Aluminum alloy clad material

The aluminum alloy clad material with a nobler core material potential and controlled impurities addresses corrosion issues at high temperatures, ensuring effective corrosion resistance up to 100°C or higher.

JP7590302B2Active Publication Date: 2024-11-26KOBE STEEL LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021167043
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-11
Publication Date
2024-11-26
Estimated Expiration
2041-10-11

AI Technical Summary

Technical Problem

Conventional aluminum alloy clad materials and brazing sheets exhibit poor corrosion resistance at temperatures above 90°C, necessitating improved materials for higher temperature applications.

Method used

An aluminum alloy clad material with a core material and sacrificial anode layer, where the core material's pitting potential is nobler than the anode layer by at least 50 mV, composed of specific alloy compositions, and a pitting potential difference is maintained through controlled impurity levels and thickness ratios.

Benefits of technology

The material provides excellent corrosion resistance at temperatures up to 100°C or higher, preventing penetrating corrosion and maintaining long-term protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590302000001
    Figure 0007590302000001
  • Figure 0007590302000002
    Figure 0007590302000002
Patent Text Reader

Abstract

To provide an aluminum alloy clad material that has excellent corrosion resistance even in the case of being used in a heat exchanger with use conditions of 100°C or higher.SOLUTION: An aluminum alloy clad material comprises: a core having a pair of opposing principal surfaces; and a sacrificial anode layer provided on at least one of the principal surfaces of the core, where regarding pitting potential obtained from anode polarization measurement of the following conditions, the pitting potential of the core is nobler than the pitting potential of the sacrificial anode layer, and its potential difference is 50 mV or more. (Conditions) working electrode: the core or the sacrificial anode layer, counter electrode: Pt, reference electrode: Ag / AgCl / saturation KCl, electrolytic solution: aqueous solution containing Cl- by 300 ppm and SO42- by 100 ppm, temperature: 95°C, atmosphere: high purity nitrogen gas, and sweeping rate: 1 mV / sec.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum alloy clad material, and more particularly to an aluminum alloy clad material suitable for an aluminum alloy brazing sheet. [Background technology]

[0002] Automotive heat exchangers are usually manufactured by forming, assembling, and brazing aluminum alloy sheets, which are lightweight and have excellent thermal conductivity. To obtain high strength, good brazing properties, and high corrosion resistance, aluminum alloy brazing sheets are used, which have a brazing material formed on one main surface of a core material and a sacrificial anode layer formed on the other main surface.

[0003] Many studies have been conducted on aluminum alloy clad materials and aluminum alloy brazing sheets, which have a core material and a sacrificial anode layer formed on one of the main surfaces of the core material.

[0004] For example, Patent Document 1 discloses an aluminum alloy three-layer clad material in which a sacrificial anode material, which is an aluminum alloy containing specific amounts of Mn, Cu, Si, and Ti, is clad on one side of a core material, which is an aluminum alloy containing specific amounts of Zn, Si, and Ni, and a brazing material, which is an aluminum alloy containing specific amounts of Si and Sr, is clad on the other side. In the sacrificial anode material, Zn is said to have a lower potential, exert a sacrificial anode effect on the core material, and prevent the occurrence of pitting corrosion or crevice corrosion of the core material, and such an aluminum alloy three-layer clad material is said to be able to obtain excellent corrosion resistance and heat brazing properties, as well as high strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-293062 A Summary of the Invention [Problem to be solved by the invention]

[0006] The operating temperature of heat exchangers manufactured from such conventional aluminum alloy clad materials or aluminum alloy brazing sheets is generally 90°C or lower. However, in recent years, the operating conditions for heat exchangers have tended to become higher, and aluminum alloy clad materials and aluminum alloy brazing sheets are required to have good corrosion resistance even in operating environments of 100°C or higher.

[0007] In response to the above, when the operating conditions of heat exchangers become higher than before, especially when they reach 100°C or higher, the knowledge gained about conventional aluminum alloy clad materials and aluminum alloy brazing sheets cannot be applied as is, and new consideration is required. In fact, it has been found that aluminum alloy clad materials that show good corrosion resistance at temperatures below 90°C often have poor corrosion resistance at temperatures above 100°C.

