that the contact area between the metal material and the polymer material is insufficient in the pores or recesses formed on the protrusion surface, and the bonding effect due to the nanometer-order structure is not fully obtained. [Means for solving the problem]
[0005] The joint of a metal member and a resin member according to the present disclosure 、 The present invention comprises a metal member and a resin member bonded to the metal member, the metal member having a dendritic structure on a bonding surface with the resin member, at least a part of the dendritic structure having a diameter on the order of nanometers, the resin member being impregnated with the dendritic structure, and the metal member having a recess on a bonding surface with the resin member. 、 The recess includes a first recess having a dendritic structure on its surface and a second recess deeper than the first recess, and the first recess and the second recess are alternately formed in a positional relationship. A joint of a metal member and a resin member according to the present disclosure includes a metal member and a resin member joined to the metal member, the metal member has a dendritic structure on a joint surface with the resin member, at least a part of the dendritic structure has a diameter on the order of nanometers, the resin member is impregnated with the dendritic structure, and the metal member has a recess on a joint surface with the resin member. 、The recess includes a third recess formed at an inclination with respect to the surface of the metal member, and a first recess formed on the surface of the third recess, and the surface of the first recess has a dendritic structure formed thereon.
[0006] Ma Further, a semiconductor device according to one aspect of the present disclosure is a semiconductor device in which a surface electrode, a conductive layer, an electrode terminal, or a wire is resin-sealed with a resin member, the surface electrode, the conductive layer, the electrode terminal, and the wire are metal members, and in at least a part of a bond between the surface electrode, the conductive layer, the electrode terminal, or the wire member and the resin member, the surface electrode, the conductive layer, the electrode terminal, or the wire member has a dendritic structure portion on a bonding surface with the resin member, the diameter of at least a part of the dendritic structure portion is on the order of nanometers, and the resin member is impregnated with the dendritic structure portion. 、 The recess includes a first recess having a dendritic structure on its surface and a second recess deeper than the first recess, and the first recess and the second recess are formed alternately. A semiconductor device according to one aspect of the present disclosure is a semiconductor device in which a surface electrode, a conductive layer, an electrode terminal, or a wire is resin-encapsulated with a resin member, the surface electrode, the conductive layer, the electrode terminal, and the wire are metal members, and in at least a part of a bond between the surface electrode, the conductive layer, the electrode terminal, or the wire member and the resin member, the surface electrode, the conductive layer, the electrode terminal, or the wire member has a dendritic structure on a bonding surface with the resin member, a diameter of at least a part of the dendritic structure is on the order of nanometers, the resin member is impregnated with the dendritic structure, and the metal member has a recess on a bonding surface with the resin member. 、 The recess includes a third recess formed at an inclination with respect to the surface of the metal member, and a first recess formed on the surface of the third recess, and the surface of the first recess is characterized in that a dendritic structure portion is formed. Effect of the Invention
[0008] According to the present disclosure, a sufficient contact area can be secured between the resin member and a dendritic structure portion on the nanometer order formed in the metal member, thereby making it possible to obtain a resin-metal bonded body in which the metal member and the resin member are firmly bonded. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view of a bonded body according to embodiment 1. FIG. [Diagram 2] 2A to 2C are schematic cross-sectional views illustrating a manufacturing process of a bonded body according to the first embodiment. [Diagram 3] 1 is an SEM image of the surface of a metal member 101 after being irradiated with a pulsed laser. [Figure 4] 1 is an enlarged SEM image of the surface of a metal member 101 after being irradiated with a pulsed laser. [Diagram 5] 1 is an SEM image of a cross section of a metal member 101 after being irradiated with a pulsed laser. [Figure 6] 1 is a TEM image of a cross section of a metal member 101 after being irradiated with a pulsed laser. [Figure 7] 1 shows the cross-sectional analysis results of the metal member 101 after irradiation with a laser with an energy density of 20 J / cm2. (a) is a cross-sectional TEM image, (b) is a cross-sectional TEM-EDX analysis result showing the distribution of Al elements, and (c) is a cross-sectional TEM-EDX analysis result showing the distribution of O elements. [Figure 8] 1 shows the cross-sectional analysis results of the metal member 101 after irradiation with a laser having an energy density of 50 J / cm2. (a) is a cross-sectional TEM image, (b) is a cross-sectional TEM-EDX analysis result showing the distribution of Al elements, and (c) is a cross-sectional TEM-EDX analysis result showing the distribution of O elements. [Figure 9] 1 shows cross-sectional SEM images of joints used in fatigue strength tests, where (a) is a cross-sectional SEM image of a joint produced as an example, and (b) is a cross-sectional SEM image of a joint produced as a comparative example. [Figure 10] FIG. 11 is a schematic cross-sectional view of a bonded body according to a second embodiment. [Figure 11] 1 is an SEM image of the surface of a metal member 101 according to the second embodiment. [Figure 12] 1 is a TEM image of a cross section of a first recess 103 of a metal member 101 according to the second embodiment. [Figure 13] 11 is a schematic cross-sectional view of a bonded body 120 according to the third embodiment. FIG. [Figure 14]13 is an SEM image of a cross section of the surface of a metal member 101 obtained in the third embodiment. [Figure 15] 13 is a TEM image of a cross section of a first recess 103 of a metal member 101 obtained in the third embodiment. [Figure 16] FIG. 11 is a schematic cross-sectional view of a semiconductor device 200 according to a fourth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In addition, in order to clarify the description, the drawings may be appropriately simplified and repeated descriptions may be omitted.
