Setting and hardening accelerator for cement, mortar or concrete compositions, optionally including additional cementitious materials, and use of said accelerator

An aqueous nitrate solution with alkaline hydroxide enhances the setting and hardening of cement, mortar, and concrete compositions, addressing corrosion issues and improving cold-weather performance.

JP7590182B2Active Publication Date: 2024-11-26YARA INTERNATIONAL ASA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020546146
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-05
Filing Date
2019-03-05
Publication Date
2024-11-26
Estimated Expiration
2039-03-05

AI Technical Summary

Technical Problem

Existing accelerators for cement, mortar, and concrete compositions, such as calcium chloride and calcium nitrate, face issues like corrosion of metals and insufficient acceleration in cold climates, necessitating a more effective solution.

Method used

A setting accelerator comprising an aqueous nitrate solution with dissolved alkaline hydroxide solids, maintaining a pH of at least 9.0, optionally with a hydroxide precipitate, to enhance the crystallization reaction and accelerate setting and hardening, particularly in cold conditions.

Benefits of technology

The accelerator effectively speeds up the setting and hardening process of cement, mortar, and concrete compositions, including those with cementitious supplementary materials, even at low temperatures, without causing metal corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590182000003
    Figure 0007590182000003
  • Figure 0007590182000004
    Figure 0007590182000004
  • Figure 0007590182000005
    Figure 0007590182000005
Patent Text Reader

Abstract

The present application relates to a setting and hardening accelerator for cement, mortar, or concrete compositions optionally containing a cement substitute material (CSM). The accelerator composition comprises an aqueous nitrate solution and an alkali hydroxide. In particular, the aqueous accelerator composition comprises 30 to 55 wt. % nitrate as a nitrate solution and 0.02 to 0.1 wt. % alkali hydroxide, the alkali hydroxide dissolved in the nitrate solution and optionally present in the accelerator composition as a hydroxide precipitate, and the accelerator composition has a pH of at least 9.0. When the cement, mortar, or concrete composition contains a CSM, the accelerator composition has a pH of at least 12.0. The present application further relates to the use of the accelerator composition according to the present application and to a method for accelerating a cement, mortar, or concrete composition, particularly at low temperatures, by reacting the composition with the accelerator according to the present application. [Selection diagram] None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application relates to accelerating the setting and hardening of cement, mortar and concrete compositions, which optionally contain one or more supplemental cementitious materials (CSMs). [Background technology]

[0002] The hydration of cement is slow, so there is a need to accelerate the setting and hardening process to speed up the construction process, especially the work process of applying fresh concrete, which is of economic interest. In addition to accelerating the setting and hardening process in cold climates, accelerating the setting and hardening process is essential to counteract the cooling of concrete caused by the environment.

[0003] Calcium chloride (CaCl2) is a possible accelerator for the setting of concrete, but it stimulates the conjunctive oxidation of ferrous structural conduits or reinforcing steel or aluminum conduits embedded in concrete. In addition, CaCl2 has a detrimental effect on the concrete itself, resulting in spalling and weakening. When concrete is in contact with moist soil, the attack of sulfates in the soil is enhanced by CaCl2. As a result, there is an upper limit to the amount of CaCl2 that can be added to cement, mortar, and concrete compositions, even when the concrete does not contain metals or when corrosion of metals in concrete is not a significant problem. Although CaCl2 is low cost, problems associated with its use limit its desirability in reinforced concrete structures.

[0004] Neutral or acidic calcium nitrate (Ca(NO3)2) is a common set accelerator for concrete. It is usually added in the form of a solution after mixing the concrete blend with water. Usually, 1% to 2% calcium nitrate should be added based on the weight of cement (= bwoc). Calcium nitrate does not cause corrosion when applied up to the levels approved in the European or ASTM mix standards of 4% and 5% by weight, respectively. However, the acceleration effect is based on the ability of calcium nitrate to generate calcium hydroxide to raise the pH value, and the pH value of calcium nitrate is only 5-8. As a result, the acceleration effect in cold climates is not sufficient and to achieve faster acceleration, CaCl2 is commonly added, which exhibits the corrosion problems described in the previous paragraph.