[0008] Therefore, an object of the present invention is to provide an aluminum alloy clad material that has excellent corrosion resistance even when used in a heat exchanger where the operating conditions are 100°C or higher. [Means for solving the problem]

[0009] The present invention relates to the following [1] and [2]. [1] An aluminum alloy clad material comprising a core material having a pair of opposing main surfaces and a sacrificial anode layer provided on at least one of the main surfaces of the core material, wherein, in terms of the pitting potential determined by anodic polarization measurement under the following conditions, the pitting potential of the core material is more noble than the pitting potential of the sacrificial anode layer, and the potential difference is 50 mV or more. (conditions) Working electrode: core material or sacrificial anode layer, counter electrode: Pt, reference electrode: Ag / AgCl / saturated KCl, electrolyte: Cl - 300 ppm and SO4 2- Aqueous solution containing 100 ppm, temperature: 95°C, atmosphere: high-purity nitrogen gas, sweep speed: 1 mV / s "2" The core material contains 0.05 to 0.6 mass% Si, 1.0 to 1.5 mass% Mn, and 0.05 to 1.8 mass% Cu, with the remainder being Al and unavoidable impurities. The aluminum alloy clad material according to [1] above, wherein the sacrificial anode layer is an Al-Zn alloy layer containing 1.0 to 5.0 mass % of Zn, with the remainder being Al and unavoidable impurities. Effect of the Invention

[0010] According to the present invention, it is possible to provide an aluminum alloy clad material having excellent corrosion resistance and suitable for use in environments where the operating conditions are 100° C. or higher. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiment of the aluminum alloy clad material according to the present invention will be described in detail. Note that the numerical range "to" is used to mean that the numerical range includes the numerical range before and after it as the lower and upper limits. In addition, when simply written as ppm, it means mass ppm.

[0012] <Aluminum alloy clad material> The aluminum alloy clad material according to the present embodiment includes a core material having a pair of opposing main surfaces, and a sacrificial anode layer provided on at least one of the main surfaces of the core material. The pitting potential of the core material is more noble than the pitting potential of the sacrificial anode layer, and the potential difference therebetween is 50 mV or more.

[0013] A method for determining the pitting potential of the core material or the sacrificial anode layer in this specification will be described. The aluminum alloy clad material is subjected to a brazing-equivalent heat treatment and then cut to an appropriate size to prepare a test piece, and the center of the core material excluding the sacrificial anode layer or a 10 mm x 10 mm area of ​​the sacrificial anode layer is masked. The center of the core material refers to the center in the thickness direction of the core material, and the sacrificial anode layer and the surface of the core material are etched and dissolved in a 5% NaOH aqueous solution to expose them. Using this as the working electrode, anode polarization measurement is performed using a three-electrode method under the following conditions. In the polarization curve obtained in the anode polarization measurement, the potential at the inflection point where the current density increases sharply is taken as the pitting potential of the core material or the sacrificial anode layer. The temperature under the following conditions is 95°C, which is lower than the assumed operating temperature of the heat exchanger, which is 100°C or higher. This is because the anode polarization measurement is performed in an open system where pressure cannot be applied, so the electrolyte boils and cannot remain in a liquid state, and the temperature cannot be increased any higher. However, even if the temperature is 95°C, in consideration of the results of the high-temperature corrosion test described below and the results of the pitting potential when the temperature is set to 60°C, it can be said that the temperature is sufficient to judge the superiority or inferiority of corrosion resistance at 100°C or higher, at least at 100 to 120°C. (conditions) Working electrode: core material or sacrificial anode layer Counterpole: Pt Reference electrode:Ag / AgCl / saturated KCl Electrolyte:Cl - 300 ppm and SO4 2- Aqueous solution containing 100 ppm Temperature: 95℃ Atmosphere: High purity nitrogen gas Sweep speed: 1mV / sec As a pretreatment, the working electrode is immersed in a 5% NaOH aqueous solution for 30 seconds, rinsed with water, and then immersed in a 30% HNO3 aqueous solution for 60 seconds and rinsed with water. The natural potential is then measured for 20 minutes, after which the anode polarization measurement is performed. The measurement is also performed in a high-purity nitrogen gas atmosphere, but the measurement is performed with high-purity nitrogen gas being blown in.

[0014] If the pitting potential of the core material is more noble than the pitting potential of the sacrificial anode layer and the potential difference is 50 mV or more, the core material is prevented from penetrating corrosion at high temperatures of 100° C. or more, at least 100 to 120° C., and has excellent corrosion resistance. The potential difference is preferably 60 mV or more, more preferably 80 mV or more, and even more preferably 100 mV or more. In addition, from the viewpoint of making the sacrificial anode layer last longer and maintaining corrosion resistance for a long period of time, the potential difference is preferably 250 mV or less, more preferably 200 mV or less, and even more preferably 150 mV or less.