[0011] Embodiment 1 FIG. 1 is a schematic cross-sectional view of a bonded body according to the first embodiment. As shown in FIG. 1, the bonded body 100 is a bonded body of a metal member 101 and a resin member 102, and a first recess 103 and a dendritic structure 104 mainly composed of the metal member 101 are formed on the surface of the metal member 101 at the bonded portion. A plurality of first recesses 103 are formed on the surface bonded to the resin member 102, and a dendritic structure 104 is formed on the surface of each of the first recesses 103. The dendritic structure 104 includes dendrites having a diameter of at least 1 nm to less than 10 nm, which is on the order of nanometers, and the dendritic structure 104 is spatially spread so that adjacent dendrites are entangled with each other. Furthermore, the resin member 102 is impregnated between the spatially spread dendrites. The metal member 101 is a pure metal such as Al, Cu, or Fe. Or, the metal member 101 is an alloy mainly composed of at least one of Al, Cu, Fe, Ni, Au, Pd, Ag, and Sn. In the first embodiment, an alloy mainly composed of Al is shown as an example. The main component here means a component that accounts for 50 wt% or more of the weight ratio of the entire metal member 101. The resin member 102 is not particularly limited as long as it can be impregnated into the dendritic structure 104, and examples thereof include epoxy resin, silicone, nylon, urethane, and polyphenylene sulfide resin. The depth to the bottom of the first recess 103 is preferably in the range of 100 nm to 10 μm, and the ratio of the depth to the width of the first recess 103 is preferably in the range of 0.002 to 0.2. The thickness of the dendritic structure 104 is preferably in the range of 1 / 1000 to 1 / 100 of the width of the first recess 103, and the thickness of the dendritic structure 104 is preferably in the range of 1 / 100 to 1 / 10 of the depth of the first recess 103.
[0012] In the bonded body 100 configured in this manner, the resin member 102 is impregnated into the dendritic structure portion 104, thereby ensuring a sufficient contact area between the resin member 102 and the dendritic structure portion 104. Furthermore, the molecules constituting the resin member 102 and the molecules constituting the dendritic structure portion 104 are close to each other on the nanometer order, which causes an intermolecular force to act, thereby firmly bonding the resin member 102 and the dendritic structure portion 104.
[0013] As described above, the configuration shown in the first embodiment makes it possible to obtain a resin-metal bonded body having high strength and long-term durability without using functional molecules or the like, while suppressing a decrease in productivity associated with the formation of a structure for obtaining the anchor effect.
[0014] Next, a process for producing the bonded body according to embodiment 1 will be described below. Figures 2(a) to 2(d) are schematic cross-sectional views illustrating the process for producing the bonded body according to embodiment 1. First, as shown in FIG. 2(a), a metal member 101 is prepared. The metal member 101 is, for example, a pure metal such as Al, Cu, or Fe. Alternatively, the metal member 101 is an alloy containing at least one of Al, Cu, Fe, Ni, Au, Pd, Ag, and Sn as a main component. The surface of the metal member 101 may be subjected to a plating treatment such as Ni plating or Cu plating, or a stabilization treatment such as a chromate treatment or an anodization treatment. Furthermore, if necessary, the surface of the metal member 101 may be subjected to a pretreatment such as a plasma treatment, a corona treatment, or an ultraviolet irradiation treatment before the stabilization treatment. By doing so, the joining surface is cleaned, and a uniform metal member surface can be obtained. Therefore, in the manufacturing process, FIG. 2(a) is positioned as a preparation step.
[0015] Next, as shown in FIG. 2(b), a laser is irradiated onto the surface of the metal member 101 to form a first recess 103 and a dendritic structure 104 on the surface of the metal member 101. The irradiated laser is preferably a pulsed laser, and in order to avoid the shape of the surface of the metal member 101, the first recess 103, and the dendritic structure 104 being affected by deformation or the like due to heat, it is preferable that the pulse width is as short as possible. More specifically, the pulse width is preferably 10 ns or less, but since a smaller pulse width increases the equipment cost, it can be selected in consideration of the balance with productivity. In addition, the wavelength of the pulsed laser is not particularly limited, but examples of wavelengths suitable for metal processing include wavelengths of 200 nm or more and 10,000 nm or less, and more preferably wavelengths of 400 nm or more and 2,000 nm or less. In addition, the energy density of the pulsed laser irradiated per unit area is 0.5 J / cm 2 More than 50J / cm 2 The following range is preferable. Furthermore, 5 J / cm 2 More than 30J / cm 2 The following range is more preferable: 5 J / cm 2 When the energy supply is less than 30 J / cm, the amount of energy supplied is small, and the first recesses 103 cannot be formed, so that the dendritic structures 104 are not formed. 2 If the energy supply exceeds 100%, the dendritic structure 104 melts and only the first recess 103 is formed. 2 Laser irradiation may be performed in a gas atmosphere such as Ar or He. By performing laser irradiation in an inert gas atmosphere, for example, oxidation of the metal member 101, as well as the first recess 103 and the dendritic structure 104 can be suppressed, and therefore the laser irradiation can also be applied to control the wettability of the metal member 101, as well as the first recess 103 and the dendritic structure 104 after laser irradiation. Furthermore, for the purpose of cooling, laser irradiation can also be performed while flowing an inert gas. Therefore, in the manufacturing process, FIG. 2(b) is positioned as a surface processing step.
[0016] FIG. 2(c) is a cross-sectional view in which a first recess 103 and a dendritic structure 104 are formed on the surface of the metal member 101 by irradiating the metal member 101 with a pulsed laser. When the surface of the metal member 101 is irradiated with a laser, a part of the metal member 101 melts or evaporates by ablation. The first recess 103 is formed by melting or evaporating a part of the metal member 101 by ablation, and the dendritic structure 104 is formed on the first recess 103. The dendritic structure 104 has dendrites with a diameter of at least 1 nm to less than 10 nm, which is on the order of nanometers, and the adjacent dendrites are spatially spread so as to be entangled with each other. The interval of the laser irradiation on the metal member 101 can be controlled by irradiating the metal member 101 with the laser light source while moving it with a galvano lens or the like. It is preferable that the relative positions of the spots of the irradiating laser be within a range of 1 to 5 times the center interval of the spot diameter of the irradiating laser. For example, when the magnification is set to 1x, the laser spots are in contact with each other and lined up with no gaps, resulting in a densely packed array of spots. Therefore, in the manufacturing process, FIG. 2(c) shows the state after the surface processing step.
[0017] 2(d) is a schematic cross-sectional view of a bonded body 100 in which a resin member 102 is bonded to a metal member 101 having a first recess 103 and a dendritic structure 104 formed thereon. The resin member 102 is not particularly limited, and examples thereof include epoxy resin, silicone, nylon, urethane, and polyphenylene sulfide (PPS). When bonding the metal member 101 and the resin member 102, the resin member 102 in a partially or entirely molten state is bonded to the surfaces of the metal member 101 having the dendritic structure 104 formed thereon and the first recess 103. The dendritic structure 104 includes at least some dendrites having a diameter on the order of nanometers, and the resin member 102 is impregnated between the dendrites to obtain a bonded body 100 having high strength and long-term durability. Therefore, in the manufacturing process, FIG. 2(d) is positioned as the bonding process.