[0005] US Patent No. 4,897,120 describes an accelerator for Portland cement derived from fertilizers. More specifically, it relates to a method for chemically modifying the composition of calcium nitrate, including ammonium nitrate, which has traditionally been used as a fertilizer or additive thereto, to allow its use as an additive in Portland cement concrete and mortar. In this method, the calcium ammonium nitrate composition is reacted with a tri- or tetramethylol glycoluril compound under alkaline conditions, with a pH of about 7.5 or higher, preferably in the range of about pH 9 to 11. It has been found that the presence of hexamine (urotropine) not only has a positive effect on the conversion of the calcium ammonium nitrate hydrate composition for use as a Portland cement accelerator, but also on its performance in terms of setting more quickly and achieving higher compressive strength performance. The resulting set accelerator is suitable for use in cold climates.

[0006] Another way to improve the setting acceleration of calcium nitrate is to use polyethanolamine accelerators in combination with calcium nitrate. WO1982004038 relates to an additive composition that accelerates the setting time and also improves the compressive strength of Portland type cements, mortars and concretes, especially concretes containing metal reinforcement. This additive composition essentially consists of a concentrated aqueous solution of calcium nitrate and a waste by-product stream of a mixture of polyethanolamine to which a small amount of a solution of an alkali metal or alkaline earth metal salt of a polyhydroxy aliphatic compound such as gluconic acid or lignosulfonic acid is added. WO1984004089 relates to a setting accelerator comprising calcium nitrate and triethanolamine. However, in practice, these amine accelerators are hazardous substances that are difficult to use with respect to the environment and its users.

[0007] It is concluded that there remains a need to improve the setting and hardening of cement, mortar or concrete compositions, especially under low temperature conditions. Accordingly, it is an object of the present application to provide an accelerator for improving the setting and hardening of cement, mortar or concrete compositions, including at low temperatures.

[0008] A further object of this application is to improve the setting and hardening of cement, mortar or concrete compositions containing the CSM (cement additive). Summary of the Invention

[0009] According to one aspect of the present application, a setting and hardening accelerator for a cement, mortar or concrete composition is disclosed. The accelerator includes a supernatant containing an aqueous nitrate solution. The supernatant further includes dissolved alkaline hydroxide supernatant solids. The supernatant has a pH of at least 9.0. The accelerator may also optionally include hydroxide precipitate. An advantage of such an alkaline supernatant is that it provides a high pH value required for the crystallization reaction of the cementitious material. The alkaline supernatant has been found to accelerate the setting and hardening of cement, mortar or concrete compositions and is of economic interest. Acceleration is particularly interesting for applications in cold climates where the setting and hardening of cement is slow.

[0010] In particular, the setting and hardening accelerator for a cement, mortar or concrete composition of the present application is an aqueous composition comprising 30-55 w / w %, more particularly 30-50 w / w %, of a nitrate as a nitrate solution, and 0.02-0.1 w / w % of an alkali hydroxide dissolved in the nitrate solution and optionally included as a hydroxide precipitate in the accelerator composition, the accelerator composition having a pH of at least 9.0.

[0011] In a possible accelerator according to the present application, the alkaline hydroxide is selected from calcium hydroxide, sodium hydroxide or potassium hydroxide.

[0012] In a possible accelerator according to the present application, the aqueous nitrate solution is selected from an aqueous calcium nitrate solution, an aqueous sodium nitrate solution, or an aqueous potassium nitrate solution. Thus, in a possible accelerator composition according to the present application, the nitrate is selected from an aqueous calcium nitrate solution, an aqueous sodium nitrate solution, or an aqueous potassium nitrate solution.

[0013] In one possible enhancer composition according to the present application, the aqueous composition has a pH of 9.0 to 14.0. In another possible enhancer composition according to the present application, the aqueous composition has a pH of 12.0 to 14.0.

[0014] In a possible promoter according to the present application, the supernatant contains an aqueous nitric acid solution obtained by dissolving 30-55 w / w %, more particularly 30-50 w / w %, of calcium nitrate (solid), sodium nitrate (solid) or potassium nitrate (solid) in water, to which 0.02-0.1 w / w % of solid calcium hydroxide, solid sodium hydroxide or solid potassium hydroxide is added.