[0015] The superiority or inferiority of corrosion resistance at high temperatures is judged by a high-temperature corrosion test performed under the following conditions. The aluminum alloy clad material is cut into appropriate sizes to prepare test pieces, and a corrosion test is carried out for 6 or 24 hours in a 120°C aqueous solution using a high-temperature heat transfer surface corrosion tester. 2+ 10 ppm, Cl - 300 ppm and SO4 2- Contains 100 ppm of . After the test, the test piece is washed with water and then with nitric acid. The part corresponding to the maximum corrosion depth is selected using the focal depth method, the corroded part is embedded in resin, polished, and the cross-sectional shape is observed with an optical microscope. The maximum corrosion depth is measured from the distance between the surface of the sacrificial anode layer and the deepest part of the corrosion in the cross-sectional photograph.

[0016] The maximum corrosion depth obtained from the above-mentioned high-temperature corrosion test varies depending on the thickness of the sacrificial anode layer. However, in both the 6-hour corrosion test and the 24-hour corrosion test, if the thickness of the sacrificial anode layer is x μm, then the maximum corrosion depth is preferably (x+20) μm or less, more preferably (x+10) μm or less, even more preferably x μm or less, and the shallower the better.

[0017] The maximum corrosion depth obtained from the high temperature corrosion test is said to be more stable in the depth direction as the difference between the maximum corrosion depth after the 6-hour corrosion test and the maximum corrosion depth after the 24-hour corrosion test is smaller, which is preferable from the viewpoint of maintaining corrosion resistance for a long period of time. Therefore, when the difference between the maximum corrosion depth after the 24-hour corrosion test and the maximum corrosion depth after the 6-hour corrosion test is 10 μm or less, it is considered that the corrosion in the depth direction has stopped. The lower limit of the difference in the maximum corrosion depth is not particularly limited, and it may be 0 μm, i.e., there may be no difference.

[0018] The composition of the core material and the sacrificial anode layer is not particularly limited as long as there is the above-mentioned difference in pitting potential, but for example, the core material preferably contains 0.05 to 0.6 mass% Si, 1.0 to 1.5 mass% Mn, and 0.05 to 1.8 mass% Cu, with the balance being Al and unavoidable impurities. The sacrificial anode layer preferably contains 1.0 to 5.0 mass% Zn, with the balance being Al and unavoidable impurities, and is an Al-Zn alloy layer. The core material and the sacrificial anode layer may contain one or more components other than those described above, as long as the effect of the present invention is not impaired. Each of these will be explained in detail below.

[0019] (Heartwood) Si:0.05~0.6% by mass Si is a component that improves the strength after brazing when an aluminum alloy brazing sheet is made by providing a brazing material to an aluminum alloy clad material by dissolving in the parent phase or by forming an Al-Mn-Si intermetallic compound together with Mn. From the viewpoint of improving the strength, the Si content is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.15 mass% or more. In addition, from the viewpoint of preventing the solidus temperature from lowering and melting during brazing, the Si content is preferably 0.6 mass% or less, more preferably 0.5 mass% or less, and even more preferably 0.4 mass% or less.

[0020] Mn: 1.0~1.5% by mass Mn is a component that improves the strength after brazing when an aluminum alloy brazing sheet is made by providing a brazing material to an aluminum alloy clad material by dissolving in the parent phase or by forming an Al-Mn-Si intermetallic compound together with Si. From the viewpoint of improving the strength, the Mn content is preferably 1.0 mass% or more, more preferably 1.1 mass% or more, and even more preferably 1.2 mass% or more. In addition, from the viewpoint of preventing the intermetallic compounds from precipitating coarsely, reducing the rollability and making the manufacturing difficult, the Mn content is preferably 1.5 mass% or less, more preferably 1.4 mass% or less, and even more preferably 1.3 mass% or less.