[0018] Next, the results of observing the surface and cross section of metal member 101 obtained in the first embodiment are shown in FIG. 3 to FIG. 3 is an example of an SEM image (scanning electron microscope image) of the surface of metal member 101 after irradiation with a pulsed laser. As a result of irradiating the laser with a distance equal to the length of the spot diameter of the irradiating laser, in other words, one time the spot diameter, first recesses 103 formed by the laser irradiation do not overlap with adjacent recesses 103, but are in contact with adjacent recesses 103 on the surface, with no gaps between them. FIG. 4 is an example of an enlarged SEM image (scanning electron microscope image) of the surface of the metal member 101 after irradiation with a pulsed laser. From FIG. 4, it can be confirmed that a dendritic structure 104 is formed on the first recess 103 formed on the surface of the metal member 101. At least a part of the dendrites constituting the dendritic structure 104 has a diameter of about several nm, and the adjacent dendrites are spatially spread so as to be entangled with each other. The interval at which the laser is irradiated is not particularly limited, but by irradiating at an interval of 1.0 to 5.0 times the spot diameter, the dendritic structure 104 is formed on the surface of the first recess 103, and the resin member 102 is impregnated into the dendritic structure 104, thereby forming a strong bonded body 100 between the metal member 101 and the resin member 102. Note that when the laser is irradiated at an interval of 1.0 times or more, the dendritic structure 104 may also be formed on the surface of the metal member 101 not irradiated with the laser around the first recess 103.
[0019] Fig. 5 is an example of a SEM image (scanning electron microscope image) of a cross section of metal member 101 after irradiation with a pulsed laser. Fig. 6 is an example of a TEM image (transmission electron microscope image) of a cross section of metal member 101 after irradiation with a pulsed laser. From Figs. 5 and 6, it can be seen that first recesses 103 are formed without overlapping with adjacent recesses 103 and in contact with adjacent recesses 103 with no gaps, and that dendritic structures 104 having a thickness of about several hundreds of nm from the surface of first recesses 103 are formed on the surface of first recesses 103.
[0020] Figures 7(a) to (c) and Figures 8(a) to (c) compare the cross-sectional TEM-EDX (energy dispersive X-ray spectroscopy) analysis results of the metal component 101 after irradiating it with a pulsed laser under two conditions with different energy densities, using Al as the metal component 101. First, Fig. 7(a)-(c) shows the results for 20 J / cm 2 7(a) shows the cross-sectional TEM analysis results, FIG. 7(b) shows the cross-sectional TEM-EDX analysis results showing the distribution of Al elements, and FIG. 7(c) shows the cross-sectional TEM-EDX analysis results showing the distribution of O elements. From the results of FIGS. 7(a) to (c), it is clear that the cross-sectional TEM-EDX analysis results show the distribution of O elements after irradiation with a laser having an energy density of 20 J / cm 2 When a laser with an energy density of 50 J / cm was irradiated, a dendritic structure 104 was formed on the surface of the first recess 103 formed in the metal member 101, and the dendritic structure 104 was composed of oxidized Al. 2 8(a) shows the cross-sectional TEM analysis results, FIG. 8(b) shows the cross-sectional TEM-EDX analysis results showing the distribution of Al elements, and FIG. 8(c) shows the cross-sectional TEM-EDX analysis results showing the distribution of O elements. From the results of FIGS. 8(a) to (c), it is clear that the cross-sectional TEM-EDX analysis results showing the distribution of O elements were obtained after irradiation with a laser having an energy density of 50 J / cm. 2 When a laser with this energy density was irradiated, dendritic structures 104 were not formed on the surface of first recesses 103 formed in metal member 101. This is presumably because the energy density of the irradiated laser was too high, and the Al of metal member 101 irradiated with the laser melted or evaporated without forming dendritic structures 104. From these observation results, it is considered that the dendritic structure 104 is mainly composed of oxides of the metal member 101 generated by ablation caused by laser irradiation of the metal member 101.
[0021] Next, the results of a fatigue strength test using a joint body produced as an example of the first embodiment and a joint body produced as a comparative example will be shown. <Example of the first embodiment> First, the configuration of an example of the first embodiment will be described with reference to FIGS. 2(a) to (d). In FIG. 2(a), aluminum A5052 whose surface had been degreased with acetone was prepared as the metal member 101. In FIG. 2(b), a pulsed laser was irradiated onto the metal member 101 in an area of 20 mm × 20 mm. For the pulsed laser irradiation, an MX-Z2000H (wavelength: 1,062 nm, laser spot diameter: approximately 45 μm) manufactured by Omron Corporation was used. At this time, the frequency and speed were adjusted so that adjacent laser spots were adjacent to each other, in other words, so that the interval was 1.0 times the laser spot diameter. The energy density of the irradiated laser was 20 J / cm. 2 A first recess 103 and a dendritic structure 104 were formed at the irradiated location. 2(c), first recesses 103 having a width of about 50 μm and a depth of about 10 μm were formed on the surface of metal member 101 by laser irradiation. Dendritic structures 104 had a thickness of about 200 nm and were formed over the entire area of 20 mm × 20 mm irradiated with the laser. 2(d), liquid epoxy resin (manufactured by Ryoden Kasei Co., Ltd.) was potted in a cylindrical shape of φ5 mm on the surface of the metal member 101 irradiated with the laser, and cured by heating at 180° C. to form a resin member 102, thereby obtaining a bonded body 100. FIG 9(a) is a cross-sectional SEM image of a bonded body produced as an example.
[0022] The obtained bonded body was subjected to an initial adhesive strength test and a fatigue strength test. In the initial adhesive strength test, a load was applied in a direction parallel to the bonded surface at a speed of 1 mm / sec to a portion 1 mm high from the bonded interface of the bonded body 100 toward the resin member 102, and the shear strength was evaluated. As a result, the shear bond strength was 28.9 MPa. The fracture location was the resin member 102. Next, in the fatigue strength test, a load with a stress amplitude of 2.8 MPa was applied to a portion of the bonded body at a height of 1 mm toward the resin member 102 side from the bonded interface, and the fatigue strength was evaluated. As a result, the number of cycles to fracture of the bonded body was 4.9×10 6The break occurred in the resin member 102.