[0015] In a possible accelerator according to the present application, the supernatant contains an aqueous calcium nitrate solution obtained by dissolving 44-55 w / w % of calcium nitrate salt in water, to which is added 0.02-0.1 w / w % of solid calcium hydroxide, which causes the formation of a calcium hydroxide precipitate. Thus, a possible accelerator composition according to the present application contains 44-55 w / w % calcium nitrate and 0.02-0.1 w / w % calcium hydroxide as a nitrate solution.

[0016] In a possible accelerator according to the present application, the supernatant contains an aqueous calcium nitrate solution obtained by dissolving about 49.98 w / w % calcium nitrate salt in water and adding about 0.04 w / w % solid calcium hydroxide to the prepared aqueous calcium nitrate solution, which causes the formation of a calcium hydroxide precipitate. Thus, a possible accelerator composition according to the present application contains about 49.98 w / w % calcium nitrate salt and about 0.04 w / w % calcium hydroxide in water.

[0017] When the cement, mortar or concrete composition contains one or more CSMs, optionally including fly ash or limestone, the pH of the accelerator composition or the supernatant of the accelerator composition is at least 12.0. The advantage of such a pH value is that it provides the high pH value necessary for the crystallization reaction of the composition of the CSMs as well as the cement, mortar or concrete in the composition. It has been found that such pH values ​​accelerate the setting and hardening of the cement, mortar or concrete composition containing one or more CSMs.

[0018] A further aspect of the present application provides a cement, mortar or concrete composition comprising an accelerator composition according to the present application. In certain embodiments, a cement, mortar or concrete composition is provided comprising one or more cement-substitute materials, optionally including fly ash or limestone, and an accelerator composition as described above having a pH of at least 12.0.

[0019] According to a further aspect of the present application, there is disclosed the use of an accelerator composition comprising an aqueous nitrate solution and dissolved alkaline hydroxide solids, having a pH of at least 9, and optionally including a hydroxide precipitate, for accelerating the setting and hardening of a cement, mortar or concrete composition.

[0020] More specifically, the supernatant which forms part of the enhancer according to the present application as described above is used.

[0021] According to a further aspect of the present application, there is disclosed the use of an accelerator composition according to the present application, having a pH of at least 12.0, optionally containing a hydroxide precipitate, and comprising one or more CSMs for accelerating the setting and hardening of a cement, mortar or concrete composition.

[0022] More specifically, the supernatant which forms part of the enhancer according to the present application as described above is used.

[0023] According to a further aspect of the present application, there is disclosed a method for accelerating the setting and hardening of a cement, mortar or concrete composition, optionally including one or more CSMs, comprising the steps of preparing an accelerator according to the present application as described above and adding the accelerator to a cementitious material or one or more CSMs or coarse aggregate or any combination thereof at a temperature between 5°C and 20°C.

[0024] In a possible method according to the present application, the addition of the cement material or one or more CSMs or coarse aggregates or any combination thereof is carried out at a temperature of about 5°C.

[0025] According to a further aspect of the present application, there is disclosed a method for producing the accelerator composition described herein, comprising the steps of dissolving 30-55 w / w %, more particularly 30-50 w / w %, of a nitrate, more particularly calcium nitrate, sodium nitrate or potassium nitrate, in water, thereby obtaining an aqueous nitrate solution, and adding 0.02-0.1 w / w % of an alkaline hydroxide, more particularly solid calcium hydroxide, solid sodium hydroxide or solid potassium hydroxide, to the aqueous nitrate solution, thereby obtaining an accelerator composition having a pH of at least 9.0. [Brief description of the drawings]

[0026] [Figure 1] In FIG. 1, hydration curves of samples of cement paste containing none, one or both of sodium nitrate and sodium hydroxide are shown. [Diagram 2] In Figure 2, the hydration curves of cement paste samples containing calcium nitrate, a combination of calcium nitrate and sodium hydroxide, or a combination of calcium nitrate and calcium hydroxide are shown: a) ambient; b) 0% CN; c) 1% CN55; d) 1% CN55 + Ca(OH)2; e) 1% CN55 + NaOH. [Figure 3a] In Figure 3a, the effect of calcium nitrate and alkaline calcium nitrate on the setting time of various cements and CSM at 5°C is shown. [Figure 3b] Figure 3b shows the effect of calcium nitrate and alkaline calcium nitrate on the setting time of various cements and CSMs at 20 °C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Detailed Description As defined herein, the singular forms "a," "an," and "the" include both the singular and the plural unless the context clearly indicates otherwise. As used below, the terms "comprise," "comprises," and "comprises" are synonymous with "including," "include," or "contain," and are inclusive or open and do not exclude additional parts, elements, or method steps not mentioned. When this description refers to a product or process that "comprises" a particular feature, part, or step, this refers to the possibility that other features, parts, or steps may also be present, but may also refer to an embodiment that includes only the recited feature, part, or step. All references cited in this description are deemed to be incorporated herein by reference in their entirety.