[0021] Cu:0.05~1.8% by mass Cu is a component that contributes to improving corrosion resistance by making the pitting potential of the core material nobler and increasing the potential difference with the pitting potential of the sacrificial anode layer. From the viewpoint of obtaining such a potential difference, the Cu content is preferably 0.05% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more. In addition, from the viewpoint of suppressing the deterioration of corrosion resistance caused by the diffusion of components to the surface during brazing when the aluminum alloy clad material is provided with a brazing material to form an aluminum alloy brazing sheet, and from the viewpoint of preventing melting during brazing due to a decrease in solidus temperature, the Cu content is preferably 1.8% by mass or less, more preferably 1.5% by mass or less, and even more preferably 1.2% by mass or less.

[0022] Ti: 0.3% by mass or less Ti is a component that distributes in layers in the aluminum alloy, and thereby allows the potential distribution of the aluminum alloy brazing sheet or aluminum alloy clad material to correspond to the concentration of Ti content. Therefore, the corrosion form becomes layered, the rate of corrosion progression in the depth direction is reduced, and it can contribute to improving corrosion resistance. Therefore, when Ti is contained, the Ti content is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and even more preferably 0.05 mass% or more. In addition, from the viewpoint of suppressing the formation of coarse Al3Ti intermetallic compounds during casting, which reduces workability and causes cracks during tube molding, the Ti content is preferably 0.3 mass% or less, more preferably 0.2 mass% or less, and even more preferably 0.15 mass% or less.

[0023] Cr: 0.3% by mass or less Cr is a component that contributes to improving the strength after brazing when an aluminum alloy brazing sheet is made by forming Al3Cr dispersed particles and dispersing them to improve corrosion resistance by refining crystal grains. Therefore, when Cr is contained, the Cr content is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and even more preferably 0.05 mass% or more. In addition, from the viewpoint of easily forming coarse Al3Cr intermetallic compounds and suppressing a decrease in ductility, the Cr content is preferably 0.3 mass% or less, more preferably 0.2 mass% or less, and even more preferably 0.15 mass% or less.

[0024] Zr: 0.3% by mass or less Zr is a component that contributes to improving the strength after brazing when an aluminum alloy brazing sheet is made by forming Al3Zr dispersed particles and dispersing them to improve corrosion resistance by refining crystal grains. Therefore, when Zr is contained, the Zr content is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and even more preferably 0.05 mass% or more. In addition, from the viewpoint of suppressing the formation of coarse Al3Zr intermetallic compounds during casting, which reduces workability and causes cracks during tube molding, the Zr content is preferably 0.3 mass% or less, more preferably 0.2 mass% or less, and even more preferably 0.15 mass% or less.

[0025] Fe: 0.15% by mass or less Fe is a component that improves strength by solid solution strengthening. Therefore, when Fe is contained, the Fe content is preferably 0.01 mass% or more, more preferably 0.03 mass% or more, and even more preferably 0.05 mass% or more. In order to prevent the corrosion resistance from decreasing, the Fe content is preferably 0.15 mass% or less, more preferably 0.1 mass% or less, and even more preferably 0.08 mass% or less.

[0026] Remainder: Al and inevitable impurities The remainder of the core material in this embodiment is Al and inevitable impurities. Inevitable impurities are impurities that are inevitably mixed in when the raw materials are melted, and examples thereof include V, Ni, Ca, Na, Sr, Li, Mo, Zn, Sn, and In. These may be contained alone or in combination as long as they do not impair the effects of the present invention. The contents of the above-listed V, Ni, Ca, Na, Sr, Li, Mo, Zn, Sn, and In are each preferably 0.05 mass% or less. The total content of these is preferably 0.2 mass% or less. The above-mentioned inevitable impurity components may be added not only as inevitable impurities, but also intentionally. On the other hand, the above-mentioned Ti, Cr, Zr, and Fe may be added not only as inevitable impurities, but also intentionally. The total content of Ti, Cr, Zr and Fe is preferably 0.4 mass % or less.

[0027] (Sacrificial anode layer) Zn: 1.0~5.0% by mass Zn is a component that prevents pitting corrosion and crevice corrosion by making the potential of the base material lower and enhancing the sacrificial corrosion protection effect with respect to the core material. From the viewpoint of preventing such corrosion, the Zn content is preferably 1.0 mass% or more, more preferably 1.5 mass% or more, and even more preferably 2.0 mass% or more. In addition, from the viewpoint of preventing the self-corrosiveness of the sacrificial anode layer from becoming excessive and reducing the corrosion protection life of the entire aluminum alloy clad material, the Zn content is preferably 5.0 mass% or less, more preferably 4.5 mass% or less, and even more preferably 4.0 mass% or less.