[0023] <Comparative Example> The configuration of the comparative example will be described with reference to FIGS. 2(a) to (d). In FIG. 2(a), aluminum A5052 whose surface had been degreased with acetone was prepared as the metal member 101. In FIG. 2(b), a pulsed laser was irradiated onto the metal member 101 in an area of 20 mm × 20 mm. For the pulsed laser irradiation, an MX-Z2000H (wavelength: 1,062 nm, laser spot diameter: approximately 45 μm) manufactured by Omron Corporation was used. At this time, the frequency and speed were adjusted so that adjacent laser spots were adjacent to each other, in other words, so that the interval was 1.0 times the laser spot diameter. The energy density of the irradiated laser was 50 J / cm. 2 The same spot was irradiated ten times with the same laser beam. No dendritic structure 104 was formed in the irradiated spot, and only first recessed portion 103 was formed. In FIG. 2(c), a first recess 103 was formed on the surface of the metal member 101 by laser irradiation, and the first recess 103 had a width of about 50 μm and a depth of about 70 μm. 2(d), liquid epoxy resin (manufactured by Ryoden Kasei Co., Ltd.) was potted in a cylindrical shape of φ5 mm on the surface of the metal member 101 irradiated with the laser, and cured by heating at 180° C. to form a resin member 102, thereby obtaining a bonded body 100. FIG 9(b) is a cross-sectional SEM image of a bonded body produced as a comparative example.
[0024] An initial adhesive strength test and a fatigue strength test were performed on the resulting bonded body. In the initial adhesive strength test, a load was applied in a direction parallel to the bonded surface at a speed of 1 mm / sec to a portion 1 mm high from the bonded interface of the bonded body toward the resin member 102, and the shear strength was evaluated. As a result, the shear bond strength was 32.2 MPa. The fracture location was the resin member 102. Next, in the fatigue strength test, a load with a stress amplitude of 2.8 MPa was applied to a portion of the bonded body at a height of 1 mm toward the resin member 102 side from the bonded interface, and the fatigue strength was evaluated. As a result, the number of cycles to fracture of the bonded body was 1.0×10 6 The fracture occurred at the bonding interface between the metal member 101 and the resin member 102.
[0025] Therefore, from the comparison of the fatigue strength test results, it was found that the joined body produced as the example had about five times as many cycles to fracture as the joined body produced as the comparative example, and thus had a longer fatigue life. In addition, it was found that the fracture location of the joined body produced as the example was the resin member 102, whereas the fracture location of the joined body produced as the comparative example was the bonding interface between the metal member 101 and the resin member 102. Therefore, it was shown that by applying the first embodiment, a resin-metal joined body having high strength and long-term durability can be obtained.
[0026] As described above, the resin-metal bonded body in embodiment 1 comprises a metal member 101 and a resin member 102 bonded to the metal member 101, the metal member 101 has a dendritic structure 104 on the bonding surface with the resin member 102, at least a portion of the dendritic structure 104 has a diameter on the order of nanometers, and the resin member 102 is impregnated into the dendritic structure 104.
[0027] With this configuration, a sufficient contact area can be secured between the resin member 102 and the dendritic structure 104 of the nanometer order formed on the metal member 101, so that a bonded body 100 can be obtained in which the metal member 101 and the resin member 102 are firmly bonded.
[0028] Furthermore, the manufacturing method of the joined body 100 in embodiment 1 includes a surface processing step of forming a first recess 103 and a dendritic structure 104, at least a portion of which has a diameter on the order of nanometers, on the surface of the metal member 101, and a joining step of impregnating the dendritic structure 104 with the resin member 102 to join the metal member 101 and the resin member 102.
[0029] According to this configuration, a sufficient contact area can be secured between the resin member 102 and the dendritic structure 104 on the nanometer order formed in the metal member 101, thereby providing a manufacturing method for a bonded body 100 in which the metal member 101 and the resin member 102 are firmly bonded together.
[0030] Embodiment 2 FIG. 10 is a schematic cross-sectional view of a bonded body 110 according to the second embodiment. 10, the bonded body 110 is a bonded body of a metal member 101 and a resin member 102, and differs from the first embodiment in that a second recess 111 is formed on the surface of the metal member 101 at the bonding portion in addition to a first recess 103. The other configurations are the same as those of the first embodiment. As in the first embodiment, a plurality of first recesses 103 are formed on the surface to be bonded to the resin member 102, and a dendritic structure 104 is formed on the surface of each of the first recesses 103. A plurality of second recesses 111 are formed on the surface to be bonded to the resin member 102, and are formed deeper than the first recesses 103, and the second recesses 111 bond the metal member 101 and the resin member 102 more firmly by the anchor effect. The depth of the second recesses 111 is not particularly limited as long as it is deeper than the first recesses 103, but is more preferably 50 μm or more. On the other hand, the dendritic structure 104 is not formed on the surface of the second recesses 111. The ratio of the first recesses 103 and the second recesses 111 formed on the surface of the metal member 101 is not particularly limited, but is preferably about 50% each. In addition, the positional relationship between the first recess 103 and the second recess 111 formed on the surface of the metal member 101 is not particularly limited, but it is preferable that both the first recess 103 and the second recess 111 are formed evenly on the surface of the metal member 101, and it is more preferable that the first recess 103 and the second recess 111 are formed alternately.
[0031] In the bonded body 110 configured in this manner, the resin member 102 impregnates the dendritic structure 104 formed in the first recess 103, thereby ensuring a sufficient contact area between the resin member 102 and the dendritic structure 104. Furthermore, the molecules constituting the resin member 102 and the molecules constituting the dendritic structure 104 are close to each other on the nanometer order, which causes an intermolecular force to act, thereby firmly bonding the resin member 102 and the dendritic structure 104. Furthermore, in the bonded body 110, an anchor effect is obtained by the resin member 102 entering the second recess 111, which is deeper than the first recess 103, so that the metal member 101 and the resin member 102 are more firmly bonded to each other.
[0032] As described above, the configuration shown in embodiment 2 has the same effects as embodiment 1, and in addition, an anchor effect is obtained by the resin member 102 penetrating into the second recess 111 which is deeper than the first recess 103, so that a resin-metal bonded body that is more firmly bonded can be obtained.