[0028] As used herein, w / w % means weight percent. When used in the context of an accelerator composition, it means weight percent relative to the total weight of the accelerator composition. Thus, the phrase "dissolve X % w / w of nitrate in water" means dissolving X weight percent of nitrate (solids) relative to the total weight of the accelerator in water. It is also that percentage of nitrate that is ultimately present in the accelerator composition. Similarly, the phrase "add X w / w % hydroxide solids to a made nitrate solution" means that X weight percent of hydroxide solids, based on the total weight of the accelerator, is added to a made nitrate solution, dissolves therein, and is ultimately present in the accelerator.

[0029] The present application relates to a setting and hardening accelerator for cement, mortar or concrete compositions.

[0030] Cement is used as a binding material that hardens to form a bond between solids. Cements used in construction are either hydraulic (harden in water) or nonhydraulic. Hydraulic cements (e.g. Portland cement) harden by hydration, a chemical reaction between anhydrous cement powder and water. As a result, they can harden in water or when exposed to continued rain. The chemical reaction results in a hydrate that is less water soluble and more durable in water. Nonhydraulic cements do not harden in water. Hydrated lime, for example, hardens by reaction with carbon dioxide in the air.

[0031] Portland cement is by far the most common type commonly used around the world. It is made by heating limestone (calcium carbonate) with small amounts of other materials (such as clay) in a kiln to a temperature of 1450 °C, a process called calcination. During the calcination process, the calcium carbonate releases carbon dioxide molecules to form calcium oxide, also known as quicklime, which is then blended with the other materials in the mixture. The resulting hard substance, called "clinker," is ground into a powder along with a small amount of gypsum to create "ordinary Portland cement" (often called OPC), the most commonly used type of cement.

[0032] There are different types of cement, designated CEM I to CEM V, with low or high content of blast furnace cement, such as Portland cement, or cement substitutes, also called cement-based supplementary materials (CSM), such as limestone or fly ash, i.e. CEM I: OPCs containing up to 5% other compounds; CEM II: All kinds of mixtures of OPC with e.g. fly ash, limestone or slate, OPC min. 65%, CEM III: Three classes of high blast-furnace / Portland cement mixtures: A, B and C. CEM III / A contains the lowest amount of blast furnace slag (40%), CEM III / C contains the highest amount (60%). CEM IV: A type of pozzolanic cement. · CEM V: Composite cement made from OPC, blast furnace slag and pozzolanic compounds It is.

[0033] The term "cement-substitute material" is used herein interchangeably with the term "cement-based supplemental material", abbreviated as CSM, and generally refers to a cement-based material rich in calcium and / or silicate. In particular, the CSM is selected from the group consisting of fly ash, limestone, or blast furnace slag. More specifically, CSM as contemplated herein does not include alumina or aluminate materials such as fused or tabular alumina, zircon, alumina silicate, etc.

[0034] Dry mortar mixes are usually made from a mixture of aggregates such as sand, binders such as cement or lime, and water. Generally, dry mortar mixes consist of about 25 w / w % cement and about 75 w / w % sand. Just before use, the dry mortar mix is ​​mixed with water to make a workable mortar paste. It is useful as a general construction material to bind building blocks and fill gaps between them. The mortar paste hardens as it sets, resulting in a stronger aggregate structure. Mortar can also be used to secure masonry or apply joints once the original mortar has been washed away. Dry mortar blends are stored dry in bags.

