Method for thermally bonding plastic bags and method for manufacturing plastic bags

The method uses fine protrusions on heat bars to form a mold adhesive band, addressing the issue of bag breakage and adhesive strength in thermal bonding, achieving strong and reliable sealing with reduced plastic usage.

JP7590046B1Active Publication Date: 2024-11-26菱沼一夫
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024103604
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-26
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing thermal bonding methods for plastic bags fail to achieve both strong adhesive strength and bag breakage prevention, often resulting in pinholes and edge breakage due to uneven heat distribution and protruding plastic beads.

Method used

A method involving fine semicircular or trapezoidal protrusions on heat bars to control the injection of molten sealant, forming a mold adhesive band that matches the inherent breaking strength and elongation properties of the material, preventing edge breakage and ensuring cohesive adhesion.

Benefits of technology

Simultaneously achieves adhesive strength asymptotic to the material's breaking force while preventing bag breakage, reducing plastic usage, and ensuring reliable sealing without pinholes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590046000001_ABST
    Figure 0007590046000001_ABST
Patent Text Reader

Abstract

To provide a method for thermally bonding plastic bags and a method for manufacturing plastic bags, which can simultaneously achieve prevention of bag breakage, sealing, and adhesive strength approaching the breaking strength of the material. [Solution] A method for thermally sealing plastic bags, which includes sandwiching a heat seal material between a pair of heating bodies and heat sealing it, wherein one of the pair of heating bodies has linear protrusions with fine semicircular or trapezoidal cross-sectional shapes, and the heated linear protrusions are pressed against a sealant of the heat seal material, thereby injecting the sealant, molten in a cohesive adhesion temperature range, in a band-like shape along the side ends of the linear protrusions to form a molded adhesive band.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for thermally bonding plastic bags and a method for manufacturing plastic bags. Specifically, the present invention relates to a method for thermally sealing plastic bags and a method for manufacturing plastic bags that can simultaneously achieve bag breakage prevention, sealing, and adhesive strength approaching the breaking strength of the material. [Background technology]

[0002] Bags / container packaging (flexible packaging) made of plastic film or sheet materials are made by thermal bonding (hereafter referred to as "heat sealing"), in which a heated metal body is pressed against the outer surface to be bonded, or by utilizing the internal heat generated by electromagnetic waves or ultrasonic waves, and the bag is then sealed after being filled with the contents. As a result of many years of intensive research by the present inventors, technical progress in thermal bonding has been accumulating (see, for example, Patent Documents 1 to 4), expectations in thermal bonding can be summarized into the following two points. (1) Simultaneous achievement of "sealing" and "easy opening" without cutting the inner edge of the heat-sealed surface (2) Obtaining adhesive strength that approaches the material's breaking strength without edge breakage

[0003] (Basic operation of heat sealing technique) For soft packaging products, plastic films and sheets are used. Heat sealing techniques, taking advantage of the thermoplasticity of plastic materials, are used to make bags and seal packages after they have been filled. Heat sealing techniques involve pressing a heating element (heat bar) against the outer surface of the plastic material to heat the bonding surface through thermal conduction, or by using electromagnetic waves or ultrasonic waves to generate heat inside the material and heat the area near the bonding surface. The plastic materials discussed here are composite materials in which a surface material and a sealant are bonded together (lamination).

[0004] The heat jaw system, which is made up of a pair of heat bars 1-1 and 1-2, generates heat from heaters 2-1 and 2-2, and presses and heats the outer surface of material 3, is shown in Figure 1. The automatic heat jaw system performs several dozen operations per minute, and is characterized by completing the target operation in just 0.5 to 1.0 seconds. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-313782 A [Patent Document 2] JP 2016-43988 A [Patent Document 3] JP 2017-114018 A [Patent Document 4] Patent Publication No. 2021-014039 Summary of the Invention [Problem to be solved by the invention]

[0006] (Explanation of heat seal strength) The primary parameter for heat seal completion is the adhesive interface temperature. The thermal adhesive strength (heat seal strength) of the heated specimen, with the controlled adhesive surface temperature as a parameter, is measured by a group of tensile tests in which both ends of the specimen are pinched and cut to a width of 15 mm. Figure 2 shows a graph plotting the weld surface temperature on the horizontal axis and the tensile strength (N / 15 mm) on the vertical axis. Since heat seal strength changes depending on the heating speed, Figure 2 shows three representative examples of heating speeds: high, medium, and low.

[0007] (Instructions for completing the heat seal surface) To achieve heat seal strength, adhesion on the order of nanometers is necessary. The nanometer-scale minute uneven surface of a material can be sealed by pressing the material softened by heating. ASTM F2029:2000 (the only public standard in the world that uses the heating temperature as a parameter in heat sealing techniques) specifies that the pressure applied to the heated surface should be 0.1 to 0.4 MPa.

[0008] (Explanation of the establishment of adhesive state on heat seal surface) When examining a single heated specimen, if the same heating rate is strictly observed, the effect of the heating rate can be ignored. The rise in heat seal strength begins with the interfacial adhesion where peeling occurs on the adhesive surface, and gradually increases until the adhesive surface becomes a molded cohesive adhesive state in the molten state. The tensile test strength in this state approaches the breaking strength of the packaging material.