[0033] Next, a manufacturing process according to the second embodiment will be described. The manufacturing process of the bonded body according to the second embodiment differs from that of the first embodiment in that in the surface processing step shown in the first embodiment, second recesses 111 are formed in addition to first recesses 103 and dendritic structures 104 on the surface of metal member 101. The other steps are the same as those of the first embodiment. Second recesses 111 are formed deeper than first recesses 103, preferably to a depth of 50 μm or more, by repeatedly irradiating the surface of metal member 101 with a laser. The laser to be irradiated is not particularly limited, but a pulsed laser similar to the laser used to form first recesses 103 and dendritic structure 104 is preferable. The method for forming the first recess 103 and the tree-like structure 104 is the same as that in the first embodiment, and therefore the description will be omitted. The order in which the first recess 103 and the tree-like structure 104 are formed and the second recess 111 are formed does not matter.
[0034] The joining process shown in embodiment 1 can be applied to the joining surface of the metal member 101 obtained as described above, on which the first recess 103 and second recess 111 having the dendritic structure portion 104 are formed, to join the resin member 102, thereby obtaining the joined body 110.
[0035] Next, the results of observing the surface and cross section of metal member 101 obtained in the second embodiment are shown in FIG. 11 and FIG. Fig. 11 is an SEM image of the surface of metal member 101 according to embodiment 2. Fig. 11 shows an example in which first recesses 103 and second recesses 111 are adjacent to each other without overlapping and are formed side by side with no gaps. This is obtained by making the spot diameter of the laser used to form first recesses 103 and second recesses 111 the same, and forming first recesses 103 and second recesses 111 at a distance twice the spot diameter. Fig. 12 is a TEM image of a cross section of first recess 103 of metal member 101 according to embodiment 2. More specifically, this shows a cross section of a rectangular region indicated by a dashed line in Fig. 11. It can be seen that dendritic structure 104 having a thickness of about several hundred nm from the surface of first recess 103 is formed on the surface of first recess 103.
[0036] Next, the results of evaluation of the bonding strength using the bonded bodies produced as examples of the second embodiment will be shown. <Example of the second embodiment> Although not shown in the drawings, the configuration of the example of the second embodiment will be described following the same flow as the example of the first embodiment. First, aluminum A5052 whose surface had been degreased with acetone was prepared as the metal member 101 . Next, a first recess 103 and a second recess 111 each having a dendritic structure 104 were formed in the metal member 101. To form the second recess 111, a pulsed laser was irradiated onto the metal member 101 in an area of 20 mm x 20 mm. For the pulsed laser irradiation, an MX-Z2000H (wavelength: 1,062 nm, laser spot diameter: approximately 45 μm) manufactured by Omron Corporation was used. At this time, the frequency and speed were adjusted so that the spots formed by the laser were adjacent to each other at an interval twice the laser spot diameter. The energy density of the irradiated laser was 200 J / cm. 2 A second recess 111 having a depth of about 50 μm was formed at the irradiated location. Next, a pulsed laser was irradiated onto the metal member 101 with the second recess 111 formed therein. At this time, the frequency and speed were adjusted so that the interval between adjacent laser spots was such that they did not overlap with the second recess 111. The energy density of the irradiated laser was 20 J / cm2. 2 A first recess 103 having a dendritic structure 104 was formed at the irradiated location. As a result of surface processing by laser irradiation, first recesses 103 and second recesses 111 each having a dendritic structure 104 were formed alternately on the surface of metal member 101. The width of first recesses 103 and second recesses 111 was approximately 50 μm, and the depth of first recesses 103 was approximately 10 μm. Furthermore, dendritic structure 104 had a thickness of approximately 200 nm. Next, liquid epoxy resin (manufactured by Ryoden Kasei Co., Ltd.) was potted in a cylindrical shape of φ5 mm onto the surface of the surface-treated metal member 101, and heat-cured at 180° C. to form a resin member 102, and a bonded body 110 was obtained.
[0037] An initial adhesive strength test was performed on the resulting bonded body. In the initial adhesive strength test, a load was applied in a direction parallel to the bonded surface at a speed of 1 mm / sec to a portion 1 mm high from the bonded interface of the bonded body 110 toward the resin member 102, and the shear strength was evaluated. As a result, the shear bond strength was 33.0 MPa. The fracture occurred at the resin member 102.
[0038] Therefore, it was found that the joined body produced in the Example of the Second Embodiment, like the Example of the First Embodiment, had a higher initial joining strength than the joined body produced in the Comparative Example of the First Embodiment. This shows that by applying the Second Embodiment, it is possible to obtain a resin-metal joined body that has high strength and long-term durability like the First Embodiment, and also has a higher initial joining strength.
[0039] As described above, in the resin-metal bonded body of embodiment 2, in addition to the configuration of embodiment 1, metal member 101 has a recess on the bonding surface with resin member 102, and the recess includes first recess 103 having dendritic structure portion 104 on the surface and second recess 111 deeper than first recess 103, and first recess 103 and second recess 111 are formed alternately in a positional relationship.
[0040] According to such a configuration, in addition to being able to secure a sufficient contact area between the resin member 102 and the dendritic structure 104 on the nanometer order formed in the metal member 101, the resin member 102 penetrates into the second recess 111 that is deeper than the first recess 103. Thus, in addition to the same effects as in the first embodiment, an anchor effect can be obtained by the second recess 111, and therefore a bonded body 110 in which the metal member 101 and the resin member 102 are more firmly bonded can be obtained.
[0041] Embodiment 3 FIG. 13 is a schematic cross-sectional view of a bonded body 120 according to the third embodiment. 13, the bonded body 120 differs from the first embodiment in that a third recess 121 is formed on the surface of the metal member 101 at the metal member bonded portion, and a first recess 103 having a dendritic structure portion 104 is formed on the surface of the third recess 121. The other configurations are the same as those of the first embodiment. The third recess 121 is formed with an inclination with respect to the surface of the metal member 101, and is deeper than the first recess 103, and the first recess 103 is formed on the surface of the third recess 121. Similarly to the first embodiment, the dendritic structure 104 is formed on the surface of the first recess 103. Furthermore, a plurality of third recesses 121 are formed on the surface of the metal member 101 that is bonded to the resin member 102. The depth of the third recess 121 is not particularly limited as long as it is deeper than the first recess 103, but is preferably 50 μm or more. The ratio of the first recess 103 to the surface area of the third recess 121 is not particularly limited, but is preferably 10% or more. Furthermore, the inclination of the third recess 121 with respect to the surface of the metal member 101 is not particularly limited, but is preferably less than 90 degrees because the first recess 103 is formed on the surface of the third recess 121.