[0035] Concrete is a composite building material composed primarily of aggregates, cement, and water. There are many formulations that offer different properties. The aggregates are usually coarse gravel or crushed stone, such as limestone or granite, along with fine aggregates, such as sand. Cement, commonly Portland cement, and other cementitious materials, such as fly ash or slag cement, act as binders for the aggregates. Various chemical admixtures are also added to achieve different properties. Water is mixed with the dry concrete mix, which is then shaped (usually poured or cast), and then it sets and hardens into rock-strength concrete through a chemical process called hydration. The water reacts with the cement, which binds the other ingredients together, ultimately creating a sturdy stone-like material. Concrete is widely used to make building structures, foundations, brick / block walls, pavements, bridges / overpasses, highways / roads, runways, parking lots, dams, pools / reservoirs, pipes, gates, fences and columns, and even boat foundations.

[0036] Concrete can be damaged by many processes, including the freezing of water trapped in the pores of the concrete. It is difficult to cast and cure concrete in cold weather, especially at or below sustained freezing temperatures. The most common problem is that the concrete undergoes freezing and / or freeze / thaw cycles before it can gain adequate strength during curing. In the cold weather conditions described above, water begins to freeze within the capillaries of the concrete at -2°C, and upon freezing, it can expand by up to 9% of its volume, causing cracks in the concrete matrix, and a loss of compressive strength of up to 50% can occur if the concrete freezes before it reaches a compressive strength of at least 500 psi.

[0037] The present setting and hardening accelerator for cement, mortar or concrete compositions detailed above includes a supernatant or solution that initially contains a nitrate solution and further contains dissolved alkaline hydroxide solids. Depending on the composition of the aqueous nitrate solution and the nature of the solid alkaline hydroxide dissolved in the supernatant, the accelerator may further contain hydroxide precipitate. In particular, the solubility of calcium hydroxide in water is only 1.89 g / L at 0°C and 1.73 g / L at 20°C. Thus, if the amount of calcium hydroxide added or made in the following procedure exceeds the solubility of calcium hydroxide at the temperature of the supernatant, precipitation will occur. 1. Add calcium hydroxide to the nitrate solution, or 2. Calcium hydroxide is made by the addition of a solid alkaline hydroxide (e.g., solid sodium hydroxide or solid potassium hydroxide) to an aqueous solution of calcium nitrate. Therefore, the setting and hardening accelerator according to the present application generally includes an aqueous nitrate solution and an alkaline hydroxide.

[0038] Depending on whether the cement, mortar or concrete composition contains one or more CSMs or not, the accelerator composition, or the supernatant thereof, in particular, has a typical pH. In the absence of a CSM, the accelerator composition or the supernatant has a pH of at least 9.0, whereas in the presence of a CSM, the accelerator composition or the supernatant typically has a pH of at least 12.0. As used herein, "pH" is the conventional unit of hydrogen ion activity in an aqueous solution measured at 25°C and 1 atmosphere [i.e., ISO standard conditions]. A pH of at least 9.0 includes any measured pH value rounded to 9.1 or higher. A pH of at least 12.0 includes any measured pH value rounded to 12.1 or higher. A pH between 9.0 and 14.0 includes any measured pH value between a pH value rounded to 9.1 or higher and a pH value rounded to 14.1 or lower.

[0039] More specifically, the aqueous nitrate solution contained in the accelerator is selected from an aqueous calcium nitrate solution, an aqueous sodium nitrate solution or an aqueous potassium nitrate solution. In particular, an aqueous calcium nitrate solution is used. This is because calcium nitrate already has a pH value of 5 to 8 and therefore already accelerates the setting and hardening of the cement, mortar or concrete composition. However, this pH is still not high enough and, if no CSM is present, it usually has to be 9 or higher. This pH value is obtained by adding a solid alkaline hydroxide which dissolves in the aqueous nitrate solution. The solid alkaline hydroxide is in particular selected from solid calcium hydroxide, solid sodium hydroxide or solid potassium hydroxide. In the absence of CSM, in particular the pH of the supernatant is 9.0 to 14.0, whereas in the presence of CSM the pH of the supernatant is 12.0 to 14.0.