[0009] The adhesion of the interface adhesive band utilizes the peel energy of the adhesive surface to simultaneously realize easy opening and resistance to tearing, so the heat seal strength is 0.5 to 10 N / 15 mm, which is much smaller than the breaking strength of the packaging material. In reality, to utilize the peel energy function, the adhesive surface needs to have a peel seal width of at least 5 mm.

[0010] Today, the expected functions of the interface adhesion state have been solved by applying the technologies shown in Patent Documents 1 to 4. In cohesive adhesion, peeling of the adhesive surface does not occur, so peeling energy cannot be utilized, and the elongation energy of the material is utilized to absorb the bag rupture energy.

[0011] (Actual heat adhesion properties of retort pouch materials) An example of analog output from a tensile test of a normal flat-surface heat-sealed specimen (retort pouch material) is shown in Figure 3. To improve gas barrier properties, retort pouches have highly thermally conductive aluminum foil inserted into the surface material. This aluminum foil allows the heat flow from the heat bar to flow outside the system, so even if the heat is uniformly applied, the heat-sealed surface exhibits a characteristic temperature distribution in which the center is the highest. (1) When heated to 146°C, the heat seal surface has a mixture of interfacial adhesion (peel seal) and cohesive adhesion. This is the heating temperature required to obtain the highest heat seal strength and prevent edge tearing. (2) At temperatures below 145°C, the entire surface is in a peel-sealed state, so the edges of the heat seal do not break. (3) In high-temperature adhesive zones above 150°C, the entire surface is in a molten, cohesive adhesive state, resulting in a strong adhesive state, but unevenly protruding sealant poly beads are formed at the heat-sealed edges. When poly beads are formed in a peak shape at the edge, the bag-breaking force becomes a concentrated load at the apex, and even a low bag-breaking force can easily create a pinhole, which then becomes the starting point for bag-breaking. At this point, the heat-sealed width of the cohesive adhesive zone has no effect on the break resistance. Table 1 shows the relationship between the fine protrusions on the heat-sealed edge and the bag-rupturing force (the force that creates pinholes on an uneven heat-sealed edge).

[0012] [Table 1]

[0013] Table 1 shows that even in adhesive surfaces with a breaking load of 20 to 70 N / 15 mm, pinholes can easily occur under a localized load of several N, and these pinholes can become the starting point for fracture. In the case of cohesive adhesion (20N / 15mm), even if the pile width (poly ball dimension) is 5mm, it can cause bag breakage of 7N / 15mm. In the case of 70N / 15mm, the size of the plastic ball is 1mm and a pinhole will easily occur with a bag breakage source of 5N / 15mm.

[0014] (Actual measurement of peeling energy) Figure 3 shows an example of a tensile test pattern of a heat-sealed sample heated at each temperature (example: retort pouch). Figure 4 shows an example of an evaluation test of the resistance to breakage of a heat-sealed sample (example: retort pouch sample), and is a calculation result of analyzing the resistance to breakage of the interfacial adhesive zone using peel energy theory based on the data in Figure 3, with heating temperature as a parameter. Regarding the peel energy, the measured values ​​at each peel point in the tensile test at each temperature were converted to 1 / 15=1 mm, the peel energy (mJ) at each point was calculated, and the verification range was integrated to create a graph. (1) For cohesively bonded specimens, the tensile distance to the breaking point was integrated. (2) For the interfacial adhesion specimens, the integral value up to the partial break point (11 mm) at 146°C was taken. (3) The integral value up to the breaking point at 170°C (≒1 mm) was set to 1, and the other calculation results were shown as "multiples of peel energy." Heating to 146°C showed approximately four times the breaking resistance of 170°C, where there is a risk of edge cutting. Looking at the starting point of peeling from the edge of the heated surface, at 146°C it begins at approximately 0.8 mm. When heated to 170°C, due to the effect of residual heat, it starts at (-0.5 mm) and reaches the yield point at about 1 mm. For reference, heat seal strength data, which is an index for normal heat seal management, is also shown. From the perspective of peel energy theory, the suitability of "heat seal strength" used to evaluate heat seal properties is questionable.

[0015] Figure 5 shows an example of a specimen where an edge break occurred after a tensile test of OPP (biaxially oriented polypropylene) / LLDPE (low density polyethylene) was stopped midway. The heat seal line is established. It can be seen that pinholes / breaks have occurred at multiple points starting from the heat seal edge.

[0016] The inventors attempted to establish a thermal adhesion method that avoids the generation of pinholes by utilizing the adhesive strength near the inherent breaking strength of plastic materials, that is, by suppressing the molten sealant from protruding from the bonding surface to the edge as a poly bead, and by realizing precise cohesive adhesion control near the melting temperature (Tm).

[0017] (Analysis of the mechanism behind bag breakage) The causes of composite failure can be classified into the following situations: (1) The whole thing breaks at once (2) The adhesive strength (lamination strength) between the sealant and the surface material is related. (3) The differences in tensile strength and breaking strength of each component material are related. 1) (Delamination strength) < (Elongation strength of sealant) < (Elongation strength of surface material) → The sealant stretches and delamination occurs. 2) (Elongation strength of sealant) > (Elongation strength of surface material) > (Delamination strength) → The surface material stretches and delamination occurs. (4) After (3)-1), the tensile strength of the sealant becomes greater than the tensile strength of the surface layer. → Surface layer breaks → Sealant stretches and breaks → End (5) After (3)-2), the tensile strength of the sealant becomes less than the tensile strength of the surface layer. → Sealant stretches and breaks → End In reality, most applications fall into the categories of (4) and (5), so the rupture resistance of composite materials is evaluated based on two criteria: (i) the breaking strength of the surface material and (ii) the tensile breaking strength of the sealant. (4) is related to the loss of barrier performance of the surface material, and (5) is related to preventing leakage of the contents.