[0042] In the bonded body 120 configured in this manner, an anchoring effect is obtained by the resin member 102 entering the third recess 121, which is formed at an angle to the surface of the metal member 101 and is deeper than the first recess 103. Furthermore, the first recess 103 having the dendritic structure portion 104 is formed on the surface of the third recess 121 providing the anchoring effect, and the resin member 102 impregnates the dendritic structure portion 104, thereby ensuring a sufficient contact area. Therefore, a stronger anchoring effect is obtained by bonding the resin member 102 and the dendritic structure portion 104, and the metal member 101 and the resin member 102 are bonded more firmly than in the case where the dendritic structure portion 104 is not present.
[0043] As described above, with the configuration shown in embodiment 3, a sufficient contact area between resin member 102 and dendritic structure 104 on the surface of third recess 121 is ensured, and a stronger anchor effect can be obtained, resulting in a resin-metal bonded body that is stronger bonded than the conventional anchor effect.
[0044] Next, a manufacturing process according to the third embodiment will be described. The manufacturing process of the bonded body according to the third embodiment is different from that of the first embodiment in that, in the surface processing step shown in the first embodiment, third recesses 121 are formed on the surface of metal member 101, and first recesses 103 and dendritic structures 104 are further formed on the surface of third recesses 121. The other steps are the same as those of the first embodiment. Third recesses 121 are formed to a depth deeper than first recesses 103 by repeatedly irradiating the surface of metal member 101 with a laser. The angle of the irradiated laser is not particularly limited as long as it is inclined with respect to the surface of metal member 101, but is preferably about 45 degrees. In addition, the irradiated laser is not particularly limited, but is preferably a pulsed laser similar to the laser used to form first recesses 103 and dendritic structure 104. After forming third recesses 121 on the surface of metal member 101, a pulsed laser is irradiated onto third recesses 121 to form first recesses 103 having dendritic structures 104. The methods for forming first recesses 103 and dendritic structures 104 are the same as those in the first embodiment, and therefore will not be described.
[0045] By applying the joining process described in embodiment 1 to the joining surface of metal member 101, on which the third recess is formed, obtained as described above, resin member 102 can be joined to obtain joined body 120.
[0046] Next, the results of observing the cross section of the surface of the metal member 101 obtained in the third embodiment are shown in FIG. 14 and FIG. 14 is an SEM image of a cross section of the surface of metal member 101 obtained in embodiment 3. More specifically, it is an SEM image of a cross section of the surface of metal member 101 in which third recesses 121 with a depth of 50 μm are formed at an angle of 45 degrees to the surface, and first recesses 103 with dendritic structures 104 are formed on the surface of third recesses 121. Fig. 15 is a TEM image of a cross section of first recess 103 of metal member 101 obtained in embodiment 3. More specifically, this shows a cross section of a rectangular region indicated by a dashed line in Fig. 14. It can be seen that dendritic structure 104 having a thickness of about several hundred nm from the surface of first recess 103 is formed on the surface of first recess 103.
[0047] Next, the results of evaluation of the bonding strength of the bonded body produced as an example of the third embodiment will be shown. <Example of the third embodiment> Although not shown in the drawings, the configuration of the example of the third embodiment will be described following the same flow as the example of the first embodiment. First, aluminum A5052 whose surface had been degreased with acetone was prepared as the metal member 101 . Next, a third recess 121 was formed in the metal member 101, and a first recess 103 having a dendritic structure 104 was formed on the surface of the third recess 121. To form the third recess 121, the metal member 101 was placed at an angle of 45 degrees to the laser, and a pulsed laser was irradiated over an area of 20 mm x 20 mm. For the pulsed laser irradiation, an MX-Z2000H (wavelength: 1,062 nm, laser spot diameter: approximately 45 μm) manufactured by Omron Corporation was used. At this time, the frequency and speed were adjusted so that adjacent laser spots were adjacent to each other. The energy density of the irradiated laser was 200 J / cm. 2 A third recess 121 having a depth of about 50 μm was formed at the irradiated portion. Next, a pulsed laser was irradiated onto the surface of the third recess 121. At this time, the frequency and speed were adjusted so that adjacent laser spots were adjacent to each other. The energy density of the irradiated laser was 20 J / cm. 2 A first recess 103 having a dendritic structure 104 was formed at the irradiated portion on the surface of the third recess 121 . As a result of the surface processing by laser irradiation, a third recess 121 was formed on the surface of metal member 101, and a first recess 103 having a dendritic structure 104 was formed on the surface of third recess 121. The depth of first recess 103 was about 10 μm, similar to the examples of embodiment 1 and embodiment 2. Furthermore, dendritic structure 104 had a thickness of about 200 nm. Next, liquid epoxy resin (manufactured by Ryoden Kasei Co., Ltd.) was potted in a cylindrical shape of φ5 mm onto the surface of the surface-treated metal member 101, and heat-cured at 180° C. to form a resin member 102, and a bonded body 120 was obtained.
[0048] An initial adhesive strength test was performed on the resulting bonded body. In the initial adhesive strength test, a load was applied in a direction parallel to the bonded surface at a speed of 1 mm / sec to a portion 1 mm high from the bonded interface of the bonded body 120 toward the resin member 102, and the shear strength was evaluated. As a result, the shear bond strength was 32.8 MPa. The fracture occurred at the resin member 102.
[0049] Therefore, it was found that the joined body produced in the Example of the embodiment 3, like the Example of the embodiment 1, had a higher initial joining strength than the joined body produced in the Comparative example of the embodiment 1. This shows that by applying the embodiment 3, it is possible to obtain a resin-metal joined body that has high strength and long-term durability like the embodiment 1, and also has a higher initial joining strength.
[0050] In the manufacturing process according to the third embodiment, the third recess 121 is inclined at an angle of 45 degrees to the surface of the metal member 101, that is, obliquely inclined, but the third recess 121 may be inclined at an angle of 90 degrees to the surface of the metal member 101, that is, perpendicular to the surface of the metal member 101. When the third recess 121 is perpendicular to the surface of the metal member 101, the first recess 103 having the dendritic structure 104 is formed deeper on the surface of the third recess 121 than when the third recess 121 is inclined at an angle, and the same effect can be obtained by impregnating the dendritic structure 104 with the resin member 102.