[0028] Remainder: Al and inevitable impurities The remainder of the sacrificial anode layer in this embodiment is Al and inevitable impurities. The inevitable impurities are impurities that are inevitably mixed in when the raw material is melted, and examples thereof include Si, Mn, Ti, Cr, Zr, V, Ni, Ca, Na, Sr, Li, Mo, Sn, and In. These may be contained in one or more types within a range that does not impair the effects of the present invention. The contents of the above-mentioned Si, Mn, Ti, Cr, Zr, V, Ni, Ca, Na, Sr, Li, Mo, Zn, Sn, and In are each preferably 0.05% by mass or less. In addition, the total content of these is preferably 0.2% by mass or less. The above-mentioned inevitable impurity components may be added not only as inevitable impurities but also actively. On the other hand, the above-mentioned Zn may be added not only as inevitable impurities but also as inevitable impurities.

[0029] (Thickness, cladding rate) The thickness of the aluminum alloy clad material according to the present embodiment is not particularly limited, but considering application to components of automobile heat exchangers, for example, the thickness is preferably 0.5 mm or less, more preferably 0.45 mm or less, and even more preferably 0.4 mm or less from the viewpoint of formability, and is preferably 0.2 mm or more, more preferably 0.25 mm or more, and even more preferably 0.3 mm or more from the viewpoint of strength and corrosion resistance. The thickness of the aluminum alloy clad material is the total thickness of the core material and the sacrificial anode layer.

[0030] The thickness of the sacrificial anode layer in this embodiment is compared in terms of the cladding ratio, which is the ratio of the thickness when the total thickness of the aluminum alloy cladding material is taken as 100%. The cladding ratio of the sacrificial anode layer is not particularly limited, but is preferably 10% or more, more preferably 13% or more, and even more preferably 15% or more, from the viewpoint of corrosion resistance. Also, from the viewpoint of strength, the cladding ratio is preferably 25% or less, more preferably 22% or less, and even more preferably 20% or less.

[0031] (Aluminum alloy brazing sheet) The aluminum alloy clad material according to this embodiment includes the above-mentioned core material and the sacrificial anode layer, and can be made into an aluminum alloy brazing sheet by providing a brazing material on the main surface of the core material opposite to the side on which the sacrificial anode layer is provided. An intermediate layer may be further provided between the core material and the brazing material or between the core material and the sacrificial anode layer.

[0032] The brazing material may be one having a conventionally known composition, and is not particularly limited. For example, it may be made of an Al-Si alloy or an Al-Si-Zn alloy. It may also contain other elements. For example, in the case of an Al-Si alloy, general JIS alloys such as 4343 and 4045 specified in JIS Z 3263: 2002 can be mentioned. The Al-Si alloy preferably contains 5 to 15 mass %, more preferably 7 to 13 mass %, of Si, but the Si content is not limited to this range. Examples of other components besides Al, Si, and Zn include Mg, Bi, Cu, Mn, Ti, Ca, Be, Sr, Na, Sb, rare earth elements, Li, etc. These may be intentionally added or may be contained as unavoidable impurities.

[0033] The intermediate layer may have a known composition and is not particularly limited. For example, other components that may be contained in addition to Al include Si, Mn, Cu, Zn, Mg, Bi, Ti, Cr, Zr, V, Ni, Ca, Na, Sr, Li, Mo, Zn, Sn, and In. These may be added intentionally or may be contained as unavoidable impurities.

[0034] When the aluminum alloy clad material according to the present embodiment is used as an aluminum alloy brazing sheet, the thickness of the aluminum alloy brazing sheet is not particularly limited, but considering application to a member of an automobile heat exchanger, for example, from the viewpoint of formability, the thickness is preferably 0.7 mm or less, more preferably 0.6 mm or less, and even more preferably 0.5 mm or less. Also, from the viewpoints of strength and corrosion resistance, the thickness is preferably 0.2 mm or more, more preferably 0.3 mm or more, and even more preferably 0.4 mm or more. The thickness of the aluminum alloy brazing sheet is the total thickness of the core material, the sacrificial anode layer, the brazing material and the intermediate layer.

[0035] In this embodiment, the cladding ratio, which is the ratio of the thickness of each of the sacrificial anode layer, the brazing material, and the intermediate layer when the total thickness of the aluminum alloy brazing sheet is taken as 100%, is not particularly limited.