[0018] (Bag breakage control method) The bursting forces that damage heat-sealed edges are caused by static stacking compression forces and dynamic shocks and vibrations during transportation and storage. Since it is statically defined as (compressive stress) = (peel force) x (peel length), preparation should be made so that (bag-breaking force) < (compressive stress).

[0019] In the case of a quadrilateral bag, the bag-rupturing force starts at the tangent point of the inscribed circle, and the peel line expands / progresses in an arc. In the case of a static load such as compression, the relationship begins with [(peel force) = (heat seal strength) x peel length] < (bag breaking force), and as the peeling of the heat seal surface progresses, the peeling stops when the above relationship becomes equal. If the bag-breaking force is below this condition for the next load, peeling will not progress. The resistance to tearing of the bag can be controlled by selecting the heat seal strength and width.

[0020] However, impacts from drops and vibrations during transportation act locally on the heat-sealed edge in a pulsed manner. Since multiple impacts act individually each time, there is a limit to the use of bag-break resistance due to the expansion of the peel surface. The current standard, JIS Z 0238:1968 (Test method for heat-sealed flexible packaging bags and semi-rigid containers), specifies break resistance on the premise of absorbing two impact loads, so greater improvement in resistance is required. It is expected that dynamic bag-break resistance will be developed through cohesive adhesion (molded adhesion) that utilizes the inherent breaking strength and elongation of the material.

[0021] One object of the present invention is to provide a method for thermally sealing plastic bags and a method for manufacturing plastic bags that can simultaneously achieve prevention of bag breakage, sealing, and adhesive strength approaching the breaking strength of the material. [Means for solving the problem]

[0022] (Definition of the common name of the present invention) Hereinafter, the adhesive formed by the present invention may be commonly referred to as "mold adhesive."

[0023] It is desirable to establish a method for eliminating edge severance in a heat bonding operation of cohesively bonded strips of plastic materials, and to utilize the heat seal strength and elongation properties of the material that approach the inherent breaking strength of the material. (1) To clarify the defect conditions of the conventional surface pressing / heating method that causes poly beads to form at the heat seal edge. (2) The end side of the bag is locally molded (see Figure 6). (3) This will be addressed during the filling and sealing process and the bag making process. (4) The surface material is modeled after a microscopic pressure vessel and used as an injection device. (5) The heat bar's compression section is shaped into a minute semicircle or trapezoid to create a micro injection pump. (6) The width of the heat seal fin is to be shortened (see Figure 7). (7) We present a direct method to reduce the amount of plastic materials used as required by the SDGs. The pouch size in Figure 7 is (115mm x 150mm = 17,250mm 2 If the heat seal width is reduced by 9 mm by introducing "mold bonding", the result is (140 mm x 9 mm x 2) + (105 mm x 9 mm x 2) = 4,410 mm. 2 The reduction in area is (4,410 / 17,250) = 26%.

[0024] The problem to be solved by the present invention can be solved in the filling and sealing process and the bag making process of packaging. (1) The outer edge 7 of the sealant is finished into a molded state 6 (see FIG. 6). (2) A portion of the sealant is locally heated and a small amount of molten sealant is injected into the area corresponding to the outer edge of the bag, creating a new structure that prevents plastic beads from forming at the joint surface of the sealant.

[0025] An example of a method for solving the problems of the present invention will be described below. (1) A semicircular or trapezoidal fine projection 8 or 9 is provided on the heating / pressure bonding surface of the heat bar (see FIG. 9). (2) The outer edge side portion 17 of the sealant is heated to near its melting temperature (Tm). (3) The melted sealant in the fine parts flows, and the bonding pressure 14 of the semicircular or trapezoidal protrusions is adjusted so that the surface layers come into contact with each other. To prevent overpressurization, spacers 19 and 20 are installed on both ends of the heat bar, and the compression dimension is automatically adjusted to approximately the width of two surface layers. (4) The surface material around the heating portion is used as the pressure vessel 18. (5) By heating / pressing the fine semicircular or trapezoidal protrusions, the molten mold mass 15 inside the pressure vessel 18 is injected into the outer edge side portion 17 of the weakly heated portion, bringing the sides of the bag body into a "mold bonded" state.

[0026] (6) The dimensions of the semicircular or trapezoidal protrusions are changed to optimize the injection amount. (7) Depending on the thickness of the sealant to be applied, the semicircle or trapezoid can be completed with a heat seal fin that is about twice the base dimension, so a heat seal fin of 2 to 3 mm will suffice (see Figure 7). (8) FIG. 8 shows a cross-sectional micrograph of an embodiment using semicircular single protrusions (1 and 3 mm). For comparison, we have attached a video of flat compression bonding. It can be seen that the desired mold mass is formed even with the thin sealant OPP / LLDPE (thickness 20 μm). The sealant for retort pouches is 50μm thick. The molded mass produced when a single protrusion of 3mm was selected was sufficient. It was found that the desired effect could be obtained even with a single protrusion of 1mm. Weakness of the heat-sealed edges of the cohesively bonded flat-pressed specimens was observed.