[0051] The method for forming the third recess 121 having an inclination of 90 degrees with respect to the surface of the metal member 101 can be performed by setting the irradiation angle of the laser when forming the third recess 121 to 90 degrees with respect to the surface of the metal member 101 in the forming method described above in the third embodiment. First, the third recess 121 having an inclination of 90 degrees with respect to the surface of the metal member 101 is formed, and the surface of the formed third recess 121 is irradiated with a laser, thereby forming the first recess 103 having the dendritic structure 104 on the surface. In this manner, the metal member 101 having the third recess 121 formed at an angle of 90 degrees with respect to the surface can be obtained. Next, as in the other embodiments, the resin member 102 is formed on the surface of the metal member 101, thereby obtaining the bonded body 120 having the third recess 121 having an inclination of 90 degrees with respect to the surface of the metal member 101.
[0052] As described above, in the resin-metal bonded body of embodiment 3, in addition to the configuration of embodiment 1, metal member 101 has a recess on the bonding surface with resin member 102, the recess includes third recess 121 formed at an angle with respect to the surface of metal member 101, and first recess 103 formed on the surface of third recess 121, and dendritic structure 104 is formed on the surface of first recess 103.
[0053] According to this configuration, the resin member 102 fills the third recess 121 formed in the metal member 101, and a sufficient contact area can be ensured between the resin member 102 and the dendritic structure 104 of the nanometer order formed on the surface of the first recess 103. This provides a stronger anchor effect, resulting in a bonded body 120 in which the metal member 101 and the resin member 102 are bonded more strongly.
[0054] Embodiment 4 FIG. 16 is a schematic cross-sectional view of a semiconductor device 200 according to the fourth embodiment. As shown in FIG. 16, in a semiconductor device 200, a semiconductor element 201 is mounted on an insulating substrate 207, and the surface of the insulating substrate 207 opposite to the surface on which the semiconductor element 201 is mounted is joined to a heat spreader 209. The semiconductor element 201 is formed by forming an insulated gate bipolar transistor (IGBT) or a diode (Di) on a semiconductor substrate such as silicon (Si), silicon carbide (SiC), or gallium nitride (GaN). However, the semiconductor element 201 is not limited to the above configuration, and may be, for example, an insulated gate field effect transistor (MOSFET) or a high electron mobility transistor (HEMT). Also, the semiconductor element 201 may be formed of a plurality of pieces, and a plurality of types of semiconductor elements may be mounted. The surface of the insulating substrate 207 is provided with a conductive layer 208 formed of a metal member, and the semiconductor element 201 is joined to the conductive layer 208 by solder 206. The insulating substrate 207 is formed of, for example, aluminum nitride (AlN). A resin case 205 is fixed to the insulating substrate 207 on which the semiconductor element 201 is mounted. An electrode terminal 203 formed of a metal member is attached to the resin case 205. The resin case 205 is formed of, for example, polyphenylene sulfide resin. The electrode terminal 203 and the surface electrode 210 formed of a metal member are electrically connected by the wire 202. The wire 202 is a wire using a conductive metal member such as Au or Al, and connects the electrode terminal 203 and the surface electrode 210 by wire bonding. Here, the first recess 103 is formed on at least a part of the surface of the surface electrode 210, the electrode terminal 203, and the conductive layer 208, and the dendritic structure 104 is formed on the surface of the first recess 103. The depth of the first recess 103 to the bottom is preferably in a range deeper than 100 nm and shallower than 10 μm, and the ratio of the depth to the width of the first recess 103 is preferably 0.002 or more and 0.2 or less. Moreover, the thickness of the dendritic structure 104 is preferably within a range of 1 / 1000 to 1 / 100 of the width of the first recess 103, and further preferably within a range of 1 / 100 to 1 / 10 of the depth of the first recess 103. Furthermore, the semiconductor device 200 is sealed with a resin member 204 as a sealing resin.The resin member 204 is impregnated into the dendritic structure 104 formed on at least a part of the surface of the surface electrode 210, the electrode terminal 203, and the conductive layer 208, to form a resin-metal bonded body.
[0055] In the semiconductor device configured in this manner, resin member 204 is impregnated into tree-like structure portion 104, thereby ensuring a sufficient contact area between resin member 204 and tree-like structure portion 104. Furthermore, the molecules constituting resin member 204 and the molecules constituting tree-like structure portion 104 are close to each other on the nanometer order, which causes intermolecular forces to act, thereby firmly bonding resin member 204 and tree-like structure portion 104.
[0056] As described above, the configuration shown in the fourth embodiment makes it possible to obtain a semiconductor device equipped with a resin seal having high strength and long-term durability without using functional molecules, etc., while suppressing the decrease in productivity associated with the formation of a structure to obtain an anchor effect.
[0057] Next, an example of a method for manufacturing the above-mentioned semiconductor device 200 will be described. First, an insulating substrate 207 is prepared. A conductive layer 208 formed of a metal member is provided on the surface of the insulating substrate 207. A semiconductor element 201 is disposed on the conductive layer 208 via solder 206, and the semiconductor element 201 is bonded to the conductive layer 208 by a reflow process. This electrically connects the semiconductor element 201 and the conductive layer 208. Here, the semiconductor element 201 may be one in which the first recess 103 and the dendritic structure 104 are formed in advance on a surface electrode 210 formed of a metal member. The first recess 103 and the dendritic structure 104 are preferably formed by irradiating a pulsed laser. In addition, in order to prevent the shapes of the first recess 103 and the dendritic structure 104 from being affected by deformation or the like due to heat, it is preferable that the pulse width is as short as possible. Specifically, the pulse width is preferably 10 ns or less. The wavelength of the pulsed laser is not particularly limited, but examples of wavelengths suitable for metal processing include wavelengths of 200 nm to 10,000 nm, and more preferably wavelengths of 400 nm to 2,000 nm. The energy density of the pulsed laser irradiated per unit area is 0.5 J / cm.2 More than 50J / cm 2 The following range is preferable. Furthermore, 5 J / cm 2 More than 30J / cm 2 The following range is more preferable: 5 J / cm 2 If the energy supply amount is less than 30 J / cm, the first recess 103 and the dendritic structure 104 are not formed because of the small amount of energy supplied. 2 If the energy supply exceeds 100%, the dendritic structure 104 melts due to the excessive energy supply, and only the first recess 103 is formed. 2 Laser irradiation may be performed in a gas atmosphere such as Ar or He. By performing laser irradiation in an inert gas atmosphere, for example, oxidation of the surface electrode 210, the first recess 103, and the dendritic structure 104 can be suppressed, and therefore, the method can also be applied to control the wettability of the surface electrode 210, the first recess 103, and the dendritic structure 104 after laser irradiation. Furthermore, for the purpose of cooling, laser irradiation can also be performed while flowing an inert gas. Furthermore, the above-mentioned pulse laser may be irradiated to the conductive layer 208 in addition to the surface electrode 210, to form the first recess 103 and the dendritic structure 104 on the surface of the conductive layer 208.