[0040] The accelerator composition is prepared by dissolving 30-55 w / w %, particularly 30-50 w / w %, of solid calcium nitrate (salt), solid sodium nitrate (salt) or solid potassium nitrate (salt) in water to an aqueous solution of calcium nitrate, sodium nitrate or potassium nitrate, and then adding 0.02-0.1 w / w % of solid calcium hydroxide, solid sodium hydroxide or solid potassium hydroxide to the aqueous solution of calcium nitrate, sodium nitrate or potassium nitrate to prepare the accelerator composition according to the present invention. The accelerator composition is in the form of a solution / supernatant or in the form of a solution / supernatant and precipitate, depending on whether the solubility of calcium hydroxide is exceeded. In particular, the accelerator composition is prepared by first dissolving 44-55 w / w % of solid calcium nitrate in water to obtain an aqueous calcium nitrate solution, and then adding 0.02-0.1 w / w % of solid calcium hydroxide to the aqueous calcium nitrate solution obtained. Very specifically, the accelerator composition is prepared by dissolving about 49.98 w / w % solid calcium nitrate in water to produce an aqueous calcium nitrate solution, and then dissolving about 0.04 w / w % solid calcium hydroxide in the resulting aqueous calcium nitrate solution.

[0041] Thus, the present application provides an aqueous accelerator composition comprising 30-55 w / w %, more particularly 30-50 w / w % of a nitrate, even more particularly calcium nitrate, sodium nitrate or potassium nitrate, and 0.02-0.1 w / w % of an alkaline hydroxide, especially an alkali metal or alkaline earth metal hydroxide, more particularly calcium hydroxide, sodium hydroxide or potassium hydroxide, in water. In particular, the aqueous accelerator composition comprises 44-55 w / w % calcium nitrate and 0.02-0.1 w / w % calcium hydroxide in water. Even more particularly, the aqueous accelerator composition comprises about 49.98 w / w % calcium nitrate in water and about 0.04 w / w % calcium hydroxide.

[0042] In a particular embodiment, the present application provides an aqueous accelerator composition comprising: (i) 30-55 w / w %, more particularly 30-50 w / w %, of a nitrate, more particularly calcium nitrate, sodium nitrate or potassium nitrate; (ii) 0.02-0.1 w / w % of an alkali hydroxide, particularly an alkali metal or alkaline earth metal hydroxide, more particularly calcium hydroxide, sodium hydroxide or potassium hydroxide; and (iii) water. In particular, the aqueous accelerator composition comprises 44-55 w / w % of calcium nitrate, 0.02-0.1 w / w % of calcium hydroxide, and water. More particularly, the aqueous accelerator composition comprises about 49.98 w / w % of calcium nitrate, about 0.04 w / w % of calcium hydroxide, and water.

[0043] The present application further discloses the use of an accelerator as described above according to the present application for accelerating the setting and hardening of a cement, mortar or concrete composition. In particular, an accelerator as envisaged herein is used, comprising a supernatant or solution comprising an aqueous nitrate solution and dissolved alkaline hydroxide solids, optionally including hydroxide precipitate. In the absence of CSM in the cement, mortar or concrete composition, the accelerator composition has a pH of at least 9.0, whereas in the presence of CSM, the supernatant has a pH of at least 12.0. In the absence of CSM, the pH of the supernatant is in particular between 9.0 and 14.0, whereas in the presence of CSM, the pH of the supernatant is between 12.0 and 14.0.

[0044] The present application further discloses a method for accelerating the setting and hardening of a cement, mortar or concrete composition, optionally comprising one or more CSMs, comprising the steps of preparing an accelerator according to the present application and adding the accelerator to a cementitious material, optionally comprising one or more CSMs, at a temperature between 5° C. and 20° C. In particular, the addition of the cementitious material or the one or more CSMs or coarse aggregates or any combination thereof is carried out at a temperature of about 5° C.

[0045] The present application further discloses a method for producing the accelerator composition according to the present application, the method comprising the steps of: (a) dissolving a nitrate, in particular 30-55 w / w %, more particularly 30-50 w / w %, of a nitrate, more particularly solid calcium nitrate, solid sodium nitrate, or solid potassium nitrate, in water, thereby obtaining an aqueous nitrate solution; and (b) adding 0.02-0.1 w / w % of an alkaline hydroxide, more particularly solid calcium hydroxide, solid sodium hydroxide, or solid potassium hydroxide, to the aqueous nitrate solution, thereby obtaining an accelerator composition having a pH of at least 9.0; Includes. EXAMPLES