[0027] (9) The characteristics of the “mold bonding” of the present invention and the conventional flat pressure bonding method are illustrated in FIG. 1) The heat seal width of the flat pressure bonding method is 10 to 15 mm. When the entire surface is melted and pressure bonded, a large amount of the sealant becomes paste-like and unevenly protrudes onto the heat seal edge, forming poly beads. If the flat pressure bonding width is set to 10 mm and the heat bonding area is compared, it is about 10 times larger (see Figure 10 (b)). 2) The protruding polystyrene beads 25 are welded 26 to the surface of the sealant 13. A bag-breaking force acts, and the intersection of the load line 27 and the polystyrene beads becomes the pinhole generation point, leading to a sudden breakage. 3) The stress required for pinhole generation in this state is as shown in Table 1, and even the durable sealant 13 will break at a few Newtons. 4) A large amount of molten sealant is generated during flat pressure bonding. Reducing this amount is a solution to the problem. 5) In the present invention, as shown in FIG. 9, the amount of molten sealant produced is controlled by heating and compressing the material using minute semicircular or trapezoidal protrusions, preferably of about 1 mm.

[0028] According to the present invention, the following method for thermally bonding plastic bags can be provided. 1. A method for thermally sealing plastic bags, comprising sandwiching a heat seal material between a pair of heating bodies and heat sealing it, wherein one of the pair of heating bodies has linear protrusions with fine semicircular or trapezoidal cross-sectional shapes, and the heated linear protrusions are pressed against a sealant of the heat seal material, thereby injecting the sealant, which has been melted in a temperature range for cohesive adhesion, in a band-like shape along the side edges of the linear protrusions to form a molded adhesive band. 2. The method for thermally sealing plastic bags described in 1, wherein the heat-sealing material is a composite material containing a surface material and a sealant, and in the injection, the surface material of the composite material is used as a pressure vessel. 3. The method for thermally sealing plastic bags described in 1 or 2, wherein the diameter of the semicircle is 0.5 to 3 mm and the lower base of the trapezoid is 0.5 to 3 mm. 4. A method for thermally sealing plastic bags described in any one of 1 to 3, which includes adjusting the amount of molten sealant injected by changing the dimensions of the semicircle or trapezoid. 5. A method for producing a plastic bag, comprising producing a plastic bag having the molded adhesive band formed thereon, using the method for thermally bonding a plastic bag described in any one of 1 to 4. Effect of the Invention

[0029] According to the present invention, it is possible to provide a method for thermally sealing plastic bags and a method for manufacturing plastic bags, which can simultaneously achieve prevention of bag breakage, sealing, and adhesive strength that approaches the breaking strength of the material. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a diagram illustrating an implementation model (heat jaw method) of thermal adhesion (heat sealing). [Diagram 2] FIG. 1 is a diagram illustrating a model for expressing heat seal strength. [Diagram 3] FIG. 1 is a diagram illustrating the tensile test patterns of heat-sealed specimens heated at each temperature (example: retort pouch). [Figure 4] FIG. 1 is a diagram illustrating an evaluation test of the fracture resistance of a heat-sealed specimen (example: retort pouch specimen). [Diagram 5] This is a photograph to explain an example of a broken bag caused by OPP / LLDPE plastic balls. [Figure 6] FIG. 1 is a diagram illustrating a model of “mold adhesion.” [Figure 7] FIG. 1 is a diagram illustrating the difference between the heat seal surfaces of "mold bonding" and flat bonding. [Figure 8] This is a micrograph (example) of the crimped cross section of a heat-sealed specimen with cohesive adhesion. [Figure 9] FIG. 1 is a diagram illustrating a working model of "mold bonding." [Figure 10] FIG. 1 is a diagram for comparing and explaining the characteristics of the tensile test of "mold bonding" and flat pressure bonding. [Figure 11] FIG. 1 is a diagram illustrating a tensile test pattern for "mold adhesion" of a retort pouch. [Figure 12] FIG. 13 is a diagram illustrating the “mold bond” pattern differentiation calculation for a retort pouch. [Figure 13] This is a photograph of a fracture in a tensile test of "mold adhesion" of a retort pouch material. [Figure 14] FIG. 1 is a diagram illustrating the application of "mold bonding" to an OPP / LLDPE film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The method for thermally bonding plastic bags and the method for producing plastic bags of the present invention will be described in detail below. In this specification, "x to y" represents a numerical range of "not less than x and not more than y." The upper and lower limit values ​​described in relation to the numerical ranges can be combined in any combination. In addition, among the individual embodiments of the aspects of the present invention described below, it is possible to combine two or more embodiments that are not mutually contradictory, and an embodiment combining two or more embodiments is also an embodiment of the aspects of the present invention.

[0032] A method for thermally bonding a plastic bag according to one aspect of the present invention includes the steps of: A method for heat-sealing a plastic bag, comprising: sandwiching a heat-sealing material between a pair of heaters and heat-sealing the material; One of the pair of heating bodies has a linear protrusion having a fine semicircular or trapezoidal cross-sectional shape, The method includes pressing the heated linear protrusion against the sealant of the heat seal material, thereby injecting the sealant molten at a temperature range for cohesive adhesion in a band shape along the side end of the linear protrusion to form a molded adhesive band. According to this embodiment, it is possible to simultaneously achieve prevention of bag breakage, sealing, and adhesive strength approaching the breaking strength of the material. Furthermore, according to this embodiment, the following effects can be obtained in particular. (1) An accurate heat sealing method for cohesive adhesion (mold adhesion) approaching the breaking strength of the plastic material can be perfected, ensuring strong resistance to bag breakage. (2) It will be possible to concretely reduce the amount of plastic used, as required by the SDGs.