[0058] Next, the electrode terminal 203 formed of a metal member and the semiconductor element 201 are electrically connected by the wire 202 formed of a metal member. The wire 202 is bonded to the electrode terminal 203 and the semiconductor element 201 by, for example, a wire bonding device. Similarly, the electrode terminal 203 and the conductive layer 208 are electrically connected by the wire 202. Note that the wire 202 may be one in which the first recess 103 and the dendritic structure 104 have been formed in advance by the above-mentioned pulsed laser irradiation.
[0059] Next, the insulating substrate 207 and the semiconductor element 201 mounted on the insulating substrate 207 are sealed with the resin member 204. For example, a liquid sealing material such as an epoxy resin is used as the resin member 204, which is poured into the resin case 205 until the semiconductor element 201 and the wires 202 mounted on the insulating substrate 207 are immersed in the resin member 204, and is hardened by heat treatment.
[0060] As a result of the above, a first recess 103 and a dendritic structure 104 are formed in at least a portion of the surface electrode 210, conductive layer 208, electrode terminal 203 and wire 202 formed from metal members, and the portions in which the first recess 103 and the dendritic structure 104 are formed are firmly bonded to the resin member 204.
[0061] Therefore, in the semiconductor device of embodiment 4, a surface electrode, a conductive layer, an electrode terminal or a wire is resin-sealed with a resin member, and at least a part of the bond between the surface electrode, the conductive layer, the electrode terminal or the wire and the resin member comprises the bond described in embodiment 1.
[0062] With this configuration, a sufficient contact area can be secured between the resin member 204 and the surface electrode 210, the conductive layer 208, the electrode terminal 203, and the dendritic structure 104 of nanometer order provided on the wire 202, which are formed from a metal member, so that a semiconductor device 200 can be obtained, which includes a bonded body in which the surface electrode 210, the conductive layer 208, the electrode terminal 203, and the wire 202 are firmly bonded to the resin member 204.
[0063] The embodiment shown here is merely an example and is not intended to be limiting. For example, immediately before sealing with resin member 204, first recess 103 and dendritic structure 104 may be formed by irradiating at least a part of surface electrode 210, conductive layer 208, electrode terminal 203, and wire member with a pulsed laser, thereby fabricating semiconductor device 200.
[0064] Furthermore, the present disclosure is not limited to application to the above-mentioned semiconductor device, but is a technology that can be widely applied to fields in which resin-metal bonding is used. For example, examples of applications of resin-metal bonding include vehicle parts, electric railway parts, elevator parts, aircraft parts, artificial satellite parts, optical communication parts, industrial robot parts, generator parts, air conditioning and heating equipment parts, and home appliance parts. [Explanation of symbols]
[0065] 100 zygote 101 Metallic parts 102 Resin parts 103 First recess 104 Dendritic structure 110 Zygote 111 Second recess 120 Zygote 121 Third recess 200 Semiconductor device 201 Semiconductor elements 202 Wire 203 Electrode terminal 204 Resin parts 205 Resin Case 206 Solder 207 Insulating Substrate 208 Conductive Layer 209 Heat spreader 210 Surface electrode
Claims
1. A metal member; a resin member bonded to the metal member; Equipped with the metal member has a dendritic structure on a surface to be joined with the resin member, At least a part of the dendritic structure has a diameter on the order of nanometers; The resin member is impregnated into the dendritic structure portion, the metal member has a recess on a surface to be joined with the resin member, the recess includes a first recess having the dendritic structure on a surface thereof and a second recess deeper than the first recess, the first recess and the second recess being alternately formed in a positional relationship; A conjugate characterized in that
2. A metal member, a resin member bonded to the metal member; Equipped with the metal member has a dendritic structure on a surface to be joined with the resin member, At least a part of the dendritic structure has a diameter on the order of nanometers; The resin member is impregnated into the dendritic structure portion, the metal member has a recess on a surface to be joined with the resin member, the recess includes a third recess formed at an inclination with respect to a surface of the metal member, and a first recess formed on a surface of the third recess, and the dendritic structure portion is formed on a surface of the first recess. A conjugate characterized in that
3. The depth of the recess is 10 μm or less.
3. The bonded body according to claim 1 or 2.
4. The ratio (X / Y) of the depth (X) to the width (Y) is 0.2 or less; 4. The bonded body according to claim 3.
5. The dendritic structure is formed on a surface of the recess, The thickness of the dendritic structure is 1 / 100 or less of the width of the recess.
3. The bonded body according to claim 1 or 2.
6. The thickness of the dendritic structure is equal to or less than one-tenth of the depth of the recess.
3. The bonded body according to claim 1 or 2.
7. The dendritic structure is formed around the recess.
3. The bonded body according to claim 1 or 2.
8. The third recess has an inclination of less than 90 degrees with respect to the surface of the metal member.
3. The bonded body according to claim 2.
9. A semiconductor device in which a surface electrode, a conductive layer, an electrode terminal, or a wire is resin-encapsulated with a resin member, the surface electrode, the conductive layer, the electrode terminal, and the wire are metal members, 3. A semiconductor device, wherein at least a part of a bonded structure between said surface electrode, said conductive layer, said electrode terminal or said wire and said resin member is the bonded structure according to claim 1.
Citation Information
Patent Citations
Manufacturing of high capacity prismatic lithium-ion alloy anode
JP2017130457A
Electronic device and method for manufacturing the same
JP2018067600A
Hybrid composite material of metal surface and polymer material surface and method for manufacturing the hybrid composite material
JP2019528182A
Metal member, metal member surface processing method, semiconductor device, semiconductor device manufacturing method, and composite molded body
WO2015087482A1
Joining metal member and joining body
WO2020230200A1