[0036] An aluminum alloy brazing sheet using the aluminum alloy clad material according to this embodiment can be used as a tube material for a radiator or an intercooler, for example, in the case of a component of an automobile heat exchanger.

[0037] <Method of manufacturing aluminum alloy clad material> The method for producing the aluminum alloy clad material according to the present embodiment is not particularly limited, and the material can be produced by, for example, a known production method, an example of which will be described below. First, aluminum alloys having the respective component compositions of the core material and the sacrificial anode layer are melted and cast, and then, if necessary, surface smoothing treatments such as facing and homogenization treatments are performed to obtain respective ingots. The ingot of the sacrificial anode layer is hot rolled or mechanically sliced ​​to a predetermined thickness, and combined with the ingot of the core material, and hot rolled according to a conventional method to obtain an aluminum alloy clad material. The preferred embodiments of the core material and the sacrificial anode layer used here are the same as those of the core material and the sacrificial anode layer described above in the <Aluminum clad material>.

[0038] When manufacturing an aluminum alloy brazing sheet, the aluminum alloy having the composition of the core material, the sacrificial anode layer, the brazing material, and, if necessary, the intermediate layer are melted and cast, and if necessary, the ingot is subjected to surface smoothing treatment such as facing and homogenization treatment to obtain each ingot. The obtained ingot is hot rolled or mechanically sliced ​​to a predetermined thickness, combined with the ingot of the core material, and hot rolled according to the usual method to obtain a clad material. The clad material is then subjected to cold rolling, intermediate annealing if necessary, final cold rolling, and final annealing if necessary to obtain an aluminum alloy brazing sheet. When final annealing is performed, intermediate annealing can be omitted. In addition, the tempering may be any of H1n, H2n, and H3n (JIS H 0001:1998).

[0039] The aluminum alloy clad material according to this embodiment and the method for manufacturing an aluminum alloy brazing sheet using the same are as described above. For conditions not explicitly stated in each of the above steps, conventionally known conditions may be used, and the conditions may be changed as appropriate as long as the effects obtained by the treatment in each step are achieved. EXAMPLES

[0040] The present invention will be described in more detail below with reference to examples, comparative examples, and reference examples. However, the present invention is not limited to these examples, and can be practiced with modifications within the scope of the invention, all of which are included in the technical scope of the present invention.

[0041] (Examples 1 to 3 and Comparative Example 1) An aluminum alloy having the composition shown in Table 1 was cast, and the core material was homogenized at 500-600°C for 3-5 hours, and the sacrificial anode layer was homogenized at 450-550°C for 3-5 hours. Next, the combination shown in Table 2 was subjected to homogenization at 450-550°C for about 30 minutes, hot rolling, and cold rolling. Next, intermediate annealing was performed at 300-400°C for 3-5 hours, and finally, final cold rolling was performed so that the overall thickness was 0.3 mm to obtain an aluminum alloy clad material. The thickness of the sacrificial anode layer was measured by cross-sectional observation. The results are shown in Table 1. The obtained aluminum alloy clad material with a thickness of 0.3 mm was cut to the required size and subjected to a heat treatment equivalent to brazing by holding it at 590°C or higher for 3 minutes or more in a nitrogen atmosphere, and the resultant material was used for evaluation as a test material.

[0042] [Table 1]

[0043] [Table 2]

[0044] (Evaluation: High temperature corrosion test) The test material was cut into a size of 70 mm x 70 mm, and a corrosion test was carried out for 6 or 24 hours in a 120°C aqueous solution using a high-temperature heat transfer surface corrosion tester (compliant with ASTM D-4340-1984). 2+ 10 ppm, Cl - 300 ppm and SO4 2-After the test, the test piece was washed with water and then with nitric acid, and the maximum corrosion depth was measured from the cross section of the corrosion using an optical microscope (Olympus, PMG3). The results are shown in Table 2.