[0033] An embodiment of this aspect will be described with reference to Fig. 9. Fig. 9 is an explanatory diagram of an operating model of "mold bonding." In Fig. 9, (a) is a side cross-sectional view showing a standby state of mold bonding, (b) is a side cross-sectional view showing the mold bonding during compression (an example of compression of a semicircular protrusion), and (c) is a front view explaining the installation of a spacer for adjusting the compression pressure.

[0034] One embodiment of this aspect can be carried out according to the following (1) to (7). (1) A fine single projection having a semicircular 8 or trapezoidal 9 shape is provided on the heating / pressure bonding surface of a heat bar (FIG. 9(a)). In FIG. 9(a), the case where the cross section of the fine single projection is a semicircular 8 is shown by a solid line, and the case where the cross section is a trapezoidal 9 is shown by a dashed line. The heat-sealing device used in this embodiment is equipped with a pair of heating elements arranged to face each other. Here, one heating element is composed of a heat bar body 10 and a fine single protrusion of semicircular 8 or trapezoidal 9 attached to the surface of the heat bar body 10 facing the other heating element. The fine single protrusion is provided along the longitudinal direction of the heat bar body 10. The fine single protrusion can be formed by performing fine processing on the surface of a heat bar made of a commonly used metal such as brass, copper, aluminum, stainless steel, etc. The other heating element is constituted by a heat bar main body 11. The surface of the heat bar main body 11 on the side of one heating element is constituted to be wider than the fine single-line projections. The material of the member constituting the contact surface of the heat bar main body 11 with the heat seal material (surface layer materials 12-1, 12-2 and sealant 13) can be, for example, a resin. As the resin, a material that does not soften even at the heating temperature during heat sealing can be suitably used, and for example, a fluororesin (for example, polytetrafluoroethylene), a polyimide resin, etc. can be used. Specific examples of such resins include Teflon and Kapton (both are registered trademarks of DuPont). In addition, the member constituting the contact surface does not necessarily have to be an elastic body (for example, an elastic body with a Shore hardness of 40A to 90A, such as silicone rubber or fluororubber) as described in Patent Document 2. Here, the heat seal material disposed between the pair of heaters is composed of two composite materials. Each composite material is a laminate including a surface layer material and a sealant. The two composite materials are disposed with the sealant sides facing each other. The thickness of the surface layer material in one composite material can be appropriately set, for example, 10 to 3,000 μm, and preferably 20 to 2,000 μm. The surface layer material may be a single layer, or may be a laminate of two or more layers. The surface layer material may be a layer other than the sealant in the composite material, and may also be called a "substrate layer." The thickness of the sealant in one sheet of composite material can be appropriately set, for example, from 10 to 3,000 μm, and preferably from 20 to 2,000 μm.

[0035] At least one of the pair of heated heating bodies is moved to sandwich the heat seal material (surface materials 12-1, 12-2 and sealant 13) between the pair of heating bodies. This makes it possible to press the heated fine projections toward the sealant of the heat seal material. At this time, the molten sealant is injected in a band shape along the side edge of the fine projections to form a mold adhesive band made of the mold block 15 (FIG. 9(b)). Specifically, this is as follows.

[0036] (2) The outer edge side portion 17 of the sealant is heated to near its melting temperature (Tm). The mold block 15 formed by the fine single projection 8 is generated on the bag side (inside the bag) and on the outer edge side of the bag. In this embodiment, the mold block formed on the bag side can be utilized. In addition, the "outer edge side portion 17 of the sealant" is the boundary portion between the bonded / non-bonded portions of the sealant 13 of the surface materials 12-1, 12-2 on the inside of the bag, and is the portion of the molded mass 15 formed on the bag side that is located on the inside of the bag. The outer edge side portion 17 of the sealant is preferably heated to a temperature near the melting temperature (Tm) of the sealant, for example, in the range of Tm±5 to 10°C, preferably Tm to Tm+10°C, and more preferably Tm to Tm+5°C.

[0037] (3) The compression pressure 14 of the semicircular or trapezoidal projections is adjusted so that the molten sealant in the fine portions (portions compressed by the fine single projections) flows and the surface layers come into contact with each other. At this time, in order to automatically prevent excessive pressurization, it is preferable to install spacers 19, 20 on both ends of the heat bar (between the heat bar bodies 10, 11) and satisfy the following condition (i) or (ii) (see FIG. 9(c)). Condition (i): Spacer height H [mm] ≒ (thickness of one surface layer [mm]) × 2 + (height of one protrusion h [mm]) Condition (ii): Spacer height H [mm] × α = (thickness of one surface layer [mm]) × 2 + (height of one protrusion h [mm]) Here, α is in the range of 0.9 to 1.1. In addition to or instead of the embodiment in which a spacer is provided (or the distance between the pair of heating bodies is adjusted when the pair of heating bodies is closest to each other), the bonding pressure 14 may be adjusted. The compression by the pair of heating bodies is driven by an air cylinder, and the bonding pressure 14 can be adjusted by the driving pressure of the air cylinder. Excessive pressurization can be prevented by providing spacers (or adjusting the distance between the pair of heating bodies when they are closest to each other) or by adjusting the bonding pressure 14. Here, "excessive pressurization" corresponds to, for example, pressurizing the heat seal material so that the thickness becomes thinner than the total thickness of the two surface layers of the heat seal material.