[0046] comparison Example 1 Table 1 shows the composition of three different cement paste samples A, B, and C. CEM II / AV 42.5 is a Portland composite cement containing 80-94 w / w % Portland cement clinker, 6-20 w / w % ground slag and limestone, and 0-5 w / w % gypsum and mineral fertilizers. As defined herein, w / c represents the weight / weight ratio of water / cement. To prepare the cement paste samples, cement was mixed with water in a given ratio, after which the indicated weights of admixtures consisting of solid sodium nitrate (NaNO3) and solid sodium hydroxide (NaOH) were added to this mixture. The resulting paste was then mixed in a kitchen mixer for 60 seconds, scraped off the walls of the bowl with a spatula, and mixed for an additional 30 seconds. This was done to ensure uniform distribution of water, cement, and admixtures. The resulting paste was filled into a 500 ml cube-shaped plastic bottle. The samples were then left to stand at 20°C. The hydration activity was measured by recording the temperature using a PT-100 sensor embedded in the cement paste samples. [Table 1]

[0047] Figure 1 shows the hydration reactivity as expressed by the hydration temperature. From Figure 1, it can be concluded that in the presence of sodium nitrate or a combination of sodium nitrate and sodium hydroxide, the first reaction peak is slightly stronger. Figure 1 also shows that the setting time of both samples containing sodium nitrate is accelerated by about 1 hour and the hardening activity increases after 9-12 hours of reaction in both samples containing sodium nitrate. The fastest reaction in Figure 1 is observed for the sample containing both sodium nitrate and sodium hydroxide, 3 hours earlier than the sample containing sodium nitrate after 12 hours and 6 hours earlier than the sample containing neither sodium nitrate nor sodium hydroxide. Finally, the maximum temperature is significantly (about 1°C) lower for the sample containing both sodium nitrate and sodium hydroxide than the sample containing sodium nitrate and at the same level as the sample containing neither sodium nitrate nor sodium hydroxide. Thus, the alkaline sodium nitrate sample acts as a moderate setting hardening accelerator for fly ash cement.

[0048] Example 2 Table 2 shows the composition of the 4,500 ml cement paste samples 1-4 used in the hydration tests. The cement used in all experiments was CEM II / AV 42.5, a Portland composite cement containing 80-94 w / w % Portland cement clinker, 6-20 w / w % ground slag and limestone, and 0-5 w / w % gypsum and mineral fertilizers. As defined herein, w / c represents the weight / weight ratio of water / cement. To prepare the cement paste samples, the cement was mixed with water in the given ratio, and then the indicated weight of calcium nitrate aqueous solution was added to the mixture. To make samples 3 and 4, solid sodium hydroxide and solid calcium hydroxide were each added to a 55 wt % calcium nitrate aqueous solution to achieve a pH of 10.4 and then added to the cement mixed with water. The calcium nitrate solution was added to the cement-water mixture to obtain a paste, which in all cases was then mixed in a kitchen mixer for 60 seconds, scraped off the walls of the bowl with a spatula, and mixed for another 30 seconds. This was done to ensure a uniform distribution of water, cement, and admixtures. The paste was filled into 500 ml cube-shaped plastic bottles. The samples were then left to stand at 20°C. The hydration activity was measured by recording the temperature using a PT-100 sensor embedded in the cement paste samples. [Table 2]

[0049] The hydration reactivity expressed by the hydration temperature is shown in Figure 2. From Figure 2, it can be concluded that there is a higher activity when using calcium nitrate with added calcium hydroxide (pH 10.4) compared to using calcium nitrate alone or calcium nitrate with added sodium hydroxide.

[0050] Example 3 A 50 w / w % calcium nitrate solution at pH 10.4 was prepared by adding solid alkaline hydroxide to a 50 w / w % calcium nitrate solution to bring the resulting solution to pH 10.4. Water, calcium nitrate solution (50 w / w %), or a 50 w / w % calcium nitrate solution at pH 10.4 was added at 2 w / w % to three types of cement mixed with sand, with a sand / cement w / w ratio of 1 / 3: I: Portland (OPC) II -AM: Portland / Pozzolana / Limestone II -A-LL: Portland / Limestone Generate. Standard sand and cement were mixed in a mortar mixer according to EN 196 / 1. Setting times were recorded according to EN 480 / 2.