[0045] (Evaluation: Anode polarization measurement) The test material was cut into a size of 20 mm x 20 mm to prepare a test piece, and the central part of the core material excluding the sacrificial anode layer or the 10 mm x 10 mm area of ​​the sacrificial anode layer was masked with Teflon tape and silicon. Using this as the working electrode, anode polarization measurement was performed in a three-electrode system under the following conditions. In the polarization curve obtained by the anode polarization measurement, the potential at the inflection point where the current density suddenly increased was taken as the pitting potential of the core material or the sacrificial anode layer. (conditions) Working electrode: core material or sacrificial anode layer Counterpole: Pt Reference electrode:Ag / AgCl / saturated KCl Electrolyte:Cl - 300 ppm and SO4 2- Aqueous solution containing 100 ppm Temperature: 95℃ Atmosphere: High purity nitrogen gas Sweep speed: 1mV / sec As a pretreatment, the working electrode was immersed in a 5% NaOH aqueous solution for 30 seconds, washed with water, and then immersed in a 30% HNO3 aqueous solution for 60 seconds and washed with water. The natural potential was then measured for 20 minutes, after which the anode polarization measurement was carried out. The measurement in a high-purity nitrogen gas atmosphere was carried out with high-purity nitrogen gas blown in. The pitting potentials of the obtained core materials were all higher than the pitting potential of the sacrificial anode layer. The potential differences are shown in Table 2.

[0046] (Reference example 1) As Reference Example 1, a corrosion test was carried out on the aluminum alloy clad material of Comparative Example 1 in the same manner as above (evaluation: high temperature corrosion test) except that the temperature of the aqueous solution was set to 50°C. For the aluminum alloy clad material specimen of Comparative Example 1, the pitting potential of the core material and the pitting potential of the sacrificial anode layer were determined in the same manner as above (evaluation: anode polarization measurement) except that the temperature of the aqueous solution was set to 60° C. The pitting potential of the core material was more noble than the pitting potential of the sacrificial anode layer, and the potential difference is shown in Table 2.

[0047] From the above results, it was found that in Examples 1 to 3, in which the pitting potential of the core material is more noble than the pitting potential of the sacrificial anode layer and the potential difference is 50 mV or more, the maximum corrosion depth is shallower than in Comparative Example 1, corrosion in the depth direction is stopped, and the corrosion resistance is excellent even in a high temperature environment such as 120°C. As shown in Reference Example 1, the aluminum alloy clad material of Comparative Example 1 showed a potential difference at 60°C similar to that of the Examples tested at 95°C, and showed very good corrosion resistance at 50°C, but the corrosion resistance deteriorated at a high temperature of 120°C. This makes it clear that a material that has previously shown good corrosion resistance does not necessarily show similarly good corrosion resistance in a high-temperature environment of 100°C or higher.

Claims

1. An aluminum alloy clad material comprising a core material having a pair of opposing main surfaces and a sacrificial anode layer provided on at least one of the main surfaces of the core material, The core material contains 0.05 to 0.6 mass% Si, 1.0 to 1.5 mass% Mn, and 0.05 to 1.8 mass% Cu, with the balance being Al and unavoidable impurities; the sacrificial anode layer is an Al-Zn alloy layer containing 1.0 to 5.0 mass % Zn, with the remainder being Al and unavoidable impurities; The thickness of the aluminum alloy clad material is 0.25 mm or more, The cladding ratio of the sacrificial anode layer is 10 to 22%; Regarding the pitting potential obtained by anodic polarization measurement under the following conditions, the pitting potential of the core material is more noble than the pitting potential of the sacrificial anode layer, and the potential difference therebetween is 50 mV or more; An aluminum alloy clad material used in environments where the operating conditions are 100°C or higher. (conditions) Working electrode: core material or sacrificial anode layer Counter electrode: Pt Reference electrode: Ag / AgCl / saturated KCl Electrolyte: Cl - and SO 4 2- An aqueous solution containing 100 ppm of Temperature: 95℃ Atmosphere: High purity nitrogen gas Sweep speed: 1mV / sec

2. The core material contains 0.05 to 0.4 mass % of Si, 1.1 to 1.5 mass % of Mn, and 0.05 to 1.8 mass % of Cu, with the balance being Al and unavoidable impurities.

2. The aluminum alloy clad material according to claim 1, wherein the sacrificial anode layer is an Al-Zn alloy layer containing 2.0 to 4.7 mass % Zn, with the remainder being Al and unavoidable impurities.

Citation Information

Patent Citations

  • Highly corrosion resistant brazing sheet

    JP2002206129A

  • Aluminum alloy three layer clad plate

    JP2003293062A

  • Aluminum alloy brazing sheet for brazed pipe making tubes, and its producing method

    JP2004017116A

  • Brazing sheet and heat exchanger

    JP2005298913A

  • Aluminum alloy material, and aluminum alloy brazing sheet

    JP2009127122A