[0038] (4) The load on the fine single protrusion shall be 20 to 30 N / 10 mm. This load corresponds to 0.15 to 0.2 MPa for surface pressure bonding of a width of 15 mm, which is not a particularly large operating force.

[0039] (5) The surface material around the heating portion is used as the pressure vessel 18. That is, the heat seal material is a composite material containing a surface layer material and a sealant, and in the injection molding, it is preferable to use the surface layer material of the composite material as a pressure vessel.

[0040] (6) By heating / pressing the fine single protrusion, the molten sealant in the pressure vessel is injected into the outer edge side portion 17 of the sealant in the weakly heated portion, bringing the side of the bag body into a "molded adhesive" state. Here, the "weakly heated area" refers to a region shifted laterally from the tip of the fine single projection, and although the sealant in this area is preheated by a pair of heating elements, it is heated less strongly (the temperature rises more slowly due to heating) than the sealant in the area pressed by the tip of the fine single projection, and since it is not cohesively bonded, no polymer beads are formed. The mold adhesive band thus formed is in the form of a band along the side edge of the linear protrusion (fine single protrusion), and its width (band width) is, for example, 0.5 to 3 mm, and preferably 1 to 2 mm.

[0041] (7) By changing the dimensions of the semicircular or trapezoidal shape, the amount of molten sealant injected is adjusted. The size is determined depending on the thickness of the sealant and the desired heating speed, but the size is preferably in the range of 0.5 to 3 mm, and more preferably in the range of 0.25 to 1.5 mm. Here, the above dimensions can be applied as diameters in the case of a semicircle, and as lower bases in the case of a trapezoid.

[0042] In the example of FIG. 9, the cross-sectional shape of the linear protrusion is mainly semicircular, but as shown by the dashed line in FIG. 9(a), the cross-sectional shape of the linear protrusion may be a trapezoid 9. In the case of the trapezoid 9, it is preferable that its upper base (the side forming the contact surface with the heat seal material) is shorter than its lower base (the side on the heat bar body 10 side). For example, when the length of the lower base of the trapezoid 9 is 100%, the length of the upper base is 20 to 80%. Each of the two interior angles (base angles) at both ends of the lower base of trapezoid 9 is preferably an acute angle, particularly preferably 45 to 80°. The two base angles may be the same or different. In addition, the term "trapezoid" includes not only a trapezoid but also a trapezoid with rounded corners at both ends of the upper base.

[0043] In this embodiment, it is essential to set the temperature during heat sealing in the temperature range of cohesive adhesion (also referred to as the "temperature region"). This gives fluidity to the sealant melted in the temperature range of cohesive adhesion, causes injection, and forms a molded adhesive. As described above, the temperature range of cohesive adhesion may be a temperature near the melting temperature (Tm) of the sealant, for example, in the range of Tm±5 to 10°C, preferably Tm to Tm+10°C, and more preferably Tm to Tm+5°C. The molded adhesive zone can achieve strong adhesion and sealing, and can provide reliable sealing even if the filling is liquid, for example. In contrast, in the technology described in Patent Document 2, the temperature during heat sealing is set to the temperature range for interfacial adhesion (the temperature range for forming a peel seal). The object of easy opening is achieved by such a peel seal. In this case, a temperature range lower than the melting temperature (Tm) of the sealant is applied. Furthermore, even if the sealant can be softened in this temperature range, it does not have enough fluidity to cause injection, and a mold adhesive zone is not formed.

[0044] A method for producing a plastic bag according to one aspect of the present invention includes producing a plastic bag having a molded adhesive band formed thereon using a thermal bonding method for a plastic bag according to one aspect of the present invention. According to this embodiment, the resulting plastic bag can simultaneously achieve bag breakage prevention, sealing, and adhesive strength approaching the breaking strength of the material. EXAMPLES

[0045] Examples of the present invention will be described below, but the present invention is not limited to these examples.

[0046] (Example 1): Confirmation of injection function using a semicircular single protrusion (thin plastic material) Applying the method shown in FIG. 9, a “mold-bonded” specimen was prepared under the following conditions: <Specimen material> Thin plastic material: OPP (biaxially oriented polypropylene) / LLDPE (low density polyethylene) 20μm, Tm of LLDPE sealant: 100~115℃ <Heating and bonding conditions> ·Heating: Equilibrium temperature heating, 114℃, 1 second - Single protrusion; semicircular cross section, diameter 1mm Crimping pressure: 100mm / 300N=30N / 10mm

[0047] (Example 2): Confirmation of injection function by semicircular single protrusion (retort pouch) Using the method shown in FIG. 9, “mold bonded” specimens were prepared and evaluated under the following conditions. <Specimen material> Retort pouch: PET (polyethylene terephthalate) / AL (aluminum) / CPP (non-oriented polypropylene) 50μm, Tm of CPP sealant: 170℃ <Heating and bonding conditions> ·Heating: Equilibrium temperature heating, 170℃, 2 seconds ·Single protrusion: semicircular cross section, diameter 3mm Crimping pressure: 100mm / 300N=30N / 10mm

[0048] 8 shows micrographs of Examples 1 and 2 using semicircular single protrusions (1 mm and 3 mm). For comparison, a photograph of flat surface compression bonding (flat surface adhesion) is also shown. It can be seen that the desired molded mass is formed even with the thin sealant OPP / LLDPE 20μm. The reinforcement effect of the heat seal edge is not seen in the flat pressure bonding specimen. The sealant for retort pouches is 50μm thick. When a single protrusion of 3mm was selected, the generation of a molded mass was sufficient. It was found that the desired effect could be obtained even with a protrusion of 1mm.