[0051] The effect of alkaline calcium nitrate in shortening the setting time by an immediately sufficiently high pH value is well shown in the results of CEM I in both Figures 3a and 3b. The effect of alkaline CN in shortening the setting time of the cement substitute materials by high pH value is shown in the results of CEM II in both Figures 3a and 3b. This further implies that the cement substitute materials of pozzolan and limestone are activated by the initial high pH value resulting from the faster setting of Portland cement.

[0052] From the various examples, it can be concluded that when cement is mixed with the alkaline accelerator according to the present application, the setting time is found to be accelerated with respect to when the cement is mixed with a solution containing only dissolved calcium nitrate. Moreover, such an improvement is observed both at low temperatures (Figure 3a) and at 20°C (Figure 3b). Moreover, this acceleration of setting time was not only observed for OPC (CEM I), but also for cement mixtures containing OPC and limestone ("II-A-LL" in Figures 3a and 3b) and OPC, limestone and pozzolan ("II-AM" in Figures 3a and 3b). This shows that the alkaline nitrate solution can accelerate not only the setting time of the cement, but also that of the cement substitute material. The increase in the cement mixtures containing OPC and CSM may indirectly contribute to the acceleration of the setting of the cement substitute material, since the faster hydration of OPC leads to an increase in the pH value, which results in a faster hydration of the cement substitute material.

[0053] Furthermore, it was further observed that alkaline nitrate solutions resulted in faster hydration of the cement (Figure 1) and the use of calcium hydroxide as the alkaline source resulted in faster hydration of the cement compared to the use of sodium hydroxide as the alkaline source (Figure 2).

Claims

1. An aqueous setting and hardening accelerator composition for a cement, mortar or concrete composition, the accelerator composition having a pH of at least 9.0, the aqueous solution being an aqueous solution of 30-55 w / w % calcium nitrate, calcium hydroxide and water, wherein the calcium hydroxide is dissolved in the aqueous solution in an amount sufficient to bring the pH of the aqueous solution to at least 9.

0.

2. The accelerator composition of claim 1, wherein the accelerator composition has a pH of 9.0 to 14.

0.

3. The accelerator composition of claim 1, which is an aqueous solution of 44-55 w / w % calcium nitrate, calcium hydroxide, and water, more specifically, about 49.98 w / w % calcium nitrate, calcium hydroxide, and water, the calcium hydroxide being present in an amount sufficient to provide a pH of the aqueous solution of at least 9.

0.

4. A cement, mortar or concrete composition comprising the accelerator composition according to any one of claims 1 to 3.

5. 5. The cement, mortar or concrete composition of claim 4, comprising one or more cement-substitute materials and the accelerator composition of any one of claims 1 to 3 having a pH of at least 12.0, the cement-substitute materials optionally comprising fly ash or limestone.

6. Use of the accelerator composition according to any one of claims 1 to 3 for accelerating the setting and hardening of a cement, mortar or concrete composition.

7. 7. The use according to claim 6, wherein the cement, mortar or concrete composition comprises one or more cement-substitute materials, the accelerator composition having a pH of at least 12.0, the cement-substitute materials optionally comprising fly ash, blast furnace slag or limestone.

8. - a step of producing an accelerator composition according to any one of claims 1 to 3, and - adding the accelerator composition to a cementitious material, one or more cement substitute materials, coarse aggregate or any combination thereof at a temperature between 5°C and 20°C.

1. A method for accelerating the setting and hardening of a cement, mortar or concrete composition, optionally containing one or more cement-substitute materials, comprising:

9. 9. The method of claim 8, wherein the addition to the cementitious material, one or more cement substitute materials, coarse aggregate, or any combination thereof, is performed at a temperature of about 5°C.

10. (a) dissolving 30-55 w / w % solid calcium nitrate in water, thereby obtaining an aqueous calcium nitrate solution; (b) adding a sufficient amount of solid calcium hydroxide to the aqueous calcium nitrate solution to bring the pH of the aqueous calcium nitrate solution to at least 9.0, thereby obtaining an accelerator composition having a pH of at least 9.

0. A method for producing the accelerator composition according to any one of claims 1 to 3, comprising:

Citation Information

Patent Citations

  • Chloride-free hardening accelerator for Portland cement and process for its production

    DE3543874A1

  • Setting agent accelerator for refractory material

    US20120252653A1

  • High early strength agent for cements, high early strength cement using same, and method for producing high early strength concrete

    WO2017221749A1