[0049] (Example 3): Application of "mold bonding" to retort pouches The thermal sealing of retort pouches is subject to HACCP (Hazard Analysis and Critical Control Point) regulations, and requires the most advanced measures in the operation of heat sealing techniques. The material composition is PET / AL / CPP 50μm, and the Tm is 170℃. Applying the method shown in FIG. 9, a “mold-bonded” specimen was prepared under the following conditions: For reference, a specimen was also prepared using the conventional "flat compression" method, which does not use a single protrusion. <Heating conditions> Heating: Equilibrium temperature Heating: Each temperature shown in Figure 11, 2 seconds - Single protrusion: semicircular cross section, diameter 1mm -Material specific breaking strength: 66N / 15mm

[0050] The measurement results of the tensile test patterns of the conventional "flat pressure bonding" method and the "mold bonding" method of the present invention are shown in Figure 11. Figure 12 shows the differential value calculation results of the tensile test data, and Figure 13 shows the fracture state of the surface layer material in the tensile test.

[0051] The characteristics according to the heating temperature from the graph in FIG. 11 are as follows: ◆145℃: Tensile test response of interfacial adhesion (peel seal). Adhesive strength (20~30N / 15mm) is not uniform. 150℃: The bond width is 2 mm. Although it is “mold bonding”, it breaks at a tension of 2.7 mm because it is a mixture of interfacial and cohesive bonding. 160°C to 175°C: This shows the adhesive state in the target area for "mold bonding." The response to tensile load is a combination of the elongation of the material itself and the fracture of the surface layer. The bag-breaking mechanism corresponds to (4) defined in "(Bag-breaking mechanism analysis)" above.

[0052] (Analysis of characteristics of test results) *◆The result at 145℃ is a peeling pattern for flat pressure bonding, with the entire surface being in a peeled and sealed state. *At 150℃ and 160℃ for "mold bonding," the "mold bonding" is incomplete and the bonded parts easily break due to the peeling force, and the effect of "mold bonding" is not seen. *The characteristic of flat pressure bonding at ◆160℃~◆175℃ is that a tensile test pattern similar to that of "molded bonding" is obtained, but the heat seal edge has a curved finish and pinholes are observed. *The tensile test pattern for "mold bonding" between 170°C and 175°C shows a smooth rise. Between 170°C and 175°C for "mold bonding", the breaking strength of the heat seal edge is strengthened. The sudden change in tensile strength occurs due to the breakage of the sealant, and is observed as expected. Since 175°C exceeds the Tm of 170°C, signs of high-temperature thermal denaturation are observed. The tensile test results of heated specimens of cohesive adhesive zones vary, but when a uniform load is applied to a 15 mm width, and when delamination and peeling occurs from the side edge with only slight deviation, the tensile test value becomes smaller. In this case, if no fracture occurs in the "mold adhesive" part of the delaminated sealant, it is evaluated as the desired result.

[0053] • The tensile test pattern at 170°C was differentiated with respect to the tensile length to evaluate the characteristics of the progress of the tensile test. The fracture point of the surface layer was identified by visual observation and differential values. In the test specimen, an inflection point was observed at the tensile length (initial elongation length) of [3 mm / 60 mm (initial length of specimen)], and it was determined that fracture of the surface layer occurred after this elongation. As shown in Figure 13, the response beyond a tensile length of 3 mm is the elongation characteristic of the sealant alone.

[0054] The resistance to rupture of the interfacial bond is [(adhesive strength) x (peel length)]. The resistance to rupture of a molded adhesive is [(adhesive strength) x (elongation)]. The peel length can be adjusted by the heat seal width, but the elongation length is an inherent property of the material.

[0055] A comparison was made between integral calculations of the peeling seal at ◆145°C and the “mold bonded” pattern at ●170°C. The heat seal strength (N / 15 mm) was converted to adhesive strength (N / 1 mm) and integrated using the pull length and peel length. The results are shown in Figure 12. ◆The integral value at 145℃ is the heating condition at which the material exhibits its highest fracture resistance. ●The integral value of "mold adhesion" at 170℃ exceeds the peel energy at 145℃ in all ranges. From the analysis results in Figure 11, the surface layer breaks after stretching about 3 mm. The sealant does not break, but the gas barrier properties are compromised due to the breakage of the surface layer, creating a risk. When evaluating the breakage resistance in this situation, the breakage resistance of the surface layer until it breaks is equivalent to 3.7 mm for the peeled seal, confirming the superiority of "molded adhesion."

[0056] (Example 4): Confirmation of application of "mold adhesion" to OPP / LLDPE film This specimen (material specific breaking strength: 48N / 15mm) is the most widely available general-purpose material on the market. The sealant is thin, at 20μm. A test was conducted to confirm the suitability of "mold adhesion" to this thin material. Using the method shown in Figure 9, specimens were prepared under the following conditions, and tensile tests were performed on the conventional flat compression bonding method and the "mold bonding" method. The results are shown in Figure 14. <Heating conditions> Heating: Equilibrium temperature heating, each temperature shown in Figure 14 Heating time: 1 second - Single protrusion; semicircular cross section, diameter 1mm

[0057] (Analysis of characteristics of test results) (1) The flat pressure bonding temperature of 112°C indicates the interface adhesion state. The tensile test pattern shows the peeling characteristics. (2) The flat pressure bonding temperature of 114°C is a cohesive adhesive zone. The tensile test pattern is disordered and there are many edge cuts. This situation is explained in Figure 10 and an example is shown in Figure 5. (3)● Edge chipping is prevented even with “mold bonding” at 112°C. (4) At 114°C and 116°C, a heat seal strength of 21N / 15mm can be achieved, ensuring complete "mold bonding." (5) At 118°C, the effects of overheating can be seen. (6) When the response at 114°C was differentiated, an inflection point was observed at a pulling distance of 1.7 to 2.0 mm. It can be seen that the sealant began to break after this pulling distance, leading to complete failure at a pulling of 2.5 mm. (7) It was found that even with a thin sealant material (20 μm), a highly hermetic adhesion was possible using “mold bonding,” which is superior to flat pressure bonding. [Industrial Applicability]

[0058] The expected functions of general-purpose packaging using plastic materials are as follows: (1) The adhesive strength approaches the breaking strength of the applied packaging material, so compression and impact during distribution do not cause pinholes or breakage of the heat-sealed edges. (2) Sealing assurance is established. (3) Consumers want packages that can be easily opened by picking them up without the need for tools such as scissors. The adhesion mechanism relies on the thermoplastic properties of the plastic material. Depending on the heating temperature, the adhesive surface of the plastic material changes from an interfacial adhesion where the adhesive surface remains to a cohesive adhesion in a molded state where the adhesive surface disappears. The simultaneous achievement of "sealing" without tearing of the heat seal edge and "easy opening" has been achieved in the inventions of Patent Documents 2 and 3. However, a method for controlling the adhesive strength equivalent to the breaking strength of the material based on precise logic has not been achieved. The present invention creates a molten sealant injection function at fine heat bonding operation sites, and has succeeded in applying "mold bonding" to the outer edge of the bag, which prevents the poly bag from breaking. This method can achieve a heat seal surface of about 3 mm. The SDGs set a deadline and require the reduction of the use of plastic packaging. This invention can specifically address this requirement. [Explanation of symbols]

[0059] 1-1: Heat bar (1) 1-2: Heat Bar (2) 2-1: Heater (1) 2-2: Heater (2) 3: Material 4-1: Surface material (1) 4-2: Surface material (2) 5: Sealant 6: Mold lump 7: Side edge 8: Semicircular protrusion 9: Trapezoidal protrusion 10: Heat bar body (1) 11: Heat bar body (2) 12-1: Surface material (1) 12-2: Surface material (2) 13: Sealant 14: Clamping pressure 15: Mold block 16: Bag body 17: Outer edge side part 18: Pressure vessels 19: Spacer (1) 20: Spacer (2) 21: Heat seal surface 22: Heat seal surface 23: Heat seal edge 24: Heat seal edge 25: Poly ball 26: Pinhole occurrence point 27: Load line

Claims

1. A method for heat-sealing a plastic bag, comprising: sandwiching a heat-sealing material between a pair of heaters and heat-sealing the material; One of the pair of heating bodies has a fine linear protrusion having a semicircular or trapezoidal cross-sectional shape, The method for thermally sealing the plastic bag includes pressing the heated linear protrusion against the sealant of the heat seal material, thereby injecting the sealant molten at a temperature range for cohesive adhesion in a band shape along the side end of the linear protrusion to form a molded adhesive band.

2. The heat seal material is a composite material including a surface material and a sealant, In the injection, the surface material of the composite material is used as a pressure vessel. The method for thermally bonding plastic bags according to claim 1.

3. The diameter of the semicircle is 0.5 to 3 mm; The lower base of the trapezoid is 0.5 to 3 mm.

3. The method for thermally bonding plastic bags according to claim 1 or 2.

4. 3. The method for thermally sealing plastic bags according to claim 1 or 2, further comprising adjusting an injection amount of the molten sealant by changing a dimension of the semicircle or trapezoid.

5. A method for thermally sealing plastic bags as described in claim 1 or 2, wherein the contact surface of the other of the pair of heating elements with the heat sealing material is made of resin.

6. A method for producing a plastic bag, comprising producing a plastic bag having the molded adhesive band formed thereon by using the method for thermally bonding a plastic bag according to claim 1 or 2.

7. A method for manufacturing a plastic bag, comprising manufacturing a plastic bag having the molded adhesive band formed thereon using the thermal bonding method for plastic bags described in claim 3 or 4.

8. A method for manufacturing a plastic bag, comprising manufacturing a plastic bag having the molded adhesive band formed thereon using the thermal bonding method for plastic bags described in claim 5.

Citation Information

Patent Citations

  • Method for controlling temperature of heat sealing device

    JP2007313782A

  • Composite heat-sealing structure capable of adapting to lapped part step

    JP2016043988A

  • Method for selection of sealant layer on base material

    JP2017114018A

  • Heat sealer provided with boundary surface temperature sensor

    JP2021014039A

  • Heat sealing device forming composite heat sealing structure to which linear peelable seal is added in longitudinal direction of strip-shaped peelable seal

    JP2024040544A